Secondary battery
The secondary battery design with lithium cobalt oxide and fluorinated carbonates in the electrolyte addresses initial characteristic issues, achieving high discharge capacity and low-temperature stability by stabilizing the crystal structure and reducing internal resistance.
Patent Information
- Application Number
- PCT/IB2024/053967
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-02
- Filing Date
- 2024-04-24
- Publication Date
- 2024-11-07
AI Technical Summary
Existing secondary batteries face challenges in achieving good initial characteristics, such as maximum discharge capacity and discharge capacity retention rate, due to issues like swelling from gas generation and low-temperature performance.
A secondary battery design incorporating a positive electrode with lithium cobalt oxide and a surface layer containing additives like magnesium, aluminum, or nickel, paired with an electrolyte using fluorinated cyclic and chain carbonates, specifically fluoroethylene carbonate and methyl trifluoropropionate, to enhance stability and performance.
The proposed battery exhibits excellent initial characteristics, including high discharge capacity retention and improved low-temperature performance, with the additives stabilizing the crystal structure and reducing internal resistance.
Smart Images

Figure IB2024053967_07112024_PF_FP_ABST
Abstract
Description
secondary battery
[0001] The present invention relates to a secondary battery. Note that the present invention is not limited to secondary batteries, and other embodiments of the present invention include semiconductor devices, display devices, light-emitting devices, power storage devices, lighting devices, electronic devices, vehicles, and manufacturing methods thereof. The above-mentioned electronic devices include information terminal devices equipped with the secondary battery of the present invention. The above-mentioned power storage devices include stationary power storage devices.
[0002] Studies have been conducted on electrolytes for secondary batteries. For example, Patent Document 1 studies additives having a fluoro group, such as fluoroethylene carbonate, as electrolytes for secondary batteries, and proposes a technique of mixing a siloxane compound to suppress swelling of the battery due to gas generation when maintained at high temperatures.
[0003] Furthermore, Non-Patent Document 1 focuses on the low-temperature characteristics of secondary batteries and proposes a technique of mixing methyl 3,3,3-trifluoropropionate (MTFP):fluoroethylene carbonate (FEC) at a ratio of 9:1 as the organic solvent for the electrolyte.
[0004] JP 2011-507207 A
[0005] John, H. et al. , “An All-Fluorinated Ester Electrolyte for Stable High-Voltage Li Metal Batteries Capable of Ultra-Low-Temperature Operation”, ACE Energy LETTERS, 2020, 5, 1438-1447
[0006] Although a lithium ion secondary battery can be obtained according to Patent Document 1 and Non-Patent Document 1, there is one battery characteristic that is not suggested in these documents: initial characteristics. Therefore, one of the objects of the present invention is to provide a secondary battery that exhibits good initial characteristics.
[0007] The above-mentioned problems do not preclude the existence of other problems. Furthermore, the above-mentioned problems are considered to be independent of each other, and it is not necessary to solve all of the above-mentioned problems by one embodiment of the present invention. Furthermore, problems other than those mentioned above can be extracted from the description of the specification, drawings, and claims (collectively referred to as "this specification, etc.").
[0008] In order to solve the above-described problems, one aspect of the present invention is a secondary battery including a positive electrode having a positive electrode active material and an electrolyte, wherein the positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material includes an additive element, the additive element being one or more selected from magnesium, aluminum, and nickel, the electrolyte includes an organic solvent, and the organic solvent includes a fluorinated cyclic carbonate and a fluorinated chain carbonate, and after a charge-discharge cycle test is repeated three or more cycles on the secondary battery, the positive electrode is removed from the secondary battery, and the additive element is detected by XPS analysis of the positive electrode.
[0009] Another aspect of the present invention is a secondary battery including a positive electrode having a positive electrode active material and an electrolyte, wherein the positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material includes magnesium, the electrolyte includes an organic solvent, and the organic solvent includes a fluorinated cyclic carbonate and a fluorinated chain carbonate, and after a charge-discharge cycle test is repeated three or more cycles on the secondary battery, the positive electrode is removed from the secondary battery, and magnesium is detected by XPS analysis of the positive electrode.
[0010] Another aspect of the present invention is a secondary battery including a positive electrode having a positive electrode active material and an electrolyte, wherein the positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material includes magnesium, and the electrolyte includes an organic solvent, which includes a fluorinated cyclic carbonate and a fluorinated chain carbonate. After a charge-discharge cycle test is repeated 100 cycles on the secondary battery, the positive electrode is removed from the secondary battery, and magnesium is detected by XPS analysis of the positive electrode.
[0011] Another aspect of the present invention is a secondary battery including a positive electrode having a positive electrode active material and an electrolyte, wherein the positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material includes an additive element, the additive element including at least one selected from magnesium, aluminum, and nickel, the electrolyte includes an organic solvent, and the organic solvent includes fluoroethylene carbonate and methyl trifluoropropionate, wherein when the total volume of the fluoroethylene carbonate and the methyl trifluoropropionate is 100 vol %, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is y:100-y (where 5≦y≦30), and after three or more cycles of charge-discharge cycle testing of the secondary battery are repeated, the positive electrode is removed from the secondary battery and the additive element is detected in XPS analysis of the positive electrode.
[0012] Another aspect of the present invention is a secondary battery including a positive electrode having a positive electrode active material and an electrolyte, wherein the positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material includes magnesium, the electrolyte includes an organic solvent, and the organic solvent includes fluoroethylene carbonate and methyl trifluoropropionate, and when the total volume of the fluoroethylene carbonate and the methyl trifluoropropionate is taken as 100 vol %, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is y:100-y (where 5≦y≦30), and after a charge-discharge cycle test of the secondary battery is repeated three or more cycles, the positive electrode is removed from the secondary battery and magnesium is detected in XPS analysis of the positive electrode.
[0013] Another aspect of the present invention is a secondary battery including a positive electrode having a positive electrode active material and an electrolyte, wherein the positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material includes magnesium, the electrolyte includes an organic solvent, and the organic solvent includes fluoroethylene carbonate and methyl trifluoropropionate, and when the total volume of the fluoroethylene carbonate and the methyl trifluoropropionate is 100 vol %, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is y:100-y (where 5≦y≦30), and after the secondary battery is subjected to 100 cycles of a charge-discharge cycle test, the positive electrode is removed from the secondary battery and magnesium is detected in XPS analysis of the positive electrode.
[0014] In the present invention, lithium cobalt oxide is Li x CoO 2 and Li x CoO 2 When x is 1, lithium cobaltate has a layered rock salt type crystal structure belonging to the space group R-3m, and Li x CoO 2 When x satisfies the condition 0.1<x≦0.24, the lithium cobaltate preferably has a crystal structure of space group P2 / m, a=0.4880±0.005 nm, b=0.2817±0.005 nm, c=0.4839±0.005 nm, α=90°, β=109.6±0.1°, and γ=90°.
[0015] In the present invention, lithium cobalt oxide is Li x CoO 2 and Li x CoO 2 When x is 1, lithium cobaltate has a layered rock salt type crystal structure belonging to the space group R-3m, and Li x CoO 2 When x is 0.1<x≦0.24, it is preferable that the lithium cobalt oxide has diffraction peaks at least at 2θ=19.37° or more and 19.57° or less and at 2θ=45.57° or more and 45.67° or less when analyzed by XRD.
[0016] According to the present invention, a secondary battery having good initial characteristics can be provided.
[0017] The above-described effects do not preclude the existence of other effects. Furthermore, the above-described effects are considered to be independent of each other, and the present invention does not necessarily achieve all of the above-described effects. Furthermore, effects other than those described above can be extracted from the description of this specification and the like.
[0018] FIGS. 1A and 1B are diagrams illustrating a secondary battery according to one embodiment of the present invention. FIGS. 2A and 2B are diagrams illustrating a cathode active material according to one embodiment of the present invention. FIG. 3 is a diagram illustrating a crystal structure of a cathode active material according to one embodiment of the present invention. FIG. 4 is a diagram illustrating a crystal structure of a cathode active material. FIG. 5 is a diagram illustrating an XRD pattern. FIG. 6 is a diagram illustrating an XRD pattern. FIGS. 7A and 7B are diagrams illustrating XRD patterns. FIG. 8 is a graph showing changes in the c-axis length of a cathode active material. FIGS. 9A to 9C are diagrams illustrating a method for manufacturing a cathode active material according to one embodiment of the present invention. FIGS. 10A to 10C are diagrams illustrating a method for manufacturing a cathode active material according to one embodiment of the present invention. FIG. 11 is a diagram illustrating a method for manufacturing a cathode active material according to one embodiment of the present invention. FIGS. 12A to 12C are diagrams illustrating a method for manufacturing a cathode active material according to one embodiment of the present invention. FIGS. 13A to 13D are diagrams illustrating a cathode according to one embodiment of the present invention. FIG. 14A is an exploded perspective view of a coin-type secondary battery, FIG. 14B is a perspective view of the coin-type secondary battery, and FIG. 14C is a cross-sectional perspective view thereof. FIG. 15A is a diagram illustrating an example of a cylindrical secondary battery. FIG. 15B is a diagram illustrating an example of a cylindrical secondary battery. FIG. 15C is a diagram illustrating an example of a plurality of cylindrical secondary batteries. FIG. 15D is a diagram illustrating an example of a power storage system having a plurality of cylindrical secondary batteries. FIGS. 16A and 16B are diagrams illustrating an example of a secondary battery, and FIG. 16C is a diagram illustrating the interior of a secondary battery. FIGS. 17A to 17C are diagrams illustrating an example of a secondary battery. FIGS. 18A and 18B are diagrams illustrating the appearance of a secondary battery. FIGS. 19A to 19C are diagrams illustrating a method for manufacturing a secondary battery. FIGS. 20A to 20D are diagrams illustrating an example of a transportation vehicle. FIG. 20E is a diagram illustrating an example of an artificial satellite. Fig. 21A is a diagram showing an electric bicycle, Fig. 21B is a diagram showing a secondary battery for an electric bicycle, and Fig. 21C is a diagram showing a scooter. Figs. 22A to 22E are diagrams explaining an example of an electronic device. Fig. 23 is a graph showing calculation results of LUMO levels and HOMO levels of an organic compound. Fig. 24 is a graph showing calculation results of LUMO levels and HOMO levels of an organic compound. Fig. 25 is a graph showing a charging curve of a half cell. Fig. 26 is a graph showing a dQ / dV curve.27A to 27C are graphs showing the results of a charge-discharge cycle test. FIG. 28A is an STEM image, and FIG. 28B is a graph showing the results of STEM-EDX analysis. FIGS. 29A to 29C are SEM images of the positive electrode. FIGS. 30A and 30B are graphs showing the results of a charge-discharge cycle test. FIG. 31A is an SEM image of the positive electrode, FIGS. 31B to 31E are mapping images of the positive electrode, and FIG. 31F is a graph of the energy spectrum. FIG. 32A is an SEM image of the positive electrode, FIGS. 32B to 32E are mapping images of the positive electrode, and FIG. 32F is a graph of the energy spectrum. FIG. 33A is an SEM image of the positive electrode, FIGS. 33B to 33E are mapping images of the positive electrode, and FIG. 33F is a graph of the energy spectrum. FIG. 34 is a graph showing fluorine bonding. FIGS. 35A to 35C are graphs showing the results of a charge-discharge cycle test. 36A to 36C are graphs showing the results of a charge-discharge cycle test. Fig. 37 shows NMR spectra of organic compounds. Fig. 38A to 38C show NMR spectra of organic compounds.
[0019] Embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various modifications in form and detail can be made without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below. In the configuration of the invention described below, the same reference numerals will be used in common between different drawings for the same parts or parts having similar functions, and repeated descriptions thereof may be omitted.
[0020] Ordinal numbers such as "first" and "second" used in this specification are used to avoid confusion between components, and do not indicate the order or ranking of processes or stacking order. Furthermore, even if a term is not used in this specification, an ordinal number may be used in the claims to avoid confusion between components. Furthermore, even if a term is used in this specification, a different ordinal number may be used in the claims. Furthermore, even if a term is used in this specification, the ordinal number may be omitted in the claims.
[0021] In this specification, the initial characteristics refer to the characteristics up to the fifth cycle in a charge-discharge cycle test. Good initial characteristics include exhibiting the maximum discharge capacity up to the fifth cycle in a charge-discharge cycle test. Furthermore, good initial characteristics include a discharge capacity retention rate at the fifth cycle in a charge-discharge cycle test of 95% or more, preferably 97% or more, and more preferably 99% or more of the discharge capacity retention rate at the first cycle. Good initial characteristics also include a fluctuation range of the discharge capacity at the fifth cycle relative to the discharge capacity at the first cycle in a charge-discharge cycle test of 5% or less, preferably 1% or less. Good initial characteristics also include a fluctuation range of the charge-discharge efficiency at the fifth cycle relative to the charge-discharge efficiency at the first cycle in a charge-discharge cycle test of 5% or less, preferably 1% or less. Charge-discharge efficiency, also known as coulomb efficiency, is a percentage value of the amount of discharged electricity relative to the amount of charged electricity.
[0022] In this specification, room temperature is 25°C unless otherwise specified. In this specification, the term "electrolyte" refers to a liquid in which a lithium salt is dissolved in an organic solvent at room temperature. The organic solvent contains an organic compound that exhibits carrier ion conductivity. The electrolyte of the present invention is not limited to being a liquid at room temperature. Therefore, in this specification, the concept related to the electrolyte may be referred to as "electrolyte."
[0023] In this specification, a secondary battery using lithium ions as carrier ions is referred to as a lithium ion secondary battery. Other carrier ions include lithium ions, sodium ions, and magnesium ions. However, the carrier ions of the present invention are not limited to lithium ions.
[0024] In this specification and the like, carbonate refers to an organic compound having at least one carbonate ester in its molecular structure, and includes cyclic carbonates and chain carbonates unless otherwise specified. Furthermore, chain carbonates include both linear and branched chain carbonates.
[0025] In this specification, etc., uneven distribution refers to the concentration of an element in a certain region being different from that in other regions. It is synonymous with uneven distribution or the coexistence of areas with high and low concentrations. The uneven distribution of an element through solid solution is called segregation. In this specification, etc., segregation of an element includes a state in which an element (e.g., A) is unevenly distributed in a solid composed of multiple elements (e.g., A, B, C).
[0026] In this specification, the distribution of a certain element refers to the continuous presence of that element when the element is detected in a range that is not noise using any analytical method. A continuous change in the concentration of the element is sometimes called a concentration gradient. The maximum value in the distribution is sometimes called a peak. When identifying a peak, a distribution limited to a certain region can be targeted. The above-mentioned distribution is not limited to a normal distribution. For a distribution in which a peak has been identified, the half-width of the distribution can be determined.
[0027] In this specification, the surface layer of the positive electrode active material refers to a region having a depth of 100 nm or less, preferably a region having a depth of 50 nm or less. The surface layer is synonymous with the near-surface and near-surface region. The depth refers to the distance from the surface of the positive electrode active material toward the interior, and is the distance in a direction perpendicular or approximately perpendicular to the surface. "Almost perpendicular to the surface" refers to an angle with the surface of 80° or more and 100° or less (excluding 90°). The region deeper than the surface layer of the positive electrode active material is referred to as the "interior." The "interior" is synonymous with the bulk or core.
[0028] In this specification and the like, characteristics of a positive electrode active material may be described, but not all of the positive electrode active materials in a positive electrode necessarily have the characteristic. For example, if three or more of five or more randomly selected positive electrode active materials have the characteristic, the characteristics of the positive electrode active materials are sufficiently exhibited, and it can be said that there is an effect of improving the characteristics of a secondary battery including the positive electrode active materials.
[0029] In this specification, space groups are expressed using short notation in international notation (or Hermann-Mauguin notation). Crystal planes and crystal directions are expressed using Miller indices. In crystallography, space groups, crystal planes, and crystal directions are expressed by adding a superscript bar to the numbers. However, due to formatting constraints, in this specification, instead of adding a bar above the numbers, a minus sign (-) may be added before the numbers. Furthermore, for ease of understanding the structure, trigonal crystals expressed by the space group R-3m are generally expressed as a hexagonal complex hexagonal lattice, and unless otherwise specified, the space group R-3m will be expressed as a complex hexagonal lattice in this specification.
[0030] In this specification, the (001) plane, the (003) plane, and the like may be collectively referred to as the (001) plane. In this specification, the (001) plane may also be referred to as the C plane, the basal plane, and the like. Furthermore, in lithium cobalt oxide, lithium has a two-dimensional diffusion path. In other words, it can be said that the lithium diffusion path exists along the plane. In this specification, the plane where the lithium diffusion path is exposed may be referred to as the edge plane. In other words, the edge plane corresponds to a plane other than the plane where lithium is inserted and extracted (specifically, the (001) plane).
[0031] In this specification and the like, the positive electrode active material is described as being particulate, but the particulate shape is not limited to a spherical shape (a circular cross-sectional shape) and includes cross-sectional shapes such as an ellipse, a rectangle, a trapezoid, a triangle, a square with rounded corners, or an asymmetric shape. The cross-sectional shapes of the multiple positive electrode active materials do not have to be the same, and may be different.
[0032] In this specification, the theoretical capacity of a positive electrode active material refers to the amount of electricity when all of the intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated. 2The theoretical capacity of LiNiO is 274 mAh / g per weight of the positive electrode active material. 2 The theoretical capacity of LiMn is 275 mAh / g per weight of the positive electrode active material. 2 O 4 The theoretical capacity of the positive electrode active material is 148 mAh / g.
[0033] In this specification, the amount of lithium remaining in the positive electrode active material that can be inserted or removed is determined by x in the composition formula, for example, Li x MO 2 In the above formula, M represents a transition metal, and unless otherwise specified in this specification, M is cobalt and / or nickel. In the case of a positive electrode active material in a secondary battery, x can be expressed as (theoretical capacity - charging capacity) / theoretical capacity (both are capacity per weight of the positive electrode active material). For example, Li x MO 2 When a secondary battery using Li as the positive electrode active material is charged up to 219.2 mAh / g per weight of the positive electrode active material, 0.2 MO 2 Or we can say x = 0.2. x MO 2 When the x in the formula is small, it means that 0.1<x≦0.24. When the lithium cobalt oxide satisfies the stoichiometric ratio, the composition formula is LiCoO 2 When lithium cobalt oxide is used for the positive electrode, the lithium cobalt oxide in the secondary battery after discharge is also LiCoO 2 It can be said that x = 1. The completion of discharge here refers to a state in which the current per weight of the positive electrode active material is 100 mA / g or less and the voltage is 3.0 V or less or 2.5 V or less.
[0034] Li x MO 2 The charge capacity and / or discharge capacity used to calculate x in the above should preferably be calculated under conditions where there is no influence of short circuit and / or decomposition of the electrolyte in the secondary battery, or where such influence is minimal. For example, data from a secondary battery that has experienced a sudden change in capacity that is considered to be due to a short circuit should not be used to calculate x.
[0035] Unless otherwise specified, the materials (positive electrode active material, negative electrode active material, electrolyte, separator, etc.) contained in the secondary battery are described in their pre-degradation state. A decrease in discharge capacity due to aging and burn-in treatments during secondary battery manufacturing is not considered to be degradation. For example, a secondary battery consisting of a single cell or a battery pack can be said to be in its pre-degradation state if it has a discharge capacity of 97% or more of its rated capacity. For secondary batteries for portable devices, the rated capacity conforms to JIS C 8711:2019. For other secondary batteries, the rated capacity conforms not only to the above JIS standard but also to various JIS and IEC standards for electric vehicle propulsion, industrial use, etc.
[0036] In this specification and the like, the state of the materials of a secondary battery before deterioration is sometimes referred to as an initial product or initial state, and the state after deterioration (the state when the secondary battery has a discharge capacity of less than 97% of the rated capacity) is sometimes referred to as a product in use or a state in use, or a used product or a used state.
[0037] In this specification, a full cell refers to a battery assembled to have different electrodes, such as a unit cell having a positive electrode and a negative electrode, whereas a half cell refers to a battery assembled using lithium metal as the negative electrode (counter electrode).
[0038] In this specification, unless otherwise specified, the voltage of a secondary battery is expressed based on the potential of lithium metal. When a material other than lithium metal is used for the counter electrode, the potential of the secondary battery and the potential of the positive electrode differ. For example, when focusing on the potential of the positive electrode, charging to 4.5 V when the counter electrode is graphite is roughly equivalent to charging to 4.6 V when the counter electrode is lithium metal.
[0039] In this specification and the like, the phrase "having A and / or B" may be used, which means having A, having B, or having A and B.
[0040] Embodiment 1 In this embodiment, a secondary battery of one embodiment of the present invention will be described with reference to the drawings.
[0041] <Electrolyte> One feature of the secondary battery of the present invention is that the electrolyte contains fluorine. A fluorine-containing electrolyte can be obtained by using a fluorine-containing organic compound as the organic solvent. A fluorine-containing electrolyte can also be obtained by using a fluorine-containing organic compound as the lithium salt. A fluorine-containing electrolyte can also be obtained by using a fluorine-containing organic compound as an additive. A fluorine-containing electrolyte is less susceptible to oxidation than an electrolyte that does not contain fluorine, i.e., it exhibits high oxidation resistance. Therefore, using a fluorine-containing electrolyte in a secondary battery in which a redox reaction occurs is preferable because it provides high stability and good initial characteristics. Furthermore, a fluorine-containing electrolyte can provide a stable secondary battery even when the charging voltage is increased. When the above electrolyte is liquid at room temperature, it is called an electrolytic solution.
[0042] <Organic Solvent> Organic solvents using fluorine-containing organic compounds will be described. Specific examples of fluorine-containing organic compounds include fluorinated cyclic carbonates (sometimes referred to as fluorinated cyclic carbonates). Another example of fluorine-containing organic compounds is fluorinated chain carbonates (sometimes referred to as fluorinated chain carbonates). Both fluorinated cyclic carbonates and fluorinated chain carbonates have electron-withdrawing substituents. Organic compounds having electron-withdrawing substituents are more susceptible to desolvation with lithium ions than organic compounds without electron-withdrawing substituents; specifically, the solvation energy of lithium ions is lower. For this reason, fluorine-containing organic compounds are suitable for organic solvents, and such organic solvents can provide secondary batteries with good initial characteristics. It is more preferable for the organic solvent to contain both fluorinated cyclic carbonates and fluorinated chain carbonates.
[0043] Examples of fluorinated cyclic carbonates that can be used include fluoroethylene carbonate (also called fluorinated ethylene carbonate or fluoroethylene carbonate, abbreviated as FEC or F1EC), difluoroethylene carbonate (abbreviated as DFEC or F2EC), trifluoroethylene carbonate (abbreviated as F3EC), tetrafluoroethylene carbonate (abbreviated as F4EC), and pentafluoroethylene carbonate (abbreviated as F5EC). DFEC includes isomers such as cis-4,5 and trans-4,5. Since all of the fluorinated cyclic carbonates have electron-withdrawing substituents, the solvation energy of lithium ions in organic solvents containing the fluorinated cyclic carbonates is thought to be low.
[0044] The structural formula of FEC is shown below in (H11): In FEC, the electron-withdrawing substituent is an F group.
[0045]
[0046] The structural formula of 4,5-difluoroethylene carbonate is shown below as (H12): In 4,5-difluoroethylene carbonate, the electron-withdrawing substituent is an F group.
[0047]
[0048] The structural formula of 4,4-difluoroethylene carbonate is shown below as (H13): In 4,4-difluoroethylene carbonate, the electron-withdrawing substituent is an F group.
[0049]
[0050] The structural formula of F3EC is shown below in (H14): In F3EC, the electron-withdrawing substituent is an F group.
[0051]
[0052] The structural formula of F4EC is shown below in (H15): In F4EC, the electron-withdrawing substituent is an F group.
[0053]
[0054] The above-mentioned fluorinated cyclic carbonates are sometimes collectively referred to as cyclic molecules.
[0055] Methyl trifluoropropionate is an example of a fluorinated chain carbonate. A typical structural formula of methyl 3,3,3-trifluoropropionate is shown below (H21). The abbreviation for methyl 3,3,3-trifluoropropionate is "MTFP." In MTFP, the electron-withdrawing substituent is CF 3 It is the base.
[0056]
[0057] An example of a fluorinated chain carbonate is methyl 2,2-difluoropropionate. The structural formula of methyl 2,2-difluoropropionate is shown below in (H22). In methyl 2,2-difluoropropionate, the electron-withdrawing substituent is CF 2 It is the base.
[0058]
[0059] An example of a fluorinated chain carbonate is trifluoromethyl propionate. The structural formula of trifluoromethyl propionate is shown below (H23). In trifluoromethyl propionate, the electron-withdrawing substituent is CF 3 It is the base.
[0060]
[0061] Methyl pentafluoropropionate is an example of a fluorinated chain carbonate. The structural formula of methyl pentafluoropropionate is shown below (H24). The electron-withdrawing substituent in methyl pentafluoropropionate is CF 3 It is the base.
[0062]
[0063] An example of a fluorinated chain carbonate is trifluoromethyl 3,3,3-trifluoropropionate. The structural formula of trifluoromethyl 3,3,3-trifluoropropionate is shown below in (H25). In trifluoromethyl 3,3,3-trifluoropropionate, the electron-withdrawing substituent is CF 3 It is the base.
[0064]
[0065] The above-mentioned fluorinated chain carbonates are sometimes collectively referred to as chain molecules.
[0066] The organic solvent preferably contains one or more selected from the above-mentioned fluorinated cyclic carbonates and one or more selected from the fluorinated chain carbonates. This makes it possible to provide a secondary battery that exhibits good initial characteristics. More preferably, the organic solvent contains both FEC and MTFP. The reason for this will be explained below.
[0067] <FEC and MTFP> FEC is a cyclic carbonate with a high dielectric constant, and therefore, when used in an organic solvent, it has the effect of promoting the dissociation of lithium salts. On the other hand, because FEC has an electron-withdrawing substituent, it is more likely to desolvate with lithium ions than ethylene carbonate (EC). Specifically, the solvation energy of lithium ions in FEC is smaller than that of EC that does not have an electron-withdrawing substituent. Therefore, it is easier to separate lithium ions from the surface of the positive electrode active material and the surface of the negative electrode active material, thereby reducing the internal resistance of the secondary battery. Furthermore, because FEC has a deep highest occupied molecular orbital (HOMO), it is less susceptible to oxidation and has improved oxidation resistance. On the other hand, there are concerns about the high viscosity of FEC. Therefore, it is recommended to use a mixed organic solvent containing not only FEC but also MTFP in the electrolyte. MTFP is a type of chain carbonate, and can have the effect of reducing the viscosity of the electrolyte solution or maintaining the viscosity at room temperature (typically 25° C.) even at low temperatures (typically 0° C.). Furthermore, although MTFP has a lower solvation energy than methyl propionate (abbreviated as "MP"), which does not have an electron-withdrawing substituent, it may form a solvate with lithium ions when used in the electrolyte solution.
[0068] The blending ratio of FEC and MTFP will be explained. The total content of FEC and MTFP is 100 vol%, and the volume ratio should be FEC:MTFP = y:100-y (where 5≦y≦30, preferably 10≦y≦20). In other words, it is preferable that the amount of MTFP is greater than that of FEC. An organic solvent containing FEC and MTFP exhibits an appropriate viscosity as an electrolyte. This allows for the provision of a secondary battery with good initial characteristics. Furthermore, because FEC and MTFP can maintain an appropriate viscosity as an electrolyte, the low-temperature characteristics of the secondary battery are improved.
[0069] The above volume ratio is measured before mixing as an organic solvent. Even if some volatilization occurs during mixing, it is not a problem as long as good initial properties can be exhibited. The organic solvent should be mixed at room temperature.
[0070] Although FEC has been described as a representative example above, any of the organic compounds described as fluorinated cyclic carbonates has the effect of promoting dissociation of lithium salts, is easily desolvated with lithium ions, and has a high viscosity that does not result in an appropriate viscosity when used alone. Furthermore, although MTFP has been described as a representative example above, any of the organic compounds described as fluorinated chain carbonates can also exhibit the effect of reducing or maintaining the viscosity of the electrolyte. Therefore, if the organic solvent contains a fluorinated cyclic carbonate and a fluorinated chain carbonate, a secondary battery exhibiting good initial characteristics can be provided.
[0071] The organic solvent described above is free from granular dust or molecules other than the constituent molecules of the organic solvent (hereinafter simply referred to as "impurities"), and oxygen (O 2 ), water (H 2 The electrolyte preferably contains a low content of 0 or water, and is highly purified. Specifically, the amount of impurities in the electrolyte is 100 ppm or less, preferably 50 ppm or less, and more preferably less than 10 ppm. The water concentration can be detected by Karl Fischer titration.
[0072] Furthermore, it is preferable that the organic solvent has almost no peaks due to impurities that can be confirmed by NMR measurement, etc. The term "almost no peaks due to impurities" means that the ratio of the integrated area of the peak due to the impurity to the integrated area of the peak due to the main component (simply referred to as "integral ratio") is 0.005 or less, preferably 0.002 or less.
[0073] The organic solvents mentioned above are preferably those that contain reduced amounts of reaction by-products during synthesis, i.e., organic solvents that have been appropriately purified are desirable.
[0074] <Lithium Salt> The lithium salt dissolved in the organic solvent is LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiAlCl 4 , LiSCN, LiBr, LiI, Li 2 SO 4 , Li 2 B 10 Cl 10 , Li 2 B 12 Cl 12 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 4 F 9 SO 2 ) (CF 3 SO 2 ), LiN(C 2 F 5 SO 2 ) 2At least one of lithium bis(oxalate)borate (LiBOB) can be used. Two or more of the above-mentioned lithium salts may be used in any combination, and in such a case, any ratio can be used. To obtain an electrolyte containing fluorine, it is preferable to use a fluorine-containing lithium salt among the above-mentioned lithium salts. When the organic solvent contains fluorine, a fluorine-free lithium salt can be used. Furthermore, the electrolyte of the present invention does not necessarily contain the above-mentioned lithium salt.
[0075] <Additives> It is also preferable to mix an additive with the organic solvent for the purpose of improving safety, etc. The additive may be one or more selected from vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), SUN (suberonitrile), or dinitrile compounds such as succinonitrile or adiponitrile. It is also preferable to select an organic compound different from the organic solvent as the additive. The concentration of the additive is preferably 0.1 wt% or more and 5 wt% or less, for example, with respect to the total organic solvent. The electrolyte of the present invention does not need to contain the above-mentioned additive.
[0076] <Analytical Methods for Electrolytes> The composition of the electrolytes was analyzed by X-ray photoelectron spectroscopy (XPS), gas chromatography-mass spectrometry (GC-MS), liquid chromatography-mass spectrometry (LC-MS), ion chromatography (IC), and inductively coupled plasma atomic emission spectrometry (ICP-AES). The presence or absence of hydroxyl groups can be confirmed using techniques such as atomic absorption spectroscopy (AAS), glow discharge mass spectrometry (GD-MS), nuclear magnetic resonance (NMR), and Fourier transform infrared spectroscopy (FT-IR).
[0077] <Analysis by GC-MS> GC-MS can be used to identify the structural formula and other information of compounds contained in the electrolyte. The electrolyte may be recovered from a secondary battery. When recovering the electrolyte, it is preferable to disassemble the secondary battery in a glove box under an argon atmosphere and extract the electrolyte. Furthermore, if the amount of electrolyte contained in the secondary battery is small, a solvent that does not affect GC-MS analysis may be poured into the secondary battery, and a liquid mixture of the solvent and electrolyte may be extracted. Deuterium acetonitrile is preferably used as the solvent. The apparatus and conditions used for the analysis are not particularly limited, but the following apparatus and conditions can be used, for example. Furthermore, when using the following apparatus, a structural formula with a hit percentage (Hit%) of 80% or more, preferably 90% or more, and more preferably 93% or more with reference data can be adopted as the structural formula of the compound contained in the electrolyte. Apparatus name: Agilent Technologies 7890A GC System Agilent Technologies 5975C inert MSD
[0078] <Analysis by LC-MS> LC-MS can be used to identify the structural formula, etc., of the compound contained in the electrolyte. The electrolyte may be recovered from a secondary battery. When recovering the electrolyte, it is preferable to disassemble the secondary battery in a glove box under an argon atmosphere and extract the electrolyte. Furthermore, if the amount of electrolyte contained in the secondary battery is small, a solvent that does not affect LC-MS analysis may be poured into the secondary battery, and a liquid mixture of the solvent and the electrolyte may be extracted. Deuterium acetonitrile is preferably used as the solvent. The apparatus and conditions used for the analysis are not particularly limited, but the following apparatus and conditions can be used, for example. Furthermore, when using the apparatus below, a structural formula that matches the reference data by 80% or more, preferably 90% or more, and more preferably 93% or more can be adopted as the structural formula of the compound contained in the electrolyte. LC apparatus name: Acquity UPLC MS apparatus name: Xevo QTof MS, manufactured by Waters
[0079] A secondary battery having the above-described electrolyte will be described with reference to the drawings.
[0080] <Secondary Battery> Fig. 1A shows a secondary battery 200a according to one embodiment of the present invention. The secondary battery 200a has an electrolyte 109, an anode 106, a separator 108, and a cathode 107. Another embodiment of the present invention is a secondary battery that does not have a separator. In the secondary battery 200a, the electrolyte 109 is present throughout the anode 106, the separator 108, and the cathode 107. In the present invention, the electrolyte 109 contains fluorine, resulting in a secondary battery with good initial characteristics.
[0081] 1B illustrates the configuration of a secondary battery 200b that does not have the negative electrode active material layer 102, unlike FIG. 1A. Specifically, the negative electrode current collector 101 may have a region in contact with the separator 108. Other configurations of the secondary battery 200b shown in FIG. 1B are similar to those of the secondary battery 200a in FIG. 1A. In this specification and the like, when there is no need to distinguish between the secondary battery 200a and the secondary battery 200b, they are referred to as the secondary battery 200.
[0082] The negative electrode 106 in FIGS. 1A and 1B includes a negative electrode current collector 101 and a negative electrode active material layer 102. The negative electrode active material layer 102 includes at least a negative electrode active material and may include a conductive material and / or a binder. A known material can be used for the negative electrode active material, as described in detail below. The positive electrode 107 in FIGS. 1A and 1B includes a positive electrode current collector 105 and a positive electrode active material layer 104. The positive electrode active material layer 104 includes at least a positive electrode active material and may include a conductive material and / or a binder. Although a known material can be used for the positive electrode active material, the use of a positive electrode active material according to one embodiment of the present invention allows the secondary battery to withstand high-voltage charging and therefore exhibits good discharge capacity. Furthermore, the use of a positive electrode active material according to one embodiment of the present invention results in a secondary battery exhibiting good cycle characteristics. The positive electrode active material according to one embodiment of the present invention will be described below.
[0083] By including the electrolyte according to one embodiment of the present invention, a secondary battery having at least good initial characteristics can be realized. Furthermore, by including the above-described electrolyte and a positive electrode active material, a secondary battery having good initial characteristics, improved discharge capacity, and good cycle characteristics can be realized.
[0084] This embodiment mode can be freely combined with other embodiment modes.
[0085] (Embodiment 2) In this embodiment, a positive electrode active material and a manufacturing method thereof according to one embodiment of the present invention will be described. Note that the positive electrode active material according to one embodiment of the present invention is preferably a material that is less susceptible to deterioration during charge and discharge at a high charge voltage. A known material that is less susceptible to deterioration during charge and discharge at a high charge voltage can also be used. The high charge voltage is defined as a condition of 4.6 V or higher relative to the potential of lithium metal.
[0086] [Positive Electrode Active Material] A positive electrode active material 100 according to one embodiment of the present invention will be described. The positive electrode active material 100 contains carrier ions, typically lithium ions (Li +A compound containing a transition metal and oxygen capable of inserting and removing ions may be used. The transition metal may be one or more selected from cobalt (Co), nickel (Ni), manganese (Mn), iron (Fe), etc., but it is preferable to have at least cobalt and / or nickel. FIG. 2A shows an example of the cross-sectional structure of a positive electrode active material 100. The positive electrode active material 100 has a surface layer 100a and an interior 100b, and the (001) plane is indicated by a dashed line in the figure.
[0087] <Main Component> In the positive electrode active material 100 according to one embodiment of the present invention, it is preferable to use cobalt and / or nickel as the main component of the transition metal M responsible for the oxidation-reduction reaction. In this specification and the like, the main component of the transition metal M refers to the transition metal M having the highest atomic ratio, and it is preferable to apply cobalt rather than nickel. For example, as a compound using Co as the transition metal, lithium cobalt oxide can be applied to the positive electrode active material 100. Alternatively, the positive electrode active material 100 can be lithium cobalt oxide (LiCoO 2 ) to which an additive element described below has been added. Therefore, the composition of the lithium cobalt oxide is not strictly limited to Li:Co:O=1:1:2. The positive electrode active material 100 according to one embodiment of the present invention preferably has a crystalline structure described below, particularly a crystalline structure in a charged state.
[0088] FIG. 2B shows a positive electrode active material 100 having a crystal grain boundary 110. The crystal grain boundary 110 refers to, for example, a portion where particles of the positive electrode active material 100 are adhered to each other, a portion where the crystal orientation changes inside the positive electrode active material 100, that is, a portion where the repetition of bright and dark lines in an STEM image (scanning transmission electron microscopy: an image observed by scanning transmission electron microscopy) or the like becomes discontinuous, a portion containing many crystal defects, a portion where the crystal structure is disordered, or the like. Furthermore, crystal defects refer to defects that can be observed in a cross-sectional TEM image (an image observed by transmission electron microscopy: an image observed by transmission electron microscopy), a cross-sectional STEM image, or the like, that is, a structure in which other atoms have entered between the lattices, cavities, or the like. The crystal grain boundary 110 can be said to be one of the planar defects. The vicinity of the grain boundary 110 includes a region within 10 nm of the grain boundary 110 within the positive electrode active material.
[0089] FIG. 2B shows a positive electrode active material 100 having a crack 112. A crack is sometimes referred to as a region where the crystal plane is displaced or a region where the crystal plane is broken, and often occurs along the (001) plane. It is preferable that such a crack 112 is not observed in a cross-sectional TEM image or a cross-sectional STEM image. The vicinity of the crack 112 includes a region within 10 nm of the crack 112 within the positive electrode active material.
[0090] <Additive Element> The positive electrode active material 100 preferably contains an additive element. The additive element is preferably present in the surface layer portion 100 a, but may also be present in the interior portion 100 b. As the additive element, one or more selected from magnesium, fluorine, nickel, and aluminum can be used.
[0091] [Magnesium] Magnesium becomes a divalent cation, and in the layered rock salt crystal structure, magnesium ions tend to exist at the lithium site rather than the cobalt site. 2Since it functions as a pillar supporting the layers, it is easy to maintain the layered rock salt type crystal structure at least in the inner part 100b. In addition, it is preferable that magnesium exists at a higher concentration in the surface layer part 100a than in the inner part 100b. Since magnesium can remain in the surface layer part 100a of the lithium cobalt oxide even after a charge-discharge cycle test, deterioration can be suppressed. The presence of magnesium can suppress the desorption of oxygen around the magnesium. Therefore, Li x CoO 2 In the charging state, the value of x is 0.24 or less, and thus the thermal decomposition reaction can be suppressed. Furthermore, the presence of magnesium in the surface layer portion 100a is expected to improve corrosion resistance against hydrofluoric acid produced by decomposition of the electrolyte, etc., and is therefore preferable.
[0092] [Fluorine] Fluorine becomes a monovalent anion, and when present in the surface layer 100a or adsorbed on the surface, the energy required for lithium ions to desorb from the positive electrode active material 100 is reduced. This is because the redox potential of cobalt ions accompanying lithium ion desorption differs depending on the presence or absence of fluorine. In other words, in the absence of fluorine, cobalt ions change from trivalent to tetravalent upon lithium desorption. On the other hand, when fluorine is present, cobalt ions change from divalent to trivalent upon lithium desorption. The redox potential of cobalt ions differs between the two. Therefore, the desorption and insertion of lithium ions near the fluorine is more likely to occur smoothly, and it is preferable to have fluorine in the surface layer or on the surface of the positive electrode active material 100. As long as the energy required for lithium ion desorption is reduced, fluorine may replace oxygen in the surface layer 100a. Furthermore, the presence of fluorine in the surface layer or on the surface, which is the portion in contact with the electrolyte, can suppress excessive reaction between the positive electrode active material 100 and the electrolyte. Furthermore, corrosion resistance to hydrofluoric acid produced by decomposition of the electrolyte and the like can be effectively improved.
[0093] [Nickel] Nickel can exist on either the cobalt site or the lithium site. When present on the cobalt site, nickel has a lower redox potential than cobalt, so it can be said that it is easier to release lithium during charging, for example. This is expected to result in faster charge and discharge speeds.
[0094] Furthermore, when nickel is present at the lithium site, the layer structure consisting of octahedra of cobalt and oxygen can be prevented from shifting. Also, the volume change during charging and discharging is prevented. This is because nickel present at the lithium site can also be prevented from shifting to CoO 2 This is presumably because they function as pillars supporting the layers together. Therefore, it is expected that the crystal structure will be more stable, particularly in a charged state at high temperatures, for example, 45° C. or higher, which is preferable.
[0095] On the other hand, excessive nickel is undesirable because it increases the influence of distortion due to the Jahn-Teller effect. Furthermore, excessive nickel may adversely affect lithium insertion and desorption. Therefore, it is preferable that the amount of nickel contained in the entire positive electrode active material 100 is appropriate. For example, the number of nickel atoms contained in the positive electrode active material 100 is less than the number of cobalt atoms, preferably more than 0% to 7.5% of the number of cobalt atoms, preferably 0.05% to 4%, preferably 0.1% to 2%, and more preferably 0.2% to 1%. The amount of nickel shown here may be a value obtained by performing elemental analysis of the entire positive electrode active material using, for example, GD-MS, ICP-MS, or the like, or may be based on the value of the raw material composition during the production process of the positive electrode active material.
[0096] [Aluminum] Aluminum can also be present at the cobalt site in the layered rock salt crystal structure. Aluminum is a typical element, and aluminum ions are trivalent cations whose valence does not change. Therefore, lithium ions around the aluminum are less likely to move during charging and discharging. Therefore, the aluminum and its surrounding lithium function as pillars, suppressing changes in the crystal structure. It is preferable that aluminum be present at least in the interior 100b, and deterioration of the positive electrode active material 100 can be suppressed even if a force that causes expansion and contraction in the c-axis direction occurs due to the insertion and desorption of lithium ions, i.e., even if a force that causes expansion and contraction in the c-axis direction occurs due to changes in the charge depth or charge rate.
[0097] Furthermore, aluminum has the effect of suppressing the elution of surrounding cobalt and improving continuous charge durability. Furthermore, because the Al-O bond is stronger than the Co-O bond, it can suppress the detachment of oxygen from the aluminum. These effects improve thermal stability. Furthermore, it is possible to obtain a positive electrode active material 100 whose crystalline structure is resistant to collapse even after repeated charge and discharge.
[0098] [Titanium] Titanium oxide is known to have superhydrophilic properties. Therefore, by forming the cathode active material 100 with titanium oxide in the surface layer portion 100a, it is possible that the cathode active material 100 has good wettability with highly polar solvents. When used in a secondary battery, this improves the contact at the interface between the cathode active material 100 and a highly polar electrolyte, which may suppress an increase in internal resistance.
[0099] [Phosphorus] When the positive electrode active material 100 contains phosphorus, the phosphorus reacts with hydrofluoric acid generated by decomposition of the electrolyte or lithium salt, which may reduce the concentration of hydrofluoric acid in the electrolyte. 6 When the compound has the formula (I), HF may be generated by hydrolysis.
[0100] Furthermore, hydrofluoric acid may be generated by a reaction between polyvinylidene fluoride (PVDF), which is used as a component of the positive electrode, and alkali. The reaction between hydrofluoric acid and phosphorus reduces the hydrofluoric acid concentration in the electrolyte, which may prevent the gelation and / or insolubilization of PVDF and result in reduced adhesion. Furthermore, the reaction between hydrofluoric acid and phosphorus reduces the hydrofluoric acid concentration in the electrolyte, which may prevent the corrosion of the current collector.
[0101] [Multiple Additional Elements] It is preferable to have multiple additional elements as described above, since the effects of the respective additional elements are synergistic. As a result, further stabilization of the surface layer portion 100a is expected. In particular, it is preferable to have magnesium, nickel, and aluminum, since this enhances the effect of forming a stable crystal structure.
[0102] However, if the surface layer 100a is occupied only by a compound of the additive element and oxygen, it is not preferable because it makes it difficult to insert and extract lithium ions. Therefore, the surface layer 100a must contain at least cobalt, and in a discharged state, it must also contain lithium, and must have a path for the insertion and extraction of lithium ions.
[0103] In order to ensure sufficient paths for lithium ion insertion and desorption, the concentration of cobalt is preferably higher than that of magnesium in the surface layer portion 100a. For example, when measured from the surface of the positive electrode active material 100 using XPS (X-ray photoelectron spectroscopy), the ratio Mg / Co of the number of magnesium atoms Mg to the number of cobalt atoms Co is preferably 0.62 or less, and more preferably 0.5 or less. The concentration of cobalt is preferably higher than that of nickel in the surface layer portion 100a. The concentration of cobalt is preferably higher than that of aluminum in the surface layer portion 100a. The concentration of cobalt is preferably higher than that of fluorine in the surface layer portion 100a.
[0104] <Median diameter (D50) of positive electrode active material> The median diameter (D50) of the positive electrode active material will be described. If the positive electrode active material is too small, it may be difficult to coat the positive electrode during production. Furthermore, if the positive electrode active material is too small, the surface area may become too large, which may result in excessive reaction between the positive electrode active material surface and the electrolyte. Furthermore, if the positive electrode active material is too small, it may be necessary to mix a large amount of conductive material, which may result in a decrease in discharge capacity or charge capacity. In these respects, the median diameter (D50) of the positive electrode active material is preferably 1 μm or more, preferably 5 μm or more, and more preferably 9 μm or more. Furthermore, a small positive electrode active material that satisfies the above median diameter (D50) is preferred because it is less likely to crack even after undergoing a pressing process.
[0105] On the other hand, if the active materials are too small, there is a concern that the density of the positive electrode active material layer will decrease, side reactions with the electrolyte will increase, etc. In this respect, the median diameter (D50) of the positive electrode active material is preferably 20 μm or less, preferably 18 μm or less, and more preferably 15 μm or less.
[0106] That is, the median diameter (D50) of the positive electrode active material can be any combination of the above upper and lower limits. For example, the median diameter is preferably 1 μm or more and 20 μm or less, more preferably 1 μm or more and 18 μm or less, and even more preferably 1 μm or more and 15 μm or less.
[0107] The above-mentioned median diameter (D50) can be measured, for example, by observation using an SEM (scanning electron microscope) or TEM, or by a particle size distribution analyzer using a laser diffraction / scattering method. When measured using a particle size distribution analyzer using a laser diffraction / scattering method, the median diameter (D50) is the particle diameter at which the integrated amount in a cumulative curve of the particle size distribution measurement results accounts for 50%. Note that, as a method for measuring the median diameter (D50) by analysis using an SEM or TEM, for example, it is preferable to measure 20 or more particles, create an integrated particle amount curve, and use the particle diameter at which the integrated amount accounts for 50%.
[0108] <Crystallinity> The positive electrode active material 100 preferably has high crystallinity, and is more preferably single crystalline or polycrystalline. In particular, if the positive electrode active material 100 has single crystallinity, cracks are less likely to occur even if a volume change occurs in the positive electrode active material 100 due to charge and discharge, which is preferable. Furthermore, the positive electrode active material 100 is preferably a primary particle (also referred to as a single particle) rather than a secondary particle.
[0109] <Smoothness> The surface of the positive electrode active material 100 is preferably smooth. In this specification and the like, a smooth surface includes a state in which the surface roughness is at least 10 nm or less when surface unevenness information is quantified in a cross section of the positive electrode active material 100. In this specification and the like, a cross section corresponds to a cross section obtained as, for example, a TEM image or an STEM image.
[0110] <Few defects including dislocations> The interior 100b preferably has few defects including dislocations. Dislocations are a type of crystal defect and are different from vacancy defects. Such dislocations can be observed, for example, in a TEM image. When there are sufficiently few defects including dislocations, dislocations may not be observed in an observation area (e.g., 1 μm square) of the positive electrode active material 100.
[0111] <Crystallite Size> The crystallite size of the positive electrode active material measured by XRD (X-ray diffraction) is preferably 300 nm or more. The larger the crystallite size, the more Li x CoO 2 When x in the graph is small, the O3'-type crystal structure is easily maintained, and the contraction of the c-axis length is easily suppressed. There is a relationship that the fewer dislocations there are in the region observed in the TEM image, the larger the crystallite size measured by XRD.
[0112] To calculate the crystallite size, for example, a Bruker D8 ADVANCE XRD device is used, with a CuKα source as the X-ray source, 2θ of 15° to 90° in increments of 0.005°, and a LYNXEYE XE-T detector. The diffraction pattern obtained is based on the literature value of lithium cobalt oxide, as specified in ICSD Coll. Code 172909. Analysis can be performed using DIFFRAC. TOPAS ver. 6 crystal structure analysis software. It is preferable to use the LVol-IB value calculated by this method as the crystallite size.
[0113] When calculating the crystallite size, the diffraction pattern is preferably obtained using only the positive electrode active material as the measurement target. However, it may also be obtained for the positive electrode, which includes the positive electrode active material, a current collector, a binder, a conductive material, etc. However, in the positive electrode state, the positive electrode active material may be oriented due to the influence of pressure, etc., during the positive electrode fabrication process. Strong orientation may prevent accurate calculation of the crystallite size. Therefore, it is more preferable to obtain the pattern by removing the positive electrode active material layer from the positive electrode, removing some of the binder, etc., in the positive electrode active material layer using an organic solvent, etc., and then loading the sample into a sample holder. Alternatively, for powder samples, the diffraction pattern can be obtained by applying grease to a silicon anti-reflection plate and then adhering the powder.
[0114] <Crystalline Structure of the Positive Electrode Active Material in a Discharged State and a Charged State> The crystalline structures of the positive electrode active material 100 in one embodiment of the present invention in a discharged state and a charged state will be described in comparison with conventional positive electrode active materials. The positive electrode active material 100 is lithium cobalt oxide (LiCoO 2 ) and the conventional positive electrode active material is lithium cobalt oxide that does not contain any additional elements.
[0115] <Li x CoO 2 When x in the figure is 1, the horizontal axis is Li x CoO 2 The figure shows the crystal structure of the positive electrode active material 100 when x is 1, 0.2, and 0.15. x CoO 2 When x is 1, the positive electrode active material 100 can be said to be in a discharged state.
[0116] In a discharged state, the positive electrode active material 100 has a layered rock-salt crystal structure belonging to the space group R-3m. In the layered rock-salt crystal structure, lithium ions occupy octahedral sites, and CoO 2 There are three layers. For this reason, the layered rock salt type crystal structure belonging to the space group R-3m is sometimes called an O3 type crystal structure. 2 The layer refers to a structure in which an octahedral structure in which oxygen is six-coordinated to a transition metal M is continuous on a plane in an edge-sharing state.
[0117] In Fig. 3, the crystal structure when x = 1 is labeled R-3m(O3). The crystal structure represented by R-3m(O3) has a unit cell lattice constant of a = 2.81610 × 10 −10 (m), b=2.81610×10 −10 (m), c=14.05360×10 −10 (m), α = 90.0000, β = 90.0000, and γ = 120.0000. The coordinates of lithium, cobalt, and oxygen in the unit cell are Li(0,0,0), Co(0,0,0.5), and O(0,0,0.23951). When x = 1, FIG. 3 shows lithium ions present at all lithium sites, but in the case of a positive electrode active material 100 containing an additive element, magnesium ions may be present at some of the lithium sites.
[0118] The surface layer 100a of the positive electrode active material 100 is CoO 2 In particular, when lithium ions are released from the positive electrode active material 100 due to charging, the surface layer 100a is reinforced by the CoO 2 It is preferable that the surface layer 100a has a reinforcing function so that the layer structure is not broken. The surface layer 100a is called a barrier film of the positive electrode active material 100. The above-mentioned reinforcement includes suppressing oxygen desorption from the positive electrode active material 100. The above-mentioned reinforcement also includes suppressing oxygen desorption from the positive electrode active material 100. 2 The reinforcement mentioned above includes suppressing the structural deviation of the layers. The reinforcement mentioned above also includes suppressing structural changes in the surface layer portion 100 a and the interior portion 100 b. The reinforcement mentioned above also includes suppressing decomposition of the electrolyte on the surface of the positive electrode active material 100.
[0119] The surface layer 100a is one of the regions that easily becomes unstable during charging and discharging, and where deterioration of the crystalline structure is likely to begin. Therefore, it is preferable that the surface layer 100a have a composition and crystalline structure that are more stable at room temperature than the inner portion 100b. For example, it is preferable that at least a portion of the surface layer 100a has a rock salt-type crystalline structure. Alternatively, it is preferable that the surface layer 100a has both a layered rock salt-type crystalline structure and a rock salt-type crystalline structure. In this way, the surface layer 100a has a crystalline structure different from that of the inner portion 100b, thereby significantly achieving the above-mentioned reinforcing effect. Of course, the surface layer 100a may have the same crystalline structure as the inner portion 100b, as long as the above-mentioned reinforcing effect is achieved.
[0120] <Li x CoO 2 When x in the formula is small (0.1<x≦0.24)≫ Li x CoO 2 When x satisfies 0.1<x≦0.24, the positive electrode active material 100 is in a charged state, which can be said to be a state in which the positive electrode active material 100 is charged at a high voltage of 4.6 V or more, preferably 4.8 V or more, based on the counter electrode lithium metal. When the positive electrode active material 100 is in a charged state at a high voltage, it has a crystal structure different from that of conventional positive electrode active materials. In other words, the change in crystal structure of the positive electrode active material 100 between the discharged state and the charged state is different from that of conventional positive electrode active materials.
[0121] First, the change in the crystal structure of a conventional positive electrode active material in a discharged state and in a charged state at a high voltage will be described with reference to FIG. 4. The horizontal axis of FIG. 4 represents Li x CoO 2 The figure shows the crystal structure of the conventional positive electrode active material when x is 1, 0.5, 0.12, or 0. x CoO 2 4 shows the crystal structure of lithium cobalt oxide when x = 1. In the discharged state, conventional lithium cobalt oxide has the same crystal structure as the positive electrode active material 100, and in FIG. 4, the crystal structure when x = 1 is labeled R-3m(O3).
[0122] In addition, conventional lithium cobalt oxide is Li x CoO 2It is known that when x = 0.5, the symmetry of lithium increases and the crystal structure belongs to the monoclinic space group P2 / m. This structure has CoO 2 There is one layer, so it is sometimes called O1 type or monoclinic O1 type.
[0123] In addition, conventional lithium cobalt oxide is Li x CoO 2 It is known that when x = 0, it has a crystal structure of the trigonal space group P-3m1. This structure also contains CoO in the unit cell. 2 There is one layer. Therefore, this crystal structure is sometimes called O1 type or trigonal O1 type. In addition, when the trigonal crystal is converted into a composite hexagonal lattice, it is sometimes called hexagonal O1 type.
[0124] In addition, conventional lithium cobalt oxide is Li x CoO 2 When x is about 0.12, the crystal structure has the space group R-3m. This structure is similar to CoO, such as trigonal O1 type. 2 and LiCoO such as R-3m(O3). 2 It can also be said that the structure of and the structure are stacked alternately. Therefore, this crystal structure is sometimes called an H1-3 type crystal structure. In fact, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is twice that of other structures. In addition, the actual insertion and desorption of lithium ions does not necessarily occur uniformly in the positive electrode active material, and the lithium ions are unevenly distributed, that is, the lithium concentration becomes uneven. Therefore, in experiments, Li x CoO 2 In this case, an H1-3 type crystal structure is observed from about x=0.25.
[0125] As an example of the H1-3 type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be expressed as Co (0,0,0.42150±0.00016), O1 (0,0,0.27671±0.00045), and O2 (0,0,0.11535±0.00045).
[0126] The unit cell that should be used to represent the crystal structure of the positive electrode active material can be determined, for example, by Rietveld analysis of the XRD diffraction pattern. For example, it is preferable to adopt a unit cell whose GOF (goodness of fit) value is close to 1.
[0127] Li x CoO 2 When charging and discharging are repeated so that x is 0.24 or less (typically, charging at about x = 0.12), the conventional positive electrode active material alternates between the H1-3 type crystal structure and the R-3m(O3) crystal structure, and the crystal structure changes between these, i.e., non-equilibrium phase changes occur repeatedly. 2 Specifically, as shown by the dotted line in the H1-3 type crystal structure in FIG. 2 The layers deviate significantly from R-3m(O3). Such dynamic structural changes can adversely affect the stability of the crystal structure.
[0128] Furthermore, the difference in volume between these two crystal structures is large: when compared per equal number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the R-3m(O3) crystal structure is greater than 3.5%, typically 3.9% or more.
[0129] In addition, the H1-3 type crystal structure has CoO like the trigonal O1 type. 2 A structure with continuous layers is likely to be unstable.
[0130] For these reasons, the crystalline structure of conventional positive electrode active materials collapses when they are repeatedly charged and discharged so that x becomes 0.24 or less. When the crystalline structure collapses, the number of sites where lithium ions can exist stably decreases, and it becomes difficult for lithium to be inserted and extracted, causing a deterioration in cycle characteristics.
[0131] On the other hand, in the positive electrode active material 100 shown in FIG. x CoO 2 In this case, the change in the crystal structure between the discharge state where x = 1 and the state where x is 0.24 or less is smaller than that of conventional positive electrode active materials. 2The layer misalignment is small. Furthermore, when compared per the same number of cobalt atoms, the difference in volume between the H1-3 type crystal structure and the R-3m(O3) type crystal structure can be made small. Therefore, the positive electrode active material 100 is resistant to collapse of its crystal structure even when repeatedly charged and discharged so that x is 0.24 or less, and sites where lithium ions can exist stably are maintained, thereby achieving excellent cycle characteristics.
[0132] Li x CoO 2 The crystal structure of the positive electrode active material 100 when x = about 0.2 and x = about 0.15 is shown in Figure 3. Since the inner portion 100b occupies most of the volume of the positive electrode active material 100, the crystal structure shown in Figure 3 can be said to be the crystal structure of the inner portion 100b of the positive electrode active material 100. Since the inner portion 100b is the portion that contributes greatly to charge and discharge, CoO 2 It is preferable that the displacement of the layers is small and that the volume change of the inner portion 100b is small.
[0133] As shown in FIG. 3, the positive electrode active material 100 has a different crystal structure from that of conventional positive electrode active materials when x is 0.24 or less, for example, when x is about 0.2 or about 0.15, in which case the positive electrode active material has an H1-3 type crystal structure.
[0134] <When x = approximately 0.2> When x = approximately 0.2, the positive electrode active material 100 has a crystal structure belonging to the trigonal space group R-3m. 2 The layer symmetry is the same as that of O3. Therefore, this crystal structure is called an O3'-type crystal structure. Although this crystal structure is not a spinel structure, it is sometimes called a pseudo-spinel structure because a pattern similar to that of a spinel structure may appear in the diffraction pattern. This crystal structure is shown in Figure 3 with the notation R-3m(O3)'.
[0135] By analyzing the diffraction pattern of the O3' type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be estimated. The O3' type crystal structure can be shown as the coordinates of cobalt and oxygen in the unit cell Co(0,0,0.5), O(0,0,x), in the range of 0.20≦x≦0.25. The coordinates of lithium in the unit cell can be said to be Li(0,0,0). The lattice constant of the unit cell is 2.797×10 for the a-axis. −10 ≦a≦2.837×10 −10 (m) is preferred, and 2.807 × 10 −10 ≦a≦2.827×10 −10 (m) is more preferable, and typically a=2.817×10 −10 (m). The c-axis is 13.681 × 10 −10 ≦c≦13.881×10 −10 (m) is preferred, and 13.751 × 10 −10 ≦c≦13.811×10 −10 (m) is more preferable, and typically c=13.781×10 −10 (m).
[0136] <When x = approximately 0.15> When x = approximately 0.15, the positive electrode active material 100 has a crystal structure belonging to the monoclinic space group P2 / m. This is because CoO 2 There is one layer. Furthermore, when x = 0.15, it can be considered that the lithium present in the positive electrode active material 100 is about 15 atomic % in the discharged state. Therefore, this crystal structure is called a monoclinic O1(15) type crystal structure. This crystal structure is shown in Figure 3 with the P2 / m monoclinic O1(15) symbol.
[0137] The monoclinic O1(15) type crystal structure has the coordinates of cobalt and oxygen in the unit cell as Co1(0.5,0,0.5), Co2(0,0.5,0.5), O1(X O1 , 0, Z O1 ), 0.23≦X O1 ≦0.24, 0.61≦Z O1 ≦0.65, O2(X O2 , 0.5, Z O2 ), 0.75≦X O2 ≦0.78, 0.68≦Z O2The lattice constants of the unit cell are a = 0.4880 ± 0.005 nm, b = 0.2817 ± 0.005 nm, c = 0.4839 ± 0.005 nm, α = 90°, β = 109.6 ± 0.1°, and γ = 90°.
[0138] In addition, this crystal structure can show the lattice constant even in the space group R-3m if a certain degree of error is allowed in the Rietveld analysis etc. In this case, the coordinates of cobalt and oxygen in the unit cell are Co(0,0,0.5), O(0,0,Z O ), 0.21≦Z O The lattice constants of the unit cell are a = 0.2817 ± 0.002 nm and c = 1.368 ± 0.01 nm.
[0139] In both the O3' and monoclinic O1(15) crystal structures, ions of cobalt, nickel, magnesium, etc. occupy hexacoordinated oxygen sites, although lighter elements such as lithium and magnesium may occupy tetracoordinated oxygen sites.
[0140] As shown by the dotted line in FIG. 3, the difference between R-3m(O3) in the discharged state and the O3′-type crystal structure is 2 There is almost no layer misalignment. In addition, the R-3m(O3) in the discharge state and the monoclinic O1(15) type crystal structure have a CoO 2 There is almost no layer misalignment.
[0141] The difference in volume per the same number of cobalt atoms between R-3m(O3) in a discharged state and the O3' type crystal structure is 2.5% or less, more specifically 2.2% or less, typically 1.8%.
[0142] The difference in volume per the same number of cobalt atoms between R-3m(O3) in a discharged state and the monoclinic O1(15) type crystal structure is 3.3% or less, more specifically 3.0% or less, typically 2.5%.
[0143] In this way, in the positive electrode active material 100 of one embodiment of the present invention, Li x CoO 2When x is small, i.e., when a large amount of lithium is released, the change in crystal structure is suppressed compared to conventional positive electrode active materials. Furthermore, the change in volume is also suppressed when compared per the same number of cobalt atoms. Therefore, the positive electrode active material 100 is resistant to collapse of its crystal structure even when repeatedly charged and discharged so that x is 0.24 or less, and the decrease in discharge capacity in charge-discharge cycle tests is suppressed. Furthermore, because more lithium ions can be stably utilized than in conventional positive electrode active materials, the positive electrode active material 100 has a large discharge capacity per weight and per volume. Therefore, by using the positive electrode active material 100, a secondary battery with a high discharge capacity per weight and per volume can be fabricated.
[0144] It is not necessary for all particles in the interior 100b of the positive electrode active material 100 to have the O3′-type and / or monoclinic O1(15)-type crystal structure, but rather they may contain other crystal structures, or some of them may be amorphous.
[0145] Also Li x CoO 2 To make the x in the cell small, it is generally necessary to charge the cell at a high charging voltage. x CoO 2 The state where x is small can be rephrased as a state where the battery is charged at a high charging voltage. For example, when CC / CV charging is performed at a voltage of 4.6 V or higher relative to the potential of lithium metal in an environment of 25°C, a H1-3 type crystal structure appears in conventional positive electrode active materials. Therefore, a charging voltage of 4.6 V or higher relative to the potential of lithium metal can be considered a high charging voltage.
[0146] Therefore, in other words, the cathode active material 100 of one embodiment of the present invention is preferable because it can maintain the R-3m(O3) type crystal structure even when charged at a high charging voltage, for example, a voltage of 4.6 V or more at 25° C. In other words, it is preferable because it can adopt a monoclinic O1(15) type crystal structure when charged at an even higher charging voltage, for example, a voltage of more than 4.7 V but not more than 4.8 V at 25° C.
[0147] Even in the cathode active material 100 of one embodiment of the present invention, when the charging voltage is further increased, the H1-3 type crystal structure may finally be observed in some cases. That is, depending on the charge / discharge conditions, the cathode active material 100 may transition from the O3' type crystal structure to the H1-3 type crystal structure, but even if the cathode active material 100 transitions from the O3' type crystal structure to the H1-3 type crystal structure, it is estimated that the effect of suppressing oxygen release is still achieved.
[0148] Furthermore, as described above, since the crystal structure is affected by the number of charge / discharge cycles, charge / discharge current, temperature, electrolyte, etc., when the charge voltage is lower, for example, even when the charge voltage is 4.5 V or more and less than 4.6 V at 25° C., the positive electrode active material 100 may have an O3′-type crystal structure. Similarly, when charged at a voltage of 4.65 V or more and 4.7 V or less at 25° C., the positive electrode active material 100 may have a monoclinic O1(15)-type crystal structure.
[0149] In a secondary battery, for example, when graphite is used as the negative electrode active material, the voltage of the secondary battery is lower than the above by the potential of the graphite. The potential of graphite is about 0.05 V to 0.2 V with respect to the potential of lithium metal. Therefore, in the case of a secondary battery using graphite as the negative electrode active material, the battery has a similar crystal structure at a voltage obtained by subtracting the potential of graphite from the above voltage.
[0150] <Analysis method> In a certain positive electrode active material, Li x CoO 2 When x in the formula is small, whether the crystal structure is O3'-type and / or monoclinic O1(15)-type depends on Li x CoO 2 This can be determined by analyzing the positive electrode active material, positive electrode active material layer, or positive electrode in a charged state where x is small using XRD, electron beam diffraction, neutron diffraction, or the like.
[0151] XRD is particularly preferred in that it can analyze the symmetry of transition metals such as cobalt contained in lithium cobalt oxide with high resolution, it can compare the level of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, and it can obtain sufficient accuracy even when measuring the positive electrode obtained by disassembling the secondary battery as it is.
[0152] Among XRD methods, analysis using powder XRD provides diffraction peaks that reflect the crystalline structure of the interior 100b, which occupies the majority of the volume of the positive electrode active material 100. Powder XRD refers to a case where the measurement sample is a powder. The powder can be set by methods such as placing it in a glass sample holder or sprinkling it on a greased silicone anti-reflective plate. When the measurement sample is a positive electrode, the positive electrode can be attached to a measurement substrate with double-sided tape, and the positive electrode active material layer can be set to match the measurement surface required by the device.
[0153] Furthermore, even in the case of a cathode active material 100 that can be used as one embodiment of the present invention, if x is too small, such as 0.1 or less, or under conditions where the charge voltage exceeds 4.9 V, an H1-3 type or trigonal O1 type crystal structure may be formed. Therefore, in order to determine whether or not the cathode active material 100 can be used as one embodiment of the present invention, information such as the charge capacity or the charge voltage is required.
[0154] Furthermore, when the positive electrode active material 100 has a small x, its crystal structure may change when exposed to the air. For example, when exposed to the air, the crystal structure may change from the O3′-type and monoclinic O1(15)-type to the H1-3-type. Therefore, it is preferable to handle all samples for XRD measurement in an inert atmosphere such as an argon atmosphere.
[0155] <Evaluation Conditions> Evaluation conditions for determining whether a certain composite oxide is a cathode active material 100 that can be used as one embodiment of the present invention include a method of preparing a coin cell (e.g., CR2032 type, diameter 20 mm, height 3.2 mm) having lithium metal as a counter electrode and charging it under predetermined conditions. As mentioned above, information such as charge capacity or charge voltage is required to determine whether the composite oxide is a cathode active material 100 that can be used as one embodiment of the present invention.
[0156] The procedure 1 described below is an example for confirming the characteristics of the positive electrode active material 100 that can be used as one embodiment of the present invention. Therefore, there is no problem if an electrolyte different from that of the secondary battery that is one embodiment of the present invention is used.
[0157] Evaluation Procedure 1: A secondary battery is disassembled, the electrolyte-impregnated positive electrode is removed, and the electrolyte is removed by washing with an organic solvent or the like. The positive electrode is then punched out to fit a coin cell prepared for evaluation. The punched positive electrode contains a conductive material and a binder in addition to the positive electrode active material.
[0158] The coin cells prepared for evaluation had lithium metal as the counter electrode.
[0159] The coin cell was prepared using an electrolyte containing 1 mol / L lithium hexafluorophosphate (LiPF) in an organic solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7 and 2 wt% vinylene carbonate (VC). 6 ) dissolved in the solvent. A solvent containing two or more organic solvents is sometimes called a mixed solvent.
[0160] The coin cell has a 25 μm thick porous polypropylene film as a separator.
[0161] The coin cell has a positive electrode can made of stainless steel (SUS), and a negative electrode can made of stainless steel (SUS).
[0162] In this way, a coin cell A for evaluation is prepared.
[0163] The coin cell A for evaluation prepared under the above conditions is subjected to constant current charging (also called CC charging) to an arbitrary voltage (4.6 V, 4.65 V, 4.7 V, 4.75 V, or 4.8 V). To observe the phase change of the positive electrode active material, it is desirable to charge at a small current value. Typically, CC charging at a current value of 10 mA / g (equivalent to 0.05 C when 1 C is 200 mA / g of positive electrode active material weight) is preferred, but the current value is not limited in this evaluation.
[0164] The temperature during charging of the evaluation coin cell A can be 25° C. The temperature during charging may be the temperature of the thermostatic bath in which the coin cell A is placed.
[0165] After charging under these conditions, coin cell A is disassembled in a glove box under an argon atmosphere and the positive electrode is removed, thereby obtaining a positive electrode active material with a desired charging voltage or charging capacity. When various analyses are performed thereafter, it is preferable to seal the cell in an argon atmosphere to suppress reactions with external components. For example, XRD can be performed by sealing the cell in a sealed container under an argon atmosphere. Furthermore, it is preferable to remove and analyze the positive electrode promptly after charging is completed. Specifically, it is preferable to do so within one hour, and more preferably within 30 minutes, after charging is completed.
[0166] <<XRD>> An XRD measurement is performed on the positive electrode in the above-mentioned charged state. The measurement device and conditions are not particularly limited. For example, the measurement can be performed using the following device and conditions. XRD device: D8 ADVANCE manufactured by Bruker AXS X-ray source: CuKα 1 Source output: 40 kV, 40 mA Divergence angle: Div. Slit, 0.5° Detector: LynxEye Scan method: 2θ / θ continuous scan Measurement range (2θ): 15° to 90° Step width (2θ): 0.01° setting Counting time: 1 second / step Sample stage rotation: 15 rpm The obtained XRD pattern was analyzed using analysis software such as DIFFRAC.EVA to separate the background and CuKα 2 The peaks of the lines can be removed.
[0167] CuKα calculated from the O3' type crystal structure, the monoclinic O1(15) type crystal structure, and the H1-3 type crystal structure model 1 The ideal powder XRD patterns of the lines are shown in Figures 5, 6, 7A and 7B. x CoO 2 LiCoO where x=1 2 (O3) and the trigonal O1 crystal structure with x = 0 (CoO 2 7A and 7B show the XRD patterns of the O3' type crystal structure, the monoclinic O1(15) type crystal structure, and the H1-3 type crystal structure, with Fig. 7A showing an enlarged view of the region where 2θ is in the range of 18° to 21°, and Fig. 7B showing an enlarged view of the region where 2θ is in the range of 42° to 46°.2 (O3) and CoO 2 The pattern of (O1) was created using Reflex Powder Diffraction, one of the modules of Materials Studio (BIOVIA), from crystal structure information obtained from ICSD (Inorganic Crystal Structure Database). The 2θ range was 15° to 75°, step size = 0.01, and wavelength λ = 1.540562 × 10 −10 m and λ2 were not set, and the monochromator was single.
[0168] As shown in Figures 5, 7A and 7B, in the O3' type crystal structure, diffraction peaks appear at 2θ = 19.25 ± 0.12° (19.13° or more and less than 19.37°) and 2θ = 45.47 ± 0.10° (45.37° or more and less than 45.57°).
[0169] In addition, in the monoclinic O1(15) type crystal structure, diffraction peaks appear at 2θ=19.47±0.10° (19.37° or more and 19.57° or less) and 2θ=45.62±0.05° (45.57° or more and 45.67° or less).
[0170] However, as shown in Figures 6, 7A and 7B, no peaks appear at these positions in the H1-3 type crystal structure and trigonal O1. x CoO 2 It can be said that the appearance of diffraction peaks at angles of 19.13° or more and less than 19.37° and / or 19.37° or more and less than 19.57°, and 45.37° or more and less than 45.57° and / or 45.57° or more and less than 45.67° when x is small is a characteristic of the positive electrode active material 100.
[0171] FIG. 8 shows lithium cobalt oxide that can be used as the positive electrode active material 100. x CoO 21 is a graph showing the change in c-axis length (Å) with respect to x in the graph. The O3'-type crystal structure is a crystal structure when x is approximately 0.2. It can be said that the O3'-type crystal structure has a c-axis length of 13.6 Å or more and 13.9 Å or less when x is 0.2. When charging at a high voltage such as x 0.2, the c-axis does not collapse and the lithium ion insertion / extraction pathway is maintained, thereby exhibiting good cycle characteristics. In order to satisfy the above-described c-axis length, it is important to have an additive element, and it is further preferable that the additive element be appropriately distributed in the surface layer. The additive element is preferably one of those described above, with magnesium being particularly suitable. Furthermore, the c-axis length can be maintained by appropriately distributing the additive element even in the interior. The additive element is preferably one of those described above, with elements other than magnesium being particularly suitable, with nickel and / or aluminum being particularly suitable.
[0172] XPS: X-ray photoelectron spectroscopy (XPS) is a type of surface analysis that can analyze a region from the surface to a depth of approximately 2 to 8 nm (usually 5 nm or less), providing information on the quantitative determination and bonding state of elements present in the measurement region. A depth of 5 nm corresponds to approximately half the depth of the surface layer 100a. The measurable region of XPS is 20 μmφ to 100 μmφ. Therefore, analysis of the positive electrode in addition to the positive electrode active material is possible, and the concentration of each element in the positive electrode can be quantitatively analyzed. Furthermore, narrow scan analysis is preferable to obtain information on the bonding state.
[0173] During surface analysis of the positive electrode active material 100, it is preferable to exclude the electrolyte, binder, conductive material, or compounds derived therefrom that adhere to the surface of the positive electrode active material 100. Therefore, when quantifying the elements contained in the positive electrode active material 100, corrections may be made to exclude carbon, hydrogen, excess oxygen, excess fluorine, and the like detected by XPS. For example, C—F bonds derived from the binder may be identified by narrow scan analysis, and corrections may be made to exclude these C—F bonds. Alternatively, during sample processing for XPS, cleaning or other procedures may be performed to remove the electrolyte, binder, conductive material, or compounds derived therefrom that adhere to the surface of the positive electrode active material. While lithium may dissolve in the organic solvent used for cleaning, even in this case, the added elements are unlikely to dissolve, and therefore the atomic ratio of the added elements is not affected. During surface analysis of the positive electrode, no bonds need to be removed, but it is recommended to remove the electrolyte during sample processing.
[0174] For example, as a result of the XPS analysis, the positive electrode active material 100 preferably has a ratio of magnesium atoms to cobalt atoms of 0.4 to 1.2, preferably 0.65 to 1.0. The ratio of nickel atoms to cobalt atoms is 0.15 to 0.15, preferably 0.03 to 0.13. The ratio of aluminum atoms to cobalt atoms is 0.12 to 0.09, preferably 0.09. The ratio of fluorine atoms to cobalt atoms is 0.3 to 0.9, preferably 0.1 to 1.1. The above ranges indicate that these additive elements are not attached to a narrow area on the surface of the positive electrode active material 100, but are widely distributed at preferred concentrations in the surface layer 100a of the positive electrode active material 100.
[0175] Furthermore, it is more preferable that aluminum and / or nickel, etc., among the added elements, are widely distributed in a deep region of the positive electrode active material 100, for example, in a region having a depth of 5 nm to 50 nm from the surface. Therefore, it is more preferable that aluminum and / or nickel are detected in an analysis of the entire positive electrode active material 100 using ICP-MS, GD-MS, etc., but that aluminum and / or nickel are not detected by XPS, etc.
[0176] <EDX> Preferably, one or more selected from the additive elements contained in the positive electrode active material 100 have a concentration gradient. Furthermore, it is more preferable that the depth of the concentration peak from the surface of the positive electrode active material 100 differs depending on the additive element. The concentration gradient of the additive element can be evaluated, for example, by analysis using energy dispersive X-ray spectroscopy (EDX). Among EDX measurements, EDX area analysis is performed by scanning an area and evaluating the area two-dimensionally. Linear analysis is performed by linear scanning and evaluating the distribution of atomic concentration within the positive electrode active material. Furthermore, linear analysis may be used to extract data for a linear area from the results of EDX area analysis. Point analysis is also used to measure a certain area without scanning. More preferably, the concentration gradient of the added element is determined by exposing a cross section of the positive electrode active material 100 using a focused ion beam (FIB) or the like, performing EDX area analysis on the cross section, and extracting the EDX analysis results from the results. The cross section of the positive electrode active material 100 is preferably observed using an STEM image, which is called STEM-EDX analysis.
[0177] The surface of the positive electrode active material 100 in a cross-sectional STEM image or the like is the boundary between the region where an image derived from the crystalline structure of the positive electrode active material is observed and the region where it is not observed, and is the outermost region where atomic columns derived from the atomic nuclei of metal elements having atomic numbers larger than that of lithium among the metal elements constituting the positive electrode active material are observed. Alternatively, it is the intersection of the tangent line drawn to the brightness profile from the surface toward the bulk of the STEM image and the axis in the depth direction. The surface in a STEM image or the like may be determined in conjunction with an analysis with higher spatial resolution.
[0178] The reference point of a positive electrode active material in STEM-EDX-ray analysis, etc., is the point where oxygen or cobalt is 50% of the average internal detection amount MAVE. Note that if the 50% points of the average internal detection amount MAVE differ between cobalt and oxygen, this is likely due to the influence of metal oxides, carbonates, etc. containing oxygen attached to the surface, and therefore the 50% point of the average internal detection amount MAVE of cobalt can be used as the reference point. The reference point of a positive electrode active material in STEM-EDX-ray analysis, etc., is sometimes called the surface.
[0179] The minimum spatial resolution of STEM-EDX is about 1 nm. Therefore, the maximum value of the additive element profile may deviate by about 1 nm. For example, even if the maximum value of the additive element profile of magnesium or the like is outside the surface obtained above, if the difference between the maximum value and the surface is less than 1 nm, this can be considered an error.
[0180] The peak in STEM-EDX-ray analysis refers to the detected intensity in each element profile or the maximum value of the characteristic X-ray for each element. Note that noise in STEM-EDX-ray analysis may be a measured value with a half-width less than the spatial resolution (R), for example, R / 2 or less.
[0181] STEM-EDX analysis can be performed, for example, as follows: First, a protective film is vapor-deposited on the surface of the region of the positive electrode active material to be analyzed. For example, a carbon film vapor-deposited using a carbon coating unit of an ion sputtering apparatus (MC1000 manufactured by Hitachi High-Technologies) can be used as the protective film.
[0182] Next, the positive electrode active material is sliced to prepare a STEM cross-section sample. For example, the slice processing can be performed using an FIB-SEM device (Hitachi High-Tech XVision 200TBS). Pickup is performed using an MPS (microprobing system), and the finishing conditions can be, for example, an acceleration voltage of 10 kV.
[0183] The STEM-EDX analysis can be performed using, for example, a STEM device (NEOARM manufactured by JEOL), and the EDX detector can be a Dual SDD detector manufactured by JEOL.
[0184] For example, when EDX area analysis or EDX point analysis is performed on a cathode active material 100 containing magnesium as an additive element, it is preferable that the magnesium concentration in the surface layer 100a be higher than that in the interior 100b. Furthermore, when STEM-EDX ray analysis is performed, the peak of the magnesium concentration in the surface layer 100a is preferably present at a depth of 3 nm from the surface toward the center of the cathode active material 100, more preferably at a depth of 1 nm, and even more preferably at a depth of 0.5 nm. Note that the concentration peak here refers to the maximum value of the concentration.
[0185] In addition, in the positive electrode active material 100 containing magnesium and fluorine as additive elements, the distribution of fluorine preferably overlaps with the distribution of magnesium. For example, the difference in the depth direction between the peak of the fluorine concentration and the peak of the magnesium concentration is preferably within 10 nm, more preferably within 3 nm, and even more preferably within 1 nm.
[0186] Furthermore, when STEM-EDX ray analysis is performed, the fluorine concentration peak of the surface layer portion 100a preferably exists within a depth of 3 nm from the surface toward the center of the positive electrode active material 100, more preferably exists within a depth of 1 nm, and even more preferably exists within a depth of 0.5 nm. Furthermore, it is more preferable for the fluorine concentration peak to exist slightly closer to the surface than the magnesium concentration peak, as this increases resistance to hydrofluoric acid. For example, it is more preferable for the fluorine concentration peak to be 0.5 nm or more closer to the surface than the magnesium concentration peak, and even more preferable for it to be 1.5 nm or more closer to the surface.
[0187] In the cathode active material 100 containing nickel as an additive element, the nickel concentration peak in the surface layer 100a preferably exists within a depth of 3 nm from the surface toward the center of the cathode active material 100, more preferably within a depth of 1 nm, and even more preferably within a depth of 0.5 nm. In the cathode active material 100 containing magnesium and nickel, the nickel distribution preferably overlaps with the magnesium distribution. For example, the difference in depth between the nickel concentration peak and the magnesium concentration peak is preferably within 10 nm, more preferably within 3 nm, and even more preferably within 1 nm.
[0188] Furthermore, when the positive electrode active material 100 contains aluminum as an additive element, it is preferable that the magnesium, nickel, or fluorine concentration peak be closer to the surface than the aluminum concentration peak in the surface layer portion 100 a when subjected to STEM-EDX ray analysis. For example, the aluminum concentration peak is preferably present at a depth of 0.5 nm to 50 nm, more preferably 5 nm to 50 nm, from the surface toward the center of the positive electrode active material 100.
[0189] <AC Impedance Measurement> AC impedance measurement can be performed to characterize the positive electrode active material. For AC impedance measurement, a coin cell (e.g., CR2032 type, 20 mm diameter, 3.2 mm height) with lithium metal as the counter electrode is prepared, charged under specified conditions, and then the coin cell is disassembled and the removed positive electrode is used. For example, AC impedance measurement can be performed after the third charging cycle. A symmetric cell is used for AC impedance measurement. Therefore, two positive electrodes removed from the coin cell are prepared. A separator can be placed between the two positive electrodes to assemble a symmetric cell. When assembling a symmetric cell, the amount of electrolyte may be insufficient, so new electrolyte can be added. Note that the electrolyte added should be the same as that of the coin cell.
[0190] For measuring AC impedance, fitting can be performed using a known Nyquist diagram and an equivalent circuit diagram used for fitting. In the Nyquist diagram, the resistance of the electrolyte is Rs, and the resistance related to the electron conduction in the electrode or the absorption and desorption of lithium ions on the electrode surface is R HF , the resistance related to the solvation and desolvation of lithium ions, the charge transfer resistance to the insertion and desorption of lithium ions, and the surface film resistance is R LF The surface film mentioned above refers to a film that is deposited on the positive electrode active material as a result of the decomposition of the electrolyte.
[0191] In a positive electrode having a positive electrode active material 100 and an electrolyte containing fluorine, the resistance corresponding to Rs is preferably 1 Ω or more and 3 Ω or less at room temperature, and R LF The resistance corresponding to R is preferably 50Ω or more and 100Ω or less. HF It is preferable that the resistance corresponding to the above satisfies 2Ω or more and 5Ω or less.
[0192] 9A to 9C, a method 1 for producing the positive electrode active material 100 will be described. A smooth positive electrode active material 100 can be provided by undergoing initial heating.
[0193] <Step S11> In step S11 shown in FIG. 9A, a lithium source (Li source) and a cobalt source (Co source) are prepared as starting materials for lithium and transition metal, respectively.
[0194] As the lithium source, it is preferable to use a compound containing lithium, such as lithium carbonate, lithium hydroxide, lithium nitrate, or lithium fluoride. It is preferable that the lithium source has high purity, and it is preferable to use a material with a purity of, for example, 99.99% or higher.
[0195] As the cobalt source, it is preferable to use a compound containing cobalt, for example, cobalt oxide such as tricobalt tetroxide, cobalt hydroxide, or the like.
[0196] <Step S12> Next, in step S12 shown in FIG. 9A, the lithium source and the cobalt source are pulverized and mixed to prepare a mixed material. The pulverization and mixing can be performed by a dry method or a wet method. The wet method is preferable because it allows for smaller pulverization. When performing the wet method, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium.
[0197] A ball mill, a bead mill, or the like can be used as a means for pulverizing and mixing. When using a ball mill, it is preferable to use aluminum oxide balls or zirconium oxide balls as media. Zirconium oxide balls are preferred because they emit less impurities. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media.
[0198] 9A, the mixed material is heated at a temperature of preferably 800° C. to 1100° C., more preferably 900° C. to 1000° C., and even more preferably about 950° C.
[0199] After heating, the material may be crushed and sieved as necessary. The material after heating may be recovered by transferring it from the crucible to a mortar and then recovering it. The mortar is preferably an aluminum oxide mortar or a zirconium oxide mortar.
[0200] <Step S14> By the above steps, lithium cobalt oxide (LiCoO 2 In order to obtain a positive electrode active material 100 having a small median diameter (D50), it is preferable to pulverize lithium cobalt oxide.
[0201] Although an example of producing lithium cobalt oxide by a solid phase method as in steps S11 to S14 has been shown, lithium cobalt oxide may also be produced by a coprecipitation method or a hydrothermal method.
[0202] 9A, the lithium cobalt oxide is heated. Because this is the first heating of the lithium cobalt oxide, the heating in step S15 is sometimes called initial heating. Alternatively, because this heating is performed before the next step S20, it is sometimes called preheating or pretreatment.
[0203] The crucible used for heating in step S15 is preferably an aluminum oxide crucible. An aluminum oxide crucible is a material that does not easily release impurities. In this embodiment, an aluminum oxide crucible with a purity of 99.9% is used. It is preferable to place a lid on the crucible when heating, as this can prevent volatilization or sublimation of the material. Placing a lid on the crucible means that it is sufficient to prevent volatilization or sublimation of the material from the time the temperature is increased to the time the temperature is decreased in this step, and it is not necessary to seal the crucible with a lid. For example, as described above, by filling the reaction chamber with oxygen, this step can be performed without sealing the crucible.
[0204] Furthermore, it is preferable to use a used crucible rather than a new one. In this specification, a new crucible refers to one that has undergone the process of heating with lithium cobalt oxide added thereto two or fewer times. A used crucible refers to one that has undergone the process of heating with lithium cobalt oxide and / or a material containing an additive element added thereto three or more times. This is because when a new crucible is used, there is a risk that some of the materials, including lithium fluoride, may be absorbed, diffused, migrated, and / or adhered to the sheath during heating. If some of the materials are lost as a result of this, there is a growing concern that the distribution of elements, particularly in the surface layer of the positive electrode active material, may not fall within a desirable range. On the other hand, this risk is less likely with a used crucible.
[0205] The following effects are expected from the initial heating, but the initial heating is not essential for obtaining the positive electrode active material of one embodiment of the present invention.
[0206] The initial heating causes lithium to be desorbed from a portion of the surface layer 100a of the lithium cobalt oxide. This is also expected to have the effect of improving the crystallinity of the interior 100b. Impurities may be present in the lithium source and / or cobalt source prepared in step S11, etc. The initial heating can reduce the amount of impurities in the lithium cobalt oxide completed in step S14.
[0207] Furthermore, initial heating has the effect of smoothing the surface of the lithium cobalt oxide. A smooth surface of a composite oxide means that there are few irregularities, the composite oxide is rounded overall, and the corners are rounded. Furthermore, a smooth surface means that there is little foreign matter adhering to the surface. Foreign matter is thought to be a cause of irregularities, so it is preferable that it does not adhere to the surface.
[0208] For this initial heating, it is not necessary to prepare a lithium source, a source of an additional element, or a material that functions as a flux.
[0209] If the heating time in this step is too short, sufficient effects will not be obtained, but if it is too long, productivity will decrease. For example, the heating conditions can be selected from those described in step S13. In addition to the heating conditions, the heating temperature in this step is preferably lower than the temperature in step S13 in order to maintain the crystalline structure of the complex oxide. Furthermore, the heating time in this step is preferably shorter than the time in step S13 in order to maintain the crystalline structure of the complex oxide. For example, heating at a temperature of 700°C or higher and 1000°C or lower for 2 hours or longer and 20 hours or shorter is recommended.
[0210] The effect of increasing the crystallinity of the inner portion 100b is, for example, the effect of alleviating distortion, displacement, etc. resulting from the difference in shrinkage of the lithium cobalt oxide produced in step S13.
[0211] The heating in step S13 may cause a temperature difference between the surface and the interior of the lithium cobalt oxide. This temperature difference may induce a shrinkage difference. It is also believed that the temperature difference causes a difference in fluidity between the surface and the interior, resulting in a shrinkage difference. The energy associated with the shrinkage difference causes an internal stress difference in the lithium cobalt oxide. This internal stress difference is also called strain, and this energy is sometimes called strain energy. It is believed that the internal stress is removed by the initial heating in step S15; in other words, the strain energy is homogenized by the initial heating in step S15. When the strain energy is homogenized, the strain in the lithium cobalt oxide is alleviated. This may result in a smoother surface for the lithium cobalt oxide. This is also referred to as an improved surface. In other words, it is believed that the shrinkage difference in the lithium cobalt oxide is alleviated and the surface of the composite oxide is smoother after step S15.
[0212] Furthermore, the difference in shrinkage may cause microscopic deviations, such as crystal deviations, in the lithium cobalt oxide. It is preferable to carry out this step in order to reduce such deviations. This step makes it possible to equalize the deviations in the composite oxide. Equalizing the deviations may result in a smoother surface of the composite oxide. This is also referred to as the alignment of crystal grains. In other words, it is believed that step S15 reduces the deviations of crystals and other particles in the composite oxide, resulting in a smoother surface of the composite oxide.
[0213] When lithium cobalt oxide with a smooth surface is used as the positive electrode active material, deterioration during charge and discharge in a secondary battery is reduced and cracking of the positive electrode active material can be prevented.
[0214] Note that pre-synthesized lithium cobalt oxide may be used in step S14. In this case, steps S11 to S13 can be omitted. By performing step S15 on pre-synthesized lithium cobalt oxide, lithium cobalt oxide with a smooth surface can be obtained.
[0215] <Step S20> Next, as shown in step S20, it is preferable to add the additional element A to the lithium cobalt oxide that has undergone the initial heating. When the additional element A is added to the lithium cobalt oxide that has undergone the initial heating, the additional element A can be added evenly. Therefore, it is preferable to add the additional element A after the initial heating. The step of adding the additional element A will be described with reference to FIGS. 9B and 9C.
[0216] 9B, a source of an additional element A (A source) to be added to lithium cobalt oxide is prepared. A lithium source may be prepared together with the additional element A source.
[0217] As the additional element A, it is possible to use the additional elements described in the previous embodiment, specifically, one or more selected from magnesium, fluorine, nickel, aluminum, titanium and phosphorus.
[0218] When magnesium is selected as the additive element, the source of the additive element can be called a magnesium source. As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. can be used. Furthermore, a plurality of the above-mentioned magnesium sources may be used.
[0219] When fluorine is selected as the additive element, the source of the additive element can be called a fluorine source. Examples of the fluorine source include lithium fluoride (LiF) and magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF 4 ), cobalt fluoride (CoF 2 , CoF 3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 3 , CeF4 ), lanthanum fluoride (LaF 3 ), or sodium aluminum hexafluoride (Na 3 AlF 6 Among these, lithium fluoride is preferred because it has a relatively low melting point of 848° C. and is easily melted in the heating step described below.
[0220] Magnesium fluoride can be used as both a fluorine source and a magnesium source, and lithium fluoride can be used as both a fluorine source and a lithium source. Another lithium source that can be used in step S21 is lithium carbonate.
[0221] The fluorine source is preferably a gas, and fluorine (F 2 ), fluorocarbon, sulfur fluoride, or oxygen fluoride (OF 2 , O 2 F 2 , O 3 F 2 , O 4 F 2 , O 5 F 2 , O 6 F 2 , O 2 F) or the like may be used and mixed into the atmosphere in the heating step described below. Also, a plurality of the above-mentioned fluorine sources may be used.
[0222] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and the magnesium source. 2 Lithium fluoride and magnesium fluoride are prepared as LiF:MgF 2 The effect of lowering the melting point is greatest when the molar ratio of lithium fluoride and magnesium fluoride is about 65:35. On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be excessive and the cycle characteristics will deteriorate. Therefore, the molar ratio of lithium fluoride and magnesium fluoride is set to LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2= x: 1 (x = 0.33 or its vicinity) is more preferable. Here, "or its vicinity" refers to a value that is greater than 0.9 times and less than 1.1 times the value.
[0223] 9B, the magnesium source and the fluorine source are pulverized and mixed. This step can be performed under pulverization and mixing conditions selected from those described in step S12.
[0224] 9B, the pulverized and mixed materials are collected to obtain a source of the additional element A (A source). Note that the source of the additional element A shown in step S23 contains a plurality of starting materials and can be called a mixture.
[0225] The particle size of the mixture is preferably such that the median diameter (D50) is 600 nm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less. Even when a single material is used as the additive element source, the median diameter (D50) is preferably 600 nm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less.
[0226] Such a finely powdered mixture (including the case where only one type of additive element is included) can be easily adhered uniformly to the surface of the lithium cobalt oxide when mixed with the lithium cobalt oxide in a later step. If the mixture is evenly adhered to the surface of the lithium cobalt oxide particles, it is preferable because the additive element can be easily distributed or diffused uniformly in the surface layer portion 100a of the composite oxide after heating.
[0227] <Step S21a> A step different from that shown in Fig. 9B will be described with reference to Fig. 9C. In step S21a shown in Fig. 9C, four types of additive element sources to be added to lithium cobalt oxide are prepared. That is, Fig. 9C differs from Fig. 9B in the types of additive element sources. A lithium source may be prepared together with the additive element sources.
[0228] As sources of four additive elements, a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source) are prepared. The magnesium source and the fluorine source can be selected from the compounds described with reference to FIG. 9B . Nickel oxide, nickel hydroxide, etc. can be used as the nickel source. Aluminum oxide, aluminum hydroxide, etc. can be used as the aluminum source.
[0229] <Steps S22 and S23> Steps S22 and S23 shown in FIG. 9C are similar to the steps described with reference to FIG. 9B.
[0230] 9A , lithium cobalt oxide is mixed with a source of additional element A. The ratio of the number of cobalt atoms Co in the lithium cobalt oxide to the number of magnesium atoms Mg in the source of additional element A is preferably Co:Mg=100:y (0.1≦y≦6), and more preferably Co:Mg=100:y (0.3≦y≦3).
[0231] The mixing conditions in step S31 are preferably milder than those in step S12 so as not to destroy the shape of the lithium cobalt oxide particles. For example, the mixing conditions are preferably lower in rotation speed or shorter in time than those in step S12. It can also be said that dry mixing provides milder conditions than wet mixing. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconium oxide balls as the media.
[0232] In this embodiment, dry mixing is performed in a ball mill using zirconium oxide balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of −100° C. or higher and −10° C. or lower.
[0233] <Step S32> Next, in step S32 of Fig. 9A, the mixed materials are collected to obtain a mixture 903. When collecting the materials, they may be crushed and then sieved, if necessary.
[0234] 9A to 9C illustrate a fabrication method in which an additive element is added after initial heating, but the present invention is not limited to the above method. The additive element may be added at a different timing, or may be added multiple times. The timing may be changed depending on the additive element.
[0235] For example, as shown in Figures 10A to 10C, the additive elements may be added to the lithium source and the cobalt source in step S11, i.e., at the stage of the starting material for the composite oxide. Figure 10A shows a flow of adding a magnesium source to a lithium source and a cobalt source. Figure 10B shows a flow of adding a magnesium source and an aluminum source to a lithium source and a cobalt source. Figure 10C shows a flow of adding a magnesium source and a nickel source to a lithium source and a cobalt source. The additive element sources shown in Figures 10A to 10C are examples.
[0236] Subsequently, the process proceeds to step S12, then step S13, and finally step S14, where lithium cobalt oxide containing the additive element can be obtained. The distribution of the additive element can also be controlled depending on the timing of the addition of the additive element. The additive element added as shown in FIGS. 10A to 10C is expected to be located inside the positive electrode active material 100. Furthermore, in the case of the flow shown in FIGS. 10A to 10C, the above-described steps S11 to S14 and steps S21 to S23 do not need to be separated, making this a simple and highly productive method. Of course, even in the flow shown in FIGS. 10A to 10C, a new additive element may be added in step S20.
[0237] Alternatively, lithium cobalt oxide containing some of the additive elements may be used. For example, if lithium cobalt oxide containing magnesium and fluorine is used, steps S11 to S14 and some of step S20 can be omitted. This method is simple and has high productivity.
[0238] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be heated in step S15, and then a magnesium source and a fluorine source, or a magnesium source, a fluorine source, a nickel source, and an aluminum source may be added as in step S20.
[0239] <Step S33> Next, in step S33 shown in Fig. 9A, the mixture 903 is heated. The heating can be performed under heating conditions selected from those described in step S15. The heating time is preferably 2 hours or more. At this time, the pressure inside the furnace may exceed atmospheric pressure in order to increase the oxygen partial pressure in the heating atmosphere. This is because if the oxygen partial pressure in the heating atmosphere is insufficient, cobalt and the like may be reduced, and lithium cobalt oxide and the like may no longer be able to maintain a layered rock salt type crystal structure.
[0240] Here, a supplementary note about the heating temperature will be provided. The lower limit of the heating temperature in step S33 must be equal to or higher than the temperature at which the reaction between the lithium cobalt oxide and the additive element source proceeds. The temperature at which the reaction proceeds is preferably a temperature at which interdiffusion between the lithium cobalt oxide and the elements contained in the additive element source occurs, and may be lower than the melting temperature of these materials. An oxide will be used as an example for explanation, but the melting temperature T m 0.757 times (Tammann temperature T d ) solid-phase diffusion occurs. Therefore, the heating temperature in step S33 is preferably 650° C. or higher.
[0241] Of course, the reaction is more likely to proceed if the temperature is equal to or higher than the melting point of one or more of the materials contained in the mixture 903. For example, LiF and MgF are used as the additive element source. 2 When LiF and MgF 2 Since the eutectic point of is around 742°C, the lower limit of the heating temperature in step S33 is preferably set to 742°C or higher.
[0242] Also, LiCoO 2 :LiF:MgF 2 In the mixture 903 obtained by mixing so that the molar ratio was 100:0.33:1, an endothermic peak was observed around 830° C. in DSC measurement. Therefore, the lower limit of the heating temperature is more preferably 830° C. or higher.
[0243] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.
[0244] The upper limit of the heating temperature is set to be lower than the decomposition temperature of lithium cobalt oxide (melting point 1130°C). At temperatures close to the decomposition temperature, there is a concern that lithium cobalt oxide may decompose, albeit only slightly. Therefore, the upper limit of the heating temperature is more preferably 1000°C or lower, even more preferably 950°C or lower, and even more preferably 900°C or lower.
[0245] In consideration of these, the heating temperature in step S33 is preferably 650°C or higher and 1130°C or lower, more preferably 650°C or higher and 1000°C or lower, even more preferably 650°C or higher and 950°C or lower, and even more preferably 650°C or higher and 900°C or lower. Also, it is preferably 742°C or higher and 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, even more preferably 742°C or higher and 950°C or lower, and even more preferably 742°C or higher and 900°C or lower. Also, it is preferably 830°C or higher and 1130°C or lower, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, and even more preferably 830°C or higher and 900°C or lower. The heating temperature in step S33 is preferably lower than the heating temperature in step S13.
[0246] The cooling after heating in step S33 can be performed by natural cooling, but it is preferable that the time required for the temperature to drop from the specified temperature to room temperature is between 10 and 50 hours. For example, the temperature drop rate (hereinafter also referred to as the cooling rate) is preferably between 80°C / h and 250°C / h, and more preferably between 180°C / h and 210°C / h. The cooling rate in step S33 is preferably faster than that in step S13. A fast cooling rate is called rapid cooling. Rapid cooling after the melting allows for the appropriate production of a shell. Specifically, it is possible to produce a narrow shell. The temperature at the end of the temperature drop does not necessarily have to be room temperature; it is sufficient to cool to a temperature acceptable for the next step.
[0247] Furthermore, when heating the mixture 903, it is preferable to control the partial pressure of fluorine or a fluorine compound resulting from the fluorine source or the like within an appropriate range. The partial pressure can also be controlled by heating the crucible used in this step with a lid. As mentioned above, the lid can prevent the volatilization or sublimation of the material. Therefore, it is not necessary to seal the crucible with a lid, as long as the volatilization or sublimation of the material can be prevented from occurring during the temperature increase and decrease periods in this step. For example, by filling the reaction chamber in which the crucible is placed with oxygen, it is possible to perform this step without sealing the crucible. A positive electrode active material containing an appropriate amount of fluorine or a fluorine compound is preferable because it can suppress heat generation and smoke generation even in the event of an internal short circuit.
[0248] In the manufacturing method described in this embodiment, some materials, for example, LiF as a fluorine source, may function as a flux, which allows the heating temperature to be lowered below the decomposition temperature of lithium cobalt oxide, for example, to 742° C. or higher and 950° C. or lower, and allows additive elements such as magnesium to be distributed in the surface layer, thereby enabling the manufacture of a positive electrode active material with excellent characteristics.
[0249] However, since LiF has a lower specific gravity in a gaseous state than oxygen, there is a possibility that LiF may volatilize or sublime when heated, and if it volatilizes, the amount of LiF in the mixture 903 will decrease. This will weaken its function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., LiCoO 2 There is a possibility that Li on the surface reacts with F in the fluorine source to produce LiF, which may then volatilize. Therefore, even if a fluorine compound with a higher melting point than LiF is used, it is still necessary to suppress volatilization.
[0250] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF is high in the heating furnace. By heating in this manner, it is possible to suppress the volatilization of LiF in the mixture 903. In order to suppress the volatilization of LiF, it is preferable to place a lid on the crucible.
[0251] The heating in this step is preferably performed so as not to cause the particles of the mixture 903 to stick together. If the particles of the mixture 903 stick together during heating, the contact area with oxygen in the atmosphere will decrease and the route along which the added element (e.g., fluorine) diffuses will be blocked, which may result in poor distribution of the added element (e.g., magnesium and fluorine) in the surface layer. In order to promote the reaction with oxygen in the atmosphere, the crucible does not need to be sealed with a lid.
[0252] Furthermore, it is believed that uniform distribution of the additive element (e.g., fluorine) in the surface layer portion results in a smooth cathode active material with few irregularities. Therefore, in order to maintain the smooth state of the surface after the heating in step S15 or to make it even smoother, it is preferable that the particles of mixture 903 do not stick to each other.
[0253] Furthermore, when heating in a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln during heating. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and then not flow the atmosphere after introducing the oxygen atmosphere into the kiln. Flowing oxygen may cause the fluorine source to evaporate, which is undesirable in terms of maintaining surface smoothness.
[0254] When heating is performed using a roller hearth kiln, the mixture 903 can be heated in an atmosphere containing LiF by placing a lid on a container containing the mixture 903, for example, in the same way as a lid placed on a crucible.
[0255] Regarding the heating time, the heating time varies depending on conditions such as the heating temperature, the size and composition of the lithium cobalt oxide obtained in step S14, etc. When the lithium cobalt oxide is small, a lower temperature or a shorter heating time may be more preferable than when the lithium cobalt oxide is large.
[0256] 9A , when the median diameter (D50) of the lithium cobalt oxide obtained in step S14 is about 12 μm, the heating temperature is preferably, for example, 650° C. or more and 950° C. or less. The heating time is preferably, for example, 3 hours or more and 60 hours or less, more preferably 10 hours or more and 30 hours or less, and even more preferably about 20 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or more and 50 hours or less.
[0257] On the other hand, when the median diameter (D50) of the lithium cobalt oxide obtained in step S14 is about 5 μm, the heating temperature is preferably, for example, 650° C. or higher and 950° C. or lower. The heating time is preferably, for example, 1 hour or higher and 10 hours or lower, and more preferably about 5 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.
[0258] <Step S34> Next, in step S34 shown in Fig. 9A, the heated material is recovered to obtain the positive electrode active material 100. The recovered particles may be further sieved. Through the above steps, the positive electrode active material 100 according to one embodiment of the present invention can be produced. The positive electrode active material 100 has a smooth surface.
[0259] 11 to 12C , a method for producing a positive electrode active material, which is an embodiment of the present invention and differs from the method for producing a positive electrode active material, will be described. The method for producing a positive electrode active material, which differs from the method for producing a positive electrode active material, is mainly the number of times that an additive element is added and the mixing method. For other details, the description of the method for producing a positive electrode active material, which differs from the method for producing a positive electrode active material, can be referred to.
[0260] In FIG. 11, steps S11 to S15 are performed in the same manner as in FIG. 9A to prepare lithium cobalt oxide that has undergone initial heating.
[0261] <Step S20a> Next, as shown in step S20a, it is preferable to add an additional element A1 to the lithium cobalt oxide that has undergone the initial heating.
[0262] <Step S21> In step S21 shown in Fig. 12A, a first additive element source (A1 source) is prepared. The first additive element source can be selected from the additive elements described in step S21 shown in Fig. 12B and used. For example, one or more selected from magnesium and fluorine can be suitably used as the first additive element source. Fig. 12A illustrates an example in which a magnesium source (Mg source) and a fluorine source (F source) are used as the first additive element source.
[0263] Steps S21 to S23 shown in Fig. 12A can be performed under the same conditions as steps S21 to S23 shown in Fig. 9B, as a result of which the first additive element source can be obtained in step S23.
[0264] Furthermore, steps S31 to S33 shown in FIG. 11 can be performed in the same manner as steps S31 to S33 shown in FIG. 9A.
[0265] <Step S34a> Next, the material heated in step S33 is recovered to produce lithium cobalt oxide containing the first additive element source. To distinguish it from the composite oxide in step S14, this is also called a second composite oxide.
[0266] <Step S40> In step S40 shown in Fig. 11, a second additive element source (A2 source) is added. This will be described with reference to Figs. 12B and 12C.
[0267] <Step S41> In step S41 shown in Fig. 12B, a second additive element source is prepared. The second additive element source can be selected from the additive elements described in step S21 shown in Fig. 9C and used. For example, one or more selected from nickel, titanium, and aluminum can be suitably used as the second additive element source. Fig. 12B illustrates an example in which a nickel source (Ni source) and an aluminum source (Al source) are used as the second additive element source.
[0268] Steps S41 to S43 shown in Fig. 12B can be performed under the same conditions as steps S21 to S23 shown in Fig. 9B, as a result of which the second additive element source can be obtained in step S43.
[0269] 12C shows a modified example of the steps described with reference to FIG. 12B. In step S41 shown in FIG. 12C, a nickel source (Ni source) and an aluminum source (Al source) are prepared, and in step S42a, they are independently pulverized. As a result, in step S43, a plurality of second additive element sources are prepared. The steps of FIG. 12C differ from those of FIG. 12B in that the additive elements are independently pulverized in step S42a.
[0270] <Steps S51 to S54> Next, steps S51 to S54 shown in Fig. 11 can be performed under the same conditions as steps S31 to S34 shown in Fig. 9A. The conditions for step S53, which is a heating step, may be a lower temperature and a shorter time than those for step S33. Through the above steps, in step S54, a positive electrode active material 100 according to one embodiment of the present invention can be produced. The positive electrode active material 100 has a smooth surface.
[0271] 11 to 12C , in the fabrication method 2, the additive element to the lithium cobalt oxide is introduced separately from a first additive element source and a second additive element source. By introducing the additive elements separately, the position of each additive element in the depth direction can be changed. For example, it is possible to position the first additive element so that its concentration is higher in the surface layer portion than in the interior, and to position the second additive element so that its concentration is higher in the interior than in the surface layer portion.
[0272] The initial heating shown in this embodiment is performed on lithium cobalt oxide. Therefore, the initial heating is preferably performed at a temperature lower than that required for obtaining lithium cobalt oxide and for a shorter heating time than that required for obtaining lithium cobalt oxide. The step of adding an additive element to lithium cobalt oxide is preferably performed after the initial heating. This addition step can be performed in two or more steps. Following this order of steps is preferable because it maintains the surface smoothness obtained by the initial heating.
[0273] This embodiment mode can be freely combined with other embodiment modes.
[0274] Embodiment 3 In this embodiment, a configuration other than the positive electrode active material and the electrolyte contained in the secondary battery will be described.
[0275] <Positive Electrode> The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer includes a positive electrode active material and may further include at least one of a conductive additive and a binder. The positive electrode active material described in Embodiment 1 can be used.
[0276] FIG. 13A shows an example of a schematic cross-sectional view of a positive electrode.
[0277] The current collector 550 can be, for example, a metal foil. The positive electrode can be formed by applying a slurry to a metal foil and drying it. Note that pressing may be performed after drying. The positive electrode is formed by forming an active material layer on the current collector 550.
[0278] The slurry is a material liquid used to form an active material layer on the current collector 550, and refers to a material containing an active material, a binder, and a solvent, and preferably further mixed with a conductive additive. The slurry is also called an electrode slurry or an active material slurry, and is sometimes called a positive electrode slurry when forming a positive electrode active material layer, and a negative electrode slurry when forming a negative electrode active material layer.
[0279] The positive electrode active material 561 can be a material that does not deteriorate much with charge and discharge even at high charge voltages. Two or more types of materials with different particle sizes can be used for the positive electrode active material 561, as long as they do not deteriorate much with charge and discharge even at high charge voltages. In FIG. 9A , the positive electrode active material 561 is mixed with a positive electrode active material 562 having a smaller median diameter (D50) than the positive electrode active material 561.
[0280] The conductive additive is also called a conductivity-imparting agent or a conductive material, and a carbon material can be used. By attaching the conductive additive between multiple active materials, the multiple active materials are electrically connected to each other, thereby increasing the conductivity. In this specification, the term "attachment" does not only refer to physical adhesion between the active material and the conductive additive, but also includes cases where a covalent bond is formed, bonding due to van der Waals forces, the conductive additive covers part of the surface of the active material, the conductive additive is embedded in the surface irregularities of the active material, and electrical connection even when not in contact with each other.
[0281] Specific examples of carbon materials that can be used as the conductive additive include carbon black (furnace black, acetylene black, graphite, etc.).
[0282] FIG. 13A illustrates carbon black 553 as a conductive additive.
[0283] A binder (resin) may be mixed to bond the current collector 550, such as a metal foil, and the active material to form the positive electrode of the secondary battery. The binder is also called a binding agent. The binder is a polymer material, and adding a large amount of binder reduces the proportion of active material in the positive electrode, thereby reducing the discharge capacity of the secondary battery. Therefore, it is preferable to mix the minimum amount of binder. In FIG. 13A, the areas not filled with the positive electrode active material 561, the positive electrode active material 562, and the carbon black 553 represent voids or binders.
[0284] 13A shows an example in which the positive electrode active material 561 and the like are spherical, but this is not particularly limited. For example, FIG. 13B shows an example in which the positive electrode active material 561 has a polygonal shape with rounded corners. In this way, the cross-sectional shape of the positive electrode active material may be elliptical, rectangular, trapezoidal, conical, polygonal with rounded corners, or asymmetrical.
[0285] 13B , graphene 554 is used as a carbon material used as a conductive additive in addition to carbon black 553. That is, FIG. 13B shows a positive electrode active material layer including a positive electrode active material 561, carbon black 553, and graphene 554 over a current collector 550. Note that in FIG. 13B , regions not filled with the positive electrode active material 561, the graphene 554, or the carbon black 553 indicate voids or binders.
[0286] In the step of mixing the graphene 554 and the carbon black 553 to obtain electrode slurry, the weight of the carbon black to be mixed is preferably 1.5 to 20 times, more preferably 2 to 9.5 times, that of the graphene.
[0287] Furthermore, when the mixture of graphene 554 and carbon black 553 is within the above range, the dispersion stability of carbon black 553 is excellent and agglomerations are less likely to occur during slurry preparation. Furthermore, when the mixture of graphene 554 and carbon black 553 is within the above range, a higher electrode density can be achieved than a positive electrode using only carbon black 553 as a conductive additive. Increasing the electrode density can increase the capacity per unit weight. Specifically, the density of the positive electrode active material layer measured gravimetrically can be 3.5 g / cc or more.
[0288] Although the electrode density is lower than that of a positive electrode using only graphene as a conductive additive, by adjusting the mixture of graphene and carbon black to the above range, it can accommodate rapid charging, making it particularly effective for use as an in-vehicle secondary battery.
[0289] 13C illustrates an example of a positive electrode in which carbon fibers 555 are used instead of graphene. The other configurations in FIG. 13C are the same as those in FIG. 9B. The carbon fibers 555 can prevent the carbon black 553 from agglomerating and improve dispersibility.
[0290] In FIG. 13C, the regions not filled with the positive electrode active material 561, the carbon fibers 555, and the carbon black 553 indicate voids or binders.
[0291] Another example of a positive electrode is shown in Fig. 13D. Fig. 13D shows an example in which carbon fibers 555 are used in addition to graphene 554. The other configurations in Fig. 13D are the same as those in Fig. 13B. Using both graphene 554 and carbon fibers 555 can prevent aggregation of carbon black such as carbon black 553 and further improve dispersibility.
[0292] In FIG. 13D , regions that are not filled with the positive electrode active material 561 , the carbon fibers 555 , the graphene 554 , and the carbon black 553 indicate voids or binders.
[0293] A secondary battery can be produced by using any one of the positive electrodes shown in FIGS. 13A to 13D , placing a separator on the positive electrode, and placing the laminate obtained by placing the negative electrode on the separator in a container (such as an outer casing or a metal can) and filling the container with an electrolyte.
[0294] <Positive Electrode Current Collector> For example, a metal foil can be used as the current collector 550. The positive electrode can be formed by applying a slurry onto the metal foil and drying it. Note that pressing may be performed after drying.
[0295] The metal foil can be made of a highly conductive material, such as stainless steel, gold, platinum, aluminum, titanium, or an alloy thereof. The material used for the positive electrode current collector preferably does not dissolve at the potential of the positive electrode. Aluminum alloys containing elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, or molybdenum, can also be used. The current collector may also be made of a metal element that reacts with silicon to form a silicide. Examples of metal elements that react with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector can be in the form of a foil, plate, sheet, mesh, punched metal, expanded metal, or the like. The current collector preferably has a thickness of 5 μm to 30 μm.
[0296] The slurry is a material liquid used to form a positive electrode active material layer on the current collector 550, and refers to a material containing an active material, a binder, and a solvent, and preferably further mixed with a conductive material. The slurry is also called an electrode slurry or an active material slurry, and is sometimes called a positive electrode slurry when forming a positive electrode active material layer, and a negative electrode slurry when forming a negative electrode active material layer.
[0297] <Binder> The positive electrode of the secondary battery may contain a binder (resin) to bond the current collector 550 and the active material together. The binder is also called a binding agent.
[0298] As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Furthermore, as the binder, fluororubber can be used.
[0299] Furthermore, it is preferable to use, for example, a water-soluble polymer as the binder. Examples of the water-soluble polymer that can be used include polysaccharides. Examples of the polysaccharide that can be used include one or more of cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, and starch. It is even more preferable to use these water-soluble polymers in combination with the above-mentioned rubber material.
[0300] The binder may be used in combination with two or more of the above.
[0301] For example, a material with a particularly excellent viscosity adjusting effect may be used in combination with another material. For example, while rubber materials have excellent adhesive strength and / or elasticity, it may be difficult to adjust the viscosity when mixed with a solvent. In such cases, it is preferable to mix them with a material with a particularly excellent viscosity adjusting effect. For example, a water-soluble polymer may be used as a material with a particularly excellent viscosity adjusting effect. Furthermore, as water-soluble polymers with a particularly excellent viscosity adjusting effect, the aforementioned polysaccharides, for example, carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, and diacetyl cellulose, cellulose derivatives such as regenerated cellulose, and starch may be used.
[0302] The binder is a polymer material, and if a large amount of the binder is added, the ratio of the active material in the positive electrode or negative electrode decreases, resulting in a decrease in the discharge capacity of the secondary battery. Therefore, it is preferable to mix the binder in a minimum amount.
[0303] <Negative Electrode> The negative electrode has a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer has a negative electrode active material, and may further have a conductive material and a binder.
[0304] <Negative Electrode Active Material> As the negative electrode active material, for example, an alloy material and / or a carbon material can be used.
[0305] In addition, the negative electrode active material can be an element capable of undergoing a charge-discharge reaction by alloying / de-alloying with lithium. For example, one or more materials selected from silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. These elements have a larger capacity than carbon, and silicon in particular has a high theoretical capacity of 4200 mAh / g per active material weight. For this reason, it is preferable to use silicon as the negative electrode active material. Alternatively, compounds containing these elements may be used. For example, SiO, Mg 2 Si, Mg 2 Ge, SnO, SnO 2 , Mg 2 Sn, SnS 2 , V 2 Sn 3, FeSn 2 , CoSn 2 , Ni 3 Sn 2 , Cu 6 Sn 5 , Ag 3 Sn, Ag 3 Sb, Ni 2 MnSb, CeSb 3 , LaSn 3 , La 3 Co 2 Sn 7 , CoSb 3 , InSb, SbSn, etc. Here, elements that can undergo charge-discharge reactions by alloying / dealloying reactions with lithium, and compounds containing such elements, are sometimes referred to as alloy-based materials.
[0306] In this specification, "SiO" refers to, for example, silicon monoxide. x Here, x preferably has a value of 1 or close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.
[0307] The carbon material may be one or more selected from graphite, graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon fiber (carbon nanotube), graphene, carbon black, and the like.
[0308] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, spherical graphite having a spherical shape can be used as the artificial graphite. For example, MCMB may have a spherical shape and is therefore preferred. Furthermore, it is relatively easy to reduce the surface area of MCMB, and this may be preferred. Examples of natural graphite include flake graphite and spherical natural graphite.
[0309] When lithium ions are inserted into graphite (when a lithium-graphite intercalation compound is formed), graphite exhibits a potential as low as that of metallic lithium (0.05 V to 0.3 V vs. Li / Li +This allows secondary batteries using graphite to exhibit high operating voltages. Graphite is also preferred because it has advantages such as a relatively high capacity per unit volume, relatively small volume expansion, low cost, and higher safety than lithium metal.
[0310] Titanium dioxide (TiO 2 ), lithium titanium composite oxide (Li 4 Ti 5 O 12 ), lithium-graphite intercalation compound (Li x C 6 ), niobium pentoxide (Nb 2 O 5 ), tungsten dioxide (WO 2 ), molybdenum dioxide (MoO 2 ) and the like can be used.
[0311] In addition, as the negative electrode active material, a nitride of lithium and a transition metal, Li 3 Li with N-type structure 3−x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N has a large discharge capacity (900 mAh / g (per weight of negative electrode active material), 1890 mAh / cm 3 ) and is preferred.
[0312] When a nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, so V, which does not contain lithium ions, is used as the positive electrode active material. 2 O 5 , Cr 3 O 8 It is preferable that the material can be combined with a material such as the above. Even when a material containing lithium ions is used as the positive electrode active material, it is possible to use a nitride of lithium and a transition metal as the negative electrode active material by first desorbing the lithium ions contained in the positive electrode active material.
[0313] Furthermore, a material that undergoes a conversion reaction can also be used as the negative electrode active material. For example, a transition metal oxide that does not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), or iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include Fe 2 O 3 ,CuO,Cu 2 O, RuO 2 , Cr 2 O 3 oxides such as CoS 0.89 , sulfides such as NiS and CuS, Zn 3 N 2 , Cu 3 N, Ge 3 N 4 Nitrides such as NiP 2 , FeP 2 , CoP 3 Phosphides such as FeF 3 , BiF 3 This also occurs with fluorides such as
[0314] The conductive material and binder that can be contained in the negative electrode active material layer can be the same as the conductive material and binder that can be contained in the positive electrode active material layer.
[0315] <Negative electrode current collector> The negative electrode current collector may be made of the same material as the positive electrode current collector, or may be made of copper, etc. It is preferable that the negative electrode current collector be made of a material that does not alloy with carrier ions such as lithium.
[0316] [Electrolyte] The electrolyte described in the first embodiment and the like can be used.
[0317] [Separator] When the electrolyte is liquid, a separator is disposed between the positive electrode and the negative electrode. Examples of separators that can be used include those made of cellulose-containing fibers such as paper, nonwoven fabrics, glass fibers, ceramics, or synthetic fibers such as nylon (polyamide), vinylon (polyvinyl alcohol-based fibers), polypropylene, polyimide, polyester, acrylic, polyolefin, and polyurethane. The porosity of the separator can be 35% to 90%, preferably 60% to 85%. Separators using polypropylene can have a porosity of 35% to 45%. Separators using polyimide can have a porosity of 75% to 85%. The thickness of the separator is preferably 10 μm to 80 μm, more preferably 20 μm to 60 μm. Separators using polyimide can have a high porosity and can be made thicker (typically, a thickness of 50 μm to 60 μm).
[0318] The separator is preferably processed into a bag shape and disposed so as to encase either the positive electrode or the negative electrode.
[0319] The separator may have a multilayer structure. For example, an organic film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine-based material, a polyamide material, or a mixture of these. Examples of ceramic materials include aluminum oxide particles and silicon oxide particles. Examples of fluorine-based materials include PVDF and polytetrafluoroethylene. Examples of polyamide materials include nylon and aramid (meta-aramid, para-aramid).
[0320] When a separator with a multilayer structure is used, the safety of the secondary battery can be maintained even if the overall thickness of the separator is thin, and therefore the capacity per volume of the secondary battery can be increased.
[0321] [Exterior Body] The exterior body of the secondary battery can be made of a metal material such as aluminum or a resin material. A film-like exterior body can also be used. Examples of the film include a multilayer film in which a highly flexible metal thin film made of aluminum, stainless steel, copper, nickel, or the like is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and an insulating synthetic resin film made of polyamide resin, polyester resin, or the like is further provided on the metal thin film as the outer surface of the exterior body. A multilayer film using aluminum as the metal is called an aluminum laminate film.
[0322] This embodiment can be used in combination with other embodiments.
[0323] Embodiment Mode 4 In this embodiment mode, an example of a secondary battery having a positive electrode manufactured by the manufacturing method described in the previous embodiment mode will be described.
[0324] [Coin-Type Secondary Battery] An example of a coin-type secondary battery will be described. Fig. 14A is an exploded perspective view of a coin-type (single-layer flat) secondary battery, Fig. 14B is an external view, and Fig. 14C is a cross-sectional view thereof. Coin-type secondary batteries are mainly used in small electronic devices.
[0325] 14A is a schematic diagram that shows the overlapping of components (upper and lower relationships and positional relationships) for ease of understanding, and therefore, FIGS. 14A and 14B are not completely identical corresponding views.
[0326] In Fig. 14A, a positive electrode 304, a separator 310, a negative electrode 307, a spacer 322, and a washer 312 are stacked. These are sealed with a negative electrode can 302 and a positive electrode can 301 by a gasket. Note that the gasket for sealing is not shown in Fig. 14A. The spacer 322 and the washer 312 are used to protect the inside or to fix the position inside the can when the positive electrode can 301 and the negative electrode can 302 are crimped together. The spacer 322 and the washer 312 are made of stainless steel or an insulating material.
[0327] A positive electrode 304 has a laminated structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 .
[0328] FIG. 14B is a perspective view of the completed coin-type secondary battery.
[0329] In the coin-type secondary battery 300, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, are insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed by a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed by a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. The negative electrode 307 is not limited to a laminated structure, and may be formed of lithium metal foil or a lithium-aluminum alloy foil.
[0330] It is preferable that the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 each have an active material layer formed on only one surface.
[0331] The positive electrode can 301 and the negative electrode can 302 can be made of a metal such as nickel, aluminum, or titanium that is corrosion-resistant to the electrolyte, or an alloy of these metals or an alloy of these metals with other metals (e.g., stainless steel). Furthermore, to prevent corrosion by the electrolyte, etc., they are preferably coated with nickel, aluminum, or the like. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.
[0332] As shown in FIG. 10C , the negative electrode 307, the positive electrode 304, the separator 310, the negative electrode 307, and the negative electrode can 302 are stacked in this order with the positive electrode can 301 facing downwards, and the positive electrode can 301 and the negative electrode can 302 are crimped together via a gasket 303 to produce a coin-shaped secondary battery 300.
[0333] By having the above-described configuration, the coin-type secondary battery 300 can have a high discharge capacity and excellent cycle characteristics.
[0334] [Cylindrical Secondary Battery] An example of a cylindrical secondary battery will be described with reference to Fig. 15A. As shown in Fig. 15A, a cylindrical secondary battery 616 has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap 601 and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0335] 15B is a schematic diagram showing a cross section of a cylindrical secondary battery. The cylindrical secondary battery shown in FIG. 15B has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0336] A battery element is provided inside a hollow cylindrical battery can 602, in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with a separator 605 sandwiched between them. Although not shown, the battery element is wound around a central axis. One end of the battery can 602 is closed and the other end is open. The battery can 602 can be made of a metal such as nickel, aluminum, or titanium that is corrosion-resistant to the electrolyte, or an alloy of these metals or an alloy of these metals with other metals (e.g., stainless steel). Furthermore, to prevent corrosion by the electrolyte, the battery can 602 is preferably coated with nickel, aluminum, or the like. Inside the battery can 602, the wound battery element, in which the positive electrode, negative electrode, and separator are wound, is sandwiched between a pair of opposing insulating plates 608 and 609.
[0337] Since the positive and negative electrodes used in a cylindrical storage battery are wound, it is preferable to form active materials on both sides of the current collector.
[0338] By using the positive electrode active material 100 of one embodiment of the present invention for the positive electrode 604, a cylindrical secondary battery 616 with high capacity, high discharge capacity, and excellent cycle characteristics can be obtained.
[0339] A positive electrode terminal (positive electrode current collecting lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collecting lead) 607 is connected to the negative electrode 606. The positive electrode terminal 603 can be made of a metal material such as aluminum. The negative electrode terminal 607 can be made of a metal material such as copper. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 613, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 613 is electrically connected to the positive electrode cap 601 via a PTC (Positive Temperature Coefficient) element 611. The safety valve mechanism 613 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the increase in internal pressure of the battery exceeds a predetermined threshold. The PTC element 611 is a thermosensitive resistor whose resistance increases when the temperature rises, and the increase in resistance limits the amount of current to prevent abnormal heat generation. 3 )-based semiconductor ceramics, etc. can be used.
[0340] 15C shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616. The positive electrodes of each secondary battery are in contact with and electrically connected to conductors 624 separated by insulators 625. The conductors 624 are electrically connected to a control circuit 620 via wiring 623. The negative electrodes of each secondary battery are electrically connected to the control circuit 620 via wiring 626. The control circuit 620 may be a charge / discharge control circuit that performs charging and discharging, or a protection circuit that prevents overcharging and / or overdischarging.
[0341] 15D shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616, which are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of secondary batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 by wiring 627. The plurality of secondary batteries 616 may be connected in parallel, in series, or in parallel and then further connected in series. By configuring the power storage system 615 to have a plurality of secondary batteries 616, it is possible to extract a large amount of power.
[0342] A plurality of secondary batteries 616 may be connected in parallel and then further connected in series.
[0343] Furthermore, a temperature control device may be provided between the multiple secondary batteries 616. When the secondary batteries 616 are overheated, they can be cooled by the temperature control device, and when the secondary batteries 616 are too cold, they can be heated by the temperature control device. This makes it difficult for the performance of the power storage system 615 to be affected by the outside air temperature.
[0344] 15D , the power storage system 615 is electrically connected to a control circuit 620 via wiring 621 and wiring 622. The wiring 621 is electrically connected to the positive electrodes of the plurality of secondary batteries 616 via a conductive plate 628, and the wiring 622 is electrically connected to the negative electrodes of the plurality of secondary batteries 616 via a conductive plate 614.
[0345] [Another Structural Example of Secondary Battery] Another structural example of a secondary battery will be described with reference to FIGS. 16 and 17. FIG.
[0346] A secondary battery 913 shown in FIG. 16A has a wound body 950 provided with terminals 951 and 952 inside a housing 930. The wound body 950 is immersed in an electrolyte inside the housing 930. The terminal 952 contacts the housing 930, and the terminal 951 is not in contact with the housing 930 by using an insulating material or the like. Note that in FIG. 16A , for convenience, the housing 930 is shown separated, but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (e.g., aluminum) or a laminate of a metal material and a resin material.
[0347] 16B, the housing 930 shown in Fig. 16A may be formed from a plurality of materials. For example, the secondary battery 913 shown in Fig. 16B has a housing 930a and a housing 930b bonded together, and a wound body 950 is provided in the area surrounded by the housing 930a and the housing 930b.
[0348] By using a material such as organic resin for the surface of the housing 930a on which the antenna is formed, it is possible to prevent the secondary battery 913 from blocking the electric field. Note that if the housing 930a does not block the electric field much, the antenna may be provided inside the housing 930a. The housing 930b can be made of, for example, a metal material (such as aluminum) or a laminate of a metal material and a resin material.
[0349] 16C shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the separator 933 sandwiched therebetween, and the laminated sheet is wound. Note that multiple layers of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked.
[0350] Alternatively, a secondary battery 913 may be provided that has a wound body 950a as shown in Fig. 17A. The wound body 950a shown in Fig. 17A has a negative electrode 931, a positive electrode 932, and a separator 933. The negative electrode 931 has a negative electrode active material layer 931a. The positive electrode 932 has a positive electrode active material layer 932a.
[0351] By using the positive electrode active material 100 of one embodiment of the present invention for the positive electrode 932, the secondary battery 913 can have a large capacity, a high discharge capacity, and excellent cycle characteristics.
[0352] The separator 933 has a width wider than the negative electrode active material layer 931 a and the positive electrode active material layer 932 a, and is wound so as to overlap the negative electrode active material layer 931 a and the positive electrode active material layer 932 a. From the standpoint of safety, it is preferable that the negative electrode active material layer 931 a be wider than the positive electrode active material layer 932 a. A wound body 950 a having such a shape is preferable due to its high safety and productivity.
[0353] 17B , the negative electrode 931 is electrically connected to a terminal 951 by ultrasonic bonding, welding, or crimping. The terminal 951 is electrically connected to a terminal 911a. The positive electrode 932 is electrically connected to a terminal 952 by ultrasonic bonding, welding, or crimping. The terminal 952 is electrically connected to a terminal 911b.
[0354] 17C , the wound body 950a and the electrolyte are covered by the housing 930 to form the secondary battery 913. It is preferable to provide the housing 930 with a safety valve, an overcurrent protection element, etc. The safety valve is a valve that opens when the internal pressure inside the housing 930 reaches a predetermined value to prevent the battery from exploding.
[0355] As shown in Fig. 17B, the secondary battery 913 may have multiple wound bodies 950a. Using multiple wound bodies 950a can result in a secondary battery 913 with a larger discharge capacity. For other elements of the secondary battery 913 shown in Figs. 17B and 17C, refer to the description of the secondary battery 913 shown in Figs. 16A and 16B.
[0356] 18A and 18B show examples of the external appearance of a laminated secondary battery. As shown in Fig. 18A and 18B, a laminated secondary battery 500 has a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511.
[0357] 18A shows an external view of a positive electrode 503 and a negative electrode 506. The positive electrode 503 has a positive electrode current collector 501, and a positive electrode active material layer 502 is formed on the surface of the positive electrode current collector 501. The positive electrode 503 also has a region where the positive electrode current collector 501 is partially exposed (hereinafter referred to as a tab region). The negative electrode 506 has a negative electrode current collector 504, and a negative electrode active material layer 505 is formed on the surface of the negative electrode current collector 504. The negative electrode 506 also has a region where the negative electrode current collector 504 is partially exposed, i.e., a tab region. Note that the area or shape of the tab regions of the positive electrode 503 and the negative electrode 506 are not limited to the example shown in FIG. 18A .
[0358] <Method of Manufacturing Laminated Secondary Battery> An example of a method of manufacturing the laminated secondary battery 500 whose external view is shown in FIG. 18A will be described with reference to FIGS. 19A to 19C.
[0359] First, a positive electrode 503 and a negative electrode 506 are prepared as shown in FIG. 19A . Next, as shown in FIG. 19B , the negative electrode 506, the separator 507, and the positive electrode 503 are laminated. Here, an example is shown in which five pairs of negative electrodes 506 and four pairs of positive electrodes 503 are used. This can also be called a laminate consisting of the negative electrode 506, the separator 507, and the positive electrode 503. Next, the tab regions of the positive electrodes 503 are bonded to each other, and a positive electrode lead electrode 510 is bonded to the tab region of the outermost positive electrode 503. For example, ultrasonic welding or the like may be used for bonding. Similarly, the tab regions of the negative electrodes 506 are bonded to each other, and a negative electrode lead electrode 511 is bonded to the tab region of the outermost negative electrode 506.
[0360] Next, as shown in FIG. 19C, the above-described laminate is placed on an exterior body 509.
[0361] Next, as shown in Fig. 19C, the exterior body 509 is folded at the portion indicated by the dashed line. Thereafter, the outer periphery of the exterior body 509 is joined. For example, thermocompression bonding or the like may be used for joining. At this time, an area (hereinafter referred to as an inlet) that is not joined is provided in a part (or one side) of the exterior body 509 so that an electrolyte can be introduced later.
[0362] Next, the electrolyte solution is introduced into the inside of the exterior body 509 through an inlet provided in the exterior body 509. The introduction of the electrolyte solution is preferably carried out under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is joined. In this manner, the laminated secondary battery 500 can be produced.
[0363] By using the positive electrode active material 100 of one embodiment of the present invention for the positive electrode 503, the secondary battery 500 can have a high capacity, a high discharge capacity, and excellent cycle characteristics.
[0364] This embodiment mode can be implemented in appropriate combination with other embodiment modes or examples.
[0365] Embodiment 5 In this embodiment, an example of a vehicle including a secondary battery according to one embodiment of the present invention will be described. The secondary battery according to one embodiment of the present invention is preferable because it is less likely to catch fire.
[0366] When a secondary battery according to an embodiment of the present invention is installed in a vehicle, next-generation clean energy automobiles such as hybrid vehicles (HVs), electric vehicles (EVs), or plug-in hybrid vehicles (PHVs) can be realized. The secondary battery can also be installed in agricultural machinery, mopeds including electrically assisted bicycles, motorcycles, electric wheelchairs, electric carts, ships, submarines, aircraft, rockets, artificial satellites, space probes, planetary probes, or spacecraft. The secondary battery according to an embodiment of the present invention can be a high-capacity secondary battery. Therefore, the secondary battery according to an embodiment of the present invention is suitable for miniaturization and weight reduction, and can be suitably used in transportation vehicles.
[0367] 20A to 20D illustrate examples of transportation vehicles using one embodiment of the present invention. An automobile 2001 shown in FIG. 20A is an electric automobile that uses an electric motor as a power source for traveling. Alternatively, the automobile 2001 is a hybrid automobile that can appropriately select and use an electric motor or an engine as a power source for traveling. When a secondary battery is mounted on a vehicle, an example of the secondary battery described in Embodiment 4 is installed in one or more locations. The automobile 2001 shown in FIG. 20A includes a battery pack 2200, which includes a secondary battery module to which a plurality of secondary batteries are connected. It is preferable that the automobile 2001 further includes a charge control device electrically connected to the secondary battery module.
[0368] Furthermore, automobile 2001 can charge its secondary battery by receiving power supply from an external charging facility using a plug-in system, a contactless power supply system, or the like. When charging, the charging method or connector standard may be a predetermined system such as CHAdeMO (registered trademark) or Combo. The charging facility is preferably a charging station installed in a commercial facility, or may be a household power source. For example, plug-in technology can be used to charge an electric storage device installed in automobile 2001 using an external power supply. Charging can be performed by converting AC power to DC power via a conversion device such as an AC-DC converter.
[0369] Although not shown, a power receiving device can be mounted on a vehicle and power can be supplied contactlessly from a ground-based power transmitting device to charge the vehicle. In the case of this contactless power supply method, by incorporating a power transmitting device into a road or an exterior wall, charging can be performed not only while the vehicle is stopped but also while the vehicle is moving. This contactless power supply method can also be used to transmit and receive power between two vehicles. Furthermore, solar cells can be installed on the exterior of the vehicle to charge the secondary battery while the vehicle is stopped or moving. For such contactless power supply, an electromagnetic induction method or a magnetic field resonance method can be used.
[0370] 20B shows a large transport vehicle 2002 having an electrically controlled motor as an example of a transport vehicle. The transport vehicle 2002 has a battery pack 2201, which has a secondary battery module in which multiple secondary batteries are connected. The secondary battery module of the transport vehicle 2002 has, for example, a four-cell unit of secondary batteries with a nominal voltage of 3.0 V to 5.0 V, with 48 cells connected in series for a maximum voltage of 170 V. Other than the number of secondary batteries constituting the secondary battery module of the battery pack 2201, the transport vehicle has the same functions as those shown in FIG. 20A, and therefore a description thereof will be omitted.
[0371] FIG. 20C shows, as an example, a large transport vehicle 2003 having an electrically controlled motor. The transport vehicle 2003 has a battery pack 2202, which has a secondary battery module in which multiple secondary batteries are connected. The secondary battery module of the transport vehicle 2003 has, for example, a maximum voltage of 600 V, in which one hundred or more secondary batteries with a nominal voltage of 3.0 V or more and 5.0 V or less are connected in series. Therefore, a secondary battery with little variation in characteristics is required. By using a secondary battery in which the positive electrode active material 100 described in the first and second embodiments is used as a positive electrode, a secondary battery with stable battery characteristics can be manufactured, and mass production at low cost from the standpoint of yield is possible.
[0372] Fig. 20D shows, as an example, an aircraft 2004 having an engine that burns fuel. Since the aircraft 2004 shown in Fig. 20D has wheels for takeoff and landing, it can also be said to be part of a transportation vehicle, and has a battery pack 2203 that includes a secondary battery module formed by connecting multiple secondary batteries and the secondary battery module and a charge control device.
[0373] The secondary battery module of the aircraft 2004 has, for example, eight 4 V secondary batteries connected in series to produce a maximum voltage of 32 V. Other than the number of secondary batteries constituting the secondary battery module of the battery pack 2203, the secondary battery module has the same functions as those shown in Fig. 20A, and therefore a description thereof will be omitted.
[0374] 20E shows, as an example, a satellite 2005 equipped with a secondary battery 2204. Since the satellite 2005 is used in the extremely low temperature of outer space, it is preferable that the satellite 2005 be equipped with a secondary battery 2204 according to an embodiment of the present invention, which has excellent low temperature resistance. It is further preferable that the secondary battery 2204 be mounted inside the satellite 2005 while being covered with a heat insulating member.
[0375] This embodiment mode can be implemented in appropriate combination with other embodiment modes or examples.
[0376] (Embodiment 6) In this embodiment, an example in which a lithium ion battery according to one embodiment of the present invention is mounted on a motorcycle or a bicycle will be described as an example in which a secondary battery is mounted on a vehicle.
[0377] FIG. 21A illustrates an example of an electric bicycle using a secondary battery according to one embodiment of the present invention. An electric bicycle 8700 can use a secondary battery 8701 according to one embodiment of the present invention as a power storage device 8702, and power from the secondary battery is supplied to a motor that assists a rider. The power storage device 8702 is preferably portable, and FIG. 21B illustrates the power storage device 8702 detached from the bicycle. The power storage device 8702 preferably includes a display unit 8703 that can display the remaining battery level and the like. The power storage device 8702 preferably includes a control circuit 8704 that can control charging or detect an abnormality of the secondary battery. The control circuit 8704 is electrically connected to the positive and negative electrodes of the secondary battery 8701. An electric bicycle equipped with a secondary battery according to one embodiment of the present invention is safe even when operated at high voltage.
[0378] 21C is an example of a two-wheeled vehicle using a secondary battery of one embodiment of the present invention. A scooter 8600 shown in FIG. 21C includes a power storage device 8602, a side mirror 8601, and a turn signal light 8603. A secondary battery 8701 of one embodiment of the present invention can be applied to the power storage device 8702, and power from the secondary battery is supplied to the turn signal light 8603. Furthermore, a two-wheeled vehicle equipped with a secondary battery of one embodiment of the present invention is safe even when operated at high voltage.
[0379] 21C can store a power storage device 8602 in an under-seat storage compartment 8604. The power storage device 8602 can be stored in the under-seat storage compartment 8604 even if the under-seat storage compartment 8604 is small.
[0380] This embodiment mode can be implemented in appropriate combination with other embodiment modes or examples.
[0381] (Embodiment 7) In this embodiment, an example in which a secondary battery according to one embodiment of the present invention is mounted in an electronic device will be described. The secondary battery according to one embodiment of the present invention is preferable because it is less likely to ignite. Examples of electronic devices in which a secondary battery is mounted include television devices (also referred to as televisions or television receivers), computer monitors, digital cameras, digital video cameras, digital photo frames, mobile phones (also referred to as mobile phones or mobile phone devices), portable game consoles, personal digital assistants, sound players, and large game consoles such as pachinko machines. Examples of personal digital assistants include notebook personal computers, tablet devices, e-book readers, and mobile phones.
[0382] 22A shows an example of a mobile phone. The mobile phone 2100 includes a display portion 2102 built into a housing 2101, operation buttons 2103, an external connection port 2104, a speaker 2105, a microphone 2106, and the like. The mobile phone 2100 includes a secondary battery 2107. A mobile phone equipped with the secondary battery 2107 of one embodiment of the present invention is safe even when operated at high voltage.
[0383] The mobile phone 2100 can execute various applications such as mobile phone calls, e-mail, document browsing and creation, music playback, internet communication, and computer games.
[0384] The operation button 2103 can be provided with various functions such as time setting, power on / off operation, wireless communication on / off operation, silent mode activation / deactivation, power saving mode activation / deactivation, etc. For example, the functions of the operation button 2103 can be freely set by an operating system incorporated in the mobile phone 2100.
[0385] The mobile phone 2100 is also capable of performing standardized short-range wireless communication, and can also make hands-free calls by communicating with a wirelessly enabled headset, for example.
[0386] The mobile phone 2100 also includes an external connection port 2104, and can directly exchange data with other information terminals via a connector. Charging can also be performed via the external connection port 2104. Note that charging may be performed by wireless power supply without using the external connection port 2104.
[0387] Furthermore, the mobile phone 2100 preferably has a sensor. As the sensor, for example, a fingerprint sensor, a pulse sensor, a body temperature sensor or other human body sensor, a touch sensor, a pressure sensor, an acceleration sensor, or the like is preferably mounted.
[0388] FIG. 22B shows an unmanned aerial vehicle 2300 having multiple rotors 2302. The unmanned aerial vehicle 2300 is sometimes called a drone. The unmanned aerial vehicle 2300 has a secondary battery 2301 according to an embodiment of the present invention, a camera 2303, and an antenna (not shown). The unmanned aerial vehicle 2300 can be remotely controlled via the antenna. Furthermore, the unmanned aerial vehicle 2300 equipped with the secondary battery 2301 according to an embodiment of the present invention is safe even when operated at high voltages. Furthermore, it can be used safely for long periods of time.
[0389] Fig. 22C shows an example of a robot. A robot 6400 shown in Fig. 22C includes a secondary battery 6409, an illuminance sensor 6401, a microphone 6402, an upper camera 6403, a speaker 6404, a display unit 6405, a lower camera 6406, an obstacle sensor 6407, a movement mechanism 6408, a computing device, etc.
[0390] The microphone 6402 has a function of detecting the user's speaking voice, environmental sounds, etc. The speaker 6404 has a function of emitting sound. The robot 6400 can communicate with the user using the microphone 6402 and the speaker 6404.
[0391] The display unit 6405 has a function of displaying various information. The robot 6400 can display information desired by the user on the display unit 6405. The display unit 6405 may be equipped with a touch panel. The display unit 6405 may also be a detachable information terminal, which can be installed in a fixed position on the robot 6400 to enable charging and data transfer.
[0392] The upper camera 6403 and the lower camera 6406 have the function of capturing images of the surroundings of the robot 6400. In addition, the obstacle sensor 6407 can detect the presence or absence of obstacles in the direction of travel when the robot 6400 moves forward using the movement mechanism 6408. The robot 6400 can recognize the surrounding environment and move safely using the upper camera 6403, the lower camera 6406, and the obstacle sensor 6407.
[0393] The robot 6400 includes a secondary battery 6409 according to one embodiment of the present invention and a semiconductor device or an electronic component in its internal area. The robot equipped with the secondary battery 6409 according to one embodiment of the present invention is safe even when operated at high voltage. Furthermore, the robot can be used safely for a long period of time.
[0394] FIG. 22D illustrates an example of a portable fan. The portable fan 6200 illustrated in FIG. 22D includes a secondary battery 6209 according to one embodiment of the present invention, an operation button 6205, a fan 6202, an external connection port 6204, and the like, and the secondary battery 6209 is housed in a housing 6201. The portable fan 6200 can operate a motor using power supplied from the secondary battery 6209 to rotate the fan 6202, and the secondary battery 6209 can be charged via the external connection port 6204. The secondary battery 6209 is illustrated as a cylindrical secondary battery, but the shape is not particularly limited. Furthermore, the portable fan 6200 equipped with the secondary battery 6209 according to one embodiment of the present invention is safe even when operated at a high voltage. Furthermore, it can be used safely for a long period of time.
[0395] 22E shows an example of a cleaning robot. The cleaning robot 6300 includes a display unit 6302 arranged on the top surface of a housing 6301, a plurality of cameras 6303 arranged on the side surfaces, a brush 6304, an operation button 6305, a secondary battery 6306, various sensors, and the like. Although not shown, the cleaning robot 6300 is provided with tires, a suction port, and the like. The cleaning robot 6300 can move by itself, detect dust 6310, and suck the dust 6310 from a suction port provided on the bottom surface of the housing 6301.
[0396] The cleaning robot 6300 can analyze an image captured by the camera 6303 and determine whether or not there is an obstacle such as a wall, furniture, or a step. Furthermore, if an object that may become entangled in the brush 6304, such as a wire, is detected through image analysis, the cleaning robot 6300 can stop the rotation of the brush 6304. The cleaning robot 6300 includes a secondary battery 6306 according to one embodiment of the present invention and a semiconductor device or electronic component in its internal area. Furthermore, the cleaning robot 6300 equipped with the secondary battery 6209 according to one embodiment of the present invention is safe even when operated at a high voltage. Furthermore, it can be used safely for a long period of time.
[0397] This embodiment mode can be implemented in appropriate combination with other embodiment modes or examples.
[0398] <Calculation of HOMO Level and LUMO Level> In this example, the HOMO level and LUMO level of each organic compound were calculated. The calculation was performed using the quantum chemistry calculation program Gaussian09. B3LYP was used as the functional, and 6-311G(d,p) was used as the basis function. With the above-mentioned basis functions, for example, in the case of a hydrogen atom, the 1s to 3s orbitals are considered, and in the case of a carbon atom, the 1s to 4s and 2p to 4p orbitals are considered. Furthermore, to improve the calculation accuracy, a p function was added to hydrogen atoms and a d function was added to atoms other than hydrogen atoms as a polarization basis set.
[0399] The organic compounds used for the calculations were fluorine-free organic compounds and fluorine-containing organic compounds, and the advantages of fluorine-containing organic compounds were verified. Table 1 shows the calculation conditions and the organic compounds used for the calculations. Ethylene carbonate (EC) and methyl propionate (MP) are fluorine-free organic compounds, while structural formulas H11 to H15 and H21 to H25 are fluorine-containing organic compounds. In Table 1, organic compounds with cyclic molecular structures are listed in the upper row, and organic compounds with chain molecular structures are listed in the lower row. The fluorine-containing group in a fluorine-containing organic compound can be called an electron-withdrawing substituent, and a fluorine-containing organic compound is called a fluorine-substituted organic compound.
[0400]
[0401] The HOMO and LUMO levels of each organic compound were determined using quantum chemical calculations, and changes in these levels were analyzed. In the calculations, the structure of the singlet ground state of each organic compound was optimized, and it was assumed to be a stable structure. The calculation results of the HOMO and LUMO levels of each organic compound are shown in Figures 23 and 24.
[0402] It has been confirmed that organic compounds containing fluorine tend to have a deeper HOMO level than organic compounds not containing fluorine. Furthermore, it has been confirmed that the HOMO level tends to become deeper as the number of fluorine substituents increases. It has also been confirmed that organic compounds containing fluorine tend to have a deeper LUMO level than organic compounds not containing fluorine. It has also been confirmed that the LUMO level tends to become deeper as the number of fluorine substituents increases. Since a deeper HOMO level makes an organic compound less susceptible to oxidation, it has been confirmed that organic compounds containing fluorine tend to be less susceptible to oxidation than organic compounds not containing fluorine.
[0403] By using a fluorine-containing organic compound in the electrolyte, a secondary battery with improved oxidation resistance can be provided. Oxidation resistance means that the surface of the positive electrode is less susceptible to oxidation, which means that the electrolyte is less susceptible to decomposition. Therefore, a secondary battery using a fluorine-containing organic compound in the electrolyte is expected to have improved initial characteristics and cycle characteristics compared to a secondary battery using a non-fluorine-containing organic compound in the electrolyte.
[0404] In this example, a half-cell was prepared to obtain a charge curve and a dQ / dV curve. A half-cell is a secondary battery that uses lithium metal as the counter electrode. The conditions for preparing the half-cell will be described below.
[0405] <Conditions for Fabricating Half-Cell> As the electrolyte for the half-cell, an organic solvent (mixed solvent) was prepared in a volume ratio of FEC:MTFP=2:8. As a lithium salt, lithium hexafluorophosphate (LiPF ) was added to the organic solvent at a concentration of 1 mol / L. 6 ) was added. No additives were used.
[0406] The positive electrode active material produced in this example will be described with reference to the production method shown in FIGS.
[0407] LiCoO in step S14 of FIG. 2 As the starting material, commercially available lithium cobalt oxide (Cellseed C-10N, manufactured by Nippon Chemical Industry Co., Ltd.) containing cobalt as the transition metal M and no additional elements was prepared and sieved using an automatic sieving machine. For the initial heating in step S15, the lithium cobalt oxide was placed in a scabbard, covered, and heated at 850°C for 2 hours using a roller hearth kiln simulator furnace (manufactured by Noritake Company, Ltd.). Oxygen was flowed through the furnace at a rate of 10 L / min. Specifically, the opening width of the exhaust port was adjusted so that the furnace differential pressure gauge indicated 5 Pa. The furnace was cooled at a rate of 200°C / hour, and the air flow was not stopped until the temperature reached 200°C.
[0408] In this example, LiF was prepared as the F source and MgF was prepared as the Mg source according to step S21 of FIG. 12A. 2 LiF:MgF was prepared. 2 were weighed out so that the molar ratio was 1:3, and sieved using an automatic sieving machine. 2 The above was mixed in dehydrated acetone at a rotation speed of 500 rpm for 20 hours to prepare an additive element source (A1 source).
[0409] Next, in step S31, the Al source and the initially heated lithium cobalt oxide were dry-mixed using a Picobond (manufactured by Hosokawa Micron Co., Ltd.) as a mixing means, and the mixture was stirred at a rotation speed of 3000 rpm for 10 minutes, and then sieved with an automatic sieving machine to obtain a mixture 903 (step S32).
[0410] Next, in step S33, the mixture 903 was heated. The heating conditions were 900° C. and 20 hours. During heating, a lid was placed on the scabbard containing the mixture 903. By placing the lid, the inside of the scabbard was made into an oxygen-containing atmosphere, and the inflow and outflow of the oxygen could be blocked (O 2 A roller hearth kiln simulator furnace (manufactured by Noritake Co., Ltd.) was used as the firing furnace. Oxygen was flowed through the furnace at a rate of 10 L / min (O 2 Specifically, the opening width of the exhaust port was adjusted so that the differential pressure gauge of the furnace was 5 Pa (positive pressure inside the furnace). When the furnace was cooled, it was cooled at a rate of 200°C / hour, and the flow of oxygen was not stopped until the temperature reached 200°C. In this way, a composite oxide containing Mg and F was obtained (step S34a).
[0411] Next, according to step S41 of Fig. 12C, nickel hydroxide that had undergone a pulverization process was prepared as the nickel source, and aluminum hydroxide that had undergone a pulverization process was prepared as the aluminum source, each of which served as an additional element source (A2 source). According to step S51, the nickel hydroxide and aluminum hydroxide were weighed out so that the nickel content of the nickel hydroxide was 0.5 mol% of the cobalt, and the aluminum content of the aluminum hydroxide was 0.5 mol% of the cobalt, and the A2 source and the composite oxide were dry-mixed. A Picobond (manufactured by Hosokawa Micron) was used as the mixing means, and the mixture was stirred at a rotation speed of 3000 rpm for 10 minutes, yielding mixture 904 (step S52).
[0412] Next, in step S53, the mixture 904 was heated. The heating conditions were 850°C and 10 hours. During heating, a lid was placed on the sagger containing the mixture 904. A roller hearth kiln simulator furnace (manufactured by Noritake Co., Ltd.) was used as the firing furnace, and the sagger was placed in the furnace and heated at the above heating temperature. Oxygen was flowed through the furnace at a rate of 10 L / min (O 2Flow). The opening width of the exhaust port was adjusted so that the differential pressure gauge of the furnace was 5 Pa. When the furnace was cooled, it was cooled at a rate of 200°C / hour, and the oxygen flow was not stopped until the temperature reached 200°C. In this way, lithium cobalt oxide containing Mg, F, Ni, and Al was obtained (step S54). In this way, the positive electrode active material 100 was designated as Sample 1.
[0413] The positive electrode was prepared using the positive electrode active material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVDF) as a binder. The PVDF was dissolved in N-methyl-2-pyrrolidone (NMP) as a solvent at a weight ratio of 5%. Next, a slurry containing the positive electrode active material, AB, and PVDF in a weight ratio of 95:3:2 was prepared, and the slurry was applied to an aluminum positive electrode current collector. The cathode was then pressed at a linear pressure of 210 kN / m and 120°C. The amount of the positive electrode active material supported was approximately 7 mg / cm. 2 It was.
[0414] Polypropylene was used as the separator.
[0415] A half-cell 1 was assembled containing the positive electrode and separator. The half-cell 1 was a CR2032 type cell with a diameter of 20 mm and a height of 3.2 mm. A lithium metal counter electrode was used. Stainless steel (SUS) was used for the positive electrode can and the negative electrode can.
[0416] <Charge / Discharge Measuring Instrument> The charge capacity of the above-described half cell 1 was measured using a charge / discharge measuring system (TOSCAT-3100) manufactured by Toyo Systems Co., Ltd. as a charge / discharge measuring instrument.
[0417] Rates are used as conditions for measuring charge capacity, discharge capacity, and cycle characteristics, and will be explained below. Rates include discharge rates, which represent the relative ratio of the current value during discharge to the battery capacity and are expressed in units of C. For example, for a battery with a rated capacity of X (Ah), the current equivalent to 1 C is X (A). When measuring charge capacity, discharge capacity, and cycle characteristics, discharging at a current of 2X (A) is said to have been performed at a discharge rate of 2C, and discharging at a current of X / 2 (A) is said to have been performed at a discharge rate of 0.5C. Rates also include charge rates, but the charge rate can be understood by replacing the discharge rate and discharge with the charge rate and charge, respectively. In the examples herein, 1C = 200 mA / g (current per weight of positive electrode active material is 200 mA / g).
[0418] <Aging> Aging was performed on half-cell 1. Note that aging is sometimes referred to as initial charge / discharge or conditioning. First, half-cell 1 was placed in a thermostatic chamber for 6 hours. Since the temperature of the thermostatic chamber was not controlled, the temperature of the thermostatic chamber can be understood to be 23°C ± 5°C. In other words, an error of ± 5°C is allowed for the temperature of the thermostatic chamber that is not temperature-controlled. Then, a charge / discharge cycle was repeated twice under the following charge / discharge conditions. Charge condition: 4.6 V (CCCV charge, 0.1 C rate, 0.01 C cutoff). Discharge condition: 2.5 V (CC discharge, 0.1 C rate). In this example, the current value corresponding to 1 C was 200 mA / g per weight of positive electrode active material. After the end of charge, a 10-minute rest period was allowed before the next discharge. If the cutoff current of the charge condition is not reached, the time may be cut off. The charge condition of 4.6 V is called the upper limit voltage, and is maintained at the upper limit voltage during CV charging. The discharge condition of 2.5 V is called the lower limit voltage.
[0419] <Charging curve> Figure 25 shows the charging curve obtained after aging. The charging conditions were as follows, and were the same as the charging conditions during aging. The horizontal axis of Figure 25 represents the charging capacity (mAh / g), and the vertical axis represents the charging voltage (V). The charging capacity is per weight of the positive electrode active material. Charging conditions: 4.6 V (CCCV charging, 0.1 C rate, 0.01 C cutoff)
[0420] The charging curve confirmed that there was no abnormality in half-cell 1.
[0421] <dQ / dv curve> Figure 26 shows the dQ / dv curve obtained from the above charging curve. The horizontal axis of Figure 26 indicates the charging voltage (V), and the vertical axis indicates the value of dQ / dv. In order to obtain the dQ / dv curve, first, the measurement data (v 1 , q 1 ), (v 2 , q 2 ), ... (v n , q n ) is v when using integer i i <v i+1 Therefore, measurement data that did not satisfy the above criteria were thinned out. The charging voltage value on the horizontal axis was the average value of 32 adjacent points. The dQ / dv value on the vertical axis was calculated by dividing the "change in capacity ΔQ at 32 adjacent points" by the "change in voltage ΔV at 32 adjacent points." Figure 26 shows a gradual increase between 4.6 V and 4.75 V. This may indicate that the electrolyte did not decompose even at 4.75 V or higher, and may indicate a reaction between the positive electrode active material and the electrolyte or a phase change in the positive electrode active material.
[0422] <Charge-Discharge Cycle Test> After the aging, a charge-discharge cycle test was started. The temperature of the thermostatic chamber was confirmed to be 25°C, and the charge-discharge cycle was repeated 100 times under the following charge-discharge conditions: Charge condition: 4.7 V or 4.8 V (CCCV charge, 0.5 C rate, 0.05 C cutoff); Discharge condition: 2.5 V (CC discharge, 0.5 C rate).
[0423] As another condition, the temperature of the thermostatic bath was set to 45°C, and 100 charge / discharge cycles were repeated under the following charge / discharge conditions: Charge condition: 4.7 (CCCV charge, 0.5C rate, 0.05C cutoff); Discharge condition: 2.5V (CC discharge, 0.5C rate). In this example, the current value corresponding to 1C was 200mA / g per weight of positive electrode active material. After charging, a 10-minute rest period was provided before the next discharge. If the cutoff current of the charge condition is not reached, the time may be cut off. The charge condition of 4.7V or 4.8V is called the upper limit voltage, and is maintained at the upper limit voltage during CV charging. The discharge condition of 2.5V is called the lower limit voltage.
[0424] The results of the discharge capacity are shown in Figures 27A to 27C. In the graphs of the discharge capacity, the horizontal axis indicates cycles (times) and the vertical axis indicates discharge capacity (mAh / g). The charge and discharge conditions are also shown in the figures. Table 2 shows the cycle number at which the maximum discharge capacity was reached, the maximum discharge capacity value, and the discharge capacity retention rate up to the fifth cycle. The cycle at which the maximum discharge capacity was reached was the first cycle under all conditions. Furthermore, it was found that under all conditions, the discharge capacity retention rate for each cycle up to the fifth cycle was 95% or more, preferably 97% or more. Under all conditions, the maximum discharge capacity was good, at 200 mAh / g or more, preferably 220 mAh / g or more. Thus, it was found that the battery exhibited good initial characteristics.
[0425]
[0426] Table 3 shows the discharge capacity retention rates at the 10th, 20th, 30th, 40th, 50th, and 100th cycles. Good cycle characteristics were observed under all conditions. In particular, at 4.7 V and 25°C, a discharge capacity retention rate of 80% or more was observed even at the 50th cycle.
[0427]
[0428] <SEM Observation 1> To examine the surface state of the positive electrode before and after charge-discharge cycles, three positive electrodes were prepared and subjected to SEM observation. SEM observation was performed using a Hitachi High-Technologies S4800, with the acceleration voltage fixed at 5 kV. For this observation, a new positive electrode active material (Sample 2) was prepared according to the procedure for preparing the positive electrode active material described above. For Sample 2, a muffle furnace was used instead of the roller hearth kiln simulator furnace used in Sample 1, and the other conditions were the same as for Sample 1.
[0429] <Cross-sectional SEM image> As a pretreatment for analysis, Sample 2 was thinned (to a thickness of 60 nm) by FIB. Etching was performed using gallium to thin the sample. A carbon film was formed as a protective film. A cross-sectional STEM image of Sample 2 thinned in this manner is shown in FIG. 28A.
[0430] <STEM-EDX analysis> STEM-EDX analysis was performed on the region surrounded by the dashed line in Fig. 28A. The region surrounded by the dashed line corresponds to the edge surface of Sample 2 (positive electrode active material). For the STEM-EDX analysis, for example, a STEM device (NEOARM manufactured by JEOL Ltd.) was used, and a Dual SDD detector manufactured by JEOL Ltd. was used as the EDX detector.
[0431] The distribution of oxygen, cobalt, fluorine, magnesium, nickel, and aluminum, which is the result of STEM-EDX-ray analysis, is shown in Figure 28B. The horizontal axis represents distance (nm), and the vertical axis represents atomic ratio (atomic %). The horizontal axis is superimposed at 10 nm at a position corresponding to 50% of the average detected amount of oxygen (MAVE) inside Sample 2 (positive electrode active material). 50% of the average detected amount of oxygen (MAVE) is the reference point for this measurement.
[0432] Figure 28B shows that the magnesium distribution is located in the surface layer. Specifically, the magnesium distribution starts from around 8 nm on the horizontal axis, and the magnesium concentration peaks at 11 nm on the horizontal axis. At this time, the magnesium concentration was 14 atomic %. As mentioned above, since the surface is at 10 nm on the horizontal axis, it was found that the magnesium concentration peak is located 1 nm from the reference point.
[0433] It was found from Figure 28B that the fluorine distribution was located in the surface layer. Specifically, the fluorine distribution began to rise near 8 nm on the horizontal axis and overlapped with the rise of magnesium, with the fluorine concentration peaking at 9 nm on the horizontal axis. At this time, the fluorine concentration indicated 4 atomic %. From these, the peak position of the fluorine concentration was located 2 nm on the surface side from the peak position of the magnesium concentration. It is believed that this type of fluorine distribution increases the resistance of sample 2 to hydrofluoric acid.
[0434] From Figure 28B, it was found that the nickel distribution was located in the surface layer. Specifically, the nickel distribution started to rise near 10 nm on the horizontal axis, with the nickel concentration peaking at 11 nm on the horizontal axis. At this time, the nickel concentration indicated 2 atomic %. As mentioned above, since 10 nm on the horizontal axis is the surface, it was found that the nickel concentration peak was located 1 nm from the reference point. The entire nickel distribution was superimposed on the entire magnesium distribution.
[0435] It was found from Figure 28B that aluminum was present from the surface layer to the interior. Specifically, the aluminum distribution began near 10 nm on the horizontal axis and continued deeper than the magnesium distribution, that is, into the deeper region. The aluminum concentration peak was located at 23 nm on the horizontal axis, where the aluminum concentration was 2.5 atomic %. As mentioned above, since the horizontal axis is at 10 nm, which is the surface, the aluminum concentration peak was located 13 nm from the reference point, and it was found that this position was located deeper than the concentration peaks of magnesium and other elements.
[0436] <Assembly of Coin Cell> A positive electrode containing Sample 2 was then assembled according to the procedure for preparing the positive electrode of Half Cell 1 described above. The state of Sample 2 before contact with the electrolyte, i.e., before assembly into a coin cell, is referred to as the first positive electrode and is referred to as the state before coin cell assembly. SEM observation was performed on the positive electrode before coin cell assembly. The SEM image is shown in Figure 29A. The positive electrode active material and AB were visible in the SEM image. The surface of the positive electrode active material was smooth. Cracks were also observed in the positive electrode active material. It is estimated that cracks occur after pressing at a linear pressure of 210 kN / m. AB was observed to be attached to a portion of the positive electrode active material. Because this is a layered rock salt type positive electrode active material, it is preferable that AB contact a portion of the AB plane, which is the lithium ion insertion / extraction surface.
[0437] <Charge-Discharge Cycle Test A (3 Cycles)> Next, a new positive electrode containing Sample 2 was prepared, and this positive electrode was assembled into a coin cell (referred to as Half Cell 1). The charge-discharge cycle test was started on Half Cell 1 without aging. The temperature of the thermostatic chamber was confirmed to be 25°C, and the charge-discharge cycle was repeated three times under the following charge-discharge conditions: Charge condition: 4.6 V (CCCV charge, 0.1 C rate, 0.01 C cutoff); Discharge condition: 2.5 V (CC discharge, 0.1 C rate). In this example, the current value corresponding to 1 C was 200 mA / g per weight of positive electrode active material. After the end of charge, a 10-minute rest period was allowed before the next discharge. If the cutoff current of the charge condition was not reached, the time may be cut off. The 4.6 V charge condition is called the upper limit voltage, and is maintained at the upper limit voltage during CV charging. The 2.5 V discharge condition is called the lower limit voltage.
[0438] After three cycles, the coin cell was disassembled, and the positive electrode was removed and washed. This state is referred to as the second state and is called "after three cycles." SEM observation of the positive electrode after three cycles was performed. The SEM image is shown in Figure 29B. In comparison with Figure 29A, in Figure 29B, deposits were observed near the positive electrode active material and A and B. The deposits are thought to correspond to at least decomposition products of the electrolyte.
[0439] <Aging> Next, a new positive electrode having Sample 2 was prepared, and this positive electrode was assembled into a coin cell (referred to as Half Cell 2). Aging was performed on Half Cell 2. First, Half Cell 2 was placed in a thermostatic bath for 6 hours. Since the temperature of the thermostatic bath was not controlled, the temperature of the thermostatic bath was understood to be 23°C ± 5°C. In other words, an error of ± 5°C is allowed for the temperature of the thermostatic bath that is not temperature-controlled. Then, a charge-discharge cycle was repeated twice under the following charge-discharge conditions: Charge condition: 4.6 V (CCCV charge, 0.1 C rate, 0.01 C cutoff); Discharge condition: 2.5 V (CC discharge, 0.1 C rate). In this example, the current value corresponding to 1 C was 200 mA / g per weight of positive electrode active material. After the end of charge, a 10-minute rest period was allowed before the next discharge. If the cutoff current of the charge condition is not reached, the time may be cut off. The 4.6 V charge condition is called the upper limit voltage, and is maintained at the upper limit voltage during CV charging. The discharge condition of 2.5 V is called the lower limit voltage.
[0440] <Charge-Discharge Cycle Test B (100 Cycles)> After aging, a charge-discharge cycle test was initiated on half-cell 2. The temperature of the thermostatic chamber was confirmed to be 25°C, and 100 charge-discharge cycles were repeated under the following charge-discharge conditions. Charge conditions: 4.6 V (CCCV charge, 0.5 C rate, 0.05 C cutoff). Discharge conditions: 2.5 V (CC discharge, 0.5 C rate). In this example, the current value corresponding to 1 C was 200 mA / g per weight of positive electrode active material. After charging, a 10-minute rest period was allowed before the next discharge. If the cutoff current of the charge conditions was not reached, the time was sometimes cut off. The 4.6 V charge condition is called the upper limit voltage, and is maintained at the upper limit voltage during CV charging. The 2.5 V discharge condition is called the lower limit voltage.
[0441] FIG. 30A shows the results of the discharge capacity, and FIG. 30B shows the results of the discharge capacity retention. Some of the above-mentioned charge and discharge conditions are shown in the figure. In the graph of discharge capacity, the horizontal axis represents cycles (number of times) and the vertical axis represents discharge capacity (mAh / g). The discharge capacity was measured per weight of the positive electrode active material. In the graph of the discharge capacity retention, the horizontal axis represents cycles (number of times) and the vertical axis represents discharge capacity retention (%). Table 4 shows the number of cycles at which the maximum discharge capacity was achieved, the maximum discharge capacity value, and the discharge capacity retention rate up to the fifth cycle. The cycle at which the maximum discharge capacity was achieved was the second cycle. Furthermore, it was found that the discharge capacity retention rate for each cycle up to the fifth cycle was 98% or higher, preferably 99% or higher. The maximum discharge capacity was 190 mAh / g or higher, preferably 200 mAh / g or higher, which was favorable. Thus, it was found that the battery exhibited favorable initial characteristics.
[0442]
[0443] Table 5 shows the discharge capacity retention rates at the 10th, 20th, 30th, 40th, 50th, and 100th cycles. Excellent cycle characteristics were observed. Particularly under conditions of 4.6 V and 25° C., the discharge capacity retention rate was 90% or more, preferably 91% or more, even at the 100th cycle.
[0444]
[0445] Next, after 100 cycles, the coin cell was disassembled, and the positive electrode was removed and washed. This state is referred to as the third state, "after 100 cycles." SEM observation of the positive electrode after 100 cycles was performed. Figure 29C shows the SEM image. Comparing Figures 29A and 29B, Figure 29C shows that in addition to the positive electrode active material and A and B, fine particles can be seen in the positive electrode active material, and the gaps between the A and B aggregates appear to be filled. The material filling the gaps between these particles and / or aggregates is likely a deposit derived from electrolyte decomposition products. The coating may be similar to an insulator with low electrical conductivity, which may be a factor in the decrease in discharge capacity during charge-discharge cycle testing.
[0446] <Elemental Mapping> Next, a mapping image obtained by scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX) of the surface is shown. The EDX measurement device used was an Oxford Instruments Ultim Max 170 energy dispersive X-ray analyzer, with an acceleration voltage of 3 kV to 30 kV, and a Si drift detector was used for X-ray detection. In EDX elemental analysis, the detection depth is several nm to several μm depending on the acceleration voltage, and the energy resolution is 130 eV to 140 eV.
[0447] Figure 31A shows a surface SEM image of the positive electrode before assembly of the coin cell. Figure 31B shows an oxygen mapping image in the surface SEM image of the positive electrode of Figure 31A. Figure 31C shows a fluorine mapping image in the surface SEM image of the positive electrode of Figure 31A. Figure 31D shows a carbon mapping image in the surface SEM image of the positive electrode of Figure 31A. Figure 31E shows an aluminum mapping image in the surface SEM image of the positive electrode of Figure 31A. The mapping image is created by irradiating an arbitrary area, such as a 192 pixel x 256 pixel area, with X-rays and converting the intensity of the target element into brightness. This is sometimes called area analysis. The mapping image visualizes the presence of the target element in the target area, and the bright spots in Figures 31B to 31E are considered to represent the presence of each element. However, since the presence of an element cannot be determined from the mapping image alone, it is preferable to determine the presence of the element using an energy spectrum. Figure 31F shows the energy spectrum of the area labeled Spectrum 1 in Figure 31A. The region to which spectrum 1 is attached is a region overlapping with lithium cobalt oxide, and cobalt and oxygen were also confirmed in the energy spectrum. Magnesium, aluminum, and fluorine were also confirmed in the energy spectrum. Although the energy spectrum is not shown, the energy spectrum of carbon was confirmed in the energy spectrum of the region to which spectrum 3 is attached in Figure 31A. The region to which spectrum 3 is attached is considered to be a region overlapping with AB. Note that a description of the energy spectrum of the region to which spectrum 2 is attached in Figure 31A will be omitted.
[0448] FIG. 32A shows a surface SEM image of the positive electrode after three cycles, FIG. 32B shows a mapping image of oxygen in the surface SEM image of the positive electrode of FIG. 32A, FIG. 32C shows a mapping image of fluorine in the surface SEM image of the positive electrode of FIG. 32A, FIG. 32D shows a mapping image of carbon in the surface SEM image of the positive electrode of FIG. 32A, and FIG. 32E shows a mapping image of phosphorus in the surface SEM image of the positive electrode of FIG. 32A. The mapping image corresponds to a visualization of the presence of a target element in a target region, and the bright spots in FIGS. 32B to 32E are considered to represent the presence of each element. However, since the presence of an element cannot be determined from a mapping image alone, it is desirable to determine the presence of the element using an energy spectrum. FIG. 32F shows the energy spectrum of the region marked with spectrum 1 in FIG. 32A. The region marked with spectrum 1 overlaps with lithium cobalt oxide, and cobalt and oxygen were also confirmed in the energy spectrum. Magnesium, aluminum, fluorine, and phosphorus were also confirmed in the energy spectrum. Although the energy spectrum is not shown, the energy spectrum of carbon was confirmed in the energy spectrum of the region to which spectrum 2 is added in Figure 32A. The region to which spectrum 2 is added is considered to be the region overlapping with A and B. Note that a description of the energy spectrum of the region to which spectrum 3 is added in Figure 32A will be omitted.
[0449] FIG. 33A shows a surface SEM image of the positive electrode after 100 cycles, FIG. 33B shows a mapping image of oxygen in the surface SEM image of the positive electrode of FIG. 33A, FIG. 33C shows a mapping image of fluorine in the surface SEM image of the positive electrode of FIG. 33A, FIG. 33D shows a mapping image of carbon in the surface SEM image of the positive electrode of FIG. 33A, and FIG. 33E shows a mapping image of phosphorus in the surface SEM image of the positive electrode of FIG. 33A. The mapping image corresponds to a visualization of the presence of the target element in the target region, and the bright spots in FIGS. 33B to 33E are considered to represent the presence of each element. However, since the presence of an element cannot be determined from the mapping image alone, it is desirable to determine the presence of the element using the energy spectrum. FIG. 33F shows the energy spectrum of the region marked with spectrum 1 in FIG. 33A. The region marked with spectrum 1 overlaps with lithium cobalt oxide, and cobalt and oxygen were also confirmed in the energy spectrum. Magnesium, aluminum, fluorine, and phosphorus were also confirmed in the energy spectrum. Although the energy spectrum is not shown, the energy spectrum of carbon was confirmed in the energy spectrum of the region to which spectrum 2 is added in Figure 33A. The region to which spectrum 2 is added is considered to be the region overlapping with A and B. Note that a description of the energy spectrum of the region to which spectrum 3 is added in Figure 33A will be omitted.
[0450] <XPS Measurement> Next, XPS analysis was performed on each positive electrode. The XPS measurement conditions are as follows: Measurement device: Quantera II manufactured by PHI Corporation X-ray source: Monochromated Al Kα (1486.6 eV) Detection area: 100 μmφ Detection depth: Approximately 4 to 5 nm (take-off angle 45°) Measurement spectrum: Wide scan, narrow scan of each detected element
[0451] Figure 34 shows the fluorine bonding state when XPS analysis was performed on the positive electrode after 3 cycles and after 100 cycles. The horizontal axis represents binding energy (eV). The peaks with binding energies of 682 eV to 686 eV, indicated by arrows in Figure 34, were higher than those of the positive electrode before assembly of the coin cell. The peaks of 682 eV to 686 eV are thought to be peaks due to deposits. Furthermore, the peaks of 682 eV to 686 eV are peaks due to fluorine-lithium or fluorine-magnesium bonding. When the binding energy of Mg, 1300 eV to 1310 eV, was confirmed for the positive electrode after 3 cycles and after 100 cycles, the MgO bonding peak was higher than the MgF bonding peak. It is believed that the deposits contained a large amount of MgO, and the peaks of 682 eV to 686 eV were thought to be due to fluorine and lithium.
[0452] Waveform separation and other techniques were performed on several spectra, including the above spectrum, using the accompanying software to derive the atomic ratio of each element, and the XPS analysis results shown in Table 6 were obtained. In Table 6, the atomic number of each element is shown as a percentage, with the total atomic number of C, F, Li, Co, O, P, S, N, Mg, Na, and Al in the positive electrode in each state being 100%. Note that for table purposes, the values after analysis were rounded to one decimal place. Therefore, although the total may be 99.9%, the XPS analysis was calculated assuming the total atomic number to be 100.0%.
[0453]
[0454] After 100 cycles, the cobalt ratio was detected lower than before coin cell assembly. This is thought to be due to the formation of deposits on the positive electrode active material, which obscured the surface of the lithium cobalt oxide. The deposits are also presumed to have a low cobalt concentration. The fluorine before coin cell assembly is thought to be derived from additive elements and / or binders in the positive electrode active material. The increase in fluorine after 3 and 100 cycles may be due to the electrolyte, i.e., the presence of fluorine in the deposits, but the possibility of binder contamination cannot be ruled out. Of course, the presence of binders in the deposits is also possible. Phosphorus may be derived from lithium salts. Because no lithium salts were present before coin cell assembly, the phosphorus concentration was zero. The increase in fluorine and phosphorus after 3 and / or 100 cycles compared to before coin cell assembly suggests the presence of decomposition products of lithium salts as deposits. Carbon may be derived from AB and / or the binder. Furthermore, if the sample was exposed to air, atmospheric contamination is possible. Because carbon decreased after 3 cycles and 100 cycles compared to before coin cell assembly, it is possible that deposits obscured the surface of AB. Mg originated from an additive element and was also detected before coin cell assembly. This suggests the presence of Mg on the surface of the positive electrode active material. Since Mg was detected after 3 cycles and / or 100 cycles (3 or more cycles), it is possible that Mg was detected on the surface of the positive electrode active material or that Mg was present in the deposits. Furthermore, the Mg concentration after 100 cycles was 0.9 to 1.1 times that before coin cell assembly, suggesting that the Mg concentration did not substantially decrease, and it is possible that Mg remained on the positive electrode.
[0455] Based on the results of the XPS analysis shown in Table 6, the number of Mg atoms relative to the number of Co atoms (Mg / Co), the number of F atoms relative to the number of Co atoms (F / Co), and the number of P atoms relative to the number of Co atoms (P / Co) were calculated, and the results shown in Table 7 were obtained.
[0456]
[0457] As the number of cycles increased, the ratio of F atoms to Co atoms (F / Co) and the ratio of P atoms to Co atoms (P / Co) tended to increase, while the ratio of Mg atoms to Co atoms (Mg / Co) remained almost unchanged.
[0458] <Preparation of Full Cell> Next, a full cell was prepared, and a new charge-discharge cycle test was performed. The electrolyte for the full cell was the same as that for the half cell. The positive electrode active material for the full cell was the same as that for the half cell. For the positive electrode of the full cell, a slurry was prepared in which the positive electrode active material:AB:PVDF ratio was 95:3:2 (weight ratio), and the slurry was applied to an aluminum positive electrode current collector. Then, pressing was performed at a linear pressure of 210 kN / m and 120°C. At this time, the amount of the positive electrode active material supported was approximately 10 mg / cm. 2 The separator for the full cell was the same as that for the half cell.
[0459] A full-cell negative electrode was fabricated as follows. An anode active material layer was fabricated using artificial graphite (MCMB-High rate discharge-G10 manufactured by Linyi Gelon) as the anode active material, VGCF (registered trademark) (VGCF-H manufactured by Showa Denko) as the conductive additive, SBR (TRD2001 manufactured by JSR) as the binder, and CMC (manufactured by Kishida Chemical) as the thickener. In the anode active material layer, the mixing ratio (weight ratio) of the artificial graphite, VGCF, CMC, and SBR was 96:1:1:2. The slurry corresponding to the anode active material layer used deionized water as the solvent. The slurry was coated on one side of a copper foil using a coater with a dryer, and the solvent was dried to fabricate the anode. Pressing was not performed. An aluminum laminate film was prepared as the exterior body. These were assembled to form full cell 1.
[0460] <Aging> Aging was performed on full cell 1. First, full cell 1 was left to stand in a thermostatic bath for 24 hours. Since the temperature of the thermostatic bath was not controlled at this time, the temperature of the thermostatic bath can be understood to be 23°C ± 5°C. In other words, the temperature of a thermostatic bath that is not temperature-controlled is allowed to have an error of ± 5°C. Then, aging was performed as shown in Table 8.
[0461]
[0462] <Charge-Discharge Cycle Test> After the aging, a charge-discharge cycle test was initiated. The temperature of the thermostatic chamber was confirmed to be 25°C, and the charge-discharge cycle was repeated 100 times, 300 times, or 500 times under the following charge-discharge conditions. Charge conditions: 4.47 V, 4.6 V, or 4.7 V (CCCV charge, 0.3 C rate, 0.03 C cutoff). Discharge conditions: 3.0 V (CC discharge, 0.3 C rate). In this example, the current value corresponding to 1 C was 200 mA / g per weight of positive electrode active material. After the end of charge, a 10-minute rest period was provided before the next discharge. If the cutoff current of the charge condition was not reached, the time was sometimes cut off. The 4.7 V or 4.8 V in the charge condition is called the upper limit voltage, and is maintained at the upper limit voltage during CV charge. The 3.0 V in the discharge condition is called the lower limit voltage.
[0463] Figures 35A to 35C show the results of discharge capacity, and Figures 36A to 36C show the results of discharge capacity retention. The charge / discharge conditions are also shown in each figure. In the graphs of discharge capacity, the horizontal axis represents cycles (number of times) and the vertical axis represents discharge capacity (mAh / g). The discharge capacity was measured per weight of the positive electrode active material. In the graphs of discharge capacity retention, the horizontal axis represents cycles (number of times) and the vertical axis represents discharge capacity retention (%). Table 9 shows the number of cycles at which the maximum discharge capacity was achieved, the maximum discharge capacity value, and the discharge capacity retention rate up to the fifth cycle. The cycle at which the maximum discharge capacity was achieved was within the third cycle. Furthermore, under all conditions, the discharge capacity retention rate for each cycle up to the fifth cycle was 98% or higher, preferably 99% or higher. Under all conditions, the maximum discharge capacity was 170 mAh / g or higher, preferably 180 mAh / g or higher, which was favorable. Thus, it was found that the batteries exhibited favorable initial characteristics.
[0464]
[0465] Table 10 shows the discharge capacity retention rates at the 10th, 20th, 30th, 40th, 50th, and 100th cycles. Good cycle characteristics were observed under all conditions. In particular, under the conditions of 4.47 V and 25°C, a discharge capacity retention rate of 95% or more, preferably 97% or more, was observed even at the 100th cycle. Under the charging condition of 4.47 V, a discharge capacity retention rate of 95% or more was observed even at the 400th cycle.
[0466]
[0467] <Quantitative Determination of MTFP Impurities> In this example, nuclear magnetic resonance (NMR) was used to confirm the impurities contained in MTFP. 1 Measurements were carried out using H-NMR. The nuclear magnetic resonance measurement device used was an "ADVANCE III 400" manufactured by Bruker. The device used in the above examples was designated MTFP2, and MTFP1, which was not used in the above examples, was also prepared. MTFP1 was purchased from a different manufacturer than MTFP2.
[0468] MTFP1 and MTFP2 were mixed in a deuterated acetonitrile solution and analyzed by nuclear magnetic resonance spectroscopy ( 1 The measurements were performed by H-NMR. A chart of the measurement results for MTFP1 and MTFP2 is shown in Figure 37. In Figure 37, the range of δ is shown as 0 ppm or more and 5.5 ppm or less. Figure 38A shows an enlarged view of δ from 3.2 ppm to 3.4 ppm, Figure 38B shows an enlarged view of δ from 1 ppm to 2 ppm, and Figure 38C shows an enlarged view of δ from 4 ppm to 5 ppm.
[0469] As shown in Figure 38A, a peak derived from MTFP was observed in MTFP1 and MTFP2 at δ between 3.29 ppm and 3.43 ppm. On the other hand, a clear peak was observed only in MTFP1 at δ between 3.24 ppm and 3.29 ppm. An arrow is attached to this peak in Figure 38A. This is thought to be a peak derived from impurities. Therefore, the ratio (integral ratio) of the peak area between 3.24 ppm and 3.29 ppm to the peak area between 3.29 ppm and 3.43 ppm for MTFP1 and MTFP2 was calculated. The results are shown in Table 11. For MTFP2, the integral ratio of impurities was 0.002 or less, and almost no peaks due to impurities were observed.
[0470]
[0471] Furthermore, in Figure 38B, peaks were confirmed in the areas indicated by arrows next to MTFP1 and MTFP2. These are thought to be peaks derived from impurities. Furthermore, in Figure 38C, peaks were confirmed in the areas indicated by arrows next to MTFP1 and MTFP2. These are thought to be peaks derived from impurities.
[0472] The above-mentioned impurities are thought to be raw materials or reaction by-products during the synthesis of MTFP. MTFP2 used in the above examples had fewer peaks derived from impurities than MTFP1, and was found to be a suitable electrolyte for secondary batteries.
[0473] [Explanation of symbols] 100a: surface layer portion 100b: interior, 100: positive electrode active material, 101: negative electrode current collector, 102: negative electrode active material layer, 104: positive electrode active material layer, 105: positive electrode current collector, 106: negative electrode, 107: positive electrode, 108: separator, 109: electrolyte, 110: grain boundary, 112: crack
Claims
A secondary battery including a positive electrode having a positive electrode active material and an electrolyte, The positive electrode active material includes lithium cobalt oxide, The surface layer portion of the positive electrode active material has an additive element, The additive element includes one or more selected from magnesium, aluminum, and nickel, The electrolyte comprises an organic solvent; the organic solvent comprises a fluorinated cyclic carbonate and a fluorinated chain carbonate, After repeating a charge-discharge cycle test for the secondary battery for three or more cycles, the positive electrode is removed from the secondary battery, and the additive element is detected by XPS analysis of the positive electrode. Secondary battery. A secondary battery including a positive electrode having a positive electrode active material and an electrolyte, The positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material containing magnesium, The electrolyte comprises an organic solvent; the organic solvent comprises a fluorinated cyclic carbonate and a fluorinated chain carbonate, After repeating a charge-discharge cycle test for the secondary battery for three or more cycles, the positive electrode is removed from the secondary battery, and magnesium is detected by XPS analysis of the positive electrode. Secondary battery. A secondary battery including a positive electrode having a positive electrode active material and an electrolyte, The positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material containing magnesium, The electrolyte comprises an organic solvent; the organic solvent comprises a fluorinated cyclic carbonate and a fluorinated chain carbonate, After repeating a charge-discharge cycle test for 100 cycles on the secondary battery, the positive electrode is removed from the secondary battery, and magnesium is detected by XPS analysis of the positive electrode. Secondary battery. A secondary battery including a positive electrode having a positive electrode active material and an electrolyte, The positive electrode active material includes lithium cobalt oxide, The surface layer portion of the positive electrode active material has an additive element, The additive element includes one or more selected from magnesium, aluminum, and nickel, The electrolyte comprises an organic solvent; the organic solvent contains fluoroethylene carbonate and methyl trifluoropropionate, and when the total volume of the fluoroethylene carbonate and the methyl trifluoropropionate is taken as 100 vol%, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is y:100-y (5≦y≦30); After repeating a charge-discharge cycle test on the secondary battery for three or more cycles, the positive electrode is removed from the secondary battery, and an additive element is detected in an XPS analysis of the positive electrode. Secondary battery. A secondary battery including a positive electrode having a positive electrode active material and an electrolyte, The positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material containing magnesium, The electrolyte comprises an organic solvent; the organic solvent contains fluoroethylene carbonate and methyl trifluoropropionate, and when the total volume of the fluoroethylene carbonate and the methyl trifluoropropionate is taken as 100 vol%, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is y:100-y (5≦y≦30); After repeating a charge-discharge cycle test on the secondary battery for three or more cycles, the positive electrode is removed from the secondary battery, and magnesium is detected in an XPS analysis of the positive electrode. Secondary battery. A secondary battery including a positive electrode having a positive electrode active material and an electrolyte, The positive electrode active material includes lithium cobalt oxide, a surface layer portion of the positive electrode active material containing magnesium, The electrolyte comprises an organic solvent; the organic solvent contains fluoroethylene carbonate and methyl trifluoropropionate, and when the total volume of the fluoroethylene carbonate and the methyl trifluoropropionate is taken as 100 vol%, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is y:100-y (5≦y≦30); After repeating a charge-discharge cycle test for 100 cycles on the secondary battery, the positive electrode is removed from the secondary battery, and magnesium is detected in an XPS analysis of the positive electrode. Secondary battery. In any one of claims 1 to 6, The lithium cobalt oxide is Li x CoO 2 It is expressed as The Li x CoO 2 When x is 1, the lithium cobaltate has a layered rock-salt crystal structure belonging to the space group R-3m; The Li x CoO 2 When x is 0.1<x≦0.24, the lithium cobalt oxide is space group P2 / m, a=0.4880±0.005nm, b=0.2817±0.005nm, c=0.4839±0.005nm, α=90°, β=109.6±0.1°, A secondary battery having a crystal structure of γ=90°. In any one of claims 1 to 6, The lithium cobalt oxide is Li x CoO 2 It is expressed as The Li x CoO 2 When x is 1, the lithium cobaltate has a layered rock-salt crystal structure belonging to the space group R-3m; The Lix CoO 2 When x is 0.1<x≦0.24, the lithium cobalt oxide is analyzed by XRD to have at least 2θ=19.37° or more and 19.57° or less; A secondary battery having a diffraction peak at 2θ=45.57° or more and 45.67° or less.
Citation Information
Patent Citations
Electrode active material, method of preparing the same, electrode for lithium secondary battery which includes the same, and lithium secondary battery using the electrode
US20120301788A1
Electrode active material for lithium secondary battery, method of preparing the electrode active material, electrode for lithium secondary battery including the same, and lithium secondary battery using the same
US20130089786A1
Nonaqueous electrolyte for rechargeable battery and rechargeable battery with nonaqueous electrolyte
WO2008102493A1
Non-aqueous electrolyte for secondary battery, and non-aqueous electrolyte secondary battery
WO2008102638A1
Nonaqueous electrolyte secondary battery
WO2015004841A1