Electrolyte solution and lithium-ion battery

By using additives and organic solvents with specific structures in lithium-ion batteries, a stable membrane structure is formed, which solves the problem of poor storage performance of electrolyte at high temperatures, significantly improves the capacity retention and capacity recovery rate of lithium-ion batteries, and improves the capacity retention rate of lithium-ion batteries. The battery cycle life and safety are provided.

WO2024230065A1PCT designated stage expired Publication Date: 2024-11-14HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
PCT/CN2023/123836
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2023-10-10
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The existing lithium-ion battery electrolyte has poor storage performance in high-temperature environments, resulting in poor capacity retention and capacity recovery rates, affecting the performance and safety of the battery.

Method used

Adopt additives with specific structures, including compounds with C-F bonds and sulfonate groups, and electrolytes combined with components such as vinyl carbonate, vinyl sulfate, etc., form stable SEI and CEI films to inhibit the oxidative decomposition of the electrolyte and the positive electrode metal. The dissolution of ions reduces the oxidation potential and improves the high-temperature storage performance of the battery.

Benefits of technology

It significantly improves the capacity retention and capacity recovery rate of lithium-ion batteries, extends the battery cycle life, and maintains the stability and safety of the battery in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023123836_14112024_PF_FP_ABST
    Figure CN2023123836_14112024_PF_FP_ABST
Patent Text Reader

Abstract

An electrolyte solution and a lithium-ion battery. The electrolyte solution comprises a first additive, a lithium salt and an organic solvent, wherein the first additive comprises a compound with a structure as shown in formula I and / or a compound with a structure as shown in formula II, where R is selected from C1-C12 alkyl or C1-C12 alkoxy. On this basis, the electrolyte solution has good high-temperature storage performance, and the lithium-ion battery has a relatively high capacity retention rate and a relatively high capacity recovery rate.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte and lithium-ion battery

[0001] This application claims priority to Chinese patent application No. 202310525563.1, filed May 10, 2023. This application incorporates the entire text of the aforementioned Chinese patent application. Technical Field

[0002] The present application relates to the field of lithium-ion batteries, and more specifically, to an electrolyte and a lithium-ion battery. Background Art

[0003] Lithium-ion batteries have recently become a new research hotspot and garnered widespread attention. The electric vehicle sector is focusing on hybrid vehicles and mobile device power supplies, among other applications. This is due to their high energy density, environmental friendliness, and economic benefits. It is well known that high temperatures are a significant factor affecting the performance, lifespan, and safety of lithium-ion batteries. Specifically, high temperatures accelerate the aging of lithium-ion batteries. Furthermore, the lithium salts and organic solvents in lithium-ion battery electrolytes have poor thermal stability. Under high temperature conditions, the electrolyte decomposes and produces large amounts of gas, which can easily cause battery expansion, thereby reducing performance and safety.

[0004] In summary, existing lithium-ion battery electrolytes have poor high-temperature storage performance, resulting in poor battery capacity retention and capacity recovery. Therefore, it is urgent to develop an electrolyte with good high-temperature performance to improve the above problems.

[0005] Summary of the Invention

[0006] The main purpose of this application is to provide an electrolyte and a lithium-ion battery to solve the problems of poor capacity retention and capacity recovery rate of lithium-ion batteries caused by poor high-temperature storage performance of the electrolyte in the prior art.

[0007] To achieve the above objectives, according to one aspect of the present application, an electrolyte is provided, the electrolyte comprising a first additive, a lithium salt, and an organic solvent; wherein the first additive comprises a compound having a structure represented by Formula I and / or a compound having a structure represented by Formula II:

[0008] R is selected from C1-C12 alkyl or C1-C12 alkoxy.

[0009] Furthermore, R is selected from C1-C4 alkyl or C1-C4 alkoxy.

[0010] Furthermore, the compound of the structure shown in formula I is

[0011] Furthermore, the electrolyte further includes a second additive, which is selected from one or more of vinylene carbonate, vinyl sulfate, tris(trimethylsilyl)phosphite, methylene methanedisulfonate, fluoroethylene carbonate or tris(trimethylsilyl)borate.

[0012] Furthermore, in the electrolyte, the total weight of the first additive and the second additive is 0.1 to 5 wt %; and the weight ratio of the first additive to the second additive is 0.1 to 2:1.

[0013] Furthermore, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium dioxalatoborate, lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium bis(fluorosulfonyl)imide salt or lithium bis(trifluoromethylsulfonyl)imide; and the concentration of the lithium salt is 0.5 to 1.5M.

[0014] Furthermore, the organic solvent is one or more of a chain carbonate compound, a cyclic carbonate compound or a carboxylate compound; the cyclic carbonate compound is selected from one or more of ethylene carbonate and / or propylene carbonate; the chain carbonate compound is selected from one or more of dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate; and the carboxylate compound is selected from propyl acetate and / or ethyl acetate.

[0015] Furthermore, the electrolyte includes a first additive, a second additive, a lithium salt and an organic solvent; wherein the first additive is The second additive is vinylene carbonate, tris(trimethylsilyl)phosphite and methylene disulfonate, the lithium salt is lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide salt, and the organic solvent is ethylene carbonate, diethyl carbonate and ethyl methyl carbonate; and the weight ratio of the first additive to the second additive is 1 to 2:1; in the first additive, The weight ratio of vinylene carbonate, tris(trimethylsilyl)phosphite and methylene disulfonate in the second additive is 1:4.5-5.5; the weight ratio of vinylene carbonate, tris(trimethylsilyl)phosphite and methylene disulfonate is 0.75-0.85:0.5:0.75-0.85; the molar ratio of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide salt in the lithium salt is 0.65-0.75:0.3; the weight ratio of ethylene carbonate, diethyl carbonate and ethyl methyl carbonate in the organic solvent is 0.5-1.5:1:0.5-1.5; or the first additive is The second additive is vinyl sulfate, tris(trimethylsilyl) borate and fluoroethylene carbonate, the lithium salt is lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide salt, and the organic solvent is vinyl carbonate, dimethyl carbonate and ethyl acetate; and the weight ratio of the first additive to the second additive is 1 to 2:1; in the first additive, The weight ratio of the second additive is 1:1.5~2.5; in the second additive, the weight ratio of vinyl sulfate, tris(trimethylsilyl)borate and fluoroethylene carbonate is 0.75~0.85:0.5:0.75~0.85; in the lithium salt, the molar ratio of lithium hexafluorophosphate and lithium bisfluorosulfonyl imide salt is 0.65~0.75:0.3; in the organic solvent, the weight ratio of ethylene carbonate, dimethyl carbonate and ethyl acetate is 0.5~1.5:1:0.5~1.5.

[0016] In order to achieve the above object, according to one aspect of the present application, a lithium ion battery is provided, which includes a negative electrode sheet, a positive electrode sheet and an electrolyte, wherein the material of the positive electrode sheet is LiNi (1-x-y) Co x Mn y , wherein 0≤x≤1, 0≤y≤1, and x+y≤1; the material of the negative electrode sheet is graphite, and the electrolyte is the aforementioned electrolyte.

[0017] Furthermore, the material of the positive electrode is LiNi (1-x-y) Co x Mn y , wherein 0<x<1, 0<y<1, and x+y<1; preferably, the material of the positive electrode is LiNi 0.7 C0 0.1 Mn 0.2 .

[0018] The CF bond is easy to break, and LiF (the main component of the SEI film) is easily generated, with good thermal stability. The sulfonate group can coordinate with transition metal ions (such as nickel ions, cobalt ions, and manganese ions) to form a complex, which passivates the positive electrode surface, inhibits the dissolution of positive electrode metal ions, and reduces the decomposition effect of high-oxidation state active substances on the solvent. The silyl group substituted on the benzene ring serves as an electron-donating group, with a large electron cloud density, which reduces the oxidation potential and easily forms a CEI interface film on the electrode surface, thereby avoiding direct contact between the electrode and the electrolyte at high temperature. At the same time, it can also delay the oxidative decomposition reaction of the electrolyte, thereby effectively improving the high-temperature storage performance of the electrolyte, thereby significantly improving the battery capacity retention rate and capacity recovery rate. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments in this application can be combined with each other. The present application will be described in detail below with reference to the embodiments.

[0020] As described in the background section of this application, prior art electrolytes have poor high-temperature storage performance, resulting in poor capacity retention and capacity recovery in lithium-ion batteries. To address this issue, this application provides an electrolyte comprising a first additive, a lithium salt, and an organic solvent; wherein the first additive comprises a compound of formula I and / or a compound of formula II:

[0021] R is selected from C1-C12 alkyl or C1-C12 alkoxy.

[0022] Compared with other parent nuclei and substituent groups, the electrolyte high temperature storage performance composed of the above-mentioned specific structural additives in this application is better, and the capacity retention rate and capacity recovery rate of lithium-ion batteries are both very excellent. Specifically, first, the CF bond is easily broken, and LiF (the main component of SEI film) is easily generated, with good thermal stability. Second, the sulfonate group can coordinate with transition metal ions (Ni ions, Co ions, Mn ions) to form a complex, which passivates the positive electrode surface, inhibits the dissolution of positive electrode metal ions, and reduces the decomposition effect of high oxidation state active substances on the solvent. Third, the silyl group substituted on the benzene ring serves as an electron-donating group, with a large electron cloud density, which reduces the oxidation potential and is easy to form a CEI interface film on the electrode surface, thereby avoiding direct contact between the electrode and the electrolyte at high temperature, and also delaying the oxidative decomposition reaction of the electrolyte, thereby effectively improving the high temperature storage performance of the electrolyte, thereby greatly improving the battery capacity retention rate and capacity recovery rate.

[0023] In order to further improve the battery capacity retention rate and capacity recovery rate, preferably R is selected from C1-C4 alkyl, C1-C4 alkoxy. More preferably, the compound of formula I is

[0024] Further preferably, the electrolyte further comprises a second additive, the second additive being selected from one or more of vinylene carbonate, vinyl sulfate, tris(trimethylsilyl)phosphite, methylene disulfonate, fluoroethylene carbonate or tris(trimethylsilyl)borate. The synergistic use of vinylene carbonate and the first additive of the above-mentioned specific structure can provide overcharge protection for the battery. The synergistic use of vinyl sulfate and the first additive of the above-mentioned specific structure can effectively reduce the impedance of the negative electrode, significantly improving the low-temperature performance and cycle performance, and even high-temperature performance, of the battery. The synergistic use of tris(trimethylsilyl)phosphite and the first additive of the above-mentioned specific structure can preferentially form a stable CEI film on the surface of the positive electrode material at high voltage, effectively inhibiting the oxidative decomposition of the electrolyte, thereby improving the cycle performance of the battery. Methylene disulfonate has excellent high-temperature cycle performance, and the synergistic use of the first additive of the above-mentioned specific structure can prevent metal ions (such as manganese ions) dissolved at high temperature from being adsorbed on the negative electrode surface, inhibiting the impedance rise, effectively improving the cycle period characteristics, and thus greatly increasing the cycle life of the battery. The synergistic use of fluoroethylene carbonate and the first additive of the above-mentioned specific structure forms a SEI film with better performance, forming a tight structural layer without increasing impedance, which can prevent further decomposition of the electrolyte and improve the low-temperature performance of the electrolyte.

[0025] In order to further improve the capacity retention and recovery rate of the battery, it is preferred that the weight ratio of the first additive to the second additive in the electrolyte is 0.1 to 2:1, for example, it can be 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 1:1, 1.2:1, 1.5:1, 1.8:1 or 2:1.

[0026] In a preferred embodiment, the total weight of the first additive and the second additive in the electrolyte is 0.1 to 5 wt%. Based on this, the battery not only has excellent electrochemical performance, but also has excellent capacity retention and capacity recovery rates. If the amount of additives is too high, the positive and negative electrode films will become thicker and the impedance will increase; if the amount of additives is too low, the film formation efficiency will be poor. Further preferably, the content of the additives in the electrolyte is 0.5 to 3 wt%, for example, it can be 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt% or 3 wt%.

[0027] In consideration of selecting a lithium salt that is more compatible with the above-mentioned additives, in a preferred embodiment, in the electrolyte, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium dioxalatoborate, lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium bis(fluorosulfonyl)imide salt, or lithium bis(trifluoromethylsulfonyl)imide. The concentration of the lithium salt is 0.5 to 1.5 M, for example, 0.5 M, 0.75 M, 1 M, 1.25 M, or 1.5 M. The concentration of the lithium salt is limited to the above range, so that the battery can simultaneously take into account better electrochemical performance, capacity retention rate, and capacity recovery rate.

[0028] In a preferred embodiment, the organic solvent is one or more of a linear carbonate compound, a cyclic carbonate compound, or a carboxylate compound. The cyclic carbonate compound is selected from ethylene carbonate and / or propylene carbonate; the linear carbonate compound is selected from one or more of dimethyl carbonate, diethyl carbonate, or ethyl methyl carbonate; and the carboxylate compound is selected from propyl acetate and / or ethyl acetate. These additives are highly compatible with this type of organic solvent, enabling the battery to simultaneously achieve superior electrochemical performance, capacity retention, and capacity recovery.

[0029] In order to further balance the performance of the product, in a preferred embodiment, the electrolyte includes a first additive, a second additive, a lithium salt and an organic solvent; wherein the first additive is The second additive is vinylene carbonate, tris(trimethylsilyl)phosphite and methylene disulfonate, the lithium salt is lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide salt, and the organic solvent is ethylene carbonate, diethyl carbonate and ethyl methyl carbonate; and the weight ratio of the first additive to the second additive is (1-2):1; in the first additive, The weight ratio of vinylene carbonate, tris(trimethylsilyl)phosphite and methylene disulfonate in the second additive is 1:4.5-5.5; the weight ratio of vinylene carbonate, tris(trimethylsilyl)phosphite and methylene disulfonate is 0.75-0.85:0.5:0.75-0.85; the molar ratio of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide salt in the lithium salt is 0.65-0.75:0.3; the weight ratio of ethylene carbonate, diethyl carbonate and ethyl methyl carbonate in the organic solvent is 0.5-1.5:1:0.5-1.5. Alternatively, the first additive is The second additive is vinyl sulfate, tris(trimethylsilyl) borate and fluoroethylene carbonate, the lithium salt is lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide salt, and the organic solvent is vinyl carbonate, dimethyl carbonate and ethyl acetate; and the weight ratio of the first additive to the second additive is 1 to 2:1; in the first additive, The weight ratio of the second additive is 1:1.5~2.5; in the second additive, the weight ratio of vinyl sulfate, tris(trimethylsilyl)borate and fluoroethylene carbonate is 0.75~0.85:0.5:0.75~0.85; in the lithium salt, the molar ratio of lithium hexafluorophosphate and lithium bisfluorosulfonyl imide salt is 0.65~0.75:0.3; in the organic solvent, the weight ratio of ethylene carbonate, dimethyl carbonate and ethyl acetate is 0.5~1.5:1:0.5~1.5.

[0030] In a preferred embodiment, the electrolyte can be prepared by the following preparation method: first adding a lithium salt to an organic solvent, and after the lithium salt is completely dissolved, adding an additive to the system to obtain the electrolyte. Based on this, the electrolyte obtained in this application has better performance uniformity.

[0031] The present application also provides a lithium-ion battery, which includes a negative electrode, a positive electrode and an electrolyte. The positive electrode is made of LiNi (1-x-y) Co x Mn y , where 0≤x≤1, 0≤y≤1, and x+y≤1; the negative electrode is made of graphite, and the electrolyte is the aforementioned electrolyte. Based on the foregoing reasons, the lithium-ion battery of the present application has excellent capacity retention and capacity recovery rates.

[0032] In a preferred embodiment, the material of the positive electrode is LiNi (1-x-y) Co x Mn y , wherein 0<x<1, 0<y<1, and x+y<1; further preferably, the material of the positive electrode is LiNi 0.7 C0 0.1 Mn 0.2 The charging voltage of the lithium-ion battery is not higher than 4.8V, preferably 2.8 to 4.35V.

[0033] The present application is further described in detail below with reference to specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in this application.

[0034] Example

[0035] Example 1

[0036] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of EC:DEC:EMC = 1:1:1 to obtain a mixed organic solvent system. 1M lithium hexafluorophosphate (LiPF6) was added to the system. After the lithium salt was completely dissolved, 0.5wt% of the additive was added to the system. (CAS No. 556812-41-0), 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0037] Example 2

[0038] Ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of EC:PC:DEC:EMC=1:1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salts were completely dissolved, 3wt% of the additive was added to the system. 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0039] Example 3

[0040] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed at a weight ratio of EC:DEC:EMC=1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salts were completely dissolved, 0.5wt% of LiFSI was added to the system. (CAS No.: 262373-15-9), 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0041] Example 4

[0042] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of EC:DEC:EMC=1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salts were completely dissolved, 3wt% of the additive was added. 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0043] Example 5

[0044] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of EC:DEC:EMC=1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salts were completely dissolved, 0.5wt% of the additive was added. (CAS No. 780820-43-1), 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0045] Example 6

[0046] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of EC:DEC:EMC=1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salts were completely dissolved, 3wt% of the additive was added. (CAS No. 780820-43-1), 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0047] Example 7

[0048] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of EC:DEC:EMC=1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salts were completely dissolved, 0.5wt% of 2.5wt% 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0049] Example 8

[0050] Ethylene carbonate, dimethyl carbonate and ethyl acetate were mixed in a weight ratio of ethylene carbonate: dimethyl carbonate: ethyl acetate = 1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salt was completely dissolved, 1wt% of 2wt% 0.8 wt% of vinyl sulfate, 0.5 wt% of tris(trimethylsilyl)borate and 0.8 wt% of fluoroethylene carbonate.

[0051] Example 9

[0052] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of EC:DEC:EMC=1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salts were completely dissolved, 0.5wt% of 0.5wt% 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0053] Example 10

[0054] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a weight ratio of EC:DEC:EMC=1:1:1 to obtain a mixed organic solvent system. 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added to the system. After the lithium salts were completely dissolved, 0.5wt% of 0.5wt% 0.5wt% 0.8 wt% of vinylene carbonate (VC), 0.5 wt% of tris(trimethylsilyl)phosphite (TMSP) and 0.8 wt% of methylene methanedisulfonate (MMDS).

[0055] Example 11

[0056] The only difference from Example 1 is: additive The dosage is 8wt%.

[0057] Comparative Example:

[0058] Comparative Example 1

[0059] The only difference from Example 1 is that the first additive is not added.

[0060] Comparative Example 2

[0061] The only difference from Example 1 is that the additives in Example 1 An equal weight amount was replaced with 1,3-propanesultone (PS).

[0062] Comparative Example 3

[0063] The only difference from Example 7 is that Replace with PS of equal weight, An equal weight amount was replaced with tris(trimethylsilyl)borate (TMSB).

[0064] Comparative Example 4

[0065] The only difference from Example 1 is that the additive Replace with equal weight (CAS:2047348-50-3).

[0066] Comparative Example 5

[0067] The only difference from Example 1 is that the additive Replace with equal weight

[0068] Battery preparation:

[0069] 1. Preparation of positive electrode: LiNi0 0.7 C0 0.1 Mn 0.2 The conductive agent Super P, the adhesive PVDF and the carbon nanotube (CNT) are mixed evenly in a weight ratio of 97.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for the current collector. The coating amount is 360g / m 2 , dried at 85°C and then cold pressed; then striped and sliced, and then baked at 85°C in vacuum for 4 hours to make lithium-ion battery positive electrodes.

[0070] 2. Preparation of negative electrode sheet: artificial graphite, conductive agent Super P, thickener CMC, and adhesive SBR (styrene-butadiene rubber emulsion) are mixed in a weight ratio of 95:1.5:1.0:2.5 to form a slurry, mix them evenly, and apply the mixed slurry on both sides of the copper foil. After drying and roller pressing, the negative electrode sheet is obtained, and then it is dried at 85°C in a vacuum for 4 hours to prepare the negative electrode sheet of the lithium-ion battery.

[0071] 3. Preparation of a Lithium-Ion Battery: The aforementioned positive electrode sheet, negative electrode sheet, and separator were laminated to form a lithium-ion battery with a thickness of 0.5 mm, a width of 8 mm, and a length of 10 mm, and a capacity of 3 Ah. The battery was then vacuum-baked at 85°C for 48 hours, and the electrolytes described in the Examples and Comparative Examples were injected to complete the battery production.

[0072] The capacity retention rate and capacity recovery rate of the above battery were tested, and the test results are shown in Table 1:

[0073] Table 1

[0074] The above are merely preferred embodiments of the present application and are not intended to limit the present application. Those skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present application shall be included within the scope of protection of the present application.

Claims

1. An electrolyte, characterized in that: The electrolyte includes a first additive, a lithium salt and an organic solvent; wherein the first additive includes a compound of the structure shown in Formula I and / or a compound of the structure shown in Formula II: R is selected from C1-C12 alkyl or C1-C12 alkoxy.

2. The electrolyte according to claim 1, characterized in that The R is selected from C1-C4 alkyl or C1-C4 alkoxy.

3. The electrolyte according to claim 2, characterized in that The compound of the structure shown in Formula I is 4. The electrolyte according to claim 1 or 3, characterized in that The electrolyte further includes a second additive, which is selected from one or more of vinylene carbonate, vinyl sulfate, tris(trimethylsilyl)phosphite, methylene methanedisulfonate, fluoroethylene carbonate or tris(trimethylsilyl)borate.

5. The electrolyte according to claim 4, characterized in that In the electrolyte, the total weight of the first additive and the second additive is 0.1 to 5 wt %; The weight ratio of the first additive to the second additive is 0.1 to 2:

1.

6. The electrolyte according to claim 5, characterized in that In the electrolyte, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium dioxalate borate, lithium difluorooxalate borate, lithium difluorooxalate phosphate, lithium bis(fluorosulfonyl)imide salt or lithium bis(trifluoromethylsulfonyl)imide; The molar concentration of the lithium salt is 0.5-1.5M.

7. The electrolyte according to claim 6, characterized in that The organic solvent is one or more of a chain carbonate compound, a cyclic carbonate compound or a carboxylate compound; The cyclic carbonate compound is selected from one or more of ethylene carbonate and / or propylene carbonate; The chain carbonate compound is selected from one or more of dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate; The carboxylate compound is selected from propyl acetate and / or ethyl acetate.

8. The electrolyte according to claim 7, characterized in that The electrolyte includes the first additive, the second additive, the lithium salt and the organic solvent; Wherein, the first additive is The second additive is vinylene carbonate, tris(trimethylsilyl)phosphite and methylene disulfonate, the lithium salt is lithium hexafluorophosphate and bis(fluorosulfonyl)imide lithium salt, the organic solvent is vinyl carbonate, diethyl carbonate and ethyl methyl carbonate; and the weight ratio of the first additive to the second additive is 1 to 2:1; in the first additive, The weight ratio of the second additive is 1:4.5-5.5; the weight ratio of vinylene carbonate, tris(trimethylsilyl)phosphite and methylene disulfonate is 0.75-0.85:0.5:0.75-0.85; In the lithium salt, the molar ratio of lithium hexafluorophosphate to lithium bis(fluorosulfonyl)imide salt is 0.65-0.75:0.3; in the organic solvent, the weight ratio of ethylene carbonate, diethyl carbonate and ethyl methyl carbonate is 0.5-1.5:1:0.5-1.5; Alternatively, the first additive is The second additive is vinyl sulfate, tris(trimethylsilyl)borate and fluoroethylene carbonate, the lithium salt is lithium hexafluorophosphate and bis(fluorosulfonyl)imide lithium salt, the organic solvent is vinyl carbonate, dimethyl carbonate and ethyl acetate; and the weight ratio of the first additive to the second additive is 1 to 2:1; in the first additive, The weight ratio of vinyl sulfate, tris(trimethylsilyl)borate and fluoroethylene carbonate in the second additive is 0.75-0.85:0.5:0.75-0.85; the molar ratio of lithium hexafluorophosphate and bis(fluorosulfonyl)imide lithium salt in the lithium salt is 0.65-0.75:0.3; the weight ratio of vinyl carbonate, dimethyl carbonate and ethyl acetate in the organic solvent is 0.5-1.5:1:0.5-1.

5.

9. A lithium ion battery comprising a negative electrode sheet, a positive electrode sheet and an electrolyte, characterized in that: The material of the positive electrode is LiNi (1-x-y) Co x Mn y , wherein 0≤x≤1, 0≤y≤1, and x+y≤1; the material of the negative electrode sheet is graphite, and the electrolyte is the electrolyte according to any one of claims 1 to 8.

10. The lithium ion battery according to claim 9, characterized in that: The material of the positive electrode is LiNi 0.7 C0 0.1 Mn 0.2 .

Citation Information

Patent Citations

  • Additive for non-aqueous electrolyte, non-aqueous electrolyte, and power storage device

    CN106133984A

  • Electrolyte and lithium ion battery

    CN115458810A

  • Electrolyte and lithium ion battery

    CN116247301A

  • Lithium ion secondary battery

    JP2015125949A

  • Electrolyte additive, electrolyte containing same, and lithium-ion battery

    WO2023040119A1

Cited By

  • High-voltage-resistant lithium battery electrolyte and preparation method thereof

    CN119297410A

  • Electrolyte and lithium ion battery

    CN119518095A

  • Battery cell, electrolyte, battery device, and electric device

    CN120127224A

  • Electrolyte additive for improving high-temperature performance of lithium battery and electrolyte

    CN121064236A

  • Electrolyte, battery and electrical device

    WO2026194590A1