Anolyte for extracting lithium from salt lake by means of electrochemical de-intercalation method, and lithium extraction device and method

By using an electrochemical deintercalation/intercalation method with alcohol solvents and supporting electrolytes during lithium extraction from salt lakes, combined with a monovalent anion exchange membrane, the problem of reduced lithium purity caused by sodium intercalation competition was solved, and high-purity lithium recovery was achieved.

WO2024229741A1PCT designated stage expired Publication Date: 2024-11-14GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/093219
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

In the process of lithium extraction from salt lakes or seawater, sodium-intercalated cathode materials compete with lithium-intercalated cathode materials, resulting in a decrease in the purity of recovered lithium. Improving the purity of lithium is a challenge.

Method used

Methanol, ethanol, or n-propanol are used as the anolyte solvent, combined with lithium bis(fluorosulfonyl)imide as the supporting electrolyte, and a monovalent anion exchange membrane is used to isolate the cathode and anode chambers. Lithium is extracted and recovered through an electrochemical deintercalation method. Taking advantage of the high solubility of lithium salts and the low solubility of sodium salts in alcohol solvents, a high-purity lithium solution is obtained through solid-liquid separation after electrolysis.

Benefits of technology

This effectively reduced the sodium ion content in the recovery liquid, improved the purity of lithium, and achieved efficient lithium recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023093219-FTAPPB-I100001
    Figure PCTCN2023093219-FTAPPB-I100001
Patent Text Reader

Abstract

An anolyte for extracting lithium from a salt lake by means of an electrochemical de-intercalation method, and a lithium extraction device and method. The anolyte comprises a solvent and a supporting electrolyte, wherein the solvent is at least one of methanol, ethanol and n-propanol, and the water content of the anolyte is lower than 100 ppm. In the lithium extraction device, a cathode chamber and an anode chamber are separated by using a monovalent anion exchange membrane, and ethanol and a supporting electrolyte are used as lithium extraction recovery liquids in the anode chamber. Since the solubility of lithium chloride in methanol, ethanol and n-propanol is high, and potassium chloride and sodium chloride are basically insoluble in methanol, ethanol and n-propanol, the sodium ions released into the recovery liquid during the process of electrolysis recovery of lithium form sodium chloride and then precipitate in the ethanol solution. After the electrolysis process is finished, a lithium-rich solution with relatively high purity can be obtained by means of solid-liquid separation.
Need to check novelty before this filing date? Find Prior Art

Description

Anolyte, lithium extraction device and method for extracting lithium from salt lakes using electrochemical deintercalation method Technical Field

[0001] The present disclosure relates to the technical field of lithium extraction from salt lakes, and in particular to an anode electrolyte, a lithium extraction device, and a method for extracting lithium from salt lakes using an electrochemical deintercalation method. Background Art

[0002] Lithium electroextraction is a method based on highly selective lithium ion screening and low-energy electrochemical redox methods to achieve the lithium extraction and insertion process. It effectively avoids the use of acids or strong oxidants and has become an emerging lithium extraction method with great development potential.

[0003] Researchers have developed a new type of 1 X FePO4 and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 The lithium extraction system uses O2 as the working electrode and Ag, Zn and polypyrrole (PPy) as the counter electrode. However, this process requires the lithium to be inserted and removed in steps, which reduces the lithium extraction efficiency to a certain extent. + , Mg 2+ , Na + , and K + In LiFePO4 / FePO4 structures[J]. Transactions of Nonferrous Metals Society of China, 2013, 23(4): 1157-1164), the LiFePO4 / FePO4 “rocking chair” structure electrode system was used to achieve simultaneous lithium extraction and recovery on different electrodes. Previous research by Zhao Mengyao et al. from Hebei University of Technology (Zhao Mengyao. Research on electrochemical lithium extraction based on LiMn2O4[D]. Hebei University of Technology, 2017) also developed a LiMn2O4 / Li with higher lithium extraction efficiency. 1 x Mn2O4 electrode system.

[0004] Although there have been breakthroughs in lithium extraction efficiency, the Li / Na concentration ratio of salt lake brine is between 0.0016-0.06, and the Li / Na concentration ratio in seawater is even lower, ranging from 1.69×10 -5 to 5.3×10 -5In actual production, when faced with such a low lithium-sodium ratio system, sodium-intercalated cathode materials easily compete with lithium-intercalated cathode materials, and the sodium embedded in the electrode material lattice is released into the recovery liquid, resulting in a decrease in the overall purity of the recovered lithium. Therefore, how to improve the purity of the recovered lithium is one of the bottlenecks limiting the use of electrochemical deintercalation methods for lithium extraction from salt lakes or seawater.

[0005] In view of this, the present disclosure is proposed.

[0006] Summary of the Invention

[0007] The purpose of the present disclosure is to provide an anolyte, a lithium extraction device and a method for extracting lithium from salt lakes by electrochemical deintercalation, so as to improve the lithium-sodium ratio of the anolyte and reduce the difficulty of subsequent lithium recovery.

[0008] The present disclosure is achieved as follows:

[0009] In a first aspect, the present disclosure provides an anode electrolyte for lithium extraction from salt lakes by an electrochemical deintercalation method, comprising a solvent and a supporting electrolyte, wherein the solvent is at least one of methanol, ethanol and n-propanol, and the water content in the electrolyte is less than 100 ppm.

[0010] In alternative embodiments, water is not included.

[0011] In an alternative embodiment, the supporting electrolyte comprises lithium bis(fluorosulfonyl)imide.

[0012] In an optional embodiment, the concentration of the supporting electrolyte is 30 mmol / L-100 mmol / L.

[0013] In a second aspect, the present disclosure provides a device for extracting lithium from salt lakes using an electrochemical deintercalation method, comprising:

[0014] an anode electrode for releasing lithium ions into the anolyte;

[0015] a cathode electrode for absorbing lithium ions from the cathode electrolyte;

[0016] an anode chamber for containing the anolyte according to any one of the preceding embodiments;

[0017] a cathode chamber for containing a catholyte;

[0018] Anion membrane: used to separate the anode chamber and the cathode chamber.

[0019] In an optional embodiment, a water absorbent is further added to the anolyte.

[0020] In an optional embodiment, the water absorbent is at least one of calcium oxide and molecular sieve.

[0021] In an optional embodiment, the mass of the water absorbent is 5%-15% of the mass of the anolyte.

[0022] In an optional embodiment, the anode electrode comprises LiFePO4, LiMn2O4, LiNi x Co y Mn (1-x-y) One of O2 or its doped modified derivatives; LiNi x Co y Mn (1-x-y) 0<x, y<1, 0<x+y<1 in O2.

[0023] In an optional embodiment, the cathode electrode comprises delithiated LiFePO4, LiMn2O4, LiNi x Co y Mn (1-x-y) One of O2 or its doped modified derivatives, LiNi x Co y Mn (1-x-y) 0<x, y<1, 0<x+y<1 in O2.

[0024] In an optional embodiment, the cathode electrode is an active material that releases lithium ions under the action of an electric field, and the active material includes LiFePO4, LiMn2O4, LiNi x Co y Mn (1-x-y) One of O2 or its doped modified derivatives, LiNi x Co y Mn (1-x-y) 0<x, y<1, 0<x+y<1 in O2.

[0025] In an alternative embodiment, the cathode electrolyte is brine.

[0026] In an optional embodiment, the Li / Na mass ratio in the brine is between 1.69×10 -5 -6×10 -2 between.

[0027] In an optional embodiment, the anion membrane is a monovalent anion exchange membrane.

[0028] In a third aspect, the present disclosure provides a method for extracting lithium from a salt lake using the electrochemical deintercalation method described in any one of the aforementioned embodiments, wherein a voltage is applied between the cathode electrode and the anode electrode so that the cathode electrode absorbs lithium ions in the cathode electrolyte, and / or the anode electrode releases lithium ions into the anode electrolyte.

[0029] In an optional embodiment, the anode electrolyte is subjected to solid-liquid separation to obtain a lithium-rich liquid as the liquid phase.

[0030] In an optional embodiment, the solid-liquid separation step is to filter the anolyte.

[0031] In an optional embodiment, the sodium-lithium mass ratio in the lithium-rich liquid is 1×10 -4 -1×10 -2 .

[0032] The present disclosure has the following beneficial effects:

[0033] In the process of lithium extraction, sodium ions and potassium ions are relatively similar in radius to lithium ions, and the sodium concentration in salt lake brine or seawater is relatively high. During the lithium extraction process, sodium ions are easily adsorbed on the electrode surface or embedded in the electrode material. As a result, during the process of releasing lithium ions from the electrode material, sodium ions are also released into the lithium-rich liquid in the anode chamber, resulting in a decrease in the purity of the lithium ions. The present invention uses a monovalent anion exchange membrane to separate the cathode chamber and the anode chamber, and the anode chamber uses alcohol and a supporting electrolyte as the lithium extraction recovery liquid. Since lithium chloride has a high solubility in methanol, ethanol and n-propanol, and potassium chloride and sodium chloride are basically insoluble in methanol, ethanol and n-propanol, the sodium ions released into the recovery liquid during the electrolytic recovery of lithium form sodium chloride, which precipitates in the ethanol solution. After the electrolysis process is completed, a high-purity lithium-rich solution can be obtained by solid-liquid separation. DETAILED DESCRIPTION

[0034] To make the purpose, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions in the embodiments of the present disclosure are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer were followed. Reagents or instruments used where the manufacturer is not specified are conventional products that can be purchased commercially.

[0035] This embodiment provides an anode electrolyte for lithium extraction from salt lakes using an electrochemical deintercalation method, comprising a solvent and a supporting electrolyte, wherein the solvent is at least one of methanol, ethanol, and n-propanol, and the water content in the electrolyte is less than 100 ppm.

[0036] In the process of lithium extraction, sodium ions and potassium ions are relatively similar in radius to lithium ions, and the sodium concentration in salt lake brine or seawater is relatively high. During the lithium extraction process, sodium ions are easily adsorbed on the electrode surface or embedded in the electrode material. As a result, during the process of releasing lithium ions from the electrode material, sodium ions are also released into the lithium-rich liquid in the anode chamber, resulting in a decrease in the purity of the lithium ions. The present invention uses a monovalent anion exchange membrane to separate the cathode chamber and the anode chamber, and the anode chamber uses alcohol and a supporting electrolyte as the lithium extraction recovery liquid. Since lithium chloride has a high solubility in methanol, ethanol and n-propanol, and potassium chloride and sodium chloride are basically insoluble in methanol, ethanol and n-propanol, the sodium ions released into the recovery liquid during the electrolytic recovery of lithium form sodium chloride, which precipitates in the ethanol solution. After the electrolysis process is completed, a high-purity lithium-rich solution can be obtained by solid-liquid separation.

[0037] Since methanol, ethanol and n-propanol have low ionization degrees and weak conductivity, if methanol, ethanol and n-propanol are used as anolytes, their conductivity needs to be improved, so supporting electrolytes are also added.

[0038] In some optional embodiments, water is not included. The presence of water will increase the solubility of sodium chloride, potassium chloride, etc. in the anolyte, thereby causing more sodium chloride and potassium chloride to dissolve in the anolyte. Even after subsequent solid-liquid separation, it is difficult to separate sodium chloride and lithium chloride, which is not conducive to improving the purity of recovered lithium. Therefore, the anolyte is optionally methanol, ethanol and n-propanol with a supporting electrolyte.

[0039] In some optional embodiments, the supporting electrolyte includes lithium bis(fluorosulfonyl)imide, which can be ionized in an alcohol solution and has high conductivity and thermal stability; other lithium salts such as lithium hexafluorophosphate have low solubility in alcohol solutions and low conductivity, thereby affecting the lithium extraction effect.

[0040] In some optional embodiments, the concentration of the supporting electrolyte is 30 mmol / L-100 mmol / L. If the concentration is too low, the conductivity of the solution is poor; but as the concentration increases, the viscosity of the electrolyte will also increase. Excessive viscosity will lead to reduced lithium extraction efficiency.

[0041] Another embodiment of the present disclosure provides a device for extracting lithium from salt lakes using an electrochemical deintercalation method, comprising:

[0042] an anode electrode for releasing lithium ions into the anolyte;

[0043] a cathode electrode for absorbing lithium ions from the cathode electrolyte;

[0044] an anode chamber for containing the anolyte according to any one of the preceding embodiments;

[0045] a cathode chamber for containing a catholyte;

[0046] Anion membrane: used to separate the anode chamber and the cathode chamber.

[0047] In some optional embodiments, a water absorbent is further added to the anode electrolyte, which can be used to absorb a small amount of water generated in the anode chamber during the lithium extraction process.

[0048] In some optional embodiments, the water absorbent is at least one of calcium oxide and molecular sieves. These water absorbents are almost insoluble in the solvent before and after absorbing water, making it easy to separate the water absorbent from the liquid by solid-liquid separation.

[0049] In some optional embodiments, the mass of the water absorbent is 5%-15% of the mass of the anolyte. If the amount of water absorbent is too small, the water-free environment of the anolyte cannot be guaranteed. A slightly excessive amount of water absorbent can reduce or avoid the presence of water in the anolyte to reduce the purity of the recovered lithium. However, if the amount added is too large, it will cause a waste of resources.

[0050] In some optional embodiments, the anode electrode includes LiFePO4, LiMn2O4, LiNi x Co y Mn (1-x-y) One of O2 or its doped modified derivatives; LiNi x Co y Mn (1-x-y) In O2, 0<x, y<1, 0<x+y<1. When the voltage is just applied, the anode electrode is in a lithium-saturated state. As the voltage application time increases, the lithium in the anode electrode active material is gradually released and gradually approaches the delithiated electrode active material serving as the cathode electrode.

[0051] In some optional embodiments, the cathode electrode includes LiaFePO4, LiaMn2O4, LiaNi x Co y Mn (1-x-y) One of O2 or its doped and modified derivatives, wherein 0<a<1, 0<x, y<1, 0<x+y<1, when the voltage is just applied, the cathode electrode is in a lithium-deficient state, and as the voltage application time increases, the lithium ions in the cathode electrolyte are gradually embedded in the cathode electrode active material, gradually approaching the lithium-saturated electrode active material serving as the cathode electrode.

[0052] In some optional embodiments, the cathode electrode is an active material that releases lithium ions under the action of an electric field, and the active material includes LiFePO4, LiMn2O4, LiNi x Co y Mn (1-x-y) One of O2 or its doped modified derivatives, LiNix Co y Mn (1-x-y) 0<x, y<1, 0<x+y<1 in O2.

[0053] In some optional embodiments, the cathode electrolyte is brine. Specifically, the brine may contain elements such as lithium, sodium, potassium, magnesium, and boron.

[0054] In some optional embodiments, the Li / Na mass ratio in the brine is between 1.69×10 -5 -6×10 -2 between.

[0055] In some optional embodiments, the anion membrane is a monovalent anion exchange membrane, for example, an ASV anion exchange membrane or an ACS anion exchange membrane.

[0056] Another embodiment of the present disclosure provides a method for extracting lithium from a salt lake using the electrochemical deintercalation method described in any one of the aforementioned embodiments, wherein a voltage is applied between the cathode electrode and the anode electrode so that the cathode electrode absorbs lithium ions in the cathode electrolyte and / or the anode electrode releases lithium ions into the anode electrolyte.

[0057] In some optional embodiments, the anode electrolyte is subjected to solid-liquid separation to obtain a lithium-rich liquid as the liquid phase.

[0058] In some optional embodiments, the solid-liquid separation step is to filter the anolyte.

[0059] In some optional embodiments, the mass ratio of sodium to lithium in the lithium-rich liquid is 1×10 -4 -1×10 -2 .

[0060] The features and performance of the present disclosure are further described in detail below with reference to the embodiments.

[0061] Specific embodiment 1:

[0062] This embodiment provides a method for extracting lithium, comprising the following steps:

[0063] (1) Preparation of lithium-extracting anode: The LiFePO4 active material and the conductive agent acetylene black, short carbon fiber, pore-forming agent NH4HCO3, PVDF and N-methylpyrrolidone are mixed evenly to form an electrode slurry (the amount of acetylene black, short carbon fiber, pore-forming agent NH4HCO3, PVDF and N-methylpyrrolidone is 10%, 2%, 20%, 10% and 150% of the mass of LiFePO4 respectively), and then the slurry is evenly coated on the current collector titanium mesh and dried to prepare a "lithium-saturated" LiFePO4 anode.

[0064] Preparation of lithium extraction cathode: The prepared LiFePO4 electrode was used as the anode, nickel foam was used as the cathode, and NaCl solution with a concentration of 20 g / L was used as the electrolyte. In addition, sulfuric acid was used to adjust the pH of the cathode solution to 2-3. A voltage of 1.0 V was applied until the current density was lower than 0.5 A / m 2 , which can produce lithium-deficient state Li 1x FePO4 electrode served as cathode.

[0065] (2) The electrolytic cell is divided into a cathode chamber and an anode chamber using an ASV monovalent anion exchange membrane. The cathode chamber contains brine, and the composition of the brine is 0.24 (g / L) Li, 98.56 (g / L) Na, 12.76 (g / L) Mg, 1.68 (g / L) K, 1.03 (g / L) B, and 11.17 (g / L) SO4 2- The anode chamber contains anhydrous ethanol solution and 50 mmol / L lithium bis(fluorosulfonyl)imide as supporting electrolyte, and the mass of calcium oxide added is 10% of the mass of the anode chamber solution.

[0066] (3) A voltage of 0.6 V was applied to the anode and cathode, and after electrolysis at room temperature of 15°C for 3.5 hours, the anode and cathode were exchanged and lithium extraction was carried out 8 times to enrich the lithium in the salt lake brine into the anode chamber.

[0067] (4) The lithium-rich liquid in the anode chamber is subjected to solid-liquid separation to obtain a lithium-containing liquid with a higher lithium purity.

[0068] Specific embodiment 2:

[0069] This embodiment provides a method for extracting lithium, comprising the following steps:

[0070] (1) Preparation of lithium-extracting anode: The LiMn2O4 active material and the conductive agent acetylene black, short carbon fiber, pore-forming agent NH4HCO3, PVDF and N-methylpyrrolidone are mixed evenly to form an electrode slurry (the amount of acetylene black, short carbon fiber, pore-forming agent NH4HCO3, PVDF and N-methylpyrrolidone is 10%, 2%, 20%, 10% and 150% of the mass of LiMn2O4 respectively). The slurry is then evenly coated on the current collector titanium mesh and dried to prepare a "lithium-saturated" LiMn2O4 anode.

[0071] Preparation of lithium cathode: The prepared LiMn2O4 electrode was used as the anode, nickel foam was used as the cathode, and NaCl solution with a concentration of 20 g / L was used as the electrolyte. In addition, sulfuric acid was used to adjust the pH of the cathode solution to 2-3. A voltage of 1.0 V was applied until the current density was lower than 0.5 A / m 2 , which can produce lithium-deficient state Li 1-x The Mn2O4 electrode served as the cathode.

[0072] (2) The electrolytic cell is divided into a cathode chamber and an anode chamber using an ASV monovalent anion exchange membrane. The cathode chamber contains brine, and the composition of the brine is 0.24 (g / L) Li, 98.56 (g / L) Na, 12.76 (g / L) Mg, 1.68 (g / L) K, 1.03 (g / L) B, and 11.17 (g / L) SO4 2- The anode chamber contains anhydrous ethanol solution and 30 mmol / L lithium bis(fluorosulfonyl)imide as supporting electrolyte, and the mass of calcium oxide added is 5% of the mass of the anode chamber solution.

[0073] (3) A voltage of 0.8 V was applied to the anode and cathode. After electrolysis at room temperature of 20°C for 3 hours, the anode and cathode were exchanged and lithium extraction was carried out 4 times to enrich the lithium in the salt lake brine into the anode chamber.

[0074] (4) The lithium-rich liquid in the anode chamber is subjected to solid-liquid separation to obtain a lithium-containing liquid with a higher lithium purity.

[0075] Specific embodiment 3:

[0076] This embodiment provides a method for extracting lithium, comprising the following steps:

[0077] (1) Preparation of lithium anode: LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 active material and conductive agent acetylene black, short carbon fiber, pore-forming agent NH4HCO3, PVDF and N-methylpyrrolidone are mixed evenly to prepare electrode slurry (the amount of acetylene black, short carbon fiber, pore-forming agent NH4HCO3, PVDF and N-methylpyrrolidone is respectively 1 / 3 Co 1 / 3 Mn 1 / 3 The slurry is evenly coated on the current collector titanium mesh and dried to prepare the "lithium saturated state" LiFePO4 anode.

[0078] Preparation of lithium cathode: Prepare the above-prepared LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 The O2 electrode was used as the anode, nickel foam was used as the cathode, and a 20 g / L NaCl solution was used as the electrolyte. In addition, sulfuric acid was used to adjust the pH of the solution to 2-3 at the cathode. A voltage of 1.0 V was applied until the current density was lower than 0.5 A / m 2 , which can produce lithium-deficient state Li 1-x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 The O2 electrode serves as the cathode.

[0079] (2) The electrolytic cell is divided into a cathode chamber and an anode chamber using an ASV monovalent anion exchange membrane. The cathode chamber contains brine, and the composition of the brine is 0.24 (g / L) Li, 98.56 (g / L) Na, 12.76 (g / L) Mg, 1.68 (g / L) K, 1.03 (g / L) B, and 11.17 (g / L) SO4 2- The anode chamber contains anhydrous ethanol solution and 75 mmol / L lithium bis(fluorosulfonyl)imide as supporting electrolyte, and the mass of the added molecular sieve is 15% of the mass of the anode chamber solution.

[0080] (3) A voltage of 1 V was applied to the anode and cathode. After electrolysis for 6 h at room temperature (10°C), the anode and cathode were exchanged and lithium extraction was carried out 8 times to enrich the lithium in the salt lake brine into the anode chamber.

[0081] (4) The lithium-rich liquid in the anode chamber is subjected to solid-liquid separation to obtain a lithium-containing liquid with a higher lithium purity.

[0082] Specific embodiment 4:

[0083] This embodiment provides a method for extracting lithium, comprising the following steps:

[0084] (1) Preparation of lithium-extracting anode: The LiFePO4 active material and the conductive agent acetylene black, short carbon fiber, pore-forming agent NH4HCO3, PVDF and N-methylpyrrolidone are mixed evenly to form an electrode slurry (the amount of acetylene black, short carbon fiber, pore-forming agent NH4HCO3, PVDF and N-methylpyrrolidone is 10%, 2%, 20%, 10% and 150% of the mass of LiFePO4 respectively), and then the slurry is evenly coated on the current collector titanium mesh and dried to prepare the "lithium saturated" LiFePO4 anode.

[0085] Preparation of lithium extraction cathode: The prepared LiFePO4 electrode was used as the anode, nickel foam was used as the cathode, and NaCl solution with a concentration of 20 g / L was used as the electrolyte. In addition, sulfuric acid was used to adjust the pH of the cathode solution to 2-3. A voltage of 1.0 V was applied until the current density was lower than 0.5 A / m 2 , which can produce lithium-deficient state Li 1x FePO4 electrode served as cathode.

[0086] (2) The electrolytic cell is divided into a cathode chamber and an anode chamber using an ASV monovalent anion exchange membrane. The cathode chamber contains brine, and the composition of the brine is 0.24 (g / L) Li, 298 (g / L) Na, 12.76 (g / L) Mg, 1.68 (g / L) K, 1.03 (g / L) B, and 11.17 (g / L) SO4 2- The anode chamber contains anhydrous ethanol solution and 100 mmol / L lithium bis(fluorosulfonyl)imide as supporting electrolyte, and the mass of the added molecular sieve is 10% of the mass of the anode chamber solution.

[0087] (3) A voltage of 0.4 V was applied to the anode and cathode. After electrolysis at room temperature of 15°C for 4 hours, the anode and cathode were exchanged and lithium extraction was carried out 6 times to enrich the lithium in the salt lake brine into the anode chamber.

[0088] (4) The lithium-rich liquid in the anode chamber is subjected to solid-liquid separation to obtain a lithium-containing liquid with a higher lithium purity.

[0089] Specific embodiment 5:

[0090] This embodiment provides a method for extracting lithium, which differs from Example 3 only in that ethanol is replaced by n-propanol.

[0091] Specific embodiment 6:

[0092] This embodiment provides a method for extracting lithium, which differs from Example 3 only in that ethanol is replaced by methanol.

[0093] Specific embodiment 7:

[0094] This embodiment provides a method for extracting lithium, which differs from Example 3 only in that ethanol is replaced by a mixture of ethanol and n-propanol in a volume ratio of 1:1.

[0095] Comparative Example 1:

[0096] The difference between Comparative Example 1 and Example 1 is that in step (2), the anode chamber is filled with 10 mmol / L lithium chloride aqueous solution as the electrolyte for lithium extraction.

[0097] Comparative Example 2:

[0098] The difference between Comparative Example 2 and Example 1 is that calcium oxide or other water-absorbing substances are not added in step (2) to extract lithium.

[0099] Comparative Example 3:

[0100] This comparative example provides a method for extracting lithium, which differs from Example 3 only in that the concentration of lithium bis(fluorosulfonyl)imide is 200 mmol / L.

[0101] Comparative Example 4:

[0102] This comparative example provides a method for extracting lithium, which differs from Example 3 only in that the anode chamber solution contains 0.5% water.

[0103] Comparative Example 5:

[0104] This comparative example provides a method for extracting lithium, which differs from Example 3 only in that ethanol is replaced by n-butanol.

[0105] Performance testing:

[0106] The lithium ion concentration and other impurity concentrations in brine and lithium-rich solution were tested using an inductively coupled plasma spectrometer (ICP). The results are shown in the following table.

[0107] As shown in Table 1, the mass ratio of sodium to lithium in the lithium-rich liquid obtained after electrolysis in the embodiment is 1.45×10 -3 -6.58×10 -4 The mass ratio of sodium to lithium in Comparative Example 1 is 0.358. The sodium to lithium ratio obtained by using ethanol as the recovery liquid is reduced by 2-3 orders of magnitude, indicating that the use of ethanol as the recovery liquid can effectively separate sodium and lithium and improve the purity of lithium in the recovery liquid. The sodium to lithium ratio in Comparative Example 2 is 8.04×10 -2 This indicates that the small amount of water contained in the ethanol recovery liquid has a certain impact on the separation of sodium and lithium, reducing the purity of the recovered lithium. In addition, since potassium chloride and sodium chloride have the same properties, their solubility in ethanol is smaller and their solubility in water is larger. Therefore, using ethanol as the recovery liquid is also beneficial to the separation of potassium and lithium, and improves the purity of lithium in the lithium recovery liquid. Industrial Applicability

[0108] The present invention uses a monovalent anion exchange membrane to separate the cathode chamber and the anode chamber, and uses alcohol and a supporting electrolyte as lithium extraction recovery liquid in the anode chamber. Since lithium chloride has a high solubility in methanol, ethanol and n-propanol, and potassium chloride and sodium chloride are basically insoluble in methanol, ethanol and n-propanol, the sodium ions released into the recovery liquid during the electrolytic lithium recovery process form sodium chloride, which precipitates in the ethanol solution. After the electrolysis process is completed, a high-purity lithium-rich solution can be obtained through solid-liquid separation, which has great application prospects.

Claims

1. An anolyte for extracting lithium from salt lakes by electrochemical deintercalation, characterized in that: The invention comprises a solvent and a supporting electrolyte, wherein the solvent is at least one of methanol, ethanol and n-propanol, and the water content in the electrolyte is less than 100 ppm.

2. The anolyte for extracting lithium from salt lakes by electrochemical deintercalation method according to claim 1, characterized in that: Water not included.

3. The anolyte for extracting lithium from salt lakes by electrochemical deintercalation method according to claim 1 or 2, characterized in that: The supporting electrolyte includes at least one lithium bis(fluorosulfonyl)imide.

4. The anolyte for extracting lithium from salt lakes by electrochemical deintercalation method according to any one of claims 1 to 3, characterized in that: The concentration of the supporting electrolyte is 30 mmol / L-100 mmol / L.

5. An electrochemical deintercalation method for extracting lithium from salt lakes, characterized in that: include: an anode electrode for releasing lithium ions into an anode electrolyte; a cathode electrode for absorbing lithium ions from the cathode electrolyte; an anode chamber for containing the anolyte according to any one of claims 1 to 4; a cathode chamber for containing a cathode electrolyte; Anion membrane: used to separate the anode chamber and the cathode chamber.

6. The electrochemical deintercalation method for extracting lithium from salt lakes according to claim 5, characterized in that: A water absorbing agent is also added to the anode electrolyte.

7. The electrochemical deintercalation method for extracting lithium from salt lakes according to claim 6, characterized in that: The water absorbent is at least one of calcium oxide and molecular sieve.

8. The electrochemical deintercalation method for extracting lithium from salt lakes according to claim 6 or 7, characterized in that: The mass of the water absorbent is 5%-15% of the mass of the anolyte.

9. The electrochemical deintercalation method for extracting lithium from salt lakes according to any one of claims 5 to 8, characterized in that: The anode electrode includes LiFePO4, LiMn2O4, LiNi x Co y Mn (1-x-y) One of O2 or its doped modified derivatives; LiNi x Co y Mn (1-x-y) 0<x, y<1, 0<x+y<1 in O2.

10. The device for extracting lithium from salt lakes by electrochemical deintercalation method according to any one of claims 5 to 9, characterized in that: The cathode electrode includes LiaFePO4, LiaMn2O4, LiaNi x Co y Mn (1-x-y) One of O2 or its doped modified derivatives, wherein 0<a<1, 0<x, y<1, 0<x+y<1.

11. The device for extracting lithium from salt lakes by electrochemical deintercalation method according to any one of claims 5 to 10, characterized in that: The cathode electrode is obtained by releasing lithium ions from active materials under the action of an electric field. The active materials include LiFePO4, LiMn2O4, LiNi x Co y Mn (1-x-y) One of O2 or its doped modified derivatives, LiNi x Co y Mn (1-x-y) 0<x, y<1, 0<x+y<1 in O2.

12. The electrochemical deintercalation method for extracting lithium from salt lakes according to any one of claims 5 to 11, characterized in that: The cathode electrolyte is brine.

13. The electrochemical deintercalation method for extracting lithium from salt lakes according to claim 12, characterized in that: The mass ratio of Li / Na in the brine is between 1.69×10 -5 -6×10 -2 between.

14. The electrochemical deintercalation method for extracting lithium from salt lakes according to any one of claims 5 to 13, characterized in that: The anion membrane is a monovalent anion exchange membrane.

15. A method for extracting lithium from a salt lake using the electrochemical deintercalation method lithium extraction device according to any one of claims 5 to 14, characterized in that: A voltage is applied between the cathode electrode and the anode electrode, causing the cathode electrode to absorb lithium ions in the cathode electrolyte and / or the anode electrode to release lithium ions into the anode electrolyte.

16. The method for extracting lithium from salt lakes by electrochemical deintercalation according to claim 15, characterized in that: The anode electrolyte is subjected to solid-liquid separation to obtain a liquid phase which is a lithium-rich liquid.

17. The method for extracting lithium from salt lakes by electrochemical deintercalation according to claim 16, characterized in that: The solid-liquid separation step is to filter the anolyte.

18. The method for extracting lithium from salt lakes by electrochemical deintercalation according to claim 16 or 17, characterized in that: The mass ratio of sodium to lithium in the lithium-rich liquid is 1×10 -4 -1×10 -2 .

Citation Information

Patent Citations

  • Device and method for electrochemically preparing high-purity battery-grade lithium hydroxide

    CN110616438A

  • Method for extracting lithium from salt lake brine

    CN115818801A

  • Method and device for extracting and enriching lithium

    US20130186760A1

  • Method for preparing lithium hydroxide from lithium-containing low-magnesium brine

    WO2021190402A1