Thermoplastic resin composition and molded article

The thermoplastic resin composition, incorporating polycarbonate and ethylene/α-olefin rubber-reinforced vinyl resin with a hydrogenated glycerin fatty acid ester, addresses the balance of mechanical and noise reduction challenges, offering improved mechanical properties and color development for applications like automobile parts.

WO2024202903A1PCT designated stage expired Publication Date: 2024-10-03TECHNO UMG CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007558
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-02-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Thermoplastic resin compositions, such as PC/ABS and AES, face challenges in balancing mechanical properties, color development, and noise reduction, particularly in applications requiring heat resistance, impact resistance, and moldability, with existing solutions like AES resin causing color issues and methacrylic acid ester resins being inferior in fluidity and mechanical strength.

Method used

A thermoplastic resin composition combining polycarbonate resin, ethylene/α-olefin rubber-reinforced vinyl resin, non-rubber reinforced vinyl resin, and a lubricant with a saturated fatty acid ester, specifically hydrogenated glycerin fatty acid ester, to achieve excellent mechanical properties, color development, and long-term squeak noise reduction.

Benefits of technology

The composition provides enhanced mechanical properties, color development, and sustained squeak noise reduction, making it suitable for applications like automobile parts where impact resistance and quietness are critical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

A thermoplastic resin composition comprising a polycarbonate resin (A), a rubber-reinforced vinyl resin (B), a non-rubber-reinforced vinyl resin (C), and a lubricant (D), wherein the rubber-reinforced vinyl resin (B) contains at least an ethylene-(α-olefin) rubber-reinforced resin (B1) produced by the graft polymerization of a vinyl monomer in the presence of an ethylene-(α-olefin) rubbery polymer (b1), the non-rubber-reinforced vinyl resin (C) is a copolymer containing at least an acrylonitrile unit and a styrene unit, and the lubricant (D) has a saturated fatty acid ester having 12 or more carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic resin composition and molded article

[0001] The present invention relates to a thermoplastic resin composition and a molded article. This application claims priority to Japanese Patent Application No. 2023-052919, filed on March 29, 2023, the contents of which are incorporated herein by reference.

[0002] Rubber-modified graft polymers such as ABS resins and AES resins are materials with excellent mechanical strength and moldability, but their heat resistance and impact resistance may be insufficient for use in applications requiring heat resistance and high impact resistance (automobile parts, office automation parts, etc.). On the other hand, polycarbonate-based resins are materials with excellent heat resistance and impact resistance, but their moldability may be insufficient. A known method for compensating for these mutual drawbacks is to blend a polycarbonate-based resin with a rubber-modified graft polymer.

[0003] Such materials have been widely used in automobile interior parts, such as PC / ABS, a blend of polycarbonate and ABS resin. Furthermore, with the recent spread of hybrid and electric vehicles, there has been an increasing demand for quieter interiors, and AES resin, which excels in quietness, is being used as an alternative to ABS resin.

[0004] However, if the amount of AES required to ensure sufficient quietness is used, problems such as poor color development occur.

[0005] A thermoplastic resin composition containing AES resin and methacrylic acid ester resin has been proposed as an AES resin composition with excellent noise reduction and color development (Patent Document 1). Also, a thermoplastic resin composition containing a fatty acid ester as a lubricant to impart noise suppression has been proposed (Patent Document 2). However, Patent Document 1 does not consider acrylonitrile-styrene copolymers as non-rubber-reinforced resins, and instead uses methacrylic acid ester resins, resulting in inferior fluidity and mechanical strength. Furthermore, Patent Document 2 discloses that fatty acid esters contribute to noise suppression, but does not consider the long-term stability of the effect of reducing squeak noise due to bleed-out or the like.

[0006] JP 2018-95722 A JP 2021-31561 A

[0007] The present invention provides a resin composition and a molded article thereof that are excellent in mechanical properties, color development, and quietness by using a specific saturated fatty acid ester in combination with an ethylene-α-olefin rubber-reinforced resin as a rubber-reinforced vinyl resin.

[0008] The present invention has the following aspects: [1] A thermoplastic resin composition comprising a polycarbonate resin (A), a rubber-reinforced vinyl resin (B), a non-rubber-reinforced vinyl resin (C), and a lubricant (D), wherein the rubber-reinforced vinyl resin (B) comprises an ethylene-α-olefin rubber-reinforced resin (B1) obtained by graft polymerization of a vinyl monomer in the presence of at least an ethylene-α-olefin rubber polymer (b1), the non-rubber-reinforced vinyl resin (C) is a copolymer containing at least acrylonitrile units and styrene units, and the lubricant (D) is a lubricant containing a saturated fatty acid ester having 12 or more carbon atoms, and wherein, when the total of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C) is 100 parts by mass, the polycarbonate resin (A) is 30 to 70 parts by mass, the rubber-reinforced vinyl resin (B) is 3 to 16 parts by mass, and the ethylene-α-olefin rubber-reinforced resin (B1) is 3 to 16 parts by mass, and 1 to 8 parts by mass of the lubricant (D). [2] The thermoplastic resin composition according to [1], wherein the non-rubber-reinforced vinyl resin (C) is contained in an amount of 20 to 60 parts by mass, relative to 100 parts by mass of the total of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C). [3] The thermoplastic resin composition according to [1] or [2], wherein the lubricant (D) is at least one hydrogenated glycerin fatty acid ester. [4] The thermoplastic resin composition according to any one of [1] to [3], wherein the rubber-reinforced vinyl resin (B) further contains a diene-based rubber-reinforced resin (B2) obtained by graft polymerization of a vinyl monomer in the presence of a diene-based rubber polymer (b2). [5] A molded article of the thermoplastic resin composition according to any one of [1] to [4].

[0009] According to the present invention, when a glycerin fatty acid ester is used in combination with an ethylene-α-olefin rubber-reinforced resin, it is possible to provide a resin composition and a molded article thereof that are excellent in mechanical properties and color development as well as in long-term squeak noise reduction (silence).

[0010] In this specification, "(meth)acrylic" means acrylic and methacrylic, "(meth)acrylic acid ester" means acrylic acid ester and methacrylic acid ester, and "(co)polymer" means homopolymer and copolymer. "Unit" means a structural portion contained in a polymer and derived from a compound (monomer) before polymerization. For example, "acrylonitrile unit" means "structural portion derived from acrylonitrile," and "styrene unit" means "structural portion derived from styrene." The content ratio of each monomer unit in a copolymer corresponds to the blending ratio of each monomer used in producing the copolymer. "To" indicating a numerical range means that the numerical values ​​written before and after it are included as the lower and upper limits.

[0011] [Resin Composition] The resin composition of the first aspect of the present invention contains a polycarbonate resin (A), a rubber-reinforced vinyl resin (B), a non-rubber-reinforced vinyl resin (C), and a lubricant (D). The resin composition of this aspect may further contain other thermoplastic resins and additives, as necessary, within the scope of the present invention.

[0012] <Polycarbonate Resin (A)> The polycarbonate resin (A) is a resin having a carbonate bond in the main chain. The polycarbonate resin (A) is not particularly limited, and examples thereof include aromatic polycarbonates, aliphatic polycarbonates, aliphatic-aromatic polycarbonates, and aromatic polyester carbonates. These polycarbonate resins may be modified at the terminal with an R—CO— group or an R′—O—CO— group (R and R′ both represent organic groups). These polycarbonate resins may be used alone or in combination of two or more.

[0013] As the polycarbonate resin (A), from the viewpoints of impact resistance and heat resistance, at least one selected from the group consisting of aromatic polycarbonates and aromatic polyester carbonates is preferred, and from the viewpoint of impact resistance in particular, aromatic polycarbonates are more preferred.

[0014] Examples of aromatic polycarbonates include reaction products obtained by transesterification of aromatic dihydroxy compounds with carbonic acid diesters, polycondensates obtained by interfacial polycondensation of aromatic dihydroxy compounds with phosgene, and polycondensates obtained by pyridine method of aromatic dihydroxy compounds with phosgene.

[0015] The aromatic dihydroxy compound may be any compound having two hydroxy groups bonded to an aromatic ring in the molecule, and examples thereof include dihydroxybenzenes such as hydroquinone and resorcinol, 4,4'-biphenol, 2,2-bis(4-hydroxyphenyl)propane (hereinafter referred to as "bisphenol A"), 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl-3-methylphenyl)propane, 2,2-bis(3-tert-butyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)methane, 1,1-bis(p-hydroxyphenyl)ethane, 2,2-bis(p-hydroxyphenyl)butane, 2,2-bis(p-hydroxyphenyl)pentane, 1,1-bis(p-hydroxyphenyl)cyclohexane, 1,1-bis(p-hydroxyphenyl)-4- Examples of such compounds include isopropylcyclohexane, 1,1-bis(p-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(p-hydroxyphenyl)-1-phenylethane, 9,9-bis(p-hydroxyphenyl)fluorene, 9,9-bis(p-hydroxy-3-methylphenyl)fluorene, 4,4'-(p-phenylenediisopropylidene)bisphenol, 4,4'-(m-phenylenediisopropylidene)bisphenol, bis(p-hydroxyphenyl)oxide, bis(p-hydroxyphenyl)ketone, bis(p-hydroxyphenyl)ether, bis(p-hydroxyphenyl)ester, bis(p-hydroxyphenyl)sulfide, bis(p-hydroxy-3-methylphenyl)sulfide, bis(p-hydroxyphenyl)sulfone, bis(3,5-dibromo-4-hydroxyphenyl)sulfone, and bis(p-hydroxyphenyl)sulfoxide. These compounds may be used alone or in combination of two or more.

[0016] The aromatic dihydroxy compound is preferably a compound having a hydrocarbon group between two benzene rings. In this compound, the hydrocarbon group may be, for example, an alkylene group. The hydrocarbon group may be a halogen-substituted hydrocarbon group. The benzene ring may have a hydrogen atom substituted with a halogen atom. Examples of compounds having a hydrocarbon group between two benzene rings include bisphenol A, 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl-3-methylphenyl)propane, 2,2-bis(3-tert-butyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)methane, 1,1-bis(p-hydroxyphenyl)ethane, and 2,2-bis(p-hydroxyphenyl)butane. These compounds may be used alone or in combination of two or more. Of these, bisphenol A is particularly preferred.

[0017] Examples of the carbonate diester used to obtain an aromatic polycarbonate by transesterification include dimethyl carbonate, diethyl carbonate, di-tert-butyl carbonate, diphenyl carbonate, ditolyl carbonate, etc. These may be used alone or in combination of two or more.

[0018] Aromatic polyester carbonate is a resin having carbonate bonds and ester bonds in the main chain. Examples of aromatic polyester carbonate include poly-4,4'-isopropylidenediphenyl carbonate (for example, commercially available as "Novarex" described below).

[0019] The lower limit of the viscosity average molecular weight (Mv) of the polycarbonate resin (A) is preferably 15,000 or more, more preferably 17,000 or more, and particularly preferably 18,000 or more. When Mv is equal to or greater than the above lower limit, the impact resistance is better. The upper limit is preferably 40,000 or less, more preferably 30,000 or less, and particularly preferably 28,000 or less. When Mv is equal to or less than the above upper limit, the flowability and moldability are better. The Mv of the polycarbonate resin (A) is a value determined by melt viscosity.

[0020] <Rubber-reinforced vinyl resin (B)> The rubber-reinforced vinyl resin (B) is obtained by polymerizing (graft polymerizing) a vinyl monomer component in the presence of a rubber polymer, and contains a rubber polymer and a vinyl polymer. The vinyl monomer component is composed of one or more vinyl monomers. The vinyl polymer is a polymer of the vinyl monomer component and contains structural units based on the vinyl monomer.

[0021] Examples of rubbery polymers include ethylene-α-olefin rubbery polymers, diene rubbery polymers, and acrylic rubbery polymers. These may be used alone or in combination of two or more. From the viewpoint of impact resistance, the rubbery polymer is preferably at least one selected from the group consisting of ethylene-α-olefin rubbery polymers and diene rubbery polymers. From the viewpoint of reducing creaking noise when molded articles come into contact with each other, ethylene-α-olefin rubbery polymers are more preferred. An ethylene-α-olefin rubbery polymer and a diene rubbery polymer may be used in combination. In this case, molded articles of the resin composition undergo ductile fracture upon impact even in extremely low-temperature environments such as -30°C, making the resin composition suitable as a molding material for molded articles (such as automotive parts) that require safety.

[0022] The ethylene-α-olefin rubber polymer contains structural units based on ethylene and structural units based on an α-olefin having 3 or more carbon atoms. Examples of the α-olefin include α-olefins having 3 to 20 carbon atoms, specifically propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-hexadecene, and 1-eicosene. These α-olefins can be used alone or in combination of two or more. The α-olefin preferably has 3 to 20 carbon atoms, more preferably 3 to 12 carbon atoms, and even more preferably 3 to 8 carbon atoms. When the α-olefin has 20 or less carbon atoms, copolymerization with ethylene is favorable, and the surface appearance of molded articles of the resin composition is superior.

[0023] The proportion of ethylene-based structural units relative to the total mass of ethylene-based structural units and structural units based on an α-olefin having 3 or more carbon atoms is typically 5 to 95 mass%, preferably 50 to 95 mass%, more preferably 60 to 95 mass%, and particularly preferably 70 to 90 mass%. The proportion of the α-olefin-based structural units relative to the total mass is the value obtained by subtracting the proportion of the ethylene-based structural units from the total mass (100 mass%). When the proportion of ethylene-based structural units is within the above range, the ethylene-α-olefin rubber polymer will have sufficient rubber elasticity and will have better impact resistance.

[0024] The ethylene-α-olefin rubbery polymer may further contain structural units based on non-conjugated dienes, such as 1,4-hexadiene, 1,5-hexadiene, 5-ethylidene-2-norbornene, and dicyclopentadiene, as needed.

[0025] When the ethylene-α-olefin rubbery polymer further contains a structural unit based on a non-conjugated diene, from the viewpoint of reducing squeak noise, the proportion of the structural unit based on a non-conjugated diene relative to the total mass (100% by mass) of the structural units based on ethylene and the structural units based on the α-olefin is preferably 0 to 10% by mass, more preferably 1 to 9% by mass, even more preferably 2 to 8% by mass, and particularly preferably 3 to 7% by mass.

[0026] The ethylene-α-olefin rubber polymer is preferably an ethylene-propylene copolymer, an ethylene-1-butene copolymer, or an ethylene-1-octene copolymer, and more preferably an ethylene-propylene copolymer. The ethylene-α-olefin rubber polymer may be used alone or in combination of two or more.

[0027] The Mooney viscosity (ML1+4) at 100°C of the ethylene-α-olefin rubbery polymer (which may contain structural units based on a non-conjugated diene) is typically 5 to 80, preferably 10 to 65, and more preferably 10 to 45. If the Mooney viscosity is within the above range, the flowability of the rubber-modified graft polymer (B) will be better and the moldability will be more excellent. The Mooney viscosity is a value measured according to the method specified in JIS K 6300.

[0028] From the viewpoint of reducing squeak noise, it is preferable that the ethylene-α-olefin rubbery polymer has a melting point (Tm). The fact that the ethylene-α-olefin rubbery polymer has a Tm means that the rubbery polymer has a crystalline portion. The presence of a crystalline portion in the rubbery polymer is thought to suppress the occurrence of the stick-slip phenomenon, thereby suppressing the occurrence of squeak noise.

[0029] The Tm of the ethylene-α-olefin rubbery polymer (which may contain structural units based on a non-conjugated diene) is preferably 0 to 120°C, more preferably 10 to 100°C, and particularly preferably 20 to 80°C. If the Tm is 0°C or higher, the effect of reducing squeak noise is more excellent. The Tm is the value obtained by measuring the endothermic change at a constant temperature increase rate of 20°C per minute using a differential scanning calorimeter (DSC) and reading the peak temperature of the obtained endothermic pattern, and details are specified in JIS K 7121:1987. Note that in the DSC measurement, those that do not clearly show a peak of the endothermic change are considered to have substantially no crystallinity and do not have a Tm.

[0030] The glass transition temperature (Tg) of the ethylene-α-olefin rubber polymer (which may contain structural units based on a non-conjugated diene) is preferably −20° C. or lower, more preferably −30° C. or lower, and particularly preferably −40° C. or lower. If Tg is −20° C. or lower, the impact resistance of molded articles of the resin composition will be superior. Tg can be measured using DSC in the same manner as for measuring Tm, according to the method specified in JIS K 7121:1987.

[0031] The weight-average molecular weight of the ethylene-α-olefin rubber polymer is typically 50,000 to 1,000,000, preferably 80,000 to 800,000, and more preferably 80,000 to 500,000. When the weight-average molecular weight is within the above range, the flowability and moldability of the resin composition, and the impact resistance and appearance of molded articles of the resin composition are superior. The weight-average molecular weight is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0032] Examples of diene rubbery polymers include homopolymers such as polybutadiene and polyisoprene; butadiene copolymers such as styrene-butadiene copolymer, styrene-butadiene-styrene copolymer, acrylonitrile-styrene-butadiene copolymer, and acrylonitrile-butadiene copolymer; and isoprene copolymers such as styrene-isoprene copolymer, styrene-isoprene-styrene copolymer, and acrylonitrile-styrene-isoprene copolymer. These may be random copolymers or block copolymers. The diene rubbery polymer may be a crosslinked polymer or an uncrosslinked polymer. The diene rubbery polymer may be a (co)polymer obtained by hydrogenating a (co)polymer containing units composed of a conjugated diene compound. The hydrogenation rate of the diene rubbery polymer is typically 95% or more, preferably 98% or more. The diene rubbery polymers may be used alone or in combination of two or more. Note that the diene rubbery polymer does not contain structural units based on α-olefins.

[0033] The proportion of the rubbery polymer relative to the total mass of the rubbery polymer and the vinyl polymer (total mass of the rubbery polymer and the vinyl monomer component) is preferably 10 to 60 mass%, more preferably 15 to 40 mass%, and even more preferably 20 to 30 mass% when the rubbery polymer is an ethylene-α-olefin rubbery polymer. On the other hand, when the rubbery polymer is a diene rubbery polymer, the proportion is preferably 40 to 75 mass%, more preferably 50 to 70 mass%, and even more preferably 55 to 65 mass%.

[0034] (Vinyl Monomer Component) Examples of vinyl monomers constituting the vinyl monomer component include aromatic vinyl compounds, vinyl cyanide compounds, (meth)acrylic acid esters, and other vinyl monomers copolymerizable with these compounds. Examples of other vinyl monomers include maleimide compounds, unsaturated acid anhydrides, carboxyl group-containing unsaturated compounds, hydroxyl group-containing unsaturated compounds, oxazoline group-containing unsaturated compounds, and epoxy group-containing unsaturated compounds. These can be used alone or in combination of two or more.

[0035] Specific examples of aromatic vinyl compounds include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, β-methylstyrene, ethylstyrene, p-tert-butylstyrene, vinyltoluene, vinylxylene, and vinylnaphthalene. These compounds can be used alone or in combination of two or more. Of these, styrene and α-methylstyrene are preferred, and styrene is particularly preferred.

[0036] Specific examples of vinyl cyanide compounds include acrylonitrile, methacrylonitrile, ethacrylonitrile, α-ethylacrylonitrile, α-isopropylacrylonitrile, etc. These compounds can be used alone or in combination of two or more. Of these, acrylonitrile is preferred.

[0037] Specific examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate. These compounds can be used alone or in combination of two or more. Of these, methyl methacrylate is preferred.

[0038] Specific examples of the maleimide-based compound include N-phenylmaleimide, N-cyclohexylmaleimide, etc. These compounds may be used alone or in combination of two or more.

[0039] Specific examples of unsaturated acid anhydrides include maleic anhydride, itaconic anhydride, citraconic anhydride, etc. These compounds may be used singly or in combination of two or more.

[0040] Specific examples of the carboxyl group-containing unsaturated compound include (meth)acrylic acid, ethacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, cinnamic acid, etc. These compounds can be used alone or in combination of two or more.

[0041] Specific examples of the hydroxy group-containing unsaturated compound include 3-hydroxy-1-propene, 4-hydroxy-1-butene, cis-4-hydroxy-2-butene, trans-4-hydroxy-2-butene, 3-hydroxy-2-methyl-1-propene, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, etc. These compounds can be used alone or in combination of two or more.

[0042] From the viewpoint of compatibility between the rubber-modified graft polymer (B) and other resins, the vinyl-based monomer component preferably contains an aromatic vinyl compound. From the viewpoint of compatibility, the proportion of the aromatic vinyl compound relative to the total mass of the vinyl-based monomer component is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and particularly preferably 70% by mass or more. This proportion may be 100% by mass, but is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less.

[0043] From the viewpoint of compatibility between the rubber-modified graft polymer (B) and other resins, the vinyl-based monomer component preferably contains, in addition to the aromatic vinyl compound, at least one selected from the group consisting of a vinyl cyanide compound and a (meth)acrylic acid ester, and more preferably contains a vinyl cyanide compound. When the vinyl cyanide compound is contained together with the aromatic vinyl compound, the chemical resistance, toughness, etc. of the molded article of the resin composition are more excellent.

[0044] When the vinyl monomer component contains an aromatic vinyl compound and a vinyl cyanide compound, from the viewpoint of compatibility, the proportion of the aromatic vinyl compound relative to the total mass of the vinyl monomer components is preferably 40 to 90 mass%, more preferably 55 to 85 mass%, and even more preferably 65 to 80 mass%. Furthermore, the proportion of the vinyl cyanide compound relative to the total mass of the vinyl monomer components is preferably 10 to 60 mass%, more preferably 15 to 45 mass%, and even more preferably 20 to 35 mass%. The proportion of the aromatic vinyl compound relative to the total mass of the vinyl monomer components can be considered as the proportion of structural units based on the aromatic vinyl compound relative to the total mass of all structural units constituting the vinyl polymer. The same applies to the proportion of the vinyl cyanide compound.

[0045] (Method for producing rubber-reinforced vinyl resin (B)) The rubber-reinforced vinyl resin (B) is obtained by polymerizing a vinyl monomer component in the presence of a rubber polymer. The polymerization method is not particularly limited, and examples thereof include emulsion polymerization, solution polymerization, bulk polymerization, and suspension polymerization.

[0046] An example of a method for obtaining a rubber-reinforced vinyl resin (B) by emulsion polymerization is a method in which a vinyl monomer component is polymerized in the presence of a rubber polymer latex. This results in a rubber-reinforced vinyl resin (B) latex. The rubber polymer latex can be produced by known methods. Known methods for producing latex include a method in which a molten rubber polymer is homogenized in water by stirring and shearing, and a method in which a polymerizable monomer is emulsion-polymerized in the presence of an emulsifier (see, for example, JP-B 4-30970, JP-B 3403828, and JP-A 11-269206).

[0047] The vinyl monomer component may be polymerized by adding the entire amount to the rubber polymer latex all at once, or by adding it in small amounts in portions or continuously. Polymerization may also be performed by a combination of these methods. Furthermore, the entire amount or a portion of the rubber polymer latex may be added during the polymerization. A polymerization initiator, a chain transfer agent (molecular weight regulator), an emulsifier, etc. may be used in the polymerization.

[0048] Examples of polymerization initiators include redox initiators combining an organic peroxide such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, or paramenthane hydroperoxide with a reducing agent such as sugar-containing pyrophosphate or sulfoxylate; persulfates such as potassium persulfate; and peroxides such as benzoyl peroxide (BPO), azobisisobutyronitrile, lauroyl peroxide, t-butyl peroxylaurate, or t-butyl peroxymonocarbonate. The polymerization initiator may be oil-soluble or water-soluble, or may be used in combination. The polymerization initiator may be used alone or in combination of two or more. The polymerization initiator may be added to the rubber polymer latex all at once or continuously. The amount of polymerization initiator used is preferably 0.1 to 1.5 parts by mass, more preferably 0.2 to 0.7 parts by mass, per 100 parts by mass of the total amount of monomer components.

[0049] Examples of chain transfer agents include mercaptans such as octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, n-hexamethyl mercaptan, n-tetradecyl mercaptan, and t-tetradecyl mercaptan; terpinolenes; and α-methylstyrene dimers. The chain transfer agents can be used alone or in combination of two or more. The chain transfer agent can be added to the rubber polymer latex all at once or continuously. The amount of the chain transfer agent used is preferably 5 parts by mass or less, more preferably 3 parts by mass, per 100 parts by mass of the total amount of the monomer components.

[0050] Examples of emulsifiers include anionic surfactants and nonionic surfactants. Examples of anionic surfactants include sulfate esters of higher alcohols; alkylbenzenesulfonates such as dodecylbenzenesulfonic acid; aliphatic sulfonates such as sodium lauryl sulfate; and aliphatic phosphates. Examples of nonionic surfactants include alkyl ester compounds of polyethylene glycol and alkyl ether compounds. The emulsifiers can be used alone or in combination of two or more. The amount of emulsifier used is, for example, 0.3 to 5 parts by mass per 100 parts by mass of the total amount of the monomer components.

[0051] Emulsion polymerization can be carried out under known conditions depending on the types of vinyl monomer, polymerization initiator, etc. The method for recovering the rubber-reinforced vinyl resin (B) from the latex obtained by emulsion polymerization is not particularly limited, but includes, for example, a method in which the latex is introduced into an aqueous coagulant solution to coagulate the latex and recover the polymer; a method in which an aqueous coagulant solution is introduced into the latex and coagulate the latex and recover the polymer; a method in which the coagulation process is divided into two or more stages with a temperature gradient from low to high and recover the polymer; a method in which the coagulation process is divided into two or more stages with an acidity gradient from weak to strong acidity or from strong to weak acidity and recover the polymer; and a method in which the latex is mixed with an aqueous coagulant solution to form a paste, which is then extruded into warm water through a fine hole to coagulate the paste and recover the polymer. Recovery can also be achieved by selecting and combining two or more of these methods. The coagulant can be, for example, one or more selected from inorganic acids such as sulfuric acid, phosphoric acid, and nitric acid; organic acids such as acetic acid and lactic acid; and inorganic salts such as magnesium sulfate, calcium chloride, magnesium chloride, and sodium chloride. Thereafter, the polymer can be recovered by dehydrating and drying the latex by a known method, for example, using a centrifugal dehydrator or a fluidized bed dryer. In this case, various antioxidants and stabilizers may be added to the latex in advance, if necessary, and these may also be added after emulsification.

[0052] The graft ratio of the rubber-reinforced vinyl resin (B) is typically 10 to 50 mass%, preferably 15 to 120 mass%, more preferably 20 to 100 mass%, and particularly preferably 30 to 80 mass%. If the graft ratio is within this range, the resin composition will have better impact resistance and moldability.

[0053] The graft ratio can be calculated by the following formula (1): Graft ratio (mass%) = {(S - T) / T} × 100 (1) In the formula, S is the mass (g) of the insoluble fraction obtained by adding 1 g of the rubber-modified graft polymer (B) to 20 mL of acetone, shaking the mixture at 25°C for 2 hours using a shaker, and then centrifuging the mixture at 5°C for 60 minutes using a centrifuge (rotation speed: 23,000 ppm) to separate the insoluble and soluble fractions, and T is the mass (g) of the rubbery polymer contained in 1 g of the rubber-reinforced vinyl resin (B). The mass of the rubbery polymer can be calculated from the polymerization formulation and polymerization conversion rate, or obtained by infrared absorption spectroscopy (IR), pyrolysis gas chromatography, CHN elemental analysis, or other methods.

[0054] The graft ratio can be adjusted by appropriately selecting, for example, the type and amount of chain transfer agent used during polymerization of the monomer component, the type and amount of polymerization initiator, the amount of monomer component added during polymerization, the addition method and addition time, the polymerization temperature, etc.

[0055] The intrinsic viscosity [η] of the acetone-soluble portion of the rubber-reinforced vinyl resin (B) (in methyl ethyl ketone at 30°C) is typically 0.1 to 1.5 dL / g, preferably 0.20 to 1.0 dL / g, and more preferably 0.30 to 0.70 dL / g. When the intrinsic viscosity [η] is within the above range, the impact resistance and moldability are better.

[0056] The intrinsic viscosity [η] can be measured by the following method. First, the acetone-soluble portion of the rubber-reinforced vinyl resin (B) is dissolved in methyl ethyl ketone to prepare five measurement samples with different concentrations. Next, an Ubbelohde viscosity tube is used to measure the reduced viscosity of the measurement samples at each concentration at 30°C, and the intrinsic viscosity [η] is determined from the results. The unit is dL / g. The acetone-soluble portion can be obtained by adding 1 g of the rubber-modified graft polymer (B) to 20 mL of acetone, shaking the mixture at 25°C for 2 hours in a shaker, and then centrifuging the mixture at 5°C for 60 minutes in a centrifuge (rotation speed: 23,000 ppm), separating the insoluble portion from the soluble portion (acetone solution of the acetone-soluble portion), and drying the soluble portion (removing the acetone).

[0057] The intrinsic viscosity [η] can be adjusted by, for example, appropriately selecting the type and amount of chain transfer agent used during polymerization of the monomer components, the type and amount of polymerization initiator, the method and time of adding the monomer components during polymerization, the polymerization temperature, the polymerization time, etc. Alternatively, the intrinsic viscosity [η] can also be adjusted by appropriately selecting and mixing two or more rubber-reinforced vinyl resins (B) having different intrinsic viscosities [η].

[0058] <Non-rubber-reinforced vinyl resin (C)> The non-rubber-reinforced vinyl resin (C) is a copolymer containing at least acrylonitrile units and styrene units, and is a copolymer obtained by copolymerizing a monomer mixture (c1) containing acrylonitrile and styrene in the absence of a rubber polymer. The monomer mixture (c1) may contain a monomer other than acrylonitrile and styrene (hereinafter also referred to as "other monomers") as necessary. That is, the non-rubber-reinforced vinyl resin (C) is a copolymer having acrylonitrile units, styrene units, and, as necessary, other monomer units.

[0059] Other monomers that may be contained in the monomer mixture (c1) include the vinyl monomers exemplified above in the description of the rubber-reinforced vinyl resin (B).

[0060] Regarding the proportions of the respective monomers in the monomer mixture (c1), the content of acrylonitrile units is preferably 10 to 45 mass%, more preferably 15 to 40 mass%, and even more preferably 20 to 35 mass%, relative to the total mass of the monomer mixture (c1), and the content of styrene units is preferably 55 to 90 mass%, more preferably 60 to 85 mass%, and even more preferably 65 to 80 mass%. The proportions of the other monomers are preferably 0 to 30 mass%, more preferably 0 to 20 mass%, even more preferably 0 to 10 mass%, and most preferably 0 mass%, relative to the total mass of the monomer mixture (c1).

[0061] The intrinsic viscosity [η] of the acetone-soluble portion of the non-rubber-reinforced vinyl resin (C) (in methyl ethyl ketone at 30°C) is, for example, preferably 0.10 to 1.2 dL / g, more preferably 0.30 to 0.9 dL / g, and even more preferably 0.40 to 0.70 dL / g. When the intrinsic viscosity [η] is within the above range, the impact resistance and moldability are superior. The intrinsic viscosity [η] can be measured by the same method as for the intrinsic viscosity [η] of the rubber-reinforced vinyl resin (B) described above.

[0062] The non-rubber-reinforced vinyl resin (C) can be produced by copolymerizing acetonitrile, styrene, and, if necessary, other monomers. The polymerization method for each monomer can be any known polymerization method, such as emulsion polymerization, suspension polymerization, bulk polymerization, or a combination of these. Only one type of non-rubber-reinforced vinyl resin (C) may be used, or two or more types of non-rubber-reinforced vinyl resins (C) with different monomer compositions, molecular weights, etc. may be mixed and used.

[0063] <Lubricant (D)> Lubricant (D) is a lubricant having a saturated fatty acid ester in which a saturated fatty acid having 12 or more carbon atoms (C12) is ester-bonded to an alcohol. The saturated fatty acid ester may be one obtained by hydrogenating an unsaturated fatty acid ester. Lubricant (D) may be a waxy mixture containing the saturated fatty acid ester as the main component (50% by mass or more relative to the total mass of lubricant (D)) and other components as secondary components.

[0064] Specific examples of saturated fatty acids of C12 or more include saturated fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, arachidic acid, hardened beef tallow oil, and palm oil.

[0065] Examples of fatty acid esters include glycerin fatty acid esters in which a fatty acid is ester-bonded to one or more of the three hydroxyl groups of glycerin, such as monoacylglycerols having one fatty acid, diacylglycerols having two or more fatty acids, and triacylglycerols having three or more fatty acids.

[0066] Specific examples of saturated fatty acid esters of C12 or more include glycerol monostearate, which is a monoacylglycerol, and hydrogenated castor oil, which is a triacylglycerol.

[0067] The melting point of the lubricant (D) is preferably room temperature or higher, more preferably 50°C or higher, and even more preferably 80°C or higher, from the viewpoint of preventing bleeding out from the molded product and long-term stability of physical properties.

[0068] As the lubricant (D), saturated fatty acids or saturated fatty acid esters are preferred from the viewpoint of color development.

[0069] As the lubricant (D), saturated fatty acid esters are preferred over saturated fatty acids from the viewpoint of reducing squeak noise. Among saturated fatty acid esters, triacylglycerols, which have a lower emulsifying effect, are preferred over monoacylglycerols and diacylglycerols.

[0070] The lubricant (D) may be used alone or in combination of two or more. Commercially available products may be used as the lubricant (D). Examples of commercially available products include hydrogenated castor oil.

[0071] <Other Thermoplastic Resins> Examples of other thermoplastic resins other than the above-described components (A) to (D) include polyester resins such as polyethylene terephthalate (PET) resin and polybutylene terephthalate (PBT) resin, and polyurethane (PU) resin. These thermoplastic resins can be used alone or in combination of two or more.

[0072] <Other Additives> The resin composition of this embodiment may contain other additives. Examples of other additives include ultraviolet absorbers, weathering agents, fillers, antioxidants, antiaging agents, antistatic agents, flame retardants, antifogging agents, lubricants, antibacterial agents, tackifiers, plasticizers, and colorants. These additives may be used alone or in combination of two or more.

[0073] <Content Ratio> In the resin composition of this embodiment, the total content of the polycarbonate resin (A), rubber-reinforced vinyl resin (B), non-rubber-reinforced vinyl resin (C), and lubricant (D) is, for example, preferably 50 to 100 mass%, more preferably 60 to 99 mass%, even more preferably 70 to 98 mass%, particularly preferably 80 to 98 mass%, and most preferably 90 to 98 mass%, relative to the total mass of the resin composition. When the content is equal to or greater than the lower limit of the above range, the effects of the present invention are fully exhibited. When the content is equal to or less than the upper limit of the above range, components other than components (A) to (D) (e.g., pigments) can be contained.

[0074] The blending ratios of the above components (A) to (D) in the resin composition of this embodiment can be appropriately selected depending on the required impact resistance, heat resistance, mechanical strength, moldability, etc.

[0075] The proportion of the polycarbonate resin (A) relative to the total mass of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C) is preferably 30% by mass or more, more preferably 40% by mass or more, with the upper limit being preferably 70% by mass or less, more preferably 60% by mass or less. When the proportion of the polycarbonate resin (A) is equal to or greater than the lower limit, the impact resistance and heat resistance are superior. When the proportion of the polycarbonate resin (A) is equal to or less than the upper limit, the mechanical strength and moldability are superior.

[0076] The total content of the rubber-reinforced vinyl resin (B) is preferably 3% by mass or more, more preferably 5% by mass or more, based on the total mass of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C). The upper limit is preferably 16% by mass or less, more preferably 14% by mass or less, and even more preferably 9% by mass or less. When the total content of the rubber-reinforced vinyl resin (B) is equal to or greater than the lower limit, the impact resistance and squeak noise reduction properties are superior. When the content of the rubber-reinforced vinyl resin (B) is equal to or less than the upper limit, the color development properties are superior.

[0077] The content of the ethylene-α-olefin rubber-reinforced resin (B1) is preferably 3% by mass or more, more preferably 5% by mass or more, based on the total mass of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C). The upper limit is preferably 16% by mass or less, more preferably 14% by mass or less, and even more preferably 9% by mass or less. When the content of the ethylene-α-olefin rubber-reinforced resin (B1) is equal to or greater than the lower limit, the impact resistance and squeak noise reduction properties are superior. When the content of the rubber-reinforced vinyl resin (B) is equal to or less than the upper limit, the color development properties are superior.

[0078] The content of the diene rubber-reinforced resin (B2) is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on the total mass of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C). The upper limit is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less. When the content of the diene rubber-reinforced resin (B2) is equal to or greater than the lower limit, the impact resistance is better. When the content of the diene rubber-reinforced resin (B2) is equal to or less than the upper limit, the squeak noise reduction and color development are better.

[0079] The content of the non-rubber-reinforced vinyl resin (C) is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 41% by mass or more, based on the total mass of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C). The upper limit is preferably 60% by mass or less, more preferably 50% by mass or less. When the content of the non-rubber-reinforced vinyl resin (C) is equal to or greater than the lower limit, the impact resistance and squeak noise reduction properties are better. When the content of the non-rubber-reinforced vinyl resin (C) is equal to or less than the upper limit, the color development and glossiness are better.

[0080] The content of the lubricant (D) is preferably 1% by mass or more, more preferably 2% by mass or more, based on the total mass (100% by mass) of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C). The upper limit is preferably 8% by mass or less, more preferably 6% by mass or less, and even more preferably 4% by mass or less. When the content of the lubricant (D) is equal to or greater than the lower limit, the color development and squeak noise reduction properties are better. When the content of the lubricant (D) is equal to or less than the upper limit, the impact resistance, heat resistance, etc. are better.

[0081] From the viewpoint of impact resistance, the content of the other thermoplastic resin is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and most preferably 5% by mass or less, based on the total mass of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C). The lower limit of the content of the other thermoplastic resin is not particularly limited, and may be 0% by mass.

[0082] The content of the other additives is, for example, preferably 0 to 5 mass%, more preferably 0 to 2 mass%, relative to the total mass (100 mass%) of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), and the non-rubber-reinforced vinyl resin (C).

[0083] The melt mass flow rate (MFR) of the resin composition at a temperature of 240°C and a load of 98 N is preferably 20 to 80 g / 10 min, more preferably 35 to 65 g / 10 min, and even more preferably 40 to 55 g / 10 min. If the MFR is equal to or higher than the lower limit, the fluidity and moldability are better. If the MFR is equal to or lower than the upper limit, the impact resistance is better. The MFR is a value measured according to the method specified in ISO 1133.

[0084] The resin composition of this embodiment can be produced, for example, by mixing the polycarbonate resin (A), the rubber-reinforced vinyl resin (B), the non-rubber-reinforced vinyl resin (C), and the lubricant (D), and if necessary, other thermoplastic resins and other additives, using a mixer such as a tumbler mixer or a Henschel mixer, and then melt-kneading the mixture under appropriate conditions using a kneader such as a single-screw extruder, a twin-screw extruder, a Banbury mixer, a kneader, a roll, a feeder ruder, etc. After kneading using a Banbury mixer or kneader, the mixture can also be pelletized using an extruder.

[0085] The order of mixing the components is not particularly limited; some components may be mixed first, followed by the remaining components, or all components may be mixed at once. When kneading the components, the components may be kneaded all at once, or may be kneaded in multiple stages or in separate blends. For fibrous fillers, it is preferable to feed them midway through the extruder using a side feeder to prevent breakage during kneading. The melt-kneading temperature is usually 200 to 300°C, preferably 220 to 280°C.

[0086] The resin composition of the present invention described above contains a polycarbonate resin (A), a rubber-reinforced vinyl resin (B), a non-rubber-reinforced vinyl resin (C), and a lubricant (D), and therefore has excellent color development and squeak noise reduction. Furthermore, since an ethylene-α-olefin rubber-reinforced resin is used as the rubber-reinforced vinyl resin (B), the composition has excellent long-term squeak noise reduction and mechanical properties.

[0087] [Molded Article] The molded article of the second aspect of the present invention comprises the resin composition of the first aspect. The molded article of this aspect can be produced, for example, by molding the resin composition of the first aspect. The molding method is not particularly limited, and examples thereof include known methods such as injection molding, injection compression molding, gas-assisted molding, press molding, blow molding, profile extrusion molding, calender molding, and T-die extrusion molding.

[0088] The molded article of the present invention is suitable for use as, for example, electric or electronic equipment, optical equipment, lighting equipment, office equipment, automobile parts, office equipment parts, housing parts, home appliance parts, and the like.

[0089] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. In the following examples, "%" and "parts" are by mass unless otherwise specified.

[0090] [Measurement Method] <MFR> The MFR of the resin composition pellets was measured according to the method specified in ISO 1133 under the conditions of a temperature of 240°C and a load of 98N.

[0091] <Charpy impact strength (IMP)> Pellets of the resin composition were injection molded using an injection molding machine ("J110AD-180H" manufactured by The Japan Steel Works, Ltd.) at a cylinder temperature of 240°C to obtain test specimens. The IMP of the obtained test specimens was measured at 23°C according to the method specified in ISO 179-1. The higher the IMP, the better the impact resistance, and IMP≧15 kJ / m 2 The impact resistance was judged to be good.

[0092] <Heat Resistance (HDT)> Using an injection molding machine (Toshiba Machine Co., Ltd., "IS55FP-1.5A"), a test piece having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm was prepared from the pelletized thermoplastic resin composition under conditions of a cylinder setting temperature of 260 ° C. and a mold temperature of 30 ° C. The deflection temperature under load (HDT) of the obtained test piece was measured in accordance with ISO 75 using an HDT tester (Toyo Seiki Seisakusho Co., Ltd., "6A-2") under a load of 1.83 MPa and flatwise (4 mm thickness). The higher the HDT value, the better the heat resistance, and it was determined that the heat resistance was good when HDT ≧ 90 ° C.

[0093] <Color Development> Pellets of each thermoplastic resin composition were injection molded under conditions of a cylinder temperature of 240°C, a mold temperature of 60°C, and an injection rate of 20 g / sec to obtain plate-shaped molded articles measuring 100 mm in length, 100 mm in width, and 3 mm in thickness. (Lightness L*) The lightness L* of these molded articles was measured using a spectrophotometer ("CM-3500d" manufactured by Konica Minolta Optips Co., Ltd.) according to the SCE method. The measured L* was designated "L* (ma)." The lower the L*, the blacker the color, and an L* of 9.0 or less was determined to be good color development. "Lightness L*" refers to the lightness value (L*) of the color values ​​in the L*a*b* color system adopted in JIS Z 8729. The "SCE method" refers to a method in which a spectrophotometer conforming to JIS Z 8722 is used to measure color by removing specularly reflected light using a light trap. (Surface Gloss) Using a "Digital Variable Gloss Meter UGV-5D" manufactured by Suga Test Instruments Co., Ltd., the reflectance (%) of the surface of the molded article was measured at an incident angle of 60° and a reflection angle of 60° in accordance with JIS K 7105. A higher reflectance indicates better surface appearance, and a gloss of 100% or greater was determined to indicate good color development.

[0094] <Squeaking noise resistance> Each thermoplastic resin composition was injection molded using a Toshiba Machine IS-170FA injection molding machine at a cylinder temperature of 250°C, an injection pressure of 50 MPa, and a mold temperature of 60°C to obtain an injection-molded plate measuring 150 mm in length, 100 mm in width, and 4 mm in thickness. From this plate, a test piece measuring 60 mm in length, 100 mm in width, and 4 mm in thickness, and a test piece measuring 50 mm in length, 25 mm in width, and 4 mm in thickness were cut using a disc saw. The edges of these two plates, one large and one small, were chamfered with #100 grit sandpaper, and then fine burrs were removed with a cutter knife to prepare the test pieces. Two test pieces were aged for 300 hours in an oven adjusted to 80 ° C ± 5 ° C, and then cooled at 25 ° C for 24 hours. The large and small test pieces were fixed to a ZIEGLER stick-slip tester SSP-02 and rubbed three times with an amplitude of 20 mm under four conditions: a load of 5 N or 40 N and a speed of 1 mm / sec or 10 mm / sec under an atmosphere of 23 ° C and 50% RH. The abnormal noise risk value was measured. The largest abnormal noise risk value was then adopted as the measured value. The higher the abnormal noise risk value, the higher the risk of squeak noise generation, and an abnormal noise risk value of 3 or less is considered good. In this test, aging was performed for 300 hours under the above conditions, so a low abnormal noise risk value indicates that the squeak noise reduction effect is stably exerted over the long term.

[0095] [Materials Used] <Polycarbonate Resin (A)> "Novarex 7022PJ-LH1" (aromatic polycarbonate with Mv of 18,700 (catalog value)) manufactured by Mitsubishi Engineering Plastics Corporation was used.

[0096] <Ethylene-α-olefin rubber-reinforced resin (B1)> A 20 L stainless steel autoclave equipped with a ribbon-type agitator blade, an auxiliary continuous addition device, a thermometer, and the like was charged with 22 parts of an ethylene-α-olefin rubber polymer, an ethylene-propylene-dicyclopentadiene copolymer (ethylene / propylene / dicyclopentadiene=75 / 20 / 5 (%), Mooney viscosity (ML1+4, 100°C) 20, melting point (Tm) 40°C, glass transition temperature (Tg) -50°C), 55 parts of styrene, 23 parts of acrylonitrile, 0.5 parts of t-dodecyl mercaptan, and 110 parts of toluene. The internal temperature was raised to 75°C, and the contents of the autoclave were stirred for 1 hour to obtain a homogeneous solution. Thereafter, 0.45 parts of t-butylperoxyisopropyl monocarbonate was added, and the internal temperature was further raised. After reaching 100 ° C., the polymerization reaction was carried out while maintaining this temperature and stirring at a rotation speed of 100 rpm. From 4 hours after the start of the polymerization reaction, the internal temperature was raised to 120 ° C., and the reaction was carried out for another 2 hours while maintaining this temperature to complete the polymerization reaction. Thereafter, the internal temperature was cooled to 100 ° C., and 0.2 parts of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenol)-propionate and 0.02 parts of dimethyl silicone oil; KF-96-100 cSt (trade name: manufactured by Shin-Etsu Silicones Co., Ltd.) were added, and the reaction mixture was extracted from the autoclave, and the unreacted material and solvent were distilled off by steam distillation. Further, the volatile matter was substantially degassed using a 40 mmφ vented extruder (cylinder temperature 220 ° C., vacuum degree 760 mmHg), and pelletized AES resin (B1) was obtained. The resulting AES resin (B1) had a graft ratio of 70% and an intrinsic viscosity [η] of the acetone soluble portion of 0.47 dl / g.

[0097] <Diene-based rubber-reinforced resin (B2)> 280 parts of water and 60 parts (solids equivalent) of polybutadiene latex having a weight average particle size of 0.26 μm and a gel fraction of 90% as a diene-based rubber polymer, 0.3 parts of sodium formaldehyde sulfoxylate, 0.0025 parts of ferrous sulfate, and 0.01 parts of disodium ethylenediaminetetraacetate were charged into a polymerization vessel equipped with a stirrer. After deoxygenation, the mixture was heated to 60°C with stirring in a nitrogen stream, and then a monomer mixture consisting of 10 parts of acrylonitrile, 30 parts of styrene, 0.2 parts of t-dodecyl mercaptan, and 0.3 parts of cumene hydroperoxide was continuously added dropwise at 60°C over 5 hours. After completion of the dropwise addition, the polymerization temperature was raised to 65°C, and stirring was continued for 1 hour, after which the polymerization was terminated to obtain a graft copolymer latex. The polymerization conversion was 98%. Then, 0.2 parts of 2,2'-methylene-bis(4-ethylene-6-t-butylphenol) was added to the obtained latex, and calcium chloride was added to coagulate the mixture, followed by washing, filtration and drying to obtain a powdery ABS resin (B2). The graft degree of the obtained ABS resin (B2) was 40%, and the intrinsic viscosity [η] of the acetone soluble matter was 0.38 dl / g.

[0098] <Non-rubber-reinforced vinyl resin (C)> As the AS resin (C), an acrylonitrile-styrene copolymer was used, in which the proportions of acrylonitrile units and styrene units were 27% and 73%, respectively, and the intrinsic viscosity [η] of the acetone-soluble portion (in methyl ethyl ketone, 30°C) was 0.47 dl / g and the glass transition temperature (Tg) was 103°C.

[0099] <Lubricant (D)> The following lubricants were used. D1: Kao's "Kaowax 85P" (melting point 85-87°C, hydrogenated castor oil, triglyceride saturated fatty acid ester). D2: Kao's "Rheodol MS-60" (melting point 59-62°C, monostearate glyceride, monoglyceride saturated fatty acid ester). D3: Mitsui-Dow Polychemical's "Elbaloy HP661" (melting point 62°C, ethylene-acrylic acid ester terpolymer). D4: EVONIK's "TEGOMER H-Si6441P" (melting point 53°C, polyester-modified polysiloxane).

[0100] <Pigment> "ROYAL BLACK 971G" (trade name) manufactured by Koshigaya Chemical Industry Co., Ltd. was used. This is a masterbatch containing 40% carbon black with an acrylonitrile-styrene copolymer as the base resin.

[0101] [Examples 1 to 6, Comparative Examples 1 to 12] The components shown in Table 1 were mixed in the blending ratios (parts) shown in Table 1 using a Henschel mixer, and then melt-kneaded using a vented twin-screw extruder (manufactured by The Japan Steel Works, Ltd., TEX44, barrel set temperature 260°C) to obtain pellets of a resin composition. The MFR of the obtained pellets was measured using the method described above. In addition, test specimens were molded using the method described above to measure IMP, HDT, and color development, and to evaluate squeak resistance.

[0102]

[0103] In the resin compositions and molded articles of Examples 1 to 6 according to the present invention, the contents of each of the components (A) to (D) are appropriate, and therefore the fluidity, mechanical properties (IMP, HDT), color development (L*, gloss), and squeak noise (noise risk value; quietness) are all well-balanced and excellent. Comparative Examples 1 and 2 do not contain lubricant (D), and therefore exhibit poor squeak noise. Comparative Example 1 has an insufficient content of ethylene-α-olefin-based rubber-reinforced resin (B1), and therefore exhibits poor mechanical properties. Comparative Example 3 does not contain lubricant (D) and has an excessive content of ethylene-α-olefin-based rubber-reinforced resin (B1), and therefore exhibits poor color development. Comparative Example 4 has an insufficient content of ethylene-α-olefin-based rubber-reinforced resin (B1), and therefore exhibits poor mechanical properties and squeak noise. Comparative Example 5 has an excessive content of lubricant (D), and therefore exhibits poor mechanical properties. Comparative Example 6 does not contain an ethylene-α-olefin rubber-reinforced resin (B1) and instead contains a diene rubber-reinforced resin (B2), resulting in poor squeakability. Comparative Example 7 has an excessive total content of rubber-reinforced vinyl resins (B), resulting in poor color development. Comparative Example 8 has an insufficient content of polycarbonate resin (A), resulting in poor mechanical properties and color development. Comparative Example 9 has an excessive content of polycarbonate resin (A), resulting in poor fluidity and squeakability. Comparative Example 11 does not contain a saturated fatty acid ester having 12 or more carbon atoms as the lubricant (D), but instead contains another lubricant, resulting in poor color development and squeakability. Comparative Example 12 does not contain a saturated fatty acid ester having 12 or more carbon atoms as the lubricant (D), but instead contains another lubricant, resulting in poor mechanical properties, color development, and squeakability.

[0104] The resin composition of the present invention is excellent in color development and squeak noise reduction, and is therefore useful as a molding material for articles used in the interior and exterior of vehicles.

Claims

1. A thermoplastic resin composition comprising a polycarbonate resin (A), a rubber-reinforced vinyl resin (B), a non-rubber-reinforced vinyl resin (C) and a lubricant (D), wherein the rubber-reinforced vinyl resin (B) comprises an ethylene-α-olefin-based rubber-reinforced resin (B1) obtained by graft polymerization of a vinyl monomer in the presence of at least an ethylene-α-olefin-based rubber polymer (b1), the non-rubber-reinforced vinyl resin (C) is a copolymer containing at least an acrylonitrile unit and a styrene unit, and the lubricant (D) is a lubricant having a saturated fatty acid ester having 12 or more carbon atoms, and wherein, when the total of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B) and the non-rubber-reinforced vinyl resin (C) is 100 parts by mass, the polycarbonate resin (A) is 30 to 70 parts by mass, the rubber-reinforced vinyl resin (B) is 3 to 16 parts by mass, and the ethylene-α-olefin-based rubber-reinforced resin (B1) is 3 to 16 parts by mass. and the lubricant (D) in an amount of 1 to 8 parts by mass.

2. The thermoplastic resin composition according to claim 1, comprising 20 to 60 parts by mass of the non-rubber-reinforced vinyl resin (C) when the total of the polycarbonate resin (A), the rubber-reinforced vinyl resin (B) and the non-rubber-reinforced vinyl resin (C) is 100 parts by mass.

3. The thermoplastic resin composition according to claim 2, wherein the lubricant (D) is at least one hydrogenated glycerin fatty acid ester.

4. The thermoplastic resin composition according to claim 3, wherein the rubber-reinforced vinyl resin (B) further comprises a diene-based rubber-reinforced resin (B2) obtained by graft polymerization of a vinyl monomer in the presence of a diene-based rubber polymer (b2).

5. A molded article made from the thermoplastic resin composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Information recording and reproducing device

    JP1989269206A

  • Mobile truck

    JP1992030970A

  • Thermoplastic resin composition and method for producing the same, and molded article

    JP2018095722A

  • Polypropylene resin composition, polypropylene resin molded article

    JP2021031561A

  • Deimmunized Shiga toxin A subunit scaffolds and cell-targeting molecules containing same

    JP2023052919A