Electrolyte solution and battery
By adding additives such as fluoroethylene carbonate and fluorobenzene to the electrolyte of lithium-ion batteries, combined with modified polymer binders, the problem of low anti-oxidation performance of the electrolyte is solved, and the performance of the battery at high voltage and high temperature is significantly improved. Lower performance, enhanced battery stability and safety.
Patent Information
- Application Number
- PCT/CN2024/084803
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-31
AI Technical Summary
The anti-oxidation performance of the electrolyte in lithium-ion batteries is low under high voltage, causing the interface between the electrode and the electrolyte to deteriorate, affecting battery performance.
Additives such as fluoroethylene carbonate and fluorobenzene are added to the electrolyte to form a stable SEI film, improve the anti-oxidation performance of the electrolyte, and use modified polymers as binders to reduce side reactions at the negative electrode interface and enhance the battery. stability.
It effectively inhibits the oxidation and decomposition reaction of the electrolyte under high voltage, improves the performance of the battery under high voltage and high temperature, and improves the endurance and safety of the battery.
Smart Images

Figure PCTCN2024084803-FTAPPB-I100001 
Figure PCTCN2024084803-FTAPPB-I100002 
Figure PCTCN2024084803-FTAPPB-I100003
Abstract
Description
Electrolyte and battery Technical Field
[0001] The present disclosure belongs to the technical field of batteries, and particularly relates to an electrolyte and a battery including the electrolyte. Background Art
[0002] Lithium-ion batteries have experienced rapid development in recent years due to their superior performance, including high operating voltage, high energy density, long cycle life, low self-discharge rate, and lack of memory effect. Simultaneously, the application scope of lithium-ion batteries continues to expand, from the information industry (e.g., mobile phones, PDAs, and laptops) to energy transportation (e.g., electric vehicles, grid peak regulation, and solar and wind power plant storage). High reliability and high safety have become fundamental requirements for lithium-ion batteries. As the application requirements for lithium-ion batteries continue to change, people are demanding higher performance from lithium-ion batteries, expecting them to have longer battery life and good safety performance. The energy density of lithium-ion batteries can be increased by increasing the operating voltage of the battery. However, increasing the operating voltage causes oxidative decomposition reactions of electrolyte components at high voltage, resulting in a decrease in the electrolyte's antioxidant properties, deterioration of the electrode-electrolyte interface, and a sharp decline in battery performance.
[0003] Summary of the Invention
[0004] The purpose of the embodiments of the present disclosure is to provide an electrolyte and a battery including the electrolyte, so as to solve the problem of low antioxidant performance of the electrolyte.
[0005] In a first aspect, an embodiment of the present disclosure provides an electrolyte, comprising:
[0006] Electrolyte, solvent and first additive, the structural formula of the first additive is:
[0007] Furthermore, the electrolyte further includes at least one of a second additive and a third additive, the second additive includes fluoroethylene carbonate, and the third additive includes fluorobenzene.
[0008] Furthermore, the electrolyte includes the second additive, the second additive includes fluoroethylene carbonate, and the mass of the fluoroethylene carbonate is 5%-15% of the mass of the electrolyte; and / or
[0009] The electrolyte includes the third additive, the third additive includes fluorobenzene, and the mass of the fluorobenzene is 2%-10% of the mass of the electrolyte; and / or
[0010] The mass of the first additive is 0.5%-2% of the mass of the electrolyte.
[0011] Furthermore, the mass concentration of the electrolyte is 0.5 mol / L-2 mol / L; and / or
[0012] The electrolyte comprises:
[0013] At least one of lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium perchlorate, lithium trifluorosulfonyl, lithium difluoro(trifluoromethylsulfonyl)imide, and lithium tris(trifluoromethylsulfonyl)methyl.
[0014] Furthermore, the electrolyte further comprises:
[0015] At least one of succinonitrile, adiponitrile, 1,3,6-hexanetrinitrile, glycerol trinitrile, vinylene carbonate, vinyl sulfate, butylene sulfite, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide) and lithium bis(fluorosulfonyl imide); and / or
[0016] The solvent includes:
[0017] At least one of a cyclic carbonate, a linear carbonate and a linear carboxylic acid ester, the cyclic carbonate includes at least one of ethylene carbonate and propylene carbonate, the linear carbonate includes at least one of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate, and the linear carboxylic acid ester includes at least one of ethyl propionate, propyl propionate and propyl acetate.
[0018] In a second aspect, an embodiment of the present disclosure provides a battery, comprising:
[0019] The electrolyte described in the above embodiments.
[0020] Furthermore, the battery further comprises:
[0021] A positive electrode sheet, wherein the active layer of the positive electrode sheet comprises a positive electrode active material and a binder, wherein the binder comprises a polymer having at least one of a nitrile group and a pyridine group.
[0022] Furthermore, the adhesive includes polyvinylidene fluoride modified with acrylonitrile and 4-vinylpyridine.
[0023] Furthermore, the structural formula of the adhesive is:
[0024] Wherein, a, b, c and d are positive integers.
[0025] Furthermore, the mass of the adhesive is 0.5%-3% of the mass of the active layer of the positive electrode sheet.
[0026] The electrolyte of the embodiment of the present disclosure includes: an electrolyte, a solvent and a first additive. The F atoms in the first additive can improve the antioxidant performance of the electrolyte. By adding the first additive to the electrolyte, the antioxidant performance of the electrolyte can be improved. At the same time, the first additive can form a film at the positive / negative ends. The formed SEI film contains lithium alkyl sulfonate, which can improve the ionic conductivity and stability of the SEI film, effectively inhibit the gas production caused by membrane decomposition, and make the electrolyte components less likely to undergo oxidative decomposition reactions under high voltage, preventing deterioration of the interface between the electrode and the electrolyte, thereby ensuring the stability of the interface, which is beneficial to improving the performance of the battery at high voltage and high temperature. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present disclosure to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the embodiments described are part of the embodiments of the present disclosure, but not all of them. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present disclosure.
[0028] The terms "first," "second," and the like in the specification and claims of this disclosure are used to distinguish similar objects and are not intended to describe a particular order or precedence. It should be understood that such terms are interchangeable where appropriate, so that the embodiments of this disclosure can be implemented in sequences other than those described herein. In addition, the term "and / or" in the specification and claims refers to at least one of the connected objects, and the character " / " generally indicates that the connected objects are in an "or" relationship.
[0029] The electrolyte of the embodiment of the present disclosure includes:
[0030] Electrolyte, solvent and first additive, the structural formula of the first additive is:
[0031] The electrolyte may include a lithium salt, which may include at least one of lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium perchlorate, trifluorosulfonyl lithium, difluoro (trifluoromethylsulfonyl) imide lithium, and tris (trifluoromethylsulfonyl) methyl lithium. For example, the lithium salt may be lithium hexafluorophosphate. The specific electrolyte may be selected based on actual conditions. The solvent may be selected from at least one of cyclic carbonate, linear carbonate, and linear carboxylic acid ester. For example, the cyclic carbonate may include at least one of ethylene carbonate and propylene carbonate, and the linear carbonate may include at least one of dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. The linear carboxylic acid ester may include at least one of ethyl propionate, propyl propionate, and propyl acetate. The specific solvent may be selected based on actual conditions.
[0032] In the electrolyte of the embodiment of the present disclosure, the antioxidant performance of the electrolyte can be improved by adding the first additive to the electrolyte. At the same time, the first additive can form a film at the positive / negative ends, and the formed SEI film contains lithium alkyl sulfonate, which can improve the ionic conductivity and stability of the SEI film, effectively inhibit the gas production caused by membrane decomposition, and make the electrolyte components less likely to undergo oxidative decomposition reactions under high voltage, preventing the deterioration of the interface between the electrode and the electrolyte, thereby ensuring the stability of the interface, which is beneficial to improving the performance of the battery at high voltage and high temperature.
[0033] In some embodiments, the electrolyte may further include at least one of a second additive and a third additive. For example, the electrolyte may further include the second additive or the third additive. For another example, the electrolyte may further include the second additive and the third additive at the same time. The second additive may include fluoroethylene carbonate (FEC). The third additive may include fluorobenzene (FB). Fluoroethylene carbonate can construct a stable SEI film at the negative terminal and reduce the interfacial side reactions of the electrolyte at the negative terminal. Fluorobenzene can improve the wetting of the electrolyte on the positive / negative electrode sheets, improve the interfacial properties of the positive / negative electrodes, make the positive / negative electrode interface film more stable and have lower impedance, thereby improving battery performance. At the same time, due to the structural characteristics of fluorobenzene, the oxidation resistance of the electrolyte can be further improved, and fluorobenzene can undergo electropolymerization at high voltage, thereby improving the overcharge performance of the battery.
[0034] In some embodiments, the second additive is fluoroethylene carbonate (FEC) and the third additive is fluorobenzene (FB).
[0035] By adding the first additive, the electrolyte can be made less susceptible to oxidative decomposition reactions, thereby effectively inhibiting gas production due to membrane decomposition; the second additive can construct a stable SEI film at the negative electrode, reducing the interfacial side reactions of the electrolyte at the negative end; the third additive can further improve the antioxidant properties of the electrolyte, making it less susceptible to oxidative decomposition reactions. Regardless of whether the electrolyte undergoes redox reactions or other side reactions, it will bring changes or adverse effects to the electrodes and electrolyte, resulting in reduced battery performance. Through the synergistic effect between the first additive, the second additive, and the third additive in the electrolyte, a stable film layer can be better constructed on the electrode surface, while the redox reaction of the electrolyte can be inhibited and the occurrence of other side reactions can be reduced, ensuring the stability of the electrolyte and the electrode, and ensuring that the battery has better stability while achieving better high temperature performance and fast charging performance.
[0036] In some embodiments, the electrolyte may include the second additive, which includes fluoroethylene carbonate. The mass of the fluoroethylene carbonate may be 5%-15% of the mass of the electrolyte. For example, the mass of the fluoroethylene carbonate is 5%, 10% or 15% of the mass of the electrolyte. The specific percentage of the mass of the fluoroethylene carbonate to the mass of the electrolyte can be selected according to actual conditions.
[0037] In some embodiments, the mass of the fluoroethylene carbonate is 10%-15% of the mass of the electrolyte.
[0038] In the present disclosure, the percentage of the mass of the fluoroethylene carbonate to the mass of the electrolyte can be measured by conventional methods in the art, such as gas chromatography.
[0039] In other embodiments, the electrolyte may include the third additive, and the third additive includes fluorobenzene. The mass of the fluorobenzene may be 2%-10% of the mass of the electrolyte. For example, the mass of the fluorobenzene is 2%, 5%, 7% or 10% of the mass of the electrolyte. The specific percentage of the mass of the fluorobenzene to the mass of the electrolyte can be selected according to actual conditions.
[0040] In the present disclosure, the percentage of the mass of the fluorobenzene to the mass of the electrolyte can be measured by conventional methods in the art, such as gas chromatography.
[0041] In an embodiment of the present disclosure, the mass of the first additive may be 0.5%-2% of the mass of the electrolyte. For example, the mass of the first additive is 0.5%, 1%, 1.5% or 2% of the mass of the electrolyte. The specific percentage of the mass of the first additive to the mass of the electrolyte can be selected according to actual conditions.
[0042] In the present disclosure, the percentage of the mass of the first additive to the mass of the electrolyte can be measured by conventional methods in the art, such as gas chromatography.
[0043] In some embodiments, the electrolyte may include the first additive, the second additive, and the third additive. The mass of the first additive may be 0.5%-2% of the mass of the electrolyte, the second additive may be fluoroethylene carbonate, and the third additive may be fluorobenzene. The mass of fluoroethylene carbonate may be 5%-15% of the mass of the electrolyte, and the mass of fluorobenzene may be 2%-10% of the mass of the electrolyte. For example, the mass of the first additive is 0.5% of the mass of the electrolyte, the mass of fluoroethylene carbonate is 15% of the mass of the electrolyte, and the mass of fluorobenzene is 2% of the mass of the electrolyte; for another example, the mass of the first additive is 2% of the mass of the electrolyte, the mass of fluoroethylene carbonate is 5% of the mass of the electrolyte, and the mass of fluorobenzene is 10% of the mass of the electrolyte; for another example, the mass of the first additive is 1.5% of the mass of the electrolyte, the mass of fluoroethylene carbonate is 10% of the mass of the electrolyte, and the mass of fluorobenzene is 6% of the mass of the electrolyte.
[0044] In some embodiments, the mass concentration of the electrolyte may be 0.5 mol / L-2 mol / L. For example, the mass concentration of the electrolyte may be 0.5 mol / L, 1 mol / L, 1.5 mol / L, or 2 mol / L. The mass concentration of the electrolyte may be selected according to actual conditions.
[0045] Optionally, the electrolyte may include at least one of lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium perchlorate, lithium trifluorosulfonyl, lithium difluoro(trifluoromethylsulfonyl)imide, and lithium tris(trifluoromethylsulfonyl)methyl. For example, the electrolyte is lithium hexafluorophosphate. For another example, the electrolyte includes lithium hexafluorophosphate and lithium trifluorosulfonyl. The specific type of the electrolyte can be selected based on actual conditions.
[0046] In some embodiments, the electrolyte may further include at least one of succinonitrile, adiponitrile, 1,3,6-hexanetrinitrile, glycerol trinitrile, vinylene carbonate, vinyl sulfate, butylene sulfite, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide), and lithium bis(fluorosulfonyl imide). For example, the electrolyte may further include vinylene carbonate, butylene sulfite, lithium bis(trifluoromethanesulfonyl imide), or lithium bis(fluorosulfonyl imide). For another example, the electrolyte may further include vinylene carbonate and lithium bis(fluorosulfonyl imide). The specific electrolyte may be selected based on actual needs.
[0047] Optionally, the solvent may include:
[0048] At least one of cyclic carbonate, linear carbonate and linear carboxylic acid ester. The cyclic carbonate can include at least one of ethylene carbonate and propylene carbonate. The linear carbonate can include at least one of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate. The linear carboxylic acid ester can include at least one of ethyl propionate, propyl propionate and propyl acetate. For example, the solvent can include ethylene carbonate, diethyl carbonate and propyl acetate. The specific type of the solvent can be selected according to actual conditions.
[0049] The battery according to an embodiment of the present disclosure includes:
[0050] The electrolyte described in the above embodiment. In a battery having the above embodiment, the addition of the first additive to the electrolyte can improve the antioxidant properties of the electrolyte, making the electrolyte components less susceptible to oxidative decomposition reactions at high voltages, thereby preventing deterioration of the electrode-electrolyte interface and ensuring interface stability, thereby improving the performance of the battery at high voltages and temperatures. The battery can have a charge cutoff voltage of 4.5 V or above.
[0051] In some embodiments, the battery is a lithium-ion battery.
[0052] The battery of the embodiment of the present disclosure may further include:
[0053] A positive electrode sheet, wherein the active layer of the positive electrode sheet may include a positive electrode active material and a binder, wherein the binder includes a polymer having at least one of a nitrile group and a pyridine group. The positive electrode active material may be selected from at least one of lithium cobalt oxide, a nickel-cobalt-manganese-lithium ternary material, lithium iron phosphate, and lithium manganate.
[0054] The nitrile group in the binder can serve as a positive electrode film-forming additive to effectively protect the positive electrode. The pyridine group in the binder can complex with metal ions to reduce the concentration of free metal ions at the negative electrode interface, thereby reducing the side reactions of the negative electrode solvent.
[0055] In some embodiments, the adhesive may include polyvinylidene fluoride modified with acrylonitrile and 4-vinyl pyridine. Polyvinylidene fluoride can be modified by acrylonitrile and 4-vinyl pyridine to connect nitrile groups and pyridine groups in the side chain. By grafting polyacrylonitrile and 4-vinyl pyridine, the crystallization of polyvinylidene fluoride can be reduced, the flexibility of polyvinylidene fluoride can be improved, and the adhesion can be improved. The introduced nitrile group can be used as a positive electrode film-forming additive to effectively protect the positive electrode, and the pyridine group can be complexed with metal ions to reduce the concentration of free metal ions at the negative electrode interface, thereby reducing the side reactions of the negative terminal solvent.
[0056] Polyvinylidene fluoride (PVDF) can be dissolved in a suitable first solvent, which can include at least one of N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP) and dimethyl sulfoxide (DMSO), and then an appropriate amount of acrylonitrile and 4-vinyl pyridine is added. A suitable catalyst can be selected according to the polymerization system to carry out a polymerization reaction to prepare an adhesive. In the process of modifying polyvinylidene fluoride by acrylonitrile and 4-vinyl pyridine, the polymerization method can be free radical polymerization or oxidation-reduction system polymerization, reversible addition-fragmentation chain transfer polymerization (RAFT), atom transfer radical polymerization (ATRP) or oxidation-reduction polymerization. The polymerization reaction can be carried out under the protection of an inert gas, and the inert gas can be high-purity nitrogen or argon. The temperature of the polymerization reaction can be 30°C-100°C (such as 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C), preferably 40°C-80°C. The weight-average molecular weight of the polymer obtained by co-modifying polyvinylidene fluoride with acrylonitrile and 4-vinylpyridine can be 3000Da-2 million Da. Polymers with molecular weights in this range can meet the controllable adjustment of adhesion. If the molecular weight of the polymer is too low, for example, below 3000Da, the cohesion between the molecules is reduced and the adhesion is also too low. If the molecular weight is too high, for example, above 2 million Da, the molecules are severely entangled during use, which is not conducive to the adhesion of the active substance.
[0057] The adhesive synthesis method may include the following steps: dissolving 5g of PVDF in 100mL of N-methylpyrrolidone (NMP) in a 250mL Schlenk flask, adding 1g of acrylonitrile monomer and 1.2g of 4-vinylpyridine, and adding 0.05g of an ATRP catalyst, a bisoxazoline (SaBOX) / copper catalyst system. Under an argon atmosphere, oxygen is removed three times by freeze-thawing, and then reacting at 65°C for 24 hours. After the reaction is completed, the product can be precipitated with diethyl ether and vacuum-dried at 100°C for 12 hours to obtain the final product with a yield of up to 80%.
[0058] In some embodiments, the structural formula of the adhesive may be:
[0059] Wherein, a, b, c and d are positive integers. a, b, c and d can each independently select a positive integer (such as, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 50, 100, 150, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 2000, 3000, 4000, 5000, 10000 or 50000) of 1-50000. The nitrile group in the adhesive can be used as a positive electrode film-forming additive to effectively protect the positive pole, and the pyridine group in the adhesive can be complexed with metal ions, reduces the free metal ion concentration at the negative electrode interface, thereby can reduce the side reaction of the negative pole extreme solvent.
[0060] In some embodiments, a, b, c, and d are each independently selected from positive integers ranging from 1 to 10.
[0061] Optionally, the mass of the adhesive may be 0.5%-5% of the mass of the active layer of the positive electrode sheet. For example, the mass of the adhesive may be 0.5%, 2%, 3%, 4%, or 5% of the mass of the active layer of the positive electrode sheet. The specific percentage of the mass of the adhesive to the mass of the active layer of the positive electrode sheet may be selected based on actual conditions.
[0062] In some embodiments, the mass of the adhesive is 1.5%-5% of the mass of the active layer of the positive electrode sheet.
[0063] In some embodiments, the mass of the adhesive is 1.5%-3% of the mass of the active layer of the positive electrode sheet.
[0064] In the present disclosure, the percentage of the mass of the adhesive to the mass of the active layer of the positive electrode sheet can be tested by conventional methods in the art, such as peeling off the active layer of the positive electrode sheet, heating it to 800°C in an argon atmosphere using a thermogravimetric analyzer (TGA), and performing a weight loss analysis. Since only the adhesive in the positive electrode sheet decomposes within 800°C, the content of the adhesive can be calculated through thermogravimetric testing.
[0065] The present disclosure is further illustrated below through some specific embodiments.
[0066] Example 1
[0067] (1) Preparation of adhesive:
[0068] In a 250 mL Schlenk flask, 5 g of PVDF was dissolved in 100 mL of N-methylpyrrolidone (NMP), followed by the addition of 1 g of acrylonitrile monomer and 1.2 g of 4-vinylpyridine. 0.05 g of an ATRP catalyst, bisoxazoline (SaBOX) / copper catalyst system, was added. Under an argon atmosphere, oxygen was removed three times using the freeze-thaw method, and the mixture was reacted at 65°C for 24 hours. After the reaction, the product was precipitated with diethyl ether and vacuum-dried at 100°C for 12 hours to obtain an adhesive, wherein a, b, c, and d are positive integers ranging from 1 to 50,000, and the weight-average molecular weight is 3,000 Da to 2,000,000 Da.
[0069] (2) Preparation of positive electrode sheet:
[0070] The positive electrode active material lithium cobalt oxide (LCO), the binder prepared in step (1) and the conductive agent acetylene black are mixed in a weight ratio of 97:0:1.5, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on the current collector aluminum foil; the coated aluminum foil is baked in an oven with 5 different temperature gradients, and then dried in an oven at 120°C for 8 hours, and then rolled and cut to obtain the desired positive electrode sheet.
[0071] (3) Preparation of negative electrode sheet:
[0072] The negative electrode active material graphite, thickener sodium carboxymethyl cellulose (CMC-Na), binder styrene-butadiene rubber and conductive agent acetylene black were mixed in a weight ratio of 97:1:1:1, deionized water was added, and a negative electrode slurry was obtained under the action of a vacuum mixer; the negative electrode slurry was evenly coated on a high-strength carbon-coated copper foil, dried at room temperature, and then transferred to an 80°C oven for drying for 10 hours, and then rolled and slit to obtain a negative electrode sheet.
[0073] (4) Preparation of electrolyte:
[0074] In a glove box filled with inert gas (such as argon) (H2O <0.1ppm, O2 <0.1ppm), ethylene carbonate, propylene carbonate and diethyl carbonate were mixed in a mass ratio of 1:1:1, and then fully dried lithium hexafluorophosphate (LiPF6) was quickly added thereto. The concentration of lithium hexafluorophosphate was 1.25mol / L and stirred evenly. After passing the moisture and free acid tests, the basic electrolyte was obtained. Different additives were added to the basic electrolyte to obtain the experimental group electrolyte, as shown in Table 1.
[0075] (5) Preparation of lithium-ion batteries:
[0076] The positive electrode sheet prepared in step (2), the isolation film (with a thickness of 9 μm, wherein the polypropylene base film is 5 μm, and the adhesive layer (2 μm) and the ceramic layer (2 μm) are respectively located on both sides of the polypropylene base film) and the negative electrode sheet prepared in step (3) are stacked in order, ensuring that the isolation film is located between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then a bare battery cell without liquid injection is obtained by winding; the bare battery cell is placed in an outer packaging foil, and the electrolyte prepared in step (4) is injected into the dried bare battery cell, and the corresponding lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping, sorting and other processes.
[0077] The differences between Comparative Examples 1-2 and Examples 2-18 and Example 1 are: the components and contents of the electrolyte are different, and the contents of the binder in the active layer are different. The specific contents can be seen in Table 1.
[0078] Table 1 Composition of lithium-ion batteries of comparative examples and embodiments
[0079] Among them, the adhesive in Comparative Example 2 is unmodified polyvinylidene fluoride, and the adhesive in Examples 2-18 is the adhesive prepared in step (1) of Example 1.
[0080] Performance testing of lithium-ion batteries
[0081] (1) 45℃ shallow charge and discharge test: The batteries prepared in the examples and comparative examples were ① adjusted to 50% SOC at a constant temperature of 25℃, and the initial thickness T1 of the battery was tested at the time of delivery; ② charged to the upper limit voltage (4.5V) at a constant current and constant voltage of 0.7C at a cut-off current of 0.05C at a temperature of 45℃; ③ left to stand for 10 minutes, and then discharged to 95% SOC at a constant current and constant voltage of 0.05C; ④ left to stand for 10 minutes, and charged to the upper limit voltage (4.5V) at a constant current and constant voltage of 0.7C at a cut-off current of 0.05C; steps ③-④ constitute one cycle, and the thickness T2 of the battery was tested after every 100 cycles of full charge. The thickness expansion rate of the lithium battery shallow charge and discharge test at 45℃ = (T2-T1) / T1×100%, with the battery being obviously bulged or having run 1200T as the limit. The results can be seen in Table 2, where the battery status is ranked from good to bad as follows: no abnormality, slight bulging, bulging, and severe bulging.
[0082] (2) 45℃ 1D voltage reduction test: The batteries prepared in the examples and comparative examples were ① adjusted to 50% SOC at a constant temperature of 25℃, and the initial voltage, internal resistance, and thickness T1 of the batteries were tested at the time of delivery; ② at 45℃, the batteries were allowed to stand for 2 hours, and charged to the upper limit voltage (4.5V) at a constant current and constant voltage of 0.7C, with a cut-off current of 0.05C; ③ the batteries were allowed to stand for 10 minutes, and then discharged to 3.0V at a constant current and constant voltage of 0.5C; ④ the batteries were allowed to stand for 10 minutes, and charged to the upper limit voltage (4.5V) at a constant current and constant voltage of 0.7C, with a cut-off current of 0.05C; ⑤ the batteries were allowed to stand for 20 hours after being fully charged, and the steps ③-⑤ were repeated. The test cycle lasts for one cycle (1 cycle per day). After 23 cycles, the voltage is reduced by 50 Mv (to 4.45 V). Starting from the 24th cycle (and continuing until the 136th cycle), the upper limit voltage drops to 4.45 V. The test process data nodes are: 24D, 40D, 56D, 68D, 84D, 91D, 95D, 100D, 105D, 110D, 115D, 120D, 125D, 130D, and 136D. The cycle discharge energy is recorded and divided by the discharge energy of the third cycle to obtain the cycle energy retention rate. After the above cycles are completed, the fully charged battery is removed from the 45°C constant temperature chamber and its hot fully charged thickness T2 is immediately measured after the corresponding number of cycles. The cycle capacity retention rate and the cycle thickness expansion rate of the battery during the corresponding cycle are recorded, respectively. The battery is measured for obvious bulging or energy retention.
[0083] (3) 0.25C-10V Overcharge Test: The batteries prepared in the Examples and Comparative Examples were charged at a constant current of 0.25C to 10V at an ambient temperature of (25±5)°C. The discharged batteries were then switched to constant voltage charging. Charging was stopped when the charging time was limited to 6 hours. Judgment criteria: The battery cells did not catch fire or explode. The specific test results can be shown in Table 2.
[0084] Table 2 Electrical properties and safety test results of lithium-ion batteries of comparative examples and embodiments
[0085] As shown in Table 2, in the embodiment of the present disclosure, by adding the first additive to the electrolyte, the antioxidant properties of the electrolyte can be improved, the gas production due to membrane decomposition can be suppressed, the electrolyte components are not prone to oxidative decomposition reactions at high voltages, and the interface between the electrode and the electrolyte can be prevented from deteriorating, ensuring the stability of the interface, which is beneficial to improving the performance of the battery at high voltages and high temperatures. By modifying the adhesive, the crystallization of polyvinylidene fluoride can be reduced, the flexibility of polyvinylidene fluoride can be improved, the adhesion can be improved, and the side reactions of the negative terminal solvent can be reduced. The performance of the battery can be improved by the first additive and the adhesive. In summary, it can be seen that the lithium-ion battery using the present disclosure has excellent 45°C shallow charge and discharge, 45°C 1D step-down cycle performance and good overcharge performance, showing extremely high application value.
[0086] The above describes the embodiments of the present disclosure, but the present disclosure is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present disclosure, ordinary technicians in this field can also make many forms without departing from the scope of protection of the purpose of the present disclosure and the claims, all of which are protected by the present disclosure.
Claims
1. An electrolyte, characterized in that: include: An electrolyte, a solvent and a first additive, wherein the structural formula of the first additive is:
2. The electrolyte according to claim 1, characterized in that The electrolyte further includes at least one of a second additive and a third additive, wherein the second additive includes fluoroethylene carbonate, and the third additive includes fluorobenzene.
3. The electrolyte according to claim 1 or 2, characterized in that The electrolyte includes a second additive, the second additive includes fluoroethylene carbonate, and the mass of the fluoroethylene carbonate is 5%-15% of the mass of the electrolyte; Preferably, the mass of the fluoroethylene carbonate is 10%-15% of the mass of the electrolyte.
4. The electrolyte according to any one of claims 1 to 3, characterized in that The electrolyte includes a third additive, the third additive includes fluorobenzene, and the mass of the fluorobenzene is 2%-10% of the mass of the electrolyte.
5. The electrolyte according to any one of claims 1 to 4, characterized in that The mass of the first additive is 0.5%-2% of the mass of the electrolyte.
6. The electrolyte according to any one of claims 1 to 5, characterized in that The mass concentration of the electrolyte is 0.5 mol / L-2 mol / L; Preferably, the electrolyte includes: lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium perchlorate, trifluorosulfonyl At least one of lithium, lithium difluoro(trifluoromethylsulfonyl)imide and tris(trifluoromethylsulfonyl)methyllithium.
7. The electrolyte according to any one of claims 1 to 6, characterized in that The electrolyte further comprises: at least one of succinonitrile, adiponitrile, 1,3,6-hexanetrinitrile, glyceroltrinitrile, vinylene carbonate, vinyl sulfate, butylene sulfite, lithium difluorophosphate, lithium bistrifluoromethanesulfonyl imide and lithium bisfluorosulfonyl imide.
8. The electrolyte according to any one of claims 1 to 7, characterized in that The solvent includes at least one of a cyclic carbonate, a linear carbonate and a linear carboxylate; Preferably, the cyclic carbonate comprises at least one of ethylene carbonate and propylene carbonate; Preferably, the linear carbonate comprises at least one of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; Preferably, the linear carboxylic acid ester includes at least one of ethyl propionate, propyl propionate and propyl acetate.
9. A battery, characterized in that: include: The electrolyte according to any one of claims 1 to 8.
10. The battery according to claim 9, characterized in that The battery also includes: A positive electrode sheet, wherein the active layer of the positive electrode sheet comprises a positive electrode active material and a binder, wherein the binder comprises a polymer having at least one of a nitrile group and a pyridine group.
11. The battery according to claim 10, characterized in that The adhesive comprises polyvinylidene fluoride modified by acrylonitrile and 4-vinylpyridine; Preferably, the weight average molecular weight of the polymer obtained by modifying polyvinylidene fluoride with acrylonitrile and 4-vinylpyridine is 3000 Da to 2 million Da.
12. The battery according to claim 10 or 11, characterized in that: The structural formula of the adhesive is: Wherein, a, b, c and d are positive integers.
13. The battery according to claim 12, characterized in that a, b, c and d are each independently selected from a positive integer of 1-50000; preferably a positive integer of 1-10.
14. The battery according to any one of claims 10 to 13, characterized in that: The mass of the adhesive is 0.5%-5% of the mass of the active layer of the positive electrode sheet; Preferably, the mass of the adhesive is 1.5%-5% of the mass of the active layer of the positive electrode sheet; More preferably, the mass of the adhesive is 1.5%-3% of the mass of the active layer of the positive electrode sheet.
15. The battery according to any one of claims 9 to 14, characterized in that: The charging cut-off voltage of the battery is 4.5V and above.
Citation Information
Patent Citations
Method for producing disulfonyl fluride compound
CN101155777A
Secondary cell nonaqueous electrolyte and secondary cell
CN102017273A
Electrolyte solution for electrical energy storage devices, and electrical energy storage device
CN102365781A
Electrolyte and battery
CN116259845A
Positive electrode and lithium ion secondary battery
US20090117465A1
Cited By
Secondary battery and electronic device
CN119852554A
High-energy-density solid-state lithium ion battery and preparation method thereof
CN120221757A