Polymer and preparation method therefor, gel polymer electrolyte, battery, and electrical device
By using polymers with a specific structure in lithium-ion batteries, the electrolyte gelation is achieved under high temperature or overcharge conditions, reducing the risk of thermal runaway, solving the problem of insufficient thermal stability of lithium-ion batteries, and improving battery performance. safety performance.
Patent Information
- Application Number
- PCT/CN2023/131064
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-11-10
- Publication Date
- 2024-10-31
AI Technical Summary
The accumulation of heat in lithium-ion batteries caused by overcurrent, internal dendrites, etc. may trigger an exothermic chain reaction of the electrolyte, cathode, and other materials, leading to thermal runaway. Existing technology cannot effectively reduce this risk.
Using a polymer with a specific structure, the general formula is formula I, including oxygen, sulfur or imino groups, which can undergo ring-opening polymerization at high temperatures or when the battery is overcharged, causing the electrolyte to gel and increase battery life. Internal resistance, thereby reducing the probability of thermal runaway, and improving the flame retardant effect through halogen substituent groups.
It effectively improves the thermal stability of the battery, reduces the probability of thermal runaway and combustion, and improves the safety performance of the battery.
Smart Images

Figure CN2023131064_31102024_PF_FP_ABST
Abstract
Description
Polymer and preparation method thereof, gel polymer electrolyte, battery and electrical device Technical Field
[0001] The present application belongs to the field of batteries, and specifically relates to polymers and preparation methods thereof, gel polymer electrolytes, batteries and electrical devices. Background Art
[0002] Lithium-ion batteries, known for their green, environmentally friendly, high-energy, and low-carbon nature, are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. With the development of society, people's demands for lithium-ion batteries are becoming increasingly stringent.
[0003] Public content
[0004] In view of the technical problems existing in the background technology, the present application provides a polymer, which aims to improve the thermal stability of the battery and reduce the probability of thermal runaway.
[0005] In order to achieve the above-mentioned object, the first aspect of the present application provides a polymer, the general formula of the polymer is shown in Formula I:
[0006] wherein: m includes 0 and / or 1; n is a positive integer; X1 and X2 each independently include oxygen, sulfur or imino; X3 includes oxygen or sulfur;
[0007] Y includes oxygen, sulfur, imino, -SC 1~8 Alkylene, unsubstituted or substituted -NH-C 1~8 Alkylene, unsubstituted or substituted C 1~8 Alkylene, unsubstituted or substituted C 1~8 Any one of alkyleneoxy; R1, R2, R3, R4 independently include hydrogen, fluorine, unsubstituted or substituted C 1~10 Alkyl, unsubstituted or substituted C 1~10 Any of the alkoxy groups; R5 includes C 1~10 alkyl, Any one of; R9 includes C which is unsubstituted or substituted by any group 1~10 Alkyl; the arbitrary group includes at least one of halogen, alkyl, alkoxy, ester, and carbonyl.
[0008] Compared with the prior art, the polymer of the first aspect of the present application can have the following beneficial effects: the polymer has flame retardant properties. When it is used in a battery (for example, a polymer monomer including a cyclic phosphate compound containing a double bond can be introduced into the electrolyte, and polymerized under the action of an initiator to obtain a polymer network), on the one hand, the polymer can undergo ring-opening polymerization under conditions of high temperature or battery overcharge and other abuse conditions to gel the electrolyte, increase the internal resistance of the battery, and reduce the probability of thermal runaway of the battery. On the other hand, the substituent groups of the polymer can be used to further meet the expected effects. For example, halogen substitution can be used to improve the flame retardant effect or reduce the side reactions of the battery. In summary, introducing the polymer into the battery is beneficial to improving the thermal stability of the battery and reducing the probability of battery combustion and thermal runaway.
[0009] The second aspect of this application provides a method for preparing the polymer described in the first aspect of this application, comprising: self-polymerizing a cyclic phosphate compound containing a double bond; and / or copolymerizing the cyclic phosphate compound containing a double bond with a second polymerizable compound. Compared to the prior art, this method not only produces a polymer having a cyclic phosphate structure, but also allows the specific type or structure of the polymerizable monomer and / or the second polymerizable compound to be selected according to actual needs to meet different additional requirements. This method can be used in the battery field to improve the thermal stability of the battery and reduce the probability of battery combustion and thermal runaway.
[0010] The third aspect of the present application provides a gel polymer electrolyte comprising a polymer matrix and an electrolyte, wherein the polymer matrix comprises the polymer described in the first aspect of the present application or a polymer obtained by the method described in the second aspect of the present application.
[0011] The fourth aspect of the present application provides a battery comprising: the gel polymer electrolyte described in the third aspect of the present application, and / or the polymer obtained by the method described in the second aspect of the present application, and / or the polymer described in the first aspect of the present application.
[0012] The fifth aspect of the present application provides an electrical device, which includes: the battery described in the fourth aspect of the present application.
[0013] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become obvious from the description below, or will be learned through practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0015] FIG1 is a schematic structural diagram of a battery according to an embodiment of the present application.
[0016] FIG2 is a schematic structural diagram of a battery module according to an embodiment of the present application.
[0017] FIG3 is a schematic structural diagram of a battery pack according to an embodiment of the present application.
[0018] FIG4 is an exploded view of a battery pack according to one embodiment of the present application.
[0019] FIG5 is a schematic diagram of an embodiment of an electric device using a battery as a power source according to an embodiment of the present application.
[0020] Reference numerals: 1: secondary battery; 2: battery module; 3: battery pack; 4: upper case; 5: lower case. DETAILED DESCRIPTION
[0021] The present application will be further described below in conjunction with specific embodiments. It should be understood that these specific embodiments are only used to illustrate the present application and are not used to limit the scope of the present application.
[0022] References to "embodiments" in this application mean that a particular feature, structure, or characteristic described in connection with the embodiment may be included in at least one embodiment of the application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described in this application may be combined with other embodiments.
[0023] " Scope " disclosed in the present application is limited in the form of lower limit and / or upper limit, and given range is limited by selecting a lower limit and / or an upper limit, and the selected lower limit and / or the rear upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form the scope of not clearly recording, and any lower limit can be combined with other lower limits to form the scope of not clearly recording, and any upper limit can be combined with any other upper limit to form the scope of not clearly recording. In addition, each separately disclosed point or single numerical value itself can be used as lower limit or upper limit and any other point or single numerical value combination or with other lower limit or upper limit combination to form the scope of not clearly recording.
[0024] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0025] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0026] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps S1 and S2, which means that the method may include steps S1 and S2 performed sequentially, or may include steps S2 and S1 performed sequentially. For example, the method may further include step S3, which means that step S3 may be added to the method in any order, for example, the method may include steps S1, S2, and S3, or may include steps S1, S3, and S2, or may include steps S3, S1, and S2, etc.
[0027] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or comprised, or may mean that only the listed components are included or comprised. Furthermore, as used in this application, the terms "plurality" and "multiple" refer to two or more components.
[0028] Unless otherwise specified, the term "and / or" in this application simply describes an association between related objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. Furthermore, the character " / " in this document generally indicates that the related objects are in an "or" relationship.
[0029] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned description of the drawings and any variations thereof are intended to cover non-exclusive inclusions. Unless otherwise specified, the terms used in this application have the well-known meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0030] With the continued advancement of green environmental protection, the application of lithium-ion batteries has become increasingly widespread in all aspects of life, including vehicles, electronic devices, and energy storage devices. However, as their application continues to deepen, potential problems are also receiving increasing attention. Lithium-ion batteries can accumulate internal heat due to factors such as overcurrent, internal dendrites leading to internal short circuits, or overcharging. When this heat accumulates to a certain level, it triggers an exothermic chain reaction in the electrolyte, cathode, and other internal materials, ultimately leading to thermal runaway.
[0031] In the present application, by using a polymer having a structure shown in Formula I in a battery, the polymer can be used to undergo ring-opening polymerization under conditions of high temperature or battery overcharge or other abuse conditions to gel the electrolyte, thereby increasing the internal resistance of the battery, thereby reducing the probability of thermal runaway of the battery and improving the thermal stability of the battery. At the same time, the expected effect can be further achieved by allowing the polymer to carry a substituent group, for example, halogen substitution can be used to improve the flame retardant effect or reduce the side reactions of the battery.
[0032] In view of this, the first aspect of the present application provides a polymer, the general formula of the polymer is shown in Formula I:
[0033] Wherein: m includes 0 and / or 1; n is a positive integer; X1 and X2 independently include oxygen, sulfur or imino (-NH-); X3 includes oxygen or sulfur; Y includes oxygen, sulfur, imino, unsubstituted or substituted -SC 1~8 Alkylene, unsubstituted or substituted -NH-C 1~8 Alkylene, unsubstituted or substituted C 1~8 Alkylene, unsubstituted or substituted C 1~8 Alkyleneoxy (ie -OC 1~8 any one of alkylene); R1, R2, R3, and R4 are independently hydrogen, fluorine, unsubstituted or substituted C 1~10 Alkyl, unsubstituted or substituted C 1~10 Any of the alkoxy groups; R5 includes C 1~10 alkyl, Any one of; R9 includes C which is unsubstituted or substituted by any group 1~10 Alkyl; the arbitrary group includes at least one of halogen, alkyl, alkoxy, ester, and carbonyl.
[0034] Unless otherwise specified, in this application, "*" represents a connecting portion between the same or different atoms or terminal parts of a chemical formula. It should be understood that the elements or groups at the positions of X1, X2, and X3 can be the same or different. The optional scope of the term "halogen" is fluorine, chlorine, bromine and iodine. The term "C 1~8 "Alkyl" is understood to mean a linear or branched saturated monovalent hydrocarbon radical having 1, 2, 3, 4, 5, 6, 7 or 8 carbon atoms; the term "C 1~8 "Alkoxy" should be understood as -OC 1~8 Alkyl means an alkyl group attached to the rest of the molecule through an oxygen atom. 1~8 "Alkylene" is understood to mean a straight-chain or branched saturated divalent hydrocarbon radical having 1, 2, 3, 4, 5, 6, 7 or 8 carbon atoms; the term "C1~8 "Alkyleneoxy" should be understood as -OC 1~8 Accordingly, the term "C 1~10 "Alkyl" is understood to mean a linear or branched saturated monovalent hydrocarbon radical having 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms; the term "C 1~10 "Alkoxy" should be understood as -OC 1~10 The term "C 3~10 “Alkyl” is understood to mean a linear or branched saturated monovalent hydrocarbon radical having 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms.
[0035] In the term "unsubstituted or substituted by any group", the "substituted by any group" means that at least one hydrogen atom bonded to a carbon atom is replaced by any group other than hydrogen, for example, it may be replaced by fluorine. 1~10 For example, "alkyl" should be understood as C 1~10 Alkyl groups may be unsubstituted or substituted by one or more (such as 1, 2, 3, or 4) substituents at any position. When there are two or more substituents, the multiple substituents may be the same or different, located at the same position or at different positions. In the "substituted by any group" described in this application, the any group includes but is not limited to at least one of halogen, alkyl, alkoxy, ester group, and carbonyl group, wherein the alkyl or alkoxy included in the any group may be chain or cyclic, for example, the any group may include one or more of halogen, chain alkyl, cyclic alkyl, chain alkoxy, and cyclic alkoxy. In addition, it should also be understood that when one or more of "R1", "R2", "R3", "R4", "R5", and "R9" are substituted by "any group", the substituent groups located on "R1", "R2", "R3", "R4", "R5", and "R9" may be the same or different, and the number and substitution positions of the substituent groups located on "R1", "R2", "R3", "R4", "R5", and "R9" are also independent of each other.
[0036] In the polymer of the first aspect of the present application, when m is 0 or 1, even if the polymer has a five-membered ring or a six-membered ring structure, the polymer can have better stability. The polymer having the structure of formula I has a cyclic structure that is the same as or similar to the cyclic phosphate (e.g., the oxygen in the cyclic phosphate is replaced by a sulfur, (im)amino group, etc.), that is, The polymer has good flame retardancy and can improve the thermal stability of the battery. Under conditions of abuse such as high temperature or battery overcharge, it can undergo ring-opening polymerization to gel the electrolyte, increase the internal resistance of the battery, and reduce the probability of thermal runaway of the battery. In addition, the substituent groups of the polymer can be used to further meet the expected effects. For example, halogen substitution can be used to improve the flame retardant effect or reduce the side reactions of the battery. In summary, introducing the polymer into the battery is beneficial to improving the thermal stability of the battery and reducing the probability of battery combustion and thermal runaway. Among them, the structural characterization of the polymer can be combined with infrared spectroscopy (IR), nuclear magnetic resonance (NMR, for example 1 H. 13 C. 19 F. 31 P, etc.), mass spectrometry (MS), elemental analysis, gel permeation chromatography (GPC), laser Raman spectroscopy (LR) and other common methods.
[0037] It is understood that in the general formula shown in Formula I, n represents the number of repeating units in the general formula shown in Formula I, and the value range of n can be selected within a reasonable polymer molecular weight. The polymer of the first aspect of the present application may include multiple compounds that satisfy the general formula shown in Formula I, or may include only a single compound that satisfies the general formula shown in Formula I. When the polymer includes only a single compound that satisfies the general formula shown in Formula I, the value of n in Formula I may be greater than 1, for example, not less than 5 or not less than 10, etc.
[0038] It can be understood that the polymer of the first aspect of the present application can be either a single compound or a compound comprising multiple compounds satisfying the general structure shown in Formula I.
[0039] Furthermore, the polymer of the first aspect of the present application, in addition to satisfying the above conditions, can further control the type, selectable range, average molecular weight of its substituent groups, the type and specific selection of polymerized monomers, etc., to further improve the performance of the polymer, including but not limited to flame retardancy, electrolyte retention, and improvement of battery thermal stability. That is, in addition to satisfying the above conditions, one or more of the following conditions can also be optionally satisfied.
[0040] In some embodiments of the present application, the "halogen" includes fluorine. That is, in Formula I, Y may include oxygen, sulfur, imino, unsubstituted or fluorine-substituted -NH-C 1~8 Alkylene, unsubstituted or fluorine-substituted C 1~8 Alkylene, unsubstituted or fluorine-substituted C 1~8 Any one of the alkyleneoxy groups; R1, R2, R3, and R4 may independently include hydrogen, fluorine, unsubstituted or fluorine-substituted C 1~10 Alkyl, unsubstituted or fluorinated C 1~10Any of the alkoxy groups; R5 may include unsubstituted or fluorine-substituted C 1~10 alkyl, Any one of the following. The polymer having the structural formula described in Formula I has better antioxidant stability after being combined with a fluorine-containing substituent (such as a fluorine-substituted or fluorinated alkyl group). It can not only reduce the heat release value and spontaneous combustion rate of the battery, thereby reducing the probability of battery combustion and thermal runaway, thereby further improving the flame retardancy and thermal stability of the battery, but also passivate the negative electrode, reduce the side reaction between the negative electrode and the electrolyte, and improve the liquid retention of the electrolyte.
[0041] In some embodiments of the present application, X1 and X2 may each independently include oxygen or sulfur; Y may include oxygen, unsubstituted or fluorine-substituted C 1~8 Alkylene, unsubstituted or fluorine-substituted C 1~8 Any one of the alkyleneoxy groups; R1, R2, R3, and R4 may independently include hydrogen, fluorine, unsubstituted or fluorine-substituted C 1~10 Alkyl, unsubstituted or fluorinated C 1~10 Any of the alkoxy groups; R5 may include unsubstituted or fluorine-substituted C 1~10 alkyl, Any one of; R9 includes unsubstituted or fluorine-substituted C 1~10 Alternatively, X1 and X2 may each independently include oxygen; X3 may include oxygen; Y may include oxygen, unsubstituted or fluorine-substituted C 1~8 Alkylene, unsubstituted or fluorine-substituted C 1~8 Any one of the alkyleneoxy groups. Selecting X1, X2, X3, Y, R1, R2, R3, R4, R5, and R9 within the given range can further reduce the probability of battery combustion and thermal runaway.
[0042] In some embodiments of the present application, the average molecular weight of the polymer can be 20,000 to 60,000, such as 25,000, 30,000, 35,000, 40,000, 45,000, 50,000, 55,000, etc., or can be a range composed of any of the above values. The test method for the average molecular weight of the polymer includes but is not limited to gel permeation chromatography (GPC). The polymer can be used in the electrolyte to improve the thermal stability of the battery. If its average molecular weight is too low, it is difficult to form a network polymer, which affects the improvement effect on the thermal stability of the battery. If its average molecular weight is too high, it is difficult to dissolve in the electrolyte. By making the average molecular weight of the polymer within the given range, its dispersibility in the electrolyte can be improved, which is beneficial for its uniform film formation on the surface of the positive and negative electrode sheets, improving the compatibility of the electrolyte with the positive and negative electrode sheets, and at the same time, when it undergoes ring-opening polymerization, it is also beneficial to promote the gelation of the electrolyte, improve the thermal stability of the battery, and reduce the probability of battery combustion and thermal runaway.
[0043] In some embodiments of the present application, in the polymer represented by Formula I, R1, R2, R3, and R4 may independently include unsubstituted or fluorine-substituted C 1~10 Alkyl, unsubstituted or fluorinated C 1~10 Any one of the alkoxy groups; optionally, R1, R2, R3, and R4 may each independently include a C substituted by fluorine 1~10 Alkyl, fluorine-substituted C 1~10 Any of the alkoxy groups. Compared to direct substitution with hydrogen or fluorine, substitution with a (fluoro)alkyl or (fluoro)alkoxy group with 1 to 10 carbon atoms further increases the polymer's molecular weight and forms a network polymer, further improving the battery's thermal stability. Furthermore, substitution with a fluoroalkyl (oxy) chain not only further utilizes the strong electronegativity of the fluorine atom to significantly enhance the polymer's oxidation resistance, improve flame retardancy, and improve the battery's thermal stability, but also reduces side reactions between the electrolyte and the negative electrode. Therefore, selecting R1, R2, R3, and R4 within the given range can further reduce the probability of battery combustion and thermal runaway.
[0044] In some embodiments of the present application, the polymer monomer of the polymer of the general formula shown in Formula I may include a cyclic phosphate compound containing a double bond, and the polymer monomer may enable the polymer to obtain a cyclic phosphate or a cyclic structure similar to the cyclic phosphate structure (the cyclic phosphate or the cyclic structure similar to the cyclic phosphate structure includes ), which is beneficial to improving the thermal stability of the battery. Among them, the cyclic phosphate compounds containing double bonds can self-polymerize or graft copolymerize with other polymerizable compounds to form a network polymer under an initiator or high voltage. When used in a battery, it can have a film-forming effect on the surface of the positive and negative pole pieces of the battery, improve the compatibility of the electrolyte with the positive and negative pole pieces, inhibit the side reaction between the pole pieces and the electrolyte, and reduce the consumption of the electrolyte; in addition, the cyclic phosphate compounds containing double bonds can self-polymerize or copolymerize with other polymerizable compounds to form a network polymer, which can further increase the molecular weight of the polymer and improve the thermal stability of the battery. It should be noted that the "cyclic phosphate compounds" described in this application may include but are not limited to compounds having cyclic phosphates, compounds that are controlled by any group (such as fluorine, (sub)amino, sulfur, (sub)alkoxy, (sub)alkyl, -NH-C 1~8 and compounds having a cyclic phosphate ester substituted with at least one of an alkylene group, an alkylene group, and a cyclic phosphate ester having a similar cyclic structure (such as any oxygen in the cyclic phosphate ester is replaced by sulfur, (im) amino, (im) alkyl, (im) alkoxy, -NH-C 1~8 Alkylene, -SC 1~8As long as the cyclic phosphate compound containing a double bond can self-polymerize or copolymerize with other polymerizable compounds to obtain a polymer of the general formula shown in Formula I, the "cyclic phosphate compound" may include
[0045] In some embodiments of the present application, the polymer monomer of the polymer represented by Formula I may be solely a cyclic phosphate compound containing a double bond, wherein the cyclic phosphate compound containing a double bond may be of the same type or may include a plurality of different cyclic phosphate compounds containing a double bond. When used in a battery, the polymer monomer may be polymerized and then introduced into the electrolyte, or the polymer monomer may be directly added to the electrolyte and self-polymerized by adding an initiator or under high pressure. Using only a cyclic phosphate compound containing a double bond as a polymer monomer can further impart a better flame retardant effect to the polymer, thereby significantly improving the thermal stability of the battery.
[0046] In some embodiments of the present application, the polymer monomers of the polymer represented by Formula I may include: For example, the polymerizable monomers of the polymer represented by formula I may include but are not limited to In the actual operation process, the polymer monomers satisfying the general formula can be self-polymerized to obtain the polymer shown in Formula I, or the polymer monomers satisfying the general formula can be copolymerized with other polymerizable compounds to obtain the polymer shown in Formula I.
[0047] In some embodiments of the present application, the polymer shown in Formula I may include at least one of the 276 compounds shown in Structural Formulas I-1 to I-276. The 276 compounds shown in Structural Formulas I-1 to I-276 can be used alone in the battery, or any two or more of them can be mixed and used in the battery. The 276 compounds shown in Structural Formulas I-1 to I-276 have a five-membered ring or six-membered ring structure of a cyclic phosphate, have good stability, and can utilize fluorine substituents to further improve their antioxidant properties and passivation effect on the negative electrode. Using them in batteries can improve the thermal stability of the battery and reduce the probability of battery combustion and thermal runaway.
[0048] The structures of the 276 compounds represented by structural formula I-1 to structural formula I-276 are as follows:
[0049] In some embodiments of the present application, the polymer monomer of the polymer represented by Formula I may further include, in addition to the cyclic phosphate compound containing a double bond, a second polymerizable compound, wherein the second polymerizable compound is a polymerizable compound different from the cyclic phosphate compound containing a double bond. In this case, the general formula of the polymer may be as shown in Formula II:
[0050] Wherein: a and b are independently positive integers, and 0.5≤a / b≤4, for example, the value of a / b can be 0.5, 1, 1.5, 2, 2.5, 3, 3.5 or 4, or can be any range of the above values. R6 is C 3~10 Alkyl, unsubstituted or substituted by any of the above groups C 3~10 Epoxy, unsubstituted or substituted by any of the above groups C 3~10 Allyl, unsubstituted or substituted by any of the above groups C 3~10 (Meth)acryloyl, unsubstituted or substituted by any of the above groups, C 3~10 Any one of the acrylates. The polymer represented by Formula II and the polymer represented by Formula I both have a cyclic phosphate structure and can undergo ring-opening polymerization under conditions of abuse such as high temperature or battery overcharge to gel the electrolyte, thereby improving the thermal stability of the battery and reducing the probability of battery combustion and thermal runaway. In addition, the polymer can also have the characteristics of a second polymerizable compound. For example, the second polymerizable compound can be a polymer monomer of a gel polymer electrolyte. Thus, after copolymerization of the cyclic phosphate compound containing a double bond and the polymer monomer of the gel polymer, the resulting polymer can have both good flame retardant effects and the characteristics of a gel polymer electrolyte. Its use in batteries is also beneficial in reducing the probability of liquid electrolyte leakage and the probability of electrode corrosion, oxidative combustion, etc. caused by leakage, improving the volume expansion of the battery during charging and discharging, and further improving the thermal stability of the battery. Among them, in the compound shown in Formula II, a is the degree of polymerization of the cyclic phosphate compound containing a double bond, and b is the degree of polymerization of the second polymerizable compound. If a is too small relative to b, it is not conducive to improving the flame retardant properties of the polymer. If a is too large relative to b, it is not conducive to making the polymer meet the characteristics of the second polymerizable compound. Controlling the value of a / b within the given range is beneficial to making the polymer shown in Formula II have both good flame retardant properties and the characteristics of the second polymerizable compound.
[0051] In some embodiments of the present application, the second polymerizable compound may include at least one of a polymerizable monomer, oligomer, and copolymer of a gel polymer electrolyte, and the second polymerizable compound within the given range may be copolymerized with a cyclic phosphate compound containing a double bond to form a gel phase. The second polymerizable compound may include, but is not limited to, methyl methacrylate, styrene, methyl acrylate, ethyl acrylate, acrylic acid, trimethylsilyl methacrylate, acrolein dimethyl acetal, acrolein diethyl acetal, 2-phenoxyethyl acrylate, tridecafluoro-2-hydroxynonyl ester, trifluoroethyl methacrylate, propenyl-1,3-sultone, glycidyl methacrylate, acrylamide, trifluoroethyl acrylate, (acryloxymethyl) dimethylmethoxysilyl acrylate, Alkane, cyanoethyl acrylate, hydroxyethyl acrylate, triallyl trimesic acid ester, hydroxypropyl acrylate, 3-(perfluoro-3-methylbutyl) 2-hydroxypropyl acrylate, 1-vinyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-allyl-3-ethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-allyl-1-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide, 1,6-bis(acryloyloxy)-2,2,3,3,4,4,5,5-octadecyl At least one of fluorohexane, pentafluorophenol acrylate, vinylene carbonate, maleic anhydride, ethyl cyanoacrylate, butyl acrylate, hexafluoroisopropyl methacrylate, hexafluorobutyl methacrylate, 2-hydroxy-3-phenoxypropyl acrylate, hydroxyethyl methacrylate, and vinyl carbonate; further, the second polymerizable compound can be selected from at least one of vinylene carbonate, maleic anhydride, ethyl cyanoacrylate, butyl acrylate, hexafluoroisopropyl methacrylate, hexafluorobutyl methacrylate, hydroxypropyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, hydroxyethyl methacrylate, and vinyl carbonate. Selecting the second polymerizable compound within the given range can make the polymer have both good flame retardant properties and gel polymer electrolyte properties, which can not only improve the thermal stability of the battery and reduce the probability of battery combustion and thermal runaway, but also improve the liquid retention of the electrolyte and buffer the volume expansion of the battery during charging and discharging.
[0052] The second aspect of the present application provides a method for preparing the polymer described in the first aspect of the present application, comprising: allowing a cyclic phosphate compound containing a double bond to self-polymerize; and / or, allowing a cyclic phosphate compound containing a double bond to copolymerize with a second polymerizable compound. Both methods can produce polymers containing a cyclic phosphate structure. It can be understood that the characteristics and effects described for the polymer described in the first aspect of the present application are also applicable to the method for preparing the polymer described in the second aspect of the present application, and will not be repeated here. In general, compared with the prior art, this method can not only obtain a polymer having a cyclic phosphate structure, but also select the specific type or structure of the polymerization monomer and / or the second polymerizable compound according to actual needs to meet different additional requirements. It can be used in the battery field to improve the thermal stability of the battery and reduce the probability of battery combustion and thermal runaway.
[0053] In some embodiments of the present application, before the cyclic phosphate compound containing a double bond is self-polymerized or copolymerized with the second polymerizable compound, a polymerizable monomer of the cyclic phosphate compound containing a double bond may be prepared first. For example, an intermediate product may be prepared first, and then the intermediate product may undergo a cyclization or substitution reaction. For example:
[0054] Reaction formula I:
[0055] Reaction formula II:
[0056] In some specific embodiments of the present application, referring to the general reaction formula I, the method for preparing a polymer monomer of a cyclic phosphate compound containing a double bond may include: and A cyclization reaction occurs to obtain the general formula of compounds.
[0057] In some specific embodiments of the present application, referring to the general reaction formula II, the method for preparing a polymer monomer of a cyclic phosphate compound containing a double bond may include: Substitution reaction occurs with Y′-R8 to obtain the general formula and / or It is understood that Y′-R8 can be a single compound or a mixture of multiple compounds that meet the requirements of Y′-R8.
[0058] wherein m includes 0 and / or 1; X1' and X2' independently include hydroxyl, thiol or amino; X1 and X2 independently include oxygen, sulfur or imino; R1, R2, R3 and R4 independently include hydrogen, fluorine, unsubstituted or substituted C 1~10 Alkyl, unsubstituted or substituted C 1~10Any one of the alkoxy groups; R7 and R8 independently include C 2~11 Olefin; Y' includes hydrogen, hydroxyl, mercapto or amino; Y "includes oxygen, sulfur or imino; R9 includes C unsubstituted or substituted by any group 1~10 Alkyl; said arbitrary group includes at least one of halogen, alkyl, alkoxy, ester, and carbonyl. It is understood that All of them can be used as polymerization monomers of cyclic phosphate compounds containing double bonds.
[0059] In some embodiments of the present application, It may include but is not limited to at least one of ethylene glycol, ethylenedithiol, 2-mercaptoethanol, mercaptoethylamine, ethanolamine, ethylenediamine, 1,3-propylene glycol, 1,3-propylenedithiol, 3-mercapto-1-propanol, 3-amino-1-propanol, 3-mercapto-1-propylamine, and 1,3-propylenediamine, as long as it can react with The reaction forms a five-membered ring or a six-membered ring.
[0060] In some embodiments of the present application, the compound in the reaction formula I And the compound in the reaction formula II The synthesis method includes but is not limited to the method shown in reaction formula III and reaction formula IV, wherein, in reaction formula III, as a specific example, Br-R7 can be made into allyl bromide, P(OEt)3 (triethyl phosphite) is reacted with allyl bromide, and the prepared allyl diethyl phosphate is dissolved in an organic solvent (such as acetonitrile), anhydrous potassium iodide is added, argon is protected, trimethylsilyl chloride (TMSCl) is added dropwise at room temperature, and after a period of reaction, trimethylsilyl chloride and solvent are removed, dichloromethane is added, oxalyl chloride is added dropwise at room temperature, and after a period of reaction, it is distilled under reduced pressure to obtain
[0061] Reaction formula III:
[0062] Reaction formula IV:
[0063] In some specific embodiments of the present application, referring to the following reaction formula, the methods for preparing the polymer monomer of the cyclic phosphate compound containing a double bond may include but are not limited to the following:
[0064] The obtained monomers I-12', I-49', I-192', I-84' and I-108' can be used as monomers for polymer I-12, polymer I-49, polymer I-192, polymer I-84 and polymer I-108, respectively.
[0065] As a specific example, the method for preparing the polymer monomer I-12' may include: (a) synthesizing Specifically, triethyl phosphite (19.5 g, 117 mmol) and allyl bromide (17.3 g, 143 mmol) were heated at 70°C for 24 h, and the mixture was distilled to remove impurities to obtain a colorless liquid (19.5 g, yield: 93.56%), which was directly used in the next step. The above-mentioned colorless liquid diethyl allyl phosphate (25.0 g, 150 mmol) was dissolved in acetonitrile (100 mL), and anhydrous potassium iodide (42.0 g, 300 mmol) was added under argon protection. Trimethylsilyl chloride (68.0 g, 600 mmol) was added dropwise at room temperature. After the addition was complete, the system was reacted at 40°C for 2 h. Excess trimethylsilyl chloride and acetonitrile were removed by distillation under reduced pressure, and 100 mL of dichloromethane was added dropwise at room temperature to add oxalyl chloride (51.0 g, 600 mmol) and (0.5 mL) DMF. After the addition was complete, the mixture was stirred at room temperature for 16 h. The product was obtained by distillation under reduced pressure to obtain a colorless liquid. (14.3 g, yield: 60%). (b) Cyclization reaction: Specifically, 3,3,3-trifluoro-1,2-propanediol (10.52 g, 80.9 mmol) and triethylamine (22.5 mL, 161.8 mmol) were dissolved in anhydrous tetrahydrofuran (100 mL), protected by argon, and stirred at room temperature for 5 min. The mixture was cooled to -20°C and added dropwise. The reaction mixture was stirred at room temperature for 3 h. After completion, the mixture was quenched with water (50 mL), extracted with ethyl acetate (100 mL x 2), and washed with 0.1 M hydrochloric acid (100 mL x 2) and saturated brine (50 mL x 2). The organic phase was dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to remove the organic solvent to obtain a colorless liquid (10.89 g, 62.34%), yielding polymerized monomer I-12'.
[0066] The target product was obtained by 1 H NMR, 13 C NMR, 19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (CDCl3, 400MHz), δ (ppm): 5.70 (m, 1H), 5.01 (m, 2H), 4.74 (m, 2H), 4.12 (m, 1H), 3.68 (m, 2H); 13 C NMR (CDCl3, 100MHz), δ (ppm): 132.7, 115.9, 114.5, 100.4, 64.9, 28.8; 19F NMR (CDCl3, 376MHz), δ (ppm): -78.9; 31 P NMR (CDCl3, 160MHz), δ (ppm): 44.2; HRMS (ESI + )m / z[M] + calcd.for C6H8F3O3P:216.0163.found:216.0169.
[0067] As a specific example, the synthesis method of polymer I-12 includes: placing 1.5g of polymer monomer I-12' and 32mg of AIBN (azobisisobutyronitrile) in a 25mL single-necked bottle, solidifying the system in liquid nitrogen, evacuating to vacuum with an oil pump and maintaining for 10 minutes, then melting and filling with argon, repeating this process four times, and finally stirring in an oil bath at 70°C for 22 hours. After the reaction is complete, the solution is added dropwise to 20mL of n-hexane for precipitation. Solid precipitates, which are filtered to obtain 1.23g of solid (yield: 82%). Elemental analysis of the target product: Calcd: C, 33.35; H, 3.75; F, 26.38; O, 22.21; P, 14.33. Found: C, 34.15; H, 3.65; O, 21.28; P, 14.52. M n :36000,PDI:1.8.
[0068] As a specific example, the method for preparing the polymerizable monomer I-49' may include: (a) synthesizing As shown above. (b) The cyclization reaction is carried out. The detailed process refers to the method for preparing the polymerization monomer I-12'. The target product is obtained by 1 H NMR, 13 C NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (CDCl3, 400MHz), δ (ppm): 5.70 (m, 1H), 5.01 (m, 2H), 2.86 (m, 4H), 2.02 (m, 2H); 13 C NMR (CDCl3, 100MHz), δ (ppm): 132.7, 115.9, 31.7, 31.1; 31 P NMR (CDCl3, 160MHz), δ (ppm): 43.6; HRMS (ESI + )m / z[M] + calcd.for C5H9S2OP:179.9832.found:179.9837.
[0069] As a specific example, the method for preparing the polymer monomer I-192' may include: (a) synthesizing Specifically, 3,3,3-trifluoro-1,2-propylene glycol (10.52 g, 80.9 mmol) and triethylamine (15.23 g, 150.5 mmol) were dissolved in dichloromethane (80 ml), and phosphorus oxychloride (11.78 g, 76.8 mmol) was added dropwise at 5 ° C. After the addition was completed, the reaction was continued for 2 hours. Triethylamine hydrochloride was removed by filtration, the filtrate was dried over anhydrous magnesium sulfate, concentrated under reduced pressure to remove dichloromethane, and recrystallized from toluene to obtain (11.51 g, yield: 70.12%). (b) Perform a substitution reaction, specifically, (11.15 g, 53.0 mmol) and triethylamine (2.46 mL, 17.7 mmol) were dissolved in anhydrous dichloromethane (50 mL) under argon protection and stirred at room temperature for 5 min. Propylene thiol (4.33 g, 58.3 mmol) was added dropwise and stirred at room temperature for 2 h. After the reaction was completed, water (50 mL) was added to quench the reaction, and the mixture was extracted with ethyl acetate (100 mL × 2 times), washed with 0.1 M hydrochloric acid (100 mL × 2 times) and saturated brine (50 mL × 2 times). The organic phase was dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to remove the organic solvent to obtain a white solid (8.49 g, yield: 64.58%), and the polymerized monomer I-192' was obtained. The obtained target product was treated by 1 H NMR, 13 C NMR, 19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (CDCl3, 400MHz), δ (ppm): 5.96 (m, 1H), 5.06 (m, 2H), 4.12 (m, 1H), 3.68 (m, 2H), 3.23 (m, 2H); 13 C NMR (CDCl3, 100MHz), δ (ppm): 132.7, 115.9, 113.8, 99.2, 63.7, 21.0; 19 F NMR (CDCl3, 376MHz), δ (ppm): -76.8; 31 P NMR (CDCl3, 160MHz), δ (ppm): 43.2; HRMS (ESI + )m / z[M] + calcd.for C6H8F3O3PS:247.9884.found:247.9879.
[0070] As a specific example, the method for preparing the polymer monomer I-84' may include: (a) synthesizing As shown above. (b) The target product is subjected to a substitution reaction. Specifically, the detailed process is referred to the method for preparing the polymer monomer I-192'. 1 H NMR, 13 C NMR, 19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (CDCl3, 400MHz), δ (ppm): 5.89 (m, 1H), 5.23 (m, 2H), 4.70 (m, 2H), 4.18 (m, 2H), 4.12 (m, 1H); 13 C NMR (CDCl3, 100MHz), δ (ppm): 137.5, 115.1, 114.5, 96.6, 69.0, 61.1; 19 F NMR (CDCl3, 376MHz), δ (ppm): -74.3; 31 P NMR (CDCl3, 160MHz), δ (ppm): 46.7; HRMS (ESI + )m / z[M] + calcd.for C6H8F3O4P:232.0112.found:232.0118.
[0071] As a specific example, the method for preparing the polymer monomer I-108' may include: (a) synthesizing As shown above. (b) The target product is subjected to a substitution reaction. Specifically, the detailed process is referred to the method for preparing the polymer monomer I-192'. 1 H NMR, 13 C NMR, 19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (DMSO-d6, 400MHz), δ (ppm): 5.83 (m, 1H), 5.16 (m, 2H), 4.12 (m, 1H), 3.68 (m, 2H), 3.32 (m, 2H), 2.12 (s, 1H); 13 C NMR (DMSO-d6, 100MHz), δ (ppm): 134.3, 114.9, 114.2, 97.7, 62.2, 37.4; 19F NMR (DMSO-d6, 376MHz), δ (ppm): -73.2; 31 P NMR ((DMSO-d6,160MHz), δ (ppm): 44.8; HRMS (ESI + )m / z[M] + calcd.for C6H9F3NO3P:231.0272.found:231.0268.
[0072] As a specific example, the method for preparing the polymer monomer I-60' may include: (a) synthesizing As shown above. (b) Substitution reaction is carried out to obtain polymer monomer I-60', namely The specific detailed process refers to the method for preparing the polymer monomer I-12'. 1 H NMR, 13 C NMR, 19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (DMSO-d6, 400MHz), δ (ppm): 5.70 (s, 1H), 5.03 (s, 1H), 4.97 (s, 1H), 3.62 (m, 1H), 2.82 (m, 2H), 2.0 (s, 2H); 13 C NMR (DMSO-d6, 100MHz), δ (ppm): 132.7, 120.1, 115.9, 53.7, 31.4, 18.2; 19 F NMR (DMSO-d6, 376MHz), δ (ppm): -72.8; 31 P NMR ((DMSO-d6,160MHz), δ (ppm): 46.8; HRMS (ESI + )m / z[M] + calcd.for C6H8F3OPS2:247.9706.found:247.9748.
[0073] As a specific example, the method for preparing the polymer monomer I-125' may include: (a) synthesizing As shown above. (b) Substitution reaction is carried out to obtain polymer monomer I-125', namely The specific detailed process refers to the method for preparing the polymer monomer I-12'. 1 H NMR, 13 C NMR,19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (DMSO-d6, 400MHz), δ (ppm): 5.70 (s, 1H), 5.03 (s, 1H), 4.97 (s, 1H), 4.74 (m, 2H), 3.85 (s, 4H); 13 C NMR (DMSO-d6, 100MHz), δ (ppm): 132.7, 115.9, 114.4, 81.1, 28.8; 19 F NMR (DMSO-d6, 376MHz), δ (ppm): -89.2; 31 P NMR ((DMSO-d6,160MHz), δ (ppm): 47.4; HRMS (ESI + )m / z[M] + calcd.for C6H9F2O3P:198.0257.found:198.0271.
[0074] As a specific example, the method for preparing the polymer monomer I-137' may include: (a) synthesizing refer to The synthesis of (b) Substitution reaction was carried out to obtain the polymer monomer I-137', namely The specific detailed process refers to the method for preparing the polymer monomer I-192'. 1 H NMR, 13 C NMR, 19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (DMSO-d6, 400MHz), δ (ppm): 5.89 (s, 1H), 5.23 (s, 2H), 4.70 (m, 2H), 4.35 (s, 4H); 13 C NMR (DMSO-d6, 100MHz), δ (ppm): 137.5, 115.1, 114.4, 77.3, 69.0; 19 F NMR (DMSO-d6, 376MHz), δ (ppm): -87.5; 31 P NMR ((DMSO-d6,160MHz), δ (ppm): 47.9; HRMS (ESI + )m / z[M] +calcd.for C6H9F2O4P:214.0207.found:214.0241.
[0075] As a specific example, the method for preparing the polymerizable monomer I-149' may include: (a) synthesizing Reference monomer I-137' was synthesized by (b) Substitution reaction was carried out to obtain polymer monomer I-149', namely The specific detailed process refers to the method for preparing the polymer monomer I-192'. 1 H NMR, 13 C NMR, 19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (DMSO-d6, 400MHz), δ (ppm): 5.89 (s, 1H), 5.23 (s, 2H), 4.20 (m, 2H), 2.88 (s, 4H); 13 C NMR (DMSO-d6, 100MHz), δ (ppm): 137.5, 118.7, 115.1, 74.2, 31.9; 19 F NMR (DMSO-d6, 376MHz), δ (ppm): -88.3; 31 P NMR ((DMSO-d6,160MHz), δ (ppm): 46.5; HRMS (ESI + )m / z[M] + calcd.for C6H9F2O2PS2:245.9750.found:245.9721.
[0076] As a specific example, the method for preparing the polymer monomer I-173' may include: (a) synthesizing As shown above. (b) Substitution reaction was carried out to obtain the polymer monomer I-173', namely The specific detailed process refers to the method for preparing the polymer monomer I-192'. 1 H NMR, 13 C NMR, 19 F NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1H NMR (DMSO-d6, 400MHz), δ (ppm): 5.96 (s, 1H), 5.12 (s, 1H), 5.03 (s, 1H), 3.85 (s, 4H), 3.23 (m, 2H); 13 C NMR (DMSO-d6, 100MHz), δ (ppm): 132.7, 115.9, 113.7, 79.9, 21.0; 19 F NMR (DMSO-d6, 376MHz), δ (ppm): -73.2; 31 P NMR ((DMSO-d6,160MHz), δ (ppm): 44.8; HRMS (ESI + )m / z[M] + calcd.for C6H9F2O3PS:229.9978.found:229.9986
[0077] As a specific example, the method for preparing the polymer monomer I-205' may include: (a) synthesizing As shown above. (b) Substitution reaction is carried out to obtain polymer monomer I-205', namely The specific detailed process refers to the method for preparing the polymer monomer I-12'. 1 H NMR, 13 C NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (DMSO-d6, 400MHz), δ (ppm): 5.70 (s, 1H), 5.03 (s, 1H), 4.97 (s, 1H), 3.83 (m, 2H), 2.75 (m, 2H), 2.0 (s, 2H); 13 C NMR (DMSO-d6, 100MHz), δ (ppm): 132.7, 115.9, 79.7, 29.8, 23.5; 31 P NMR ((DMSO-d6,160MHz), δ (ppm): 43.3; HRMS (ESI + )m / z[M] + calcd.for C5H9O2PS:164.0061.found:164.0037.
[0078] As a specific example, the method for preparing the polymer monomer I-229' may include: (a) synthesizing As shown above. (b) Substitution reaction is carried out to obtain polymer monomer I-229', namely The specific detailed process refers to the method for preparing the polymer monomer I-12'. 1 H NMR, 13 C NMR, 31 The results were characterized and analyzed by P NMR and HRMS. 1 H NMR (DMSO-d6, 400MHz), δ (ppm): 5.70 (s, 1H), 5.03 (s, 1H), 4.97 (s, 1H), 3.79 (m, 2H), 2.84 (m, 2H), 2.0 (m, 3H); 13 C NMR (DMSO-d6, 100MHz), δ (ppm): 132.7, 115.9, 79.6, 39.9, 29.7; 31 P NMR ((DMSO-d6,160MHz), δ (ppm): 42.6; HRMS (ESI + )m / z[M] + calcd.for C5H 10 NO2P:147.0449.found:147.0468.
[0079] In some specific embodiments of the present application, the preparation method of the cyclic phosphate compound containing a double bond may further include: reacting the compound obtained by the reaction formula I Carry out sulfurization reaction; and / or react the obtained product of general formula II and / or For example, a solution of Lawesson reagent (2,4-bis(p-methoxyphenyl)-1,3-dithiodiphosphatane-2,4-sulfide) in tetrahydrofuran (THF) can be used to carry out the sulfidation reaction under heating conditions (such as constant temperature heating) to obtain a compound of the general formula The polymerization monomers, and / or the general formula is obtained and / or The polymerization monomer can be understood by referring to the following reaction formula:
[0080] In some embodiments of the present application, the cyclic phosphate compound containing a double bond may include one or more polymerized monomers, for example, it may include at least one of the polymerized monomer I-12' of polymer I-12, the polymerized monomer I-49' of polymer I-49, the polymerized monomer I-84' of polymer I-84, the polymerized monomer I-108' of polymer I-108, and the polymerized monomer I-192' of polymer I-192.
[0081] In some embodiments of the present application, the self-polymerization of the cyclic phosphate compound containing a double bond and / or the copolymerization of the cyclic phosphate compound containing a double bond with the second polymerizable compound can be carried out under the conditions of an initiator, and the initiator can include at least one of azobisisobutyronitrile, azobisisoheptanenitrile, 2,2 "-azabis (2-imidazoline) dihydrochloride, 2,2'-azobisisobutylamidine dihydrochloride, benzoyl peroxide, tert-butyl peroxide benzoyl, and methyl ethyl ketone peroxide. Under the action of the initiator within the given range, the self-polymerization and / or copolymerization reaction is carried out, which is conducive to the formation of a network polymer and can also be passed through By adjusting the amount of initiator and the conditions used, the polymerization rate and degree of polymerization can be controlled, thereby facilitating the production of polymers within the desired molecular weight range. Alternatively, based on the total mass of the cyclic phosphate compound containing a double bond and the second polymerizable compound, the amount of initiator used can be 1 wt% to 10 wt%, for example, 2 wt%, 4 wt%, 6 wt%, 8 wt%, 10 wt%, or any range thereof. Controlling the amount of initiator within this range can further improve the polymerization rate and degree of polymerization, thereby further facilitating the production of polymers within the desired molecular weight range.
[0082] The third aspect of the present application provides a gel polymer electrolyte, which includes: a polymer matrix and an electrolyte, wherein the polymer matrix includes the polymer of the first aspect of the present application or the polymer prepared by the method of the second aspect of the present application. It can be understood that the electrolyte may include a solvent and a lithium salt, and the solvent may be a non-aqueous solvent. Optionally, the solvent may include a main solvent and an auxiliary solvent, wherein the main solvent may dissolve the lithium salt and improve the electrochemical stability of the electrolyte, and the auxiliary solvent may reduce the viscosity of the electrolyte and further improve the ionic conductivity. It should be noted that the characteristics and effects described for the polymer of the first aspect of the present application and the method for preparing the polymer of the second aspect of the present application are also applicable to the gel polymer electrolyte of the third aspect of the present application and will not be repeated here. In general, the gel polymer electrolyte can not only improve the thermal stability of the battery and reduce the probability of combustion and thermal runaway, but also alleviate the volume expansion caused by the charge and discharge process to a certain extent, and improve the volume stability during the cycle.
[0083] In some embodiments of the present application, the main solvent in the electrolyte may include, but is not limited to, one or more of an ester solvent, an ether solvent, a sulfone solvent, a nitrile solvent, and an ionic liquid solvent. Among them, the ester solvent may include, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), ethylene sulfite (ES), propylene sulfite (PS), dimethyl sulfite (DMS), diethyl sulfite (DES), γ-butyrolactone (BL), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methylpropyl carbonate (MPC), methyl formate (MF), ethyl formate (EF), methyl acetate (MA), ethyl acetate (EA), ethyl propionate (EP), ethyl butyrate (EB), and one or more of their fluorinated derivatives. Ether solvents may include but are not limited to dimethoxymethane (DMM), ethylene glycol dimethyl ether (DME), ethylene glycol diethyl ether (DEE), 1,2-dimethoxypropane (DMP), diethylene glycol dimethyl ether (DGM), tetrahydrofuran (THF), tetrahydropyran (THP), 1,3-dioxolane (DOL), 1,3-dioxane (1,3-DXA), 1,4-dioxane (1,4-DXA), and one or more thereof, and their fluorinated derivatives. Sulfone solvents include but are not limited to dimethyl sulfone, dimethyl sulfoxide, sulfolane, ethyl methyl sulfone, tetramethylene sulfoxide, ethyl methyl sulfoxide, diethyl sulfone, diethyl sulfoxide, methyl phenyl sulfone, methyl phenyl sulfoxide, ethyl phenyl sulfone, ethyl phenyl sulfoxide, vinyl phenyl sulfone, vinyl phenyl sulfoxide, and one or more thereof, and their fluorinated derivatives. Using the main solvent within the range given above can improve the dissolution of lithium salts and make the electrolyte have good ion transport properties.
[0084] In some embodiments of the present application, the auxiliary solvent in the electrolyte can be a solvent that does not dissolve lithium salts but is well miscible with the main solvent. Generally speaking, electrolytes with low lithium salt concentrations have low viscosity and high conductivity, but slightly poor electrochemical stability. High-concentration electrolytes have a high viscosity because most solvent molecules can react with Li + The combination forms a solvated shell structure, which has high electrochemical stability. However, the high viscosity and low ion mobility caused by high concentration will lead to a decrease in the electrical performance of the electrolyte. The auxiliary solvent that does not dissolve the lithium salt but is well miscible with the main solvent is regarded as a diluent. The gel polymer electrolyte of the third aspect of the present application forms a local high-concentration electrolyte by adding a diluent to the high-concentration electrolyte. It can retain the characteristics of the high-concentration electrolyte and also obtain the advantages of low viscosity and high ionic conductivity of the low-concentration electrolyte. That is, the electrolyte can combine the advantages of low-concentration electrolyte and high-concentration electrolyte, so that it has both high ion mobility and good electrochemical stability, thereby further improving the kinetic performance of the battery.
[0085] In some embodiments of the present application, the auxiliary solvent in the electrolyte may include but is not limited to cyclohexane, benzene, toluene, p-xylene, m-xylene, o-xylene, fluorobenzene, p-difluorobenzene, m-difluorobenzene, o-difluorobenzene, trifluorotoluene, trifluoromethoxybenzene, decafluoropentane, perfluoropentanone, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, bis(2,2,2-trifluoroethyl)ether, 1,1,2,3,3,3-hexafluoropropyl ethyl ether , 1H,1H,5H octafluoropentyl 1,1,2,2-tetrafluoroethyl ether, ethyl trifluoromethyl ether, difluoromethyl-2,2,3,3,3 pentafluoropropyl ether, heptafluoropropyl-1,2,2,2-tetrafluoroethyl ether, difluoromethyl 2,2,3,3-tetrafluoropropyl ether, perfluoroisopropyl methyl ether, 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, ethyl-1,1,2,2-tetrafluoroethyl ether, ethyl-2,2,2-tetrafluoroethyl ether, bis(1,1,2,2-tetrafluoroethyl) ether, etc. Optionally, the auxiliary solvent in the electrolyte may include one or more of trifluoromethoxybenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane. The auxiliary solvent within the given range has a high electrochemical window, good compatibility, and good ability to promote the formation of fluorine-rich SEI. Combining it with the main solvent can not only improve the ionic conductivity and electrochemical stability of the electrolyte, but also help reduce the side reactions between the electrolyte and the negative electrode.
[0086] In some embodiments of the present application, the lithium salt in the electrolyte may include, but is not limited to, one or more of lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiOTF), lithium difluorophosphate (LiDFP), lithium dioxalatoborate (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium difluorodioxalatophosphate and lithium tetrafluorooxalatophosphate, for example, lithium bis(fluorosulfonyl)imide may be selected. The above lithium salts can decompose on the surface of the negative electrode to form an SEI component rich in inorganic fluorine, and at the same time have good dissociation ability, which is conducive to achieving higher electrolyte ion conductivity and lower electrolyte viscosity, thereby improving the electrochemical performance of the battery.
[0087] In some embodiments of the present application, the electrolyte may further include an initiator and a polymer monomer of the polymer matrix, and the initiator is used to initiate polymerization of the polymer monomer of the polymer matrix to form the polymer matrix. Optionally, additives may be added to the electrolyte according to actual needs to achieve the desired effect. For example, additives that inhibit the dissolution of transition metals may be added, and / or additives that promote film formation may be added. Among them, the additives that promote film formation may include but are not limited to propane sultone, vinyl sulfate, vinyl sulfite, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trifluoroethyl) phosphate, tris(trifluoroethyl) phosphite, tris(trimethylsilane) borate, dimethyl maleic anhydride and 1,4-diisocyanate. One or more of the additives within the given range are selected to further help improve the stability of the positive and negative electrodes of the battery and extend the life of the battery.
[0088] In some embodiments of the present application, the mass proportion of the polymer matrix in the gel polymer electrolyte can be 0.5 wt% to 25 wt%, for example, 1 wt%, 3 wt%, 5 wt%, 7 wt%, 9 wt%, 11 wt%, 13 wt%, 15 wt%, 17 wt%, 19 wt%, 21 wt%, 23 wt%, 25 wt%, or any range thereof. Alternatively, the mass proportion of the polymer matrix in the gel polymer electrolyte can be 5 wt% to 25 wt%, or further optionally 5 wt% to 12 wt%. With respect to the polymer composition used in the present application, if the mass proportion of the polymer matrix in the gel polymer electrolyte is too small, it is difficult to achieve a good flame retardant effect and improve the thermal stability of the battery. If the mass proportion of the polymer matrix is too large, it is easy to cause increased polarization, decreased ionic conductivity, and shorten the cycle life of the battery. By controlling the mass proportion of the polymer matrix in the gel polymer electrolyte within the given range, it is possible to simultaneously take into account the electrochemical performance and thermal stability of the battery, which is beneficial for reducing the probability of battery combustion and thermal runaway, and also obtaining a longer battery life.
[0089] A fourth aspect of the present application provides a battery comprising: the gel polymer electrolyte described in the third aspect of the present application, and / or a polymer obtained using the method described in the second aspect of the present application, and / or the polymer described in the first aspect of the present application. Optionally, the battery may be a secondary battery, for example, a lithium metal secondary battery or a lithium ion battery.
[0090] In some embodiments of the present application, when preparing a battery, the formation process of the gel polymer electrolyte includes but is not limited to: mixing the main solvent, auxiliary solvent and lithium salt of the gel polymer electrolyte, as well as the polymer monomer and initiator of the polymer matrix, and injecting the obtained mixed solution into the battery cell for packaging and curing. For example, the curing operation can be maintained at 50°C to 70°C for 8h to 12h to polymerize the polymer monomer to form a polymer matrix, and then allowed to stand. When characterizing the polymer matrix in the battery, the battery can be disassembled, and the obtained gel polymer electrolyte can be vacuum-dried to remove the solvent, washed to remove the lithium salt, and then dissolved with an appropriate amount of good solvent. Finally, it is filtered by sedimentation with n-hexane to obtain the polymer matrix. When characterizing the structure of the polymer matrix, infrared spectroscopy (IR) and nuclear magnetic resonance (NMR, for example) can be combined. 1 H. 13 C. 19 F. 31 P, etc.), mass spectrometry (MS), elemental analysis, gel permeation chromatography (GPC), laser Raman spectroscopy (LR) and other common methods.
[0091] In some embodiments of the present application, a battery may include a positive electrode sheet, a negative electrode sheet, a separator, and the gel polymer electrolyte. During the battery's charge and discharge processes, active ions are intercalated and released between the positive and negative electrode sheets. The separator is disposed between the positive and negative electrode sheets to provide isolation. The gel polymer electrolyte conducts ions between the positive and negative electrode sheets.
[0092] [Positive electrode]
[0093] In a battery, the positive electrode sheet typically includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material. The positive electrode current collector can be a conventional metal foil or a composite current collector (a composite current collector can be formed by disposing a metal material on a polymer substrate). As an example, the positive electrode current collector can be aluminum foil.
[0094] In the present application, the specific type of positive electrode active material is not limited, and active materials that can be used for battery positive electrodes known in the art can be used, and those skilled in the art can select according to actual needs. For example, the positive electrode active material may include but is not limited to lithium transition metal oxides and / or olivine structure lithium phosphate positive electrode active materials, the lithium transition metal oxides may include undoped and / or optionally doped modified lithium transition metal oxides, uncoated and / or coated modified lithium transition metal oxides, the olivine structure lithium phosphate may include undoped and / or optionally doped modified olivine structure lithium phosphates, uncoated and / or coated modified olivine structure lithium phosphates. The positive electrode active materials within the given range can be obtained either by preparation or by commercial channels.
[0095] In some specific embodiments of the present application, the positive electrode active material can be selected from lithium transition metal oxides. Optionally, the lithium transition metal oxides can include but are not limited to lithium cobalt oxides (such as LiCoO2, etc.), lithium nickel oxides (such as LiNiO2, etc.), lithium manganese oxides (such as LiMnO2, LiMn2O4, etc.), lithium nickel manganese oxides, lithium nickel cobalt manganese oxides (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (abbreviated as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (abbreviated as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (abbreviated as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (abbreviated as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (abbreviated as NCM 811 ), LiNi 0.96 Co 0.02 Mn 0.02 O2 (referred to as Ni 96 ) etc.), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2, etc.) and its modified compounds, etc.
[0096] In some specific embodiments of the present application, the positive electrode active material may include a lithium-containing phosphate with an olivine structure, for example, may include but is not limited to at least one of lithium iron phosphate (such as LiFePO4 (abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0097] In some specific embodiments of the present application, the positive electrode active material layer may also optionally include a binder, a conductive agent and other optional additives. As an example, the conductive agent may include but is not limited to one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene and carbon nanofibers. As an example, the binder may include but is not limited to one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).
[0098] [Negative electrode]
[0099] In a battery, the negative electrode plate typically includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material. The negative electrode current collector can be a conventional metal foil or a composite current collector (for example, a metal material disposed on a polymer substrate to form a composite current collector). As an example, the negative electrode current collector can be copper foil.
[0100] In some embodiments of the present application, the battery of the fourth aspect of the present application can be a lithium-ion battery. In this case, the specific type of negative electrode active material is not limited, and active materials that can be used for battery negative electrodes known in the art can be used. Those skilled in the art can flexibly choose according to actual needs. As an example, the negative electrode active material may include but is not limited to one or more of artificial graphite, natural graphite, hard carbon, soft carbon, silicon-based materials and tin-based materials. Alternatively, the silicon-based material may include one or more of elemental silicon, silicon oxide compounds (such as silicon monoxide), silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Alternatively, the tin-based material may include one or more of elemental tin, tin oxide compounds, and tin alloys. The negative electrode active material within the given range can be obtained either by preparation or by commercial channels.
[0101] In some specific embodiments of the present application, the negative electrode active material may include a silicon-based material, such as a composite negative electrode active material doped with a silicon-based material and a carbon material. The use of silicon-based materials in the negative electrode active material layer is beneficial to further improve the energy density of the battery. Optionally, the silicon content in the negative electrode active material may be not less than 10wt%.
[0102] In some specific embodiments of the present application, the negative electrode active material layer may optionally include a binder, a conductive agent and other optional additives. As an example, the conductive agent may include but is not limited to one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. As an example, the binder may include but is not limited to one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB). As an example, other optional additives may include but are not limited to thickeners and dispersants (such as sodium carboxymethyl cellulose CMC-Na), PTC thermistor materials.
[0103] In some embodiments of the present application, the battery of the fourth aspect of the present application may be a lithium metal secondary battery, in which case its negative electrode material may include, but is not limited to, metallic lithium. For example, the negative electrode material may also be an alloy of metallic lithium and various other metal or non-metal elements. Optionally, the metal elements may include, but are not limited to, tin (Sn), zinc (Zn), aluminum (Al), magnesium (Mg), silver (Ag), gold (Au), gallium (Ga), indium (In), platinum (Pt), etc.; further optionally, the non-metal elements may include, but are not limited to, boron (B), carbon (C), silicon (Si), etc.
[0104] In some embodiments of the present application, the battery of the fourth aspect of the present application can also be a negative electrode-free lithium metal battery. In this case, the negative electrode is composed of only a metal foil current collector, and there is no lithium metal on its surface. During the cycle, only the lithium in the positive electrode is used, and it is precipitated and peeled off in the form of lithium metal on the negative electrode side.
[0105] In some embodiments of the present application, the isolation membrane in the battery may include but is not limited to a polyethylene porous membrane, a polypropylene porous membrane, a polyimide porous membrane, and a porous membrane formed by a composite of multiple polymers.
[0106] In some embodiments of the present application, the shape of the battery in the fourth aspect of the present application is not particularly limited, and those skilled in the art can flexibly select it according to actual needs. For example, it can be cylindrical, square (refer to Figure 1 for understanding) or any other shape.
[0107] In some embodiments of the present application, the battery may include an outer package for encapsulating a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte.
[0108] In some embodiments, the outer packaging may include a housing and a cover. The housing may include a bottom plate and side plates connected to the bottom plate, with the bottom plate and side plates enclosing a receiving cavity. The housing may have an opening communicating with the receiving cavity, and the cover may be positioned over the opening to seal the receiving cavity.
[0109] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be wound or laminated to form an electrode assembly. The electrode assembly is encapsulated in the housing. The electrolyte may be a gel polymer electrolyte, with the electrolyte in the gel polymer electrolyte impregnating the electrode assembly. The number of electrode assemblies in a battery may be one or more, adjustable based on demand.
[0110] In some embodiments, the outer packaging of the battery may be a hard shell, which may be a metal shell or a non-metal shell, for example, a hard plastic shell, an aluminum shell, a steel shell, etc.
[0111] In some embodiments, the outer packaging of the battery may also be a soft bag, such as a bag-type soft bag. The material of the soft bag may include plastic, for example, one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc., and may also be an aluminum-plastic film.
[0112] In some embodiments of the present application, the battery may be either a battery cell 1 (refer to FIG1 for understanding), or a battery module 2 (refer to FIG2 for understanding) or a battery pack 3 (refer to FIG3 for understanding) composed of battery cells 1 .
[0113] In some embodiments, the battery may be a battery module, and the number of battery cells contained in the battery module may be one or more, and the specific number may be adjusted according to the application and capacity of the battery module. Figure 2 is a battery module 2 as an example. Referring to Figure 2, in the battery module 2, a plurality of battery cells 1 may be arranged in sequence along the length direction of the battery module 2. Of course, they may also be arranged in any other manner. The plurality of battery cells 1 may further be fixed by fasteners. Optionally, the battery module 2 may further include a housing having a housing space, and the plurality of battery cells 1 are accommodated in the housing space.
[0114] In some embodiments, the battery modules can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack. Referring to Figure 3 or Figure 4 (Figures 3 and 4 are battery packs 3 as an example), the battery pack 3 may include a battery box and a plurality of battery modules 2 disposed in the battery box. The battery box may include an upper box body 4 and a lower box body 5. The upper box body 4 can be covered on the lower box body 5 and form an enclosed space for accommodating the battery modules 2. The plurality of battery modules 2 can be arranged in the battery box in any manner.
[0115] In addition, the present application also provides an electric device, which includes: the battery of the fourth aspect of the present application. The battery, such as a battery cell, a battery module or a battery pack, can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include but is not limited to mobile devices (such as mobile phones, laptops), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, and energy storage systems. With reference to Figure 5, as a specific example, the electric device can be a vehicle. The electric device can select the specific type of battery according to its usage requirements, such as a battery cell, a battery module or a battery pack.
[0116] As an example, the electric device may be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the electric device's requirements for high power and high energy density of the battery, a battery pack or battery module may be used.
[0117] As another example, the electrical device may be a mobile phone, a tablet computer, or a laptop computer. The electrical device is generally required to be lightweight and thin, and may use a battery cell as a power source.
[0118] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0119] Example 1
[0120] (1) Preparation of positive electrode sheet
[0121] The positive electrode active material is lithium nickel cobalt manganese oxide LiNi 0.8 Co 0.1 Mn 0.1O2 (NCM811), conductive agent acetylene black, and binder PVDF were mixed in a mass ratio of 98:1:1, and solvent N-methylpyrrolidone (NMP) was added and stirred until the system became uniform to obtain a positive electrode slurry (solid content of 70 wt%); the positive electrode slurry was heated at about 25 mg / cm 2 The positive electrode sheet was evenly coated on both sides of the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying. It was then cut into 40mm×50mm rectangles as positive electrode sheets. The positive electrode surface capacity was 3.5mAh / cm 2 .
[0122] (2) Preparation of negative electrode sheet
[0123] A 50 μm lithium foil was rolled onto a 12 μm copper foil and then cut into a 41 mm × 51 mm rectangle for use as a negative electrode.
[0124] (3) Preparation of gel polymer electrolyte:
[0125] 1.0g of the main solvent 1,2-dimethoxyethane (DME), 6.4g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5g of the lithium salt lithium bis(fluorosulfonyl)imide were added to form a 1.5M concentration electrolyte, and then 0.9g of the polymerization monomer I-12' and 16.9mg of the initiator azobis(isoheptyl)onitrile were added (after injection and packaging, the solution was cured at 60°C for 12h to prepare a gel polymer electrolyte).
[0126] (4) Preparation of diaphragm
[0127] A polyethylene porous membrane with a thickness of 12 μm was selected as the separator and cut into a rectangle of 45 mm*55 mm for standby use.
[0128] (5) Preparation of secondary batteries
[0129] Battery Assembly: A pre-cut positive electrode is paired with two pre-cut negative electrodes, separated by the aforementioned separator film. The cells are then wrapped in an aluminum-plastic film bag to form a laminated dry cell. 0.3g of the prepared electrolyte is injected, and the aluminum-plastic film bag is sealed by vacuum hot pressing. After standing at room temperature for at least 6 hours, cycling testing can begin. The laminated battery prepared in this manner has a rated capacity of 140mAh.
[0130] Comparative Example 1
[0131] The difference from Example 1 is that a liquid electrolyte is used instead of the gel polymer electrolyte.
[0132] Preparation of electrolyte: 1.0 g of main solvent 1,2-dimethoxyethane (DME), 6.4 g of auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M concentration electrolyte.
[0133] Comparative Example 2
[0134] The difference from Example 1 is that different types of polymerization monomers are added when preparing the gel polymer electrolyte.
[0135] (3) Preparation of gel polymer electrolyte: 1.0 g of the main solvent 1,2-dimethoxyethane (DME), 6.4 g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of the lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M electrolyte solution, and then 0.9 g of methyl acrylate and 16.9 mg of the initiator azobis(isoheptanonitrile) were added.
[0136] Comparative Examples 3-5
[0137] The difference from Comparative Example 2 is that the type of the second polymerizable monomer added during the preparation of the gel polymer electrolyte is different.
[0138] The second polymerizable monomers used in Comparative Example 3, Comparative Example 4 and Comparative Example 5 are vinylene carbonate, hexafluoroisopropyl methacrylate and hydroxyethyl methacrylate, respectively. See Table 1 for details.
[0139] Examples 2-5
[0140] The difference from Example 1 is that different types of polymerization monomers are added when preparing the gel polymer electrolyte. The polymerization monomers used in Example 2, Example 3, Example 4 and Example 5 are I-49', I-192', I-84' and I-108', respectively. Details are shown in Table 1.
[0141] Example 6
[0142] The difference from Example 1 is:
[0143] (3) Preparation of gel polymer electrolyte: 1.0 g of the main solvent 1,2-dimethoxyethane (DME), 6.4 g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of the lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M concentration electrolyte solution, and then 0.45 g of the polymer monomer I-12', 0.45 g of the polymer monomer I-108' and 20 mg of the initiator azobis(isoheptanonitrile) were added.
[0144] Example 7
[0145] The difference from Example 1 is:
[0146] (3) Preparation of gel polymer electrolyte: 1.0 g of the main solvent 1,2-dimethoxyethane (DME), 6.4 g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of the lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M concentration electrolyte solution, and then 0.45 g of the polymer monomer I-84', 0.45 g of the polymer monomer I-192' and 20 mg of the initiator azobis(isoheptanonitrile) were added.
[0147] Example 8
[0148] The difference from Example 1 is:
[0149] (3) Preparation of gel polymer electrolyte: 1.0 g of the main solvent 1,2-dimethoxyethane (DME), 6.4 g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of the lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M concentration electrolyte solution, and then 0.45 g of the polymerization monomer I-12', 0.45 g of the second polymerizable monomer methyl acrylate and 20 mg of the initiator azobis(isoheptanonitrile) were added.
[0150] Examples 9-11
[0151] The difference from Example 8 is that the type of the second polymerizable monomer added during the preparation of the gel polymer electrolyte is different.
[0152] The second polymerizable monomers used in Example 9, Example 10, and Example 11 are vinylene carbonate, hexafluoroisopropyl methacrylate, and hydroxyethyl methacrylate, respectively. See Table 1 for details.
[0153] Examples 12-18
[0154] The difference from Example 1 is that different types of polymerization monomers are added when preparing the gel polymer electrolyte. The polymerization monomers used in Examples 12 to 18 are polymerization monomers I-60, I-125, I-137, I-149, I-173, I-205, and I-229, respectively. Details are shown in Table 1.
[0155] Example 19
[0156] The difference from Example 1 is:
[0157] (3) Preparation of gel polymer electrolyte: 1.0 g of the main solvent 1,2-dimethoxyethane (DME), 6.4 g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of the lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M concentration electrolyte solution, and then 0.089 g of the polymerization monomer I-12' and 6.0 mg of the initiator azobis(isoheptanonitrile) were added.
[0158] Example 20
[0159] The difference from Example 1 is:
[0160] (3) Preparation of gel polymer electrolyte: 1.0 g of the main solvent 1,2-dimethoxyethane (DME), 6.4 g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of the lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M concentration electrolyte solution, and then 0.445 g of the polymerization monomer I-12' and 6.0 mg of the initiator azobis(isoheptanonitrile) were added.
[0161] Example 21
[0162] The difference from Example 1 is:
[0163] (3) Preparation of gel polymer electrolyte: 1.0 g of the main solvent 1,2-dimethoxyethane (DME), 6.4 g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of the lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M concentration electrolyte solution, and then 1.335 g of the polymerization monomer I-12' and 31.0 mg of the initiator azobis(isoheptanonitrile) were added.
[0164] Example 22
[0165] The difference from Example 1 is:
[0166] (3) Preparation of gel polymer electrolyte: 1.0 g of the main solvent 1,2-dimethoxyethane (DME), 6.4 g of the auxiliary solvent 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1.5 g of the lithium salt lithium bis(fluorosulfonyl)imide were mixed to form a 1.5 M concentration electrolyte solution, and then 2.225 g of the polymerization monomer I-12' and 31.0 mg of the initiator azobis(isoheptanonitrile) were added.
[0167] It should be noted that the above embodiments of the present application exemplify several methods for preparing gel polymer electrolytes. Other gel polymer electrolytes can be prepared with reference to this exemplary method. According to the exemplary method for preparing compounds, those skilled in the art can easily obtain specific methods for implementing each synthesis step from relevant scientific literature or standard textbooks in this field. Unless otherwise specified, commercially available or known compounds in the literature are used as raw materials for synthesis. Those skilled in the art of organic synthesis will recognize that the nature and order of the proposed synthesis steps can be changed for the purpose of optimizing the generation of the compounds described herein. In addition, the raw materials, reagents, etc. whose sources are not clearly defined during the preparation process are all conventional products obtained commercially.
[0168] Performance testing:
[0169] 1. Characterization of the polymer matrix in the obtained gel polymer electrolyte
[0170] The electrolyte obtained in the preparation of the gel polymer electrolyte in step (3) was mixed with the polymerization monomer and initiator, and then cured at 60°C for 12 hours. The solvent was then removed by vacuum drying, and the lithium salt was removed by washing. The polymer matrix was then dissolved with an appropriate amount of a good solvent and finally filtered by settling with n-hexane to obtain a polymer matrix. Combined with infrared spectroscopy (IR), nuclear magnetic resonance (NMR, for example) 1 H or 13 C or 19 F or 31 The obtained polymer matrix is characterized by one or more of: P), mass spectrometry (MS), elemental analysis, gel permeation chromatography (GPC), and laser Raman spectroscopy (LR).
[0171] 2. Secondary battery puncture test
[0172] The following steps were performed at 25°C: charging at 0.2C to 4.3V, then constant voltage charging at 4.3V to 0.05C; a 3mm diameter, high-temperature resistant steel needle was inserted through the geometric center of the cell at a speed of 25mm / s, with the needle remaining in the cell, and the heating status was observed. Five parallel test groups were provided for each example. The maximum temperature reached was measured using a thermocouple installed 2cm from the puncture point on the surface of each battery cell, and the average value of the five parallel test groups was calculated.
[0173] The polymer matrices obtained in Examples 1 to 22 were characterized by nuclear magnetic resonance spectroscopy (NMR, e.g. 1 H NMR and 19F NMR) and infrared spectroscopy (IR) were used to identify the characteristic functional groups in the polymer, and elemental analysis was used to identify the polymer structure. The characterization results showed that the polymer matrix obtained by polymerizing the monomers in Examples 1 to 22 under initiator conditions had the structure shown in Formula I or Formula II of the present application.
[0174] Under the same conditions, the secondary batteries prepared in Examples 1 to 22 and Comparative Examples 1 to 5 were subjected to a needle penetration test. The test results are shown in Table 1.
[0175] Table 1 Differences and test results of Examples 1 to 22 and Comparative Examples 1 to 5 Note: The polymer monomers I-12', I-49', I-192', I-84', I-108', I-60', I-125', I-137', I-149', I-173', I-205', and I-229' used in Examples 1 to 22 were all obtained by the preparation method disclosed in this application; methyl acrylate CAS: 96-33-3, McLean, purity 99%; vinylene carbonate CAS: 872-36-6, Xienen, purity 99%; hexafluoroisopropyl methacrylate CAS: 3063-94-3, Myrel, purity 99%; hydroxyethyl methacrylate CAS: 868-77-9, Aladdin Biochemical, purity 99%.
[0176] Results and Conclusions:
[0177] Combining Examples 1 to 22 and Comparative Examples 1 to 5, it can be seen that the use of polymers having a cyclic phosphate structure in the electrolyte is beneficial to improving the thermal stability of the battery and reducing the probability of battery combustion and thermal runaway. In addition, combining Examples 1 to 5 and Examples 12 to 18, it can be seen that in the cyclic phosphate polymer, compared with X1 and X2 being sulfur or imino, when X1 and X2 are oxygen, it is beneficial to improve the thermal stability of the battery; compared with Y being sulfur or imino, when Y is alkyl or alkoxy, it is beneficial to improve the thermal stability of the battery; combining Example 2 and Example 12, it can be seen that compared with the structure without fluorine substitution, when the cyclic phosphate polymer has fluorine substitution, it is beneficial to improve the thermal stability of the battery. In addition, further combining Example 1 and Examples 19 to 22, it can be seen that as the content of the polymer matrix in the gel polymer electrolyte increases, the thermal stability of the battery also increases.
[0178] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A polymer, wherein The general formula of the polymer is shown in Formula I: Wherein: m includes 0 and / or 1; n is a positive integer; X1 and X2 each independently include oxygen, sulfur or imino; X3 includes oxygen or sulfur; Y includes oxygen, sulfur, imino, -SC which is unsubstituted or substituted by any group 1~8 Alkylene, unsubstituted or substituted by any group -NH-C 1~8 Alkylene, unsubstituted or substituted C 1~8 Alkylene, unsubstituted or substituted C 1~8 Any one of alkyleneoxy; R1, R2, R3, R4 independently include hydrogen, fluorine, unsubstituted or substituted C 1~10 Alkyl, unsubstituted or substituted by any group C 1~10 Any of the alkoxy groups; R5 includes C 1~10 alkyl, Any one of; R9 includes C which is unsubstituted or substituted by any group 1~10 Alkyl; the arbitrary group includes at least one of halogen, alkyl, alkoxy, ester and carbonyl.
2. The polymer according to claim 1, wherein The halogen includes fluorine.
3. The polymer according to claim 2, wherein X1 and X2 are independently oxygen or sulfur; Y is oxygen, unsubstituted or fluorine-substituted C 1~8 Alkylene, unsubstituted or fluorinated C 1~8 Any one of alkyleneoxy; R1, R2, R3, R4 each independently include hydrogen, fluorine, unsubstituted or fluorine-substituted C 1~10 Alkyl, unsubstituted or fluorinated C 1~10 Any of the alkoxy groups; R5 includes unsubstituted or fluorine-substituted C 1~10 alkyl, Any one of; R9 includes unsubstituted or fluorine-substituted C 1~10 alkyl.
4. The polymer according to claim 3, wherein X1 and X2 each independently include oxygen; X3 includes oxygen; Y includes oxygen, unsubstituted or fluorine-substituted C 1~8 Alkylene, unsubstituted or fluorinated C 1~8 Any of alkyleneoxy groups.
5. The polymer according to any one of claims 1 to 4, wherein The average molecular weight is 20,000 to 60,000.
6. The polymer according to any one of claims 1 to 5, wherein R1, R2, R3, and R4 are independently unsubstituted or fluorine-substituted C 1~10 Alkyl, unsubstituted or fluorinated C 1~10 Any of the alkoxy groups.
7. The polymer according to any one of claims 1 to 6, wherein The polymer monomers of the polymer include cyclic phosphate compounds containing double bonds.
8. The polymer according to any one of claims 1 to 7, wherein The polymerizable monomer is a cyclic phosphate compound containing a double bond.
9. The polymer according to any one of claims 1 to 8, wherein The polymerizable monomers include:
10. The polymer according to any one of claims 1 to 9, wherein The polymer comprises at least one of the following compounds:
11. The polymer according to claim 7 or 9, wherein The polymerizable monomer of the polymer further includes a second polymerizable compound, and the general formula of the polymer is shown in Formula II: Wherein: a and b are respectively positive integers independently, and 0.5≤a / b≤4; R6 is unsubstituted or substituted by any of the above groups. 3~10 Alkyl, unsubstituted or substituted by any of the above groups 3~10 Epoxy, unsubstituted or substituted by any of the above groups C 3~10 Allyl, unsubstituted or substituted by any of the above groups C 3~10 (Meth)acryloyl, unsubstituted or substituted by any of the above groups 3~10 Any of acrylates.
12. The polymer according to claim 11, wherein The second polymerizable compound includes at least one of a polymerizable monomer, an oligomer, and a copolymer of a gel-type polymer electrolyte.
13. The polymer according to claim 11 or 12, wherein The second polymerizable compound includes methyl methacrylate, styrene, methyl acrylate, ethyl acrylate, acrylic acid, trimethylsilyl methacrylate, acrolein dimethyl acetal, acrolein diethyl acetal, 2-phenoxyethyl acrylate, tridecafluoro-2-hydroxynonyl, trifluoroethyl methacrylate, allyl-1,3-sultone, glycidyl methacrylate, acrylamide, trifluoroethyl acrylate, (acryloxymethyl) dimethylmethoxysilane, cyanoethyl acrylate, hydroxyethyl acrylate, triallyl trimesic acid ester, hydroxypropyl acrylate, 3-(perfluoro-3-methylbutyl) 2-hydroxypropyl acrylate, 1-vinyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt, 1-allyl-3-ethylimidazole bis(trifluoromethanesulfonyl)imide salt, 1- At least one of allyl-1-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide, 1,6-bis(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, pentafluorophenol acrylate, vinylene carbonate, maleic anhydride, ethyl cyanoacrylate, butyl acrylate, hexafluoroisopropyl methacrylate, hexafluorobutyl methacrylate, 2-acrylate-2-hydroxy-3-phenoxypropyl ester, hydroxyethyl methacrylate, and vinyl carbonate, and can be selected from at least one of vinylene carbonate, maleic anhydride, ethyl cyanoacrylate, butyl acrylate, hexafluoroisopropyl methacrylate, hexafluorobutyl methacrylate, hydroxypropyl acrylate, 2-acrylate-2-hydroxy-3-phenoxypropyl ester, hydroxyethyl methacrylate, and vinyl carbonate.
14. A method for preparing the polymer according to any one of claims 1 to 13, wherein include: To make cyclic phosphate compounds containing double bonds self-polymerize; and / or, The cyclic phosphate compound containing a double bond is copolymerized with the second polymerizable compound.
15. The method according to claim 14, wherein: The preparation method of the cyclic phosphate compound containing a double bond comprises: make and A cyclization reaction occurs to obtain the general formula and / or make Substitution reaction with Y′-R8 gives the general formula and / or The compound in: m is 0 or 1; X1' and X2' independently include hydroxyl, thiol or amino; X1 and X2 independently include oxygen, sulfur or imino; R1, R2, R3, and R4 are independently hydrogen, fluorine, unsubstituted or substituted C 1~10 Alkyl, unsubstituted or substituted by any group C 1~10 Any one of the alkoxy groups; R7 and R8 independently include C 2~11 Olefin; Y' includes hydrogen, hydroxyl, mercapto or amino; Y "includes oxygen, sulfur or imino; R9 includes unsubstituted or substituted C 1~10 Alkyl; the arbitrary group includes at least one of halogen, alkyl, and alkoxy.
16. The method according to claim 15, wherein: Said The invention comprises at least one of ethylene glycol, ethylenedithiol, 2-mercaptoethanol, mercaptoethylamine, ethanolamine, ethylenediamine, 1,3-propylene glycol, 1,3-propylenethiol, 3-mercapto-1-propanol, 3-amino-1-propanol, 3-mercapto-1-propylamine and 1,3-propylenediamine.
17. The method according to claim 15 or 16, wherein: The preparation method of the cyclic phosphate compound containing double bonds also includes: right Sulfurization reaction is carried out to obtain the general formula and / or right and / or Sulfurization reaction is carried out to obtain the general formula and / or of compounds.
18. The method according to any one of claims 14 to 17, wherein: The cyclic phosphate compound containing a double bond includes a polymerized monomer of at least one of polymer I-12, polymer I-49, polymer I-84, polymer I-108 and polymer I-192.
19. The method according to any one of claims 14 to 18, wherein: The self-polymerization and / or the copolymerization is carried out under the condition of an initiator, and the initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile, 2,2"-azabis(2-imidazoline) dihydrochloride, 2,2'-azobisisobutylamidine dihydrochloride, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.
20. A gel polymer electrolyte, wherein: The invention comprises a polymer matrix and an electrolyte, wherein the polymer matrix comprises the polymer according to any one of claims 1 to 13 or a polymer obtained by the method according to any one of claims 14 to 19.
21. The gel polymer electrolyte according to claim 20, wherein The mass proportion of the polymer matrix is 0.5wt% to 25wt%, optionally 5wt% to 15wt%, and further optionally 5wt% to 12wt%.
22. A battery, wherein: The invention comprises the gel polymer electrolyte according to any one of claims 20 to 21, and / or the polymer prepared by the method according to any one of claims 13 to 18, and / or the polymer according to any one of claims 1 to 12.
23. An electrical device, wherein: Comprising the battery of claim 22.
Citation Information
Patent Citations
Electrolyte for Secondary Battery and Lithium Secondary Battery Containing Same
CN111082138A
High-adhesion flame-retardant adhesive and preparation method thereof
CN112048263A
Electrochemical device and electronic device
CN112151750A
Halogen-free flame-retardant polyethylene plastic and preparation method thereof
CN112280232A
Degradable flame-retardant polystyrene plastic and preparation method thereof