Compound for electrolyte, compound for electrolyte additive, electrolyte material, electrolyte additive, electrolyte for secondary battery, and secondary battery
The novel electrolyte solution with a compound represented by Formula 1 addresses the stability and lifespan challenges of lithium secondary batteries by forming a stable SEI film, enhancing room temperature performance and maintaining high temperature stability.
Patent Information
- Application Number
- PCT/KR2024/006491
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-10
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-14
AI Technical Summary
Lithium secondary batteries face challenges with high operating voltages, requiring electrolytes that are non-reactive and provide improved lifespan and high temperature stability, which existing organic electrolytes do not adequately address.
A novel electrolyte solution containing a compound represented by Formula 1, or its isomer, which forms a stable SEI film on the anode, minimizing resistance increase and enhancing lithium ion mobility, thereby improving room temperature lifespan performance.
The electrolyte solution with the novel compound significantly enhances the room temperature lifespan of lithium secondary batteries by forming a stable SEI film, reducing resistance and preventing cathode deterioration, while maintaining high temperature stability.
Smart Images

Figure KR2024006491_14112024_PF_FP_ABST
Abstract
Description
Compounds for electrolytes, compounds for electrolyte additives, electrolyte materials, electrolyte additives, electrolytes for secondary batteries and secondary batteries
[0001] The present invention relates to a compound for an electrolyte, a compound for an electrolyte additive, an electrolyte material, an electrolyte additive, an electrolyte for a secondary battery, and a secondary battery.
[0002] Lithium secondary batteries are used as power sources for portable electronic devices such as video cameras, cell phones, and laptop computers. Compared to conventional lead-acid, nickel-cadmium, nickel-metal hydride, and nickel-zinc batteries, rechargeable lithium secondary batteries offer more than three times the energy density per unit weight and are capable of rapid charging.
[0003] Lithium secondary batteries operate at high operating voltages, so aqueous electrolytes, which are highly reactive with lithium, cannot be used. Organic electrolytes are typically used as electrolytes for lithium secondary batteries. Organic electrolytes are prepared by dissolving lithium salts in organic solvents. Organic solvents are preferably stable at high voltages, have high ionic conductivity and dielectric constant, and have low viscosity.
[0004] Meanwhile, the voltage, lifespan, capacity, and stability of a battery can vary significantly depending on the materials used for the cathode, anode, and electrolyte. Therefore, there is a need for an electrolyte for lithium secondary batteries that can provide lithium secondary batteries with improved lifespan characteristics and high-temperature stability.
[0005] One object of the present invention is to provide an electrolyte for a secondary battery comprising a novel compound or an isomer thereof.
[0006] Another object of the present invention is to provide a secondary battery including the electrolyte for the secondary battery.
[0007] To achieve the above purpose, one embodiment of the present invention provides an electrolyte for a secondary battery comprising a compound of the following chemical formula 1, or an isomer thereof.
[0008] An electrolyte for a secondary battery, comprising a compound represented by the following chemical formula 1, or an isomer thereof:
[0009] [Chemical Formula 1]
[0010]
[0011] In the above chemical formula 1, carbons in the ring are connected by single or double bonds;
[0012] wherein X is oxygen or sulfur;
[0013] wherein Y is oxygen or sulfur;
[0014] The above Z 1 , Z 2 , and Z 3 are each independently hydrogen, substituted or unsubstituted C 1-10 Alkyl, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Amine, substituted or unsubstituted C 1-10 Acyl, substituted or unsubstituted C 1-10 alkynyl, substituted or unsubstituted C 3-10 Cycloalkyl, substituted or unsubstituted silyl, substituted or unsubstituted C 1-10 Alkoxy, substituted or unsubstituted C 1-12 Heteroalkyl, substituted or unsubstituted C 1-6 Heterocycloalkyl, -SO2R 1 , -P(=G)(OR 1 )2 and -P(=G)(R 1 ) is selected from the group consisting of 2;
[0015] The above Z 1 and Z 2 may or may not combine with each other to form a ring;
[0016] wherein G is oxygen or sulfur;
[0017] The above R 1 Silver substituted or unsubstituted C 1-6 Alkyl, C 2-6 Alkenyl, C 2-6 alkynyl or C6-20 It could be Aryl.
[0018] In one embodiment of the present invention, the substituted alkyl, alkenyl, amine, acyl, alkynyl, cycloalkyl, silyl, alkoxy, heteroalkyl, and heterocycloalkyl may each be independently substituted with one or more substituents selected from the group consisting of an alkoxy group, an alkynyloxy group, a heteroaryl group, an alkenyl group, a heterocycloalkyl group, a carbonyl group, a halogen group, a hydroxy group, an alkenyloxy group, a carboxyl group, a carbonate group, an alkyl group, an alkynyl group, an amine group, a cycloalkyl group, a silyl group, a sulfonate group, a phosphate group, a thiophosphate group, a nitro group, a cyano group, a heteroalkyl group, a cycloalkyl group, an aryl group, and an ether group.
[0019] In one embodiment of the present invention, the electrolyte may further include one or more additives selected from the group consisting of LiPO2F2, unsaturated cyclic carbonates, cyclic sultones, cyclic sulfate lactones, nitrile compounds, and mixtures thereof.
[0020] In one embodiment of the present invention, the unsaturated cyclic carbonate may be selected from the group consisting of vinylene carbonate, phenyl carbonate, vinyl carbonate, and allyl carbonate.
[0021] In one embodiment of the present invention, the electrolyte may further include an organic solvent.
[0022] In another aspect of the present invention, a lithium ion battery comprising the non-aqueous electrolyte for a secondary battery is provided.
[0023] In one embodiment of the present invention, a secondary battery may be provided, the battery including an electrode assembly including a positive electrode, a negative electrode, and a separator separating the positive electrode and the negative electrode; a case accommodating the electrode assembly; and an electrolyte solution accommodated in the case and immersing the electrode assembly.
[0024] A secondary battery including an electrolyte additive and an electrolyte for a secondary battery according to the present invention can have improved room temperature life performance.
[0025] FIG. 1 is a cross-sectional view of a secondary battery including an electrolyte and an electrolyte additive according to one embodiment of the present invention.
[0026] Figures 2 to 5 show the results of analyzing the room temperature life performance of a secondary battery according to one embodiment of the present invention.
[0027] <Explanation of symbols>
[0028] 1: Secondary battery
[0029] 10: Upper case
[0030] 20: Spring
[0031] 30: Spacer
[0032] 40: Bipolar
[0033] 50: Membrane
[0034] 60: Cathode
[0035] One embodiment of the present invention is illustrated in the accompanying drawings. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. Like reference numerals in the drawings indicate like elements.
[0036] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms including "at least one," unless the content clearly dictates otherwise. "At least one" should not be construed as limiting to the singular. As used herein, the term "and / or" includes any and all combinations of one or more of the listed items. The terms "comprises" and / or "comprising" as used in the detailed description specify the presence of stated features, regions, integers, steps, operations, components, and / or ingredients, but do not preclude the presence or addition of one or more other features, regions, integers, steps, operations, components, ingredients, and / or groups thereof.
[0037] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. Furthermore, it will be understood that terms defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning within the context of the relevant art and the present disclosure, and not in an idealized or overly formal sense.
[0038] While specific embodiments have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently anticipated or unforeseen may occur to the applicant or those skilled in the art. Accordingly, the appended claims, as filed and as amended, are intended to encompass all such alternatives, modifications, variations, improvements, and substantial equivalents.
[0039] The term "isomer" as used herein refers to a compound of the present invention or a salt thereof that has the same chemical formula or molecular formula but is structurally or sterically different. Such isomers include structural isomers such as tautomers, stereoisomers such as R or S isomers having an asymmetric carbon center, geometric isomers (trans, cis), and optical isomers (enantiomers). All of these isomers and mixtures thereof are also included within the scope of the present invention.
[0040] In the present invention, the term "alkyl" may be straight-chain or branched, unless otherwise specified, and may have 1 to 7 carbon atoms, but is not particularly limited thereto. Specific examples of alkyl groups include, but are not limited to, methyl, ethyl, propyl, n-propyl, isopropyl, butyl, n-butyl, isobutyl, tert-butyl, sec-butyl, 1-methyl-butyl, 1-ethyl-butyl, pentyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, hexyl, n-hexyl, 1-methylpentyl, 2-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl, heptyl, n-heptyl, and the like.
[0041] As used herein, the term "alkenyl" refers to an alkyl group that may be straight or branched, unless otherwise specified, and that contains one or more double bonds. The number of carbon atoms is not particularly limited, but may be from 2 to 6. Specific examples include, but are not limited to, vinyl, 1-propenyl, isopropenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 3-methyl-1-butenyl, and 1,3-butadienyl.
[0042] As used herein, the term "alkynyl" may mean an alkyl group that may be straight or branched, unless otherwise specified, and that contains one or more triple bonds. The number of carbon atoms is not particularly limited, but may be 2 to 6. Specific examples include, but are not limited to, an ethynyl group, a propynyl group, a butynyl group, and a pentaynyl group.
[0043] The term "amine" as used herein may be selected from the group consisting of -NH2, an alkylamine group, an N-alkylarylamine group, an arylamine group, an N-arylheteroarylamine group, an N-alkylheteroarylamine group, and a heteroarylamine group, and the number of carbon atoms is not particularly limited, but may be 1 to 30. More specific examples of the amine group include a methylamine group, a dimethylamine group, an ethylamine group, a diethylamine group, a phenylamine group, a naphthylamine group, a biphenylamine group, anthracenylamine group, a 9-methyl-anthracenylamine group, a diphenylamine group, a ditolylamine group, an N-phenyltolylamine group, a triphenylamine group, an N-phenylbiphenylamine group, an N-phenylnaphthylamine group, an N-biphenylnaphthylamine group; Examples thereof include, but are not limited to, N-naphthylfluorenylamine group, N-phenylphenanthrenylamine group, N-biphenylphenanthrenylamine group, N-phenylfluorenylamine group, N-phenylterphenylamine group, N-phenanthrenylfluorenylamine group, N-biphenylfluorenylamine group, etc.
[0044] The term "heteroalkyl" as used herein refers to an alkyl containing one or more of O, N, Si, B, Se, P, and S as heteroatoms, and the number of carbon atoms is not particularly limited, but may be 1 to 6. Examples of heteroalkyl include, but are not limited to, -CH2-CH2-O-CH3, -CH2-CH2-NH-CH3, -CH2-CH2-N(CH3)-CH3, -CH2-S-CH2-CH3, etc.
[0045] The term "cycloalkyl" as used herein refers to a non-aromatic carbon ring having, but is not particularly limited to, 3 to 12 carbon atoms. Examples of cycloalkyl include, but are not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, and cyclodecyl.
[0046] The term "heterocycloalkyl" as used herein refers to a cycloalkyl containing at least one of O, N, Si, B, Se, P, and S as a heteroatom, and the number of carbon atoms is not particularly limited, but may be 3 to 12. Examples of heterocycloalkyl include, but are not limited to, epoxy, tetrahydrofuranyl, tetrahydropyranyl, tetrahydrothiophenyl, and tetrahydropyrrolyl.
[0047] The term "aryl" as used herein is not particularly limited, but may have 6 to 20 carbon atoms; or 6 to 12 carbon atoms. Monocyclic aryl groups include, but are not limited to, a phenyl group, a biphenyl group, a terphenyl group, and the like. Polycyclic aryl groups include, but are not limited to, a naphthyl group, anthracenyl group, a phenanthrenyl group, a pyrenyl group, a perylenyl group, a chrysenyl group, a fluorenyl group, and the like.
[0048] The term "heteroaryl" as used herein refers to an aryl containing at least one of O, N, Si, B, Se, P, and S as a heteroatom, and the number of carbon atoms is not particularly limited, but may be 5 to 20. Examples of heteroaryl include xanthene, thioxanthen, thiophene, furan, pyrrole, imidazole, thiazole, oxazole, oxadiazole, triazole, pyridyl, bipyridyl, pyrimidyl, triazine, acridyl, pyridazine, pyrazinyl, quinolinyl, quinazoline, quinoxalinyl, phthalazinyl, pyridopyrimidinyl, pyridopyrazinyl, pyrazinopyrazinyl, isoquinoline, indole, carbazole, benzoxazole, benzimidazole, benzothiazole, benzocarbazole, benzothiophene, dibenzothiophene, benzofuranyl, phenanthroline, Examples thereof include, but are not limited to, isoxazolyl group, thiadiazolyl group, phenothiazinyl group, and dibenzofuranyl group.
[0049] The term "alkoxy" as used herein refers to an alkyl group bonded to oxygen, wherein oxygen may be bonded to the aforementioned alkyl. Examples of alkoxy include, but are not limited to, a methoxy group, an ethoxy group, a propoxy group, a butoxy group, and a pentoxy group.
[0050] The term "acyl" as used herein refers to the remainder after removing OH from the carboxylic acid group -COOH, and the number of carbon atoms is not particularly limited, but may be 1 to 6. Examples of acyl include, but are not limited to, an acetyl group, a propionyl group, a malonyl group, a benzoyl group, etc.
[0051] The term "silyl" as used herein may be represented by -SiR3, and examples of silyl may be selected from alkylsilyl groups, arylsilyl groups, alkylarylsilyl groups, and heteroarylsilyl groups, but are not limited thereto. More specific examples include, but are not limited to, trimethylsilyl groups, triethylsilyl groups, t-butyldimethylsilyl groups, vinyldimethylsilyl groups, propyldimethylsilyl groups, triphenylsilyl groups, diphenylsilyl groups, and phenylsilyl groups.
[0052] The term "substituted or unsubstituted" as used herein may mean substituted or unsubstituted with one or more groups selected from the group consisting of an alkoxy group, an alkynyloxy group, a heteroaryl group, an alkenyl group, a heterocycloalkyl group, a carbonyl group, a halogen group, a hydroxy group, an alkenyloxy group, a carboxyl group, a carbonate group, an alkyl group, an alkynyl group, an amine group, a cycloalkyl group, a silyl group, a sulfonate group, a phosphate group, a thiophosphate group, a nitro group, a cyano group, a heteroalkyl group, a cycloalkyl group, an aryl group, and an ether group.
[0053] Additionally, throughout this specification, identical symbols may have the same meaning unless specifically stated otherwise.
[0054] The present invention relates to a compound for an electrolyte, a compound for an electrolyte additive, an electrolyte material, an electrolyte additive, an electrolyte for a secondary battery, and a secondary battery.
[0055] One aspect of the present invention provides an electrolyte for a secondary battery comprising a novel compound or an isomer thereof.
[0056] The above compound can be represented by the following chemical formula 1.
[0057] [Chemical Formula 1]
[0058]
[0059] In the above chemical formula 1, carbons in the ring are connected by single or double bonds;
[0060] wherein X is oxygen or sulfur;
[0061] wherein Y is oxygen or sulfur;
[0062] The above Z 1 , Z 2 , and Z 3 are each independently hydrogen, substituted or unsubstituted C 1-10 Alkyl, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Amine, substituted or unsubstituted C 1-10 Acyl, substituted or unsubstituted C 1-10 alkynyl, substituted or unsubstituted C 3-10 Cycloalkyl, substituted or unsubstituted silyl, substituted or unsubstituted C 1-10 Alkoxy, substituted or unsubstituted C 1-12 Heteroalkyl, substituted or unsubstituted C 1-6 Heterocycloalkyl, -SO2R 1 , -P(=G)(OR 1 )2, -P(=G)(R 1 ) is selected from the group consisting of 2;
[0063] The above Z 1 and Z 2 may or may not combine with each other to form a ring;
[0064] wherein G is oxygen or sulfur;
[0065] The above R 1 Silver substituted or unsubstituted C 1-6 Alkyl, C 2-6 Alkenyl, C 2-6 alkynyl or C 6-20 It could be Aryl.
[0066] In one embodiment of the present invention, the compound represented by the above chemical formula 1 is a compound derived from a heterocyclic compound and can be added to the electrolyte as an additive for a lithium secondary battery electrolyte. The additive of the present invention can form a stable SEI (Solid Electrolyte Interphase) film on the surface of the negative electrode while minimizing an increase in the resistance of the lithium secondary battery. Therefore, by suppressing the decline in the passivation ability of the SEI at high temperatures, deterioration of the negative electrode is prevented, and a film that facilitates lithium movement is formed, thereby improving the lifespan at room temperature.
[0067] The compound represented by the chemical formula 1 of the present invention is specifically Z 1 Each of these independently hydrogen, substituted or unsubstituted C 1-10 Alkyl, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Amine, substituted or unsubstituted C 1-10 Acyl, substituted or unsubstituted C 1-10 alkynyl, substituted or unsubstituted C 3-10 Cycloalkyl, substituted or unsubstituted silyl, -SO2R 1 and -P(=G)(OR 1 )2 is selected from the group consisting of, and the Z 2 , and Z 3 are each independently hydrogen, substituted or unsubstituted C 1-10 Alkyl, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Alkoxy, substituted or unsubstituted C 1-12 It can be selected from the group consisting of heteroalkyl.
[0068] The compound represented by the chemical formula 1 of the present invention is more specifically Z 1 Each of these independently hydrogen, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Acyl, substituted or unsubstituted C 1-10alkynyl, -SO2R 1 is selected from the group consisting of, and the Z 2 , and Z 3 are each independently hydrogen, substituted or unsubstituted C 1-10 It can be selected from the group consisting of alkyl.
[0069] The substituted alkyl, alkenyl, amine, acyl, alkynyl, cycloalkyl, silyl, alkoxy, heteroalkyl, and heterocycloalkyl of the present invention may each be independently substituted with one or more substituents selected from the group consisting of an alkoxy group, an alkynyloxy group, a heteroaryl group, an alkenyl group, a heterocycloalkyl group, a carbonyl group, a halogen group, a hydroxy group, an alkenyloxy group, a carboxyl group, a carbonate group, an alkyl group, an alkynyl group, an amine group, a cycloalkyl group, a silyl group, a sulfonate group, a phosphate group, a thiophosphate group, a nitro group, a cyano group, a heteroalkyl group, a cycloalkyl group, an aryl group, and an ether group. For example, the substituted alkoxy group may be substituted with an alkenyl group, an alkynyl group, an amine group, a cycloalkyl group, a carbonyl group, or a silyl group, the substituted heterocycloalkyl group may be substituted with a carbonyl group, the substituted carboxyl group may be substituted with a heteroaryl group, an alkenyl group, a heterocycloalkyl group, a carbonyl-substituted heterocycloalkyl group, or a halogen group, and the substituted carbonate group may be substituted with an alkyl group or an alkynyl group. In addition, the substituted sulfonate group may be substituted with an alkyl group, an alkenyl group, or a halogen-substituted alkyl group, and the substituted sulfonate group and thiophosphate group may each be independently substituted with an alkyl group.
[0070] The secondary battery electrolyte of the present invention contains the compound represented by the above chemical formula 1 as an additive, and may further contain additional additives. For example, the electrolyte may further contain one or more additives selected from the group consisting of LiPO2F2, unsaturated cyclic carbonates, cyclic sultones, cyclic sulfate lactones, nitrile compounds, and mixtures thereof, but is not limited thereto.
[0071] The unsaturated cyclic carbonate of the present invention is a cyclic carbonate having a carbon-carbon unsaturated bond, for example, a carbonate having a carbon-carbon unsaturated bond such as a carbon-carbon double bond or a carbon-carbon triple bond, and is not particularly limited, and any unsaturated cyclic carbonate can be used.
[0072] As the additional additive of the present invention, for example, one or more selected from the group consisting of vinylene carbonate, phenyl carbonate, vinyl carbonate, and allyl carbonate may be added as the unsaturated cyclic carbonate. As the vinylene carbonates, one or more selected from the group consisting of vinylene carbonate, methyl vinylene carbonate, 4,5-dimethyl vinylene carbonate, phenyl vinylene carbonate, 4,5-diphenyl vinylene carbonate, vinyl vinylene carbonate, 4,5-vinyl vinylene carbonate, allyl vinylene carbonate, and 4,5-diallyl vinylene carbonate may be added.
[0073] As an additional additive of the present invention, a cyclic sultone may be added, and in one embodiment, 1,3-propane sultone, 1-fluoro-1,3-propane sultone, 2-fluoro-1,3-propane sultone, 3-fluoro-1,3-propane sultone, 1,4-butane sultone, methylene methane disulfonate, and ethylene methane disulfonate are preferable in terms of improving preservation characteristics, and at least one selected from the group consisting of 1,3-propane sultone, 1-fluoro-1,3-propane sultone, 2-fluoro-1,3-propane sultone, and 3-fluoro-1,3-propane sultone may be added.
[0074]
[0075] As a specific embodiment of the present invention, the compound represented by the chemical formula 1 may include at least one compound selected from the group represented by the following chemical formula or an isomer thereof:
[0076] [Correction pursuant to Rule 91, July 19, 2024]
[0077] [Correction pursuant to Rule 91, July 19, 2024]
[0078] [Correction pursuant to Rule 91, July 19, 2024]
[0079] [Correction pursuant to Rule 91, July 19, 2024]
[0080] [Correction pursuant to Rule 91, July 19, 2024]
[0081] [Correction pursuant to Rule 91, July 19, 2024]
[0082] [Correction pursuant to Rule 91, July 19, 2024]
[0083] [Correction pursuant to Rule 91, July 19, 2024]
[0084] [Correction pursuant to Rule 91, July 19, 2024]
[0085] [Correction pursuant to Rule 91, July 19, 2024]
[0086] [Correction pursuant to Rule 91, July 19, 2024]
[0087]
[0088]
[0089] Additionally, the compounds of the present invention may have a chiral carbon center and may therefore exist in the form of R or S isomers, racemates, individual enantiomers or mixtures, individual diastereomers or mixtures, and all such stereoisomers and mixtures thereof may fall within the scope of the present invention.
[0090] The compound of the present invention may be included in an amount of about 0.1 wt% or more based on the total weight of the entire electrolyte, but is not limited thereto, and an appropriate amount may be used as needed within the above content range.
[0091] If the content of the above compound in the entire electrolyte is excessively high, the battery may expand due to excessive gas, thereby reducing the life characteristics.
[0092] From this point of view, the content of the compound is 0.01 to 10 wt%; 0.01 to 9 wt%; 0.01 to 8 wt%; 0.01 to 7 wt%; 0.01 to 6 wt%; 0.01 to 5 wt%; 0.01 to 4 wt%; 0.01 to 3 wt%; 0.01 to 2 wt%; 0.01 to 1 wt%; 0.1 to 10 wt%; 0.1 to 9 wt%; 0.1 to 8 wt%; 0.1 to 7 wt%; 0.1 to 6 wt%; 0.1 to 5 wt%; 0.1 to 4 wt%; 0.1 to 3 wt%; 0.1 to 2 wt%; 0.1 to 1 wt%; 1 to 10 wt%; 1 to 9 wt%; 1 to 8 wt%; 1 to 7 wt%; 1 to 6 wt%; 1 to 5 wt%; 1 to 4 wt%; 1 to 3 wt%; 1 to 2 wt%; 5 to 10 wt%; 5 to 9 wt%; 5 to 8 wt%; 5 to 7 wt%; or 5 to 6 wt%, but any range that functions as an overcharge prevention agent and does not deteriorate the life characteristics may be used.
[0093] Meanwhile, in one embodiment, the electrolyte for the secondary battery may further include a lithium salt and an organic solvent.
[0094] The concentration of the lithium salt in the above electrolyte may be about 0.01 to 2.0 M, but is not necessarily limited to this range, and an appropriate concentration may be used as needed. Within the above concentration range, further improved battery characteristics can be obtained.
[0095] The lithium salt used in the above electrolyte is not particularly limited and any lithium salt that can be used in the relevant technical field may be used. For example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiC2F6NO4S2, LiB(C2O4)2, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(x and y are independent integers greater than or equal to 1), LLiCl and LiI, at least one selected from the group consisting of may be used.
[0096] The organic solvent may include at least one selected from the group consisting of dialkyl carbonates, cyclic carbonates, linear or cyclic esters, linear or cyclic amides, aliphatic nitriles, linear or cyclic ethers, and derivatives thereof.
[0097] Specifically, the organic solvent may include at least one selected from the group consisting of dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, ethyl propyl carbonate, diethyl carbonate (DEC), dipropyl carbonate, propylene carbonate (PC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), butylene carbonate, ethyl propionate (EP), ethyl butyrate, acetonitrile (AN), succinonitrile (SN), dimethyl sulfoxide, dimethyl formamide, dimethyl acetamide, gamma-valerolactone, gamma-butyrolactone, and tetrahydrofuran, but is not necessarily limited thereto, and any organic solvent that can be used in an organic electrolyte in the relevant technical field is possible.
[0098]
[0099] Another aspect of the present invention provides a secondary battery comprising the electrolyte for the secondary battery.
[0100] The secondary battery comprises an electrode assembly including a positive electrode, a negative electrode, and a separator separating the positive electrode and the negative electrode;
[0101] a case accommodating the electrode assembly; and
[0102] The secondary battery electrolyte may be contained within the case and immersed in the electrode assembly.
[0103] The above secondary battery is not particularly limited in its form, and includes, but is not limited to, a lithium ion battery, a lithium ion polymer battery, a lithium sulfur battery, a lithium air battery, etc.
[0104] For example, if the secondary battery is a lithium ion battery, it can be manufactured by the following method.
[0105] First, the anode is prepared.
[0106] For example, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The positive electrode active material composition is directly coated on a metal current collector to manufacture a positive electrode plate. Alternatively, the positive electrode active material composition may be cast on a separate support, and then a film peeled from the support may be laminated on a metal current collector to manufacture a positive electrode plate. The positive electrode is not limited to the forms listed above and may have forms other than those listed above.
[0107] The above-mentioned positive electrode active material is a lithium-containing metal oxide, and any one commonly used in the art can be used without limitation. For example, one or more types of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used, and specific examples thereof include Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α(In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Lia CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:
[0108] In the chemical formula, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.
[0109] For example, LiCoO2, LiMn x O 2x (x=1, 2), LiNi 1-x Mn x O 2x (0 <x<1), LiNi 1-x-y Co x Mn y O2(0≤x≤0.5, 0≤y≤0.5), LiFePO4, etc.
[0110] Of course, a compound having a coating layer on the surface of the compound may be used, or a compound having the compound and a coating layer may be mixed and used. The coating layer may include a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element. The compounds forming these coating layers may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating layer forming process may use any coating method as long as it can coat the compound with these elements and does not adversely affect the properties of the positive electrode active material (for example, spray coating, dipping, etc.). Since this is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0111] Carbon black, graphite particles, etc. may be used as the above-mentioned conductive material, but are not limited thereto, and any conductive material that can be used in the relevant technical field may be used.
[0112] As the above binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene and mixtures thereof, or styrene butadiene rubber polymers may be used, but are not limited thereto, and any binder that can be used in the relevant technical field may be used.
[0113] The solvent may include, but is not limited to, N-methylpyrrolidone, acetone, or water, and any solvent that can be used in the relevant technical field may be used.
[0114] The above contents of the positive electrode active material, conductive agent, binder, and solvent are at levels typically used in lithium ion batteries. Depending on the intended use and configuration of the lithium ion battery, one or more of the conductive agent, binder, and solvent may be omitted.
[0115] Next, the cathode is prepared.
[0116] For example, a negative electrode active material composition is prepared by mixing a negative electrode active material, a conductive agent, a binder, and a solvent. The negative electrode active material composition is directly coated and dried on a metal current collector to produce a negative electrode plate. Alternatively, the negative electrode active material composition may be cast on a separate support, and then a film peeled from the support may be laminated on a metal current collector to produce a negative electrode plate.
[0117] The above-mentioned negative electrode active material may be any material that can be used as a negative electrode active material for lithium-ion batteries in the relevant technical field. For example, it may include one or more selected from the group consisting of lithium metal, metals alloyable with lithium, transition metal oxides, non-transition metal oxides, and carbon-based materials.
[0118] For example, the metal that can be alloyed with the lithium may be Si, Sn, Al, Ge, Pb, Bi, Sb Si-Y alloy (wherein Y is an alkali metal, an alkaline earth metal, a group 13 element, a group 14 element, a transition metal, a rare earth element, or a combination thereof, and is not Si), Sn-Y alloy (wherein Y is an alkali metal, an alkaline earth metal, a group 13 element, a group 14 element, a transition metal, a rare earth element, or a combination thereof, and is not Sn), etc. The above element Y may be Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof.
[0119] For example, the transition metal oxide may be lithium titanium oxide, vanadium oxide, lithium vanadium oxide, or the like.
[0120] For example, the above non-transition metal oxides are SnO2, SiO x (0 <x<3) 등일 수 있다.
[0121] The carbonaceous material may be crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon may be graphite such as natural graphite or artificial graphite in an amorphous, plate-like, flake-like, spherical, or fibrous form, and the amorphous carbon may be soft carbon (low-temperature calcined carbon) or hard carbon, mesophase pitch carbide, calcined coke, or the like.
[0122] In the negative electrode active material composition, the conductive material and binder may be the same as those used in the positive electrode active material composition.
[0123] The contents of the above negative active material, conductive material, binder, and solvent are at levels typically used in lithium ion batteries. Depending on the intended use and configuration of the lithium ion battery, one or more of the conductive material, binder, and solvent may be omitted.
[0124] Next, a separator that separates the positive and negative electrodes is prepared.
[0125] Any separator commonly used in lithium-ion batteries can be used. A separator with low resistance to ion movement of the electrolyte and excellent electrolyte absorption capacity can be used. For example, a separator selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or a combination thereof may be in the form of a non-woven fabric or a woven fabric. For example, a rollable separator such as polyethylene or polypropylene is used for lithium-ion batteries, and a separator with excellent organic electrolyte absorption capacity can be used for lithium-ion polymer batteries. For example, the separator can be manufactured according to the following method.
[0126] A separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition may be directly coated and dried on an electrode to form a separator. Alternatively, the separator composition may be cast on a support and dried, and then a separator film peeled from the support may be laminated on an electrode to form a separator.
[0127] The polymer resin used in the manufacture of the above-mentioned separator is not particularly limited, and all materials used as a binder for electrode plates can be used. For example, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof can be used.
[0128] Next, the electrolyte for the secondary battery described above is prepared.
[0129] As shown in Fig. 1, the secondary battery (1) includes a positive electrode (40), a negative electrode (60), and a separator (50). The positive electrode (40), negative electrode (60), and separator (50) described above are wound or folded and accommodated in a case (10, 80). Subsequently, an electrolyte is injected into the case (10, 80), thereby completing the secondary battery (1).
[0130] The above case can have various shapes depending on the purpose of use, design specifications, etc. of the secondary battery, and can be formed to have various sizes and shapes such as a square shape, a thin film shape, and a coin shape.
[0131] For example, the secondary battery may be a coin-type battery. As a specific example, the secondary battery may be a lithium-ion battery.
[0132] A separator may be placed between the positive and negative electrodes to form an electrode assembly. The electrode assembly is then laminated in a bi-cell structure, impregnated with an electrolyte, and the resulting product is contained in a pouch and sealed, thereby completing a lithium ion polymer battery.
[0133] Additionally, the electrode assemblies are stacked in multiples to form a battery pack, which can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc.
[0134]
[0135] Hereinafter, the present invention will be described in detail through manufacturing examples, examples, and experimental examples.
[0136] However, the manufacturing examples, examples, and experimental examples described below are only specific examples of one aspect of the present invention, and the present invention is not limited thereto.
[0137]
[0138] <Manufacturing Example 1> Preparation of Compound 1
[0139]
[0140] Compound 1
[0141] 4-Hydroxymethyl-2-oxazolidinone (5 g, 0.04 mol) and triethylamine (6.5 g, 0.06 mol) were dissolved in dimethylformamide (20 ml) in a 250 mL 3-necked reactor, then ethyl acetate (80 ml) was added and cooled to 0°C. Methanesulfonyl chloride (14.9 g, 0.05 mol) was added dropwise and stirred for 1 hour.
[0142] Ethyl acetate (50 mL) and water (50 mL) were added to a reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with ethyl acetate (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0143] Compound 1 (5.6 g, yield: 70%) was obtained, which 1 H-NMR and 13 Confirmed by C-NMR.
[0144] 1 H-NMR (400 MHz, DMSO-d6) d 7.95 (s, 1H), 4.25-4.37 (m, 1H), 4.23-4.15 (m, 2H), 4.14-4.08 (m, 2H), 3.23 (s, 3H) 13 C-NMR 400 MHz, DMSO-d6) d 159.1, 71.0, 65.9, 50.9, 37.1
[0145]
[0146] <Manufacturing Example 2> Preparation of Compound 2
[0147]
[0148] Compound 2
[0149] In a 250 mL 3-necked reactor, 2-oxazolidinone (8 g, 0.09 mol) and triethylamine (18.6 g, 0.18 mol) were dissolved in methylene chloride (80 mL), and then cooled to 0°C. Propargyl chloroformate (12.5 g, 0.1 mol) was added dropwise, and the mixture was stirred for 2 hours.
[0150] Water (80 mL) was added to the reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with methylene chloride (100 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0151] Compound 2 was obtained in 13g (yield: 84%), which 1 H-NMR and 13 Confirmed by C-NMR.
[0152] 1 H-NMR (400 MHz, CDCl3) d 4.86 (d, 2H,J=0.006Hz), 4.42-4.38 (m, 2H), 4.08-4.04(m, 2H), 2.55-2.54 (m, 1H) 13 C-NMR 400 MHz, CDCl3) d 151.7, 150.3, 76.7, 76.1, 61.8, 54.4, 43.4
[0153]
[0154] <Manufacturing Example 3> Preparation of Compound 3
[0155]
[0156] Compound 3
[0157] In a 250 mL 3-necked reactor, 2-thiazolidinone (8 g, 0.08 mol) and triethylamine (15.7 g, 0.16 mol) were dissolved in methylene chloride (80 mL), and then cooled to 0 °C. Propargyl chloroformate (10.5 g, 0.09 mol) was added dropwise, and the mixture was stirred for 2 hours.
[0158] Water (80 mL) was added to the reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with methylene chloride (100 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0159] Compound 3 was obtained in 12g (yield: 84%), which 1 H-NMR and 13 Confirmed by C-NMR.
[0160] 1 H-NMR (400 MHz, CDCl3) d 4.84 (d, 2H,J=0.006Hz), 4.18-4.14 (m, 2H), 3.32-3.28 (m, 2H), 2.54-2.53 (m, 1H) 13 C-NMR 400 MHz, CDCl3) d 170.2, 149.9, 76.8, 76.0, 54.3, 47.6, 25.2
[0161]
[0162] <Manufacturing Example 4> Preparation of Compound 4
[0163]
[0164] Compound 4
[0165] In a 250 mL 3-necked reactor, 4-hydroxymethyl-2-oxazolidinone (5 g, 0.04 mol) and triethylamine (6.5 g, 0.06 mol) were dissolved in dimethylformamide (20 mL), and then cooled to 0°C. Methanesulfonyl chloride (19.7 g, 0.17 mol) was added dropwise, and the mixture was stirred for 1 hour.
[0166] Ethyl acetate (50 mL) and water (50 mL) were added to a reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with ethyl acetate (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0167] Compound 4 (7.2 g) (yield: 75.9%) was obtained, which1 Confirmed by H-NMR.
[0168] 1 H-NMR (400 MHz, CDCl3) d 4.517-4.478 (t,1H), 4.122-4.083 (t, 1H), 3.347 (s, 3H)
[0169]
[0170] <Manufacturing Example 5> Preparation of Compound 5
[0171]
[0172] Compound 5
[0173] In a 100 mL three-necked reactor, oxazolidinone (5 g, 0.048 mol) was added to dimethylformamide (60 mL), stirred at room temperature for 10 minutes, and then cooled to 0°C. After cooling, 60% sodium hydride (2.3 g, 0.058 mol) was added in portions, stirred for 30 minutes, and 80% propargyl bromide (10.1 g, 0.068 mol) was added dropwise, heated to room temperature, and stirred for 1 hour.
[0174] A saturated aqueous solution of ammonium chloride (40 mL) was added to the reactor, stirred vigorously, and allowed to settle to allow the layers to separate. The aqueous layer was extracted with ethyl acetate (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was then concentrated and purified by column chromatography.
[0175] Compound 5 (6.8 g) (yield: 80%) was obtained, which 1 H-NMR and 13 Confirmed by C-NMR.
[0176] 1 H-NMR (400 MHz, CDCl3-d) d 4.38-4.34 (m, 2H), 4.09-4.08 (m, 2H), 3.68-3.64 (m, 2H), 2.31-2.30 (m, 1H), 13 C-NMR (400 MHz, CDCl3-d) d 158.0, 76.9, 73.4, 62.1, 43.9, 34.1
[0177]
[0178] <Manufacturing Example 6> Preparation of compound 6
[0179]
[0180] Compound 6
[0181] In a 250 mL 3-necked reactor, 4-hydroxymethyl-2-oxazolidinone (5 g, 0.04 mol) and triethylamine (6.5 g, 0.06 mol) were dissolved in dimethylformamide (20 ml), then ethyl acetate (80 ml) was added and cooled to 0°C. Vinylsulfonyl chloride (6.7 g, 0.05 mol) was added dropwise and stirred for 1 hour.
[0182] Ethyl acetate (50 mL) and water (50 mL) were added to a reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with ethyl acetate (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0183] Compound 6 (6.2g, yield: 70%) was obtained, which 1 H-NMR and 13 Confirmed by C-NMR.
[0184] 1 H-NMR (400 MHz, DMSO-d6) d 7.93 (s, 1H), 7.04-6.97 (m, 1H), 6.37 (dd, 2H, J=4Hz), 4.40-4.13 (m, 1H), 4.13-4.04 (m, 4H), 13 C-NMR (400 MHz, DMSO-d6) d 159.0, 132.6, 132.5, 71.5, 65.8, 50.8
[0185]
[0186] <Manufacturing Example 7> Preparation of compound 7
[0187]
[0188] Compound 7
[0189] In a 250 mL 3-necked reactor, 4-hydroxymethyl-2-oxazolidinone (5 g, 0.04 mol) and triethylamine (6.5 g, 0.06 mol) were dissolved in dimethylformamide (20 ml), then ethyl acetate (80 ml) was added and cooled to 0°C. Trifluoromethanesulfonyl chloride (8.6 g, 0.05 mol) was added dropwise and stirred for 1 hour.
[0190] Ethyl acetate (50 mL) and water (50 mL) were added to a reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with ethyl acetate (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0191] Compound 7 was obtained in 7.9 g (yield: 73%), which 1 H-NMR, 13 C-NMR and 19 Confirmed by F-NMR.
[0192] 1 H-NMR (400 MHz, DMSO-d6) d 7.95 (s, 1H), 4.43-4.37 (m, 2H), 4.34-4.27 (m, 1H), 4.13-4.07 (m, 2H), 13 C-NMR (400 MHz, DMSO-d6) d 159.0, 128.2, 124.8, 121.5, 118.1, 70.7, 65.7, 51.5, 19 F-NMR (400 MHz, DMSO-d6) d -78.8
[0193]
[0194] <Manufacturing Example 8> Preparation of compound 8
[0195]
[0196] Compound 8
[0197] In a 100 mL 3-necked reactor, add 60% sodium hydride (1.65 g, 0.041 mol) to dimethylformamide (20 ml) and cool to 0°C. In another flask, prepare a solution of oxazolidinone (3 g, 0.034 mol) dissolved in dimethylformamide (40 ml). Once the sodium hydride solution has cooled to 0°C, the oxazolidinone solution was added dropwise and stirred for 30 minutes. After cooling to 0°C again, allyl bromide (5.53 g, 0.052 mol) was added dropwise, warmed to room temperature, and stirred for 1 hour.
[0198] Purified water (40 mL) was added to the reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with ethyl acetate (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was then concentrated and purified by column chromatography.
[0199] Compound 8 (3.4 g, yield: 77.6%) was obtained, which 1 H-NMR and 13 Confirmed by C-NMR.
[0200] 1 H-NMR (400 MHz, CDCl3-d) d 5.81-5.71 (m, 1H), 5.26-5.22 (m, 2H), 4.34-4.30 (m, 2H), 3.86-3.85 (m, 2H), 3.53-3.49 (m, 2H), 13 C-NMR (400 MHz, CDCl3-d) d 157.9, 131.8, 117.4, 63.3, 44.7, 51.8,
[0201]
[0202] <Manufacturing Example 9> Preparation of compound 9
[0203]
[0204] Compound 9
[0205] In a 100 mL 3-necked reactor, add 60% sodium hydride (1.4 g, 0.035 mol) to dimethylformamide (20 ml) and cool to 0°C. In another flask, prepare a solution of thiazolidinone (3 g, 0.029 mol) dissolved in dimethylformamide (40 ml). Once the sodium hydride solution has cooled to 0°C, the thiazolidinone solution was added dropwise and stirred for 30 minutes. After cooling to 0°C again, allyl bromide (4.67 g, 0.044 mol) was added dropwise, warmed to room temperature, and stirred for 1 hour.
[0206] Purified water (40 mL) was added to the reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with ethyl acetate (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was then concentrated and purified by column chromatography.
[0207] Compound 9 (3.1 g, yield: 74.4%) was obtained, which 1 H-NMR and 13 Confirmed by C-NMR.
[0208] 1 H-NMR (400 MHz, CDCl3-d) d 5.79-5.70 (m, 1H), 5.24-5.19 (m, 2H), 3.92-3.90 (m, 2H), 3.60-3.57 (m, 2H), 3.28-3.24 (m, 2H), 13 C-NMR (400 MHz, CDCl3-d) d 171.4, 117.4, 131.8, 53.0, 43.5, 29.0
[0209]
[0210] <Manufacturing Example 10> Preparation of compound 10
[0211]
[0212] Compound 10
[0213] 4-Hydroxymethyl-2-oxazolidinone (3.5 g, 0.03 mol) and triethylamine (6.7 g, 0.066 mol) were dissolved in dimethylformamide (30 ml) in a 100 mL 3-necked reactor and stirred.
[0214] In a 50 mL three-necked reactor, perfluorobutanoic acid (6.42 g, 0.03 mol) was dissolved in dimethylformamide (2.63 g, 0.036 mol), and then thionyl chloride (3.75 g, 0.032 mol) was added dropwise over 30 minutes. This solution was added dropwise to a 100 mL three-necked reactor over 10 minutes and stirred for 2 hours.
[0215] The reaction solution was filtered, washed with dichloromethane, and concentrated. Dichloromethane was dissolved in the concentrate, anhydrous magnesium sulfate was added, and the mixture was stirred for 5 minutes. The solid was filtered off, and the filtrate was concentrated and purified by column chromatography.
[0216] Compound 10 (6.5 g) (yield: 69%) was obtained, which 1 It was confirmed by H-NMR.
[0217] 1 H-NMR (400 MHz, CDCl3) d 6.55 (s, 1H), 4.59-4.54 (m, 1H), 4.52-4.48 (m, 1H), 4.39-4.35 (m, 1H), 4.27-4.21 (m, 2H)
[0218]
[0219] <Manufacturing Example 11> Preparation of compound 11
[0220]
[0221] Compound 11
[0222] Thiazolidinone (5 g, 0.049 mol) and triethylamine (9.82 g, 0.097 mol) were added to dichloromethane (50 ml) in a 100 mL 3-necked reactor, stirred at room temperature for 30 minutes, and then cooled to -10°C. After cooling, methanesulfonyl chloride (7.0 g, 0.058 mol) was added dropwise, followed by stirring for 1 hour.
[0223] Water (50 mL) was added to the reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with dichloromethane (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0224] Compound 11 (6.8 g, yield: 77.3%) was obtained, which 1 H-NMR and 13 Confirmed by C-NMR.
[0225] 1 H-NMR (400 MHz, CDCl3-d) d 4.18-4.14 (m, 2H), 3.42-3.40 (m, 2H), 3.31 (s, 3H), 13 C-NMR (400 MHz, CDCl3-d) d 173.2, 45.6, 36.8, 27.5
[0226]
[0227] <Manufacturing Example 12> Preparation of compound 12
[0228]
[0229] Compound 12
[0230] In a 250 mL 3-necked reactor, 4-hydroxymethyl-2-oxazolidinone (5 g, 0.04 mol) and triethylamine (6.5 g, 0.06 mol) were dissolved in dimethylformamide (20 ml), then ethyl acetate (80 ml) was added and cooled to 0°C. Propargyl chloroformate (6 g, 0.05 mol) was added dropwise and stirred for 1 hour.
[0231] Ethyl acetate (50 mL) and water (50 mL) were added to a reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with ethyl acetate (50 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0232] Compound 12 (4.3 g) (yield: 75%) was obtained, which 1H-NMR and 13 Confirmed by C-NMR.
[0233] 1 H-NMR (400 MHz, DMSO-d6) d 7.89 (s, 1H), 4.79 (s, 2H), 4.40-4.31 (m, 1H), 4.16-4.04 (m, 4H), 3.67 (s, 1H), 13 C-NMR (400 MHz, DMSO-d6) d 159.1, 154.3, 78.7, 69.8, 66.14, 55.9, 50.7
[0234]
[0235] <Manufacturing Example 13> Preparation of compound 13
[0236]
[0237] Compound 13
[0238] In a 250 mL 3-necked reactor, 1,3-oxazolidino-2-thione (5 g, 0.05 mol) and triethylamine (9.8 g, 0.1 mol) were dissolved in methylene chloride (50 mL), and then cooled to 0°C. Propargyl chloroformate (6.9, 0.06 mol) was added dropwise, and the mixture was stirred for 2 hours.
[0239] Water (80 mL) was added to the reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with methylene chloride (100 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0240] Compound 13 (7.2 g) (yield: 80.2%) was obtained and confirmed by ESI-MS.
[0241] ESI-MS m / z 185.01 [M+H] +
[0242]
[0243] <Manufacturing Example 14> Preparation of compound 14
[0244]
[0245] Compound 14
[0246] In a 250 mL 3-necked reactor, dissolve 1-amino-2-propanol (6.4 g, 0.09 mol) in methylene chloride (70 ml), add triethylamine (25.9 g, 0.26 mol), and stir under nitrogen. Then, add triphosgene (12.6 g, 0.04 mol) and stir at room temperature for 20 hours. The reaction is terminated with ammonium chloride aqueous solution (10 ml).
[0247] Water (80 mL) was added to the reactor, stirred vigorously, and allowed to settle to separate the layers. The aqueous layer was extracted with methylene chloride (100 mL x 2). Anhydrous magnesium sulfate was added to the organic layer, stirred for 5 minutes, and the solid was filtered. The filtrate was concentrated and purified by column chromatography.
[0248] Compound 14 (4g) (yield: 46.4%) was obtained and confirmed by ESI-MS.
[0249] ESI-MS m / z 102 [M+H] +
[0250]
[0251] <Example 1> Preparation of electrolyte for secondary battery
[0252] 1.0 M LiPF6 was dissolved in a solvent containing ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) in a volume ratio of 20:40:40.
[0253] Based on the total weight of the electrolyte (100 wt%), the electrolytes of the examples and comparative examples were prepared by adding additives according to Table 1 below.
[0254]
[0255]
[0256]
[0257]
[0258] <Example 2> Manufacturing of Coin Cell
[0259] A slurry of negative active material was prepared by mixing 96 wt% of artificial graphite (S360-L2-H Tiangin BTR New energy technology Co., Ltd.), 1 wt% of SuperP (TIMCAL), 1.5 wt% of styrene-butadiene rubber (SBR) binder (ZEON), and 1.5 wt% of carboxymethyl cellulose (CMC, Sigma-Aldrich), then adding it to distilled water and stirring for 60 minutes using a mechanical stirrer. The slurry was applied to a thickness of about 60 μm on a copper current collector with a thickness of 30 μm using a doctor blade and 100 o After drying for 1 hour in a C hot air dryer, the negative electrode plate was manufactured by drying again for 8 hours under vacuum conditions and rolling.
[0260] LiNi 0.6 Mn 0.2 Co 0.2 A slurry of cathode active material was prepared by mixing 2 wt% superP (TIMCAL) as a conductive agent and 2% polyvinylidene fluoride (PVdF, Sigma-Aldrich) in an N-methyl-2-pyrrolidone solvent and stirring for 30 minutes using a mechanical stirrer. The slurry was applied to a thickness of 60 μm on a 20 μm thick aluminum current collector using a doctor blade and 100 o The positive electrode plate was manufactured by drying in a C hot air dryer for 1 hour, drying again for 8 hours under vacuum conditions, and rolling (roll pressing).
[0261] Lithium batteries were manufactured using 14 μm thick polypropylene as a separator and the organic electrolytes manufactured in Examples 1 to 19 as electrolytes.
[0262]
[0263] <Experimental Example 1> Room Temperature Life Performance Evaluation
[0264] A lithium secondary battery was charged at a constant current of 1.0 C-rate to 4.2 V under constant current / constant voltage (CC / CV) conditions at 25°C, cut-off at 0.05 C-rate while maintaining 4.2 V in constant voltage mode, and then discharged at 1.0 C-rate to 2.7 V. The above charge / discharge conditions were repeated for one cycle.
[0265] The results of the analysis are shown in Table 2 and Figures 2 to 5.
[0266] ClassificationRoom temperature lifespan efficiency(%)Charge / discharge cycles (1C)Comparative example 186.2200Comparative example 289.2200Comparative example 375.7200Comparative example 489.5200Comparative example 589.6200Example 191.4200Example 293.2200Example 392.7200Example 491.8200Comparative example 689.2100Comparative example 791.4100Example 593.2100Example 693.0100Example 793.6100Example 895.1100Example 995.1100Example 1093.4100Example 1191.1200Example 1294.2100 Example 1395.4200 Example 1495.0200 Example 1595.0200 Example 1694.3200 Example 1793.5200 Example 1894.9200 Example 1993.1200
[0267] Looking at Table 2 and Figures 2 and 5 above, it was confirmed that the example using the compound of the present invention as an additive had a superior room temperature lifespan than the comparative example as a result of repeated charge / discharge cycles at 25°C. In addition, looking at Table 2 and Figures 3 and 4, it was confirmed that the lifespan increased when vinylene carbonate (VC) and lithium salt (LiPO2F2) additives were combined compared to when they were used alone.
[0268] <Experimental Example 2> Resistance Improvement Performance Evaluation
[0269] The battery manufactured according to the example was charged at 1C to 4.2 V, discharged to SOC50, and then discharged at four C-rates (0.5, 1, 2, 3 C) for 10 seconds each to measure the initial direct current resistance (DC-IR). After charging at 1C to 4.2 V and charging and discharging 200 times at room temperature, the DC resistance (DC-IR) was measured in the same manner as the initial DC resistance measurement method, and the percentage compared to the initial DC-IR was indicated in Table 3.
[0270] Discharge resistance (initial DCIR, Ω)Discharge resistance after 200 cycles (DC-IR, Ω after 200 cycles of charge and discharge)DC-IR increase rate (%)Comparative example 1 13.72 3.37 0.1Comparative example 2 13.52 2.86 8.9Comparative example 3 12.92 2.37 2.9Comparative example 4 13.72 2.16 1.3Comparative example 5 14.42 5.27 5.0Example 1 13.02 0.75 9.2Example 2 13.91 9.33 8.8Example 3 13.72 0.54 9.6Example 4 13.82 0.347.1 Example 1117.025.851.8 Example 1315.120.737.1 Example 1415.220.937.5 Example 1514.820.337.2 Example 1614.720.539.5 Example 1715.018.422.7 Example 1815.718.819.7 Example 1917.122.028.7
[0271] As can be seen in Table 3 above, in the examples using the compound manufactured according to the present invention, although the initial discharge resistance value was higher than that of the comparative example, the discharge resistance after 200 charges tended to be lower than that of the comparative example. In other words, it was confirmed that the DC-IR increase rate was lower than that of the comparative example.
[0272] Through this, it was confirmed that a film that facilitates the movement of lithium was formed by showing a low resistance increase rate when using the compound manufactured according to the present invention, and in particular, it was confirmed that the DC-IR increase rate was significantly reduced when vinylene carbonate (VC) and lithium salt (LiO2F2) additives were combined.
[0273]
[0274] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will readily appreciate that the present invention can be readily modified into other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.
[0275] The scope of the present invention is indicated by the claims described below, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.
Claims
1. An electrolyte for a secondary battery, comprising a compound represented by the following chemical formula 1, or an isomer thereof: [Chemical Formula 1] In the above chemical formula 1, carbons in the ring are connected by single or double bonds; wherein X is oxygen or sulfur; wherein Y is oxygen or sulfur; The above Z 1 , Z 2 , and Z 3 are each independently hydrogen, substituted or unsubstituted C 1-10 Alkyl, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Amine, substituted or unsubstituted C 1-10 Acyl, substituted or unsubstituted C 1-10 alkynyl, substituted or unsubstituted C 3-10 Cycloalkyl, substituted or unsubstituted silyl, substituted or unsubstituted C 1-10 Alkoxy, substituted or unsubstituted C 1-12 Heteroalkyl, substituted or unsubstituted C 1-6 Heterocycloalkyl, -SO2R 1 , -P(=G)(OR 1 )2 and -P(=G)(R 1 ) is selected from the group consisting of 2; The above Z 1 and Z 2 may or may not combine with each other to form a ring; wherein G is oxygen or sulfur; The above R 1 Silver substituted or unsubstituted C 1-6 Alkyl, C 2-6 Alkenyl, C 2-6 alkynyl or C 6-20 It's Aryl.
2. In paragraph 1, The above Z 1 are each independently hydrogen, substituted or unsubstituted C 1-10 Alkyl, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Amine, substituted or unsubstituted C 1-10 Acyl, substituted or unsubstituted C 1-10 alkynyl, substituted or unsubstituted C 3-10 Cycloalkyl, substituted or unsubstituted silyl, -SO2R 1 and -P(=G)(OR 1 ) is selected from the group consisting of 2, The above R 1 and G are as defined in clause 1, The above Z 2 , and Z 3 are each independently hydrogen, substituted or unsubstituted C 1-10 Alkyl, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Alkoxy, substituted or unsubstituted C 1-12 An electrolyte for a secondary battery, selected from the group consisting of heteroalkyl groups.
3. The above Z 1 are each independently hydrogen, substituted or unsubstituted C 1-10 Alkenyl, substituted or unsubstituted C 1-10 Acyl, substituted or unsubstituted C 1-10 alkynyl, -SO2R 1 is selected from the group consisting of, The above R 1 is as defined in paragraph 1, The above Z 2 , and Z 3 are each independently hydrogen, substituted or unsubstituted C 1-10 An electrolyte for a secondary battery, selected from the group consisting of alkyls.
4. In paragraph 1, An electrolyte for a secondary battery, wherein the above substituted alkyl, alkenyl, amine, acyl, alkynyl, cycloalkyl, silyl, alkoxy, heteroalkyl, and heterocycloalkyl are each independently substituted with one or more substituents selected from the group consisting of an alkoxy group, an alkynyloxy group, a heteroaryl group, an alkenyl group, a heterocycloalkyl group, a carbonyl group, a halogen group, a hydroxy group, an alkenyloxy group, a carboxyl group, a carbonate group, an alkyl group, an alkynyl group, an amine group, a cycloalkyl group, a silyl group, a sulfonate group, a phosphate group, a thiophosphate group, a nitro group, a cyano group, a heteroalkyl group, a cycloalkyl group, an aryl group, and an ether group.
5. In paragraph 1, An electrolyte for a secondary battery, wherein the electrolyte further comprises one or more additives selected from the group consisting of LiPO2F2, unsaturated cyclic carbonates, cyclic sultones, cyclic sulfate lactones, and nitrile compounds.
6. In paragraph 5, An electrolyte for a secondary battery, wherein the above unsaturated cyclic carbonate is selected from the group consisting of vinylene carbonate, phenyl carbonate, vinyl carbonate, and allyl carbonate.
7. [Revised on 19.07.2024 by Article 91 of the Rules] In paragraph 1, the secondary battery electrolyte comprises at least one compound selected from the group represented by the following chemical formula, or an isomer thereof:
8. In paragraph 1, An electrolyte for a secondary battery, wherein the electrolyte further comprises an organic solvent.
9. In paragraph 1, An electrolyte for a secondary battery, wherein the compound represented by the above chemical formula 1 is provided as an electrolyte additive.
10. In paragraph 1, The above secondary battery is a lithium ion battery, and the electrolyte for the secondary battery.
11. An electrode assembly including a positive electrode, a negative electrode, and a separator separating the positive electrode and the negative electrode; a case accommodating the electrode assembly; and A secondary battery comprising an electrolyte according to claim 1, which is accommodated in the case and immerses the electrode assembly.
Citation Information
Patent Citations
Non-aqueous electrolyte and lithium air battery including the same
KR1020120045464A
Nonaqueous electrolyte solution for batteries and lithium secondary battery
KR1020160032215A
Electrolyte additive for secondary battery, manufacturing method thereof, electrolyte, and secondary battery including the same
KR102283808B1
KR20200091628A
KR20240077389A