Composite modified pillared material and preparation method therefor, and fluoride-free and alkali-free accelerator based thereon and preparation method therefor

WO2024239390A1PCT designated stage expired Publication Date: 2024-11-28JIANGSU SOBUTE NEW MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/099323
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2023-06-09
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing fluorine-free and alkali-free quick-coagulant agents have problems with high supersaturation and poor stability of the solution system when increasing the aluminum phase content. The conventional modified materials have limited effect in improving the capacity of the column support material, which has affected the early stage of concrete. Strength and long-term stability.

Method used

The composite modified column support material modified with hyperbranched quaternary ammonium salt is used to significantly improve the capacity and stability of the column support material through intercalation modification with orthogonal column support material, and is used to prepare high concentration fluorine-free The alkali-free quick-coagulant combines complexing agent and ion inhibitor to form a stable three-dimensional network structure, which improves the supersaturation and stability of the system.

Benefits of technology

It achieves high solid content and long-term stability of fluorine-free and alkali-free quick-coagulant, reduces the probability of crystallization, and is suitable for high concentration fluorine-free and alkali-free quick-coagulant, which improves the early strength of concrete and the viscosity suitability in construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023099323-FTAPPB-I100001
    Figure PCTCN2023099323-FTAPPB-I100001
  • Figure PCTCN2023099323-FTAPPB-I100002
    Figure PCTCN2023099323-FTAPPB-I100002
  • Figure PCTCN2023099323-FTAPPB-I100003
    Figure PCTCN2023099323-FTAPPB-I100003
Patent Text Reader

Abstract

The present invention belongs to the technical field of concrete admixtures. Disclosed are a composite modified pillared material modified with a hyperbranched quaternary ammonium salt, and a preparation method therefor. According to the composite modified pillared material, a hyperbranched quaternary ammonium salt having a specific structure is used as a modified material, and differs from a common modified material having a long-chain structure since the material itself contains a branched structure, thereby ensuring that after an orthorhombic pillared material is intercalated, the interlayer spacing is larger, and the CEC capacity is higher. Further disclosed in the present invention are a fluoride-free and alkali-free accelerator comprising the composite modified pillared material as a stabilizer, and a preparation method therefor. Compared with a traditional alkali-free accelerator, the fluorine-free and alkali-free accelerator increases the use amount of aluminum sulfate therein to 10% or above, such that the supersaturation degree of an accelerator solution system is significantly increased, and the excellent effect of the fluorine-free and alkali-free accelerator in a concrete material is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Composite modified pillaring material and preparation method thereof, fluorine-free and alkali-free quick-setting agent based thereon and preparation method thereof Technical Field

[0001] The present invention belongs to the technical field of concrete admixtures, and specifically relates to a composite modified pillaring material modified with a hyperbranched quaternary ammonium salt and a preparation method thereof, as well as a fluorine-free and alkali-free quick-setting agent using the composite modified pillaring material as a stabilizer and a preparation method thereof. Background Art

[0002] Accelerators are a type of concrete admixture technology that allows cement and concrete to quickly set and harden. The development of accelerators is based on using aluminum salts as the core component and promoting the increase of aluminum salt concentrations through various means. Fluorine-free and alkali-free accelerators can avoid the harm of alkali-aggregate reaction to concrete, while also avoiding the hazards of fluorine-containing materials in preparation to production and life safety. Therefore, the development of fluorine-free and alkali-free accelerators is currently a research focus. In order to improve the performance of fluorine-free and alkali-free accelerators, increasing the aluminum phase content is the mainstream solution. At the same time, excessive aluminum salt content will lead to high supersaturation of the solution system, poor stability, and product stratification. Therefore, suitable stabilizers are of great practical significance.

[0003] Unlike traditional stabilizer materials, pillared materials have been widely studied due to their inherent porous / intercalated inorganic structure, which can be extensively modified to produce diverse structural characteristics. Currently, the most common modification targets are orthorhombic materials such as layered silicates, such as kaolin, montmorillonite, sepiolite, and talc. Modification techniques include ion exchange of metal ions and intercalation of organic anions and cations. Among these, modifications using anionic surfactants, such as sodium dodecyl sulfate or cationic surfactants, such as cetyltrimethylammonium bromide, have been widely reported.

[0004] For example, a suspension-type alkali-free liquid accelerator supersaturated with aluminum sulfate and its preparation method are described. The aluminum sulfate dosage is between 60% and 70%, and ultrafine sepiolite powder and polyacrylamide are used to enhance the stability of the supersaturated system. However, the system uses 1% to 4% fluoride salts, and the presence of fluoride ions is detrimental to the early strength of the product, typically failing to reach 10 MPa. Inappropriate amounts of polyacrylamide can easily lead to crosslinking and flocculation, which can negatively impact the stability of the system. The preferred ultrafine sepiolite powder has an average particle size of less than 10 μm, which significantly improves system stability. However, due to its lack of modification, the overall viscosity of the system is as high as 2000 to 4000 mPa·s, making it unsuitable for practical applications.

[0005] Another example is a modified sepiolite stabilizer for liquid accelerators and its preparation method. This involves a method for modifying sepiolite, specifically using cetyltrimethylammonium bromide and sodium silicate. However, the sepiolite stabilizer prepared by this method suffers from the gradual release of surfactants during the preparation of the accelerator. This release generates a large number of bubbles in the system, and the saturated salt system of the accelerator is easily disturbed, resulting in poor system stability.

[0006] Another example is a technology for an alkali-free accelerator-specific anti-settling agent, its preparation method, and application. The technology describes modifying sepiolite with γ-methacryloxypropyltrimethoxysilane. This method uses silane to modify sepiolite and then mixes it with a polymer obtained through free radical polymerization to create a dedicated anti-settling agent. The mechanism is that the entanglement of polymer chains and the three-dimensional network structure of the sepiolite work together synergistically. However, this technology has issues. Because the silane forms a hydrophobic layer on the sepiolite surface after affinity, the sepiolite tends to agglomerate in water and is difficult to disperse, resulting in poor dispersion. Furthermore, because the polymer in this solution is copolymerized in the presence of sepiolite, its presence may affect the molecular weight of the finished product, resulting in a lower molecular weight, a weakened entanglement effect, and a poor anti-settling effect. In addition to the aforementioned preparation and application drawbacks, the three-dimensional crosslinking of the polymer obtained by in-situ polymerization increases the overall viscosity of the system, resulting in a weakened thixotropy, which is detrimental to pumping during application.

[0007] Summary of the Invention

[0008] In response to the technical problems existing in the modifiers of pillaring materials in the prior art, the present invention uses two hyperbranched quaternary ammonium salts to modify the pillaring material to obtain a composite modified pillaring material. The composite modified pillaring material has a larger pillaring material capacity (CEC) and is more effective in improving the long-term stability when used as a stabilizer in an accelerator system.

[0009] The present invention specifically adopts the following technical solutions:

[0010] A composite modified pillaring material comprises an orthorhombic pillaring material modified by a quaternary ammonium salt corresponding to a hyperbranched polyamine as shown in the following formula I or a hyperbranched quaternary ammonium salt as shown in formula II.

[0011] In the above formula I, R is selected from the structure (a) or (b) shown in formula III, and the value of n ranges from 3 to 10; in the above formula II, the value of m ranges from 3 to 9.

[0012] It should be noted that the selection of the substituent R in the above formula I does not solely select structure (a) or structure (b), but rather, during the preparation and synthesis, structure (a) or structure (b) can be freely connected at the same time.

[0013] The hyperbranched polyamine represented by the above formula I and its corresponding quaternary ammonium salt and the hyperbranched quaternary ammonium salt represented by formula II can be prepared according to the methods reported in the literature. The preparation methods of the two are not described here one by one. For example, the hyperbranched structure represented by formula I can be prepared by the method described in the document "Preparation and Properties of Amino-Terminated Hyperbranched Polymers and Quaternary Ammonium Salts thereof", and the hyperbranched polyamine in formula I is further prepared according to the method therein to obtain the corresponding hyperbranched quaternary ammonium salt; and the hyperbranched quaternary ammonium salt represented by formula II can be prepared by the method described in the document "Synthesis, Properties and Applications of Hyperbranched Gemini Quaternary Ammonium Salts".

[0014] The orthorhombic pillaring material may be sepiolite or hydrotalcite.

[0015] The preparation method of the composite modified pillaring material comprises the following steps:

[0016] The hyperbranched quaternary ammonium salt and the orthorhombic pillaring material are mixed and modified in a mass ratio of 5 to 10:100 to obtain a composite modified pillaring material.

[0017] Specifically, the modification method can be any one of conventional pillared material modification methods such as direct intercalation method, solution blending macromolecular insertion method, melt macromolecular insertion method, etc.

[0018] The composite modified pillaring material provided by the present invention uses the hyperbranched quaternary ammonium salt with a specific structure as a modified material. Since it contains a branched structure, it is different from ordinary modified materials with a long-chain structure, ensuring that the interlayer spacing after intercalation of the orthorhombic pillaring material is larger and the CEC capacity is higher.

[0019] Compared with the modification effect of other conventional modified materials in the prior art (through Na + The comparison of the two methods is shown in Table 1 below.

[0020] Table 1 CEC values ​​of different orthorhombic pillared materials before and after modification by different modified materials

[0021] In the above-mentioned composite modified pillaring material, the hyperbranched quaternary ammonium salt structure has strong acid resistance, alkali resistance, and salt resistance, and the CEC of the modified pillaring material is significantly improved, making it suitable for high-concentration fluorine-free and alkali-free quick-setting agents as stabilizers therein. The CEC improvement of sepiolite and hydrotalcite after modification by the above-mentioned hyperbranched quaternary ammonium salt intercalation is significantly greater than that of montmorillonite, which shows that the hyperbranched quaternary ammonium salt is not suitable for every conventional orthorhombic pillaring material. To this end, the present invention also provides a fluorine-free and alkali-free quick-setting agent and a preparation method thereof. Compared with traditional alkali-free quick-setting agents, the fluorine-free and alkali-free quick-setting agent increases the amount of aluminum sulfate by more than 10%, thereby significantly improving the supersaturation of the quick-setting agent solution system.

[0022] A fluorine-free and alkali-free quick-setting agent, comprising the following components (in percentage by mass) mixed uniformly:

[0023] The balance is water;

[0024] Wherein, the stabilizer is the above-mentioned composite modified pillaring material.

[0025] Generally, the maximum solubility of aluminum sulfate, the core component of alkali-free accelerator, is 36 g / L (20°C) at room temperature, which is far from meeting the performance requirements of practical applications. The aluminum sulfate dosage in the common alkali-free accelerators on the market can reach between 40% and 50%, but it is difficult to further increase it, and the final solid content of the finished product is around 50%. Further increasing the solid content will lead to a significant decrease in the stability of the system, including multiple problems such as easy stratification of the system, excessive viscosity, and easy crystallization. The specific hyperbranched quaternary ammonium salt-modified pillaring material described in the present invention is particularly suitable for fluorine-free and alkali-free accelerators with an aluminum sulfate concentration of more than 60%. The advantages include that more complexing sites can be provided by modifying the polybasic quaternary ammonium salt, so that the high CEC of the composite modified pillaring material can provide space for intercalation exchange for a large amount of supersaturated (beyond conventional solubility) aluminum sulfate, reducing the probability of crystallization, and utilizing the characteristics of the pillaring material itself, that is, building a three-dimensional network structure to improve the stability of the entire system. Therefore, the effect of preparing a high-concentration fluorine-free and alkali-free accelerator product is achieved, and the finished product has good long-term stability and viscosity that meets construction requirements.

[0026] Furthermore, the complexing agent A is selected from diethanolamine and / or triethanolamine, and the complexing agent B is selected from at least one of EDTA, phosphoric acid, oxalic acid and urea.

[0027] Furthermore, the ion inhibitor is selected from at least one of glycerol, sodium hexametaphosphate, sodium dodecylbenzenesulfonate, sodium dodecylsulfonate, sodium lauryl sulfate, and hexadecyltrimethylammonium bromide.

[0028] The preparation method of the above-mentioned fluorine-free and alkali-free quick-setting agent specifically comprises the following steps:

[0029] The above components are mixed according to the predetermined mass ratio and dissolved uniformly.

[0030] The fluorine-free and alkali-free quick-setting agent provided by the present invention uses aluminum sulfate as the main aluminum phase component, utilizes the synergistic effect of components such as complexing, stabilization and viscosity reduction, and uses the composite modified pillaring material of the present invention as a stabilizer to ensure that the solid content of the fluorine-free and alkali-free quick-setting agent is increased by more than 10% compared with the traditional alkali-free quick-setting agent, and the supersaturation of the quick-setting agent solution system is significantly improved, thereby bringing about performance improvement. In addition, alkali metal ions and fluoride salts are not used in the fluorine-free and alkali-free quick-setting agent, which avoids the influence of fluoride ions on the early strength and the influence of alkali-aggregate reaction on the later strength in the concrete used, especially for early-strength shotcrete. It has significant value. The orthorhombic pillaring stabilizer independently synthesized by the present invention utilizes charge and thixotropy to improve the supersaturation of the fluorine-free and alkali-free quick-setting agent system on the basis of ensuring product stability, thereby ensuring its excellent effect in concrete materials. DETAILED DESCRIPTION

[0031] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. Instead, these embodiments are provided to explain the principles of the present invention and its practical application, thereby enabling other persons skilled in the art to understand the various embodiments of the present invention and various modifications suitable for specific intended applications.

[0032] Example 1

[0033] This embodiment provides a composite modified pillaring material and a preparation method thereof.

[0034] Specifically, 5 parts of the hyperbranched quaternary ammonium salt corresponding to the hyperbranched polyamine (n=3) represented by the above formula I and 100 parts of sepiolite powder are mixed by solution blending and macromolecular insertion method to prepare a composite modified pillared material.

[0035] Example 2

[0036] This embodiment provides a composite modified pillaring material and a preparation method thereof.

[0037] Specifically, 10 parts of the hyperbranched quaternary ammonium salt (m=3) represented by the above formula II and 100 parts of sepiolite powder are mixed by solution blending and macromolecular insertion method to prepare a composite modified pillared material.

[0038] Example 3

[0039] This embodiment provides a composite modified pillaring material and a preparation method thereof.

[0040] Specifically, 8 parts of the hyperbranched quaternary ammonium salt (m=9) represented by the above formula II and 100 parts of hydrotalcite powder are mixed by the melt macromolecular insertion method to prepare a composite modified pillared material.

[0041] Example 4

[0042] This embodiment provides a composite modified pillaring material and a preparation method thereof.

[0043] Specifically, 9 parts of the hyperbranched quaternary ammonium salt corresponding to the hyperbranched polyamine (n=10) represented by the above formula I and 100 parts of sepiolite powder are subjected to a melt macromolecular insertion method to prepare a composite modified pillared material.

[0044] Example 5

[0045] Based on the composite modified pillaring material provided in Example 1, this example uses it as a stabilizer to provide a fluorine-free and alkali-free quick-setting agent and a preparation method thereof.

[0046] Specifically, the fluorine-free and alkali-free quick-setting agent is prepared by heating, dissolving and cooling the mixture according to the mass ratio of 62% aluminum sulfate 18hydrate, 7% diethanolamine, 0.5% phosphoric acid, 0.8% stabilizer and the rest water.

[0047] That is, the fluorine-free and alkali-free quick-setting agent provided in this embodiment includes the following components mixed evenly:

[0048] The balance is water.

[0049] Example 6

[0050] Based on the composite modified pillaring material provided in Example 2, this example uses it as a stabilizer to provide a fluorine-free and alkali-free quick-setting agent and a preparation method thereof.

[0051] Specifically, the fluorine-free and alkali-free quick-setting agent is prepared by heating, dissolving and cooling according to the mass ratio of 66% of aluminum sulfate 18hydrate, 9% of diethanolamine, 0.5% of phosphoric acid, 1% of EDTA, 0.5% of oxalic acid, 0.5% of urea, 0.3% of glycerol, 0.6% of stabilizer, and the rest of water.

[0052] That is, the fluorine-free and alkali-free quick-setting agent provided in this embodiment includes the following components mixed evenly:

[0053] The balance is water.

[0054] Example 7

[0055] Based on the composite modified pillaring material provided in Example 3, this example uses it as a stabilizer to provide a fluorine-free and alkali-free quick-setting agent and a preparation method thereof.

[0056] Specifically, the fluorine-free and alkali-free quick-setting agent is prepared by heating, dissolving and cooling according to the mass ratio of 60% of aluminum sulfate 18hydrate, 4% of diethanolamine, 1.5% of triethanolamine, 0.5% of phosphoric acid, 0.2% of glycerol, 0.1% of sodium hexametaphosphate, 0.7% of stabilizer and the rest of water.

[0057] That is, the fluorine-free and alkali-free quick-setting agent provided in this embodiment includes the following components mixed evenly:

[0058] The balance is water.

[0059] Example 8

[0060] Based on the composite modified pillaring material provided in Example 3, this example uses it as a stabilizer to provide a fluorine-free and alkali-free quick-setting agent and a preparation method thereof.

[0061] Specifically, according to the mass proportions of 62% aluminum sulfate 18hydrate, 4.5% diethanolamine, 0.5% phosphoric acid, 0.5% EDTA, 0.2% glycerol, 0.2% cetyltrimethylammonium bromide, 0.2% sodium lauryl sulfate, 0.7% stabilizer and the rest water, the fluorine-free and alkali-free quick-setting agent is prepared after heating, dissolving and cooling.

[0062] That is, the fluorine-free and alkali-free quick-setting agent provided in this embodiment includes the following components mixed evenly:

[0063] The balance is water.

[0064] Example 9

[0065] Based on the composite modified pillaring material provided in Example 1, this example uses it as a stabilizer to provide a fluorine-free and alkali-free quick-setting agent and a preparation method thereof.

[0066] Specifically, the fluorine-free and alkali-free quick-setting agent is prepared by heating, dissolving and cooling the mixture according to the mass ratio of 61% aluminum sulfate 18hydrate, 6% diethanolamine, 0.3% phosphoric acid, 0.3% glycerol, 0.3% sodium dodecylbenzenesulfonate, 1% stabilizer and the rest water.

[0067] That is, the fluorine-free and alkali-free quick-setting agent provided in this embodiment includes the following components mixed evenly:

[0068] The balance is water.

[0069] In order to verify the effects of the fluorine-free and alkali-free quick-setting agents provided in the above embodiments, especially the stabilizing effect of the stabilizer therein, the following comparative experiments were conducted.

[0070] Comparative Example 1

[0071] This comparative example is designed to illustrate the effect of the stabilizer on the performance of the fluorine-free and alkali-free quick-setting admixture by forming a comparison with Example 5 in which the stabilizer is absent.

[0072] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0073] The balance is water.

[0074] Due to the lack of modified pillaring materials to provide stability for the supersaturated quick-setting agent, the comparative fluorine-free and alkali-free quick-setting agent quickly solidified and precipitated after being cooled and placed, and lost its fluidity as a whole and could not be used.

[0075] Comparative Example 2

[0076] This comparative example is designed to illustrate the effect of the amount of aluminum sulfate on the performance of the fluorine-free and alkali-free quick-setting admixture by forming a comparison with Example 5 in which an excess of aluminum sulfate is used.

[0077] This comparative example provides a comparative fluorine-free and alkali-free quick-setting agent, which differs from Example 5 only in that the amount of aluminum sulfate 18hydrate is adjusted to 67% and the amount of water is reduced accordingly; the rest is the same as that described in Example 5.

[0078] Although the supersaturation is increased to form a high-concentration system under the synergistic effect of the complexing agent, ion inhibitor and stabilizer, when the amount of aluminum sulfate exceeds the critical point, the excess aluminum sulfate will act as crystal nuclei to reduce the stability of the system. Therefore, the comparative fluorine-free and alkali-free quick-setting agent in this comparative example quickly condenses and precipitates after being cooled and placed, loses fluidity as a whole, and cannot be used.

[0079] Comparative Example 3

[0080] The purpose of setting this comparative example is to form a comparison without complexing agent A, so as to illustrate the effect of complexing agent A on the performance of fluorine-free and alkali-free quick-setting agent.

[0081] This comparative example provides a comparative fluorine-free and alkali-free quick-setting agent, in which the composite modified pillaring material provided in Example 2 above is used as a stabilizer.

[0082] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0083] The balance is water.

[0084] Due to the lack of complexing agent A, the aluminum sulfate that exceeds the solubility in water during the synthesis of the accelerator cannot be completely dissolved, the supersaturated stable system product cannot be effectively constructed, and the finished product preparation fails.

[0085] Comparative Example 4

[0086] This comparative example is designed to form a comparison without complexing agent B, so as to illustrate the effect of complexing agent B on the performance of fluorine-free and alkali-free quick-setting agent.

[0087] This comparative example provides a comparative fluorine-free and alkali-free quick-setting agent, in which the composite modified pillaring material provided in Example 2 above is used as a stabilizer.

[0088] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0089] The balance is water.

[0090] The fluorine-free and alkali-free quick-setting agent lacks the complexing agent B, so the viscosity of the supersaturated finished solution system is too high and is greatly affected by temperature. After cooling, it is easy to precipitate and solidify and lose fluidity, making the finished product unusable.

[0091] Comparative Example 5

[0092] This comparative example provides a comparative fluorine-free and alkali-free quick-setting agent, in which the composite modified pillaring material provided in Example 1 above is used as a stabilizer.

[0093] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0094] The balance is water.

[0095] The comparative fluorine-free and alkali-free accelerator does not contain an ion inhibitor, which reduces the stability of the system and easily leads to the precipitation of some components, resulting in excessively high viscosity of the system.

[0096] Comparative Example 6

[0097] This comparative example is designed to provide a comparison of the excessive amount of complexing agent B, in order to illustrate the effect of the amount of complexing agent B on the performance of the fluorine-free and alkali-free quick-setting agent.

[0098] This comparative example provides a comparative fluorine-free and alkali-free quick-setting agent, in which the composite modified pillaring material provided in Example 1 above is used as a stabilizer.

[0099] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0100] The balance is water.

[0101] The dosage of the fluorine-free and alkali-free accelerator complexing agent B exceeds the recommended range. Although the stability is improved, the viscosity is too high, making it unusable, and the negative effects are obvious, affecting the strength of the concrete.

[0102] Comparative Example 7

[0103] This comparative example is designed to form a comparison of a hyperbranched quaternary ammonium salt having a higher degree of branching as shown in Formula II, so as to illustrate the effect of the degree of branching of the hyperbranched quaternary ammonium salt on the performance of the fluorine-free and alkali-free accelerating setting agent.

[0104] This comparative example provides a comparative composite modified pillared material and a preparation method thereof.

[0105] Specifically, 10 parts of the hyperbranched quaternary ammonium salt (m=10) represented by the above formula II and 100 parts of sepiolite powder were mixed by solution blending and macromolecular insertion method to prepare a comparative composite modified pillared material.

[0106] The comparative composite modified pillared material prepared above was used to prepare a comparative fluorine-free and alkali-free quick-setting agent as a comparative stabilizer therein.

[0107] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0108] The balance is water.

[0109] The comparative fluorine-free and alkali-free accelerator has poor stability due to the high degree of branching of the hyperbranched quaternary ammonium salt, insufficient water solubility, and poor intercalation effect. As a result, the comparative fluorine-free and alkali-free accelerator has obvious stratification after being placed for 1 day, and the viscosity is too high, making it unusable.

[0110] Comparative Example 8

[0111] This comparative example is designed to provide a comparison with a hyperbranched quaternary ammonium salt having a lower degree of branching, as shown in Formula II, in order to illustrate the effect of the degree of branching of the hyperbranched quaternary ammonium salt on the performance of the fluorine-free and alkali-free accelerating setting agent.

[0112] This comparative example provides a comparative composite modified pillared material and a preparation method thereof.

[0113] Specifically, 10 parts of the hyperbranched quaternary ammonium salt (m=2) represented by the above formula II and 100 parts of sepiolite powder were mixed by solution blending and macromolecular insertion method to prepare a comparative composite modified pillared material.

[0114] The comparative composite modified pillared material prepared above was used to prepare a comparative fluorine-free and alkali-free quick-setting agent as a comparative stabilizer therein.

[0115] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0116] The balance is water.

[0117] The comparative fluorine-free and alkali-free quick-setting agent has a relatively low degree of branching of the hyperbranched quaternary ammonium salt, resulting in slightly poor overall stability. As a result, the comparative fluorine-free and alkali-free quick-setting agent exhibits obvious stratification after one day of storage and has a high viscosity, making it unusable.

[0118] Comparative Example 9

[0119] This comparative example is designed to form a comparison of a hyperbranched quaternary ammonium salt having a higher degree of branching as shown in Formula I, so as to illustrate the effect of the degree of branching of the hyperbranched quaternary ammonium salt on the performance of the fluorine-free and alkali-free accelerating setting agent.

[0120] This comparative example provides a comparative composite modified pillared material and a preparation method thereof.

[0121] Specifically, 8 parts of the hyperbranched quaternary ammonium salt (n=11) represented by the above formula I and 100 parts of sepiolite powder were mixed by solution blending and macromolecular insertion method to prepare a comparative composite modified pillared material.

[0122] The comparative composite modified pillared material prepared above was used to prepare a comparative fluorine-free and alkali-free quick-setting agent as a comparative stabilizer therein.

[0123] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0124] The balance is water.

[0125] The comparative fluorine-free and alkali-free accelerator has a high degree of branching of the hyperbranched quaternary ammonium salt, which makes the molecules too large to achieve good intercalation and has slightly poor overall stability. As a result, the comparative fluorine-free and alkali-free accelerator exhibits obvious stratification after one day of storage and has a too high viscosity, making it unusable.

[0126] Comparative Example 10

[0127] This comparative example is designed to provide a comparison with a hyperbranched quaternary ammonium salt having a lower degree of branching, as shown in Formula I, in order to illustrate the effect of the degree of branching of the hyperbranched quaternary ammonium salt on the performance of the fluorine-free and alkali-free accelerating setting agent.

[0128] This comparative example provides a comparative composite modified pillared material and a preparation method thereof.

[0129] Specifically, 8 parts of quaternary ammonium salt (n=2) prepared from the hyperbranched polyamine represented by the above formula I and 100 parts of sepiolite powder were mixed by solution blending and macromolecular insertion method to prepare a comparative composite modified pillared material.

[0130] The comparative composite modified pillared material prepared above was used to prepare a comparative fluorine-free and alkali-free quick-setting agent as a comparative stabilizer therein.

[0131] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0132] The balance is water.

[0133] The comparative fluorine-free and alkali-free accelerator has a low degree of branching of the hyperbranched quaternary ammonium salt, and the intercalation effect is close to that of conventional ordinary surfactant intercalation, and has no significant advantages. Therefore, the overall stability performance is slightly poor. As a result, the comparative fluorine-free and alkali-free accelerator has obvious stratification after 1 day of storage, and the viscosity is too high, making it unusable.

[0134] Comparative Example 11

[0135] The purpose of this comparative example is to change the orthorhombic pillaring material in the composite modified pillaring material to reflect the influence of the type of the orthorhombic pillaring material on the performance of the fluorine-free and alkali-free quick-setting agent.

[0136] This comparative example provides a comparative composite modified pillared material and a preparation method thereof.

[0137] Specifically, 8 parts of the quaternary ammonium salt corresponding to the hyperbranched polyamine (n=3) represented by the above formula I and 100 parts of kaolin powder were mixed by solution blending and macromolecular insertion method to prepare a comparative composite modified pillared material.

[0138] The comparative modified pillaring material prepared above was used to prepare a comparative fluorine-free and alkali-free quick-setting agent as a comparative stabilizer therein.

[0139] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0140] The balance is water.

[0141] Since kaolin itself is a triclinic material, interlayer modification cannot be carried out under the action of strong hydrogen bonds, so it is not very effective as a pillaring material. When the comparative composite modified pillaring material prepared above is used in the comparative fluorine-free and alkali-free quick-setting agent, it delaminates significantly after 1 day and has a high viscosity, making it impossible to realize engineering application.

[0142] Comparative Example 12

[0143] The purpose of this comparative example is to change the intercalation material of the orthorhombic pillaring material in the composite modified pillaring material to reflect the influence of the type of the intercalation material on the performance of the fluorine-free and alkali-free quick-setting agent.

[0144] This comparative example provides a comparative composite modified pillared material and a preparation method thereof.

[0145] Specifically, 5 parts of sodium dodecylbenzene sulfonate (SDBS) and 100 parts of sepiolite powder were mixed by solution blending and macromolecular insertion method to prepare a comparative composite modified pillared material.

[0146] The comparative composite modified pillared material prepared above was used to prepare a comparative fluorine-free and alkali-free quick-setting agent as a comparative stabilizer therein.

[0147] The comparative fluorine-free and alkali-free quick-setting agent provided in this comparative example includes the following components mixed evenly:

[0148] The balance is water.

[0149] The overall stability of the fluorine-free and alkali-free quick-setting agent is slightly worse. After one day of storage, stratification is obvious and the viscosity is too high, making it unusable.

[0150] Comparative Example 13

[0151] This comparative example provides a commercially available mature fluorine-containing alkali-free quick-setting agent as a comparison, and its specific model is Subotec SBT-N (II).

[0152] In order to verify the application effects of the above-mentioned accelerators, the fluorine-free and alkali-free accelerators provided in Examples 5 to 9, the comparative fluorine-free and alkali-free accelerators provided in Comparative Examples 2 to 11, and the fluorine-free and alkali-free accelerators prepared from the conventional modified materials provided in Comparative Example 12 were tested with the fluorine-containing alkali-free accelerator on the market in Comparative Example 13.

[0153] The various shotcrete mixes used in the application test are shown in Table 2 below; the corresponding dosage (the dosage after converting the dosage of cementitious materials), as well as the rebound rate and 8h drill core strength in the project site shotcrete test are shown in Table 3 below.

[0154] Table 2 Application test of each accelerator sprayed concrete mix ratio

[0155] Table 3 Corresponding dosage, rebound rate and 8h drill core strength of each accelerator in the application test

[0156] As can be seen from Table 3, in Comparative Example 2, due to the higher amount of aluminum sulfate, the stability cannot be guaranteed, and a rebound rate of up to 15% to 25% is obtained when the actual dosage is 4% to 6% under the actual working pump pressure; in Comparative Example 3, due to the high amount of stabilizer, the viscosity is too high, which results in the spraying machine obtaining a rebound rate of up to 20% to 25% when the actual dosage is only 4% to 5% under full load, and the actual dosage cannot be guaranteed; in Comparative Example 4, on the one hand, the viscosity of the stabilizer is too high, resulting in the spraying machine obtaining a rebound rate of up to 20% to 25% when the actual dosage is only 4% to 5% under full load, and on the other hand, the long-term stability is reduced due to the low dosage of the stabilizer; and the 8h drill core strength in each embodiment is significantly higher than that in the comparative example, indicating that the fluorine-free and alkali-free quick-setting agent based on the above-mentioned composite modified pillaring material has a positive effect on the strength growth of early shotcrete.

[0157] Generally speaking, the rebound rate of shotcrete should be controlled within 15%, below 10% is considered excellent, and close to 5% is considered very excellent. It can be seen from this that the above-mentioned fluorine-free and alkali-free accelerators of the present invention have very excellent application effects.

[0158] At the same time, the performance and stability of the accelerating setting agents provided in the above embodiments and comparative examples were tested. The specific testing method is: using benchmark cement to test the setting time and mortar strength, the accelerating setting agent dosage is 8%.

[0159] The test results are shown in Table 4 below.

[0160] Table 4 Performance and stability of each accelerator

[0161] Note: Mortar testing is carried out in accordance with QCR-807-2020

[0162] The data in Table 4 demonstrates that the Examples achieve early high strength through the synergistic effect of the high-alumina phase and other complexing additives. Furthermore, under high-solids conditions, they exhibit a relatively reasonable viscosity, generally approaching or below 500 cp, and very good stability (28-day water separation rate <5%). Viscosities exceeding 600 cp can adversely affect actual spraying, leading to insufficient dosage, uneven dispersion, and even pipe blockage. Furthermore, the Example products exhibited 6-hour mortar strengths >1 MPa and 1-day strengths >8 MPa in mortar tests against benchmark cement, demonstrating consistent early high strength.

[0163] Comparative Examples 1 to 6 are comparative fluorine-free and alkali-free quick-setting agents prepared using the composite modified pillaring materials of Examples 1 to 4. The necessity of the components in the above-mentioned mix ratio, the effect of the complexing agent A on the system stabilizer and the amount of aluminum sulfate used are equally important; other components such as the complexing agent B, ion suppression materials, etc. will also have a significant impact on the viscosity and stability of the system.

[0164] Comparative Examples 7 to 12 show the effects of different modifying materials and different pillaring materials on system performance under the same mix ratio conditions. It can be seen that although the mix ratios are the same, the viscosities and water extraction rates are not the same. Kaolin will bring the greatest viscosity improvement because of its high viscosity and therefore relatively low water extraction rate; SDBS modification has a certain effect in preparing pillaring materials, but the viscosity and stability are weaker than those in the examples; and the unsuitable I and II structures used for modification are also weaker than the benchmark products.

[0165] Comparative Example 13 is a comparison of commercially available fluorine-containing products, which has a lower solid content, low viscosity, good stability, and fast coagulation, but its early strength is significantly weaker than that of fluorine-free and alkali-free products.

Claims

1. A composite modified pillaring material, characterized in that: It comprises an orthorhombic pillaring material modified by a quaternary ammonium salt corresponding to a hyperbranched polyamine as shown in the following formula I or a hyperbranched quaternary ammonium salt as shown in the following formula II, In the above formula I, R is selected from the structure (a) or (b) shown in formula III, and n is The value range is 3 to 10; in the above formula II, the value range of m is 3 to 9; Wherein, the orthorhombic pillaring material is sepiolite or hydrotalcite.

2. The method for preparing the composite modified pillaring material according to claim 1, characterized in that: Includes steps: The quaternary ammonium salt corresponding to the hyperbranched polyamine shown in the following formula I or the hyperbranched quaternary ammonium salt shown in the following formula II is mixed and modified with the orthorhombic pillaring material in a mass ratio of 5 to 10:100 to obtain the composite modified pillaring material; In the above formula I, R is selected from the structure (a) or (b) shown in formula III, and n is in the range of 3 to 10; in the above formula II, m is in the range of 3 to 9; The orthorhombic pillaring material is sepiolite or hydrotalcite.

3. The method according to claim 2, characterized in that: The modification method is selected from any one of a direct intercalation method, a solution blending macromolecular insertion method, and a melt macromolecular insertion method.

4. A fluorine-free and alkali-free quick-setting agent, characterized in that: It comprises the following components mixed uniformly: Wherein, the stabilizer is the composite modified pillaring material described in claim 1.

5. The fluorine-free and alkali-free quick-setting agent according to claim 4, characterized in that: The complexing agent A is selected from diethanolamine and / or triethanolamine.

6. The fluorine-free and alkali-free quick-setting agent according to claim 4, characterized in that: The complexing agent B is selected from at least one of EDTA, phosphoric acid, oxalic acid and urea.

7. The fluorine-free and alkali-free quick-setting agent according to claim 4, characterized in that: The ion inhibitor is selected from at least one of glycerol, sodium hexametaphosphate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfonate, sodium dodecyl sulfate, and hexadecyltrimethylammonium bromide.

8. The method for preparing the fluorine-free and alkali-free quick-setting agent according to any one of claims 4 to 7, characterized in that: Includes steps: 60% to 66% aluminum sulfate, 4.5% to 9% complexing agent A, 0.3% to 3% complexing agent B, 0.2% to 0.6% ion inhibitor, and 0.6% to 1% stabilizer are uniformly dissolved in the remaining amount of water to obtain the fluorine-free and alkali-free accelerator; the total amount of the fluorine-free and alkali-free accelerator is 100%; Wherein, the stabilizer is the composite modified pillaring material described in claim 1.

Citation Information

Patent Citations

  • Hyperbranched quaternary ammonium salt modified organo montmorillonite and preparation method thereof

    CN101717090A

  • Aluminum sulfate supersaturated suspended alkali-free liquid accelerator and preparation method thereof

    CN110922085A

  • Suspended alkali-free liquid accelerator and preparation method thereof

    CN112745056A

  • Preparation method and application of alkali-free fluoride-free liquid accelerator

    CN115466075A

  • Concrete spraying additives

    EP0812812A1