Method for evaluating lithium-ion battery material and use thereof
Patent Information
- Application Number
- PCT/CN2023/093418
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-14
Smart Images

Figure PCTCN2023093418-FTAPPB-I100001 
Figure PCTCN2023093418-FTAPPB-I100002 
Figure PCTCN2023093418-FTAPPB-I100003
Abstract
Description
A method for evaluating lithium-ion battery materials and its application Technical Field
[0001] The present disclosure relates to the field of lithium-ion batteries, for example, a method for evaluating lithium-ion battery materials and applications thereof. Background Art
[0002] Lithium-ion batteries have achieved success due to their high energy density, long cycle life, and excellent rate performance, making them widely used in portable consumer electronics, electric vehicles, energy storage, and other fields. However, at high temperatures, the interface between the electrode material and the electrolyte in lithium-ion batteries becomes more complex, resulting in not only performance loss at high temperatures but also potential safety issues, such as gas generation that can cause battery swelling, potentially posing a potential safety hazard.
[0003] Therefore, high-temperature performance testing of lithium-ion battery cathode materials is essential. Currently, the high-temperature storage performance of cathode materials and the lithium batteries containing them is often evaluated by preparing soft-pack full cells. This is done by testing the changes in electrical performance and swelling before and after storage at different times or temperatures while fully charged. By comparing the degree of change in electrical performance indicators and the degree of battery swelling, reliability and safety are measured.
[0004] CN108267693B discloses a rapid evaluation method for the high-temperature storage performance of lithium battery cathode materials. The method uses lithium-ion button-type half-cells to perform high-temperature float charging on the cathode materials. Based on the float charge capacity test data, the differences in high-temperature storage performance between different cathode materials can be inferred. However, this rapid evaluation method can only infer differences in high-temperature storage performance between different cathode materials and cannot intuitively characterize the performance changes of the cathode materials during high-temperature storage.
[0005] CN110658473B discloses a rapid evaluation method for the high-temperature storage performance of lithium battery cathode materials. This method simulates the environmental conditions of the cathode material in full-battery high-temperature storage, prepares a delithiated cathode material through chemical delithiation, and conducts an equivalent high-temperature storage test on the delithiated cathode material. The capacity retention rate is evaluated based on the initial discharge capacity ratio. This method obtains the delithiated cathode material by increasing the oxidant. During the reaction with the oxidant, the interface becomes complex, and the amount of delithiation cannot be guaranteed. When the battery is re-prepared into a button cell, the discharge capacity is unstable, reducing the reliability of the evaluation.
[0006] From the above, it can be seen that there is still a need to develop a new evaluation method for quickly judging the high-temperature storage performance of lithium-ion battery positive electrode materials in order to improve test efficiency and reduce evaluation costs.
[0007] Summary of the Invention
[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0009] The present disclosure provides a method for evaluating lithium-ion battery materials and its application. The evaluation method first prepares the positive electrode material to be tested into a delithiated positive electrode material, then places it in an electrolyte and heats and stirs it. The filtrate obtained after solid-liquid separation is used for ICP testing to obtain the main element dissolution data. At the same time, the obtained powder is subjected to EIS testing to obtain the interface charge transfer impedance R CT The high temperature storage performance of the soft pack battery containing the positive electrode material to be tested is comprehensively evaluated based on the two obtained data. The evaluation method can simulate the actual high temperature reaction process of the positive electrode material and the electrolyte to obtain the fully charged positive electrode material and obtain its main element dissolution data and R CT The value can be used to quickly infer and evaluate the high-temperature storage performance of the positive electrode material. The evaluation method is simple to operate and has low cost, which is conducive to improving the evaluation efficiency.
[0010] To achieve this goal, the present disclosure adopts the following technical solutions:
[0011] In a first aspect, an embodiment of the present disclosure provides a method for evaluating lithium-ion battery materials, the method comprising the following steps:
[0012] (1) preparing the positive electrode material to be tested as a delithiation positive electrode material;
[0013] (2) placing the delithiated positive electrode material described in step (1) in an electrolyte, heating and stirring, and performing solid-liquid separation to obtain a filtrate and a powder;
[0014] (3) The filtrate obtained in step (2) is subjected to ICP (Inductively Coupled Plasma) testing to obtain the main element dissolution data; at the same time, the powder obtained in step (2) is used as the positive electrode material to prepare a button half-cell, and an EIS (Electrochemical Impedance Spectroscopy) test is performed to obtain the interface charge transfer impedance R CT value;
[0015] (4) The main element dissolution data and R obtained in step (3) CT The larger the value, the worse the high-temperature storage performance of the positive electrode material to be tested.
[0016] The evaluation method of the embodiment of the present disclosure prepares the positive electrode material into a delithiated positive electrode material to simulate the actual high-temperature reaction process of the positive electrode material and the electrolyte, and makes the positive electrode material fully charged (delithiated state), and then performs a test to obtain the main element dissolution data and R CTThe value can be used to quickly infer and evaluate the high-temperature storage performance of the positive electrode material. The evaluation method is simple to operate and has low cost, which is conducive to improving the evaluation efficiency.
[0017] The embodiments of the present disclosure do not impose any specific restrictions on the electrolyte used. Those skilled in the art can select an electrolyte suitable for the positive electrode material to be tested.
[0018] Exemplarily, based on the total mass of 100wt%, the electrolyte includes 9-15wt% of lithium salt, 77-88wt% of non-aqueous organic solvent and 3-8wt% of additives; the lithium salt includes at least one of lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6) or a new lithium salt lithium bis(fluorosulfonyl)imide (LiFSI); the non-aqueous organic solvent includes at least one of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC) or ethyl methyl carbonate (EMC); the additive includes at least one of a film-forming additive, a high / low temperature additive, an overcharge protection additive, a flame retardant additive, and a rate-type additive, for example, vinylene carbonate (VC) and / or fluoroethylene carbonate (FEC) can be selected.
[0019] The following are optional technical solutions for the embodiments of the present disclosure, but are not intended to limit the technical solutions provided by the present disclosure. Through the following technical solutions, the technical objectives and beneficial effects of the present disclosure can be better achieved and realized.
[0020] As an optional technical solution of the embodiment of the present disclosure, the positive electrode material to be tested in step (1) includes any one or a combination of at least two of lithium cobalt oxide, lithium iron phosphate or a ternary positive electrode material. Typical but non-limiting examples of the combination include a combination of lithium cobalt oxide and lithium iron phosphate, a combination of lithium cobalt oxide and a ternary positive electrode material, or a combination of lithium iron phosphate and a ternary positive electrode material.
[0021] As an optional technical solution of the embodiment of the present disclosure, the method for preparing the delithiated positive electrode material in step (1) includes:
[0022] An oxidant is added to the positive electrode material to be tested to carry out a delithiation reaction to obtain the delithiation positive electrode material.
[0023] As an optional technical solution of the embodiment of the present disclosure, the oxidant includes any one of hypobromous acid, metaperiodic acid, hypochlorous acid, chlorous acid, permanganic acid, perbromic acid or hydrogen peroxide, or a combination of at least two thereof. Typical but non-limiting examples of the combination include a combination of hypobromous acid and metaperiodic acid, a combination of metaperiodic acid and hypochlorous acid, a combination of chlorous acid and permanganic acid, a combination of permanganic acid and perbromic acid, and a combination of chlorous acid and hydrogen peroxide.
[0024] In one embodiment, the amount of the oxidant is 4 to 8 mL per gram of the positive electrode material to be tested, for example, 4 mL, 4.5 mL, 5 mL, 5.5 mL, 6 mL, 6.5 mL, 7 mL, 7.5 mL or 8 mL, and the concentration of the oxidant is 1.4 to 8 mol / L, for example, 1.4 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, 5.5 mol / L, 6 mol / L, 6.5 mol / L, 7 mol / L, 7.5 mol / L or 8 mol / L, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0025] As an optional technical solution of the embodiment of the present disclosure, the delithiation reaction is carried out under stirring.
[0026] In one embodiment, the delithiation reaction time is 18 to 22 hours, such as 18 hours, 19 hours, 20 hours, 21 hours or 22 hours, but is not limited to the listed values. Other values not listed within the above numerical range are also applicable.
[0027] As an optional technical solution of the embodiment of the present disclosure, the solid-liquid ratio of the delithiated positive electrode material to the electrolyte in step (2) is 1g:(1.5~2.5)g, for example, 1g:1.5g, 1g:1.6g, 1g:1.7g, 1g:1.8g, 1g:1.9g, 1g:2g, 1g:2.1g, 1g:2.2g, 1g:2.3g, 1g:2.4g or 1g:2.5g, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0028] In one embodiment, the amount of the electrolyte is 20 to 200 mL, for example, 20 mL, 50 mL, 80 mL, 110 mL, 140 mL, 170 mL or 200 mL, but is not limited to the listed values. Other values not listed within the above numerical range are also applicable.
[0029] As an optional technical solution of the embodiment of the present disclosure, the heating and stirring in step (3) is carried out in a vacuum or dehumidified environment.
[0030] The heating and stirring described in the embodiments of the present disclosure need to be carried out in a vacuum or dehumidified environment to prevent the electrolyte from absorbing moisture. After obtaining the filtrate, it should also be sealed and stored to prevent water absorption.
[0031] In one embodiment, the heating and stirring in step (3) is carried out in a hydrothermal kettle with a polytetrafluoroethylene liner.
[0032] In one embodiment, the temperature of the heating and stirring in step (3) is 40 to 80°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0033] In one embodiment, the heating and stirring time in step (3) is 2 to 4 hours, for example, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, 3 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours or 4 hours, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0034] In one embodiment, the stirring rate of the heating and stirring in step (3) is 80 to 200 r / min, for example, 80 r / min, 100 r / min, 120 r / min, 140 r / min, 160 r / min, 180 r / min or 200 r / min, etc., but is not limited to the listed values. Other values not listed within the above numerical range are also applicable.
[0035] As an optional technical solution of the embodiment of the present disclosure, step (4) of the evaluation method further includes:
[0036] The main element dissolution data and standard R CT The value is associated with the high temperature storage performance of the soft pack battery containing the positive electrode material to be tested, and a database is established to simulate the linear relationship between the main element dissolution data and the high temperature storage performance and / or simulate the R CT The linear relationship between the value and the high temperature storage performance is calculated according to the linear relationship. The high temperature storage performance of the soft-pack battery containing the positive electrode material to be tested is inferred.
[0037] In one embodiment, the database includes at least 10 different main element dissolution data of the positive electrode materials to be tested, standard R CT Values and high temperature storage performance data of soft-pack batteries containing the positive electrode material to be tested.
[0038] As an optional technical solution of the embodiment of the present disclosure, the evaluation method includes the following steps:
[0039] (1) adding an oxidant to the positive electrode material to be tested, wherein the amount of the oxidant is 4 to 8 mL per gram of the positive electrode material to be tested, and the concentration of the oxidant is 1.4 to 8 mol / L, and performing a delithiation reaction for 18 to 22 hours under stirring to obtain the delithiation positive electrode material; the positive electrode material to be tested includes any one or a combination of at least two of lithium cobalt oxide, lithium iron phosphate or a ternary positive electrode material; the oxidant includes any one or a combination of at least two of hypobromous acid, metaperiodic acid, hypochlorous acid, chlorous acid, permanganic acid, perbromic acid or hydrogen peroxide;
[0040] (2) In a dehumidified room, the delithiation positive electrode material and the electrolyte of step (1) are placed in a polytetrafluoroethylene liner in a hydrothermal kettle at a solid-liquid ratio of 1 g: (1.5-2.5) g and mixed evenly to make the amount of electrolyte 20-200 mL, and then the hydrothermal kettle is placed in an oven preheated to 40-80° C., the stirring rate is set to 80-200 r / min, and the heating and stirring are carried out for 2-4 hours. After the reaction is completed, the filter is filtered to obtain a powder, and the obtained powder is washed and dried for use;
[0041] (3) The filtrate obtained in step (2) is subjected to ICP testing to obtain the main element dissolution data; at the same time, the powder in step (2) is used as the positive electrode material to prepare a button half-cell, and an EIS test is performed to obtain the interface charge transfer impedance R CT value;
[0042] (4) According to the main element dissolution data and R obtained in step (3) CT The high temperature storage performance of the soft pack battery containing the positive electrode material to be tested is evaluated by the value, and the main element dissolution data and R CT The larger the value, the worse the high temperature storage performance of the cathode material to be tested; and the main element dissolution data and standard R CT The value is associated with the high temperature storage performance of the soft pack battery containing the positive electrode material to be tested, and a database including at least 10 sample data is established to simulate the linear relationship between the main element dissolution data and the high temperature storage performance and / or simulate the R CT The linear relationship between the value and the high temperature storage performance is calculated; and the high temperature storage performance of the soft-pack battery containing the positive electrode material to be tested is inferred according to the linear relationship.
[0043] In a second aspect, an embodiment of the present disclosure provides an application of the evaluation method according to the first aspect in the field of lithium-ion battery manufacturing.
[0044] Compared with the related technical solutions, the present disclosure has at least the following beneficial effects:
[0045] The evaluation method can simulate the actual high-temperature reaction process of the positive electrode material and the electrolyte to obtain the fully charged positive electrode material and obtain its main element dissolution data and RCT The value can be used to quickly infer and evaluate the high-temperature storage performance of the positive electrode material. The evaluation method is simple to operate and has low cost, which is conducive to improving the evaluation efficiency.
[0046] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0047] The technical solution of the present disclosure is further illustrated below through specific implementation methods.
[0048] It should be apparent to those skilled in the art that the embodiments are only intended to help understand the present disclosure and should not be considered as specific limitations of the present disclosure.
[0049] The electrolyte used in the following examples and comparative examples is the lithium ion battery electrolyte provided by CN115117445A, which comprises a lithium salt, a non-aqueous organic solvent and an additive; specifically, in an argon atmosphere glove box with a water content of <10 ppm, ethylene carbonate, diethyl carbonate, ethyl methyl carbonate and fluoroethylene carbonate are mixed according to a mass percentage of 20 wt%, 30 wt%, 40 wt% and 10 wt% to obtain a mixed organic solvent, and then the fully dried lithium salt is dissolved in the mixed organic solvent. The lithium salt is hexafluorophosphorus. The invention discloses a mixture of lithium hexafluorophosphate and lithium difluorobisoxalatophosphate, wherein the concentration of the lithium salt in the electrolyte is 1 mol / L, wherein the molar ratio of lithium hexafluorophosphate and lithium difluorobisoxalatophosphate is 95:5, and the additive is a mixture of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, vinylene carbonate and vinyl sulfate, wherein the addition amount of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, vinylene carbonate and vinyl sulfate each accounts for 1wt% of the total mass of the electrolyte, and after adding the additives and stirring evenly, the electrolyte is obtained.
[0050] Example 1
[0051] This embodiment provides a method for evaluating lithium-ion battery materials, which is used to evaluate the high-temperature storage performance of lithium cobalt oxide positive electrode materials. The method includes the following steps:
[0052] (1) Preparation of delithiated lithium cobalt oxide materials: Four groups of different lithium cobalt oxide materials were selected and labeled as lithium cobalt oxide-1, lithium cobalt oxide-2, lithium cobalt oxide-3, and lithium cobalt oxide-4, and four parallel samples were prepared for each group of lithium cobalt oxide; the delithiation process was carried out in an argon-filled glove box, 5 g of the above lithium cobalt oxide materials were placed in a beaker, 30 mL of a 6.6 mol / L hydrogen peroxide H2O2 solution was added, a magnetic stirrer was placed and the speed was set to 45 r / min, and the mixture was stirred for 20 h to obtain delithiated lithium cobalt oxide; the obtained solution was quickly filtered and deionized water was used to remove residual impurities, and the obtained delithiated lithium cobalt oxide material was dried in a vacuum oven for 8 h;
[0053] (2) Electrolyte powder reaction: The four different delithiated lithium cobalt oxide materials prepared in step (1) were mixed with the electrolyte respectively. To prevent the electrolyte from absorbing moisture, the delithiated lithium cobalt oxide materials and the electrolyte were placed in a hydrothermal kettle in a dehumidification room. 5 g of the delithiated lithium cobalt oxide material was taken, 10 g of the electrolyte was added, and after sealing, the mixture was placed in an oven preheated to 70° C. The stirring setting was turned on and the stirring speed in the hydrothermal kettle was 120 r / min. After the reaction was completed, the solution was quickly filtered to obtain a filtrate and a powder. The powder was repeatedly washed with ethanol to remove electrolyte impurities and then dried in a vacuum oven for 8 h.
[0054] (3) Testing: The filtrate obtained in step (2) is subjected to ICP testing to obtain the main element cobalt dissolution data of the electrode; a certain amount of materials are weighed according to the mass ratio of positive electrode material (lithium cobalt oxide): conductive carbon black: PVDF = 94%: 3%: 3%, PVDF is dissolved in a certain amount of NMP, the positive electrode material and conductive carbon black are added, and the mixture is placed in a blender and stirred for 35 minutes, and the above materials are evenly mixed to make a uniform positive electrode slurry. The prepared positive electrode slurry is evenly coated on aluminum foil to make a electrode, and dried in an oven at 120°C to make a positive electrode sheet for standby use; the positive electrode sheet is assembled with a diaphragm, a lithium sheet, an electrolyte, etc. into a button half-cell. The button half-cell is subjected to EIS testing, the frequency range of the EIS test is 0.05~106Hz, and the EIS test is completed within 1.5h;
[0055] (4) Analysis: The results obtained in step (3) are shown in Table 2. The data on the amount of cobalt element dissolved and R CT The value is the average of 4 parallel samples in each group of lithium cobalt oxide. At the same time, in order to more intuitively demonstrate the high-temperature storage performance of the lithium cobalt oxide material, lithium cobalt oxide-1, lithium cobalt oxide-2, lithium cobalt oxide-3, and lithium cobalt oxide-4 before delithiation were prepared into soft-pack full batteries and subjected to high-temperature storage tests at 60°C to obtain storage performance data (capacity retention rate), which are recorded together in Table 1.
[0056] Table 1
[0057] As can be seen from Table 1, the high temperature storage performance of different groups of lithium cobalt oxide is positively correlated with the amount of cobalt element dissolved. At the same time, the high temperature storage performance is also positively correlated with the charge transfer impedance value of the EIS test. The obtained cobalt element dissolution data and R CT The larger the value, the worse the high-temperature storage performance of the positive electrode material to be tested.
[0058] The above description shows that the evaluation method provided in this embodiment can effectively and quickly evaluate the storage performance of lithium cobalt oxide positive electrode materials.
[0059] Example 2
[0060] This embodiment provides a method for evaluating lithium-ion battery materials, which is used to evaluate the high-temperature storage performance of ternary cathode materials. The method includes the following steps:
[0061] (1) Preparation of delithiated ternary cathode materials: Four groups of different ternary cathode materials were selected and labeled as ternary-1, ternary-2, ternary-3, and ternary-4, and four parallel samples were prepared for each group of ternary cathode materials; the delithiation process was carried out in an argon-filled glove box, 8 g of the ternary material was placed in a beaker, 50 ml of a 2 mol / L hypochlorous acid solution was added, a magnetic stirrer was placed and the speed was set to 55 r / min, and the mixture was stirred for 24 h to obtain the delithiated ternary cathode material; the obtained solution was quickly filtered and deionized water was used to remove residual impurities, and the obtained delithiated ternary cathode material was dried in a vacuum oven for 10 h;
[0062] (2) Electrolyte powder reaction: The delithiation ternary cathode material prepared in step (1) was mixed with the electrolyte respectively. To prevent the electrolyte from absorbing moisture, it was placed in a hydrothermal kettle in a dehumidification room. 5 g of cathode material powder was taken, and 11 g of electrolyte was added. After sealing, it was placed in an oven preheated to 65°C, and the stirring setting was turned on at a stirring speed of 180 r / min. After the reaction was completed, the solution was quickly filtered to obtain a filtrate and a powder. The powder was repeatedly washed with ethanol to remove electrolyte impurities, and then dried in a vacuum oven for 12 h.
[0063] (3) Testing: The filtrate obtained in step (2) is subjected to ICP testing to obtain the main element manganese dissolution data of the electrode; a certain amount of materials are weighed according to the mass ratio of ternary positive electrode material: conductive carbon black: PVDF = 94%: 3%: 3%, PVDF is dissolved in a certain amount of NMP, the positive electrode material and conductive carbon black are added, and the mixture is placed in a blender and stirred for 35 minutes, and the above materials are evenly mixed to make a uniform positive electrode slurry. The prepared positive electrode slurry is evenly coated on aluminum foil to make a pole piece, and dried in an oven at 120°C to make a positive electrode sheet for standby use; the positive electrode sheet is assembled with a diaphragm, a lithium sheet, an electrolyte, etc. into a button half-cell. The button half-cell is subjected to EIS testing, the frequency range of the EIS test is 0.05~106Hz, and the EIS test is completed within 1.5h;
[0064] (4) Analysis: The results obtained in step (3) are shown in Table 4. The data on the amount of manganese element dissolved and R CT The value is the average of four parallel samples in each group of ternary cathode materials. At the same time, in order to more intuitively demonstrate the high-temperature storage performance of the ternary cathode materials, ternary-1, ternary-2, ternary-3, and cobalt ternary-4 before delithiation were prepared into soft-pack full batteries and subjected to high-temperature storage tests at 60°C to obtain storage performance data (capacity retention rate), which are recorded together in Table 2.
[0065] Table 2
[0066] As can be seen from Table 2, the high temperature storage performance of different groups of ternary cathode materials is positively correlated with the amount of manganese element dissolved. At the same time, the high temperature storage performance is also positively correlated with the charge transfer impedance value of the EIS test. The obtained manganese element dissolution data and R CT The larger the value, the worse the high-temperature storage performance of the positive electrode material to be tested.
[0067] The above description shows that the evaluation method provided in this embodiment can effectively and quickly evaluate the storage performance of ternary cathode materials.
[0068] Comparative Example 1
[0069] This comparative example provides a method for evaluating lithium-ion battery materials. In step (3), the delithiated lithium cobalt oxide material is only mixed with the electrolyte, and heated and allowed to stand without stirring. Other conditions are exactly the same as those in Example 1.
[0070] Comparative Example 2
[0071] This comparative example provides a method for evaluating lithium-ion battery materials. In step (3), the delithiated ternary cathode material is only mixed with the electrolyte, and heated and allowed to stand without stirring. Other conditions are exactly the same as those in Example 2.
[0072] The data obtained in step (3) of Comparative Examples 1 and 2 are shown in Table 3.
[0073] Table 3
[0074] As can be seen from Table 3, the high-temperature storage performance of different groups of lithium cobalt oxide positive electrode materials, the amount of cobalt element dissolved, and the charge transfer impedance value of the EIS test are smaller than those in Example 1. Similarly, the high-temperature storage performance of different groups of ternary positive electrode materials, the amount of manganese element dissolved, and the charge transfer impedance value of the EIS test are smaller than those in Example 2. There is no difference and reliability between the various values in the comparative example, and there is little correlation with the storage performance. This shows that stirring during the reaction with the electrolyte in step (2) is crucial to degrade the simulated storage conditions and accelerate the reaction, which is conducive to improving the accuracy of the evaluation method, that is, delithiation is a more important step.
Claims
1. A method for evaluating lithium-ion battery materials, the method comprising the following steps: (1) preparing the positive electrode material to be tested as a delithiation positive electrode material; (2) placing the delithiation positive electrode material described in step (1) in an electrolyte, heating and stirring, and performing solid-liquid separation to obtain a filtrate and a powder; (3) The filtrate obtained in step (2) is subjected to ICP testing to obtain the main element dissolution data; at the same time, the powder in step (2) is used as the positive electrode material to prepare a button half-cell, and an EIS test is performed to obtain the interface charge transfer impedance R CT value; (4) Dissolution data of main elements obtained in step (3) and R CT The larger the value, the worse the high-temperature storage performance of the positive electrode material to be tested.
2. The evaluation method according to claim 1, in, The positive electrode material to be tested in step (1) includes any one of lithium cobalt oxide, lithium iron phosphate or a ternary positive electrode material, or a combination of at least two of them.
3. The evaluation method according to claim 1 or 2, in, The method for preparing the delithiation positive electrode material in step (1) comprises: An oxidant is added to the positive electrode material to be tested to carry out a delithiation reaction to obtain the delithiation positive electrode material.
4. The evaluation method according to claim 3, in, The oxidant includes any one of hypobromous acid, metaperiodic acid, hypochlorous acid, chlorous acid, permanganic acid, perbromic acid or hydrogen peroxide, or a combination of at least two thereof.
5. The evaluation method according to claim 3 or 4, in, The dosage of the oxidant is 4 to 8 mL per gram of the positive electrode material to be tested; the concentration of the oxidant is 1.4 to 8 mol / L.
6. The evaluation method according to any one of claims 1 to 5, in, The delithiation reaction is carried out under stirring.
7. The evaluation method according to any one of claims 1 to 6, in, The time of the delithiation reaction is 18 to 22 hours.
8. The evaluation method according to any one of claims 1 to 7, in, In step (2), the solid-to-liquid ratio of the delithiated positive electrode material to the electrolyte is 1 g:(1.5-2.5) g.
9. The evaluation method according to any one of claims 1 to 8, in, The amount of the electrolyte used in step (2) is 20 to 200 mL.
10. The evaluation method according to any one of claims 1 to 9, in, The heating and stirring in step (3) is carried out in a vacuum or dehumidified environment.
11. The evaluation method according to any one of claims 1 to 10, in, The heating and stirring in step (3) is carried out in a hydrothermal kettle with a polytetrafluoroethylene liner.
12. The evaluation method according to any one of claims 1 to 11, in, The temperature of the heating and stirring in step (3) is 40 to 80°C.
13. The evaluation method according to any one of claims 1 to 12, in, The heating and stirring time in step (3) is 2 to 4 hours.
14. The evaluation method according to any one of claims 1 to 13, in, The stirring rate of the heating and stirring in step (3) is 80 to 200 r / min.
15. The evaluation method according to any one of claims 1 to 14, in, The evaluation method step (4) further includes: The main element dissolution data and standard R CT The value is associated with the high temperature storage performance of the soft-pack battery containing the positive electrode material to be tested, and a database is established to simulate the linear relationship between the main element dissolution data and the high temperature storage performance and / or simulate the R CT The linear relationship between the value and the high temperature storage performance; and inferring the high temperature storage performance of the soft-pack battery containing the positive electrode material to be tested according to the linear relationship; Optionally, the database includes at least 10 different main element dissolution data of the positive electrode materials to be tested, standard R CT Values and data on high temperature storage performance of soft-pack batteries containing the positive electrode material to be tested.
16. The evaluation method according to any one of claims 1 to 15, in, The evaluation method comprises the following steps: (1) adding an oxidant to the positive electrode material to be tested, wherein the amount of the oxidant is 4 to 8 mL per gram of the positive electrode material to be tested, and the concentration of the oxidant is 1.4 to 8 mol / L, and performing a delithiation reaction for 18 to 22 hours under stirring to obtain the delithiation positive electrode material; the positive electrode material to be tested includes any one of lithium cobalt oxide, lithium iron phosphate or a ternary positive electrode material or a combination of at least two; the oxidant includes any one of hypobromous acid, metaperiodic acid, hypochlorous acid, chlorous acid, permanganic acid, perbromic acid or hydrogen peroxide or a combination of at least two; (2) In a dehumidified room, the delithiation positive electrode material and the electrolyte in step (1) are placed in a polytetrafluoroethylene liner in a hydrothermal kettle at a solid-liquid ratio of 1 g:(1.5-2.5) g and mixed evenly, so that the amount of electrolyte is 20-200 mL, and then the hydrothermal kettle is placed in an oven preheated to 40-80° C., the stirring rate is set to 80-200 r / min, and the heating and stirring are carried out for 2-4 hours. After the reaction is completed, the filtrate is filtered to obtain a powder, and the obtained powder is washed and dried for use; (3) The filtrate obtained in step (2) is subjected to ICP testing to obtain the main element dissolution data; at the same time, the powder in step (2) is used as the positive electrode material to prepare a button half-cell, and an EIS test is performed to obtain the interface charge transfer impedance R CT value; (4) Based on the main element dissolution data and R obtained in step (3) CT The high temperature storage performance of the soft-pack battery containing the positive electrode material to be tested is evaluated by the value, and the main element dissolution data and R CT The larger the value, the worse the high temperature storage performance of the cathode material to be tested; and the main element dissolution data and standard R CT The value is associated with the high temperature storage performance of the soft-pack battery containing the positive electrode material to be tested, and a database including at least 10 sample data is established to simulate the linear relationship between the main element dissolution data and the high temperature storage performance and / or simulate the R CT The linear relationship between the value and the high temperature storage performance; The high temperature storage performance of the soft-pack battery containing the positive electrode material to be tested is estimated based on the linear relationship.
17. Application of the evaluation method according to any one of claims 1 to 16 in the field of lithium-ion battery manufacturing.
Citation Information
Patent Citations
Rapid and convenient evaluation method for heat storage stability of lithium ion battery positive electrode material
CN109459463A
Lithium cobalt oxide positive electrode material coated with nanometer lithium cobalt phosphate and preparation method of lithium cobalt oxide positive electrode material
CN112885993A
Lithium ion battery diaphragm, preparation method thereof and lithium ion battery
CN112909430A
Positive electrode active material, and electrochemical device and electronic device using same
CN113078309A
Phosphorus-containing substance coated positive electrode material and preparation method and application thereof
CN115117316A