Electrolyte for rechargeable lithium battery and rechargeable lithium battery the same
The electrolyte composition for lithium secondary batteries, featuring a cyano-functional additive, stabilizes PF6- and forms protective films to address oxidation and gas issues, enhancing battery stability and lifespan under high voltage and temperature conditions.
Patent Information
- Application Number
- KR1020220107153
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-08-25
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-08-25
AI Technical Summary
Lithium secondary batteries face issues with electrolyte oxidation at high voltages, leading to performance degradation, safety concerns, and shortened lifespan due to decomposition products like HF and PF5, which are exacerbated by high temperatures.
An electrolyte composition comprising a non-aqueous organic solvent, lithium salt, and an additive consisting of a first, second, and third compound, where the first compound has a cyano functional group to stabilize PF6-, the second compound forms a film on the anode surface to suppress oxidation, and the third compound controls gas generation, enhancing high-temperature stability and safety.
The electrolyte composition improves lithium secondary battery lifespan and safety by reducing resistance and gas generation during high-temperature storage under high voltage conditions.
Smart Images

Figure 112022089486788-PAT00011_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an electrolyte for a lithium secondary battery and a lithium secondary battery containing the same. Background Technology
[0002] Lithium secondary batteries are rechargeable and have an energy density more than three times higher per unit weight than conventional lead-acid batteries, nickel-cadmium batteries, nickel-hydrogen batteries, and nickel-zinc batteries, and can be fast-charged. As a result, they are being commercialized for laptops, mobile phones, power tools, and electric bicycles, and research and development to further improve energy density is actively underway.
[0003] In particular, as IT devices are becoming increasingly high-performance, there is a demand for high-capacity batteries. While energy density can be increased by achieving high capacity through the expansion of the voltage range, there is a problem in that the electrolyte oxidizes in the high-voltage range, degrading the performance of the anode.
[0004] For example, LiPF6, which is most widely used as a lithium salt in electrolytes, has the problem of reacting with the electrolyte solvent to accelerate solvent depletion and generate a large amount of gas. As LiPF6 decomposes, it produces decomposition products such as HF and PF5, which cause electrolyte depletion in the battery and result in high-temperature performance degradation and vulnerability to safety issues.
[0005] Decomposition products of the electrolyte are deposited as a film on the electrode surface, increasing the internal resistance of the battery and ultimately causing performance degradation and a shortened lifespan. In particular, at high temperatures where reaction rates increase, these side reactions are further accelerated, and the gaseous components generated by these side reactions rapidly increase the internal pressure of the battery, which can have a fatal adverse effect on battery stability.
[0006] It is known that electrolyte oxidation in the high-voltage region is significantly accelerated and greatly increases electrode resistance during long-term charge-discharge processes.
[0007] Accordingly, there is a demand for electrolytes applicable even under high voltage and high temperature conditions. The problem to be solved
[0008] One embodiment provides an electrolyte for a lithium secondary battery comprising an additive having a functional group capable of removing decomposition products within the electrolyte.
[0009] Another embodiment provides a lithium secondary battery with improved high-temperature storage characteristics, lifespan characteristics, and safety under high voltage conditions by applying the above electrolyte. means of solving the problem
[0010] One embodiment of the present invention provides an electrolyte for a lithium secondary battery comprising a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive is a composition comprising a first compound, a second compound, and a third compound, wherein the first compound is represented by the following chemical formula 1, the second compound is represented by the following chemical formula 2, and the third compound is a cyclic carbonate compound.
[0011] [Chemical Formula 1]
[0012]
[0013] In the above chemical formula 1,
[0014] L 1 and L 2 Each is an independently substituted or unsubstituted C1 to C10 alkylene group, and
[0015] R 1 to R 4 Each is independently a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C2 to C10 alkenyl group, a substituted or unsubstituted C2 to C10 alkynyl group, a substituted or unsubstituted C3 to C10 cycloalkyl group, a substituted or unsubstituted C3 to C10 cycloalkenyl group, a substituted or unsubstituted C3 to C10 cycloalkinyl group, or a substituted or unsubstituted C6 to C20 aryl group;
[0016] [Chemical Formula 2]
[0017]
[0018] In the above chemical formula 2,
[0019] R 5 to R 14 Each is independently hydrogen, a halogen group, a cyano group, a substituted or unsubstituted C1 to C5 alkyl group, a substituted or unsubstituted C1 to C5 alkoxy group, a substituted or unsubstituted C6 to C12 aryl group, or a combination thereof, and
[0020] n1 to n3 are each independently one of integers from 0 to 20, and
[0021] n1+n2+n3 ≥ 1, and
[0022] m1 to m3 are each independently one of the integers 0 or 1.
[0023] L of the above chemical formula 1 1 and L 2 Each may be an independently substituted or unsubstituted C3 to C10 alkylene group.
[0024] R of the above chemical formula 1 1 to R 4 Each may be an independently substituted or unsubstituted C1 to C10 alkyl group.
[0025] The first compound above may be 1,3-bis(3-cyanopropyl)tetramethyldisiloxane.
[0026] n1 to n3 of the above chemical formula 2 may be different integers.
[0027] The second compound above may be selected from 1,3,5-hexanetricarbonitrile, 1,3,6-hexanetricarbonitrile, and 1,2,3-Tris(2-cyanoethoxy)propane.
[0028] The above third compound can be represented by the following chemical formula 3.
[0029] [Chemical Formula 3]
[0030]
[0031] In the above chemical formula 3,
[0032] R 15 and R 16 Each is independently a hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2), or a fluorine-substituted C1 to C5 alkyl group, and
[0033] The above R 15 and R 16 At least one of them is a halogen group, a cyano group (CN), a nitro group (NO2), or a fluorine-substituted C1 to C5 alkyl group.
[0034] The third compound may be fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, or cyanoethylene carbonate.
[0035] The first compound may be included in an amount of 0.5 to 3.0 parts by weight per 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0036] The above second compound may be included in an amount of 1.0 to 5.0 parts by weight per 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0037] The above third compound may be included in an amount of 3.0 to 10 parts by weight per 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0038] The total weight of the first compound and the second compound may be included in an amount of 2.0 to 6.0 parts by weight per 100 parts by weight of the electrolyte for a lithium secondary battery.
[0039] The first compound and the second compound may be mixed in a weight ratio of 1:0.5 to 1:5.
[0040] The above composition may be included in an amount of 5.0 to 15 parts by weight per 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0041] Another embodiment of the present invention provides a lithium secondary battery comprising a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, and an electrolyte for a lithium secondary battery as described above.
[0042] The above-mentioned cathode active material may be a carbon-based cathode active material.
[0043] The above lithium secondary battery can operate at a high voltage of 4.5 V or higher. Effects of the invention
[0044] It is possible to realize a lithium secondary battery with improved lifespan characteristics and safety by suppressing the increase in resistance of the battery during high-temperature storage under high voltage. Brief explanation of the drawing
[0045] FIG. 1 is a schematic diagram illustrating a lithium secondary battery according to one embodiment of the present invention. Figure 2 is an EDS mapping image of the cathode surface after charging and discharging of a full cell. Figure 3 shows PO2F2 after high-temperature storage of a full cell. - It shows the content of and HF. Figure 4 is a graph showing the discharge capacity according to the progress of the high-temperature charge / discharge cycle for a lithium secondary battery. Figure 5 shows the results of measuring Coulomb efficiency according to the high-temperature charge-discharge cycle of a lithium secondary battery. Specific details for implementing the invention
[0046] Hereinafter, a lithium secondary battery according to one embodiment of the present invention will be described in detail with reference to the attached drawings. However, this is presented as an example and the present invention is not limited thereby, and the present invention is defined only by the scope of the claims set forth below.
[0047] In this specification, "substitution" means that, unless otherwise defined, at least one hydrogen of a substituent or compound is substituted with a deuterium, a halogen group, a hydroxyl group, an amino group, a substituted or unsubstituted C1 to C30 amine group, a nitro group, a substituted or unsubstituted C1 to C40 silyl group, a C1 to C30 alkyl group, a C1 to C10 alkylsilyl group, a C6 to C30 arylsilyl group, a C3 to C30 cycloalkyl group, a C3 to C30 heterocycloalkyl group, a C6 to C30 aryl group, a C2 to C30 heteroaryl group, a C1 to C20 alkoxy group, a C1 to C10 fluoroalkyl group, a cyano group, or a combination thereof.
[0048] In one example of the present invention, "substitution" means that at least one hydrogen in a substituent or compound is substituted with deuterium, a halogen group, a C1 to C30 alkyl group, a C1 to C10 alkylsilyl group, a C6 to C30 arylsilyl group, a C3 to C30 cycloalkyl group, a C3 to C30 heterocycloalkyl group, a C6 to C30 aryl group, a C2 to C30 heteroaryl group, a C1 to C10 fluoroalkyl group, or a cyano group. Furthermore, in a specific example of the present invention, "substitution" means that at least one hydrogen in a substituent or compound is substituted with deuterium, a halogen group, a C1 to C20 alkyl group, a C6 to C30 aryl group, a C1 to C10 fluoroalkyl group, or a cyano group. In addition, in a specific example of the present invention, "substitution" means that at least one hydrogen in the substituent or compound is substituted with deuterium, a halogen group, a C1 to C5 alkyl group, a C6 to C18 aryl group, a C1 to C5 fluoroalkyl group, or a cyano group. In addition, in a specific example of the present invention, "substitution" means that at least one hydrogen in the substituent or compound is substituted with deuterium, a cyano group, a halogen group, a methyl group, an ethyl group, a propyl group, a butyl group, a phenyl group, a biphenyl group, a terphenyl group, a trifluoromethyl group, or a naphthyl group.
[0049] In this specification, "aryl group" is a collective concept for a group having one or more hydrocarbon aromatic moietys, including a form in which all elements of the hydrocarbon aromatic moiety have p-orbitals and these p-orbitals form a conjugation, such as a phenyl group, a naphthyl group, etc., and a form in which two or more hydrocarbon aromatic moietys are connected through a sigma bond, such as a biphenyl group, a terphenyl group, a quarterphenyl group, etc., and a non-aromatic fused ring in which two or more hydrocarbon aromatic moietys are directly or indirectly fused, such as a fluorenyl group, etc.
[0050] Aryl groups include monocyclic, polycyclic, or fused-ring polycyclic (i.e., rings that share adjacent pairs of carbon atoms) functional groups.
[0051] More specifically, the substituted or unsubstituted C6 to C30 aryl group may be a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthrenyl group, a substituted or unsubstituted naphthacenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted p-terphenyl group, a substituted or unsubstituted m-terphenyl group, a substituted or unsubstituted o-terphenyl group, a substituted or unsubstituted crisenyl group, a substituted or unsubstituted triphenylene group, a substituted or unsubstituted perylenyl group, a substituted or unsubstituted fluorenyl group, or a combination thereof, but is not limited thereto.
[0052] Lithium secondary batteries can be classified into lithium-ion batteries, lithium-ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used; classified into cylindrical, prismatic, coin, and pouch types depending on their shape; and divided into bulk and thin-film types depending on their size. Since the structures and manufacturing methods of these batteries are widely known in this field, a detailed description is omitted.
[0053] FIG. 1 shows an exploded perspective view of a lithium secondary battery according to one embodiment of the present invention. Although the lithium secondary battery according to one embodiment is described as a pouch-type battery, the present invention is not limited thereto and can be applied to batteries of various shapes, such as cylindrical and prismatic types.
[0054] Referring to FIG. 1, a lithium secondary pouch battery (100) according to one embodiment may include an electrode assembly (110) wound with a separator (30) interposed between a positive electrode (10) and a negative electrode (20), a case (120) in which the electrode assembly (110) is housed, and an electrode tab (130) that serves as an electrical path for inducing current formed in the electrode assembly (110) to the outside. Two sides of the case (120) are sealed by overlapping the sides facing each other. Additionally, an electrolyte may be injected into the case (120) containing the electrode assembly (110), so that the positive electrode (10), the negative electrode (20), and the separator (30) are impregnated with the electrolyte (not shown).
[0055] Below, a more detailed configuration of a lithium secondary battery (100) according to one embodiment of the present invention will be described.
[0056] A lithium secondary battery according to one embodiment of the present invention comprises an electrolyte, a positive electrode, and a negative electrode.
[0057] The above electrolyte comprises a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive is a composition comprising a first compound, a second compound, and a third compound, wherein the first compound is represented by the following chemical formula 1, the second compound is represented by the following chemical formula 2, and the third compound is a cyclic carbonate compound.
[0058] [Chemical Formula 1]
[0059]
[0060] In the above chemical formula 1,
[0061] L 1 and L 2 Each is an independently substituted or unsubstituted C1 to C10 alkylene group, and
[0062] R 1 to R 4 Each is independently a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C2 to C10 alkenyl group, a substituted or unsubstituted C2 to C10 alkynyl group, a substituted or unsubstituted C3 to C10 cycloalkyl group, a substituted or unsubstituted C3 to C10 cycloalkenyl group, a substituted or unsubstituted C3 to C10 cycloalkinyl group, or a substituted or unsubstituted C6 to C20 aryl group;
[0063] [Chemical Formula 2]
[0064]
[0065] In the above chemical formula 2,
[0066] R 5 to R 14 Each is independently hydrogen, a halogen group, a cyano group, a substituted or unsubstituted C1 to C5 alkyl group, a substituted or unsubstituted C1 to C5 alkoxy group, a substituted or unsubstituted C6 to C12 aryl group, or a combination thereof, and
[0067] n1 to n3 are each independently one of integers from 0 to 20, and
[0068] n1+n2+n3 ≥ 1, and
[0069] m1 to m3 are each independently one of integers from 0 to 2.
[0070] The first compound above includes a cyano functional group, and the cyano functional group acts as an anion receptor to stably PF6 -It induces the formation of and, by including -Si-O-Si- groups and performing a function to capture HF, an electrolyte decomposition product, PF6 on the anode surface that may occur during high-temperature cycling operation of lithium secondary batteries - It is possible to improve high-rate charge / discharge characteristics and swelling characteristics by suppressing the decomposition of the electrolyte and preventing oxidation reactions of the electrolyte. In addition, performance can be improved by forming a film on the surface of the anode to suppress side reactions of the electrolyte and collapse of the electrode structure.
[0071] In addition, the anode protection function at high voltage can be further improved by further including the second compound. It is expected that the second compound can suppress side reactions between the anode and the electrolyte by stably forming a film on the anode surface through the coordination bonding of the non-covalent electron pair of N at the CN terminal with various types of metals, such as transition metals of the anode active material.
[0072] In particular, due to the three CN functional groups, coordination bonding with metal can be formed stereochemically, which enables the formation of a more robust film.
[0073] In addition, by including the above-mentioned third compound, lifespan can be improved and gases generated at the anode and cathode during high-temperature storage can be effectively controlled.
[0074] As an example, L of the above chemical formula 1 1 and L 2 Each may be an independently substituted or unsubstituted C3 to C10 alkylene group.
[0075] As an example, R of the above chemical formula 1 1 to R 4 Each may be an independently substituted or unsubstituted C1 to C10 alkyl group.
[0076] For example, the first compound above may be 1,3-bis(3-cyanopropyl)tetramethyldisiloxane.
[0077] For example, n1 to n3 of the above chemical formula 2 may be different integers.
[0078] When n1 to n3 of the above chemical formula 2 are different integers, the above chemical formula 2 may have an asymmetric structure, and in such an asymmetric structure, the binding energy with metal ions becomes much lower, which can contribute to the formation of a more stable and robust bond.
[0079] As a specific example, n3 in the above chemical formula 2 may be 0, and n1+n2 ≥ 1.
[0080] As a specific example, in the above chemical formula 2, n1+n2 ≥ 2.
[0081] For example, in the above chemical formula 2, 10 ≥ n1+n2 ≥ 2, for example 8 ≥ n1+n2 ≥ 2, or 6 ≥ n1+n2 ≥ 2.
[0082] For example, m1 to m3 of the above chemical formula 2 may be the same integers.
[0083] As a specific example, m1, m2, and m3 of the above chemical formula 2 may be simultaneously 0 or simultaneously 1.
[0084] For example, the second compound may be selected from 1,3,5-hexanetricarbonitrile, 1,3,6-hexanetricarbonitrile, and 1,2,3-Tris(2-cyanoethoxy)propane.
[0085] For example, the above third compound can be represented by the following chemical formula 3.
[0086] [Chemical Formula 3]
[0087]
[0088] In the above chemical formula 3,
[0089] R 15 and R 16 Each is independently a hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2), or a fluorine-substituted C1 to C5 alkyl group, and
[0090] The above R 15 and R 16 At least one of them is a halogen group, a cyano group (CN), a nitro group (NO2), or a fluorine-substituted C1 to C5 alkyl group.
[0091] For example, the third compound may be fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, or cyanoethylene carbonate.
[0092] For example, the first compound may be included in an amount of 0.5 to 3.0 parts by weight, for example, 0.6 to 3.0 parts by weight, 0.7 to 3.0 parts by weight, 0.8 to 3.0 parts by weight, 0.9 to 3.0 parts by weight, 1.0 to 3.0 parts by weight, 1.0 to 2.0 parts by weight, or 1.0 to 1.5 parts by weight, based on 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0093] For example, the second compound may be included in an amount of 1.0 to 5.0 parts by weight, for example, 1.0 to 4.0 parts by weight, 1.0 to 3.5 parts by weight, 1.0 to 3.0 parts by weight, 1.5 to 3.0 parts by weight, or 2.0 to 3.0 parts by weight, based on 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0094] For example, the above third compound may be included in an amount of 3.0 to 10 parts by weight, for example, 3.0 to 9.0 parts by weight, 3.0 to 8.0 parts by weight, 3.0 to 7.0 parts by weight, 4.0 to 7.0 parts by weight, or 5.0 to 7.0 parts by weight, based on 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0095] For example, the total weight of the first compound and the second compound may be included in an amount of 2.0 to 6.0 parts by weight, for example, 2.0 to 5.0 parts by weight, 2.5 to 5.0 parts by weight, or 3.0 to 5.0 parts by weight, based on 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0096] As a specific example, the first compound and the second compound may be mixed in a weight ratio of 1:0.5 to 1:5, 1:0.5 to 1:3, 1:1 to 1:3, or 1:2 to 1:3.
[0097] For example, the above composition may be included in an amount of 5.0 to 15 parts by weight, for example 7.0 to 15 parts by weight, 8.0 to 15 parts by weight, 9.0 to 15 parts by weight, or 10 to 15 parts by weight, based on 100 parts by weight of the total electrolyte for a lithium secondary battery.
[0098] When the content of the composition and the content of each component within the composition are within the above range, it is possible to realize a lithium secondary battery with improved resistance characteristics during high-temperature storage and improved lifespan characteristics at room temperature and high temperature.
[0099] The above-mentioned non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.
[0100] The above-mentioned non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent.
[0101] The above carbonate-based solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), ethylmethyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. The above ester-based solvents may include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methylpropionate, ethylpropionate, propylpropionate, decanolide, mevalonolactone, caprolactone, etc. The above ether-based solvents may include dibutyl ether, tetraglame, deglame, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. In addition, cyclohexanone, etc. may be used as the ketone-based solvent. Furthermore, ethyl alcohol, isopropyl alcohol, etc. may be used as the alcohol-based solvent, and R may be used as the aprotic solvent. 18 -CN(R 18 Nitriles such as dimethylformamide, amides such as dioxolanes such as 1,3-dioxolane, sulfolanes, etc., may be used. (It is a hydrocarbon group with a straight, branched, or ring structure having 2 to 20 carbon atoms and may include a double bond direction ring or ether bond.)
[0102] The above-mentioned non-aqueous organic solvents may be used alone or in a mixture of one or more. When used in a mixture of one or more, the mixing ratio can be appropriately adjusted according to the desired battery performance, which is widely understood by those working in the field.
[0103] The above-mentioned non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent in addition to the carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon solvent may be mixed in a volume ratio of 1:1 to 30:1.
[0104] As the above aromatic hydrocarbon solvent, an aromatic hydrocarbon compound of the following chemical formula 4 may be used.
[0105] [Chemical Formula 4]
[0106]
[0107] In the above chemical formula 4, R 23 to R 28 The groups are identical or different and are selected from the group consisting of hydrogen, halogen, alkyl groups having 1 to 10 carbon atoms, haloalkyl groups, and combinations thereof.
[0108] Specific examples of the above aromatic hydrocarbon solvents include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene. It is selected from the group consisting of 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.
[0109] The above lithium salt is a material that dissolves in a non-aqueous organic solvent and acts as a source of lithium ions within the battery, enabling the operation of a basic lithium secondary battery and facilitating the movement of lithium ions between the anode and cathode. Representative examples of such lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide): LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, and LiN(C x F 2x+1 SO2)(C y F 2y+1 One or more selected from the group consisting of SO2)(where x and y are natural numbers, for example, integers from 1 to 20), LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato) borate: LiBOB), LiDFOB (lithium difluoro(oxalato) borate), and Li[PF2(C2O4)2] (lithium difluoro(bis oxalato) phosphate). It is preferable to use a lithium salt concentration within the range of 0.1M to 2.0M. When the lithium salt concentration falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0110] The above positive electrode includes a positive current collector and a positive active material layer located on the positive current collector, and the positive active material layer includes a positive active material.
[0111] As the above-mentioned positive electrode active material, a compound capable of reversible intercalation and deintercalation of lithium (a lithated intercalation compound) may be used.
[0112] Specifically, at least one type of composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used.
[0113] Of course, a composite oxide may be used in which a portion of the metal is substituted with a metal other than another metal, or at least one phosphate compound of the composite oxide selected from the group consisting of, for example, LiFePO4, LiCoPO4, and LiMnPO4, or a composite oxide having a coating layer on its surface may be used, or a composite oxide having a coating layer may be mixed and used. This coating layer may include at least one coating element compound selected from the group consisting of oxide of the coating element, hydroxide of the coating element, oxyhydroxide of the coating element, oxycarbonate of the coating element, and hydroxycarbonate of the coating element. The compounds forming these coating layers may be amorphous or crystalline. As the coating elements included in the coating layer, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof may be used. For the coating layer formation process, any coating method may be used as long as the above-mentioned compounds are coated using these elements in a manner that does not adversely affect the physical properties of the cathode active material (e.g., spray coating, immersion method, etc.). Since this is a matter that is well understood by those skilled in the field, a detailed explanation will be omitted.
[0114] The positive active material may be one or more of the lithium complex oxides represented by, for example, Chemical Formula 5 below.
[0115] [Chemical Formula 5]
[0116] Li x M 1 y M 2 z M 3 1-y-z O2
[0117] In the above chemical formula 5,
[0118] 0.5≤x≤1.8, 0 <y≤1, 0≤z≤1, 0≤y+z≤1, M 1 , M 2 and M 3 Each may be independently selected from metals such as Ni, Co, Mn, Al, Sr, Mg, or La, and combinations thereof.
[0119] In one embodiment, the positive active material is LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi a Mn b Co c O2(a+b+c=1), LiNi a Mn b Co c Al d O2(a+b+c+d=1) and LiNi e Co f Al g It may be at least one type selected from the group consisting of O2(e+f+g=1).
[0120] For example, the above LiNi a Mn b Co c O2(a+b+c=1), LiNi a Mn b Co c Al d O2(a+b+c+d=1) and LiNi e Co f Al g The positive active material selected in O2(e+f+g=1) may be a high nickel (high Ni) based positive active material.
[0121] For example, the above LiNi a Mn b Co c O2(a+b+c=1) and LiNia Mn b Co c Al d In the case of O2(a+b+c+d=1), the nickel content may be 60% or more (a ≥ 0.6), and more specifically, 80% or more (a ≥ 0.8).
[0122] For example, the above LiNi e Co f Al g In the case of O2 (e+f+g=1), the nickel content may be 60% or more (e ≥ 0.6), and more specifically, 80% or more (e ≥ 0.8).
[0123] The content of the above positive active material may be 90% to 98% by weight based on the total weight of the positive active material layer.
[0124] In one embodiment of the present invention, the positive active material layer may optionally include a conductive material and a binder. In this case, the content of the conductive material and the binder may each be 1% to 5% by weight with respect to the total weight of the positive active material layer.
[0125] The above conductive material is used to impart conductivity to the positive electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials including mixtures thereof.
[0126] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples include polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0127] Al may be used as the anode current collector, but is not limited thereto.
[0128] The above cathode includes a cathode active material layer comprising a cathode current collector and a cathode active material formed on the cathode current collector.
[0129] The above-mentioned negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0130] As a material capable of reversibly intercalating / deintercalating the above lithium ions, any carbon-based negative electrode active material commonly used in lithium secondary batteries can be used, and representative examples include crystalline carbon, amorphous carbon, or a combination thereof. Examples of the above crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the above amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0131] As the above lithium metal alloy, an alloy of a metal selected from the group consisting of lithium, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.
[0132] Materials capable of doping and undoping the above lithium include Si, Si-C complexes, SiOx (0 < x < 2), Si-Q alloys (wherein Q is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13, Group 14, Group 15, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, and Sn-R 61 (Above R 61 Examples include elements selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof (not Sn), and at least one of these may also be mixed with SiO2.
[0133] The above elements Q and R 61 For the arbor, one may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0134] Examples of the above transition metal oxides include vanadium oxide, lithium vanadium oxide, or lithium titanium oxide.
[0135] In a specific embodiment, the negative electrode active material may include at least one of graphite and Si composites.
[0136] The graphite mentioned above may specifically be natural graphite, artificial graphite, or a combination thereof.
[0137] The above Si composite comprises a core containing Si-based particles and an amorphous carbon coating layer, for example, the Si-based particles include Si particles, Si-C composites, and SiO. x It may include one or more of (0 < x ≤ 2) and Si alloys.
[0138] For example, the core containing the above Si-based particles may include a void in the center, the radius of the center may be 30% to 50% of the radius of the above cathode active material, and the average particle size of the above Si-based particles may be 10 nm to 200 nm.
[0139] In this specification, the average particle size may be the particle size (D50) at 50% by volume ratio in the cumulative size-distribution curve.
[0140] When the average particle size of the above Si-based particles falls within the above range, volume expansion occurring during charging and discharging can be suppressed, and the disruption of the conductive path due to particle fragmentation during charging and discharging can be prevented.
[0141] The core containing the above Si-based particles further includes amorphous carbon, wherein the central part does not contain amorphous carbon, and the amorphous carbon may exist only on the surface of the negative electrode active material.
[0142] At this time, the surface region refers to the area from the outermost surface of the center to the outermost surface of the cathode active material.
[0143] In addition, Si-based particles are substantially uniformly incorporated throughout the cathode active material, that is, they can exist at a substantially uniform concentration in the center and on the surface.
[0144] The above amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbide, calcined coke, or a combination thereof.
[0145] For example, the above Si-C composite may include Si particles and crystalline carbon.
[0146] The above Si particles may be included in an amount of 1 to 60 weight% with respect to the total weight of the Si-C composite, for example, 3 It may be included in an amount of up to 60 weight%.
[0147] The above crystalline carbon may be, for example, graphite, and specifically may be natural graphite, artificial graphite, or a combination thereof.
[0148] The average particle size of the crystalline carbon above may be 5 μm to 30 μm.
[0149] As the above amorphous carbon precursor, coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, or polymer resins such as phenolic resin, furan resin, and polyimide resin may be used.
[0150] The content of the negative electrode active material in the above negative electrode active material layer may be 95% to 99% by weight with respect to the total weight of the negative electrode active material layer.
[0151] In one embodiment of the present invention, the negative electrode active material layer comprises a binder and may optionally further comprise a conductive material. The content of the binder in the negative electrode active material layer may be 1% to 5% by weight with respect to the total weight of the negative electrode active material layer. Additionally, when further comprising a conductive material, the negative electrode active material may be used in an amount of 90% to 98% by weight, the binder in an amount of 1% to 5% by weight, and the conductive material in an amount of 1% to 5% by weight.
[0152] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a water-insoluble binder, a water-soluble binder, or a combination thereof may be used.
[0153] Examples of the above-mentioned water-insoluble binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.
[0154] Examples of the above water-soluble binders include rubber-based binders or polymer resin binders. The above rubber-based binder may be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, and combinations thereof. The above polymer resin binder may be selected from polytetrafluoroethylene, ethylene-propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene-propylene-diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0155] When a water-soluble binder is used as the above-mentioned cathode binder, a cellulose-based compound capable of imparting viscosity may be further included as a thickener. As this cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. Na, K, or Li may be used as the alkali metal. The content of such a thickener may be 0.1 to 3 parts by weight per 100 parts by weight of the cathode active material.
[0156] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials comprising a mixture thereof.
[0157] The above-mentioned cathode current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0158] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. Such a separator may be a porous substrate; or a composite porous substrate.
[0159] The porous substrate is a substrate containing pores through which lithium ions can move. The porous substrate may be, for example, polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof, and of course, a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may be used.
[0160] The above composite porous substrate may be in the form of a porous substrate and a functional layer located on the porous substrate. From the perspective of enabling the addition of additional functions, the functional layer may be, for example, at least one of a heat-resistant layer and an adhesive layer, and for example, the heat-resistant layer may include a heat-resistant resin and optionally a filler.
[0161] In addition, the adhesive layer may include an adhesive resin and optionally a filler.
[0162] The above filler may be an organic filler or an inorganic filler.
[0164] Examples and comparative examples of the present invention are described below. The following examples are merely embodiments of the present invention, and the present invention is not limited to the following examples.
[0165] Production of lithium secondary batteries
[0166] Comparative Example 1
[0167] LiCoO2 as the positive active material, polyvinylidene fluoride as the binder, and Ketjen black as the conductive material are mixed in a weight ratio of 97:2:1, respectively. N - A positive electrode active material slurry was prepared by dispersing in methylpyrrolidone.
[0168] The above positive active material slurry was coated onto an Al foil with a thickness of 14 μm, dried at 110°C, and then pressed to produce a positive electrode.
[0169] Artificial graphite as a negative electrode active material, styrene-butadiene rubber as a binder, and carboxymethylcellulose as a thickener were mixed in a weight ratio of 97:1:2, respectively, and dispersed in distilled water to prepare a negative electrode active material slurry.
[0170] The above cathode active material slurry was coated onto a 10㎛ thick Cu foil, dried at 100℃, and then pressed to manufacture a cathode.
[0171] An electrode assembly was manufactured by assembling the above-manufactured positive and negative electrodes with a polyethylene separator with a thickness of 25 μm, and a lithium secondary battery was fabricated by injecting an electrolyte.
[0172] The electrolyte composition is as follows.
[0173] (Electrolyte composition)
[0174] Salt: LiPF61.3 M
[0175] Solvent: Ethylene carbonate : Propylene carbonate : Propyl propionate (volume ratio of EC : PC : PP = 10:15:75)
[0176] Comparative Example 2
[0177] A lithium secondary battery was manufactured in the same manner as Comparative Example 1, except that 7.0 parts by weight of fluoroethylene carbonate (FEC) were added to the electrolyte.
[0178] (However, in the above electrolyte composition, “parts by weight” refers to the relative weight of the additive to 100 parts by weight of the total electrolyte (lithium salt + non-aqueous organic solvent).)
[0179] Comparative Example 3
[0180] A lithium secondary battery was prepared in the same manner as Comparative Example 1, except that 7.0 parts by weight of fluoroethylene carbonate and 3.0 parts by weight of 1,3,6-hexanetricarbonitrile (HTCN) were added to the electrolyte.
[0181] Comparative Example 4
[0182] A lithium secondary battery was prepared in the same manner as Comparative Example 1, except that 7.0 parts by weight of fluoroethylene carbonate and 1.0 parts by weight of 1,3-bis(3-cyanopropyl)tetramethyldisiloxane (SiCN: 1,3-bis(3-cyanopropyl)tetramethyldisiloxane) were added to the electrolyte.
[0183] Comparative Example 5
[0184] A lithium secondary battery was prepared in the same manner as Comparative Example 1, except that 7.0 parts by weight of fluoroethylene carbonate, 3.0 parts by weight of 1,3,6-hexanetricarbonitrile, and 1.0 parts by weight of PSAN (Phenylsulfonylacetonitrile) were added to the electrolyte.
[0185] Example 1
[0186] A lithium secondary battery was prepared in the same manner as Comparative Example 1, except that 7.0 parts by weight of fluoroethylene carbonate, 3.0 parts by weight of 1,3,6-hexanetricarbonitrile, and 1.0 parts by weight of 1,3-bis(3-cyanopropyl)tetramethyldisiloxane were added to the electrolyte.
[0187] Example 2
[0188] A lithium secondary battery was prepared in the same manner as Comparative Example 1, except that 7.0 parts by weight of fluoroethylene carbonate, 3.0 parts by weight of TCEP (1,2,3-Tris(2-cyanoethoxy)propane), and 1.0 parts by weight of 1,3-bis(3-cyanopropyl)tetramethyldisiloxane were added to the electrolyte.
[0189] Comparative Example 6
[0190] A lithium secondary battery was fabricated in the same manner as in Example 1, except that the negative electrode active material was changed to SiNWs.
[0192] The compositions according to the examples and comparative examples are shown in Table 1 below.
[0193] Additive composition cathode active material First compound (parts by weight) Second compound (parts by weight) Third compound (parts by weight) Comparative Example 1 - - - Artificial graphite Comparative Example 2 - - FEC (7.0) Artificial graphite Comparative Example 3 - HTCN (3.0) FEC (7.0) Artificial graphite Comparative Example 4 SiCN (1.0) - FEC (7.0) Artificial graphite Comparative Example 5 PSAN (1.0) HTCN (3.0) FEC (7.0) Artificial graphite Example 1 SiCN (1.0) HTCN (3.0) FEC (7.0) Artificial graphite Example 2 SiCN (1.0) TCEP (3.0) FEC (7.0) Artificial graphite Comparative Example 6 SiCN (1.0) HTCN (3.0) FEC (7.0) SiNWs
[0194] Assessment 1: EDS Mapping Analysis
[0195] EDS mapping analysis was performed to verify the surface image and elemental distribution of the cathode after high-temperature charging and discharging.
[0196] The circular full cells of Example 1, Comparative Example 1, and Comparative Example 3 were fabricated and, after repeating the charging CCCV 1.5C 4.5V 0.05C cutoff and discharging CC 1.0C 3.0V cutoff conditions 300 times at 45℃, the full cells were disassembled and positive / negative EDS analysis was performed.
[0197] Figure 2 is an EDS mapping image of the cathode surface after charging and discharging of a full cell.
[0198] Referring to FIG. 2, it is confirmed that the F and P components in Example 1 are significantly reduced compared to Comparative Examples 1 and 3.
[0199] From this, it can be seen that the decomposition of the electrolyte under high temperature conditions was effectively suppressed as the first compound, the second compound, and the third compound were simultaneously included as additive components.
[0201] Evaluation 2: Measurement of gas generation after high-temperature storage
[0202] The circular pool cells of Example 1, Comparative Example 1, and Comparative Example 3 were filled to SOC 100% under conditions of CCCV 0.2C 4.5V 0.05C cutoff and left in a 60℃ chamber for 7 days. After drilling a hole in the bottom of the circular pool cell using a gas collection jig, the amount of internally generated gas was measured using a connected gas chromatograph (GC) without external leakage of the generated gas. The results of the gas generation amount measurement obtained as described above are shown in Fig. 3.
[0203] Referring to FIG. 3, it can be seen that in the case of Example 1, which contains three types of additives simultaneously, the amount of gas generated is significantly reduced compared to the case where there are no additives (Comparative Example 1) or where one type is not included (Comparative Example 3). From this, it can be confirmed that the electrolyte according to one embodiment can improve the stability of a lithium battery.
[0205] Evaluation 3: High-temperature life characteristics evaluation (discharge capacity evaluation)
[0206] For the lithium secondary batteries prepared according to Examples 1 and 2 and Comparative Examples 1 to 6, charging and discharging were performed at 0.1C for 3 cycles, and then the discharge capacity of the batteries was evaluated by continuing to charge at 1.5C and discharge at 1.0C for 300 cycles, and the results are shown in Table 2 and Figure 4. The voltage range used at this time was 3.0V to 4.5V (discharging up to 3.0V and charging up to 4.5V), and the evaluation temperature was 45℃.
[0207] Figure 4 is a graph showing the discharge capacity according to the progress of the high-temperature charge / discharge cycle for a lithium secondary battery.
[0208] Referring to Table 2 and Figure 4, it can be confirmed that the discharge capacity of Examples 1 and 2, which contain all three types of additives, exceeds 70%, indicating excellence. In particular, as the discharge capacity is much higher in Comparative Example 5, which is described later and has a Coulomb efficiency of approximately 99%, it can be predicted that the lifespan characteristics of the battery according to the examples will be further improved compared to a battery in which any one of the three additives is replaced with another additive, as in Comparative Example 5.
[0209] In addition, it can be confirmed that significantly improved lifespan characteristics are observed when applying the carbon-based cathode according to Examples 1 and 2 of the present invention, even when compared to when applying the Si-based cathode (Comparative Example 6).
[0211] Evaluation 4: High-temperature life characteristics evaluation (Coulomb efficiency evaluation)
[0212] For the lithium secondary batteries prepared according to Examples 1 and 2 and Comparative Examples 1 to 6, charging and discharging were performed at 0.1C for 3 cycles, followed by charging at 1.5C and discharging at 1.0C for 300 cycles, and the Coulomb efficiency of the batteries was evaluated, and the results are shown in Table 1 and Figure 5. The voltage range used at this time was 3.0V to 4.5V (discharging up to 3.0V and charging up to 4.5V), and the evaluation temperature was 45℃.
[0213] Figure 5 shows the results of measuring Coulomb efficiency according to the high-temperature charge-discharge cycle of a lithium secondary battery.
[0214] Referring to Table 2 and Figure 5, it can be confirmed that in the case of Examples 1 and 2, which contain all three types of additives, the Coulomb efficiency exceeds 99% and approaches 100%, and accordingly, it can be predicted that the battery life characteristics will be improved.
[0215] In addition, it can be confirmed that significantly improved Coulomb efficiency is observed when applying the carbon-based cathode according to Examples 1 and 2 of the present invention, even when compared to when applying the Si-based cathode (Comparative Example 6).
[0216] High temperature (45℃) lifespan characteristics Discharge capacity (%) Coulomb efficiency (%) Comparative Example 1 2 88.2 Comparative Example 5 50 99.2 Example 1 78 99.2 Example 2 73 99.3 Comparative Example 6 31 98.9
[0217] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention. Explanation of the symbols
[0218] 100: Lithium secondary pouch battery 10: Anode 20: Cathode 30: Separator 110: Electrode assembly 120: Case 130: Electrode tab
Claims
Claim 1 An electrolyte for a lithium secondary battery applied to a lithium secondary battery having a charging upper limit voltage of 4.5 V or higher, comprising a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive is a composition comprising a first compound, a second compound, and a third compound, wherein the first compound is represented by the following Chemical Formula 1, the second compound is represented by the following Chemical Formula 2, and the third compound is a cyclic carbonate compound, and the first compound and the second compound are mixed in a weight ratio of 1:0.5 to 1:5: [Chemical Formula 1] In the above chemical formula 1, L 1 and L 2 is each independently substituted or unsubstituted C1 to C10 alkylene group, and R 1 to R 4 Each is independently a substituted or unsubstituted C1 to C10 alkyl group, a substituted or unsubstituted C2 to C10 alkenyl group, a substituted or unsubstituted C2 to C10 alkynyl group, a substituted or unsubstituted C3 to C10 cycloalkyl group, a substituted or unsubstituted C3 to C10 cycloalkenyl group, a substituted or unsubstituted C3 to C10 cycloalkynyl group, or a substituted or unsubstituted C6 to C20 aryl group; [Chemical Formula 2] In the above chemical formula 2, R 5 to R 14 Each is independently hydrogen, a halogen group, a cyano group, a substituted or unsubstituted C1 to C5 alkyl group, a substituted or unsubstituted C1 to C5 alkoxy group, a substituted or unsubstituted C6 to C12 aryl group, or a combination thereof, n1 to n3 are each independently one of integers from 0 to 20, n1 to n3 are different integers, n1+n2+n3 ≥ 1, and m1 to m3 are each independently one of integers from 0 to 2. Claim 2 In claim 1, L of the above chemical formula 1 1 and L 2 Electrolyte for a lithium secondary battery, wherein each is an independently substituted or unsubstituted C3 to C10 alkylene group. Claim 3 In claim 1, R of the above chemical formula 1 1 to R 4 Electrolyte for a lithium secondary battery, each having an independently substituted or unsubstituted C1 to C10 alkyl group. Claim 4 In claim 1, the electrolyte for a lithium secondary battery, wherein the first compound is 1,3-bis(3-cyanopropyl)tetramethyldisiloxane. Claim 5 delete Claim 6 An electrolyte for a lithium secondary battery according to claim 1, wherein the second compound is one selected from 1,3,5-hexanetricarbonitrile, 1,3,6-hexanetricarbonitrile, and 1,2,3-Tris(2-cyanoethoxy)propane. Claim 7 In claim 1, the electrolyte for a lithium secondary battery is represented by the following chemical formula 3, wherein the third compound is represented by the following chemical formula 3: [Chemical Formula 3] In the above chemical formula 3, R 15 and R 16 Each is independently hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2), or a fluorine-substituted C1 to C5 alkyl group, and R 15 and R 16 At least one of them is a halogen group, a cyano group (CN), a nitro group (NO2), or a fluorine-substituted C1 to C5 alkyl group. Claim 8 An electrolyte for a lithium secondary battery according to claim 1, wherein the third compound is fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, or cyanoethylene carbonate. Claim 9 An electrolyte for a lithium secondary battery according to claim 1, wherein the first compound is included in an amount of 0.5 to 3.0 parts by weight per 100 parts by weight of the total electrolyte for a lithium secondary battery. Claim 10 An electrolyte for a lithium secondary battery according to claim 1, wherein the second compound is included in an amount of 1.0 to 5.0 parts by weight per 100 parts by weight of the total electrolyte for a lithium secondary battery. Claim 11 An electrolyte for a lithium secondary battery according to claim 1, wherein the third compound is included in an amount of 3.0 to 10 parts by weight per 100 parts by weight of the total electrolyte for a lithium secondary battery. Claim 12 An electrolyte for a lithium secondary battery according to claim 1, wherein the total weight of the first compound and the second compound is included in an amount of 2.0 to 6.0 parts by weight per 100 parts by weight of the electrolyte for a lithium secondary battery. Claim 13 delete Claim 14 An electrolyte for a lithium secondary battery according to claim 1, wherein the composition is included in an amount of 5.0 to 15 parts by weight per 100 parts by weight of the total electrolyte for a lithium secondary battery. Claim 15 A lithium secondary battery comprising: a positive electrode comprising a positive active material; a negative electrode comprising a negative active material; and an electrolyte for a lithium secondary battery according to any one of claims 1 to 4, 6 to 12 and 14. Claim 16 In paragraph 15, the above negative electrode active material is a carbon-based negative electrode active material for a lithium secondary battery. Claim 17 delete
Citation Information
Patent Citations
Non-aqueous electrolyte solution for lithium secondary battery and lithium secondary battery comprising the same
KR1020210055604A
Non-aqueous electrolyte for lithium secondary battery and lithium secondary battery comprising the same
KR1020210138937A
Non-aqueous electrolyte solution for lithium secondary battery and lithium secondary battery comprising the same
KR1020220009894A
Silicon-based energy storage devices with silicon containing electrolyte additives
US20200388876A1
Lithium secondary battery including electrolyte additive for lithium secondary battery
US20220158224A1