Polarizing plate and polarizing plate with optically functional layer

The polarizing plate with a thermoplastic acrylic resin protective layer and optional optical functional layer addresses durability and flexibility issues, ensuring excellent performance in flexible image display devices despite thinness.

JP7596079B2Active Publication Date: 2024-12-09NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020080789
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-30
Publication Date
2024-12-09
Estimated Expiration
2040-04-30

AI Technical Summary

Technical Problem

Thinner polarizing plates for image display devices face challenges with durability and flexibility, particularly under heated and humid conditions, and bending resistance, which compromises their optical properties.

Method used

A polarizing plate composed of a polarizer with a protective layer made from a solidified coating film of a thermoplastic acrylic resin in an organic solvent, with a glass transition temperature of 95°C or higher, and a total thickness of 20 μm or less, combined with an optional optical functional layer, enhancing durability and flexibility.

Benefits of technology

The solution provides polarizing plates with excellent durability and flexibility, maintaining optical properties even under heated and humid conditions, and allowing for applications in flexible and bendable image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596079000007
    Figure 0007596079000007
  • Figure 0007596079000008
    Figure 0007596079000008
  • Figure 0007596079000009
    Figure 0007596079000009
Patent Text Reader

Abstract

To provide a polarizing plate which is extremely thin and yet offers superior durability and superior flexibility.SOLUTION: A polarizing plate of the present invention comprises a polarizer and a protective layer provided on one side of the polarizer, the protective layer being a cured coating film of a solution of a thermoplastic acrylic resin organic solvent and having a glass transition temperature of 95°C or higher and a total thickness of 20 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate and an optically functional layer-attached polarizing plate. [Background technology]

[0002] In many image display devices (e.g., liquid crystal display devices and organic EL display devices), a polarizing plate is arranged on at least one side of the display cell due to the image formation method. In recent years, image display devices have become thinner and more flexible, and accordingly, there is a strong demand for thinner polarizing plates. However, the thinner the polarizing plate, the more pronounced the durability problem becomes, namely, the deterioration of optical properties in a heated and humidified environment.

[0003] In recent years, with the increasing demand for curved image display devices and / or bendable or foldable image display devices, polarizing plates (as a result, polarizing plates with optical functional layers) are also required to have excellent mechanical properties of bendability and optical properties that do not change when bent. However, there is still room for consideration toward practical use of polarizing plates (as a result, polarizing plates with optical functional layers) that satisfy such properties. In addition, when the bending resistance is improved, there is a problem that the strength of the polarizing plate is reduced, and the physical durability is reduced. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-210474 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made to solve the above-mentioned problems in the conventional art, and its main object is to provide a polarizing plate and a polarizing plate with an optical functional layer that are extremely thin yet have both excellent durability and excellent flexibility. [Means for solving the problem]

[0006] The polarizing plate of the present invention includes a polarizer and a protective layer disposed on one side of the polarizer. The protective layer is made of a solidified coating film of a solution of a thermoplastic acrylic resin in an organic solvent, and has a glass transition temperature of 95° C. or higher. The polarizing plate has a total thickness of 20 μm or less. In one embodiment, the protective layer has a thickness of 10 μm or less. In one embodiment, the polarizer has a thickness of 10 μm or less. In one embodiment, the thermoplastic acrylic resin has at least one selected from the group consisting of a lactone ring unit, a glutaric anhydride unit, a glutarimide unit, a maleic anhydride unit, and a maleimide unit. In another aspect of the present invention, there is provided a polarizing plate with an optical functional layer, the polarizing plate with an optical functional layer including the polarizing plate and an optical functional layer disposed on the opposite side of the polarizer to the protective layer, and having a total thickness of 25 μm or less. In one embodiment, the optical functional layer functions as a protective layer separate from the protective layer. In one embodiment, the optical functional layer is a retardation layer having a circular polarization function or an elliptically polarizing function. Effect of the Invention

[0007] According to an embodiment of the present invention, a polarizing plate and an optically functional layer-attached polarizing plate that are both excellent in durability and excellent in flexibility despite being very thin can be provided. In an embodiment of the present invention, the protective layer is made of a solidified coating film of a solution of a thermoplastic acrylic resin in an organic solvent, and the glass transition temperature of the coating film is set to a predetermined value or higher. Therefore, a polarizing plate and an optically functional layer-attached polarizing plate that are both excellent in durability and excellent in flexibility can be provided. [Brief description of the drawings]

[0008] [Figure 1] 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view of an optically functional layer-attached polarizing plate according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing an example of a drying shrinkage treatment using a heating roll in a method for producing a polarizing plate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, the angles include both clockwise and counterclockwise angles relative to a reference direction, so for example, "45°" means ±45°.

[0010] A. Overview of polarizing plates and polarizing plates with optically functional layers A-1. Overview of polarizing plates FIG. 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 in the illustrated example has a polarizer 10 and a protective layer 20 arranged on one side of the polarizer 10. The total thickness of the polarizing plate 100 is 20 μm or less. The protective layer 20 is composed of a solidified coating film of a solution of a thermoplastic acrylic resin in an organic solvent, and has a glass transition temperature of 95° C. or more. By having such a protective layer in the polarizing plate 100, it is possible to provide a polarizing plate that has both excellent durability and excellent flexibility despite its very thin thickness. In one embodiment, the thickness of the polarizer 10 is preferably 10 μm or less. In addition, in one embodiment, the thickness of the protective layer 20 is preferably 10 μm or less.

[0011] The total thickness of the polarizing plate 100 is 20 μm or less, preferably 15 μm or less, and more preferably 10 μm or less. According to the present invention, a polarizing plate that has both excellent durability and excellent flexibility can be provided even if the total thickness of the polarizing plate is within the above range. The total thickness of the polarizing plate is, for example, 5 μm or more.

[0012] Further, in the embodiment of the present invention, the glass transition temperature (Tg) of the protective layer 20 is 95°C or more, preferably 100°C or more, more preferably 105°C or more, even more preferably 110°C or more, and particularly preferably 115°C or more. If the Tg of the protective layer is in such a range, a polarizing plate (as a result, a polarizing plate with an optical function layer) having excellent durability despite being very thin can be realized due to a synergistic effect with the effect of forming the protective layer from a solidified coating film of an organic solvent solution of a thermoplastic acrylic resin. Specifically, a polarizing plate (as a result, a polarizing plate with an optical function layer) in which the deterioration of optical properties is suppressed even in a heated and humidified environment can be realized. On the other hand, the Tg of the protective layer is preferably 300°C or less, more preferably 250°C or less, even more preferably 200°C or less, and particularly preferably 160°C or less. If the Tg of the protective layer is in such a range, excellent moldability can be obtained.

[0013] Each layer or optical film constituting the polarizing plate is typically bonded via an adhesive layer. Examples of the adhesive layer include an adhesive layer and a pressure-sensitive adhesive layer. In the embodiment of the present invention, an adhesive layer can be suitably used. With such a configuration, the polarizing plate can be further thinned. Examples of the adhesive constituting the adhesive layer include an active energy ray curable adhesive (e.g., an ultraviolet ray curable adhesive).

[0014] In the embodiment of the present invention, the polarizing plate can be extremely thin. Therefore, it can be suitably applied to a flexible image display device. More preferably, the image display device has a curved shape (substantially a curved display screen) and / or can be bent or folded. Specific examples of the image display device include a liquid crystal display device and an electroluminescence (EL) display device (e.g., an organic EL display device, an inorganic EL display device). Needless to say, the above description does not prevent the polarizing plate of the present invention from being applied to a normal image display device.

[0015] A-2. Overview of polarizing plate with optical functional layer 2 is a schematic cross-sectional view of a polarizing plate with an optical functional layer according to one embodiment of the present invention. The polarizing plate with an optical functional layer 110 in the illustrated example includes a polarizer 10, a protective layer 20 arranged on one side of the polarizer, and an optical functional layer 30 arranged on the other side of the polarizer. The total thickness of the polarizing plate with an optical functional layer is 25 μm or less. In one embodiment, the polarizing plate 100 described above is used as the polarizer 10 and the protective layer 20.

[0016] The total thickness of the polarizing plate with optical functional layers 110 is 25 μm or less, preferably 20 μm or less, and more preferably 15 μm or less. According to the present invention, even if the total thickness of the polarizing plate is within the above range, it is possible to provide a polarizing plate that has both excellent durability and excellent flexibility. The total thickness of the polarizing plate with optical functional layers is, for example, 10 μm or more.

[0017] In one embodiment, the optical functional layer functions as a protective layer separate from the protective layer 20. Such a protective layer may also function as a retardation layer having a predetermined retardation and optical properties. In another embodiment, the optical functional layer is a retardation layer having a circular polarization function or an elliptical polarization function. Such a retardation layer may also function as a protective layer for a polarizer. When the optical functional layer is a retardation layer, in one embodiment, the retardation layer is an orientation-solidified layer of a liquid crystal compound. The retardation layer may be a single layer of an orientation-solidified layer, or may have a laminated structure of a first orientation-solidified layer and a second orientation-solidified layer. Hereinafter, a polarizing plate in which the optical functional layer is a retardation layer may be referred to as a retardation layer-attached polarizing plate.

[0018] Each layer or optical film constituting the polarizing plate with an optical functional layer is typically bonded via an adhesive layer. Examples of the adhesive layer include an adhesive layer and a pressure-sensitive adhesive layer. In the embodiment of the present invention, an adhesive layer can be preferably used. With such a configuration, the polarizing plate with an optical functional layer can be further thinned. Examples of the adhesive constituting the adhesive layer include an active energy ray curable adhesive (e.g., an ultraviolet ray curable adhesive).

[0019] A polarizing plate having an optical functional layer functioning as a retardation layer may further include another retardation layer. The other retardation layer is typically provided on the outside of the optical functional layer (retardation layer) 30 (opposite side to the polarizer 10). The other retardation layer typically has a refractive index characteristic of nz>nx=ny. Such another retardation layer is preferably provided when the retardation layer is a single layer of an orientation solidification layer. For convenience, the optical functional layer (retardation layer) 30 may be referred to as a first retardation layer, and the other retardation layer may be referred to as a second retardation layer. The polarizing plate with an optical functional layer may further include another retardation layer. The optical characteristics (e.g., refractive index characteristics, in-plane retardation, Nz coefficient, photoelastic coefficient), thickness, arrangement position, etc. of the other retardation layer may be appropriately set according to the purpose.

[0020] The polarizing plate with an optical functional layer may be provided with a conductive layer or a conductive layer-attached isotropic substrate. The conductive layer or the conductive layer-attached isotropic substrate is typically provided on the outside of the optical functional layer 30 (the side opposite to the polarizer 10). When the polarizing plate is a polarizing plate with a retardation layer having a retardation layer and another retardation layer, the other retardation layer and the conductive layer or the conductive layer-attached isotropic substrate are typically provided in this order from the retardation layer (optical functional layer) 30 side. When the conductive layer or the conductive layer-attached isotropic substrate is provided, the polarizing plate or the retardation layer-attached polarizing plate may be applied to a so-called inner touch panel type input display device in which a touch sensor is incorporated between an image display cell (e.g., an organic EL cell) and the polarizing plate.

[0021] As described above, by forming the protective layer from a solidified coating film of a solution of a thermoplastic acrylic resin in an organic solvent and setting the glass transition temperature to 95°C or higher, a polarizing plate with excellent durability can be realized despite being very thin. Specifically, a polarizing plate in which the deterioration of optical properties is suppressed even in a heated and humidified environment can be realized. The above polarizing plate has a very small change ΔTs in the single transmittance Ts and a very small change ΔP in the degree of polarization P after being left for 48 hours in an environment of 85°C and 85% RH. The single transmittance Ts can be measured, for example, using a UV-Vis spectrophotometer (manufactured by JASCO Corporation, product name "V7100"). The degree of polarization P is calculated from the single transmittance (Ts), parallel transmittance (Tp), and cross transmittance (Tc) measured using the UV-Vis spectrophotometer according to the following formula. Degree of polarization (P)(%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100 The above Ts, Tp, and Tc are Y values ​​measured using a 2-degree visual field (C light source) according to JIS Z 8701 and corrected for visibility. Ts and P are essentially characteristics of a polarizer. ΔTs and ΔP are calculated by the following formulas. ΔTs(%)=Ts 48 -Ts0 ΔP(%)=P 48 -P0 Here, Ts0 is the single unit transmittance before storage (initial time), and Ts 48is the single transmittance after storage, P0 is the degree of polarization before storage (initial), and P 48 is the degree of polarization after standing. ΔTs is preferably 3.0% or less, more preferably 2.7% or less, and even more preferably 2.4% or less. ΔP is preferably -1.0% to 0%, more preferably -0.5% to 0%, and even more preferably -0.3% to 0%.

[0022] For practical purposes, a pressure-sensitive adhesive layer (not shown) is provided on the opposite side of the optical functional layer from the polarizer, so that the polarizing plate can be attached to an image display cell. Furthermore, it is preferable that a release film is temporarily attached to the surface of the pressure-sensitive adhesive layer until the polarizing plate is used. By temporarily attaching the release film, the pressure-sensitive adhesive layer is protected and roll formation is possible.

[0023] The polarizing plate and the polarizing plate with an optical functional layer of the present invention may be in the form of a sheet or a long sheet. In this specification, the term "long sheet" means a long and narrow shape whose length is sufficiently longer than its width, and includes, for example, a long and narrow shape whose length is 10 times or more, preferably 20 times or more, than its width. A long and narrow polarizing plate can be wound into a roll.

[0024] The components of the polarizing plate and the polarizing plate with an optical functional layer will be described in more detail below.

[0025] B. Polarizer Any suitable polarizer may be used as the polarizer. The polarizer may typically be produced using a laminate of two or more layers. The method for producing the polarizer will be described later in Section F as the method for producing the polarizing plate.

[0026] The thickness of the polarizer is preferably 10 μm or less, more preferably 1 μm to 8 μm, further preferably 1 μm to 7 μm, and particularly preferably 2 μm to 5 μm.

[0027] The boric acid content of the polarizer is preferably 10% by weight or more, and more preferably 13% by weight to 25% by weight. When the boric acid content of the polarizer is in this range, due to a synergistic effect with the iodine content described below, it is possible to maintain ease of curl control during lamination and to improve appearance durability during heating while effectively suppressing curl during heating. The boric acid content can be calculated as the amount of boric acid contained in the polarizer per unit weight, for example, using the following formula from the neutralization method.

number

[0028] The iodine content of the polarizer is preferably 2% by weight or more, and more preferably 2% by weight to 10% by weight. When the iodine content of the polarizer is within this range, due to a synergistic effect with the above-mentioned boric acid content, it is possible to maintain ease of curl control during lamination, and to effectively suppress curling during heating, while improving appearance durability during heating. In this specification, the "iodine content" refers to the amount of all iodine contained in the polarizer (PVA-based resin film). More specifically, iodine in the polarizer is iodine ion (I - ), molecular iodine (I2), polyiodine ion (I3 - , I5 - ), and the iodine content in this specification refers to the amount of iodine including all of these forms. The iodine content can be calculated, for example, by the calibration curve method of fluorescent X-ray analysis. Note that polyiodine ions exist in the polarizer in the form of a PVA-iodine complex. The formation of such a complex can result in absorption dichroism in the wavelength range of visible light. Specifically, a complex of PVA and triiodide ion (PVA·I3 - ) has an absorption peak at around 470 nm, and the complex of PVA and pentaiodide ion (PVA·I5 - ) has an absorption peak at around 600 nm. As a result, polyiodide ions can absorb light in a wide range of visible light depending on their form. On the other hand, iodide ions (I -) has an absorption peak at about 230 nm and is not substantially involved in the absorption of visible light. Therefore, polyiodide ions present in a complex state with PVA may be mainly involved in the absorption performance of the polarizer.

[0029] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance Ts of the polarizer is preferably 40% to 48%, and more preferably 41% to 46%. The degree of polarization P of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.

[0030] C. Protective layer As described above, the protective layer is composed of a solidified coating film of a solution of a thermoplastic acrylic resin (hereinafter simply referred to as an acrylic resin) in an organic solvent. The components of the protective layer will be specifically described below, and then the characteristics of the protective layer will be described.

[0031] C-1. Acrylic resin The Tg of the acrylic resin (including blends of two or more acrylic resins and blends of an acrylic resin with another resin, as described below) is as described above in Section A for the protective layer.

[0032] As the acrylic resin, any appropriate acrylic resin may be adopted as long as it has the above Tg. The acrylic resin typically contains an alkyl(meth)acrylate as a main component as a monomer unit (repeating unit). In this specification, "(meth)acrylic" means acrylic and / or methacrylic. Examples of the alkyl(meth)acrylate constituting the main skeleton of the acrylic resin include linear or branched alkyl groups having 1 to 18 carbon atoms. These can be used alone or in combination. Furthermore, any appropriate copolymerization monomer may be introduced into the acrylic resin by copolymerization. The repeating unit derived from the alkyl(meth)acrylate is typically represented by the following general formula (1):

[0033] [ka]

[0034] In the general formula (1), R 4 represents a hydrogen atom or a methyl group, and R 5 represents a hydrogen atom, or an optionally substituted aliphatic or alicyclic hydrocarbon group having 1 to 6 carbon atoms. Examples of the substituent include halogen and a hydroxyl group. Specific examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, chloromethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2,3,4,5,6-pentahydroxyhexyl (meth)acrylate, 2,3,4,5-tetrahydroxypentyl (meth)acrylate, methyl 2-(hydroxymethyl)acrylate, ethyl 2-(hydroxymethyl)acrylate, and methyl 2-(hydroxyethyl)acrylate. In the general formula (1), R 5 is preferably a hydrogen atom or a methyl group. Thus, a particularly preferred alkyl (meth)acrylate is methyl acrylate or methyl methacrylate.

[0035] The acrylic resin may contain only a single alkyl (meth)acrylate unit, or may be a single alkyl (meth)acrylate unit represented by the general formula (1) above. 4 and R 5 It may contain a plurality of alkyl (meth)acrylate units having different structures.

[0036] The content of alkyl (meth)acrylate units in the acrylic resin is preferably 50 mol% to 98 mol%, more preferably 55 mol% to 98 mol%, even more preferably 60 mol% to 98 mol%, particularly preferably 65 mol% to 98 mol%, and most preferably 70 mol% to 97 mol%. If the content is less than 50 mol%, the effects derived from the alkyl (meth)acrylate units (e.g., high heat resistance, high transparency) may not be fully exhibited. If the content is more than 98 mol%, the resin may become brittle and easily cracked, and high mechanical strength may not be fully exhibited, resulting in poor productivity.

[0037] The acrylic resin preferably has a repeating unit containing a ring structure. Examples of the repeating unit containing a ring structure include a lactone ring unit, a glutaric anhydride unit, a glutarimide unit, a maleic anhydride unit, and a maleimide (N-substituted maleimide) unit. The repeating unit containing a ring structure may contain only one type of repeating unit, or may contain two or more types of repeating units.

[0038] The lactone ring unit is preferably represented by the following general formula (2):

[0039] [ka] In the general formula (2), R 1 , R 2 and R 3 each independently represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms. The organic residue may contain an oxygen atom. The acrylic resin may contain only a single lactone ring unit, and R 1 , R 2 and R 3 The acrylic resin may contain a plurality of lactone ring units having different ring structures. Acrylic resins having lactone ring units are described in, for example, JP-A-2008-181078, the disclosure of which is incorporated herein by reference.

[0040] The glutarimide unit is preferably represented by the following general formula (3):

[0041] [ka]

[0042] In the general formula (3), R 11 and R 12 each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 13 represents an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms. 11 and R 12 are each independently a hydrogen atom or a methyl group, and R 13 is hydrogen, a methyl group, a butyl group, or a cyclohexyl group. More preferably, R 11 is a methyl group, and R 12 is hydrogen, and R 13 is a methyl group. The acrylic resin may contain only a single glutarimide unit, and R 11 , R 12 and R 13 Acrylic resins having glutarimide units may contain a plurality of glutarimide units having different groups. Examples of acrylic resins having glutarimide units are described in JP-A-2006-309033, JP-A-2006-317560, JP-A-2006-328334, JP-A-2006-337491, JP-A-2006-337492, JP-A-2006-337493, and JP-A-2006-337569, the disclosures of which are incorporated herein by reference. Note that the glutaric anhydride unit is represented by the formula (3) above, 13 The above description regarding the glutarimide unit applies, except that the nitrogen atom substituted with is an oxygen atom.

[0043] As for the maleic anhydride unit and the maleimide (N-substituted maleimide) unit, their structures are specified by their names, and therefore specific explanations are omitted.

[0044] The content of the repeating unit containing a ring structure in the acrylic resin is preferably 1 mol% to 50 mol%, more preferably 10 mol% to 40 mol%, and further preferably 20 mol% to 30 mol%. If the content is too low, Tg may be less than 110°C, and the heat resistance, solvent resistance, and surface hardness of the resulting protective layer may be insufficient. If the content is too high, moldability and transparency may be insufficient.

[0045] The acrylic resin may contain repeating units other than the alkyl (meth)acrylate unit and the repeating unit containing a ring structure. Examples of such repeating units include repeating units derived from vinyl monomers copolymerizable with the monomers constituting the above units (other vinyl monomer units). Examples of other vinyl monomers include acrylic acid, methacrylic acid, crotonic acid, 2-(hydroxymethyl)acrylic acid, 2-(hydroxyethyl)acrylic acid, acrylonitrile, methacrylonitrile, ethacrylonitrile, allyl glycidyl ether, maleic anhydride, itaconic anhydride, N-methylmaleimide, N-ethylmaleimide, N-cyclohexylmaleimide, aminoethyl acrylate, propylaminoethyl acrylate, dimethylaminoethyl methacrylate, ethylaminopropyl methacrylate, cyclohexylaminoethyl methacrylate, N-vinyldiethylamine, N-acetylvinylamine, allylamine, methallylamine, N-methylallylamine, 2-isopropenyl-oxazoline, 2-vinyl-oxazoline, 2-acroyl-oxazoline, N-phenylmaleimide, phenylaminoethyl methacrylate, styrene, α-methylstyrene, p-glycidylstyrene, p-aminostyrene, and 2-styryl-oxazoline. These may be used alone or in combination. The type, number, combination, content ratio, etc. of the other vinyl monomer units may be appropriately set depending on the purpose.

[0046] The weight average molecular weight of the acrylic resin is preferably 1000 to 2000000, more preferably 5000 to 1000000, further preferably 10000 to 500000, particularly preferably 50000 to 500000, and most preferably 60000 to 150000. The weight average molecular weight can be determined, for example, using a gel permeation chromatograph (GPC system, manufactured by Tosoh Corporation) in terms of polystyrene. Tetrahydrofuran can be used as the solvent.

[0047] The acrylic resin may be polymerized by any suitable polymerization method using a suitable combination of the above monomer units. Two or more acrylic resins having different monomer units may be blended.

[0048] In the embodiment of the present invention, the acrylic resin may be used in combination with other resins. That is, the monomer components constituting the acrylic resin may be copolymerized with the monomer components constituting the other resins, and the copolymer may be used to form the protective layer described below; a blend of the acrylic resin and the other resin may be used to form the protective layer. Examples of the other resins include thermoplastic resins such as styrene resins, polyethylene, polypropylene, polyamide, polyphenylene sulfide, polyether ether ketone, polyester, polysulfone, polyphenylene oxide, polyacetal, polyimide, and polyetherimide. The type and amount of the resin used in combination may be appropriately set depending on the purpose and the properties desired for the resulting film. For example, a styrene resin (preferably, an acrylonitrile-styrene copolymer) may be used in combination as a retardation control agent.

[0049] When an acrylic resin is used in combination with another resin, the content of the acrylic resin in the blend of the acrylic resin and the other resin is preferably 50% by weight to 100% by weight, more preferably 60% by weight to 100% by weight, further preferably 70% by weight to 100% by weight, and particularly preferably 80% by weight to 100% by weight. If the content is less than 50% by weight, the high heat resistance and high transparency inherent to the acrylic resin may not be fully reflected.

[0050] C-2. Composition and characteristics of protective layer As described above, the protective layer is composed of a solidified coating film of an organic solvent solution of an acrylic resin. Such a solidified coating film can be made much thinner than an extrusion-molded film. The thickness of the protective layer is 10 μm or less, preferably 7 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less, as described above. The lower limit of the thickness of the protective layer can be, for example, 1 μm. Although it is not theoretically clear, such a solidified coating film has the advantages of being smaller in shrinkage during film formation than a cured product of a thermosetting resin or an active energy ray curable resin (for example, an ultraviolet ray curable resin), and being free of residual monomers, etc., suppressing deterioration of the film itself, and suppressing adverse effects on the polarizing plate (polarizer) caused by residual monomers, etc. Furthermore, it has the advantage of being excellent in humidification durability because it has smaller hygroscopicity and moisture permeability than a solidified coating film of a water-based solution such as an aqueous solution or water dispersion. As a result, a polarizing plate (as a result, a polarizing plate with a retardation layer) that can maintain optical properties even under a heated and humidified environment and has excellent durability can be realized.

[0051] The Tg of the protective layer is as described in section A above.

[0052] The iodine adsorption amount of the protective layer is preferably 4.0% by weight or less, more preferably 3.0% by weight or less, even more preferably 2.0% by weight or less, particularly preferably 1.0% by weight or less, and particularly preferably 0.5% by weight or less. The smaller the iodine adsorption amount, the more preferable, and the lower limit thereof may be, for example, 0.1% by weight. If the iodine adsorption amount is within such a range, a polarizing plate (as a result, a polarizing plate with a retardation layer) having even better durability can be obtained. The iodine adsorption amount can be measured by the method described in the examples below.

[0053] The protective layer is preferably substantially optically isotropic. In this specification, "substantially optically isotropic" means that the in-plane retardation Re(550) is 0 nm to 10 nm, and the thickness direction retardation Rth(550) is -20 nm to +10 nm. The in-plane retardation Re(550) is more preferably 0 nm to 5 nm, further preferably 0 nm to 3 nm, and particularly preferably 0 nm to 2 nm. The thickness direction retardation Rth(550) is more preferably -5 nm to +5 nm, further preferably -3 nm to +3 nm, and particularly preferably -2 nm to +2 nm. If the Re(550) and Rth(550) of the protective layer are in such ranges, adverse effects on the display characteristics can be prevented when a retardation layer-attached polarizing plate including the protective layer is applied to an image display device.

[0054] The higher the light transmittance at 380 nm when the protective layer is 3 μm thick, the more preferable. Specifically, the light transmittance is preferably 85% or more, more preferably 88% or more, and even more preferably 90% or more. If the light transmittance is within this range, the desired transparency can be ensured. The light transmittance can be measured, for example, by a method conforming to ASTM-D-1003.

[0055] The lower the haze of the protective layer, the better. Specifically, the haze is preferably 5% or less, more preferably 3% or less, even more preferably 1.5% or less, and particularly preferably 1% or less. When the haze is 5% or less, the film can be given a good sense of clarity. Furthermore, even when a polarizing plate with a retardation layer is used on the viewing side of an image display device, the display contents can be viewed well.

[0056] The YI at a thickness of 3 μm of the protective layer is preferably 1.27 or less, more preferably 1.25 or less, even more preferably 1.23 or less, and particularly preferably 1.20 or less. If the YI exceeds 1.3, the optical transparency may be insufficient. The YI can be calculated by the following formula from the tristimulus values ​​(X, Y, Z) of the color obtained by measurement using a high-speed integrating sphere type spectral transmittance measuring device (product name DOT-3C: manufactured by Murakami Color Research Laboratory). YI = [(1.28X-1.06Z) / Y] x 100

[0057] The b value (a measure of hue according to the Hunter color system) of the protective layer at a thickness of 3 μm is preferably less than 1.5, more preferably 1.0 or less. If the b value is 1.5 or more, an undesired color tone may appear. The b value can be obtained, for example, by cutting a sample of the film constituting the protective layer into a 3 cm square, measuring the hue using a high-speed integrating sphere type spectral transmittance measuring device (product name DOT-3C: manufactured by Murakami Color Research Laboratory), and evaluating the hue according to the Hunter color system.

[0058] The protective layer (solidified coating film) may contain any suitable additive depending on the purpose. Specific examples of additives include ultraviolet absorbers; leveling agents; antioxidants such as hindered phenols, phosphorus, and sulfur; stabilizers such as light stabilizers, weather stabilizers, and heat stabilizers; reinforcing materials such as glass fibers and carbon fibers; near-infrared absorbers; flame retardants such as tris(dibromopropyl)phosphate, triallyl phosphate, and antimony oxide; antistatic agents such as anionic, cationic, and nonionic surfactants; colorants such as inorganic pigments, organic pigments, and dyes; organic or inorganic fillers; resin modifiers; organic and inorganic fillers; plasticizers; lubricants; antistatic agents; and flame retardants. The additives may be added during polymerization of the acrylic resin, or may be added to the solution during film formation. The type, number, combination, and amount of additives may be appropriately set depending on the purpose.

[0059] An easy-adhesion layer may be formed on the polarizer side of the protective layer. The easy-adhesion layer contains, for example, a water-based polyurethane and an oxazoline-based crosslinking agent. By forming such an easy-adhesion layer, the adhesion between the protective layer and the polarizer can be increased. In addition, a hard coat layer may be formed on the protective layer. The hard coat layer may be formed when the protective layer is used as a protective layer on the viewing side of the viewing-side polarizing plate. When both the easy-adhesion layer and the hard coat layer are formed, they may typically be formed on different sides of the protective layer.

[0060] D. Optical functional layer D-1. Optical functional layer as a protective layer When the optical functional layer 30 functions as a protective layer separate from the protective layer 20, the protective layer is preferably a thin protective layer having a thickness of 20 μm or less. The thickness of the protective layer is more preferably 18 μm or less, further preferably 15 μm or less, and particularly preferably 10 μm or less. The thickness of the protective layer may be, for example, 1 μm or more.

[0061] The protective layer (optical functional layer) may be made of a resin film or a solidified coating film. Examples of the resin constituting the resin film include cycloolefin resins and acrylic resins. The solidified coating film may be, for example, a solidified coating film of a solution of a specific acrylic resin in an organic solvent, or a solidified coating film of a solution of an epoxy resin in an organic solvent. When the protective layer is made of a solidified coating film, the thickness can be significantly thinner than that of a resin film.

[0062] When the protective layer, which is a solidified product of the coating film, is a solidified product of the coating film of an organic solvent solution of an epoxy resin, any suitable epoxy resin can be used as the epoxy resin. Preferably, an epoxy resin having a glass transition temperature of 90° C. or higher is used. As the epoxy resin, preferably, an epoxy resin having an aromatic ring in the molecular structure is used. By using an epoxy resin having an aromatic ring, an epoxy resin having a higher Tg can be obtained. Examples of the aromatic ring in the epoxy resin having an aromatic ring in the molecular structure include a benzene ring, a naphthalene ring, and a fluorene ring. Only one type of epoxy resin may be used, or two or more types may be used in combination. When two or more types of epoxy resins are used, an epoxy resin having an aromatic ring and an epoxy resin not having an aromatic ring may be used in combination.

[0063] The protective layer (optical functional layer) is typically disposed on the image display cell side when the polarizing plate is applied to an image display device. In one embodiment, the protective layer is preferably optically isotropic. In this specification, "optically isotropic" means that the in-plane retardation Re(550) is 0 nm to 10 nm, and the retardation Rth(550) in the thickness direction is -10 nm to +10 nm. In another embodiment, the protective layer may be a retardation layer having any appropriate retardation value. In this case, the in-plane retardation Re(550) of the protective layer (retardation layer) is, for example, 110 nm to 150 nm.

[0064] D-2. Optical functional layer that is a retardation layer having a circular polarization function or an elliptically polarizing function When the optical functional layer 30 is a retardation layer having a circular polarization function or an elliptical polarization function, the retardation layer may be a stretched film of a resin film or an orientation-solidified layer of a liquid crystal compound. Preferably, it is an orientation-solidified layer of a liquid crystal compound. By using a liquid crystal compound, the difference between nx and ny of the obtained retardation layer can be significantly larger than that of a non-liquid crystal material, so that the thickness of the retardation layer for obtaining a desired in-plane retardation can be significantly smaller than that of a stretched film. As a result, a further thinning of the retardation layer-attached polarizing plate can be realized. Furthermore, a retardation layer-attached polarizing plate having extremely excellent bending properties can be realized. The orientation-solidified layer of the liquid crystal compound will be described in detail below. The retardation layer composed of a stretched film of a resin film is described, for example, in JP-A-2017-54093 and JP-A-2018-60014. The descriptions in these publications are incorporated herein by reference.

[0065] In this specification, the term "alignment layer" refers to a layer in which liquid crystal compounds are aligned in a predetermined direction within the layer and the alignment state is fixed. The term "alignment layer" encompasses a concept of an alignment layer obtained by curing a liquid crystal monomer as described below. In this embodiment, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the first retardation layer (homogeneous alignment).

[0066] Examples of liquid crystal compounds include liquid crystal compounds whose liquid crystal phase is a nematic phase (nematic liquid crystals). Examples of such liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The mechanism by which liquid crystallinity of liquid crystal compounds is expressed may be either lyotropic or thermotropic. The liquid crystal polymers and liquid crystal monomers may be used alone or in combination.

[0067] When the liquid crystal compound is a liquid crystal monomer, the liquid crystal monomer is preferably a polymerizable monomer and a crosslinkable monomer. This is because the alignment state of the liquid crystal monomer can be fixed by polymerizing or crosslinking (i.e., curing) the liquid crystal monomer. After the liquid crystal monomer is aligned, for example, the liquid crystal monomers can be polymerized or crosslinked with each other, thereby fixing the alignment state. Here, a polymer is formed by polymerization, and a three-dimensional network structure is formed by crosslinking, but these are non-liquid crystals. Therefore, the formed first retardation layer does not undergo transition to a liquid crystal phase, a glass phase, or a crystalline phase due to temperature changes specific to liquid crystal compounds, for example. As a result, the first retardation layer becomes a retardation layer that is not affected by temperature changes and has extremely excellent stability.

[0068] The temperature range in which the liquid crystal monomer exhibits liquid crystallinity varies depending on the type of the liquid crystal monomer. Specifically, the temperature range is preferably 40°C to 120°C, more preferably 50°C to 100°C, and most preferably 60°C to 90°C.

[0069] Any suitable liquid crystal monomer can be used as the liquid crystal monomer. For example, the polymerizable mesogen compounds described in JP-A-2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445 can be used. Specific examples of such polymerizable mesogen compounds include BASF's product name LC242, Merck's product name E7, and Wacker-Chem's product name LC-Sillicon-CC3767. For example, nematic liquid crystal monomers are preferred as the liquid crystal monomer.

[0070] The alignment layer of the liquid crystal compound can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. In one embodiment, the substrate is any appropriate resin film, and the alignment layer formed on the substrate can be transferred to the surface of the polarizer 10.

[0071] As the above-mentioned alignment treatment, any suitable alignment treatment can be adopted. Specifically, mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment can be mentioned. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique deposition method and photoalignment treatment. As the treatment conditions of various alignment treatments, any suitable conditions can be adopted according to the purpose.

[0072] The alignment of the liquid crystal compound is performed by treating the liquid crystal compound at a temperature at which the liquid crystal compound exhibits a liquid crystal phase according to the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compound takes on a liquid crystal state and is aligned according to the alignment treatment direction of the substrate surface.

[0073] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is a polymerizable monomer or a crosslinkable monomer, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.

[0074] Specific examples of the liquid crystal compound and details of the method for forming the alignment solidified layer are described in JP-A-2006-163343, the disclosure of which is incorporated herein by reference.

[0075] Another example of the alignment solidified layer is a form in which the discotic liquid crystal compound is aligned in any one of vertical alignment, hybrid alignment, and tilt alignment. The discotic liquid crystal compound is typically aligned such that the disc surface of the discotic liquid crystal compound is substantially perpendicular to the film surface of the first retardation layer. The discotic liquid crystal compound being substantially perpendicular means that the average angle between the film surface and the disc surface of the discotic liquid crystal compound is preferably 70° to 90°, more preferably 80° to 90°, and even more preferably 85° to 90°. The discotic liquid crystal compound generally refers to a liquid crystal compound having a discotic molecular structure in which a cyclic mother nucleus such as benzene, 1,3,5-triazine, or calixarene is arranged at the center of the molecule, and linear alkyl groups, alkoxy groups, substituted benzoyloxy groups, or the like are radially substituted as side chains. Representative examples of discotic liquid crystals include benzene derivatives, triphenylene derivatives, truxene derivatives, and phthalocyanine derivatives described in the research report by C. Destrade et al., Mol. Cryst. Liq. Cryst., Vol. 71, p. 111 (1981); cyclohexane derivatives described in the research report by B. Kohne et al., Angew. Chem. Vol. 96, p. 70 (1984); and azacrown and phenylacetylene macrocycles described in the research report by JM Lehn et al., J. Chem. Soc. Chem. Commun., p. 1794 (1985) and the research report by J. Zhang et al., J. Am. Chem. Soc., Vol. 116, p. 2655 (1994). Further specific examples of discotic liquid crystal compounds include those described in JP-A-2006-133652, JP-A-2007-108732, and JP-A-2010-244038, the disclosures of which are incorporated herein by reference.

[0076] In one embodiment, the retardation layer (optical functional layer) 30 is a single layer of an alignment and solidification layer of a liquid crystal compound. When the retardation layer (hereinafter sometimes referred to as the first retardation layer as described above) is composed of a single layer of an alignment and solidification layer of a liquid crystal compound, its thickness is preferably 0.5 μm to 7 μm, more preferably 1 μm to 5 μm. By using a liquid crystal compound, an in-plane retardation equivalent to that of a resin film can be realized with a thickness much thinner than that of the resin film.

[0077] Typically, the first retardation layer exhibits a refractive index characteristic of nx > ny = nz. The first retardation layer is typically provided to impart antireflection characteristics to a polarizing plate, and when the first retardation layer is a single layer of an alignment and solidification layer, it can function as a λ / 4 plate. In this case, the in-plane retardation Re(550) of the first retardation layer is preferably 100 nm to 190 nm, more preferably 110 nm to 170 nm, and even more preferably 130 nm to 160 nm. Here, "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, within a range not impairing the effects of the present invention, ny > nz or ny < nz may occur.

[0078] The Nz coefficient of the first retardation layer is preferably 0.9 to 1.5, more preferably 0.9 to 1.3. By satisfying such a relationship, when the polarizing plate with a retardation layer is used in an image display device, an extremely excellent reflected hue can be achieved.

[0079] The first retardation layer may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or a flat wavelength dispersion characteristic in which the retardation value hardly changes depending on the wavelength of the measurement light. In one embodiment, the first retardation layer exhibits an inverse dispersion wavelength characteristic. In this case, Re(450) / Re(550) of the retardation layer is preferably 0.8 or more and less than 1, more preferably 0.8 or more and 0.95 or less. With such a configuration, extremely excellent antireflection characteristics can be realized.

[0080] The angle θ between the slow axis of the first retardation layer and the absorption axis of the polarizer 10 is preferably 40° to 50°, more preferably 42° to 48°, and further preferably about 45°. If the angle θ is in such a range, by using a λ / 4 plate as the first retardation layer as described above, a retardation layer-attached polarizing plate having very excellent circular polarization properties (resulting in very excellent antireflection properties) can be obtained.

[0081] In another embodiment, the first retardation layer may have a laminated structure of a first alignment solidified layer and a second alignment solidified layer. In this case, either the first alignment solidified layer or the second alignment solidified layer may function as a λ / 4 plate, and the other may function as a λ / 2 plate. Therefore, the thicknesses of the first alignment solidified layer and the second alignment solidified layer may be adjusted to obtain the desired in-plane retardation of the λ / 4 plate or the λ / 2 plate. For example, when the first alignment solidified layer functions as a λ / 2 plate and the second alignment solidified layer functions as a λ / 4 plate, the thickness of the first alignment solidified layer is, for example, 2.0 μm to 3.0 μm, and the thickness of the second alignment solidified layer is, for example, 1.0 μm to 2.0 μm. In this case, the in-plane retardation Re(550) of the first alignment solidified layer is preferably 200 nm to 300 nm, more preferably 230 nm to 290 nm, and further preferably 250 nm to 280 nm. The in-plane retardation Re(550) of the second alignment solidified layer is as described above for the single-layer alignment solidified layer. The angle between the slow axis of the first alignment solidified layer and the absorption axis of the polarizer is preferably 10° to 20°, more preferably 12° to 18°, and further preferably about 15°. The angle between the slow axis of the second alignment solidified layer and the absorption axis of the polarizer is preferably 70° to 80°, more preferably 72° to 78°, and further preferably about 75°. With such a configuration, it is possible to obtain characteristics close to ideal reverse wavelength dispersion characteristics, and as a result, it is possible to realize very excellent antireflection characteristics. The liquid crystal compounds constituting the first alignment solidified layer and the second alignment solidified layer, the methods for forming the first alignment solidified layer and the second alignment solidified layer, the optical characteristics, etc. are as described above for the single alignment solidified layer.

[0082] As described above, the second retardation layer may be a so-called positive C plate whose refractive index characteristic shows the relationship nz>nx=ny. By using a positive C plate as the second retardation layer, it is possible to effectively prevent reflection in an oblique direction, and the anti-reflection function can be made to have a wide viewing angle. The second retardation layer is preferably provided when the first retardation layer is a single layer of an alignment solidified layer. The thickness direction retardation Rth(550) of the second retardation layer is preferably -50 nm to -300 nm, more preferably -70 nm to -250 nm, further preferably -90 nm to -200 nm, and particularly preferably -100 nm to -180 nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. That is, the in-plane retardation Re(550) of the second retardation layer may be less than 10 nm.

[0083] The second retardation layer having a refractive index characteristic of nz>nx=ny may be formed of any appropriate material. The second retardation layer is preferably made of a film containing a liquid crystal material fixed in a homeotropic alignment. The liquid crystal material (liquid crystal compound) that can be homeotropically aligned may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of the liquid crystal compound and the method of forming the retardation layer include the liquid crystal compound and the method of forming the retardation layer described in

[0020] to

[0028] of JP-A-2002-333642. In this case, the thickness of the second retardation layer is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 8 μm, and even more preferably 0.5 μm to 5 μm.

[0084] E. Conductive layer or isotropic substrate with conductive layer The conductive layer can be formed by forming a metal oxide film on any suitable substrate by any suitable film forming method (e.g., vacuum deposition, sputtering, CVD, ion plating, spraying, etc.). Examples of metal oxides include indium oxide, tin oxide, zinc oxide, indium-tin composite oxide, tin-antimony composite oxide, zinc-aluminum composite oxide, and indium-zinc composite oxide. Among these, indium-tin composite oxide (ITO) is preferred.

[0085] When the conductive layer contains a metal oxide, the thickness of the conductive layer is preferably 50 nm or less, more preferably 35 nm or less. The lower limit of the thickness of the conductive layer is preferably 10 nm.

[0086] The conductive layer may be transferred from the substrate to the optical functional layer (or the second retardation layer, if present) and used alone as a constituent layer of the retardation layer-attached polarizing plate, or may be laminated with the substrate (substrate with conductive layer) to the optical functional layer (or the second retardation layer, if present). Preferably, the substrate is optically isotropic, and therefore the conductive layer can be used in the polarizing plate as an isotropic substrate with conductive layer.

[0087] Any suitable isotropic substrate may be used as the optically isotropic substrate (isotropic substrate). Examples of materials constituting the isotropic substrate include materials having a resin without a conjugated system, such as norbornene resins and olefin resins, as the main skeleton, and materials having a ring structure, such as a lactone ring or a glutarimide ring, in the main chain of an acrylic resin. By using such materials, when the isotropic substrate is formed, the appearance of retardation due to the orientation of molecular chains can be suppressed to a small value. The thickness of the isotropic substrate is preferably 50 μm or less, more preferably 35 μm or less. The thickness of the isotropic substrate is, for example, 20 μm or more.

[0088] The conductive layer and / or the conductive layer of the isotropic substrate with a conductive layer may be patterned as necessary. By patterning, a conductive portion and an insulating portion may be formed. As a result, an electrode may be formed. The electrode may function as a touch sensor electrode that senses contact with the touch panel. Any appropriate method may be adopted as the patterning method. Specific examples of the patterning method include a wet etching method and a screen printing method.

[0089] F. Manufacturing method of polarizing plate F-1. Manufacturing method of polarizer The method for producing a polarizer described in the above item B includes forming a polyvinyl alcohol-based resin layer (PVA-based resin layer) containing a halide and a polyvinyl alcohol-based resin (PVA-based resin) on one side of a long thermoplastic resin substrate to form a laminate, and subjecting the laminate to an auxiliary air-stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order, in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. The content of the halide in the PVA-based resin layer is preferably 5 parts by weight to 20 parts by weight with respect to 100 parts by weight of the PVA-based resin. The drying shrinkage treatment is preferably performed using a heating roll, and the temperature of the heating roll is preferably 60° C. to 120° C. According to such a production method, the above-mentioned polarizer can be obtained. In particular, a laminate containing a PVA-based resin layer containing a halide is prepared, the laminate is stretched in multiple stages including auxiliary air stretching and underwater stretching, and the stretched laminate is heated with a heating roll, whereby a polarizer having excellent optical properties (typically, single transmittance and polarization degree) and suppressed variation in optical properties can be obtained. Specifically, by using a heating roll in the drying shrinkage treatment step, the laminate can be uniformly shrunk throughout the laminate while being transported. This not only improves the optical properties of the obtained polarizer, but also allows a polarizer having excellent optical properties to be stably produced, and suppresses variation in the optical properties (particularly, single transmittance) of the polarizer. Hereinafter, the halide and the drying shrinkage treatment will be described. Details of the manufacturing method other than these are described in, for example, JP 2012-73580 A and JP 6470455 A. The entire disclosure of these publications is incorporated herein by reference.

[0090] F-1-1. Halides The PVA-based resin layer containing a halide and a PVA-based resin can be formed by applying a coating liquid containing a halide and a PVA-based resin onto a thermoplastic resin substrate and drying the coating film. The coating liquid is typically a solution in which the above-mentioned halide and the above-mentioned PVA-based resin are dissolved in a solvent. Examples of the solvent include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine. These may be used alone or in combination of two or more. Among these, water is preferred. The concentration of the PVA-based resin in the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film that is in close contact with the thermoplastic resin substrate can be formed.

[0091] Any suitable halide may be used as the halide. For example, iodide and sodium chloride may be used. For example, iodide may be potassium iodide, sodium iodide, and lithium iodide. Among these, potassium iodide is preferred.

[0092] The amount of the halide in the coating solution is preferably 5 to 20 parts by weight, more preferably 10 to 15 parts by weight, based on 100 parts by weight of the PVA resin. If the amount of the halide is too large, the halide may bleed out, causing the finally obtained polarizer to become cloudy.

[0093] Generally, the orientation of polyvinyl alcohol molecules in the PVA-based resin increases when the PVA-based resin layer is stretched, but when the stretched PVA-based resin layer is immersed in a liquid containing water, the orientation of the polyvinyl alcohol molecules may become disordered, and the orientation may decrease. In particular, when a laminate of a thermoplastic resin substrate and a PVA-based resin layer is stretched in boric acid water, the tendency of the orientation degree to decrease is significant when the laminate is stretched in boric acid water at a relatively high temperature to stabilize the stretching of the thermoplastic resin substrate. For example, the stretching of a PVA film alone in boric acid water is generally performed at 60°C, whereas the stretching of a laminate of A-PET (thermoplastic resin substrate) and a PVA-based resin layer is performed at a high temperature of about 70°C, and in this case, the orientation of PVA at the initial stage of stretching may decrease before it increases due to underwater stretching. In response to this, a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate is prepared, and the laminate is stretched at high temperature (auxiliary stretching) in air before being stretched in boric acid water, so that the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after the auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the orientation of the polyvinyl alcohol molecules can be prevented from being disturbed and the orientation can be prevented from being reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the polarizer obtained by immersing the laminate in a liquid through a process such as a dyeing process and an underwater stretching process.

[0094] F-1-2. Drying shrinkage treatment The drying shrinkage treatment may be performed by zone heating in which the entire zone is heated, or by heating the transport roll (using a so-called heating roll) (heat roll drying method). Preferably, both are used. By drying using a heating roll, it is possible to efficiently suppress the heat curl of the laminate and produce a polarizer with excellent appearance. Specifically, by drying the laminate in a state where it is aligned with the heating roll, it is possible to efficiently promote the crystallization of the thermoplastic resin substrate and increase the crystallinity, and even at a relatively low drying temperature, it is possible to satisfactorily increase the crystallinity of the thermoplastic resin substrate. As a result, the rigidity of the thermoplastic resin substrate increases and it becomes in a state where it can withstand the shrinkage of the PVA-based resin layer due to drying, and curling is suppressed. In addition, by using a heating roll, it is possible to dry the laminate while maintaining it in a flat state, so that it is possible to suppress not only curling but also the occurrence of wrinkles. At this time, the optical properties of the laminate can be improved by shrinking it in the width direction by the drying shrinkage treatment. This is because the orientation of the PVA and the PVA / iodine complex can be effectively increased. The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment is preferably 2% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%. By using a heating roll, the laminate can be continuously shrunk in the width direction while being transported, and high productivity can be achieved.

[0095] 3 is a schematic diagram showing an example of the drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by transport rolls R1 to R6 heated to a predetermined temperature and guide rolls G1 to G4. In the illustrated example, the transport rolls R1 to R6 are arranged so as to alternately and continuously heat the surface of the PVA resin layer and the surface of the thermoplastic resin substrate, but, for example, the transport rolls R1 to R6 may be arranged so as to continuously heat only one surface of the laminate 200 (for example, the thermoplastic resin substrate surface).

[0096] Drying conditions can be controlled by adjusting the heating temperature of the transport rolls (temperature of the heating rolls), the number of heating rolls, the contact time with the heating rolls, etc. The temperature of the heating rolls is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. The crystallinity of the thermoplastic resin can be favorably increased, curling can be favorably suppressed, and an optical laminate with extremely excellent durability can be produced. The temperature of the heating rolls can be measured by a contact thermometer. In the illustrated example, six transport rolls are provided, but there is no particular restriction as long as there are multiple transport rolls. The number of transport rolls is usually 2 to 40, preferably 4 to 30. The contact time (total contact time) between the laminate and the heating rolls is preferably 1 to 300 seconds, more preferably 1 to 20 seconds, and even more preferably 1 to 10 seconds.

[0097] The heating roll may be provided in a heating furnace (for example, an oven) or in a normal production line (under room temperature environment). It is preferably provided in a heating furnace equipped with a blowing means. By using drying with a heating roll in combination with hot air drying, it is possible to suppress abrupt temperature changes between the heating rolls, and it is possible to easily control shrinkage in the width direction. The hot air drying temperature is preferably 30°C to 100°C. The hot air drying time is preferably 1 second to 300 seconds. The hot air speed is preferably about 10 m / s to 30 m / s. The wind speed is the wind speed in the heating furnace, and can be measured by a mini-vane type digital anemometer.

[0098] Preferably, after the underwater stretching treatment and before the drying shrinkage treatment, a washing treatment is carried out. The washing treatment is typically carried out by immersing the PVA-based resin layer in an aqueous potassium iodide solution.

[0099] In this manner, a laminate of a thermoplastic resin substrate and a polarizer can be obtained.

[0100] F-2. Manufacturing method of polarizing plate A solution of an acrylic resin in an organic solvent is applied to the polarizer side surface of the laminate obtained in the above F-1 to form a coating film, and the coating film is solidified to form a protective layer.

[0101] Acrylic resins are as explained in Section C-1 above.

[0102] As the organic solvent, any suitable organic solvent capable of dissolving or uniformly dispersing the acrylic resin can be used. Specific examples of the organic solvent include ethyl acetate, toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclopentanone, and cyclohexanone.

[0103] The concentration of the acrylic resin in the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film that is in close contact with the polarizer can be formed.

[0104] The solution may be applied to any suitable substrate or to a polarizer. When the solution is applied to a substrate, the solidified coating film formed on the substrate is transferred to the polarizer. When the solution is applied to a polarizer, the coating film is dried (solidified) to form a protective layer directly on the polarizer. Preferably, the solution is applied to a polarizer, and a protective layer is directly formed on the polarizer. With such a configuration, the adhesive layer or pressure-sensitive adhesive layer required for transfer can be omitted, so that the retardation layer-attached polarizing plate can be made even thinner. Any suitable method can be adopted as a method for applying the solution. Specific examples include roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, and knife coating (comma coating, etc.).

[0105] A protective layer can be formed by drying (solidifying) the coating film of the solution. The drying temperature is preferably 100° C. or less, and more preferably 50° C. to 70° C. If the drying temperature is within this range, adverse effects on the polarizer can be prevented. The drying time can vary depending on the drying temperature. The drying time can be, for example, 1 minute to 10 minutes.

[0106] In this manner, the protective layer is formed, and as a result, a laminate of thermoplastic resin substrate / polarizer / protective layer can be obtained. By peeling off the thermoplastic resin substrate from this laminate, a polarizing plate having a polarizer 10 and a protective layer 20 as shown in FIG. 1 can be obtained. Alternatively, a resin film constituting another protective layer may be attached to the polarizer surface of the thermoplastic resin substrate / polarizer laminate, and then the thermoplastic resin substrate may be peeled off, and a protective layer may be formed on the peeled surface. In this case, a polarizing plate further having another protective layer can be obtained.

[0107] G. Method for manufacturing a polarizing plate with an optically functional layer The polarizing plate with an optical function layer can be produced by any suitable method. For example, a polarizing plate is produced by the method described in the above item F, and any suitable optical function layer is laminated or transferred onto the polarizer side of the polarizing plate. The optical function layer may be laminated onto the polarizer via any suitable adhesive layer, or may be formed directly on the polarizer. EXAMPLES

[0108] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0109] (1) Glass transition temperature Tg The materials constituting the protective layer used in the examples and comparative examples were dissolved in a predetermined solvent, and the solution was applied to a substrate (PET film) with an applicator and dried at 60°C to form a coating film (thickness 40 μm). The resulting coating film was peeled off from the substrate and cut into strips to prepare a measurement sample. The measurement sample was subjected to DMA measurement to measure Tg. The measurement device and measurement conditions were as follows. (Measuring Equipment) "DMS6100" manufactured by SII Nanotechnology (Measurement conditions) Measurement temperature range: -80℃~150℃ ·Temperature increase / decrease rate: 2℃ / min Measurement sample width: 10mm Chuck distance: 20mm ·Measurement frequency: 1Hz ·Distortion amplitude: 10μm Measurement atmosphere: N2 (250mL / min) (2) Iodine adsorption amount The materials constituting the protective layer used in the examples and comparative examples were dissolved in a predetermined solvent, and the solution was applied to a substrate (PET film) with an applicator and dried at 60°C to form a coating film (thickness 40 μm). The obtained coating film was peeled off from the substrate and cut into a 1 cm x 1 cm (1 cm 2 ) was cut out as a measurement sample. The measurement sample was subjected to the combustion IC method to quantitatively analyze the amount of iodine in the sample. Specifically, the measurement sample was collected in a headspace vial (20 mL capacity) and weighed. Next, a vial (2 mL capacity) containing 1 mL of iodine aqueous solution (iodine concentration 1 wt%, potassium iodide concentration 7 wt%) was placed in this headspace vial and sealed. After that, this headspace vial was heated at 65°C for 6 hours in a dryer, and the heated sample was collected in a ceramic port and burned using an automatic combustion device. The generated gas was collected in an absorption liquid and then quantitatively analyzed to determine the weight percentage of adsorbed iodine. The following equipment was used. Automatic sample combustion device: Mitsubishi Chemical Analytical Co., Ltd., "AQF-2100H" IC (anion): Thermo Fisher Scientific, "ICS-3000" (3) Single unit transmittance and polarization degree A test piece (50 mm x 50 mm) was cut out from the polarizing plate with optical function layer obtained in the examples and comparative examples, with two sides perpendicular to the absorption axis direction of the polarizer and facing the absorption axis direction. The test piece was attached to an alkali-free glass plate with an adhesive so that the protective layer was on the outside, and the single transmittance (Ts), parallel transmittance (Tp), and crossed transmittance (Tc) of the test sample were measured using an ultraviolet-visible spectrophotometer (manufactured by JASCO Corporation, product name "V7100"), and the polarization degree (P) was calculated by the following formula. At this time, the measurement light was incident from the protective layer side. Polarization degree (P)(%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100 The above Ts, Tp and Tc are Y values ​​measured with a 2-degree visual field (C light source) according to JIS Z 8701 and corrected for visibility. Ts and P are substantially the characteristics of the polarizer. Next, the polarizing plate with the optical functional layer was left in an oven at 85° C. and 85% RH for 48 hours to heat and humidify it (heating test), and the single unit transmittance Ts0 before the heating test and the single unit transmittance Ts after the heating test were measured. 48 From this, the amount of change in single-piece transmittance ΔTs was calculated using the following formula. ΔTs(%)=Ts 48 -Ts0 Similarly, the polarization degree P0 before the heating test and the polarization degree P after the heating test 48 From the above, the change in the degree of polarization ΔP was calculated using the following formula. ΔP(%)=P 48 -P0 For the heating test, a test piece (50 mm x 50 mm) was cut out from the polarizing plate with an optical functional layer obtained in the examples and comparative examples, with two sides perpendicular to the absorption axis direction of the polarizer and facing the absorption axis direction, respectively, and the test piece was attached to an alkali-free glass plate with an adhesive so that the protective layer was on the outside to prepare a test sample. The obtained ΔTs and ΔP results were evaluated according to the following criteria. Good: ΔTs: less than 3.0%, ΔP: -0.1% to 0% Acceptable: ΔTs: 3.0% or more and less than 5.0%, ΔP: -1.0% or more and less than -0.1% Defective: ΔTs: 5% or more, ΔP: less than -1.0%, or overall discoloration (4) Bending test The polarizing plates with optical functional layers obtained in the examples and comparative examples were cut into a size of 30 mm (in a direction perpendicular to the absorption axis direction of the polarizer) x 120 mm (in the absorption axis direction) to be used as measurement samples. A continuous bending test was performed on these measurement samples using a continuous bending tester in a no-load U-shaped stretching mode (manufactured by Yuasa System Co., Ltd., product name "DLDMLH-FS"). The bending speed was 60 rpm, the bending amplitude was 20 mm, the bending curvature radius was 0.5 mm, and the number of bending times was 50,000. The bending was performed by sliding the gripping part while gripping the longitudinal end of the measurement sample so that the optical functional layer or the retardation layer of the measurement sample was on the inside. Evaluation was performed according to the following criteria. Good: No cracks after 50,000 bending cycles Failed: Cracks and / or creases in any of the components after less than 50,000 folds When cracks occurred in the measurement sample, the cracks were along a direction perpendicular to the absorption axis (the width direction of the measurement sample).

[0110] <Example 1> 1. Preparation of a laminate of polarizer / resin substrate The resin substrate was a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a water absorption rate of 0.75% and a Tg of about 75° C. One side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Mitsubishi Chemical Corporation, product name "GOHSEFFIMER Z410") in a ratio of 9:1. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched at its free end to 2.4 times its original size in the machine direction (longitudinal direction) between rolls with different peripheral speeds in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizer would be 41.5%±0.1% (dyeing process). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4.0% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, while drying in an oven maintained at 90°C, the laminate was brought into contact with a SUS heated roll whose surface temperature was maintained at 75°C for approximately 2 seconds (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 5.2%. In this way, a 5 μm-thick polarizer was formed on the resin substrate, and a laminate of the polarizer and the resin substrate was produced. The polarizer had a single transmittance (initial single transmittance) Ts0 of 41.2% and a polarization degree (initial polarization degree) P0 of 99.996%.

[0111] 2. Preparation of the first alignment layer and the second alignment layer constituting the retardation layer A liquid crystal composition (coating liquid) was prepared by dissolving 10 g of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: product name "Paliocolor LC242", represented by the following formula) and 3 g of a photopolymerization initiator for the polymerizable liquid crystal compound (manufactured by BASF: product name "Irgacure 907") in 40 g of toluene. [ka] The surface of a polyethylene terephthalate (PET) film (thickness 38 μm) was rubbed with a rubbing cloth and subjected to an alignment treatment. The direction of the alignment treatment was set to be 15° from the viewing side with respect to the direction of the absorption axis of the polarizer when it was attached to the polarizing plate. The above liquid crystal coating liquid was applied to this alignment-treated surface with a bar coater, and the liquid crystal compound was aligned by heating and drying at 90°C for 2 minutes. The liquid crystal layer thus formed was then irradiated with 100 mJ / cm using a metal halide lamp. 2 The liquid crystal layer was cured by irradiating the liquid crystal with light, forming a liquid crystal alignment solidified layer A on the PET film. The liquid crystal alignment solidified layer A had a thickness of 2.5 μm and an in-plane retardation Re(550) of 270 nm. Furthermore, the liquid crystal alignment solidified layer A exhibited a refractive index characteristic of nx>ny=nz. A liquid crystal alignment layer B was formed on a PET film in the same manner as above, except that the coating thickness was changed and the orientation treatment direction was set to a 75° direction relative to the absorption axis direction of the polarizer when viewed from the viewing side. The liquid crystal alignment layer B had a thickness of 1.3 μm and an in-plane retardation Re(550) of 140 nm. Furthermore, the liquid crystal alignment layer B showed a refractive index characteristic of nx>ny=nz.

[0112] 3. Preparation of polarizing plate with retardation layer The liquid crystal alignment solidified layer A and the liquid crystal alignment solidified layer B obtained in the above 2 were transferred in this order onto the polarizer surface of the laminate of the polarizer / resin substrate obtained in the above 1. At this time, the transfer (lamination) was performed so that the angle between the absorption axis of the polarizer and the slow axis of the alignment solidified layer A was 15°, and the angle between the absorption axis of the polarizer and the slow axis of the alignment solidified layer B was 75°. The transfer (lamination) was performed via an ultraviolet-curable adhesive (thickness 1.0 μm). Next, a substrate with adhesive was laminated to the surface of the alignment solidified layer B for reinforcement. Next, the resin substrate was peeled off to obtain a retardation layer-attached polarizing plate having a configuration of polarizer / adhesive layer / retardation layer (first alignment solidified layer / adhesive layer / second alignment solidified layer) / substrate with adhesive.

[0113] 4. Formation of an easy-to-adhere layer A polyurethane-based water-dispersed resin (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name: Superflex SF210) was applied to a thickness of 0.1 μm on the polarizer surface of the obtained polarizing plate with a retardation layer to form an easy-adhesion layer.

[0114] 5. Fabrication of Protective Layer 20 parts by weight of an acrylic resin (Kusumoto Chemicals, product name: B-728) which is 100% polymethyl methacrylate was dissolved in 80 parts by weight of methyl ethyl ketone to obtain an acrylic resin solution (20%). This acrylic resin solution was applied to the polarizer surface of the polarizing plate obtained above using a wire bar, and the coating film was dried at 60°C for 5 minutes to form a protective layer constituted as a solidified coating film. The protective layer had a thickness of 3 μm, a Tg of 116°C, and an iodine adsorption amount of 0.34 wt%. In this way, a retardation layer-attached polarizing plate having a configuration of protective layer (solidified coating film) / polarizer / retardation layer was obtained. The obtained retardation layer-attached polarizing plate was subjected to the above evaluation.

[0115] [Example 2] A polarizing plate with a retardation layer was obtained in the same manner as in Example 1, except that the thickness of the protective layer was set to 2 μm, and a hard coat layer (thickness 3 μm) was further formed on the surface of the protective layer opposite to the easy-adhesion layer. The hard coat layer was made by mixing 70 parts by weight of dimethylol-tricyclodecane diacrylate (manufactured by Kyoeisha Chemical, product name: Light Acrylate DCP-A), 20 parts by weight of isobornyl acrylate (manufactured by Kyoeisha Chemical, product name: Light Acrylate IB-XA), 10 parts by weight of 1,9-nonanediol diacrylate (manufactured by Kyoeisha Chemical, product name: Light Acrylate 1.9NA-A), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, product name: Irgacure 907) using a suitable solvent. The obtained coating liquid was applied on the protective layer surface so that the thickness would be 3 μm after curing, and then the solvent was dried, and a high-pressure mercury lamp was used to apply an integrated light amount of 300 mJ / cm. 2 The retardation layer-attached polarizing plate thus obtained was subjected to the above-mentioned evaluation.

[0116] [Example 3] A polarizing plate (protective layer (solidified layer of coating film) / polarizer / protective layer (COP film)) was produced in the same manner as in Example 1, except that a cycloolefin resin (COP) film (thickness 13 μm) was used as another protective layer instead of a retardation layer as an optical functional layer. The total thickness of the polarizing plate was 22 μm. The obtained polarizing plate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0117] [Example 4] A polarizing plate (protective layer (solidified layer of coating film) / polarizer) was produced in the same manner as in Example 1, except that the protective layer-forming composition was applied to the polarizer of the polarizer / resin substrate laminate obtained in 1 above. The total thickness of the polarizing plate was 8 μm. The obtained polarizing plate was subjected to the same evaluations as in Example 1. The results are shown in Table 1.

[0118] [Example 5] Except for using an acrylic resin (30 mol % lactone ring unit) that is polymethyl methacrylate having a lactone ring unit instead of the acrylic resin that is 100% polymethyl methacrylate, a retardation layer-attached polarizing plate having a configuration of protective layer (solidified coating film) / polarizer / retardation layer was obtained in the same manner as in Example 1. The obtained retardation layer-attached polarizing plate was subjected to the above-mentioned evaluation.

[0119] [Example 6] A polarizing plate with a retardation layer having a structure of protective layer (solidified coating film) / polarizer / retardation layer was obtained in the same manner as in Example 1, except that an acrylic resin that is 100% polymethyl methacrylate was replaced with an acrylic resin that is polymethyl methacrylate having a glutarimide ring unit (4 mol% glutarimide ring unit). The obtained polarizing plate with a retardation layer was subjected to the above evaluation.

[0120] [Example 7] Except for using an acrylic resin that is a copolymer of methyl methacrylate / butyl methacrylate (molar ratio 80 / 20) instead of the acrylic resin that is 100% polymethyl methacrylate, a polarizing plate with a retardation layer having a structure of protective layer (solidified coating film) / polarizer / retardation layer was obtained in the same manner as in Example 1. The obtained polarizing plate with a retardation layer was subjected to the above evaluation.

[0121] Comparative Example 1 A polarizing plate with a retardation layer having a structure of a protective layer (solidified coating film) / polarizer / retardation layer was obtained in the same manner as in Example 1, except that an acrylic resin (manufactured by Kusumoto Chemical Industries, Ltd., product name "B-722"), which is a copolymer of methyl methacrylate / ethyl acrylate (molar ratio 55 / 45) was used instead of the acrylic resin that is 100% polymethyl methacrylate. When the obtained polarizing plate with a retardation layer was placed in a heated and humidified environment, discoloration occurred, so the single transmittance and polarization degree were not evaluated.

[0122] Comparative Example 2 A polarizing plate with a retardation layer having a structure of a protective layer (solidified coating film) / polarizer / retardation layer was obtained in the same manner as in Example 1, except that an acrylic resin (manufactured by Kusumoto Chemical Industries, Ltd., product name "B-734"), which is a copolymer of methyl methacrylate / butyl methacrylate (molar ratio 35 / 65) was used instead of the acrylic resin that is 100% polymethyl methacrylate. When the obtained polarizing plate with a retardation layer was placed in a heated and humidified environment, discoloration occurred, so the single transmittance and polarization degree were not evaluated.

[0123] Comparative Example 3 A protective layer (cured product) was formed in the same manner as in Example 1, except that no easy-adhesion layer was formed (i.e., the protective layer was formed directly on the polarizer) and that the protective layer was formed using an ultraviolet-curable acrylic resin (manufactured by Kyoeisha Chemical, product name "Light Acrylate HPP-A", hydroxypivalic acid neopentyl glycol acrylic acid adduct), to obtain a polarizing plate with a retardation layer. Specifically, a composition containing 97% by weight of the acrylic resin and 3% by weight of a photopolymerization initiator (Irgacure 907, manufactured by BASF) was applied onto the polarizer, and an accumulated light amount of 300 mJ / cm was obtained using a high-pressure mercury lamp under a nitrogen atmosphere. 2 The coating was irradiated with ultraviolet light at a temperature of 150° C. to form a hardened layer (protective layer).

[0124] Comparative Example 4 A protective layer (cured product) was formed in the same manner as in Example 1, except that no easy-adhesion layer was formed (i.e., the protective layer was formed directly on the polarizer) and that the protective layer was formed using an ultraviolet-curable epoxy resin (manufactured by Daicel Corporation, product name "Celloxide 2021P"), and a polarizing plate with a retardation layer was obtained. Specifically, a composition containing 95% by weight of the epoxy resin and 5% by weight of a photopolymerization initiator (CPI-100P, manufactured by San-Apro Co., Ltd.) was applied onto the polarizer, and a high-pressure mercury lamp was used in an air atmosphere to obtain an accumulated light amount of 500 mJ / cm. 2 The coating was irradiated with ultraviolet light at a temperature of 150° C. to form a hardened layer (protective layer).

[0125] Comparative Example 5 A protective layer (solidified coating film) was formed in the same manner as in Example 1, except that no easy-adhesion layer was formed (i.e., a protective layer was formed directly on the polarizer) and a water-based polyester resin (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "Polyester WR905") was used, to obtain a polarizing plate with a retardation layer. When the obtained polarizing plate with a retardation layer was placed in a heated and humidified environment, discoloration occurred, so the single transmittance and polarization degree were not evaluated.

[0126] Comparative Example 6 A protective layer (solidified coating film) was formed in the same manner as in Example 1, except that no easy-adhesion layer was formed (i.e., the protective layer was formed directly on the polarizer) and a water-based polyurethane resin (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "Superflex SF210") was used, to obtain a polarizing plate with a retardation layer. When the obtained polarizing plate with a retardation layer was placed in a heated and humidified environment, discoloration occurred, so the single transmittance and polarization degree were not evaluated.

[0127] Comparative Example 7 An acrylic film (refractive index: 1.50, thickness: 20 μm) with one side treated for easy adhesion without forming an easy-adhesion layer was directly attached to the polarizer surface via an ultraviolet-curing adhesive. Specifically, the curing adhesive was applied so that the total thickness was 1.0 μm, and the films were attached using a rolling machine. Then, the adhesive was cured by irradiating it with UV light from the acrylic film side. A polarizing plate with a retardation layer was obtained in the same manner as in Example 1, except that a protective layer was laminated in this manner.

[0128] Comparative Example 8 A polarizing plate with a retardation layer was produced in the same manner as in Comparative Example 7, except that the thickness of the acrylic film was changed to 40 μm. The thickness of the polarizing plate was 51 μm. The obtained polarizing plate with a retardation layer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0129] [Table 1]

[0130] <Evaluation> As is clear from Table 1, the polarizing plates obtained in the examples were very thin, but the deterioration of optical properties was suppressed even in a heated and humidified environment, and the polarizing plates had excellent durability. Furthermore, the polarizing plates had excellent flexibility, and were able to achieve both excellent durability and excellent flexibility. [Industrial Applicability]

[0131] The polarizing plate of the present invention is preferably used in image display devices. Examples of image display devices include portable devices such as personal digital assistants (PDAs), smartphones, mobile phones, watches, digital cameras, and portable game machines; office automation devices such as personal computer monitors, notebook computers, and copy machines; home electronic devices such as video cameras, televisions, and microwave ovens; in-vehicle devices such as back monitors, monitors for car navigation systems, and car audio; exhibition devices such as digital signage and information monitors for commercial stores; security devices such as surveillance monitors; and nursing and medical devices such as nursing monitors and medical monitors. [Explanation of symbols]

[0132] 10 Polarizer 20 protective layer 30 Retardation layer 100 Polarizing Plate 110 Polarizing plate with optical functional layer

Claims

1. a polarizer and a protective layer disposed on one side of the polarizer; the protective layer is formed of a solidified coating film of a solution of a thermoplastic acrylic resin in an organic solvent, and the protective layer has a glass transition temperature of 95° C. or higher; The thickness of the protective layer is 3 μm or less, The polarizing plate with an optical functional layer includes a polarizing plate having a total thickness of 20 μm or less, and an optical functional layer disposed on the polarizer opposite to the protective layer, and the total thickness of the polarizing plate with an optical functional layer is 25 μm or less.

2. 2. The polarizing plate with an optical functional layer according to claim 1, wherein the polarizer has a thickness of 10 μm or less.

3. 3. The polarizing plate with an optical functional layer according to claim 1, wherein the thermoplastic acrylic resin has at least one selected from the group consisting of a lactone ring unit, a glutaric anhydride unit, a glutarimide unit, a maleic anhydride unit and a maleimide unit.

4. The polarizing plate with an optical functional layer according to claim 1 , wherein the optical functional layer functions as a protective layer separate from the protective layer.

5. 4. The polarizing plate with an optical function layer according to claim 1, wherein the optical function layer is a retardation layer having a circular polarization function or an elliptically polarizing function.

Citation Information

Patent Citations

  • Polarizer protection film and polarizing plate

    JP2015210474A

  • Polarizing plate and image display device containing the same

    JP2016540260A

  • Polarizing plate and liquid crystal display device

    JP2017120276A