Nonaqueous electrolytic solution and nonaqueous electrolytic solution battery including nonaqueous electrolytic solution

The use of a specific fluorosilane and anion-containing compound in the non-aqueous electrolyte of lithium-ion batteries forms a composite film to mitigate thermal decomposition, addressing gas generation and internal resistance issues at high temperatures and ensuring stable battery performance.

WO2024228316A1PCT designated stage expired Publication Date: 2024-11-07MU IONIC SOLUTIONS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013922
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-01
Filing Date
2024-04-04
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries face significant gas generation and increased internal resistance when operated at high temperatures due to thermal decomposition of traditional non-aqueous electrolytes, leading to capacity retention issues.

Method used

A non-aqueous electrolyte battery containing a specific fluorosilane compound and an anion-containing compound with a specific mass ratio, which forms a composite film on the electrode surface to suppress electrolyte decomposition and reduce gas generation, while maintaining capacity retention and preventing internal resistance increases.

Benefits of technology

The solution effectively reduces gas generation and maintains capacity retention and internal resistance stability at high temperatures, enhancing the performance of lithium-ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013922_07112024_PF_FP_ABST
    Figure JP2024013922_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a nonaqueous electrolytic solution containing an electrolyte, a nonaqueous solvent, a compound represented by general formula (I), and at least one specific anion-containing compound selected from an anion-containing compound having a P=O bond and a P-F bond, an anion-containing compound having an S=O bond and an S-F bond, and an alkyl sulfate anion-containing compound, wherein the mass ratio between the compound represented by general formula (I) and the specific anion-containing compound satisfies a specific range. The present invention also relates to a nonaqueous electrolytic solution battery comprising a negative electrode and a positive electrode capable of occluding and releasing metal ions, and the nonaqueous electrolytic solution.
Need to check novelty before this filing date? Find Prior Art

Description

Non-aqueous electrolyte, non-aqueous electrolyte battery containing the non-aqueous electrolyte

[0001] The present invention relates to a non-aqueous electrolyte and a non-aqueous electrolyte battery containing the non-aqueous electrolyte.

[0002] Non-aqueous electrolyte batteries such as lithium ion secondary batteries have been put to practical use in a wide range of applications, such as power sources for so-called small consumer devices such as mobile phones such as smartphones and laptop computers, and on-board power sources for driving electric vehicles, etc. Therefore, numerous studies have been conducted in the fields of positive and negative electrode active materials and non-aqueous electrolyte additives as means for improving the battery characteristics of non-aqueous electrolyte batteries.

[0003] In recent years, efforts to increase the capacity of lithium-ion secondary batteries have been accelerating, and in addition to the introduction of high-capacity active materials with a large theoretical capacity per mass of electrode active material (for example, lithium transition metal composite oxides with a high Ni ratio in the transition metals and Si-based active materials), studies are being conducted to increase the energy density of batteries by increasing the charging voltage of the battery. Furthermore, the applications of lithium-ion batteries are becoming more diverse, and stable operation in higher temperature environments than before is required. Non-aqueous electrolytes generally contain LiPF 6 is used as the electrolyte, but LiPF 6 It has been reported that LiPF undergoes thermal decomposition at temperatures above 68°C (Journal of Power Sources, 2006, Vol. 156, pp. 555-559). It has also been revealed that the decomposition products react with carbonate, a component of the electrolyte, and the decomposition reaction of carbonate proceeds (Journal of the Electrochemical Society, 2005, Vol. 152, No. 12, pp. A2327-A2334). Therefore, when the operating temperature of a lithium-ion secondary battery is 70°C or higher, in addition to the decomposition of the electrolyte on the electrodes, LiPF 6 Since the decomposition of the electrolyte occurs due to the thermal decomposition of the electrolyte, the deterioration is more significant than when the battery is operated at a temperature below 70°C, and gas generation and an increase in the internal resistance of the battery during operation at high temperatures become more pronounced.

[0004] Patent Document 1 discloses a nonaqueous electrolyte for secondary batteries that can improve the discharge capacity retention rate and suppress the internal resistance increase rate in a 60° C. cycle test by including a difluorosilane compound having a cycloalkyl group in the electrolyte. Patent Document 2 discloses a lithium ion secondary battery that can suppress capacity reduction and gas generation in a 25° C. cycle test by combining an electrolyte containing a difluorosilane compound having a specific structure with a positive electrode made of a lithium transition metal composite oxide with a Ni content of 70% or more.

[0005] JP 2011-222450 A U.S. Patent Application Publication No. 2019 / 0305372

[0006] However, the secondary battery using the nonaqueous electrolyte for secondary batteries described in Patent Document 1 and the lithium-ion secondary battery described in Patent Document 2 were not able to sufficiently suppress the decrease in capacity retention rate and the increase in internal resistance, and to reduce the amount of gas generation, when stored at temperatures of 70°C or higher. The present invention aims to provide a nonaqueous electrolyte battery that can reduce the amount of gas generation while suppressing the decrease in capacity retention rate and the increase in internal resistance when operated at high temperatures. Here, "amount of gas generation" refers to the amount of gas generated by decomposition of the solvent and additives, which are components of the electrolyte, on the electrodes.

[0007] As a result of extensive research aimed at solving the above-mentioned problems, the present inventors have discovered that a nonaqueous electrolyte solution containing a specific fluorosilane compound and a specific anion-containing compound can suppress a decrease in capacity retention and an increase in internal resistance while reducing the amount of gas generated when a nonaqueous electrolyte battery is operated at high temperatures, when the number of fluorine atoms bonded to silicon atoms in the specific fluorosilane compound, the content of the specific fluorosilane compound relative to the entire nonaqueous electrolyte solution, and the content of the specific anion-containing compound relative to the entire nonaqueous electrolyte solution satisfy a specific relationship, thereby completing the present invention. Specifically, the present invention relates to the following [1] to [9]. [1] A nonaqueous electrolyte solution containing an electrolyte, a nonaqueous solvent, a compound represented by general formula (I), and at least one specific anion-containing compound selected from an anion-containing compound having a P═O bond and a P—F bond, an anion-containing compound having an S═O bond and an S—F bond, and an alkyl sulfate anion-containing compound, wherein the nonaqueous electrolyte solution satisfies the following mathematical formula (II): (In formula (I), R 1 represents an alkyl group having 5 to 10 carbon atoms which may be substituted with a halogen atom, and R 2 represents an alkyl group having 1 to 4 carbon atoms which may be substituted with a halogen atom, and n represents an integer of 1 to 3. 0<Z≦8 / n 2 (II) (In formula (II), Z represents the mass ratio (=[A] / [B]) of the content [A] of the compound represented by general formula (I) in the non-aqueous electrolyte to the content [B] of the specific anion-containing compound in the non-aqueous electrolyte, and n represents n of the compound represented by general formula (I).) [2] In the general formula (I), R 2is a methyl group. [3] The nonaqueous electrolyte solution according to [1] or [2], wherein n is 1 or 2 in the general formula (I). [4] The nonaqueous electrolyte solution according to any one of [1] to [3], wherein the specific anion-containing compound is an anion-containing compound having a P═O bond and a P—F bond. [5] The nonaqueous electrolyte solution according to any one of [1] to [4], wherein the content of the compound represented by the general formula (I) is 0.001 to 10 mass % with respect to the total amount of the nonaqueous electrolyte solution. [6] The nonaqueous electrolyte solution according to any one of [1] to [5], wherein the content of the specific anion-containing compound is 0.001 to 5 mass % with respect to the total amount of the nonaqueous electrolyte solution. [7] A nonaqueous electrolyte battery comprising a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and a nonaqueous electrolyte solution, wherein the nonaqueous electrolyte solution is the nonaqueous electrolyte solution according to any one of [1] to [6]. [8] The nonaqueous electrolyte battery according to [7], wherein the positive electrode contains a positive electrode active material, and the positive electrode active material is a lithium transition metal oxide represented by the following composition formula (1): Li 1+y M 1 O 2 (1) (In the composition formula (1), y is −0.2 to 0.5, and M 1 represents a plurality of elements including at least Ni element, and M 1 The molar ratio of the content of Ni element to the content of all elements contained in 1 ) is 0.40 to 1.0. [9] The nonaqueous electrolyte battery according to [8], wherein the positive electrode active material is a lithium transition metal composite oxide represented by the following composition formula (2): Li a1 Ni b1 M 2 c1 O 2 ... (2) (In the composition formula (2), a1, b1, and c1 are numerical values ​​that satisfy 0.80≦a1≦1.10, 0.40≦b1≦0.99, and 0.01≦c1≦0.60, and b1+c1=1 is satisfied. M 2 contains at least one element selected from the group consisting of Co, Mn, Al, Mg, Zr, Fe, Ti and Er.

[0008] According to the present invention, it is possible to provide a nonaqueous electrolyte battery that can reduce the amount of gas generated when operated at high temperatures while suppressing a decrease in capacity retention rate and an increase in internal resistance when the nonaqueous electrolyte battery is operated at high temperatures.

[0009] In this specification, "α to β" or "α-β" means a numerical range of α or more and β or less.

[0010] The mechanism by which the nonaqueous electrolyte of the present invention can reduce the amount of gas generation while suppressing a decrease in capacity retention and an increase in internal resistance when a nonaqueous electrolyte battery is operated at high temperatures is not clear, but is thought to be as follows. The compound represented by general formula (I) has a structure in which a fluorine atom is bonded to a silicon atom within the molecule. When a fluorine atom is bonded to a silicon atom, the electron density of the silicon atom decreases, and the reactivity of the silicon atom in the compound represented by general formula (I) increases. Because a specific anion-containing compound has an anionic moiety, it reacts with a compound represented by general formula (I) having a silicon atom with low electron density to form a composite coating on the surface of the electrode active material. It is thought that the composite coating suppresses decomposition of the electrolyte on the electrode, thereby suppressing a decrease in capacity retention and an increase in internal resistance when a nonaqueous electrolyte battery is operated at high temperatures, while reducing the amount of gas generation. The composite coating is made of LiPF , which is commonly used as an electrolyte. 6 It is believed that the further decomposition reaction of the decomposition products produced by the thermal decomposition of (I) on the electrode can be suitably suppressed, thereby achieving the effects of the present invention. The electron density of the silicon atom in the compound represented by general formula (I) decreases roughly in proportion to the integer n. In addition, the steric hindrance around the silicon atom in the compound represented by general formula (I) decreases roughly in proportion to the integer n. Therefore, the reaction activity of the compound represented by general formula (I) is roughly n 2 Therefore, as shown in formula (II), there is a suitable range for the ratio Z of the compound represented by general formula (1) to the specific anion-containing compound, depending on n. When Z is within the range represented by formula (II), it is believed that the thickness of the composite coating can be suitably controlled, and the amount of gas generated from the battery during operation at high temperatures can be significantly reduced. In addition, the compound represented by general formula (I) has an alkyl group (R 1) The appropriate steric hindrance allows the density of the composite coating to be suitably controlled, which contributes to suppressing an increase in the battery's internal resistance. Examples of the nonaqueous electrolyte battery of the present invention include polyvalent cation batteries, metal-air secondary batteries, and secondary batteries using s-block metals other than those mentioned above. Nonaqueous electrolyte secondary batteries are preferred, and lithium ion secondary batteries are more preferred.

[0011] <1. Non-aqueous Electrolyte Solution> The non-aqueous electrolytic solution according to the present invention contains an electrolyte, a non-aqueous solvent, a fluorosilane compound represented by general formula (I), and a specific anion-containing compound, and the mass ratio of the compound represented by general formula (I) to the specific anion-containing compound satisfies a specific range. Each component will be described below.

[0012] [1-1. Compound represented by general formula (I)]

[0013]

[0014] In general formula (I), R 1 represents an alkyl group having 5 to 10 carbon atoms which may be substituted with a halogen atom, and R 2 represents an alkyl group having 1 to 4 carbon atoms which may be substituted with a halogen atom; and n represents an integer of 1 to 3.

[0015] R 1 Examples of the alkyl group having 5 to 10 carbon atoms represented by the formula (I) include a linear or branched chain alkyl group, a cycloalkyl group having a cyclic structure, and a halogenated alkyl group in which at least one hydrogen atom of the alkyl group is substituted with a halogen atom.

[0016] The R 1Examples of the linear alkyl group having 5 to 10 carbon atoms include an n-pentyl group, a methylbutyl group, an n-hexyl group, a methylpentyl group, an n-heptyl group, a methylhexyl group, an n-octyl group, a methylheptyl group, an n-nonyl group, a methyloctyl group, an n-decyl group, and a methylnonyl group. Among these, a linear alkyl group having 5 to 10 carbon atoms such as an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, or an n-decyl group is preferred, and a linear alkyl group having 5 to 8 carbon atoms such as an n-pentyl group, an n-hexyl group, an n-heptyl group, or an n-octyl group is more preferred. The linear alkyl groups described above are preferred because they suppress side reactions of the compound represented by general formula (I) on the surface of the electrode active material.

[0017] The R 1 Examples of the cycloalkyl group having 5 to 10 carbon atoms include a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, a cyclodecyl group, a cyclohexylmethyl group, a cyclohexylethyl group, a methylcyclohexyl group, a dimethylcyclohexyl group, an ethylcyclohexyl group, and a methylcyclohexylmethyl group. Among these, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group are preferred, and a cyclopentyl group and a cyclohexyl group are more preferred. The above-mentioned cycloalkyl groups are preferred because they suppress side reactions of the compound represented by general formula (I) on the surface of the electrode active material.

[0018] The R 1 Examples of the halogenated alkyl group having 5 to 10 carbon atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, with a fluorine atom and a chlorine atom being preferred, and a fluorine atom being more preferred. Examples of the halogenated alkyl group having 5 to 10 carbon atoms include a 5-fluoropentyl group, a 6-fluorohexyl group, a 5,5-difluoropentyl group, and a 5,5,5-trifluoropentyl group.

[0019] The R 1The number of carbon atoms is preferably 6 to 9, more preferably 6 to 8. When the alkyl group is one of the above, the density of the composite coating film formed is suitably controlled due to the appropriate steric hindrance of the compound represented by general formula (I), which contributes to suppressing an increase in the internal resistance of the battery.

[0020] R 2 Examples of the alkyl group having 1 to 4 carbon atoms represented by the formula (I) include a linear or branched chain alkyl group, a cycloalkyl group having a cyclic structure, and a halogenated alkyl group in which at least one hydrogen atom of the alkyl group is substituted with a halogen atom.

[0021] The R 2 Examples of the linear alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, a methylethyl group, an n-butyl group, a 1-methylpropyl group, a 2-methylpropyl group, a dimethylethyl group (tert-butyl group), etc. Among these, a linear alkyl group having 1 to 4 carbon atoms is preferred, a methyl group and an ethyl group are more preferred, and a methyl group is particularly preferred.

[0022] The R 2 Examples of the cycloalkyl group include a cyclopropyl group and a cyclobutyl group.

[0023] The R 2 Examples of the halogenated alkyl group having 1 to 4 carbon atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, with a fluorine atom and a chlorine atom being preferred, and a fluorine atom being more preferred. Examples of the halogenated alkyl group having 1 to 4 carbon atoms include a trifluoromethyl group, a 2,2,2-trifluoroethyl group, a 3-fluoropropyl group, a 3,3-difluoropropyl group, a 3,3,3-trifluoropropyl group, a heptafluoropropyl group, a 3-chloropropyl group, and a 2-chloro-3,3,3-trifluoropropyl group.

[0024] The above-mentioned R 2Among these, a chain alkyl group having 1 to 4 carbon atoms is preferred, a linear alkyl group having 1 to 4 carbon atoms is more preferred, a methyl group and an ethyl group are even more preferred, and a methyl group is most preferred. These alkyl groups reduce steric hindrance around the silicon atom, which is the reactive site of the compound represented by general formula (I), and the reaction with the specific anion-containing compound proceeds favorably, making it easier to form a composite coating on the surface of the electrode active material.

[0025] n represents the number of fluorine atoms bonded to silicon atoms in the compound represented by general formula (I) and represents an integer of 1 to 3. That is, when n is 1, Si in general formula (I) is Si—R 1 one Si—F bond, one Si—R bond 2 When n is 2, Si in general formula (I) is Si—R 1 One bond, two Si-F bonds, and one Si-R bond 2 When n is 3, Si in the general formula (I) is Si—R 1 There is one Si-F bond, three Si-R bonds, and 2 No bond is present. n is preferably 1 or 2. Within this range, the compound represented by general formula (I) and the specific anion-containing compound react favorably to form a composite coating. In particular, when n is 2, the suppression of gas generation during operation at high temperatures is excellent, and when n is 1, the balance between the capacity retention rate and the suppression of gas generation during operation at high temperatures is excellent.

[0026] Examples of the compound represented by general formula (I) are shown in formulas (F1-1) to (F1-28), (F2-1) to (F2-28), and (F3-1) to (F3-28). The compound represented by general formula (I) is not particularly limited to the following examples.

[0027]

[0028]

[0029]

[0030]

[0031]

[0032]

[0033]

[0034]

[0035] Among the above compounds, from the viewpoint of optimizing the reactivity of the compound represented by general formula (I) and reacting with the specific anion-containing compound to form a suitable composite coating, a compound selected from the group of compounds represented by formulas (F1-1) to (F1-28) and (F2-1) to (F2-28) in which n is 1 or 2 is preferred, and R 1 is an unsubstituted chain alkyl group having 5 to 10 carbon atoms or a cycloalkyl group having 5 to 10 carbon atoms, and R 2 is a methyl group, and n is 1 or 2. More preferred are compounds selected from the group of compounds represented by formulas (F1-1) to (F1-7), (F1-11) to (F1-17), (F2-1) to (F2-7), and (F2-11) to (F2-17).

[0036] The content of the compound represented by the general formula (I), relative to the total amount of the non-aqueous electrolyte, is usually 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more. Also, it is usually 10% by mass or less, preferably 8.0% by mass or less, more preferably 5.0% by mass or less. Furthermore, the content of the compound represented by the general formula (I), relative to the total amount of the non-aqueous electrolyte, is usually 0.001 to 10% by mass, preferably 0.01 to 8.0% by mass, more preferably 0.1 to 5.0% by mass, and even more preferably 0.2 to 5.0% by mass. When n is 1, the content of the compound represented by the general formula (I), relative to the total amount of the non-aqueous electrolyte, is preferably in the range of 0.01 to 10.0% by mass, and particularly preferably 0.5 to 8.0% by mass. When n is 2, the content of the compound represented by general formula (I) is preferably 0.01 to 5.0% by mass, particularly preferably 0.1 to 2.0% by mass, relative to the total amount of the non-aqueous electrolyte. When n is 3, the content of the compound represented by general formula (I) is preferably 0.1 to 3.0% by mass, particularly preferably 0.1 to 1.0% by mass, relative to the total amount of the non-aqueous electrolyte. If the content of the compound represented by general formula (I) relative to the total amount of the non-aqueous electrolyte is within the above range, the concentration of the compound represented by general formula (I) on the electrode active material surface proceeds favorably, making it easier to form a composite coating on the electrode active material surface, thereby enabling the production of a battery that has an excellent balance between suppressing the amount of gas generation and suppressing internal resistance during operation at high temperatures.

[0037] The compound represented by the general formula (I) can be produced by a known method. For example, various fluorosilane compounds can be synthesized by fluorinating a chlorosilane compound or an alkoxysilane compound with a metal fluoride, boron trifluoride, a boron trifluoride complex, anhydrous hydrogen fluoride, hydrofluoric acid, or the like.

[0038] [1-2. Specific Anion-Containing Compound] The specific anion-containing compound is at least one selected from an anion-containing compound having a P═O bond and a P—F bond, an anion-containing compound having an S═O bond and an S—F bond, and an alkyl sulfate anion-containing compound.

[0039] The specific anion-containing compound is usually an acid or a salt, and preferably a salt, and the counter cation is preferably an alkali metal cation such as lithium, sodium, or potassium, and more preferably a lithium cation.

[0040] At least one anion-containing compound selected from an anion-containing compound having a P═O bond and a P—F bond, an anion-containing compound having an S═O bond and an S—F bond, and an alkyl sulfate anion-containing compound can be used alone or in combination of two or more in any ratio. Among these, an anion-containing compound having a P═O bond and a P—F bond is preferred from the viewpoint of suppressing an increase in the amount of gas generated during operation at high temperatures.

[0041] [1-2-1. Anion-containing compound having a P═O bond and a P—F bond] Examples of anion-containing compounds having a P═O bond and a P—F bond include PO 3 F 2- monofluorophosphate anions such as PO 2 F 2 - Among these, compounds containing difluorophosphate anions are preferred from the viewpoint of the balance between the output characteristics of the battery and the protection of the electrode interface.

[0042] [1-2-2. Anion-containing compound having an S═O bond and an S—F bond] Examples of anion-containing compounds having an S═O bond and an S—F bond include FSO 3 - Fluorosulfonate anions such as (FSO 2 ) 2 N - , (FSO 2 ) (CF 3 SO 2 ) N - Fluorosulfonylimide anions such as (FSO 2 ) 3 C -Examples of suitable anion-containing compounds include compounds containing fluorosulfonylmethide anions such as those listed above. However, in the present invention, the anion-containing compounds having an S═O bond and an S—F bond do not include alkyl sulfate anion-containing compounds. Among these, from the viewpoint of the balance between the output characteristics of the battery and the protection of the electrode interface, compounds containing fluorosulfonate anions or fluorosulfonylimide anions are preferred, and compounds containing fluorosulfonate anions are more preferred.

[0043] [1-2-3. Alkyl sulfate anion-containing compound] Examples of alkyl sulfate anion-containing compounds include CH 3 SO 4 - , C.H. 3 CH 2 SO 4 - Examples of compounds include those containing alkyl sulfate anions having 1 to 4 carbon atoms, such as:

[0044] (Content of specific anion-containing compound) When the non-aqueous electrolytic solution contains a specific anion-containing compound, the content of the specific anion-containing compound (total amount when two or more types are used) in the total amount of the non-aqueous electrolytic solution is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, even more preferably 0.02 mass% or more, still more preferably 0.03 mass% or more, particularly preferably 0.04 mass% or more, particularly preferably 0.05 mass% or more, and most preferably 0.1 mass% or more, and also preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less. Furthermore, when the non-aqueous electrolyte solution contains a specific anion-containing compound, the content of the specific anion-containing compound (total amount when two or more types are used) in the total amount of the non-aqueous electrolyte solution is preferably 0.001 to 5 mass%, more preferably 0.01 to 4 mass%, even more preferably 0.02 to 3 mass%, especially preferably 0.04 to 3 mass%, particularly preferably 0.05 to 3 mass%, and most preferably 0.1 to 3 mass%. When the content of the specific anion-containing compound is within the above range, the battery characteristics, particularly the direct current resistance (DCR) retention rate during operation at high temperatures, can be improved, and an increase in the amount of gas generated during operation at high temperatures can be suppressed. While the reason for this is unclear, it is thought that when the content of the specific anion-containing compound is within the above mass ratio range, side reactions of the components of the non-aqueous electrolyte solution on the electrode can be minimized. The identification and content measurement of the specific anion-containing compound are performed using nuclear magnetic resonance (NMR) spectroscopy.

[0045] (Electrolyte and specific anion-containing compound mass ratio) The mass ratio of the content of the specific anion-containing compound (total amount if two or more) to the content of the electrolyte in the non-aqueous electrolyte solution (specific anion-containing compound [g] / electrolyte [g]) is usually 0.00005 or more, preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, even more preferably 0.025 or more, and also usually 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, even more preferably 0.35 or less. Also, the mass ratio (specific anion-containing compound [g] / electrolyte [g]), usually 0.00005 to 0.5, preferably 0.001 to 0.45, more preferably 0.01 to 0.4, even more preferably 0.02 to 0.35, even more preferably 0.025 to 0.35. When the mass ratio is within the above range, the battery characteristics, particularly the DCR maintenance rate during operation at high temperatures, can be improved, and an increase in the amount of gas generated during operation at high temperatures can be suppressed. Although the reason for this is not clear, it is thought that by containing a specific anion-containing compound and an electrolyte within the above mass ratio range, side reactions of the electrolyte in the battery system can be minimized.

[0046] [1-3. Relationship between the compound represented by general formula (I) and the specific anion-containing compound] The compound represented by general formula (I) and the specific anion-containing compound in the nonaqueous electrolyte solution of the present invention satisfy the following mathematical formula (II): 0<Z≦8 / n 2 (II)

[0047] In formula (II), Z represents the mass ratio (= [A] / [B]) of the content [A] of the compound represented by general formula (I) in the non-aqueous electrolyte to the content [B] of the specific anion-containing compound in the non-aqueous electrolyte, and n represents n in the compound represented by general formula (I). When a non-aqueous electrolyte contains multiple compounds represented by general formula (I), the content of the compound represented by general formula (I) with the highest content is defined as [A]. When a non-aqueous electrolyte contains multiple specific anion-containing compounds, the total amount of all specific anion-containing compounds is defined as [B].

[0048] Z is 8 / n 2 The following numerical value is 7 / n 2 Preferably, it is equal to or less than 6 / n2 More preferably, it is 5 / n 2 More preferably, it is 4.5 / n 2 Within this range, the thickness of the composite coating comprising the compound represented by general formula (I) and the specific anion-containing compound can be suitably controlled, and when the nonaqueous electrolyte battery is operated at high temperatures, a decrease in capacity retention rate and an increase in internal resistance can be suppressed, and the amount of gas generation can be reduced.

[0049] Z is 0 (i.e., 0 / n 2 ) and is a number greater than 0.01 / n 2 It is preferable that the ratio is 0.05 / n or more. 2 More preferably, it is 0.1 / n or more. 2 More preferably, it is 0.6 / n or more. 2 More preferably, it is 0.8 / n or more. 2 More preferably, it is 1.0 / n or more. 2 More preferably, it is 1.2 / n 2 More preferably, it is 1.5 / n 2 Within this range, the compound represented by general formula (I) and the specific anion-containing compound react to form a suitable composite coating on the surface of the electrode active material.

[0050] Also, Z is greater than 0 and is equal to 8 / n 2 The following numerical value is 0.01 / n 2 ~7 / n 2 It is preferable that the ratio is 0.05 / n 2 ~6 / n 2 More preferably, 0.1 / n 2 ~6 / n 2 More preferably, 0.6 / n 2 ~6 / n 2 More preferably, 0.8 / n 22 ~6 / n 2 More preferably, 1.0 / n 2 ~5 / n 2 More preferably, 1.2 / n 2 ~5 / n 2More preferably, 1.5 / n 2 ~4.5 / n 2 It is particularly preferred that:

[0051] [1-4. Electrolyte] Preferred examples of the electrolyte for the non-aqueous electrolyte solution include alkali metal salts such as lithium salts, sodium salts, and potassium salts. When the non-aqueous electrolyte solution of the present invention is used in a lithium ion battery, the counter cation in the electrolyte is preferably a lithium cation. When the non-aqueous electrolyte solution of the present invention is used in a sodium ion battery, the counter cation in the electrolyte is preferably a sodium ion. When the non-aqueous electrolyte solution of the present invention is used in a potassium ion battery, the counter cation in the electrolyte is preferably a potassium ion.

[0052] The lithium salt is not particularly limited, and examples thereof include lithium fluoroborates, lithium fluorophosphates, lithium tungstates, lithium carboxylates, lithium sulfonates, lithium imide salts, lithium methide salts, lithium oxalate salts, and fluorine-containing organic lithium salts, excluding anion-containing compounds having a P═O bond and a P—F bond, anion-containing compounds having an S═O bond and an S—F bond, and alkyl sulfate anion-containing compounds.

[0053] Among these, from the viewpoint of improving low-temperature output characteristics, high-rate charge / discharge characteristics, impedance characteristics, high-temperature storage characteristics, cycle characteristics, etc., LiBF is used as a lithium fluoroborate salt. 4 LiPF as lithium fluorophosphate 6 ; CH as lithium sulfonate salt 3 SO 3 Li; LiN(CF) as a lithium imide salt 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , lithium cyclic 1,2-perfluoroethanedisulfonylimide, lithium cyclic 1,3-perfluoropropanedisulfonylimide; lithium methide salts such as LiC(CF 3SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 As the lithium oxalate salt, lithium difluorooxalatoborate, lithium bis(oxalato)borate, lithium tetrafluorooxalatophosphate, lithium difluorobis(oxalato)phosphate, lithium tris(oxalato)phosphate, etc. are preferred, and LiPF 6 and lithium bis(oxalato)borate, and LiPF 6 is particularly preferred.

[0054] The electrolytes can be used alone or in combination of two or more in any ratio. There is no particular limitation on the combination of two or more electrolytes, and LiPF 6 and LiBF 4 The combination of LiPF 6 and LiN(CF 3 SO 2 ) 2 Among these, LiPF 6 and LiBF 4 The combination of two or more electrolytes and LiPF 6 When using two or more electrolytes, LiPF 6 It is preferable that the content of

[0055] The sodium salt is not particularly limited, and examples thereof include sodium fluoroborates, sodium fluorophosphates, sodium tungstates, sodium carboxylates, sodium sulfonates, sodium imide salts, sodium methide salts, sodium oxalate salts, and fluorine-containing organic sodium salts, excluding anion-containing compounds having a P═O bond and a P—F bond, anion-containing compounds having an S═O bond and an S—F bond, and alkyl sulfate anion-containing compounds.

[0056] Among these, from the viewpoint of improving low-temperature output characteristics, high-rate charge / discharge characteristics, impedance characteristics, high-temperature storage characteristics, cycle characteristics, etc., sodium fluoroborate, NaBF 4 Fluorophosphate sodium salt: NaPF 6 ; CH as sulfonic acid sodium salt 3 SO 3 Na; NaN(CF) as sodium imide salt 3 SO 2 ) 2 , NaN(C 2 F 5 SO 2 ) 2 , sodium cyclic 1,2-perfluoroethanedisulfonylimide, sodium cyclic 1,3-perfluoropropanedisulfonylimide; as sodium methide salts, NaC(CF 3 SO 2 ) 3 , NaC(C 2 F 5 SO 2 ) 3 As the sodium oxalate salt, sodium difluorooxalatoborate, sodium bis(oxalato)borate, sodium tetrafluorooxalatophosphate, sodium difluorobis(oxalato)phosphate, sodium tris(oxalato)phosphate, etc. are preferred, and NaPF 6 and sodium bis(oxalato)borate, and NaPF 6 is particularly preferred.

[0057] The other compounds that can be used as the electrolyte can be used alone or in combination of two or more in any ratio. The combination of two or more other compounds that can be used as the electrolyte is not particularly limited, and may be NaPF 6 and NaBF 4 A combination of NaPF 6 and NaN(CF 3 SO 2 ) 2 Among these, NaPF 6 and NaBF 4The combination is preferred.

[0058] Examples of potassium salts include those in which Li and Na in the above lithium salts and sodium salts are substituted with potassium (K).

[0059] The total concentration of the electrolyte is not particularly limited, but from the viewpoint of ensuring that the electrical conductivity ensures proper battery operation and sufficient output characteristics, it is typically 8% by mass or more, preferably 8.5% by mass or more, more preferably 9% by mass or more, and typically 18% by mass or less, preferably 17% by mass or less, more preferably 16% by mass or less, based on the total amount of the nonaqueous electrolyte solution. Furthermore, the total concentration of the electrolyte is typically 8 to 18% by mass, preferably 8.5 to 17% by mass, more preferably 9 to 16% by mass, based on the total amount of the nonaqueous electrolyte solution. However, when an electrolyte compound corresponding to [1-2. Specific Anion-Containing Compound] and [1-6. Auxiliary Agent] is contained in a nonaqueous electrolyte solution, an electrolyte other than the specific anion-containing compound and the lithium salt corresponding to the auxiliary agent must be contained. Furthermore, when the content of the above electrolyte compound is 5.0% by mass or less, it is classified as an "auxiliary agent" in this specification. Therefore, even if the "specific anion-containing compound" and the "compound corresponding to the auxiliary agent" are considered to be "electrolytes" as components of the nonaqueous electrolyte solution of this embodiment, the amount of the "electrolyte" does not include the amounts of the "specific anion-containing compound" and the "compound corresponding to the auxiliary agent." The electrolyte is identified and its content is measured by nuclear magnetic resonance (NMR) spectroscopy.

[0060] [1-5. Non-aqueous Solvent] The non-aqueous electrolyte solution according to the present invention, like a general non-aqueous electrolyte solution, usually contains, as its main component, a non-aqueous solvent that dissolves the above-mentioned electrolyte. There are no particular limitations on the non-aqueous solvent, and known organic solvents can be used. Examples of organic solvents include saturated cyclic carbonates such as ethylene carbonate, propylene carbonate, and butylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; cyclic carboxylic acid esters such as γ-butyrolactone and γ-valerolactone; ether compounds such as dimethoxymethane, diethoxymethane, ethoxymethoxymethane, tetrahydrofuran, 1,3-dioxane, and 1,4-dioxane; sulfone compounds such as 2-methylsulfolane, 3-methylsulfolane, 2-fluorosulfolane, 3-fluorosulfolane, dimethylsulfone, ethyl methyl sulfone, and monofluoromethyl methyl sulfone; etc. The non-aqueous solvent in this embodiment is preferably at least one selected from the group consisting of saturated cyclic carbonates, chain carbonates, chain carboxylic acid esters, cyclic carboxylic acid esters, ether compounds, and sulfone compounds. Among these, saturated cyclic carbonates, chain carbonates, and carboxylic acid esters are preferred, and saturated cyclic carbonates and chain carbonates are more preferred. These non-aqueous solvents can be used alone or in combination of two or more.

[0061] The combination of two or more non-aqueous solvents is not particularly limited, and examples thereof include a saturated cyclic carbonate and a chain carboxylic acid ester, a cyclic carboxylic acid ester and a chain carbonate, and a saturated cyclic carbonate, a chain carbonate and a chain carboxylic acid ester. Among these, the combinations of a saturated cyclic carbonate and a chain carbonate, and a saturated cyclic carbonate, a chain carbonate and a chain carboxylic acid ester are preferred.

[0062] [1-5-1. Saturated Cyclic Carbonate] The saturated cyclic carbonate, which is one aspect of the non-aqueous solvent in this embodiment, typically includes a saturated cyclic carbonate having an alkylene group having 2 to 4 carbon atoms. From the viewpoint of improving the battery characteristics resulting from an improved degree of lithium ion dissociation, saturated cyclic carbonates having 2 to 3 carbon atoms are preferably used.

[0063] Examples of saturated cyclic carbonates include ethylene carbonate, propylene carbonate, and butylene carbonate. Among these, ethylene carbonate and propylene carbonate are preferred, and ethylene carbonate, which is less susceptible to oxidation and reduction, is more preferred. The saturated cyclic carbonates may be used alone or in any combination and ratio of two or more.

[0064] The content of the saturated cyclic carbonate is not particularly limited and can be any amount as long as it does not significantly impair the effects of the present invention. It is typically 3 to 90% by volume, preferably 3 to 85% by volume, and more preferably 5 to 80% by volume, relative to the total amount of nonaqueous solvent in the nonaqueous electrolyte solution. The content is typically 3% by volume or more, preferably 5% by volume or more, and typically 90% by volume or less, preferably 85% by volume or less, and more preferably 80% by volume or less. By setting the content within this range, a decrease in electrical conductivity due to a decrease in the dielectric constant of the nonaqueous electrolyte solution is avoided, and the large-current discharge characteristics, negative electrode stability, and cycle characteristics of the nonaqueous electrolyte secondary battery are easily maintained within a favorable range. The oxidation / reduction resistance of the nonaqueous electrolyte solution is improved, and stability during high-temperature storage tends to be improved. In this embodiment, "volume percent" refers to the volume at 25°C and 1 atmosphere.

[0065] [1-5-2. Chain Carbonate] As the chain carbonate, which is one aspect of the non-aqueous solvent in this embodiment, one having 3 to 7 carbon atoms is usually used, and in order to adjust the viscosity of the electrolyte solution within an appropriate range, a chain carbonate having 3 to 5 carbon atoms is preferably used.

[0066] Specific examples of the chain carbonate include dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propyl isopropyl carbonate, ethyl methyl carbonate, and methyl-n-propyl carbonate. Dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate are particularly preferred.

[0067] Chain carbonates having fluorine atoms (hereinafter sometimes abbreviated as "fluorinated chain carbonates") can also be suitably used. The number of fluorine atoms in the fluorinated chain carbonate is not particularly limited as long as it is 1 or more, but is usually 6 or less, and preferably 4 or less. When the fluorinated chain carbonate has multiple fluorine atoms, they may be bonded to the same carbon or different carbons.

[0068] Examples of the fluorinated chain carbonate include fluorinated dimethyl carbonate derivatives such as fluoromethyl methyl carbonate, fluorinated ethyl methyl carbonate derivatives such as 2-fluoroethyl methyl carbonate, and fluorinated diethyl carbonate derivatives such as ethyl-(2-fluoroethyl) carbonate.

[0069] The chain carbonate may be used alone or in any combination of two or more kinds in any ratio.

[0070] The content of the chain carbonate is not particularly limited, but is typically 15 to 90 vol%, preferably 20 to 85 vol%, and more preferably 25 to 80 vol%, relative to the total amount of nonaqueous solvent in the nonaqueous electrolyte. The content is typically 15 vol% or more, preferably 20 vol% or more, more preferably 25 vol% or more, and typically 90 vol% or less, preferably 85 vol% or less, and more preferably 80 vol% or less. By setting the content of the chain carbonate within the above range, the viscosity of the nonaqueous electrolyte can be kept within an appropriate range, a decrease in ionic conductivity can be suppressed, and the output characteristics of the nonaqueous electrolyte secondary battery can be easily maintained within a favorable range.

[0071] Furthermore, by combining a specific chain carbonate with ethylene carbonate in a specific content, the battery performance can be significantly improved.

[0072] For example, when ethyl methyl carbonate is selected as the specific linear carbonate, the content of ethylene carbonate is not particularly limited and can be any as long as it does not significantly impair the effects of the present invention. However, it is usually 15 to 45 vol%, preferably 20 to 40 vol%, based on the total amount of non-aqueous solvent in the non-aqueous electrolyte. Here, the content is usually 15 vol% or more, preferably 20 vol% or more, and usually 45 vol% or less, preferably 40 vol% or less. Furthermore, the content of ethyl methyl carbonate is usually 55 to 85 vol%, preferably 60 to 80 vol%, based on the total amount of non-aqueous solvent in the non-aqueous electrolyte. Here, the content is usually 55 vol% or more, preferably 60 vol% or more, and usually 85 vol% or less, preferably 80 vol% or less. By setting each content within the above range, excellent high-temperature stability and suppression of gas generation tend to be achieved.

[0073] [1-5-3. Chain Carboxylic Acid Ester] Examples of the chain carboxylic acid ester, which is one aspect of the non-aqueous solvent in this embodiment, include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, methyl valerate, methyl isobutyrate, ethyl isobutyrate, and methyl pivalate. Among these, methyl acetate, ethyl acetate, propyl acetate, and butyl acetate are preferred from the viewpoint of improving battery characteristics. Chain carboxylic acid esters in which a portion of the hydrogen atoms of the above-mentioned chain carboxylic acid esters are substituted with fluorine can also be suitably used. Examples of such fluorine-substituted chain carboxylic acid esters include methyl trifluoroacetate and ethyl trifluoroacetate.

[0074] [1-5-4. Cyclic Carboxylic Acid Ester] Examples of the cyclic carboxylic acid ester, which is one embodiment of the non-aqueous solvent in this embodiment, include γ-butyrolactone and γ-valerolactone. Among these, γ-butyrolactone is more preferable. Cyclic carboxylic acid esters in which some of the hydrogen atoms of the above-mentioned cyclic carboxylic acid esters have been substituted with fluorine atoms can also be used preferably.

[0075] [1-5-5. Ether Compounds] Preferred examples of the ether compound, which is one aspect of the non-aqueous solvent in this embodiment, include chain ethers having 3 to 10 carbon atoms, such as dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, and diethylene glycol dimethyl ether, and cyclic ethers having 3 to 6 carbon atoms, such as tetrahydrofuran, 2-methyltetrahydrofuran, 3-methyltetrahydrofuran, 1,3-dioxane, 2-methyl-1,3-dioxane, 4-methyl-1,3-dioxane, and 1,4-dioxane.

[0076] Among these, as the chain ethers having 3 to 10 carbon atoms, dimethoxymethane, diethoxymethane, and ethoxymethoxymethane are preferred because they have a high solvation ability for lithium ions, improve ionic dissociation, have low viscosity, and provide high ionic conductivity, and as the cyclic ethers having 3 to 6 carbon atoms, tetrahydrofuran, 1,3-dioxane, 1,4-dioxane, and the like are preferred because they provide high ionic conductivity.

[0077] The content of the ether-based compound is not particularly limited and may be any amount as long as it does not significantly impair the effects of the present invention. However, it is typically 1 to 30 vol.%, preferably 2 to 25 vol.%, and more preferably 3 to 20 vol.%, based on the total amount of the non-aqueous solvent. Here, the content is typically 1 vol.% or more, preferably 2 vol.% or more, more preferably 3 vol.% or more, and typically 30 vol.% or less, preferably 25 vol.% or less, and more preferably 20 vol.% or less. If the content of the ether-based compound is within the above range, it is easy to ensure the improvement in the degree of lithium ion dissociation of the ether and the improvement in ionic conductivity due to the reduced viscosity. Furthermore, when the negative electrode active material is a carbon-based material, the phenomenon of co-intercalation of the chain ether with the lithium ion can be suppressed, thereby allowing the input / output characteristics and charge / discharge rate characteristics to be within appropriate ranges.

[0078] [1-5-6. Sulfone Compound] The sulfone compound, which is one aspect of the non-aqueous solvent in this embodiment, is not particularly limited and may be either a cyclic sulfone or a chain sulfone. In the case of a cyclic sulfone, the carbon number is usually 3 to 6, preferably 3 to 5. In the case of a chain sulfone, the carbon number is usually 2 to 6, preferably 2 to 5. In addition, the number of sulfonyl groups in one molecule of the sulfone compound is not particularly limited, but is usually 1 or 2.

[0079] Examples of cyclic sulfones include monosulfone compounds such as trimethylene sulfones, tetramethylene sulfones, and hexamethylene sulfones; and disulfone compounds such as trimethylene disulfones, tetramethylene disulfones, and hexamethylene disulfones. Among these, from the viewpoints of dielectric constant and viscosity, tetramethylene sulfones, tetramethylene disulfones, hexamethylene sulfones, and hexamethylene disulfones are more preferred, and tetramethylene sulfones (sulfolanes) are particularly preferred.

[0080] The sulfolanes are preferably sulfolane and / or sulfolane derivatives (hereinafter, sulfolane may also be abbreviated as "sulfolanes"). The sulfolane derivatives are preferably those in which one or more hydrogen atoms bonded to the carbon atoms constituting the sulfolane ring are substituted with a fluorine atom or an alkyl group.

[0081] Among these, 2-methylsulfolane, 3-methylsulfolane, 2-fluorosulfolane, 3-fluorosulfolane, 2,3-difluorosulfolane, 2-trifluoromethylsulfolane, 3-trifluoromethylsulfolane, and the like are preferred because they have high ionic conductivity and high input / output.

[0082] Examples of the chain sulfone include dimethyl sulfone, ethyl methyl sulfone, diethyl sulfone, monofluoromethyl methyl sulfone, difluoromethyl methyl sulfone, trifluoromethyl methyl sulfone, pentafluoroethyl methyl sulfone, etc. Among these, dimethyl sulfone, ethyl methyl sulfone, and monofluoromethyl methyl sulfone are preferred in terms of improving the high-temperature storage stability of the electrolyte solution.

[0083] The content of the sulfone-based compound is not particularly limited and may be any content as long as it does not significantly impair the effects of the present invention, but is typically 0.3 to 40 vol%, preferably 0.5 to 35 vol%, and more preferably 1 to 30 vol% relative to the total amount of nonaqueous solvent in the nonaqueous electrolyte solution. Here, the content is typically 0.3 vol% or more, preferably 0.5 vol% or more, more preferably 1 vol% or more, and typically 40 vol% or less, preferably 35 vol% or less, and more preferably 30 vol% or less. If the content of the sulfone-based compound is within the above range, an electrolyte solution with excellent high-temperature storage stability tends to be obtained.

[0084] [1-6. Auxiliary Agents] The nonaqueous electrolyte solution according to the present invention may contain various auxiliary agents as long as the effects of the present invention are not significantly impaired. Any conventionally known auxiliary agent can be used. The auxiliary agents can be used alone or in combination of two or more in any ratio. Examples of auxiliary agents include cyclic carbonates having a carbon-carbon unsaturated bond, fluorine-containing cyclic carbonates, organic compounds having an isocyanate group, organic compounds having an isocyanuric acid skeleton, sulfur-containing organic compounds, phosphorus-containing organic compounds, silicon-containing compounds, aromatic compounds, organic compounds having a cyano group, fluorine-free carboxylic acid esters, cyclic compounds having an ether bond, acid anhydrides, oxalates, triple bond-containing compounds, phosphazene compounds, phosphates having a P═O bond, and salts having an S═O bond. Examples include compounds described in International Publication No. WO 2015 / 111676.

[0085] Among these, at least one carbonate compound selected from cyclic carbonates having a carbon-carbon unsaturated bond and fluorine-containing cyclic carbonates (hereinafter also referred to as "specific carbonate compound") is preferred.

[0086] The content of the auxiliary agent is not particularly limited, and is arbitrary as long as it does not significantly impair the effects of the present invention, but when the non-aqueous electrolyte solution contains an auxiliary agent, it is usually 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, based on the total amount of the non-aqueous electrolyte solution, and also usually 10 mass% or less, preferably 5 mass% or less, more preferably 3 mass% or less, and even more preferably 2 mass% or less. Furthermore, when the non-aqueous electrolyte solution contains an auxiliary agent, the content of the auxiliary agent is usually 0.001 to 10 mass%, preferably 0.01 to 5 mass%, more preferably 0.1 to 3 mass%, and even more preferably 0.1 to 2 mass% based on the total amount of the non-aqueous electrolyte solution.

[0087] The cyclic ether compound can be used as an auxiliary agent in the non-aqueous electrolyte solution, and as shown in the section [1-5. Non-aqueous solvent], some compounds can also be used as non-aqueous solvents. When using a cyclic ether compound as an auxiliary agent, it is preferable to use it in an amount of less than 4 mass% based on the total amount of the non-aqueous electrolyte solution. Oxalates and phosphates having a P=O bond can also be used as auxiliary agents in the non-aqueous electrolyte solution, and as shown in the section [1-4. Electrolyte], some compounds can also be used as electrolytes. When using these compounds as auxiliary agents, it is preferable to use them in an amount of less than 3 mass% based on the total amount of the non-aqueous electrolyte solution.

[0088] [1-6-1. Specific Carbonate Compound] The nonaqueous electrolytic solution preferably contains, as an auxiliary agent, at least one carbonate compound selected from the group consisting of cyclic carbonates having a carbon-carbon unsaturated bond and cyclic carbonates having a fluorine atom. Among these, it is preferable to contain a cyclic carbonate having a carbon-carbon unsaturated bond, and it is more preferable to contain vinylene carbonate. These can be used alone or in combination of two or more in any ratio. It is preferable to contain at least one carbonate compound selected from the group consisting of unsaturated cyclic carbonates and fluorinated cyclic carbonates, it is more preferable to contain at least one carbonate compound selected from the group consisting of vinylene carbonate and monofluoroethylene carbonate, and it is even more preferable to contain vinylene carbonate.

[0089] When two or more specific carbonate compounds are used in combination, it is preferable to combine an unsaturated cyclic carbonate and a fluorinated cyclic carbonate, more preferably a combination of vinylene carbonate and a fluorinated cyclic carbonate, and a combination of an unsaturated cyclic carbonate and monofluoroethylene carbonate, and even more preferably a combination of vinylene carbonate and monofluoroethylene carbonate.

[0090] (Content of specific carbonate compound) When the non-aqueous electrolyte solution contains a specific carbonate compound as an auxiliary agent, the content of the specific carbonate compound (total amount when two or more types are used) in the total amount of the non-aqueous electrolyte solution is usually 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.5% by mass or more. Also, usually 10% by mass or less, preferably 5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less. Furthermore, when the non-aqueous electrolyte solution contains a specific carbonate compound as an auxiliary agent, the content of the specific carbonate compound (total amount when two or more types are used) in the total amount of the non-aqueous electrolyte solution is usually 0.001 to 10% by mass, preferably 0.01 to 5% by mass, more preferably 0.1 to 4% by mass, and even more preferably 0.5 to 3% by mass. If the content of the specific carbonate compound is within the above range, the battery characteristics, particularly the increase in internal resistance, can be suppressed. The reason for this is unclear, but it is thought that the inclusion of the carbonate compound at this ratio forms a coating on the electrode, minimizing side reactions of the components in the non-aqueous electrolyte. The identification and content of the specific carbonate compound is measured by nuclear magnetic resonance (NMR) spectroscopy.

[0091] (Mass ratio of the compound represented by the general formula (I) to the specific carbonate compound) When the non-aqueous electrolyte solution contains a specific carbonate compound as an auxiliary agent, the mass ratio of the content of the specific carbonate compound (total amount when two or more types are present) to the content of the compound represented by the general formula (I) (specific carbonate compound [g] / compound represented by the general formula (I) [g]) is usually 0.01 or more, preferably 0.05 or more, more preferably 0.1 or more, even more preferably 0.2 or more, and is usually 100 or less, preferably 50 or less, more preferably 25 or less, even more preferably 10 or less. Moreover, the mass ratio (specific carbonate compound [g] / compound represented by the general formula (I) [g]) is usually 0.01 to 100, preferably 0.05 to 50, more preferably 0.1 to 25, even more preferably 0.2 to 10. If the mass ratio is within the above range, the increase in battery characteristics, particularly internal resistance, can be suppressed. The reason for this is unclear, but it is thought that by containing a specific carbonate compound within the above mass ratio range, a coating is formed on the electrode, minimizing side reactions of the components of the non-aqueous electrolyte solution.

[0092] (Electrolyte and specific carbonate compound mass ratio) When the non-aqueous electrolyte solution contains a specific carbonate compound as an auxiliary agent, the mass ratio of the content of the specific carbonate compound (total amount if two or more) to the content of the electrolyte in the non-aqueous electrolyte solution (specific carbonate compound [g] / electrolyte [g]) is usually 0.00005 or more, preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, even more preferably 0.025 or more, also, usually 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, even more preferably 0.35 or less. Further, the mass ratio (specific carbonate compound [g] / electrolyte [g]) is usually 0.00005 to 0.5, preferably 0.001 to 0.45, more preferably 0.01 to 0.4 ~, even more preferably 0.02 to 0.35, even more preferably 0.025 to 0.35. When the mass ratio is within the above range, the battery characteristics, particularly the internal resistance, can be suppressed from increasing. Although the reason for this is unclear, it is thought that by containing the specific carbonate compound and electrolyte within the above mass ratio range, a coating is formed on the electrode, minimizing side reactions of the electrolyte within the battery system.

[0093] [1-6-1-1. Cyclic carbonate having a carbon-carbon unsaturated bond] The cyclic carbonate having a carbon-carbon unsaturated bond (hereinafter also referred to as "unsaturated cyclic carbonate") is not particularly limited as long as it is a cyclic carbonate having a carbon-carbon double bond or a carbon-carbon triple bond. Cyclic carbonates having an aromatic ring are also included in the unsaturated cyclic carbonate.

[0094] Examples of unsaturated cyclic carbonates include vinylene carbonates, ethylene carbonates substituted with a substituent having an aromatic ring, a carbon-carbon double bond, or a carbon-carbon triple bond, phenyl carbonates, vinyl carbonates, allyl carbonates, catechol carbonates, etc. Among these, vinylene carbonates and ethylene carbonates substituted with a substituent having an aromatic ring, a carbon-carbon double bond, or a carbon-carbon triple bond are preferred.

[0095] Examples of vinylene carbonates include vinylene carbonate, methyl vinylene carbonate, 4,5-dimethyl vinylene carbonate, phenyl vinylene carbonate, 4,5-diphenyl vinylene carbonate, vinyl vinylene carbonate, 4,5-vinyl vinylene carbonate, allyl vinylene carbonate, and 4,5-diallyl vinylene carbonate. Examples of ethylene carbonates substituted with a substituent having an aromatic ring or a carbon-carbon double bond or a carbon-carbon triple bond include vinyl ethylene carbonate, 4,5-divinyl ethylene carbonate, 4-methyl-5-vinyl ethylene carbonate, 4-allyl-5-vinyl ethylene carbonate, ethynyl ethylene carbonate, 4,5-diethynyl ethylene carbonate, 4-methyl-5-ethynyl ethylene carbonate, 4-vinyl-5-ethynyl ethylene carbonate, 4-allyl-5-ethynyl ethylene carbonate, phenyl ethylene carbonate, 4,5-diphenyl ethylene carbonate, 4-phenyl-5-vinyl ethylene carbonate, 4-allyl-5-phenyl ethylene carbonate, allyl ethylene carbonate, 4,5-diallyl ethylene carbonate, and 4-methyl-5-allyl ethylene carbonate. Among these, vinylene carbonate, vinylethylene carbonate, and ethynylethylene carbonate are preferred because they form a more stable composite coating on the electrode, and one or more selected from vinylene carbonate and vinylethylene carbonate are more preferred, with vinylene carbonate being even more preferred. The unsaturated cyclic carbonates can be used alone or in combination of two or more in any ratio.

[0096] [1-6-1-2. Cyclic Carbonates Having Fluorine Atoms] The cyclic carbonates having fluorine atoms are not particularly limited as long as they have a cyclic carbonate structure and contain fluorine atoms. Examples of cyclic carbonates having fluorine atoms include fluorinated cyclic carbonates having an alkylene group having 2 to 6 carbon atoms and derivatives thereof, such as fluorinated ethylene carbonate (fluoroethylene carbonate) and derivatives thereof, and ethylene carbonate having a fluorine-containing group. Examples of derivatives of fluorinated ethylene carbonate include fluorinated ethylene carbonate substituted with an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms). Among these, fluoroethylene carbonate having 1 to 8 fluorine atoms and derivatives thereof are preferred.

[0097] Examples of fluoroethylene carbonates having 1 to 8 fluorine atoms and derivatives thereof, and ethylene carbonates having a fluorine-containing group include monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, 4-fluoro-4-methylethylene carbonate, 4,5-difluoro-4-methylethylene carbonate, 4-fluoro-5-methylethylene carbonate, 4,4-difluoro-5-methylethylene carbonate, 4-(fluoromethyl)-ethylene carbonate, 4-(difluoromethyl)-ethylene carbonate, 4-(trifluoromethyl)-ethylene carbonate, 4-(fluoromethyl)-4-fluoroethylene carbonate, 4-(fluoromethyl)-5-fluoroethylene carbonate, 4-fluoro-4,5-dimethylethylene carbonate, 4,5-difluoro-4,5-dimethylethylene carbonate, and 4,4-difluoro-5,5-dimethylethylene carbonate. Among these, from the viewpoint of imparting high ionic conductivity to the electrolyte and facilitating the formation of a stable interface protective coating, one or more selected from monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, and 4,5-difluoroethylene carbonate are preferred. The fluorine atom-containing cyclic carbonates can be used alone or in combination of two or more in any ratio.

[0098] [1-6-2. Organic Compound Having an Isocyanate Group] The organic compound having an isocyanate group is not particularly limited as long as it has at least one isocyanate group in the molecule. The number of isocyanate groups in one molecule is preferably 1 to 4, more preferably 2 or 3, and even more preferably 2. Examples of organic compounds having an isocyanate group include monoisocyanate compounds such as methyl isocyanate, ethyl isocyanate, butyl isocyanate, vinyl isocyanate, propargyl isocyanate, cyclohexyl isocyanate, phenyl isocyanate, 2-isocyanatoethyl acrylate, and 2-isocyanatoethyl methacrylate; and diisocyanate compounds such as monomethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, octamethylene diisocyanate, 1,4-phenylene diisocyanate, 1,3-diisocyanatopropane, 1,3-bis(isocyanatomethyl)cyclohexane, carbonyl diisocyanate, and 1,4-diisocyanato-2-fluorobutane. In particular, from the viewpoint of forming a stable interface protective coating, organic compounds having at least two isocyanate groups are preferred, with hexamethylene diisocyanate and 1,3-bis(isocyanatomethyl)cyclohexane being more preferred, and 1,3-bis(isocyanatomethyl)cyclohexane being even more preferred.

[0099] [1-6-3. Organic Compound Having an Isocyanuric Acid Skeleton] The organic compound having an isocyanuric acid skeleton (hereinafter also referred to as an "isocyanurate compound") is not particularly limited as long as it is an organic compound having at least one isocyanuric acid skeleton in the molecule. Examples of the organic compound having an isocyanuric acid skeleton include the following compounds:

[0100]

[0101] In particular, from the viewpoint of forming a stable interface protective coating, an isocyanurate compound having a saturated or unsaturated aliphatic hydrocarbon group which may have a halogen atom is preferred, an isocyanurate compound having an unsaturated aliphatic hydrocarbon group containing a terminal carbon-carbon unsaturated bond is more preferred, and triallyl isocyanurate is even more preferred.

[0102] [1-6-4. Sulfur-Containing Organic Compounds] The sulfur-containing organic compound is not particularly limited as long as it is an organic compound having at least one sulfur atom (S) in the molecule. Preferred are organic compounds having at least one S═O bond, and more preferred are ester compounds having an S═O bond, such as chain sulfonate esters, cyclic sulfonate esters, chain sulfate esters, cyclic sulfate esters, chain sulfite esters, and cyclic sulfite esters. However, salts having an S═O bond are not considered to be "sulfur-containing organic compounds" but are included in the "salts having an S═O bond" described below. Furthermore, anion-containing compounds having an S═O bond and an S—F bond are not considered to be "sulfur-containing organic compounds" but are included in the above-mentioned "anion-containing compounds having an S═O bond and an S—F bond." Furthermore, alkyl sulfate anion-containing compounds are not considered to be "sulfur-containing organic compounds" but are included in the above-mentioned "alkyl sulfate anion-containing compounds." Examples of sulfur-containing organic compounds include chain sulfonates such as alkyl disulfonates, such as methyl fluorosulfonate, methyl methanesulfonate, ethyl methanesulfonate, busulfan, methyl methanesulfonyloxyacetate, methyl vinylsulfonate, allyl vinylsulfonate, propargyl allylsulfonate, methoxycarbonylmethyl methanedisulfonate, ethoxycarbonylmethyl methanedisulfonate, methoxycarbonylmethyl 1,3-butanedisulfonate, ethoxycarbonylmethyl 1,3-butanedisulfonate, 1-methoxycarbonylethyl 1,3-butanedisulfonate, and 1-ethoxycarbonylethyl 1,3-butanedisulfonate; cyclic sulfonate esters such as 1,3-propane sultone, 1-fluoro-1,3-propane sultone, 1-methyl-1,3-propane sultone, 1-propene-1,3-sultone, 2-propene-1,3-sultone, 1-fluoro-1-propene-1,3-sultone, 1-methyl-1-propene-1,3-sultone, 1,3-butane sultone, 2,4-butane sultone, 1,4-butane sultone, 1,5-pentane sultone, methylenemethane disulfonate, ethylenemethane disulfonate, and 2,2-dioxide-1,2-oxathiolan-4-yl acetate;Chain sulfate esters such as dimethyl sulfate, ethyl methyl sulfate, and diethyl sulfate; cyclic sulfate esters such as 1,2-ethylene sulfate, 1,2-propylene sulfate, 1,3-propylene sulfate, and 1,2-butylene sulfate; chain sulfite esters such as dimethyl sulfite, ethyl methyl sulfite, and diethyl sulfite; cyclic sulfite esters such as 1,2-ethylene sulfite, 1,2-propylene sulfite, 1,3-propylene sulfite, and 1,2-butylene sulfite; cyclic sulfones such as 1,1-dioxidetetrahydrothiophen-3-yl methanesulfonate and 1,1-dioxide-2,3-dihydrothiophen-3-yl methanesulfonate; butane-2,3-diyl dimethanesulfonate and butane-1,4-diyl Examples include sulfonic acid esters such as dimethanesulfonate or methylenemethane disulfonate, and vinyl sulfone compounds such as divinyl sulfone, 1,2-bis(vinylsulfonyl)ethane or bis(2-vinylsulfonylethyl)ether. In particular, from the viewpoint of forming a stable interface protective coating, linear or cyclic sulfonic acid esters, cyclic sulfates, or cyclic sulfites are more preferred, with cyclic sulfonic acid esters or cyclic sulfates being particularly preferred, and 1,3-propane sultone, methylenemethane disulfonate, and 1,2-ethylene sulfate being most preferred.

[0103] [1-6-5. Phosphorus-Containing Organic Compounds] Phosphorus-containing organic compounds are not particularly limited as long as they are compounds having at least one phosphorus atom in the molecule. However, salts having a P═O bond are not considered "phosphorus-containing organic compounds" but are included in the "salts having a P═O bond" described below. Furthermore, anion-containing compounds having a P═O bond and a P—F bond are not considered "phosphorus-containing organic compounds" but are included in the "anion-containing compounds having a P═O bond and a P—F bond" described above. Examples of phosphorus-containing organic compounds include trimethyl phosphate, tributyl phosphate, trioctyl phosphate, tris(2,2,2-trifluoroethyl)phosphate, ethyl 2-(diethoxyphosphoryl)acetate, and 2-propynyl 2-(diethoxyphosphoryl)acetate.

[0104] In particular, ethyl 2-(diethoxyphosphoryl)acetate or 2-propynyl 2-(diethoxyphosphoryl)acetate is preferred, with 2-propynyl 2-(diethoxyphosphoryl)acetate being more preferred.

[0105] [1-6-6. Silicon-Containing Compound] The silicon-containing compound is not particularly limited as long as it is a compound having at least one silicon atom in the molecule. Examples of silicon-containing compounds include boric acid compounds such as tris(trimethylsilyl) borate, tris(trimethoxysilyl) borate, tris(triethylsilyl) borate, and tris(dimethylvinylsilyl) borate; phosphate compounds such as tris(trimethylsilyl) phosphate, tris(triethylsilyl) phosphate, tris(triphenylsilyl) phosphate, tris(trimethoxysilyl) phosphate, and tris(dimethylvinylsilyl) phosphate; phosphite compounds such as tris(trimethylsilyl) phosphite, tris(triethylsilyl) phosphite, tris(triphenylsilyl) phosphite, tris(trimethoxysilyl) phosphite, and tris(dimethylvinylsilyl) phosphite; sulfonic acid compounds such as trimethylsilyl methanesulfonate and trimethylsilyl tetrafluoromethanesulfonate; silane compounds such as tetramethylsilane, trimethylvinylsilane, dimethyldivinylsilane, methyltrivinylsilane, and tetravinylsilane; Examples of suitable compounds include disilane compounds such as hexamethyldisilane, hexaethyldisilane, 1,1,2,2-tetramethyldisilane, and 1,2-diphenyltetramethyldisilane; and disiloxane compounds such as hexamethyldisiloxane, 1,3-divinyltetramethyldisiloxane, and 1,1,3,3-tetramethyl-1,3-diphenyldisiloxane. In particular, from the viewpoint of forming a stable interface protective coating, disilane compounds and disiloxane compounds are preferred, disiloxane compounds are more preferred, hexamethyldisiloxane and 1,3-divinyltetramethyldisiloxane are even more preferred, and 1,3-divinyltetramethyldisiloxane is particularly preferred.

[0106] [1-6-7. Aromatic Compound] The aromatic compound is not particularly limited as long as it has an aromatic group in the molecule. Examples of the aromatic compound include aromatic compounds having a branched alkyl group such as cyclohexylbenzene, tert-butylbenzene, tert-amylbenzene, and 1-fluoro-4-tert-butylbenzene, as well as aromatic compounds such as biphenyl, terphenyl (o-, m-, and p-isomers), fluorobenzene, methyl phenyl carbonate, ethyl phenyl carbonate, and diphenyl carbonate.

[0107] In particular, biphenyl, terphenyl (o-, m-, p-isomer), fluorobenzene, cyclohexylbenzene, tert-butylbenzene, and tert-amylbenzene are more preferred, and biphenyl, o-terphenyl, fluorobenzene, cyclohexylbenzene, and tert-amylbenzene are even more preferred.

[0108] [1-6-8. Organic Compound Having a Cyano Group] The organic compound having a cyano group is not particularly limited as long as it is an organic compound having at least one cyano group in the molecule. Examples of organic compounds having a cyano group include: organic compounds having one cyano group in the molecule, such as acetonitrile, propionitrile, butyronitrile, pentanenitrile, hexanenitrile, decanenitrile, undecanenitrile, dodecanenitrile, cyclohexanecarbonitrile, acrylonitrile, methacrylonitrile, and crotononitrile; organic compounds having two cyano groups in the molecule, such as succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, sebaconitrile, methylmalononitrile, ethylmalononitrile, bicyclohexyl-1,1-dicarbonitrile, 1,4-dicyanopentane, and 1,2-dicyanobenzene; and organic compounds having three cyano groups in the molecule, such as 1,2,3-propanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, 1,3,5-cyclohexanetricarbonitrile, and 1,3,5-benzenetricarbonitrile. In particular, from the viewpoint of forming a stable interface protective film, organic compounds having two cyano groups are preferred, succinonitrile and adiponitrile are more preferred, and adiponitrile is even more preferred.

[0109] [1-6-9. Fluorine-free carboxylic acid ester] The fluorine-free carboxylic acid ester is not particularly limited as long as it is a carboxylic acid ester that does not have a fluorine atom in the molecule. Preferably, it is a fluorine-free chain carboxylic acid ester, and more preferably a fluorine-free saturated chain carboxylic acid ester. The total number of carbon atoms in the fluorine-free chain carboxylic acid ester is preferably 3 or more, more preferably 4 or more, and preferably 7 or less, more preferably 6 or less, and even more preferably 5 or less. Furthermore, the total number of carbon atoms in the fluorine-free chain carboxylic acid ester is preferably 3 to 7, more preferably 4 to 6, and even more preferably 4 to 5. Examples of the chain carboxylic acid ester include methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, methyl propionate, ethyl propionate, n-propyl propionate, isopropyl propionate, n-butyl propionate, methyl pivalate, ethyl pivalate, n-propyl pivalate, isopropyl pivalate, n-butyl pivalate, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, methyl crotonate, ethyl crotonate, methyl 2-propionate, etc. In particular, from the viewpoint of improving the output characteristics of the battery, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, and n-propyl propionate are preferred, and methyl propionate is more preferred.

[0110] [1-6-10. Cyclic Compound Having an Ether Bond] The cyclic compound having an ether bond is not particularly limited as long as it is a compound having one or more ether bonds in the molecule. Examples of the cyclic compound having an ether bond include cyclic acetal compounds such as 1,3-dioxolane, 1,3-dioxane, and 1,3,5-trioxane.

[0111] In particular, cyclic acetal compounds are preferred, with 1,3-dioxolane or 1,3-dioxane being more preferred, and 1,3-dioxane being more preferred.

[0112] [1-6-11. Acid anhydride] Acid anhydrides include those having a "C(=O)-O-C(=O) group" or a "C(=O)-O-S(=O) group" in the molecule. 2 Group" or "S(=O)2 -O-S(=O) 2 There are no particular limitations on the acid anhydride, so long as it is an acid anhydride having a "group". Examples of the acid anhydride include chain carboxylic acid anhydrides such as acetic anhydride, acrylic anhydride, methacrylic anhydride, cyclohexanecarboxylic anhydride, propynoic anhydride, benzoic anhydride, fluoroacetic anhydride, 4-fluorobenzoic anhydride, and acetic propionic anhydride, succinic anhydride, maleic anhydride, citraconic anhydride, glutaric anhydride, itaconic anhydride, fluorosuccinic anhydride, allylsuccinic anhydride, 1,2-oxathiolan-5-one 2,2-dioxide, and 1,2,6-oxadithiane 2,2,6,6-tetraoxide. In particular, from the viewpoint of forming a stable interface protective coating, methacrylic anhydride, succinic anhydride, maleic anhydride, and allylsuccinic anhydride are preferred, with succinic anhydride or allylsuccinic anhydride being more preferred.

[0113] [1-6-12. Oxalate] The oxalate is not particularly limited as long as it has an oxalic acid skeleton in the molecule. (Counter Cation) Examples of the counter cation of the oxalate include alkali metals such as lithium, sodium, and potassium, with lithium being preferred. Examples of the oxalate include lithium bis(oxalato)borate, lithium difluorooxalatoborate, lithium tetrafluorooxalatophosphate, lithium difluorobis(oxalato)phosphate, and lithium tris(oxalato)phosphate. In particular, lithium bis(oxalato)borate is preferred from the viewpoint of forming a stable interface protective coating.

[0114] [1-6-13. Triple Bond-Containing Compound] The triple bond-containing compound is not particularly limited as long as it is a compound having at least one triple bond in the molecule. Examples of the triple bond-containing compound include 2-propynyl methyl carbonate, 2-propynyl acetate, 2-propynyl formate, 2-propynyl methacrylate, 2-propynyl methanesulfonate, 2-propynyl vinylsulfonate, 2-propynyl 2-(methanesulfonyloxy)propionate, di(2-propynyl)oxalate, 2-butyne-1,4-diyl dimethanesulfonate, and 2-butyne-1,4-diyl diformate.

[0115] In particular, 2-propynyl methyl carbonate, 2-propynyl methacrylate, 2-propynyl methanesulfonate, 2-propynyl vinylsulfonate, di(2-propynyl)oxalate, and 2-butyne-1,4-diyl dimethanesulfonate are preferred, and 2-propynyl methanesulfonate, 2-propynyl vinylsulfonate, di(2-propynyl)oxalate, and 2-butyne-1,4-diyl dimethanesulfonate are more preferred.

[0116] [1-6-14. Phosphazene Compound] The phosphazene compound is not particularly limited as long as it is a compound having an "N=P-N group" in the molecule. Examples of the phosphazene compound include cyclic phosphazene compounds such as methoxypentafluorocyclotriphosphazene, ethoxypentafluorocyclotriphosphazene, phenoxypentafluorocyclotriphosphazene, and ethoxyheptafluorocyclotetraphosphazene.

[0117] In particular, cyclic phosphazene compounds such as methoxypentafluorocyclotriphosphazene, ethoxypentafluorocyclotriphosphazene, and phenoxypentafluorocyclotriphosphazene are preferred, with methoxypentafluorocyclotriphosphazene and ethoxypentafluorocyclotriphosphazene being more preferred.

[0118] [1-6-15. Phosphate Salt Having a P=O Bond] The salt having a P=O bond is not particularly limited as long as it is a phosphate salt having a P=O bond in the molecule. (Counter Cation) Examples of the counter cation of the salt having a P=O bond include ions of alkali metals such as lithium, sodium, and potassium, with lithium ions being preferred. Examples of the salt having a P=O bond include phosphonates such as lithium ethyl methoxycarbonylphosphonate, lithium ethyl ethoxycarbonylphosphonate, and lithium ethyl iso-butoxycarbonylphosphonate.

[0119] [1-6-16. Salts Having an S═O Bond] There are no particular limitations on the salts having an S═O bond, as long as they are salts having an S═O bond in the molecule, and any salts can be used as long as they do not significantly impair the effects of the present invention. (Counter Cation) Examples of counter cations for salts having an S═O bond include ions of alkali metals such as lithium, sodium, and potassium, with lithium ions being preferred. Examples of salts having an S═O bond include salts having a methanesulfonyl group, such as lithium trifluoro((methanesulfonyl)oxy)borate [LiTFMSB] and lithium pentafluoro((methanesulfonyl)oxy)phosphate [LiPFMSP].

[0120] (Mass Ratio of Electrolyte to Auxiliary Agent) When the non-aqueous electrolytic solution contains an auxiliary agent other than a specific carbonate compound as an auxiliary agent, the mass ratio of the content of the auxiliary agent (total amount when there are two or more types) to the content of the electrolyte in the non-aqueous electrolytic solution (auxiliary agent [g] / electrolyte [g]) is usually 0.00005 or more, preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, still more preferably 0.025 or more, and is usually 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, still more preferably 0.35 or less. Furthermore, when the non-aqueous electrolyte solution contains an auxiliary agent other than a specific carbonate compound as an auxiliary agent, the mass ratio of the content of the auxiliary agent (total amount if two or more types) to the content of the electrolyte in the non-aqueous electrolyte solution (auxiliary agent [g] / electrolyte [g]) is typically 0.00005 to 0.5, preferably 0.001 to 0.45, more preferably 0.01 to 0.4, even more preferably 0.02 to 0.35, and even more preferably 0.025 to 0.35. If the mass ratio is within the above range, the battery characteristics, particularly the increase in internal resistance, can be suppressed. Although the reason for this is unclear, it is thought that by containing the auxiliary agent and electrolyte within the above mass ratio range, a coating is formed on the electrode, minimizing side reactions of the electrolyte within the battery system.

[0121] 2. Nonaqueous Electrolyte Battery The configuration of the nonaqueous electrolyte battery of the present invention, excluding the nonaqueous electrolyte, will be described below using a lithium ion secondary battery as an example. The nonaqueous electrolyte battery of the present invention includes at least a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and a nonaqueous electrolyte.

[0122] [2-1. Positive Electrode] The positive electrode has a positive electrode active material capable of absorbing and releasing lithium ions on at least a part of the surface of a current collector. The positive electrode active material includes a lithium transition metal compound.

[0123] [2-1-1. Positive Electrode Active Material] The positive electrode active material (lithium transition metal oxide) used in the positive electrode will be described below.

[0124] [2-1-1-1. Lithium transition metal oxide] Lithium transition metal oxide is a compound having a structure that can extract and insert lithium ions, and is represented by the following composition formula (1): Li1+y M 1 O 2 (1) In the composition formula (1), y is −0.2 to 0.5, and M 1 represents an element containing at least Ni element, and M 1 The molar ratio of the content of Ni element to the content of all elements contained in 1 ) is preferably 0.40 or more, more preferably 0.50 or more, and even more preferably 0.55 or more, and is preferably 1.00 or less, and more preferably 0.90 or less. 1 The molar ratio (Ni / M) is preferably 0.40 to 1.00, more preferably 0.50 to 0.90, and even more preferably 0.55 to 0.90. 1 ) falls within this range, the compound represented by general formula (I) can easily form a coating on the positive electrode, and a side reaction between the positive electrode and the non-aqueous electrolyte can be suppressed, thereby improving the DCR maintenance rate during operation at high temperatures of the non-aqueous electrolyte battery and suppressing an increase in the amount of gas generated during operation at high temperatures.

[0125] Specific examples of the lithium transition metal oxide represented by the composition formula (1) include LiNiO 2 , LiNi 0.85 Co 0.10 Al 0.05 O 2 , LiNi 0.80 Co 0.15 Al 0.05 O 2 , LiNi 0.5 Co 0.2 Mn 0.3 O 2 , Li 1.05 Ni 0.5 Co 0.2 Mn 0.3 O 2 , LiNi 0.6 Co 0.2 Mn 0.2 O 2 , LiNi 0.8 Co 0.1 Mn 0.1 O 2 , Li 1.0 Ni 0.82 Co 0.11 Mn 0.07 O2 , LiNi 0.91 Co 0.06 Mn 0.03 O 2 , LiNi 0.91 Co 0.06 Al 0.03 O 2 , LiNi 0.90 Co 0.03 Al 0.07 O 2 , Li 1.00 Ni 0.61 Co 0.20 Mn 0.19 O 2 etc.

[0126] Among these, from the viewpoint of improving the battery capacity, lithium transition metal composite oxides having a layered structure are preferred, and lithium transition metal composite oxides represented by the following composition formula (2) are more preferred: Li a1 Ni b1 M 2 c1 O 2 (2) In compositional formula (2), M 2 represents at least one element selected from the group consisting of Co, Mn, Al, Mg, Zr, Fe, Ti, and Er, and a1, b1, and c1 are, respectively, 0.80≦a1≦1.10, 0.40≦b1≦0.99, and 0.01≦c1≦0.60, and b1+c1=1. In composition formula (2), b1 is preferably 0.50 to 0.98, more preferably 0.60 to 0.98, even more preferably 0.70 to 0.98, and still more preferably 0.80 to 0.98.

[0127] In particular, from the viewpoint of the structural stability of the lithium transition metal composite oxide, a lithium transition metal composite oxide represented by the following composition formula (3) is preferred: Li a2 Ni b2 Co c2 M 3 d2 O 2 (3) In compositional formula (3), M 3represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er, and a2, b2, c2, and d2 are 0.80≦a2≦1.10, 0.40≦b2≦0.98, 0.01≦c2≦0.59, and 0.01≦d2≦0.59, respectively, and b2+c2+d2=1. In the above composition formula (3), b2 is preferably 0.50 to 0.98, more preferably 0.60 to 0.98, even more preferably 0.70 to 0.98, and even more preferably 0.80 to 0.98. Furthermore, d2 is preferably 0.10 to 0.59. Suitable examples of lithium transition metal composite oxides represented by the above composition formula (3) include LiNi 0.85 Co 0.10 Al 0.05 O 2 , LiNi 0.80 Co 0.15 Al 0.05 O 2 , LiNi 0.8 Co 0.1 Mn 0.1 O 2 , LiNi 0.91 Co 0.06 Mn 0.03 O 2 , LiNi 0.91 Co 0.06 Al 0.03 O 2 , LiNi 0.90 Co 0.03 Al 0.07 O 2 , Li 1.0 Ni 0.82 Co 0.11 Mn 0.07 O 2 , Li 1.00 Ni 0.61 Co 0.20 Mn 0.19 O 2 In the composition formula (1) or (2), from the viewpoint of increasing the structural stability of the lithium transition metal oxide and suppressing structural deterioration during repeated charge and discharge, M 1 or M 2 In the composition formula (3), M preferably contains Mn or Al, and more preferably Mn.3 Preferably, the positive electrode active material contains Mn or Al, and more preferably Mn. The positive electrode active material is identified by wet decomposition of a sample and then ICP emission spectroscopy.

[0128] [2-1-1-2. Introduction of a Foreign Element] The lithium transition metal oxide may contain an element (foreign element) other than the elements contained in any of the above composition formulas (1) to (3).

[0129] [2-1-1-3. Surface Coating] The positive electrode may be one in which a substance (surface-attached substance) having a different composition from the positive electrode active material is attached to the surface of the positive electrode active material. Examples of surface-attached substances include oxides such as aluminum oxide, sulfates such as lithium sulfate, and carbonates such as lithium carbonate. These surface-attached substances can be attached to the surface of the positive electrode active material, for example, by dissolving or suspending them in a solvent, impregnating the positive electrode active material, and drying. The amount of the surface-attached substance is preferably 1 μmol / g or more, more preferably 10 μmol / g or more, and typically 1 mmol / g or less, relative to the positive electrode active material. In this specification, a positive electrode active material having the surface-attached substance attached to its surface is also referred to as a "positive electrode active material."

[0130] [2-1-1-4. Blend] The positive electrode active material may be used alone or in combination of two or more kinds in any ratio.

[0131] [2-1-2. Positive Electrode Configuration and Manufacturing Method] A positive electrode using the positive electrode active material can be manufactured by a conventional method. That is, a positive electrode can be obtained by a coating method in which a positive electrode active material, a binder, and, if necessary, a conductive material and a thickener are mixed in a dry state to form a sheet and then pressed onto a positive electrode current collector, or by dissolving or dispersing these materials in a liquid medium such as an aqueous solvent or an organic solvent to form a slurry, which is then applied to a positive electrode current collector and dried to form a positive electrode active material layer on the current collector. Alternatively, for example, the positive electrode active material may be roll-formed into a sheet electrode, or may be compression-molded into a pellet electrode. Below, a case in which a slurry is sequentially applied to a positive electrode current collector and then dried will be described.

[0132] [2-1-2-1. Content of Positive Electrode Active Material] The content of the positive electrode active material in the positive electrode active material layer is usually 80 to 99.5 mass %.

[0133] [2-1-2-2. Electrode Density] The positive electrode active material layer obtained by applying and drying a binder, a conductive material, etc. is preferably compacted by a hand press, a roller press, etc. in order to increase the packing density of the positive electrode active material. The density of the positive electrode active material layer present on the current collector is usually 1.5 to 4.5 g / cm 3 is.

[0134] [2-1-2-3. Binder] When forming a positive electrode active material layer by a coating method, the type of binder is not particularly limited as long as it is a material that can be dissolved or dispersed in a liquid medium for the slurry. For example, fluorine-based resins such as polyvinyl fluoride, polyvinylidene fluoride, and polytetrafluoroethylene; and CN group-containing polymers such as polyacrylonitrile and polyvinylidene cyanide are preferred in terms of weather resistance, chemical resistance, heat resistance, and flame retardancy. Mixtures, modified products, derivatives, random copolymers, alternating copolymers, graft copolymers, and block copolymers of the above polymers can also be used. The binder can be used alone or in combination of two or more types in any ratio. When a resin is used as the binder, the weight-average molecular weight of the resin can be any value as long as it does not impair the effects of the present invention, and is typically between 10,000 and 3,000,000. A molecular weight within this range improves the strength of the electrode and allows for convenient electrode formation. The content of the binder in the positive electrode active material layer is usually 0.1 to 80 mass %.

[0135] [2-1-2-4. Conductive Material] Any known conductive material can be used as the conductive material. Specific examples include metal materials such as copper and nickel; graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; and carbon-based materials such as amorphous carbon such as needle coke. The conductive material can be used alone or in combination of two or more types in any ratio. The conductive material is typically used so that it is contained in the positive electrode active material layer in an amount of 0.01 to 50% by mass.

[0136] [2-1-2-5. Current Collector] The material of the positive electrode current collector is not particularly limited, and any known material can be used. Specific examples include metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum, with aluminum being preferred. The current collector may be in the form of a metal foil, a metal cylinder, a metal coil, a metal plate, a metal thin film, expanded metal, punched metal, or foamed metal. Of these, a metal foil or metal thin film is preferred. The metal thin film may be formed into a mesh, as appropriate. When the positive electrode current collector is in the form of a plate or film, the thickness of the current collector is optional, but is typically 1 μm to 1 mm.

[0137] [2-1-2-6. Thickness of Positive Electrode Plate] The thickness of the positive electrode plate is not particularly limited, but from the viewpoint of high capacity and high output, the thickness of the positive electrode active material layer obtained by subtracting the thickness of the current collector from the thickness of the positive electrode plate is usually 10 to 500 μm on one side of the current collector.

[0138] [2-1-2-7. Surface Coating of Positive Electrode Plate] The positive electrode plate may have a substance of a different composition from that of the positive electrode plate attached to its surface, and the substance may be the same as the surface-attached substance that may be attached to the surface of the positive electrode active material.

[0139] [2-2. Negative Electrode] The negative electrode has a negative electrode active material capable of absorbing and desorbing lithium ions on at least a portion of the current collector surface. [2-2-1. Negative Electrode Active Material] The negative electrode active material used in the negative electrode is not particularly limited as long as it is capable of electrochemically absorbing and desorbing metal ions. Specific examples include (i) carbon-based materials, (ii) materials containing metal elements and / or metalloid elements that can be alloyed with Li, (iii) lithium-containing metal composite oxide materials, and mixtures thereof. Among these, (i) carbon-based materials, (ii) materials containing metal elements and / or metalloid elements that can be alloyed with Li, and (iv) mixtures of graphite and materials containing metal elements and / or metalloid elements that can be alloyed with Li are preferred because of their excellent cycle characteristics, safety, and continuous charge characteristics. These materials can be used alone or in combination of two or more in any ratio.

[0140] [2-2-1-1. Carbon-Based Materials] (i) Examples of carbon-based materials include natural graphite, artificial graphite, amorphous carbon, carbon-coated graphite, graphite-coated graphite, and resin-coated graphite. Of these, natural graphite is preferred. The carbon-based materials can be used singly or in combination of two or more in any ratio. Examples of natural graphite include scaly graphite, flake graphite, and / or graphite particles obtained by subjecting these graphites to treatments such as spheroidization and densification. Of these, spherical or ellipsoidal graphite particles that have been subjected to a spheroidization treatment are preferred from the viewpoint of particle packing properties or charge / discharge rate characteristics. The average particle diameter (d50) of the graphite particles is typically 1 to 100 μm.

[0141] [2-2-1-2. Physical Properties of Carbon-Based Materials] Carbon-based materials used as negative electrode active materials preferably satisfy at least one of the physical properties and shape characteristics listed in (1) to (4) below, and more preferably satisfy multiple properties simultaneously. (1) X-ray Diffraction Parameters The d value (interlayer distance) of the lattice plane (002 plane) of a carbon-based material determined by X-ray diffraction using the Gakushin method is typically 0.335 to 0.360 nm. The crystallite size (Lc) of the carbon-based material determined by X-ray diffraction using the Gakushin method is typically 1.0 nm or greater. (2) Volume-Based Average Particle Size The volume-based average particle size of a carbon-based material is the volume-based average particle size (median diameter) determined by laser diffraction / scattering, and is typically 1 to 100 μm. (3) Raman R Value and Raman Half-Width Value The Raman R Value of a carbon-based material is measured using argon ion laser Raman spectroscopy and is typically 0.01 to 1.5. In addition, the carbon-based material has a 1580 cm -1 The Raman half-width in the vicinity is not particularly limited, but is usually 10 to 100 cm -1 (4) BET specific surface area The BET specific surface area of ​​a carbon-based material is the value of the specific surface area measured using the BET method, and is usually 0.1 to 100 m 2 ・g -1The negative electrode active material may contain two or more carbon-based materials with different properties. The "properties" referred to here refer to one or more characteristics selected from the group consisting of X-ray diffraction parameters, volume-based average particle size, Raman R value, Raman half-width, and BET specific surface area. Examples of containing two or more carbon-based materials with different properties include a volume-based particle size distribution that is not symmetrical about the median diameter, containing two or more carbon-based materials with different Raman R values, and having different X-ray diffraction parameters.

[0142] [2-2-1-3. Material Containing a Metal Element and / or a Metalloid Element That Can Be Alloyed with Li] (ii) Any conventionally known material containing a metal element and / or a metalloid element that can be alloyed with Li can be used. However, from the viewpoints of capacity and cycle life, a metal or metalloid selected from the group consisting of Sb, Si, Sn, Al, As, and Zn is preferable. Furthermore, when a material containing a metal element and / or a metalloid element that can be alloyed with Li contains two or more metals, the material may be an alloy material composed of an alloy of these metals. Furthermore, examples of materials containing a metal element and / or a metalloid element that can be alloyed with Li include oxides, nitrides, carbides, etc. of metals and / or metalloids. The material may contain two or more metals that can be alloyed with Li. Among these, materials containing elemental Si are preferred, and metallic Si (hereinafter also referred to as "Si") or Si-containing inorganic compounds are more preferable in terms of increasing capacity. In this specification, Si or Si-containing inorganic compounds are collectively referred to as "Si compounds." The content of the material containing a metal element and / or a metalloid element that can be alloyed with Li relative to the total mass of the negative electrode active material is preferably 0.1 to 25 mass%. Furthermore, the material containing a metal element and / or a metalloid element that can be alloyed with Li may already be alloyed with Li during the production of the negative electrode, which will be described later. As such a material, Si compounds are preferred in terms of achieving high capacity.

[0143] Examples of Si compounds include SiO x (0≦x≦2) and the like. Examples of metal compounds alloyed with Li include Li y Si (0<y≦4.4), Li 2z SiO 2+z(0<z≦2) and the like. Examples of Si compounds include Si oxides (SiO x1 , 0<x1≦2) is preferred because it has a larger theoretical capacity than graphite, and amorphous Si or nano-sized Si crystals are preferred because they allow alkali ions such as lithium ions to easily enter and exit, making it possible to obtain a high capacity. When the material containing a metal element and / or a metalloid element that can be alloyed with Li is in the form of particles, the average particle diameter (d 50 ) is usually 0.01 to 10 μm from the viewpoint of cycle life.

[0144] [2-2-1-4. Lithium-Containing Metal Composite Oxide Material] (iii) The lithium-containing metal composite oxide material is not particularly limited as long as it is capable of absorbing and releasing lithium ions. Specifically, from the viewpoint of high current density charge / discharge characteristics, a lithium-containing metal composite oxide material containing titanium is preferred, a composite oxide of lithium and titanium (hereinafter also referred to as "lithium titanium composite oxide") is more preferred, and a lithium titanium composite oxide having a spinel structure is even more preferred because it reduces output resistance. Furthermore, the lithium and / or titanium of the lithium titanium composite oxide may be substituted with another metal element, for example, at least one element selected from the group consisting of Al, Ga, Cu, and Zn. As the lithium titanium composite oxide, Li 4/3 Ti 5/3 O 4 , Li 1 Ti 2 O 4 and Li 4/5 Ti 11/5 O 4 Furthermore, examples of lithium-titanium composite oxides in which part of lithium and / or titanium is substituted with other elements include Li 4/3 Ti 4/3 Al 1/3 O 4 is also preferred.

[0145] [2-2-1-5. Mixture of Graphite and a Material Containing a Metal Element and / or a Metalloid Element That Can Be Alloyed with Li] (iv) The mixture of graphite and a material containing a metal element and / or a metalloid element that can be alloyed with Li may be the mixture described above in (ii) in which the material containing a metal element and / or a metalloid element that can be alloyed with Li and graphite are mixed in the form of independent particles, or may be a composite in which the material containing a metal element and / or a metalloid element that can be alloyed with Li is present on the surface or inside of graphite particles. The content of the material containing a metal element and / or a metalloid element that can be alloyed with Li relative to the total content of the material containing a metal element and / or a metalloid element that can be alloyed with Li and graphite is typically 1 to 99 mass%. Identification and content measurement of the negative electrode active material are performed by alkali-fusion of the sample followed by ICP emission spectroscopy.

[0146] [2-2-2. Negative Electrode Configuration and Manufacturing Method] The negative electrode can be manufactured by any known method as long as it does not impair the effects of the present invention. For example, the negative electrode can be manufactured by adding a binder, a liquid medium such as an aqueous solvent or an organic solvent, and, if necessary, a thickener, a conductive material, a filler, etc. to the negative electrode active material to form a slurry, which is then applied to a current collector, dried, and pressed to form a negative electrode active material layer.

[0147] [2-2-2-1. Content of Negative Electrode Active Material] The content of the negative electrode active material in the negative electrode active material layer is usually 80 to 99.5% by mass.

[0148] [2-2-2-2. Electrode Density] The negative electrode active material layer obtained by applying and drying a binder, a thickener, etc. is preferably compacted by a hand press, a roller press, etc. to increase the packing density of the negative electrode active material. The electrode structure when the negative electrode active material is made into an electrode is not particularly limited, but the density of the negative electrode active material layer present on the current collector is usually 1 to 2.2 g / cm 3 is.

[0149] [2-2-2-3. Binder] The binder is not particularly limited as long as it is stable in the nonaqueous electrolyte solution and the liquid medium used in electrode production. Specific examples include rubbery polymers such as styrene-butadiene rubber (SBR), isoprene rubber, butadiene rubber, fluororubber, acrylonitrile-butadiene rubber (NBR), and ethylene-propylene rubber, as well as fluorine-based polymers such as polyvinylidene fluoride, polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and tetrafluoroethylene-ethylene copolymers. These may be used alone or in combination of two or more in any ratio. The content of the binder relative to the negative electrode active material is typically 0.1 to 20% by mass. In particular, when the binder contains a rubbery polymer, such as SBR, as a primary component, the content of the binder relative to the negative electrode active material is typically 0.1 to 5% by mass. When the binder contains a fluorine-based polymer, such as polyvinylidene fluoride, as a main component, the content of the binder relative to the negative electrode active material is usually 1 to 15 mass %.

[0150] [2-2-2-4. Thickener] A thickener is typically used to adjust the viscosity of the slurry. There are no particular limitations on the thickener, but specific examples include carboxymethyl cellulose and its salts, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, and the like. These may be used alone or in combination of two or more in any ratio. When a thickener is used, the content of the thickener relative to the negative electrode active material is typically 0.001 to 5% by mass.

[0151] [2-2-2-5. Current Collector] Any known current collector can be used as the current collector that holds the negative electrode active material. Examples of negative electrode current collectors include metal materials such as aluminum, copper, nickel, stainless steel, and nickel-plated steel, with copper being particularly preferred from the standpoints of ease of processing and cost. Examples of the shape of the negative electrode current collector include metal foil, metal cylinder, metal coil, metal plate, metal thin film, expanded metal, punched metal, and foamed metal. Among these, metal foil or metal thin film is preferred. The metal thin film may be formed into a mesh shape as appropriate. When the negative electrode current collector is in the shape of a plate or film, the thickness of the current collector is optional, but is typically 1 μm to 1 mm.

[0152] [2-2-2-6. Thickness of Negative Electrode Plate] The thickness of the negative electrode (negative electrode plate) is designed to match the positive electrode (positive electrode plate) to be used and is not particularly limited, but the thickness of the negative electrode active material layer obtained by subtracting the thickness of the current collector from the thickness of the negative electrode material is usually 15 to 300 μm.

[0153] [2-2-2-7. Surface Coating of Negative Electrode Plate] The negative electrode plate may have a surface-adhered substance having a different composition from the negative electrode active material. Examples of the surface-adhered substance include oxides such as aluminum oxide, sulfates such as lithium sulfate, and carbonates such as lithium carbonate.

[0154] [2-3. Separator] A separator is usually interposed between the positive electrode and the negative electrode to prevent short-circuiting. In this case, the non-aqueous electrolyte is usually impregnated into the separator. There are no particular restrictions on the material or shape of the separator, and any known separator can be used as long as it does not impair the effects of the present invention.

[0155] [2-4. Battery Design] [2-4-1. Electrode Group] The electrode group may have either a laminated structure in which the positive electrode plate and the negative electrode plate are sandwiched between the separator, or a structure in which the positive electrode plate and the negative electrode plate are spirally wound with the separator sandwiched between them. The ratio of the volume of the electrode group to the internal volume of the battery (electrode group occupancy rate) is usually 40 to 90%.

[0156] [2-4-2. Current collecting structure] When the electrode group has the aforementioned laminated structure, a structure formed by bundling the metal core portions of each electrode layer and welding them to a terminal is preferably used. A structure in which multiple terminals are provided within the electrode to reduce resistance is also preferably used. When the electrode group has the aforementioned wound structure, the internal resistance can be reduced by providing multiple lead structures on each of the positive and negative electrodes and bundling them to a terminal.

[0157] [2-4-3. Protective Element] Protective elements that can be used include PTC (Positive Temperature Coefficient) elements whose resistance increases with heat generation due to excessive current, thermal fuses, thermistors, and valves (current cutoff valves) that cut off the current flowing in the circuit due to a sudden rise in the internal pressure or temperature of the battery during abnormal heat generation. It is preferable to select protective elements that will not operate under normal high-current use, and it is even more preferable to design the battery so that abnormal heat generation or thermal runaway does not occur even without a protective element.

[0158] [2-4-4. Exterior Body] A nonaqueous electrolyte battery is typically constructed by housing the nonaqueous electrolyte according to the present invention, a negative electrode, a positive electrode, a separator, and the like within an exterior body (exterior case). There are no limitations on the exterior body, and any known exterior body can be used as long as it does not impair the effects of the present invention. The material of the exterior case is not particularly limited as long as it is stable against the nonaqueous electrolyte used. However, from the viewpoints of weight reduction and cost, metals such as iron, aluminum, and aluminum alloys, or laminate films are preferably used. Iron is particularly preferred from the viewpoint of pressure resistance for operating the current cutoff valve. Examples of exterior cases using the above metals include those in which the metals are welded together by laser welding, resistance welding, or ultrasonic welding to form a sealed, airtight structure, or those in which the above metals are used via a resin gasket to form a crimped structure.

[0159] [2-4-5. Shape] The shape of the exterior case of the non-aqueous electrolyte battery is also arbitrary, and may be, for example, cylindrical, rectangular, laminated, coin-shaped, large, or the like.

[0160] The present invention will be explained in more detail below by way of examples and reference examples, but the present invention is not limited to these examples as long as it does not depart from the gist of the invention.

[0161] The compounds used in the present examples and comparative examples are shown below. Compound 1: Fluorodimethyloctylsilane [compound represented by formula (F1-4)] Compound 2: Cyclohexyldifluoromethylsilane [compound represented by formula (F2-12)] Compound 3: Lithium difluorophosphate (LiPO 2 F 2 ) [Specific anion-containing compounds] Compound 4: Lithium fluorosulfonate (FSO 3 Li) [specific anion-containing compound] Compound 5: lithium ethyl sulfate (CH 3 CH 2 SO 4 Li) [particular anion-containing compound] Compounds 1 and 2 used were those obtained in Synthesis Examples 1 and 2 below.

[0162] <Synthesis Examples> Various analytical methods used in the following synthesis examples are as follows. [Nuclear Magnetic Resonance (NMR) Analysis] 1 H. 13 C. 19 F-NMR was measured at 400, 101, and 376 MHz using a Bruker 400 Ultrashield. 3 ) and measured. [Gas Chromatography (GC) Analysis] 100 μL of the sample was dissolved in 1 mL of diethyl ether. The obtained solution was analyzed using a GC analyzer (Shimadzu Corporation, product name: GC-2010) under the following conditions. Column: DB-1 (length 30 m, inner diameter 0.32 mm, film thickness 0.25 μm, Agilent Technologies) Detector: FID Temperature: 40°C → 280°C, heating rate 10°C / min. Purity was calculated from the peak area %.

[0163] Synthesis Example 1 [Synthesis of Compound 1 (Fluorodimethyloctylsilane)] Methoxydimethyloctylsilane (5.00 g, 24.7 mmol) was added to a reactor, and boron trifluoride ether complex (1.05 mL, 8.40 mmol) was added under ice cooling, followed by stirring at 55°C for 1 hour. After distilling off low-boiling components, fluorodimethyloctylsilane (4.06 g, 21.3 mmol) was obtained by distillation purification. The purity estimated by GC analysis was 99%. 1 H-NMR, 13 C-NMR, 19 The results of F-NMR analysis were as follows: 1 H-NMR (400MHz, CDCl 3 ): 1.38-1.27 (m, 12H), 0.88 (t, J = 6.9Hz, 3H), 0.70-0.64 (m, 2H), 0.20 (d, J H-F =7.5Hz, 6H) 13 C-NMR (101MHz, CDCl 3 ): 33.1, 31.9, 29.3, 29.2, 22.7, 22.6, 16.5, 14.1, -1.4 19 F-NMR (376MHz, CDCl 3 ): -162.2

[0164] Synthesis Example 2 [Synthesis of Compound 2 (Cyclohexyldifluoromethylsilane)] Cyclohexyldimethoxymethylsilane (5.00 g, 26.5 mmol) was added to a reactor, and boron trifluoride ether complex (2.33 mL, 17.8 mmol) was added under ice cooling, followed by stirring at room temperature for 2 hours and at 45°C for 5 hours. After distilling off low-boiling components, cyclohexyldifluoromethylsilane (2.35 g, 14.3 mmol) was obtained by distillation purification. The purity estimated by GC analysis was 99%. 1 H-NMR, 13 C-NMR, and 19 The results of F-NMR analysis were as follows: 1 H-NMR (400MHz, CDCl 3 ): 1.80-1.71 (m, 5H), 1.35-1.24 (m, 5H), 0.96-0.90 (m, 1H), 0.29 (t, J H-F =6.5Hz, 3H)13 C-NMR (101MHz, CDCl 3 ): 27.1, 26.4, 25.2, 24.2, -6.2 19 F-NMR (376MHz, CDCl 3 ): -141.7

[0165] Examples 1 to 10 and Comparative Examples 1 to 8 [Preparation of Positive Electrode] Lithium nickel cobalt manganese composite oxide (Li 1.0 Ni 0.82 Co 0.11 Mn 0.07 O 2 ) ((Ni / M 1 95 parts by mass of the cation exchange polymer (molar ratio 0.82), 3 parts by mass of acetylene black as a conductive material, and 2 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed in N-methylpyrrolidone solvent using a disperser to form a slurry, which was uniformly applied to both sides of a 15 μm thick aluminum foil, dried, and pressed to form a positive electrode.

[0166] [Preparation of Negative Electrode] 97 parts by mass of natural graphite was mixed with 1 part by mass of an aqueous dispersion of sodium carboxymethyl cellulose (concentration of sodium carboxymethyl cellulose: 1.5% by mass) as a thickener and 1.5 parts by mass of an aqueous dispersion of styrene-butadiene rubber (concentration of styrene-butadiene rubber: 50% by mass) as a binder, and the mixture was mixed in a disperser to form a slurry. The resulting slurry was applied to one side of a 10 μm thick copper foil, dried, and then pressed to form a negative electrode.

[0167] [Preparation of non-aqueous electrolyte] In a dry argon atmosphere, a mixture of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (volume ratio EC:EMC = 3:7) was added to a non-aqueous electrolyte solution containing thoroughly dried LiPF as an electrolyte. 6 was dissolved in a concentration of 1.2 mol / L, and 1.0 mass % (as the concentration in the non-aqueous electrolyte solution) of vinylene carbonate (VC) was added (hereinafter referred to as "reference electrolyte solution 1"). Non-aqueous electrolyte solutions were prepared by adding compounds to reference electrolyte solution 1 in the amounts shown in Table 1 below. The "content (mass %)" in Table 1 is the content when the entire non-aqueous electrolyte solution is taken as 100 mass %.

[0168]

[0111]

[0112]

[0113]

[0114]

[0115]

[0116]

[0117]

[0118]

[0119]

[0120]

[0121]

[0122]

[0123]

[0124]

[0125]

[0126]

[0127]

[0128]

[0129]

[0130]

[0131]

[0132]

[0133]

[0134]

[0135]

[0136]

[0137]

[0138]

[0139]

[0140]

[0141]

[0142]

[0143]

[0144]

[0145]

[0146]

[0147]

[0148]

[0149]

[0150]

[0151]

[0152]

[0153]

[0154]

[0155]

[0156]

[0157]

[0158]

[0159]

[0160]

[0161]

[0162]

[0163]

[0164]

[0165]

[0166]

[0167]

[0168]

[0169]

[0170]

[0171]

[0172]

[0173]

[0174]

[0175]

[0176]

[0177]

[0178]

[0179]

[0180]

[0181]

[0182]

[0183]

[0184]

[0185]

[0186]

[0187]

[0188]

[0189]

[0190]

[0191]

[0192]

[0193]

[0194]

[0195] [

[0169] <Evaluation of Nonaqueous Electrolyte Batteries> [Initial Conditioning] In a thermostatic bath at 25°C, the nonaqueous electrolyte batteries prepared by the above method were subjected to constant current constant voltage charging (hereinafter referred to as "CC-CV charging") at 0.3 C to 4.4 V. Thereafter, aging was performed by holding at 45°C for 48 hours. Thereafter, the batteries were discharged to 2.8 V at 0.3 C to stabilize the nonaqueous electrolyte batteries. Further, CC-CV charging was performed at 0.3 C to 4.4 V, and then discharged at 0.3 C to 3.0 V to determine the "initial capacity." The batteries after the above initial conditioning were subjected to CC-CV charging at 0.2 C to half the initial discharge capacity. They were then discharged at 1.0 C at 25°C, and the voltage at 5 seconds was measured. The average value of the slope of the obtained current-voltage line was taken as the "initial resistance." After the initial conditioning, the battery was immersed in an ethanol bath and the volume was measured. The amount of gas generated was calculated from the change in volume before and after the initial conditioning, and this was designated as "initial gas."

[0170] [Charge storage test] After initial conditioning, the nonaqueous electrolyte battery was again subjected to CC-CV charging at 0.2 C to 4.4 V, and then subjected to high-temperature storage at 80 °C for 1 day. After that, the nonaqueous electrolyte battery was sufficiently cooled, immersed in an ethanol bath, and the volume was measured. The amount of gas generated was calculated from the change in volume before and after the storage test, and this was designated as the "80 °C storage gas amount." After the storage test, the cell was discharged to 2.8 V at 0.2 C to determine the "post-storage capacity." After CC-CV charging at 0.3 C to 4.4 V, the cell was discharged to 3.0 V at 0.3 C, and then CC-CV charging at 0.2 C to half the initial discharge capacity. The battery internal resistance after the storage test was determined, and this was designated the "post-storage resistance."

[0171] Using the data obtained above, the following increase rates of gas generation, internal resistance, and capacity retention were calculated: Increase rate of gas generation: ("Amount of gas stored at 80°C" / "Initial gas") x 100 Increase rate of internal resistance: ("Resistance after storage" / "Initial resistance") x 100 Capacity retention rate: ("Capacity after storage" / "Initial capacity") x 100 Table 1 below shows the increase rates of gas generation, internal resistance, and capacity retention rate.

[0172]

[0173] As can be seen from Table 1, Comparative Example 1, which does not contain either the compound represented by general formula (I) or the specific anion-containing compound, and Comparative Examples 2, 4, and 6 to 8, which do not contain either the compound represented by general formula (I) or the specific anion-containing compound, are unable to reduce the amount of gas generated during operation at high temperatures compared to the Examples. This is because a composite coating cannot be formed from the compound represented by general formula (I) and the specific anion-containing compound. Comparative Example 3, which contains the compound represented by general formula (I) and the specific anion-containing compound but does not satisfy formula (II), is unable to reduce the amount of gas generated during operation at high temperatures, and Comparative Example 5 is unable to suppress the decrease in capacity retention rate during operation at high temperatures. This is because if the ratio Z of the compound represented by general formula (I) to the specific anion-containing compound is not within an appropriate range, the compound represented by general formula (I) and the specific anion-containing compound cannot react properly, preventing the formation of a suitable composite coating. When the battery contains a compound represented by general formula (I) and a specific anion-containing compound and the ratio Z satisfies formula (II), the compound represented by general formula (I) and the specific anion-containing compound react favorably to form a favorable composite coating. As a result, it can be said that in Examples 1 to 10, the decrease in capacity retention rate and the increase in internal resistance during operation at high temperatures can be suppressed, and the amount of gas generated can be reduced.

[0174] The nonaqueous electrolyte battery of the present invention has improved capacity and discharge characteristics under high current density. Therefore, the nonaqueous electrolyte battery of the present invention can be suitably used in all fields of electronic devices, etc., where nonaqueous electrolyte batteries have traditionally been used. Furthermore, the nonaqueous electrolyte battery of the present invention can be used in a variety of known applications. Specific examples of applications include notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, mobile fax machines, mobile copiers, mobile printers, mobile audio players, compact video cameras, headphone stereos, video movie players, LCD televisions, handheld vacuum cleaners, portable CD players, minidisc players, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power supplies, motors, automobiles, motorcycles, mopeds, bicycles, lighting equipment, toys, game devices, watches, power tools, flash devices, cameras, home backup power supplies, business backup power supplies, load-leveling power supplies, and natural energy storage power supplies.

Claims

1. A non-aqueous electrolyte solution containing an electrolyte, a non-aqueous solvent, a compound represented by general formula (I), and at least one specific anion-containing compound selected from an anion-containing compound having a P=O bond and a P-F bond, an anion-containing compound having an S=O bond and an S-F bond, and an alkyl sulfate anion-containing compound, the non-aqueous electrolyte solution satisfying the following mathematical formula (II): (In formula (I), R 1 represents an alkyl group having 5 to 10 carbon atoms which may be substituted with a halogen atom; R 2 represents an alkyl group having 1 to 4 carbon atoms which may be substituted with a halogen atom, and n represents an integer of 1 to 3. 0<Z≦8 / n 2 (II) (In formula (II), Z represents the mass ratio (=[A] / [B]) of the content [A] of the compound represented by general formula (I) in the non-aqueous electrolyte to the content [B] of the specific anion-containing compound in the non-aqueous electrolyte, and n represents n of the compound represented by general formula (I).) 2. In the general formula (I), R 2 The nonaqueous electrolyte according to claim 1 , wherein is a methyl group.

3. The non-aqueous electrolyte according to claim 1, wherein in general formula (I), n is 1 or 2.

4. The nonaqueous electrolyte according to claim 1, wherein the specific anion-containing compound is an anion-containing compound having a P═O bond and a P-F bond.

5. The non-aqueous electrolyte solution according to claim 1, wherein the content of the compound represented by general formula (I) is 0.001 to 10 mass % based on the total amount of the non-aqueous electrolyte solution.

6. The non-aqueous electrolyte according to claim 1, wherein the content of the specific anion-containing compound is 0.001 to 5 mass % based on the total amount of the non-aqueous electrolyte.

7. A non-aqueous electrolyte battery comprising a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and a non-aqueous electrolyte, the non-aqueous electrolyte being the non-aqueous electrolyte according to any one of claims 1 to 6.

8. The nonaqueous electrolyte battery according to claim 7, wherein the positive electrode contains a positive electrode active material, and the positive electrode active material is a lithium transition metal oxide represented by the following composition formula (1): Li 1+y M 1 O 2 (1) (In the composition formula (1), y is −0.2 to 0.5, and M 1 represents a plurality of elements including at least Ni element, M 1 The molar ratio of the Ni element content to the total element content (Ni / M 1 ) is 0.40 to 1.

0.

9. The nonaqueous electrolyte battery according to claim 8, wherein the positive electrode active material is a lithium transition metal composite oxide represented by the following composition formula (2): Li a1 Ni b1 M 2 c1 O 2 In the composition formula (2), a1, b1, and c1 are numerical values ​​that satisfy 0.80≦a1≦1.10, 0.40≦b1≦0.99, and 0.01≦c1≦0.60, and b1+c1=1 is satisfied. M 2 contains at least one element selected from the group consisting of Co, Mn, Al, Mg, Zr, Fe, Ti and Er.

Citation Information

Patent Citations

  • Lithium secondary battery including an electrolyte additive

    US20190305372A1

  • Non-aqueous electrolyte solution and non-aqueous electrolyte solution secondary battery using same

    WO2015111676A1

  • Electrolyte and electrochemical device

    CN110854433A

  • High-temperature non-aqueous electrolyte solution and secondary battery

    CN115588779A

  • Nonaqueous electrolytic solution and secondary battery using the same

    JP2004171981A