Method for producing lens
By curving the polarizing laminate to specific radius ratios and aligning it with a mold, the method addresses the issue of low yield and reliability in lens manufacturing, achieving enhanced adsorption and improved lens quality.
Patent Information
- Application Number
- PCT/JP2024/013095
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Existing lens manufacturing methods using polarizing curved laminates often result in low yield due to insufficient adsorption of the laminate to the mold during resin layer formation, leading to frequent falling off and reduced reliability of the manufactured lenses.
The method involves curving the polarizing laminate to specific radius ratios (R_B1/R_1 and R_B2/R_2) to ensure proper alignment and adsorption onto a mold with a curved concave surface, preventing the laminate from falling off during resin layer formation, thereby enhancing yield and reliability.
This approach allows for accurate suppression of the polarizing curved laminate from falling off the mold, resulting in lenses with improved reliability and higher production yield by ensuring excellent adsorption properties during the resin layer formation process.
Smart Images

Figure JP2024013095_03102024_PF_FP_ABST
Abstract
Description
Lens manufacturing method
[0001] The present invention relates to a method for manufacturing a lens.
[0002] BACKGROUND ART There has been proposed a lens for eyeglasses that includes a polarizing laminate (resin substrate) configured such that both sides of a polarizing film are covered with coating layers mainly made of polycarbonate-based resin, polyamide-based resin, or the like.
[0003] This lens (eyeglass lens) is manufactured, for example, by punching a polarizing laminate having an overall flat shape into a predetermined shape, such as a circle in a plan view, with protective films attached to both sides of the polarizing laminate. The polarizing laminate is then subjected to a heat bending process under heat to form a curved polarizing curved laminate. The protective films are then peeled off from the polarizing curved laminate, and the polarizing curved laminate is placed in a mold having a curved recess so that the recess of the mold abuts against the convex portion of the polarizing curved laminate, and a resin layer composed primarily of a resin material such as a polycarbonate resin or a polyamide resin is then formed on the concave surface of the polarizing curved laminate using insert injection molding (see, for example, Patent Document 1).
[0004] In such lens manufacturing methods, the polarizing curved laminate that has been curved by thermal bending is generally designed so that the radius of curvature of the convex portion is approximately the same as the radius of curvature of the concave portion of the mold used in the insert injection molding method, thereby causing the polarizing curved laminate to be adsorbed to the mold.
[0005] However, if the radius of curvature of the convex portion of the polarizing curved laminate and the radius of curvature of the concave portion of the mold used in insert injection molding are set to be approximately the same, when manufacturing a lens by insert injection molding, i.e., when forming a resin layer on the concave surface of the polarizing curved laminate, a slight misalignment in the installation position of the polarizing curved laminate with respect to the mold or the environment in which the polarizing curved laminate is adsorbed may prevent the polarizing curved laminate from being adsorbed to the mold with sufficient adhesiveness, causing the polarizing curved laminate to fall off from the mold, resulting in a decrease in the yield of the lenses manufactured.
[0006] Japanese Patent Application Laid-Open No. 2009-294445
[0007] An object of the present invention is to provide a method for producing lenses that can produce eyeglass lenses from a polarizing curved laminate with high yield and excellent reliability.
[0008] The above object can be achieved by the present invention as set forth in the following (1) to (7): (1) A step of preparing a polarizing laminate having a flat overall shape, the polarizing laminate including a polarizing film, a first resin layer provided on one side of the polarizing film, and a second resin layer provided on the other side of the polarizing film; a first step of obtaining a polarizing curved laminate by bending the polarizing laminate into a curved shape such that one side of the polarizing laminate forms a curved concave surface and the other side of the polarizing laminate forms a curved convex surface; B1 [mm], the radius of curvature R in the orthogonal direction perpendicular to the one direction B2 a second step of bringing the polarizing curved laminate into close contact with a mold having a curved concave surface of R [mm], with the other surface of the polarizing curved laminate that is the curved convex surface facing the mold; and a third step of forming a resin layer bonded to the polarizing curved laminate on the one surface of the polarizing curved laminate that is the curved concave surface while maintaining the polarizing curved laminate in close contact with the mold, wherein the radius of curvature in the one direction of the other surface of the polarizing curved laminate that is the curved convex surface is set to R 1 [mm], and the radius of curvature in the orthogonal direction is R 2 In the first step, the polarizing laminate is curved to obtain the polarizing curved laminate so that either one of the following relational expressions (A) and (B) is satisfied, but the following relational expression (C) is not satisfied, when R is 0.70 [mm]: B1 / R 1 ≦1.00, and 1.00≦R B2 / R 2 ≦1.40... (A) 1.00≦R B1 / R 1 ≦1.40 and 0.70≦RB2 / R 2 ≦1.00... (B) 0.95<R B1 / R 1 < 1.06 and 0.95 < R B2 / R 2 <1.06... (C)
[0009] (2) In the first step, the relational expression (A) is satisfied, and further, 1.07<R 1 / R 2 <1.68, or satisfying the relation (B) and further satisfying 0.59<R 1 / R 2 The method for manufacturing a lens according to (1) above, wherein the polarizing laminate is curved so as to satisfy the relationship of ≡ 0.93.
[0010] (3) The method for manufacturing a lens according to (2) above, wherein in the first step, the polarizing laminate is further curved so as to satisfy the following relational expression (1):
[0011] (4) The radius of curvature R B1 , the radius of curvature R B2 and (3) are each independently 58 mm or more and 523 mm or less.
[0012] (5) The method for manufacturing a lens according to any one of (1) to (4) above, wherein the one direction of the polarizing curved laminate is MD, and the orthogonal direction of the polarizing curved laminate is TD.
[0013] (6) The method for manufacturing a lens according to any one of (1) to (5) above, wherein the first resin layer and the second resin layer are each independently made of a polycarbonate-based resin or a polyamide-based resin as a main material.
[0014] (7) The method for manufacturing a lens according to any one of (1) to (6) above, wherein the glass transition point of the main material is 100° C. or higher and 190° C. or lower.
[0015] According to the present invention, when manufacturing eyeglass lenses using a polarizing curved laminate that has been curved by thermal bending, i.e., when forming a resin layer on the curved concave surface of the polarizing curved laminate, it is possible to reliably suppress or prevent the polarizing curved laminate from falling off from a mold used to form the resin layer. In other words, the polarizing curved laminate can be adsorbed to the mold with excellent adsorption properties. Therefore, highly reliable lenses can be manufactured with a high yield.
[0016] 1 is a perspective view showing an embodiment of sunglasses including a lens having a polarizing curved laminate; FIG. 2 is a vertical cross-sectional view showing an embodiment of a polarizing curved laminate included in a lens; and FIG. 3 is a schematic diagram illustrating a method for manufacturing a lens having a polarizing curved laminate.
[0017] The lens manufacturing method of the present invention will be described in detail below based on preferred embodiments shown in the accompanying drawings.
[0018] In this specification, the term "main material" refers to a constituent material that accounts for 50% by weight or more in each layer. For example, a "coating layer composed primarily of polycarbonate-based resin or polyamide-based resin" means that, when the total weight of the coating layer is 100% by weight, the polycarbonate-based resin or polyamide-based resin contained in the coating layer accounts for 50% by weight or more in the coating layer.
[0019] The method for manufacturing a lens of the present invention includes the steps of: preparing a polarizing laminate 15 having an overall flat shape, the polarizing laminate 15 including a polarizing film 13, a first resin layer 11 provided on one side of the polarizing film 13, and a second resin layer 12 provided on the other side of the polarizing film; a first step of bending the polarizing laminate 15 into a curved shape such that one side of the polarizing laminate 15 forms a curved concave surface and the other side of the polarizing laminate forms a curved convex surface, thereby obtaining a polarizing curved laminate 10; and B1 [mm], the radius of curvature R in the orthogonal direction perpendicular to the one direction B2The method for manufacturing a lens of the present invention includes a second step of closely contacting the polarizing curved laminate 10 with a mold 40 having a curved concave surface of 1 / 2 [mm], with the other side of the polarizing curved laminate 10 that is the curved convex surface facing the mold 40, and a third step of forming a resin layer 35 bonded to the polarizing curved laminate 10 on the one side of the polarizing curved laminate 10 that is the curved concave surface while maintaining the state in which the polarizing curved laminate 10 is closely contacted with the mold 40, thereby obtaining a lens 30. 1 [mm], and the radius of curvature in the orthogonal direction is R 2 [mm], in the first step, the polarizing laminate 15 is curved to obtain the polarizing curved laminate 10 so that either the following relational expression (A) or the following relational expression (B) is satisfied, but the following relational expression (C) is not satisfied:
[0020] 0.70≦R B1 / R 1 ≦1.00, and 1.00≦R B2 / R 2 ≦1.40... (A) 1.00≦R B1 / R 1 ≦1.40 and 0.70≦R B2 / R 2 ≦1.00... (B) 0.95<R B1 / R 1 < 1.06 and 0.95 < R B2 / R 2 <1.06... (C)
[0021] According to this lens manufacturing method, when manufacturing eyeglass lenses 30 using polarizing curved laminate 10 that has been curved by thermal bending, i.e., when forming resin layer 35 on the curved concave surface of polarizing curved laminate 10, it is possible to accurately suppress or prevent falling off of polarizing curved laminate 10 from mold 40 used to form this resin layer 35. In other words, polarizing curved laminate 10 can be adsorbed to mold 40 with excellent adsorption properties. Therefore, highly reliable lenses 30 can be manufactured with a good yield.
[0022] A lens 30 including a polarizing curved laminate 10 manufactured by applying the lens manufacturing method of the present invention is used, for example, as a lens included in sunglasses 100, a type of eyeglasses. Therefore, hereinafter, sunglasses 100 including this lens 30 will first be described before describing the lens manufacturing method of the present invention.
[0023] <Sunglasses> Fig. 1 is a perspective view showing an embodiment of sunglasses equipped with lenses having a polarizing curved laminate, and Fig. 2 is a longitudinal cross-sectional view showing an embodiment of a polarizing curved laminate equipped with the lenses. In Fig. 1, when the sunglasses are worn on a user's head, the surface of the lens facing the user's eyes is referred to as the back side, and the opposite side is referred to as the front side. In Fig. 2, for convenience of explanation, the upper side of Fig. 2 is referred to as "top" and the lower side is referred to as "bottom."
[0024] As shown in FIG. 1, the sunglasses 100 include a frame 20 and lenses 30 (eyeglass lenses).
[0025] In this specification, the term "lens" includes both a lens having a light-condensing function and a lens having no light-condensing function.
[0026] The frame 20 is a member that is worn on the user's head and positions the lenses 30 in front of and near the user's eyes.
[0027] The frame 20 has a rim portion 21 , a bridge portion 22 , temple portions 23 , and a nose pad portion 24 .
[0028] The rim portions 21 are ring-shaped and are provided one for each of the right and left eyes, with lenses 30 attached to the inside thereof. This allows the user to view external information through the lenses 30.
[0029] The bridge portion 22 is rod-shaped and is positioned in front of the upper part of the user's nose when the glasses are worn on the user's head, connecting the pair of rim portions 21 together.
[0030] The temple portions 23 are temple-shaped and connected to the edges of the rim portions 21 on the opposite side to the positions where the bridge portions 22 are connected. The temple portions 23 are hung over the user's ears when wearing the glasses on the user's head.
[0031] The nose pads 24 are provided on the edges of the rims 21 that correspond to the nose of the user when the sunglasses 100 are worn on the head of the user, and come into contact with the nose, shaped to correspond to the contacting part of the nose at this time, thereby enabling the sunglasses 100 to be kept stably worn.
[0032] The constituent materials of the components of the frame 20 are not particularly limited, and may be, for example, various metal materials, various resin materials, etc. The shape of the frame 20 is not limited to the illustrated configuration as long as it can be worn on the user's head.
[0033] Lens 30 is a spectacle lens that is attached to each rim portion 21. Lens 30 is a light-transmitting, plate-shaped member that is curved outward, and includes resin layer 35 and polarizing curved laminate 10, and is manufactured using the lens manufacturing method of the present invention, which will be described later.
[0034] The resin layer 35 has optical transparency and is located on the rear side of the lens. When the lens 30 is given a light-collecting function, the resin layer 35 has the light-collecting function.
[0035] The constituent material of the resin layer 35 is not particularly limited as long as it is a resin material that is optically transparent, but examples include various thermoplastic resins, thermosetting resins, and various curable resins such as photocurable resins, and one or more of these can be used in combination.
[0036] Examples of resin materials include polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymers, polyvinyl chloride, polystyrene, polyamide, polyimide, polycarbonate, poly-(4-methylpentene-1), ionomers, acrylic resins, polymethyl methacrylate, acrylonitrile-butadiene-styrene copolymers (ABS resins), acrylonitrile-styrene copolymers (AS resins), butadiene-styrene copolymers, polyesters such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), polyethers, polyether ketones (PEK), and polyether ethers. Examples of suitable resins include polyetherimide (PEEK), polyetherimide, polyacetal (POM), polyphenylene oxide, polysulfone, polyethersulfone, polyphenylene sulfide, polyarylate, aromatic polyester (liquid crystal polymer), polytetrafluoroethylene, polyvinylidene fluoride, other fluorine-based resins, epoxy resin, phenolic resin, urea resin, melamine resin, silicone resin, polyurethane, etc., as well as copolymers, blends, polymer alloys, etc. that primarily contain these resins. Among these, it is preferable that the resin layer 35 be of the same type as or identical to the resin material that constitutes the first resin layer 11 of the polarizing curved laminate 10, which will be described later. This allows for improved adhesion between the resin layer 35 and the polarizing curved laminate 10.
[0037] The thickness of the resin layer 35 is not particularly limited, but is preferably 0.5 mm to 5.0 mm, and more preferably 1.0 mm to 3.0 mm, for example. This allows the lens 30 to have both relatively high strength and light weight.
[0038] The polarizing curved laminate 10 is a curved resin substrate that is bonded to the outer surface of the resin layer 35, i.e., the curved convex surface, in a curved shape that corresponds to this shape, thereby imparting polarization to the sunglasses 100. As a result, the sunglasses 100 function as polarized sunglasses with polarization. This polarizing curved laminate 10 constitutes the polarizing curved laminate of the present invention, and a detailed description of this will be given later.
[0039] The polarizing curved laminate 10 can be obtained by bending a polarizing laminate 15 having a flat overall shape into a curved shape in the manufacturing method of the lens 30 described below. As shown in Fig. 2 , the polarizing curved laminate 10 includes a polarizing film 13, a first resin layer 11 provided on one side of the polarizing film 13, and a second resin layer 12 provided on the other side of the polarizing film 13, and in this embodiment, further includes an adhesive layer 16 that bonds (adheses) the polarizing film 13 and the first resin layer 11 together, and an adhesive layer 17 that bonds (adheses) the polarizing film 13 and the second resin layer 12 together.
[0040] (Polarizing film 13) The polarizing film 13 has a function of extracting linearly polarized light having a polarization plane in a predetermined direction from incident light (unpolarized natural light). As a result, the light passing through the polarizing curved laminate 10 (polarizing laminate 15) is polarized.
[0041] The polarization degree of the polarizing film 13 is not particularly limited, but is preferably, for example, from 50% to 100%, and more preferably from 80% to 100%. The visible light transmittance of the polarizing film 13 is not particularly limited, but is, for example, preferably from 10% to 80%, and more preferably from 20% to 50%.
[0042] The material for forming such polarizing film 13 is not particularly limited as long as it has the above-mentioned function, and examples thereof include a film obtained by uniaxially stretching a polymer film made of polyvinyl alcohol (PVA), partially formalized polyvinyl alcohol, polyethylene vinyl alcohol, polyvinyl butyral, polycarbonate, ethylene-vinyl acetate copolymer partially saponified product, or the like, which is dyed by adsorbing iodine or a dichroic substance such as a dichroic dye, and polyene-based oriented films such as a dehydrated product of polyvinyl alcohol or a dehydrochlorinated product of polyvinyl chloride.
[0043] Among these, the polarizing film 13 is preferably a film obtained by adsorbing iodine or a dichroic dye onto a polymer film primarily made of polyvinyl alcohol (PVA), dyeing it, and uniaxially stretching it. Polyvinyl alcohol (PVA) is a material that is excellent in transparency, heat resistance, affinity with the dyeing agent iodine or a dichroic dye, and orientation during stretching. Therefore, the polarizing film 13 primarily made of PVA has excellent heat resistance and polarizing ability.
[0044] Examples of the dichroic dye include chloratin fast red, Congo red, brilliant blue 6B, benzopurpurine, chlorazol black BH, direct blue 2B, diamine green, chrysophenone, sirius yellow, direct fast red, and acid black.
[0045] The thickness of the polarizing film 13 is not particularly limited, but is preferably, for example, 5 μm or more and 60 μm or less, and more preferably 10 μm or more and 40 μm or less.
[0046] (First Resin Layer 11 and Second Resin Layer 12) As shown in FIG. 2 , the first resin layer 11 and the second resin layer 12 are provided on the lower surface side (one surface side) and the upper surface side (the other surface side) of the polarizing film 13, respectively, and thereby function as protective layers that protect the polarizing film 13.
[0047] The first resin layer 11 and the second resin layer 12 are not particularly limited, but may be primarily made of a resin material such as a polyamide resin, a polycarbonate resin, or a cellulose resin such as triacetyl cellulose, and may be made of one or a combination of two or more of these materials. Of these, it is preferable that the first resin layer 11 and the second resin layer 12 are primarily made of a polyamide resin or a polycarbonate resin.
[0048] The first resin layer 11 and the second resin layer 12 preferably contain 85% or more of a polycarbonate-based resin, more preferably 90% or more, even more preferably 95% or more, and particularly preferably 97% or more. The first resin layer 11 and the second resin layer 12 preferably contain 85% or more of a polyamide-based resin, more preferably 90% or more, even more preferably 95% or more, and particularly preferably 97% or more.
[0049] Polycarbonate-based resins are excellent in transparency (translucency) and mechanical strength, such as rigidity, and can therefore improve the transparency and impact resistance of the polarizing curved laminate 10. Furthermore, polycarbonate-based resins have a specific gravity of approximately 1.2, making them classified as a light type of resin among resin materials, and therefore can contribute to reducing the weight of the polarizing curved laminate 10. Furthermore, polyamide-based resins can improve chemical resistance, stress resistance, and the like, in addition to transparency and impact resistance.
[0050] The polyamide resin is not particularly limited, and various resins can be used, such as alicyclic polyamide and semi-aromatic polyamide. Alicyclic polyamide is a material with excellent impact resistance. Therefore, the polarizing curved laminate 10 can exhibit excellent impact resistance. Furthermore, semi-aromatic polyamide is a material with a high elastic modulus. Therefore, the polarizing curved laminate 10 can exhibit excellent resistance to stresses such as bending.
[0051] In this specification, semi-aromatic polyamide refers to a polyamide in which one of the dicarboxylic acid and diamine monomers constituting the polyamide is an aromatic compound and the other is an aliphatic compound, and specifically can be represented by the following formula (1B):
[0052] (However, R in formula (1B) 1 and R 2 one is a divalent aromatic substituent and the other is a divalent aliphatic substituent, and n is an integer of 2 or greater.
[0053] The polyamide may be a copolymer (random copolymer, block copolymer, etc.) containing two or more types of monomers of at least one of dicarboxylic acid and diamine.
[0054] In addition, R in the above formula (1B) 1 , R 2 Of these, the aromatic substituent is preferably one represented by the following formula (2B).
[0055] (In formula (2B), l and m each independently represent an integer of 0 or more and 2 or less.)
[0056] This makes it possible to more suitably protect the polarizing film 13 and improve the processability of the polarizing curved laminate 10. Furthermore, when retardation is imparted to the resin layers 11 and 12, the retardation can be more easily controlled by stretching the resin layers 11 and 12.
[0057] R in the above formula (1B) 1 , R 2 The aliphatic substituent is preferably a substituent having 4 to 18 carbon atoms, more preferably a hydrocarbon group having 4 to 18 carbon atoms, and even more preferably a saturated hydrocarbon group having 4 to 18 carbon atoms. This provides better processability for the polarizing curved laminate 10.
[0058] Furthermore, the semi-aromatic polyamide preferably contains an aromatic dicarboxylic acid and an aliphatic diamine as constituent monomers, which can better protect the polarizing film 13 and improve the processability of the polarizing curved laminate 10. In addition, retardation can be more easily controlled by stretching.
[0059] Alicyclic polyamides have an alicyclic chemical structure in their molecules, and may have an alicyclic chemical structure in their main chain structure or in their side chain structure.
[0060] Examples of the alicyclic polyamide include compounds in which at least one of dicarboxylic acid and diamine monomers constituting the polyamide has an alicyclic chemical structure, and specifically, for example, can be represented by the following formula (3B):
[0061] (However, in formula (3B), R 3 , R 4 are each independently a hydrogen atom or a hydrocarbon group having 4 or less carbon atoms, o is an integer of 2 or more and 14 or less, p is an integer of 0 or more and 6 or less, and n is an integer of 2 or more.
[0062] The polycarbonate resin is not particularly limited and various resins can be used, but aromatic polycarbonate resins are preferred. Aromatic polycarbonate resins have aromatic rings in their main chains, which contributes to the strength of the polarizing curved laminate 10.
[0063] The aromatic polycarbonate resin is synthesized, for example, by an interfacial polycondensation reaction between bisphenol and phosgene, or an ester exchange reaction between bisphenol and diphenyl carbonate.
[0064] Examples of bisphenols include bisphenol A and bisphenols (modified bisphenols) which are the origin of the repeating units of polycarbonates represented by the following formula (1A).
[0065] (In formula (1A), X represents an alkyl group, aromatic group, or cycloaliphatic group having 1 to 18 carbon atoms; Ra and Rb each independently represent an alkyl group having 1 to 12 carbon atoms; m and n each represent an integer of 0 to 4; and p represents the number of repeating units.)
[0066] Specific examples of bisphenols that are the source of the repeating units of the polycarbonate represented by formula (1A) include 4,4'-(pentane-2,2-diyl)diphenol, 4,4'-(pentane-3,3-diyl)diphenol, 4,4'-(butane-2,2-diyl)diphenol, 1,1'-(cyclohexanediyl)diphenol, 2-cyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 2,3-biscyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 1,1'-bis(4-hydroxy-3-methylphenyl)cyclohexane, and 2,2'-bis(4-hydroxy-3-methylphenyl)propane, and these can be used alone or in combination of two or more.
[0067] In particular, the polycarbonate resin preferably contains, as a main component, a bisphenol-type polycarbonate resin having a skeleton derived from bisphenol. By using such a bisphenol-type polycarbonate resin, the polarizing curved laminate 10 exhibits even greater strength.
[0068] The glass transition temperature (Tg) of the resin material contained as the main material in the first resin layer 11 and the second resin layer 12 is preferably 100°C or higher and 190°C or lower, and more preferably 105°C or higher and 155°C or lower. This allows for relatively easy formation of the polarizing curved laminate 10 by heat bending the polarizing laminate 15 in step [3] of the manufacturing method of the lens 30, which will be described later. Furthermore, when retardation is to be expressed in the first resin layer 11 and the second resin layer 12, stretching for expressing this retardation can be suitably performed. Furthermore, the durability and reliability of the polarizing curved laminate 10 can be improved.
[0069] Furthermore, in addition to the resin material contained as the main material, other components may be contained in the first resin layer 11 and the second resin layer 12. Such components are not particularly limited, but may include, for example, a resin material other than the main material, a colorant such as a dye, a filler, an alignment aid, a stabilizer (such as a heat stabilizer, an ultraviolet absorber, or an antioxidant), a plasticizer, a colorant, a flame retardant, an antistatic agent, and a viscosity adjuster.
[0070] In this case, the content of the resin material in the first resin layer 11 or the second resin layer 12 is not particularly limited, but is preferably 75 parts by mass or more, more preferably 85 parts by mass or more, even more preferably 90 parts by mass or more, and particularly preferably 97 parts by mass or more, per 100 parts by mass of the first resin layer 11 or the second resin layer 12. By setting the content of the resin material within the above range, a polarizing curved laminate 10 that exhibits excellent strength can be obtained.
[0071] The materials constituting the first resin layer 11 and the second resin layer 12 may be the same or different.
[0072] Furthermore, when retardation is to be exhibited in the first resin layer 11 and the second resin layer 12, it is preferable that the retardation of the first resin layer 11 and the retardation of the second resin layer 12 are different, and it is preferable that the retardation of the first resin layer 11 is lower than the retardation of the second resin layer 12.
[0073] As a result, the second resin layer 12 is likely to deform in a direction that reduces the curvature due to thermal shrinkage, while the first resin layer 11 is less likely to deform due to thermal shrinkage. Therefore, as shown in FIG. 2 , when applied to a polarizing curved laminate 10 included in a lens 30, the lens 30 is used in a curved state. In this case, it is preferable to form the curved shape so that the second resin layer 12 is located on the curved convex surface side and the first resin layer 11 is located on the curved concave surface side. In this case, the second resin layer 12 has a relatively high thermal shrinkage rate and is therefore relatively susceptible to thermal deformation. However, in the polarizing curved laminate 10, the first resin layer 11 functions to suppress thermal deformation of the second resin layer 12. Therefore, the polarizing curved laminate 10 as a whole can be prevented from excessive deformation due to heat. As a result, deformation of the shape of the lens 30 itself due to thermal deformation of the polarizing curved laminate 10 can be appropriately suppressed or prevented.
[0074] The retardation of the first resin layer 11 is preferably 0 nm or more and 500 nm or less, and more preferably 50 nm or more and 350 nm or less. The retardation of the second resin layer 12 is preferably 2600 nm or more and 8000 nm or less, and more preferably 3500 nm or more and 6500 nm or less. This allows the retardation of the first resin layer 11 to be sufficiently low, and the retardation of the second resin layer 12 to be sufficiently high. Therefore, the polarization performance of the polarizing curved laminate 10 can be sufficiently improved.
[0075] The difference in retardation between the first resin layer 11 and the second resin layer 12 can be realized by varying the constituent materials contained in the layers, the thickness, and the stretching ratio.
[0076] The average thickness of the first resin layer 11 and the second resin layer 12 is not particularly limited, and is preferably, for example, 0.05 mm or more and 0.5 mm or less, and more preferably 0.1 mm or more and 0.4 mm or less.
[0077] The stretching ratio of the first resin layer 11 is not particularly limited, but is preferably, for example, 0.95 to 1.1 so as to be set to the magnitude of the retardation. The stretching ratio of the second resin layer 12 is not particularly limited, but is preferably, for example, 1.5 to 3.5 so as to be set to the magnitude of the retardation.
[0078] It is also preferable that the stretching directions of the first resin layer 11, the second resin layer 12, and the polarizing film 13 are the same, which can further improve the polarization performance of the polarizing curved laminate 10.
[0079] (Adhesive Layer 16 and Adhesive Layer 17) The adhesive layer 16 (first adhesive layer) and the adhesive layer 17 (second adhesive layer) respectively function to bond the polarizing film 13 to the first resin layer 11 and the polarizing film 13 to the second resin layer 12. This can improve the durability of the polarizing curved laminate 10.
[0080] The adhesive (or pressure-sensitive adhesive) constituting the adhesive layers 16, 17 is not particularly limited, and examples thereof include acrylic adhesives, urethane adhesives, epoxy adhesives, and silicone adhesives. Among these, urethane adhesives are preferred. This allows the adhesive layers 16, 17 to have excellent transparency, adhesive strength, and durability, as well as particularly excellent adaptability to shape changes.
[0081] The thickness of the adhesive layers 16, 17 is not particularly limited, but is preferably 5 μm or more and 60 μm or less, and more preferably 10 μm or more and 40 μm or less, for example, so that the adhesive layers 16, 17 can reliably function.
[0082] The adhesive layers 16 and 17 may be omitted depending on the configurations of the first resin layer 11, the second resin layer 12 and the polarizing film 13, etc.
[0083] The polarizing curved laminate 10 preferably has a total thickness of 0.1 mm or more and 2 mm or less.
[0084] In the sunglasses 100 having such a configuration, as described above, the lenses 30 may or may not have a light-collecting function.
[0085] Furthermore, as described above, the sunglasses 100 may have a frame 20 or may have a frameless configuration from the viewpoint of fashionability, lightness, and the like.
[0086] Furthermore, in this embodiment, the eyeglasses of the present invention are applied to sunglasses 100, but this is not limited to this, and the eyeglasses of the present invention may also be, for example, prescription eyeglasses, fashion glasses, goggles that protect the eyes from wind, rain, dust, chemicals, etc.
[0087] In the sunglasses 100 configured as described above, the lenses 30 provided in the sunglasses 100 are manufactured by the manufacturing method of the lenses 30 of the present invention, as will be described below.
[0088] <Method of manufacturing lens> Fig. 3 is a schematic diagram for explaining a method of manufacturing a lens having a polarizing curved laminate. For convenience of explanation, the upper side of Fig. 1 will be referred to as "top" and the lower side as "bottom" below.
[0089] Each step of the method for manufacturing a lens 30 including a polarizing curved laminate 10 is described in detail below. [1] First, a polarizing laminate 15 is prepared that includes a first resin layer 11, a polarizing film 13, and a second resin layer 12, which are laminated in this order to form a flat plate-like overall shape. That is, a polarizing laminate 15 is prepared that includes a polarizing film 13, a first resin layer 11 provided on one side of the polarizing film, and a second resin layer 12 provided on the other side of the polarizing film 13. Protective films 50 (masking tape) are then attached to both sides of the polarizing laminate 15, thereby obtaining a multilayer laminate 150 in which protective films 50 are attached to both sides of the polarizing laminate 15 (see FIG. 1( a)).
[0090] [2] Next, as shown in FIG. 1(b), the prepared multilayer laminate 150, i.e., the polarizing laminate 15 with the protective films 50 attached to both sides thereof, is punched out in the thickness direction to form the multilayer laminate 150 into a circular shape in plan view.
[0091] 1(c), the circular multilayer laminate 150 is subjected to a heat bending process under heating to form the multilayer laminate 150 into a curved multilayer laminate 200 having a curved shape in which the first resin layer 11 side forms a curved concave surface and the second resin layer 12 side forms a curved convex surface. In this way, the flat polarizing laminate 15 can be formed into the curved polarizing curved laminate 10 with the protective films 50 attached to both sides.
[0092] This heat bending is usually performed by press molding or vacuum molding. In this embodiment, as described above, the heating temperature (molding temperature) of the multilayer laminate 150 (polarizing laminate 15) is set to preferably about 110°C or higher and 170°C or lower, more preferably about 140°C or higher and 160°C or lower, taking into consideration the melting or softening temperatures of the resin layers 11 and 12 in the polarizing laminate 15, which includes the resin layers 11 and 12. By setting the heating temperature within this range, the polarizing laminate 15 can be brought into a softened or molten state while preventing alteration or deterioration of the polarizing laminate 15, and the polarizing laminate 15 can be reliably heat-bent into the curved polarizing curved laminate 10.
[0093] The polarizing laminate 15 is curved through the above-described steps [1] to [3], thereby forming a first step of obtaining a polarizing curved laminate.
[0094] [4] Next, the protective film 50 is peeled off from the heat-bent polarizing curved laminate 10. Thereafter, as shown in FIG. 3(d), the radius of curvature in one direction is R B1 [mm], the radius of curvature in the orthogonal direction perpendicular to the one direction is R B2 The polarizing curved laminate 10 is placed in a mold 40 having a curved concave surface measuring 10 mm in size, with the side of the second resin layer 12 (the other side) which is the curved convex surface facing the mold 40, and the second resin layer 12 is brought into contact with the curved concave surface of the mold 40, thereby bringing the polarizing curved laminate 10 into a tightly adhered (adsorbed) state (second step).
[0095] [5] Next, while maintaining the polarizing curved laminate 10 in intimate contact with the mold 40, a resin layer 35 bonded to the polarizing curved laminate 10 is formed on the side of the first resin layer 11 (one surface) that is the curved concave surface of the polarizing curved laminate 10 (third step). This produces a lens 30 that includes the heat-bent polarizing curved laminate 10 and the resin layer 35.
[0096] The resin layer 35 can be made of the same type of material as the first resin layer 11 and the second resin layer 12. When the first resin layer 11 is made of polycarbonate, the resin layer 35 is preferably made of a polycarbonate resin. When the first resin layer 11 is made of polyamide, the resin layer 35 is preferably made of a polyamide resin.
[0097] Furthermore, the resin layer 35 may contain other components in addition to the resin material contained as the main material. Such components are not particularly limited, but may include, for example, a resin material other than the main material, a colorant such as a dye, a filler, an alignment aid, a stabilizer (such as a heat stabilizer, an ultraviolet absorber, or an antioxidant), a plasticizer, a colorant, a flame retardant, an antistatic agent, and a viscosity adjuster.
[0098] In this case, the content of the resin material in the resin layer 35 is not particularly limited, but is preferably 75 parts by mass or more, more preferably 85 parts by mass or more, even more preferably 90 parts by mass or more, and particularly preferably 97 parts by mass or more, per 100 parts by mass of the resin layer 35. By setting the content of the resin material within the above range, a polarizing curved laminate 10 that exhibits excellent strength can be obtained.
[0099] The resin layer 35 is formed on the first resin layer 11 side of this polarizing curved laminate 10 by, for example, using an insert injection molding method, injecting a resin layer 35 made of a resin material onto the curved concave surface of this polarizing curved laminate 10.
[0100] Among insert injection molding methods, injection compression molding is preferably used. Injection compression molding involves injecting the resin material for forming the resin layer 35 into a mold 40 at low pressure, and then closing the mold 40 at high pressure to apply a compressive force to the resin material. This method is therefore preferred because it is less likely to cause molding distortion in the resin layer 35 as a molded body, and therefore optical anisotropy due to the local orientation of resin molecules during molding, in the lens 30. Furthermore, by controlling the mold compression force applied uniformly to the resin material, it is possible to cool the resin material at a constant specific volume, thereby obtaining a resin layer 35 with high dimensional accuracy.
[0101] In the above-described lens manufacturing method, in the present invention, when the polarizing laminate 15 is curved into a curved shape to form the polarizing curved laminate 10 in the step [3], the degree of curvature is determined such that the radius of curvature in the one direction on the curved convex surface on the other surface side of the polarizing curved laminate 10 is R 1 [mm], and the radius of curvature in the orthogonal direction is R 2 When the distance is expressed in mm, it is set so as to satisfy either the following relational expression (A) or the following relational expression (B), but not to satisfy the following relational expression (C).
[0102] 0.70≦R B1 / R 1 ≦1.00, and 1.00≦R B2 / R 2≦1.40... (A) 1.00≦R B1 / R 1 ≦1.40 and 0.70≦R B2 / R 2 ≦1.00... (B) 0.95<R B1 / R 1 < 1.06 and 0.95 < R B2 / R 2 <1.06... (C)
[0103] Here, in forming resin layer 35 on polarizing curved laminate 10 in step [5] of the lens manufacturing method described above, it becomes necessary to adhere curved polarizing curved laminate 10 without dropping it off, with the curved convex surface of polarizing curved laminate 10 corresponding to the curved concave surface of mold 40. That is, it becomes necessary to form resin layer 35 on the curved concave surface of polarizing curved laminate 10 in step [5] while maintaining the close contact of polarizing curved laminate 10 with mold 40 in step [4].
[0104] In particular, when insert injection molding, particularly injection compression molding, is used as a method for forming the resin layer 35, the resin material for forming the resin layer 35 is injected into the mold 40 at low pressure, and at this time, it is necessary to adsorb the polarizing curved laminate 10 onto the curved concave surface of the mold 40 with high positional accuracy.
[0105] Furthermore, when forming the resin layer 35, if the mold 40 is positioned so that the opening of its curved concave surface is aligned vertically, as shown in Figure 3(d), i.e., if the mold 40 is positioned upright in the vertical direction, there is a high possibility that the polarizing curved laminate 10 will fall off from the mold 40. Therefore, at this time, it is necessary to reliably adsorb the polarizing curved laminate 10 to the curved concave surface of the mold 40.
[0106] In response to such a demand, in the step [3], in which the flat polarizing laminate 15 is subjected to a heat bending process under heating to form the curved polarizing curved laminate 10, the curvature of the curved convex surface of the polarizing curved laminate 10 is typically set to be substantially the same as the curvature of the curved concave surface of the mold 40 used in the step [4], thereby producing the polarizing curved laminate 10. However, in this case, there has been a problem in that the polarizing curved laminate 10 frequently falls off from the mold 40, due to which the polarizing curved laminate 10 cannot be adsorbed to the mold 40 with sufficient adhesiveness due to a slight misalignment in the installation position of the polarizing curved laminate 10 relative to the mold 40 or the environment in which the polarizing curved laminate 10 is adsorbed.
[0107] As a result of thorough research into this problem, the inventors have discovered that the frequency of the polarizing curved laminate 10 falling off from the mold 40 can be reduced by intentionally misaligning the curvature of the curved convex surface of the polarizing curved laminate 10 with the curvature of the curved concave surface of the mold 40 rather than making it match.
[0108] The present inventors then conducted further studies on the magnitude of this misalignment. The inventors determined that, when maintaining both the misalignment of the polarizing curved laminate 10 in the one direction and the misalignment in the orthogonal direction relative to the mold 40 at a certain magnitude or greater so as to satisfy either the following relational expression (A) or the following relational expression (B), one of the misalignment of the polarizing curved laminate 10 in the one direction and the other of the misalignment in the orthogonal direction relative to the mold 40 is set to be large and the other to be small, so as to satisfy either the following relational expression (A) or the following relational expression (B). This determined that the polarizing curved laminate 10 can be adhered to the mold 40 with excellent adhesion, thereby accurately reducing or preventing the frequency of the polarizing curved laminate 10 falling off from the mold 40. As a result, the inventors found that highly reliable lenses 30 can be manufactured with a high yield, and completed the present invention.
[0109] 0.70≦R B1 / R 1 ≦1.00, and 1.00≦R B2 / R 2 ≦1.40... (A) 1.00≦RB1 / R 1 ≦1.40 and 0.70≦R B2 / R 2 ≦1.00... (B) 0.95<R B1 / R 1 < 1.06 and 0.95 < R B2 / R 2 <1.06... (C)
[0110] The curvature of the curved concave surface of the mold 40 is set to correspond to the lens 30 to be molded, and is usually set to 1 to 9 curves in both the one direction and the orthogonal direction, and the radius of curvature R B1 , radius of curvature R B2 In terms of the polarization direction of the lens 30, it is preferable that the one direction is MD (machine direction) and the direction orthogonal to the one direction is TD (direction perpendicular to the machine direction).
[0111] When forming such a lens 30, the radius of curvature R is set so as to satisfy either the relational expression (A) or the relational expression (B) above, but not to satisfy the relational expression (C). B1 and the radius of curvature R B2 and the radius of curvature R 1 and the radius of curvature R 2 However, it is preferable to satisfy either one of the following relational expressions (a1) and (b1), and more preferably either one of the following relational expressions (a2) and (b2), while maintaining that the above relational expression (C) is not satisfied. This makes it possible to more significantly reduce the frequency of the polarizing curved laminate 10 falling off from the mold 40.
[0112] 0.75≦R B1 / R 1 ≦0.95 and 1.03≦R B2 / R 2 ≦1.30... (a1) 1.03≦R B1 / R 1 ≦1.30 and 0.75≦R B2 / R 2 ≦0.95... (b1) 0.76≦R B1 / R 1 ≦0.93 and 1.06≦R B2 / R 2 ≦1.29 … (a2) 1.06≦R B1 / R 1 ≦1.29 and 0.76≦R B2 / R 2 ≦0.93... (b2)
[0113] Furthermore, the radius of curvature R 1 and the radius of curvature R 2 It is preferable that at least one of the following two relational expressions is satisfied:
[0114] Specifically, on the one hand, R 1 / R 2 satisfies the relation (A), further, 1.07<R 1 / R 2 <1.68, and 1.26<R 1 / R 2 <1.67. When the relational expression (B) is satisfied, it is more preferable that the relational expression (B) be satisfied. 1 / R 2 <0.93, and 0.60<R 1 / R 2 It is more preferable to satisfy <0.79.
[0115] On the other hand, it is preferable that the following relational expression (1) is satisfied, and it is more preferable that the following relational expression (1') is satisfied.
[0116]
[0117] radius of curvature R B1 and the radius of curvature R B2 and the radius of curvature R 1 and the radius of curvature R 2 By setting the relational expression within the above range, it is possible to more significantly reduce the frequency with which the polarizing curved laminate 10 falls off from the mold 40. As a result, it is possible to manufacture highly reliable lenses 30 with an even higher yield.
[0118] The shape of the lens 30 is formed to be substantially the same as the shape of the mold 40, and the radius of curvature of the lens 30 is R B1 and R B2 After that, a hard coat is formed, polished, and the like to produce a final product.
[0119] Although the lens manufacturing method of the present invention has been described above, the present invention is not limited to this.
[0120] For example, in the method for manufacturing a lens of the present invention, one or more steps can be added for any purpose.
[0121] The present invention will be described in detail below based on examples, but the present invention is not limited thereto. 1. Production of a polarizing curved laminate (Example 1) First, a polyvinyl alcohol film was dyed with an aqueous solution of a dye while being stretched in a water tank, and then treated with boric acid. The treated polyvinyl alcohol film was then washed with water and dried. This resulted in a polarizing film 13 with a thickness of 35 μm.
[0122] On the other hand, a polyamide resin (alicyclic polyamide, Grilamid TR90 manufactured by EMS) was used as the first resin material, and a sheet-like first resin layer 11 having a thickness of 0.2 mm was obtained by extrusion molding using a vented single-screw extruder.
[0123] A polyamide resin ("Grilamid TR90" manufactured by EMS) was used as the second resin material, and a first sheet having a thickness of 0.5 mm was obtained by extrusion molding using a vented single-screw extruder. The first sheet was uniaxially stretched twice while being heated to 120°C, thereby obtaining a sheet-like second resin layer 12 having a thickness of 0.4 mm.
[0124] Next, a two-component moisture-curing polyurethane adhesive (main agent: Mitsui Chemicals, Inc.'s "Takelac A-520", curing agent: Mitsui Chemicals, Inc.'s "Takenate A-50") was applied as a first adhesive to one surface of the first resin layer 11 using a bar coater so that the thickness after drying would be 20 μm. Also, a two-component moisture-curing polyurethane adhesive (main agent: Mitsui Chemicals, Inc.'s "Takelac A-520", curing agent: Mitsui Chemicals, Inc.'s "Takenate A-50") was applied as a second adhesive to one surface of the second resin layer 12 using a bar coater so that the thickness after drying would be 20 μm.
[0125] Next, the first resin layer 11 and the second resin layer 12, on which the first adhesive and the second adhesive were respectively applied, were placed in an oven and heated until the solvent in the first adhesive and the second adhesive dried, thereby obtaining a first laminate in which the adhesive layer 16 (first adhesive layer) was laminated on one surface of the first resin layer 11, and a second laminate in which the adhesive layer 17 (second adhesive layer) was laminated on one surface of the second resin layer 12.
[0126] Thereafter, the first laminate was laminated on one side of the polarizing film 13 so that the adhesive layer 16 was in contact with the polarizing film 13, and the second laminate was laminated on the other side of the polarizing film 13 so that the adhesive layer 17 was in contact with the polarizing film 13, thereby obtaining a polarizing laminate 15. In this process, the first laminate, polarizing film 13, and second laminate were each pressure-bonded using the rubber rolls of a laminator, so that the total thickness of the polarizing laminate 15 was 0.75 mm.
[0127] Then, a protective film 50 made of polyolefin was laminated by a lamination method on both sides of such a polarizing laminate 15, i.e., on the side of the first resin layer 11 opposite the polarizing film 13, and on the side of the second resin layer 12 opposite the polarizing film 13.
[0128] Next, the polarizing laminate 15 was punched out to a diameter of 8 cm, and then subjected to a heat bending process while suctioning at 150°C for 10 minutes using a Rema molding machine (vacuum molding machine) (CR-32 type). This resulted in a radius of curvature R 1 is 80.5 mm, and the radius of curvature R in TD (the direction perpendicular to one direction) 2A polarizing curved laminate 10 of Example 1 having a thickness of 87.2 mm was obtained.
[0129] (Examples 2 to 9, Example 11, Comparative Examples 1 to 3) By appropriately changing the conditions for obtaining the first resin layer 11 and the second resin layer 12, the polarizing laminate 15 was subjected to a heat bending process while being suctioned using a Rema molding machine (vacuum molding machine) (CR-32 type), and the radii of curvature R shown in Table 1 were obtained. 1 and the radius of curvature R 2 The polarizing curved laminates 10 of Examples 2 to 9, Example 11, and Comparative Examples 1 to 3 were obtained in the same manner as in Example 1, except that the polarizing curved laminates 10 had a size of
[0130] Example 10 The first resin material used to form the first resin layer 11 and the second resin material used to form the second resin layer 12 were each a polycarbonate resin (Mitsubishi Engineering Plastics Corporation, "Iupilon E-2000") instead of a polyamide resin (EMS Corporation, "Grilamid TR90"). The polarizing laminate 15 was subjected to hot bending while being suctioned using a Rema molding machine (vacuum molding machine) (CR-32 type), resulting in a radius of curvature R as shown in Table 1. 1 and the radius of curvature R 2 The polarizing curved laminate 10 of Example 10 was obtained in the same manner as in Example 1, except that the polarizing curved laminate 10 had a size of .about.10.
[0131] 2. Evaluation (Removal of Polarizing Curved Laminate 10 from Mold 40) The polarizing curved laminates 10 of each Example and Comparative Example were each evaluated as follows.
[0132] That is, for the polarizing curved laminates 10 of each example and each comparative example, the radius of curvature R B1 [mm] and radius of curvature R B2 The sample was attached to a mold 40 having a curved concave surface with a thickness of 1 / 4 [mm], and whether or not it fell off from the mold 40 after 5 seconds was confirmed.
[0133] The polarizing curved laminates 10 of each Example and Comparative Example were checked for dropout, with 100 pieces for each Example and Comparative Example. The evaluation results obtained in the evaluation of dropout of the polarizing curved laminates 10 are shown in Table 1.
[0134]
[0135] As shown in Table 1, each example satisfies either the following relational expression (A) or the following relational expression (B), but does not satisfy the following relational expression (C), and it has been revealed that the polarizing curved laminate 10 can be prevented from falling off from the mold 40.
[0136] In contrast, in each of the comparative examples, either neither the following relational expression (A) nor the following relational expression (B) was satisfied, or the following relational expression (C) was satisfied, and as a result, the polarizing curved laminate 10 frequently fell off from the mold 40. B1 / R 1 ≦1.00, and 1.00≦R B2 / R 2 ≦1.40... (A) 1.00≦R B1 / R 1 ≦1.40 and 0.70≦R B2 / R 2 ≦1.00... (B) 0.95<R B1 / R 1 < 1.06 and 0.95 < R B2 / R 2 <1.06... (C)
[0137] According to the present invention, when manufacturing eyeglass lenses using a polarizing curved laminate that has been curved by thermal bending, i.e., when forming a resin layer on the curved concave surface of the polarizing curved laminate, it is possible to accurately suppress or prevent the polarizing curved laminate from falling off from a mold used to form the resin layer. In other words, the polarizing curved laminate can be adsorbed to the mold with excellent adsorption properties. Therefore, highly reliable lenses can be manufactured with a high yield. Therefore, the present invention has industrial applicability.
[0138] REFERENCE SIGNS LIST 10 Polarizing curved laminate 11 First resin layer 12 Second resin layer 13 Polarizing film 15 Polarizing laminate 16 First adhesive layer 17 Second adhesive layer 20 Frame 21 Rim portion 22 Bridge portion 23 Temple portion 24 Nose pad portion 30 Lens 35 Resin layer 40 Mold 50 Protective film 100 Sunglasses 150 Multilayer laminate 200 Curved multilayer laminate
Claims
1. A step of preparing a polarizing laminate having an overall shape of a flat plate, the polarizing laminate including a polarizing film, a first resin layer provided on one surface side of the polarizing film, and a second resin layer provided on the other surface side of the polarizing film; a first step of obtaining a polarizing curved laminate by bending the polarizing laminate into a curved shape such that one surface of the polarizing laminate constitutes a curved concave surface and the other surface of the polarizing laminate constitutes a curved convex surface; B1 [mm], the radius of curvature R in the orthogonal direction perpendicular to the one direction B2 a second step of closely contacting the polarizing curved laminate with a mold having a curved concave surface of 1 mm, with the other surface of the polarizing curved laminate being the curved convex surface facing the mold; and a third step of forming a resin layer bonded to the polarizing curved laminate on the one surface of the polarizing curved laminate being the curved concave surface while maintaining the polarizing curved laminate in close contact with the mold, wherein the radius of curvature in the one direction of the other surface of the polarizing curved laminate being the curved convex surface is set to R 1 [mm], and the radius of curvature in the perpendicular direction is R 2 A method for manufacturing a lens, comprising the steps of: in the first step, obtaining the polarizing curved laminate by curving the polarizing laminate so as to satisfy either the following relational formula (A) or the following relational formula (B) but not the following relational formula (C), where R is the angle .alpha. / 2[mm]: 0.70≦R B1 / R 1 ≦1.00, and 1.00≦R B2 / R 2 ≦1.40... (A) 1.00≦R B1 / R 1 ≦1.40 and 0.70≦R B2 / R 2 ≦1.00... (B) 0.95<R B1 / R 1 < 1.06 and 0.95 < R B2 / R 2 <1.06... (C) 2. In the first step, the relational formula (A) is satisfied, and further, 1.07<R 1 / R 2 < 1.68, or the above-mentioned relational expression (B) is satisfied, and further, 0.59 < R 1 / R 2 The method for manufacturing a lens according to claim 1 , wherein the polarizing laminate is curved so as to satisfy the relationship: φ<0.
93.
3. The method for manufacturing a lens according to claim 2, further comprising: in the first step, curving the polarizing laminate so as to satisfy the following relational expression (1):
4. The radius of curvature R B1 , the radius of curvature R B2 The method for manufacturing a lens according to claim 1 , wherein each of the above is independently 58 mm or more and 523 mm or less.
5. A method for manufacturing a lens as described in claim 1, wherein the one direction of the polarizing curved laminate is MD and the orthogonal direction of the polarizing curved laminate is TD.
6. The method for manufacturing a lens according to claim 1, wherein the first resin layer and the second resin layer are each independently made primarily of a polycarbonate-based resin or a polyamide-based resin.
7. The method for manufacturing a lens according to claim 6, wherein the glass transition point of the main material is 100°C or higher and 190°C or lower.
Citation Information
Patent Citations
Polarizing layer laminate and its manufacturing method
JP2009294445A
Polarizing laminate, polarizing lens, and polarizing spectacles
JP2011180266A
Manufacturing method of polarizing lens, polarizing lens made of thermoplastic resin, Anti-glare product and protective product
JP2012022293A
Manufacturing method of polarizing lens, polarizing lens, Anti-glair product, and protective product
JP2012215866A
Method of manufacturing glass polarizing lens utilizing polarizing film suitable for glass lens
JP2022122281A