Elastic sheet for all solid-state battery and all solid-state battery comprising same
The introduction of an elastic sheet with an acrylic binder, hollow particles, and a glass filler in all-solid-state batteries addresses the issue of compressive strength and stress on the solid electrolyte, improving the battery's lifespan and efficiency by maintaining optimal contact and buffering volume changes during charging and discharging.
Patent Information
- Application Number
- PCT/KR2024/000430
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-01-09
- Publication Date
- 2024-11-28
AI Technical Summary
All-solid-state batteries face challenges in maintaining low compressive strength during charging and discharging, which can lead to stress on the solid electrolyte, potentially causing damage and reducing the battery's lifespan.
An elastic sheet comprising an acrylic binder, hollow particles, and a glass filler is introduced, which satisfies the compression force deflection ratio of 2≤CFD70/CFD50≤4, ensuring sufficient contact between the electrode and solid electrolyte while buffering volume changes during charging and discharging.
The elastic sheet effectively reduces stress on the solid electrolyte, improves contact between components, and enhances the battery's lifespan and discharge efficiency by maintaining appropriate internal pressure and preventing damage.
Smart Images

Figure KR2024000430_28112024_PF_FP_ABST
Abstract
Description
Elastic sheet for all-solid-state battery and all-solid-state battery comprising the same
[0001] The present invention relates to an elastic sheet for an all-solid-state battery and an all-solid-state battery including the same.
[0002] Recently, rapid developments have been made in electronic devices that use batteries, such as cell phones, laptop computers, and electric vehicles.
[0003] Development of all-solid-state batteries using lithium metal as the cathode is underway. All-solid-state batteries are composed entirely of solid materials, specifically those using solid electrolytes. Because the electrolyte is solid, all-solid-state batteries are structurally robust, reducing the risk of fire or explosion due to leakage from external impacts. Furthermore, they can be shaped into a variety of battery shapes.
[0004] One embodiment provides an elastic sheet for an all-solid-state battery that can maintain a low compressive strength during compression by charge and discharge, reduce stress applied to a solid electrolyte, and improve life characteristics.
[0005] Another embodiment provides an all-solid-state battery comprising the elastic sheet.
[0006] One embodiment provides an elastic sheet for an all-solid-state battery, comprising an acrylic binder, hollow particles and a glass filler, and satisfying the following equation 1.
[0007] [Formula 1]
[0008] 2≤CFD70 / CFD50≤4
[0009] (In the above equation 1, CFD (compression force deflection) 50 is the compressive strength (MPa) measured at the point where the thickness becomes 50% of the thickness of the elastic sheet,
[0010] CFD70 is the compressive strength (MPa) measured at a point where the thickness is 30% of the thickness of the elastic sheet.
[0011] Another embodiment provides an all-solid-state battery comprising: a positive electrode; a negative electrode; a solid electrolyte layer positioned between the positive electrode and the negative electrode; and an elastic sheet positioned on the outside of at least one of the positive electrode and the negative electrode.
[0012] An elastic sheet for an all-solid-state battery according to an embodiment can maintain a low compressive strength during compression by charge and discharge, and can reduce the stress applied to a solid electrolyte, thereby exhibiting life characteristics.
[0013] Figure 1 is a schematic diagram schematically showing an all-solid-state battery according to one embodiment.
[0014] Figure 2 is a schematic cross-sectional view schematically showing an all-solid-state battery according to another embodiment.
[0015] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention. The present invention is defined solely by the scope of the claims set forth below.
[0016] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.
[0017] “Combination of these” means a mixture, laminate, composite, copolymer, alloy, blend, reaction product, etc. of the components.
[0018] It should be understood that terms such as "include," "comprise," or "have" are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0019] Throughout this specification, when it is said that a part "includes" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0020] In addition, the terms "about", "substantially", etc. used throughout this specification are used in the sense of numerical values or near numerical values when manufacturing and material tolerances inherent to the meanings stated are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that mention exact or absolute values to aid understanding of this specification.
[0021] Throughout this specification, the description of “A and / or B” means “A or B or both.”
[0022] Unless otherwise specified herein, when a part such as a layer, film, region, plate, etc. is said to be “on” another part, this includes not only cases where it is “directly on” the other part, but also cases where there is another part in between.
[0023] In the present invention, "particle size" or "particle diameter" may be an average particle diameter. In addition, the average particle diameter may be defined as the average particle diameter (D50) based on 50% of the cumulative volume in a particle diameter distribution curve. The particle diameter may be measured by a method widely known to those skilled in the art, for example, by measuring with a particle size analyzer, or by measuring with a transmission electron microscope, a scanning electron microscope, or a field emission scanning electron microscope (FE-SEM). Alternatively, the average particle diameter (D50) may be obtained by measuring with a measuring device that utilizes dynamic light-scattering, performing data analysis to count the number of particles for each particle size range, and calculating from this. Alternatively, the average particle diameter (D50) may be measured using a laser diffraction method. When measuring by laser diffraction, more specifically, after the particles to be measured are dispersed in a dispersion medium, they are introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000) and irradiated with ultrasonic waves of approximately 28 kHz at an output of 60 W, and the average particle diameter (D50) based on 50% of the particle diameter distribution in the measuring device can be calculated.
[0024] "Thickness" may be measured, for example, from photographs taken with an optical microscope such as a scanning electron microscope.
[0025] One embodiment relates to an elastic sheet for an all-solid-state battery. This elastic sheet may be expressed as a buffer layer or an elastic layer. This elastic sheet ensures that pressure is uniformly transmitted to a negative electrode, a solid electrolyte, and an electrode laminate of the negative electrode, thereby improving contact between the solid components and also alleviating stress transmitted to the solid electrolyte, etc. In addition, the elastic sheet serves to cushion changes in the thickness of the electrode during charging and discharging.
[0026] An elastic sheet for an all-solid-state battery according to an embodiment includes an acrylic binder, hollow particles and a glass filler, and satisfies the following equation 1.
[0027] [Formula 1]
[0028] 2≤CFD70 / CFD50≤4
[0029] In the above equation 1, CFD (compression force deflection) 50 is the compressive strength (MPa) measured at a point where the thickness is 50% of the thickness of the elastic sheet,
[0030] CFD70 is the compressive strength (MPa) measured at a point where the thickness is 30% of the thickness of the elastic sheet.
[0031] Thus, CFD50 refers to the compressive strength when the elastic sheet thickness is compressed to 50% of the initial thickness, and this takes into account the maximum compression state that can occur during the all-solid-state manufacturing process. For example, CFD50 refers to the compressive strength value of the elastic sheet when the all-solid-state battery is manufactured. In addition, CFD70 takes into account the maximum compression state that can occur when the all-solid-state battery is operated, i.e., when charging and discharging are performed. For example, CFD70 refers to the compressive strength value when the all-solid-state battery is charged.
[0032] When the elastic sheet satisfies the above equation 1, the electrode and the solid electrolyte can be sufficiently closely adhered, thereby facilitating lithium movement. In addition, even if the volume of the electrode expands during charge and discharge, the elastic sheet can effectively absorb, or buffer, this volume change, thereby mitigating the impact applied to the electrode and the solid electrolyte, thereby preventing damage to the electrode and the solid electrolyte, for example, preventing cracks from occurring in the electrode and the solid electrolyte. In addition, the elastic sheet can help the expanded electrode shrink, or recover, to its original thickness. This can improve the life characteristics of the all-solid-state battery, and can also enhance the discharge efficiency.
[0033] If the elastic sheet has a value lower than 2 in the above formula 1, the adhesion between electrode 1 and the solid electrolyte is not sufficient, and if the elastic sheet has a value higher than 4 in the above formula 1, it cannot buffer the expansion of the electrode volume during charging and discharging, which may cause damage to the electrode and the solid electrolyte, and is therefore not suitable.
[0034] In one embodiment, the CFD50 may be measured according to the regulations of ASTM D3574 C. For example, it indicates the compressive strength when the elastic sheet is compressed to 50% of its original thickness after being laminated to 50X50X20mm, compressed to a compressive strain of 50% in the thickness-axis, and maintained for 1 minute, i.e., the compressive strength when the elastic sheet is compressed to 50% of its original thickness. Similarly, "CFD70" means the case when it is compressed to 30% of the original elastic sheet thickness.
[0035] In one embodiment, the CFD50 may be from 0.5 MPa to 4 MPa, or from 0.8 MPa to 3 MPa. Additionally, the CFD70 may be from 2 MPa to 6 MPa, or from 2.5 MPa to 5 MPa.
[0036] When the above CFD50 and the above CFD70 satisfy the above range, the internal pressure of the all-solid-state battery is maintained at an appropriate level, so that the solid electrolyte can effectively suppress damage.
[0037] When the above CFD70 and the above CFD50 are set as the y-axis and the elastic sheet thickness strain is set as the x-axis, the slope may be 4 to 30, or 5 to 25.
[0038] Below, the components of the elastic sheet are described.
[0039] Acrylic binder
[0040] In one embodiment, the acrylic binder may be a (meth)acrylic copolymer having excellent stress relaxation properties as a main component constituting the elastic sheet.
[0041] The content of the acrylic binder may be 85 wt% to 98.5 wt%, 87 wt% to 98.5 wt%, or 90 wt% to 98 wt%, based on 100 wt% of the total weight of the elastic sheet. When the content of the acrylic binder is within the above range, an elastic sheet having excellent stress relaxation properties can be suitably obtained.
[0042] The above (meth)acrylic copolymer may be a ternary copolymer including a first repeating unit derived from a linear alkyl (meth)acrylate having a glass transition temperature (Tg) of -30°C or lower, a second repeating unit derived from a cyclic alkyl (meth)acrylate having a Tg of 50°C or higher, and a third repeating unit derived from an alkyl (meth)acrylate containing a hydroxyl group.
[0043] In one embodiment, (meth)acrylic means acrylic or methacrylic. For example, 2-ethylhexyl (meth)acrylate means 2-ethylhexyl acrylate or 2-ethylhexyl methacrylate.
[0044] The linear alkyl (meth)acrylate may have a glass transition temperature (Tg) of -30°C or lower, -30°C to -70°C, or -40°C to -60°C. The linear alkyl (meth)acrylate may be 2-ethylhexyl (meth)acrylate, 2-ethylpentyl (meth)acrylate, 2-ethylheptyl (meth)acrylate, 2-ethylnonyl (meth)acrylate, 2-propylhexyl (meth)acrylate, 2-propyloctyl (meth)acrylate, or a combination thereof.
[0045] The cyclic alkyl (meth)acrylate may have a Tg of 50°C or higher, 50°C to 80°C, or 50°C to 65°C.
[0046] The above cyclic alkyl (meth)acrylate may be isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, or a combination thereof.
[0047] The alkyl (meth)acrylate containing the above hydroxyl group may be 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, or a combination thereof.
[0048] In one embodiment, the acrylic binder is a ternary copolymer including the first repeating unit, the second repeating unit, and the third repeating unit described above, and when all of these are included, it can exhibit better stress relaxation properties.
[0049] In one embodiment, the content of the first repeating unit relative to the total weight of the ternary copolymer may be 10 wt% to 40 wt%, 10 wt% to 30 wt%, or 10 wt% to 20 wt%.
[0050] Additionally, the content of the second repeating unit relative to the total weight of the ternary copolymer may be 20 wt% to 50 wt%, 25 wt% to 50 wt%, or 30 wt% to 50 wt%.
[0051] In addition, the content of the third repeating unit with respect to the total weight of the ternary copolymer may be 10 wt% to 50 wt%, 10 wt% to 40 wt%, or 10 wt% to 35 wt%.
[0052] In the above ternary copolymer, when the content of the first to third repeating units is within the above range, the flexibility of the elastic sheet can be better maintained and can be well attached to the electrode laminate.
[0053] Hollow particle
[0054] According to one embodiment, hollow particles can maintain the initial compressive strength while maintaining the compressive function of the elastic sheet, while maintaining a low compressive strength even when the compression ratio increases, and can also serve to cushion the impact applied to the electrode and solid electrolyte. In addition, the elastic sheet can be made to exhibit a grooved shape.
[0055] These hollow particles are particles with an empty interior, and can be expressed as hollow spheres or hollow beads, and can be hollow nanoparticles or hollow microparticles.
[0056] The above hollow particles may be polymer hollow particles formed from a polymer. The polymer may be polyacrylonitrile, polymethyl methacrylate, a silicon-containing polymer, or a combination thereof. The silicon-containing polymer may be a polymer obtained from phenyl silane, propyltrimethoxysilane, ethyltrimethoxy silane, methyltrimethoxy silane, propyltriethoxysilane, vinyltriethoxysilane, or methyltriethoxysilane.
[0057] The hollow particles may be expandable or non-expandable, and may expand at, for example, 120°C to 150°C.
[0058] The content of the hollow particles may be 0.5 wt% to 5 wt%, 0.5 wt% to 4 wt%, or 0.5 wt% to 3 wt% relative to 100 wt% of the entire elastic sheet. When the content of the hollow particles is within the above range, the initial compressive strength can be better maintained, while effectively suppressing an increase in compressive strength when the compression ratio increases.
[0059] The size of the hollow particles may be 10 µm to 90 µm, 30 µm to 90 µm, 35 µm to 90 µm, 40 µm to 90 µm, or 40 µm to 80 µm. When the size of the hollow particles satisfies the above range, the initial compressive strength can be better maintained, the impact applied to the electrode and the solid electrolyte can be more effectively alleviated, and the compression can be appropriately performed.
[0060] Glass Filler
[0061] In one embodiment, the glass filler serves to reduce the density of the elastic sheet, thereby improving the compressive strength. This glass filler may be a glass bubble. Reducing the density of the elastic sheet can improve energy capacity, and is suitable because the elastic sheet does not expand in the plane when compressed.
[0062] The glass filler may include Si, amorphous silica, mesoporous silica, fumed silica, or a combination thereof.
[0063] The content of the glass filler may be 1 wt% to 10 wt%, 1 wt% to 9 wt%, 2 wt% to 8 wt%, or 2 wt% to 7 wt% based on 100 wt% of the total weight of the elastic sheet. When the content of the glass filler is within the above range, the glass filler is more uniformly dispersed within the elastic sheet, which can further reduce the density of the elastic sheet, thereby further improving the energy capacity and further increasing the compressive strength improvement effect.
[0064] In one embodiment, the size of the glass filler may be 10 μm to 90 μm, 30 μm to 90 μm, 35 μm to 90 μm, 40 μm to 90 μm, or 40 μm to 80 μm. When the size of the glass filler is within the above range, the compressive strength can be further improved.
[0065] Other additives
[0066] An elastic sheet according to one embodiment may further include suitable additives in addition to the aforementioned components. For example, the additives may be cross-linking agents (e.g., silica, polyisocyanate compounds), tackifiers (e.g., terpenes, phenols, etc.), etc.
[0067] Each additive may be included in an appropriate amount according to the intended purpose, and there is no need to limit it.
[0068] In one embodiment, the thickness of the elastic sheet may be 100 μm to 800 μm, for example, 100 μm to 600 μm, or 150 μm to 500 μm. When the thickness of the elastic sheet is within the above range, the stress due to pressing and the stress due to thickness change during charging and discharging can be sufficiently alleviated, and excellent resilience can be exhibited.
[0069] According to one embodiment, an elastic sheet can be manufactured by adding an initiator to a composition for an elastic sheet, which comprises a linear alkyl (meth)acrylate first monomer having a glass transition temperature (Tg) of -30°C or lower, hollow particles, a glass filler, a cyclic alkyl (meth)acrylate second monomer having a Tg of 50°C or higher, an alkyl (meth)acrylate third monomer containing a hydroxyl group, hollow particles, and a glass filler, and then irradiating the resulting mixture with UV light.
[0070] The above investigation process can be carried out by applying the mixture to a heterogeneous substrate and irradiating it with UV.
[0071] The above initiator may be a radical photopolymerization initiator. The radical photopolymerization initiator may be 1,2-diphenyl-2,2-dimethoxyethanone (trade name: igacure651 (Ciba)), 2-ethylhexyl acrylate, 2-isopropyl thioxanthone, polyurethane acrylate, benzophenone, 4-methylbenzophenone, 4,4'-bis(diethylamino)benzophenone, or a combination thereof.
[0072] The content of the above initiator may be 1 part by weight to 5 parts by weight, specifically 0.05 parts by weight to 3 parts by weight, and more specifically 0.1 part by weight to 1 part by weight, based on 100 parts by weight of the total solid content of the composition for the elastic sheet.
[0073] A crosslinking agent may be further added to the above mixture.
[0074] The crosslinking agent is a polyfunctional (meth)acrylate, for example, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentylglycol di(meth)acrylate, polyethyleneglycol di(meth)acrylate, neopentylglycol adipate di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified di(meth)acrylate, di(meth)acryloxyethyl isocyanurate, allylated cyclohexyl di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, ethylene oxide-modified Difunctional acrylates such as hexahydrophthalic acid di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, neopentyl glycol modified trimethylpropane di(meth)acrylate, adamantane di(meth)acrylate or 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene, etc. Trifunctional acrylates such as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, trifunctional urethane (meth)acrylate or tris(meth)acryloxyethyl isocyanurate, etc. Examples thereof include, but are not limited to, tetrafunctional acrylates such as tetra(meth)acrylate or pentaerythritol tetra(meth)acrylate, pentafunctional acrylates such as dipentaerythritol penta(meth)acrylate, and hexafunctional acrylates such as dipentaerythritol hexa(meth)acrylate and caprolactone-modified dipentaerythritol hexa(meth)acrylate. These may be used alone or in combination of two or more.
[0075] The crosslinking agent may be included in an amount of 0.001 to 1 part by weight, specifically 0.03 to 0.7 parts by weight, specifically 0.1 to 0.5 parts by weight, based on 100 parts by weight of the solid content of the composition for the elastic sheet.
[0076] The above-mentioned heteromorphic film may be, but is not limited to, polyethylene terephthalate.
[0077] The above UV irradiation is 1000mJ / cm 2 5000mJ / cm 2 It can be implemented with the amount of light, but is not limited to this.
[0078] [All-solid-state battery]
[0079] Another embodiment provides an all-solid-state battery comprising the elastic sheet. The all-solid-state battery comprises a positive electrode, a negative electrode, a solid electrolyte layer positioned between the positive electrode and the negative electrode, and the elastic sheet positioned on the outer side of at least one of the positive electrode and the negative electrode.
[0080] The above elastic sheet may be positioned on the outermost layer surface of the electrode assembly, or in a structure in which two or more electrode assemblies are laminated, it may be positioned on the outermost layer and / or inside the assembly. Considering that the thickness of the negative electrode in particular changes significantly during charge and discharge due to reasons such as dendrite formation, the elastic sheet may be positioned on the outer side of the negative electrode, i.e., on the opposite side of the surface of the negative electrode where the solid electrolyte layer is in contact, so as to buffer problems caused by thickness changes. In addition, by positioning the elastic sheet on the outer side of the positive electrode and / or the negative electrode, the phenomenon of deterioration due to reaction with lithium may be prevented, thereby increasing the Coulombic efficiency of the battery.
[0081] Bipolar
[0082] The above positive electrode includes a positive electrode current collector and a positive electrode active material layer positioned on the positive electrode current collector.
[0083] The above-mentioned positive electrode active material layer may include a positive electrode active material and a sulfide-based solid electrolyte. In addition, the above-mentioned positive electrode active material layer may further include a binder and a conductive material.
[0084] The above positive electrode active material may be a positive electrode active material capable of reversibly absorbing and releasing lithium ions.
[0085] The above-mentioned positive electrode active material may be a positive electrode active material capable of reversibly absorbing and releasing lithium ions. For example, the positive electrode active material may use at least one of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof. Specific examples of the positive electrode active material include Li a A 1-b B 1 b D 1 2(0.90≤a≤1.8, 0≤b≤0.5); Li a E 1-b B 1 b O 2-c D 1 c (0.90≤a≤1.8, 0 ≤b≤0.5, 0≤c≤0.5); Li a E 2-b B 1 b O 4-c D 1 c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤05); Li a Ni 1-b-c Co b B 1 c D 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni1-b-c Co b B 1 c O 2-α F 1 2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mr b B 1 c D 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b-c Mr b B 1 c O 2-α F 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mr b B 1 c O 2-α F 1 2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni b HAVE BEEN c G d O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1); Li a Ni b Co c L 1 d G e O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0≤e≤0.1); Li a NiG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a MnG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2Gb O4(0.90≤a≤1.8, 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiI 1 O2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2); Li (3-f) Fe2(PO4)3(0≤f≤2); or LiFePO4.
[0086] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; B 1 is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements or a combination thereof; D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F 1 is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I 1 is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof; L 1 is Mn, Al or a combination thereof.
[0087] Of course, a compound having a coating layer on the surface of the compound may be used, or a compound having the compound and a coating layer may be mixed and used. The coating layer may include at least one coating element compound selected from the group consisting of an oxide of the coating element, a hydroxide of the coating element, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, and a hydroxycarbonate of the coating element. The compounds forming these coating layers may be amorphous or crystalline. The coating elements included in the coating layer may include Li, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a combination thereof.
[0088] In addition, as the above coating layer, any known coating layer of the positive electrode active material of an all-solid-state battery can be applied, and examples thereof include Li2O-ZrO2 (LZO).
[0089] Furthermore, when the cathode active material is a ternary compound containing nickel, cobalt, and manganese, or nickel, cobalt, and aluminum, the capacity density of the all-solid-state battery can be further improved and metal dissolution from the cathode active material can be further reduced in a charged state. Consequently, the all-solid-state battery can exhibit improved long-term reliability and cycle performance in a charged state.
[0090] Here, the shape of the positive electrode active material may include, for example, a particle shape such as a sphere, an ellipsoid, a shape close to a sphere, a polyhedron, or an irregular shape.
[0091] In addition, the average particle diameter of the positive electrode active material is not particularly limited and may be within a range applicable to positive electrode active materials of existing all-solid-state secondary batteries. For example, the average particle diameter of the positive electrode active material may be 1 μm to 25 μm, for example, 4 μm to 25 μm, 5 μm to 20 μm, 8 μm to 20 μm, or 10 μm to 18 μm. A positive electrode active material having such a particle diameter range can be harmoniously mixed with other components within the positive electrode active material layer and can realize high capacity and high energy density.
[0092] The above positive electrode active material may be in the form of secondary particles formed by agglomeration of a plurality of primary particles, or may be in the form of a single crystal.
[0093] In addition, in the positive electrode active material layer, the content of the positive electrode active material is not particularly limited, but for example, with respect to 100 wt% of the entire positive electrode active material layer, the positive electrode active material may be included in an amount of 55 wt% to 99.7 wt%, for example, 74 wt% to 89.8 wt%. When included in the above range, the capacity of the all-solid-state battery can be maximized while further improving the life characteristics.
[0094] In one embodiment, the sulfide-based solid electrolyte is Li2S-P2S5, Li2S-P2S5-LiX (X is a halogen element, for example, I or Cl), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (m and n are integers greater than or equal to 0 and less than or equal to 12, respectively, and Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p and q are integers greater than or equal to 0 and less than or equal to 12, respectively; M is one of P, Si, Ge, B, Al, Ga In), Li a M b P c S d A e (a, b, c, d and e are each integers greater than or equal to 0 and less than or equal to 12, M is Ge, Sn, Si or a combination thereof, and A is one of F, Cl, Br, or I). The sulfide-based solid electrolyte may be, for example, Li 7-x PS 6-x F x (0≤x≤2), Li 7-x PS 6-x Cl x (0≤x≤2), Li 7-x PS6-x Br x (0≤x≤2) or Li 7-x PS 6-x I x (0≤x≤2) can be. Also, specifically, Li3PS4, Li7P3S 11 , Li7PS6, Li6PS5Cl, Li6PS5Cl, Li6PS5I, Li6PS5Br, Li 5.8 PS 4.8 Cl 1.2 , Li 6.2 PS 5.2 Br 0.8 It could be the back.
[0095] In one embodiment, the sulfide-based solid electrolyte may be an argyrodite-type sulfide-based solid electrolyte. The argyrodite-type sulfide-based solid electrolyte may be, for example, Li a M b P c S d A e (a, b, c, d, and e are all 0 or greater and 12 or less, M is Ge, Sn, Si, or a combination thereof, and A is one of F, Cl, Br, or I).
[0096] As specific examples, Li3PS4, Li7P3S 11 , Li7PS6, Li6PS5Cl, Li6PS5Br, Li 5.8 PS 4.8 Cl 1.2 , Li 6.2 PS 5.2 Br 0.8 , Li6PS5I, Li 5.75 PS 4.75 Cl 1.25 , (Li 5.69 Cu 0.06 )PS 4.75 Cl 1.25 , (Li 5.72 Cu 0.03 )PS 4.75 Cl 1.25 , (Li 5.69 Cu 0.06 )P(S 4.70 (SO4) 0.05)Cl 1.25 , (Li 5.69 Cu 0.06 )P(S 4.60 (SO4) 0.15 )Cl 1.25 , (Li 5.72 Cu 0.03 )P(S 4.725 (SO4) 0.025 )Cl 1.25 , (Li 5.72 Na 0.03 )P(S 4.725 (SO4) 0.025 )Cl 1.25 , Li 5.75 P(S 4.725 (SO4) 0.025 )Cl 1.25 , or combinations thereof, but are not limited thereto.
[0097] The sulfide-based solid electrolyte may be amorphous, crystalline, or a mixture thereof. For example, the sulfide-based solid electrolyte may be obtained by mixing Li2S and P2S5 in a molar ratio of 50:50 to 90:10, or in a molar ratio of 50:50 to 80:20. Within the above mixing ratio range, a sulfide-based solid electrolyte having excellent ionic conductivity can be produced. Here, the ionic conductivity can be further improved by further including other components such as SiS2, GeS2, and B2S3.
[0098] Methods for mixing sulfur-containing raw materials for manufacturing sulfide-based solid electrolytes include mechanical milling and solution methods. Mechanical milling involves placing the starting raw materials in a reactor and vigorously stirring them with a ball mill, thereby finely agitating the starting raw materials and mixing them. Using the solution method, the starting raw materials are mixed in a solvent to obtain a solid electrolyte as a precipitate. Furthermore, heat treatment after mixing can solidify the crystals of the solid electrolyte and improve ionic conductivity. For example, a sulfide-based solid electrolyte can be manufactured by mixing sulfur-containing raw materials and heat-treating them twice or more, in which case a sulfide-based solid electrolyte with high ionic conductivity and robustness can be manufactured.
[0099] Of course, a commercially available solid electrolyte can be used as the sulfide-based solid electrolyte.
[0100] With respect to the total weight of the positive electrode active material layer, the content of the solid electrolyte may be 0.1 wt% to 35 wt%, for example, 1 wt% to 35 wt%, 5 wt% to 30 wt%, 8 wt% to 25 wt%, or 10 wt% to 20 wt%. In addition, with respect to the total weight of the positive electrode active material and the solid electrolyte in the positive electrode active material layer, 65 wt% to 99 wt% of the positive electrode active material and 1 wt% to 35 wt% of the solid electrolyte may be included, for example, 80 wt% to 90 wt% of the positive electrode active material and 10 wt% to 20 wt% of the solid electrolyte may be included. When the solid electrolyte is included in the positive electrode in such an amount, the efficiency and life characteristics of the all-solid-state battery can be improved without reducing the capacity.
[0101] The above binder serves to adhere the positive electrode active material particles well to each other and also to adhere the positive electrode active material well to the current collector. Examples of the binder include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc.
[0102] The binder may be included in an amount of 0.1 wt% to 5 wt%, or 0.1 wt% to 3 wt%, based on 100 wt% of the total weight of the positive electrode active material layer. Within the above content range, the binder can sufficiently exhibit adhesive ability without degrading battery performance.
[0103] The conductive material is used to provide conductivity to the electrode, and any material that does not cause chemical changes and is electronically conductive can be used in the battery. Examples of the conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, and carbon nanotubes; metal-based materials containing copper, nickel, aluminum, silver, etc. in the form of metal powder or metal fiber; conductive polymers such as polyphenylene derivatives; or conductive materials including mixtures thereof.
[0104] The conductive material may be included in an amount of 0.1 wt% to 5 wt%, or 0.1 wt% to 3 wt%, based on 100 wt% of the total weight of the positive electrode active material layer. Within the above content range, the conductive material can improve electrical conductivity without degrading battery performance.
[0105] The thickness of the positive electrode active material layer may be 90 μm to 200 μm. For example, the thickness of the positive electrode active material layer may be 90 μm or more, 100 μm or more, 110 μm or more, 120 μm or more, 130 μm or more, 140 μm or more, 150 μm or more, 160 μm or more, 170 μm or more, 180 μm or more, or 190 μm or more, and may be 200 μm or less, 190 μm or less, 180 μm or less, 170 μm or less, 160 μm or less, 150 μm or less, 140 μm or less, 130 μm or less, 120 μm or less, or 110 μm or less.
[0106] The above anode current collector may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li) or an alloy thereof, and may be in the form of a foil or sheet.
[0107] <Cathode>
[0108] The above cathode includes a current collector and a cathode layer positioned on one surface of the current collector.
[0109] The above cathode layer may be a cathode coating layer, and the cathode coating layer may be a lithium electrodeposition induction layer or a cathode catalyst layer.
[0110] When the above-mentioned negative electrode layer is a negative electrode coating layer, it means that the negative electrode is a precipitation-type negative electrode. The precipitation-type negative electrode means a negative electrode that does not contain a negative electrode active material when the battery is assembled, but in which lithium metal or the like is precipitated when the battery is charged, and this acts as a negative electrode active material. In more detail, when the all-solid-state battery is charged, lithium ions are released from the positive electrode active material, pass through the solid electrolyte, and move toward the negative electrode, and are deposited on the negative electrode current collector, so that a lithium-containing layer, for example, a lithium precipitation layer, can be formed between the current collector and the negative electrode layer. A negative electrode having such a lithium-containing layer is called a precipitation-type negative electrode.
[0111] That is, a lithium-containing layer can be formed between the negative electrode current collector and the negative electrode layer.
[0112] The above charging process may be a chemical reaction process performed once to three times at 0.05C to 1C at about 25°C to 50°C.
[0113] The thickness of the lithium-containing layer may be 10 μm to 50 μm. For example, the thickness of the lithium-containing layer may be 10 μm or more, 20 μm or more, 30 μm or more, or 40 μm or more, or 50 μm or less, 40 μm or less, 30 μm or less, or 20 μm or less. When the thickness of the lithium-containing layer is within the above range, there may be an advantage in that lithium may be reversibly precipitated during charge / discharge, thereby further improving the lifespan.
[0114] The cathode coating layer may include a metal, a carbon material, or a combination thereof that acts as a catalyst. For example, the cathode coating layer may include a metal supported on a carbon material, or a mixture of the metal and the carbon material. In one embodiment, the cathode coating layer may include a metal and a carbon material.
[0115] The carbon material may be, for example, crystalline carbon, amorphous carbon, or a combination thereof, and may be amorphous carbon. The crystalline carbon may be, for example, natural graphite, artificial graphite, mesophase carbon microbeads, or a combination thereof.
[0116] The amorphous carbon may be, for example, carbon black, acetylene black, Denka black, Ketjen black, furnace black, activated carbon, graphene, or a combination thereof. An example of the carbon black may be Super P (Timcal). The amorphous carbon is not limited thereto, and any amorphous carbon classified as such in the relevant field may be used.
[0117] The above amorphous carbon may be a single particle, may have the form of a secondary particle formed by agglomeration of multiple primary particles, or may be a combination thereof.
[0118] The particle size of the above single particle may be 10 nm to 60 mm. In addition, the particle size of the above primary particle may be 20 nm to 100 nm, and the particle size of the above secondary particle may be 1 μm to 20 μm.
[0119] In one embodiment, the particle size of the primary particles may be 20 nm or more, 30 nm or more, 40 nm or more, 50 nm or more, 60 nm or more, 70 nm or more, 80 nm or more, or 90 nm or more, and may be 100 nm or less, 90 nm or less, 80 nm or less, 70 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, or 30 nm or less.
[0120] In one embodiment, the particle size of the secondary particles may be 1 µm or more, 3 µm or more, 5 µm or more, 7 µm or more, 10 µm or more, or 15 µm or more, and may be 20 µm or less, 15 µm or less, 10 µm or less, 7 µm or less, 5 µm or less, or 3 µm or less.
[0121] The shape of the primary particles may be spherical, elliptical, plate-shaped, or a combination thereof, and in one embodiment, the shape of the primary particles may be spherical, elliptical, or a combination thereof.
[0122] The metal may be any one selected from Ag, Zn, Al, Sn, Mg, Ge, Cu, In, Ni, Bi, Au, Si, Pt, Pd, and combinations thereof, and in one embodiment may be Ag. When the cathode coating layer includes the metal particles, the electrical conductivity of the cathode may be improved.
[0123] The metal particles may have a size of 5 nm to 800 nm. The size of the metal particles may be 5 nm or more, 50 nm or more, 100 nm or more, 150 nm or more, 200 nm or more, 250 nm or more, 300 nm or more, 350 nm or more, 400 nm or more, 450 nm or more, 500 nm or more, 550 nm or more, 600 nm or more, 650 nm or more, 700 nm or more, or 750 nm or more. In addition, the size of the metal particles may be 800 nm or less, 750 nm or less, 700 nm or less, 650 nm or less, 600 nm or less, 550 nm or less, 500 nm or less, 450 nm or less, 400 nm or less, 350 nm or less, 300 nm or less, 250 nm or less, 200 nm or less, 150 nm or less, 100 nm or less, or 50 nm or less. When the size of the metal particles is within the above range, the battery characteristics (e.g., life characteristics) of the all-solid-state battery can be improved.
[0124] When the cathode coating layer includes a carbon-based material and metal particles, the mixing ratio of the carbon-based material and the metal particles may be a weight ratio of 1:1 to 99:1. For example, the weight of the carbon-based material may be 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 10 or more, 15 or more, 20 or more, 25 or more, 30 or more, 35 or more, 40 or more, 45 or more, 50 or more, 55 or more, 60 or more, 65 or more, 70 or more, 75 or more, 80 or more, 85 or more, 90 or more or 95 or more, and may be 99 or less, 95 or less, 90 or less, 85 or less, 80 or less, 75 or less, 70 or less, 65 or less, 60 or less, 55 or less, 50 or less, 45 or less, 40 or less, 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, 10 or less, 5 or less, 4 or less, 3 or less or 2 or less. For example, the weight ratio of the carbon-based material and the metal particles may be 1:1 to 5:1, 1:1 to 10:1, 1:1 to 20:1, 1:1 to 30:1, 1:1 to 40:1, 1:1 to 50:1, 1:1 to 60:1, 1:1 to 70:1, 1:1 to 80:1, or 1:1 to 90:1. When the carbon-based material and the metal particles are included in the weight ratio, the electrical conductivity of the negative electrode can be further improved.
[0125] When the above-mentioned cathode layer is a cathode coating layer, the cathode current collector may be, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li) or an alloy thereof, and may be in the form of a foil or sheet.
[0126] The above cathode coating layer may further include a binder.
[0127] The above binder may include a non-aqueous binder, an aqueous binder, or a combination thereof.
[0128] The non-aqueous binder may include, for example, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyethylene oxide, ethylene propylene copolymer, polystyrene, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, polyacrylate, or combinations thereof.
[0129] The above-mentioned aqueous binder may include styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, polyvinyl alcohol, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenol resin, epoxy resin, acrylic rubber, butyl rubber, fluoroelastomer, or a combination thereof.
[0130] The negative electrode binder may include a cellulose-based compound. In addition, the negative electrode binder may include both the aqueous binder and the cellulose-based compound. The cellulose-based compound may include carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, an alkali metal salt thereof, or a combination thereof. The alkali metal may be Na, K, or Li. The cellulose-based compound may also function as a thickener capable of imparting viscosity in addition to being a binder.
[0131] The above binders are not limited to these, and any binder used in the relevant technical field may be used, and their content can also be appropriately adjusted.
[0132] The above cathode coating layer may further include a solid electrolyte, and the solid electrolyte may be a sulfide-based solid electrolyte as described above for the anode. The solid electrolyte included in the cathode may be the same as or different from the solid electrolyte included in the anode.
[0133] The above-described cathode coating layer may further include additives such as fillers, dispersants, and ionic conductive agents. In addition, known materials generally used in all-solid-state batteries may be used as fillers, dispersants, and ionic conductive agents that can be included in the cathode coating layer.
[0134] The thickness of the cathode coating layer may be, for example, 1 µm to 500 µm, 1 µm to 200 µm, 1 µm to 100 µm, or 1 µm to 50 µm, but is not limited thereto.
[0135] In one embodiment, the negative electrode layer may be a negative electrode active material layer.
[0136] The above negative electrode active material layer includes a negative electrode active material, may include a binder, and may further include a conductive material.
[0137] The above negative electrode active material may include lithium metal. When the negative electrode active material includes lithium metal, it may include lithium metal itself or a lithium alloy. The lithium alloy may be, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, or a Li-Si alloy.
[0138] The above negative active material may include a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0139] The material capable of reversibly intercalating / deintercalating the lithium ions may include a carbon-based negative electrode active material, for example, crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as natural graphite or artificial graphite in an amorphous, plate-like, flake-like, spherical, or fibrous form, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, and the like.
[0140] As the above lithium metal alloy, an alloy of lithium and one or more metals selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn can be used.
[0141] As the material capable of doping and dedoping the lithium, a Si-based negative electrode active material or a Sn-based negative electrode active material can be used, and the Si-based negative electrode active material may be silicon, a silicon-carbon composite, or SiO. x(0 <x<2), Si-Q 합금(상기 Q는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 15족 원소, 16족 원소, 전이금속, 희토류 원소 및 이들의 조합으로 이루어진 군에서 선택되는 원소이며, Si은 아님), 상기 Sn계 음극 활물질로는 Sn, SnO2, Sn-R 합금(상기 R은 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 15족 원소, 16족 원소, 전이금속, 희토류 원소 및 이들의 조합으로 이루어진 군에서 선택되는 원소이며, Sn은 아님) 등을 들 수 있고, 또한 이들 중 적어도 하나와 SiO2를 혼합하여 사용할 수도 있다. 상기 원소 Q 및 R로는 Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, 및 이들의 조합으로 이루어진 군에서 선택되는 것을 사용할 수 있다.
[0142] The above silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle diameter (D) of the silicon-carbon composite particles 50 ) may be, for example, 0.5 μm to 20 μm. According to one embodiment, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surface of the silicon particles. For example, it may include secondary particles (cores) in which silicon primary particles are assembled and an amorphous carbon coating layer (shell) located on the surface of the secondary particles. The amorphous carbon may also be located between the silicon primary particles, so that, for example, the silicon primary particles may be coated with amorphous carbon. The secondary particles may be dispersed and present in an amorphous carbon matrix.
[0143] The silicon-carbon composite may further comprise crystalline carbon. For example, the silicon-carbon composite may comprise a core comprising crystalline carbon and silicon particles, and an amorphous carbon coating layer positioned on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon may include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, and the like.
[0144] When the above silicon-carbon composite includes silicon and amorphous carbon, the content of silicon may be 10 wt% to 50 wt%, and the content of amorphous carbon may be 50 wt% to 90 wt%, based on 100 wt% of the silicon-carbon composite. In addition, when the composite includes silicon, amorphous carbon, and crystalline carbon, the content of silicon may be 10 wt% to 50 wt%, the content of crystalline carbon may be 10 wt% to 70 wt%, and the content of amorphous carbon may be 20 wt% to 40 wt%, based on 100 wt% of the silicon-carbon composite.
[0145] In addition, the thickness of the amorphous carbon coating layer may be 5 nm to 100 nm. The average particle diameter (D) of the silicon particles (primary particles) 50 ) may be 10 nm to 1 ㎛, or 10 nm to 200 nm. The silicon particles may exist as silicon alone, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon is SiO x (0 <x<2)로 표시될 수 있다. 이때, 산화 정도를 나타내는 Si:O의 원자 함량 비율은 99:1 내지 33:67일 수 있다. 본 명세서에서, 별도의 정의가 없는 한, 평균 입경(D 50 ) means the diameter of the particle whose cumulative volume is 50% by volume in the particle size distribution.
[0146] The above Si-based negative electrode active material or Sn-based negative electrode active material can be used in combination with a carbon-based negative electrode active material. When the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material are used in combination, the mixing ratio can be 1:99 to 90:10 by weight.
[0147] The content of the negative active material in the above negative active material layer may be 95 wt% to 99 wt% with respect to the total weight of the negative active material layer.
[0148] The content of the binder in the negative electrode active material layer may be 1 wt% to 5 wt% based on the total weight of the negative electrode active material layer. In addition, when further including a conductive material, the negative electrode active material layer may include 90 wt% to 98 wt% of the negative electrode active material, 1 wt% to 5 wt% of the binder, and 1 wt% to 5 wt% of the conductive material.
[0149] The above binder serves to adhere the negative electrode active material particles well to each other and also to adhere the negative electrode active material well to the current collector. The binder may include a non-aqueous binder, an aqueous binder, or a combination thereof.
[0150] The non-aqueous binder may include, for example, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.
[0151] The above-mentioned aqueous binder may include styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluoroelastomer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenol resin, epoxy resin, polyvinyl alcohol, or a combination thereof.
[0152] In addition, the negative electrode active material layer may include a cellulose-based compound. The cellulose-based compound may include carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, an alkali metal salt thereof, or a combination thereof. Na, K, or Li may be used as the alkali metal. The cellulose-based compound may function as a binder or as a thickener that provides viscosity. Accordingly, the content of the cellulose-based compound need not be limited, but may be, for example, 0.1 to 3 parts by weight based on 100 parts by weight of the negative electrode active material.
[0153] When the above-mentioned negative electrode layer is a negative electrode active material layer, a current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and a combination thereof.
[0154] Solid electrolyte layer
[0155] The above solid electrolyte layer may include a solid electrolyte. The solid electrolyte may be an inorganic solid electrolyte such as a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a halide-based solid electrolyte, or a solid polymer electrolyte.
[0156] The above sulfide-based solid electrolyte is as described above, and may be the same as or different from the solid electrolyte included in the positive electrode or the negative electrode.
[0157] The above oxide-based solid electrolyte is, for example, Li 1+x Ti 2-x Al(PO4)3(LTAP)(0≤x≤4), Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0≤x<1, 0≤y<1), Pb(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 <x<2, 0<y<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1, 0≤y≤1), lithium lanthanum titanate (Li x La y TiO3, 0 <x<2, 0<y<3), Li2O, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2계 세라믹스, 가넷(Garnet)계 세라믹스 Li 3+x La3M2O 12 (M= Te, Nb, or Zr, x is an integer from 1 to 10), or a mixture thereof.
[0158] The above halide-based solid electrolyte may include a Li element, an M element (M is a metal other than Li), and an X element (X is a halogen). As X, for example, F, Cl, Br, and I may be mentioned. In particular, in the halide-based solid electrolyte, at least one of Br and Cl is suitable as X. In addition, as the M, for example, a metal element such as Sc, Y, B, Al, Ga, or In may be mentioned.
[0159] The composition of the above halide-based solid electrolyte is not particularly limited, but Li 6-3a M a Br b Cl c (In the formula, M is a metal other than Li, and 0 <a<2, 0≤b≤6, 0≤c≤6, b+c=6)로 표현될 수 있다. 이때, 상기 a는 0.75 이상일 수 있고, 1 이상일 수 있고, a는, 1.5 이하일 수 있다. 상기 b는 1 이상일 수 있고, 2 이상일 수 있다. 또한, 상기 c는, 3 이상일 수 있고, 4 이상일 수도 있다. 상기 할라이드계 고체 전해질의 구체적인 예로는 Li3YBr6, Li3YCl6또는 Li3YBr2Cl4를 들 수 있다.
[0160] The above solid electrolyte layer may further include a binder. At this time, the binder may be styrene butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, an acrylate polymer, or a combination thereof, but is not limited thereto, and any binder used in the relevant technical field may be used. The acrylate polymer may be butyl acrylate, polyacrylate, polymethacrylate, or a combination thereof.
[0161] The above solid electrolyte layer can be formed by adding a solid electrolyte to a binder solution, coating the same on a base film, and drying the same. The solvent for the binder solution may be isobutyryl isobutyrate, xylene, toluene, benzene, hexane, or a combination thereof. Since the solid electrolyte layer formation process is widely known in the art, a detailed description thereof will be omitted herein.
[0162] The thickness of the solid electrolyte layer may be, for example, 10 μm to 150 μm.
[0163] The solid electrolyte layer may further include an alkali metal salt, and / or an ionic liquid, and / or a conductive polymer.
[0164] The above alkali metal salt may be, for example, a lithium salt. The content of the lithium salt in the solid electrolyte layer may be 1 M or more, for example, 1 M to 4 M. In this case, the lithium salt may improve ion conductivity by enhancing the lithium ion mobility of the solid electrolyte layer.
[0165] The above lithium salts include, for example, LiSCN, LiN(CN)2, Li(CF3SO2)3C, LiC4F9SO3, LiN(SO2CF2CF3)2, LiCl, LiF, LiBr, LiI, LiB(C2O4)2, LiBF4, LiBF3(C2F5), lithium bis(oxalato)borate (LiBOB), lithium oxalyldifluoroborate (LIODFB), lithium difluoro(oxalato)borate (LiDFOB), lithium bis(trifluoro methanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI, It may include LiN(SO2F)2), LiCF3SO3, LiAsF6, LiSbF6, LiClO4 or mixtures thereof.
[0166] In addition, the lithium salt may be an imide-based one, and for example, the imide-based lithium salt may include lithium bis(trifluoro methanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), lithium bis(fluorosulfonyl)imide (LiFSI, LiN(SO2F)2). The lithium salt may maintain or improve ionic conductivity by appropriately maintaining chemical reactivity with an ionic liquid.
[0167] The above ionic liquid has a melting point below room temperature and is a salt or room-temperature molten salt that is liquid at room temperature and consists only of ions.
[0168] The above ionic liquid comprises a) one or more cations selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof, and b) BF4. - , PF6 - , AsF6 - , SbF6 - , AlCl4 - , HSO4 - , ClO4 - , CH3SO3 - , CF3CO2 - , Cl - , Br - , I - , BF4 - , SO4 - , CF3SO3 - , (FSO2)2N - , (C2F5SO2)2N - , (C2F5SO2)(CF3SO2)N - , and (CF3SO2)2N - It may be a compound containing one or more anions selected from among.
[0169] The ionic liquid may be at least one selected from the group consisting of, for example, N-methyl-N-propylpyrrolidinium bis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(3-trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)amide, and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)amide.
[0170] In the above solid electrolyte layer, the weight ratio of the solid electrolyte and the ionic liquid may be 0.1:99.9 to 90:10, for example, 10:90 to 90:10, 20:80 to 90:10, 30:70 to 90:10, 40:60 to 90:10, or 50:50 to 90:10. A solid electrolyte layer satisfying the above range can maintain or improve ionic conductivity by improving the electrochemical contact area with the electrode. Accordingly, the energy density, discharge capacity, rate characteristics, etc. of the all-solid-state battery can be improved.
[0171] According to one embodiment, an all-solid-state battery can be manufactured by sequentially stacking a positive electrode, a solid electrolyte, and a negative electrode to prepare a laminate, adhering an elastic sheet to the outer surface of the positive electrode and / or the negative electrode, and then pressing. The pressing can be performed at a temperature of, for example, 25°C to 90°C, and at a pressure of 550 MPa or less, or 500 MPa or less, for example, 1 MPa to 500 MPa. The pressing time can vary depending on the temperature and pressure, and can be, for example, less than 30 minutes. The pressing can be, for example, isostatic pressing, warm isostatic pressing, roll pressing, or plate pressing.
[0172] Under these pressurized conditions, the elastic sheet described above can be compressed at an appropriate ratio of 30% to 70% of the initial thickness, and the recovery rate of the elastic sheet can satisfy a ratio of 60% to 90% of the initial thickness.
[0173] The above-mentioned all-solid-state battery may be a unit battery having a structure of positive electrode / solid electrolyte layer / negative electrode, a bi-cell having a structure of positive electrode / solid electrolyte layer / negative electrode / solid electrolyte layer / positive electrode, or a laminated battery in which the structure of the unit battery is repeated.
[0174] The shape of the above-mentioned all-solid-state battery is not particularly limited, and may be, for example, coin-shaped, button-shaped, sheet-shaped, stacked, cylindrical, flat, etc. In addition, the above-mentioned all-solid-state battery can be applied to medium- to large-sized batteries used in electric vehicles, etc. For example, the above-mentioned all-solid-state battery can be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, it can be applied to energy storage systems (ESS) that require a large amount of power storage, and can also be applied to electric bicycles or power tools, etc.
[0175] FIG. 1 is a cross-sectional view of an all-solid-state battery according to one embodiment. Referring to FIG. 1, the all-solid-state battery (100) may have a structure in which an electrode assembly is housed in a case such as a pouch, in which an anode (400) including an anode current collector (401) and an anode active material layer (403); a solid electrolyte layer (300); a cathode (200) including an anode active material layer (203) and a cathode current collector (201); and an elastic sheet (500) positioned on the outer side of at least one of the cathode (200) and the anode (400) is laminated. Although FIG. 1 illustrates one electrode assembly including an anode (400), a solid electrolyte layer (300), and a cathode (200), an all-solid-state battery may be manufactured by laminating two or more electrode assemblies.
[0176] The all-solid-state battery (100) is manufactured by pressurizing an electrode laminate during the manufacturing process, and has a structure in which charging and discharging are performed in a pressurized state.
[0177] FIG. 1 shows a structure in which an elastic sheet (500) is positioned on the outermost layer of an electrode assembly, but is not limited thereto. As explained above, in a structure in which two or more electrode assemblies are laminated, the elastic sheet may be positioned on the outermost layer and / or inside the assembly.
[0178] Fig. 2 is a schematic cross-sectional view of an all-solid-state battery including a precipitation-type negative electrode. Referring to Fig. 2, the precipitation-type negative electrode (400') may include a current collector (401) and a negative electrode active material layer (405) positioned on the current collector. In an all-solid-state battery including such a precipitation-type negative electrode (400'), a high-density lithium metal or the like may be precipitated between the current collector (401) and the negative electrode active material layer (405) during initial charging, thereby forming a lithium precipitation layer (404). Accordingly, in an all-solid-state battery that has been charged at least once, the precipitation-type negative electrode (400') may include a current collector (401), a lithium precipitation layer (404) positioned on the current collector, and a negative electrode active material layer (405) positioned on the lithium precipitation layer. The above lithium precipitation layer (404) refers to a layer in which lithium metal, etc. is precipitated during the charging process of the battery, and may be referred to as a metal layer or a negative electrode active material layer.
[0179] Hereinafter, examples and comparative examples of the present invention will be described. The following examples are merely exemplary of the present invention, and the present invention is not limited to the following examples.
[0180] (Example 1)
[0181] (1) Manufacturing of elastic sheets
[0182] A composition for elastic sheets was prepared by mixing a first monomer of 2-ethylhexyl acrylate, a second monomer of isobornyl acrylate, and a third monomer of 4-hydroxybutyl acrylate in a weight ratio of 25:25:50, and then adding a 1,6-hexanediol diacrylate crosslinking agent and an initiator of 1,2-diphenyl-2,2-dimethoxyethanone (igacure651 (Ciba)), acrylonitrile hollow particles (trade name: Expancel 920Det40, Akzo), glass bubbles (trade name: K-1, 3M), and finely powdered silica (trade name: R-972, Evonik). At this time, the content of the crosslinking agent was 0.05 parts by weight, the content of the initiator was 0.25 parts by weight, the content of the hollow particles was 1 part by weight, the content of the glass bubbles was 7 parts by weight, and the content of the fine powder silica was 0.5 parts by weight, based on 100 parts by weight of the composition for the elastic sheet.
[0183] The obtained mixture was applied between polyethylene terephthalate (PET) films, which are release films, and exposed to ultraviolet light at 2000 mJ / cm 2 By examining the amount of light, an elastic sheet bonded onto a PET film was manufactured. The manufactured elastic sheet included a ternary copolymer of a first repeating unit derived from the first monomer, a second repeating unit derived from the second monomer, and a third repeating unit derived from the third monomer.
[0184] (2) Manufacturing of the anode
[0185] LiNi 0.8 Co 0.15 Mn 0.05 A cathode composition was prepared by mixing 85 wt% of O2 cathode active material, 13.5 wt% of lithium argyrodite-type solid electrolyte Li6PS5Cl, 1.0 wt% of polyvinylidene fluoride binder, and 0.5 wt% of carbon nanotube conductive material in an N-methyl pyrrolidone solvent.
[0186] The manufactured positive electrode composition was coated on an aluminum positive electrode current collector using a bar coater, dried, and rolled to manufacture a positive electrode.
[0187] (3) Manufacturing of solid electrolyte layer
[0188] An acrylic binder (SX-A334, Zeon) was dissolved in an isobutyl isobutyrate (IBIB) solvent. An argyrodite-type solid electrolyte, Li6PS5Cl (D50=3㎛), was added to the binder solution, which was stirred in a sinky mixer to adjust the viscosity to an appropriate level. 2 mm zirconia balls were added and stirred again in the sinky mixer to prepare a slurry. In the prepared slurry, the content of the solid electrolyte was 98.5 wt%, and the content of the binder was 1.5 wt%.
[0189] The above slurry was applied onto a polyethylene film using a bar coater and dried at room temperature (25°C), and then the polyethylene film was removed to prepare a solid electrolyte layer.
[0190] (4) Manufacturing of cathode
[0191] Carbon black having a primary particle diameter (D50) of about 30 nm and silver (Ag) having an average particle diameter (D50) of about 60 nm are mixed in a weight ratio of 3:1, and 0.25 g of this mixture is added to 2 g of an N-methyl pyrrolidone solution containing 7 wt% of a polyvinylidene fluoride binder, and mixed to prepare a negative electrode active material layer composition.
[0192] The above negative electrode active material layer composition was applied to a nickel foil current collector using a bar coater and vacuum dried to manufacture a negative electrode.
[0193] (5) Manufacturing of all-solid-state batteries
[0194] After sequentially stacking the manufactured positive electrode, solid electrolyte layer, and negative electrode, the manufactured elastic sheet was stacked on the negative electrode. Subsequently, the negative electrode, solid electrolyte layer, and positive electrode were sequentially stacked to manufacture an assembly in the order of positive electrode / solid electrolyte / negative electrode / elastic sheet / negative electrode / solid electrolyte / positive electrode.
[0195] The above assembly was placed in a laminate film and pressurized at 80°C with a force of 500 MPa to manufacture an all-solid-state battery.
[0196] In a pressurized state, the thickness of the positive active material layer was about 100 μm, the thickness of the negative active material layer was about 7 μm, the thickness of the solid electrolyte layer was about 60 μm, and the thickness of the elastic sheet was about 120 μm.
[0197] (Example 2)
[0198] An elastic sheet was manufactured in the same manner as in Example 1, except that a composition for an elastic sheet was used in which a first monomer of 2-ethylhexyl acrylate, a second monomer of isobornyl acrylate, and a third monomer of 4-hydroxybutyl acrylate were mixed in a weight ratio of 35:15:50.
[0199] An all-solid-state battery was manufactured in the same manner as in Example 1 using the above elastic sheet.
[0200] (Example 3)
[0201] An elastic sheet was manufactured in the same manner as in Example 1, except that the content of acrylonitrile hollow particles was 0.5 parts by weight per 100 parts by weight of the composition for the elastic sheet.
[0202] An all-solid-state battery was manufactured in the same manner as in Example 1 using the above elastic sheet.
[0203] (Example 4)
[0204] An elastic sheet was manufactured in the same manner as in Example 1, except that the content of acrylonitrile hollow particles was changed to 3 parts by weight per 100 parts by weight of the composition for the elastic sheet.
[0205] An all-solid-state battery was manufactured in the same manner as in Example 1 using the above elastic sheet.
[0206] (Example 5)
[0207] An elastic sheet was manufactured in the same manner as in Example 1, except that the glass bubble content was changed to 3 parts by weight per 100 parts by weight of the composition for the elastic sheet.
[0208] An all-solid-state battery was manufactured in the same manner as in Example 1 using the above elastic sheet.
[0209] (Example 6)
[0210] An elastic sheet was manufactured in the same manner as in Example 1, except that the glass bubble content was changed to 10 parts by weight per 100 parts by weight of the composition for the elastic sheet.
[0211] An all-solid-state battery was manufactured in the same manner as in Example 1 using the above elastic sheet.
[0212] (Comparative Example 1)
[0213] An elastic sheet was manufactured in the same manner as in Example 1, except that acrylonitrile hollow particles were not added.
[0214] An all-solid-state battery was manufactured in the same manner as in Example 1 using the above elastic sheet.
[0215] (Comparative Example 2)
[0216] An elastic sheet was manufactured in the same manner as in Example 1, except that glass bubbles were not added.
[0217] An all-solid-state battery was manufactured in the same manner as in Example 1 using the above elastic sheet.
[0218] (Comparative Example 3)
[0219] An all-solid-state battery was manufactured in the same manner as in Comparative Example 3, except that a 200 μm thick urethane film manufactured from a polyurethane resin with excellent recovery rate was used as an elastic sheet.
[0220] (Comparative Example 4)
[0221] An all-solid-state battery was manufactured in the same manner as in Comparative Example 3, except that a 200 μm thick urethane film made of polyurethane resin with excellent stress relaxation properties was used as an elastic sheet.
[0222] Experimental Example 1: Compressive Strength Evaluation
[0223] The compressive strength was measured for the elastic sheets of Examples 1 to 6 and Comparative Examples 1 to 4.
[0224] Here, the compressive strength is the value of CFD50 and CFD70, which represents the compressive strength when the physically elastic sheet is compressed to 50% and 30% of its original thickness.
[0225] The above compression process was performed by compressing the specimen at a compression ratio of 0.6 mm / min (10 ㎛ / sec) using a compression tester with a spherical jig having a diameter of 10 mm.
[0226] At this time, the compressive strength was obtained when the specimen thickness was 50% and 70%. The results are shown in Table 1 below.
[0227] Experimental Example 2: Stress Relaxation Rate Evaluation
[0228] The stress relaxation rate of the elastic sheets of Examples 1 to 6 and Comparative Examples 1 to 4 was evaluated. The results are shown in Table 1 below. The stress relaxation rate was obtained by measuring the initial stress by first pressing the elastic sheet under a pressure condition of 2.5 kgf, then immediately compressing it a second time to 40 ㎛, and then maintaining it for 60 seconds after the second compression, and measuring the stress according to Equation 2.
[0229] [Formula 2]
[0230] Stress relaxation rate (%) = (Stress after 60 seconds of 40㎛ compression) / (Initial stress at 40㎛ compression) X 100
[0231] Experimental Example 3: Evaluation of Recovery Rate
[0232] The recovery rate was evaluated for the elastic sheets of Examples 1 to 6 and Comparative Examples 1 to 4.
[0233] The above recovery rate was obtained by first pressurizing the elastic sheet under a pressure condition of 2.5 kgf, then immediately compressing it a second time to 40 ㎛, maintaining it for 60 seconds, and calculating the initial stress at the time of the first pressurization and the stress upon returning to the starting point of the second compression (initial point), according to the above equation 3.
[0234] [Formula 3]
[0235] Recovery rate (%) = (Stress when restored to the initial point after 40㎛ compression) / (Initial stress when 40㎛ compressed) X 100
[0236] The compositions of the elastic sheets of Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 1 below. In Table 1 below, the thickness ratio is the ratio of the thickness of the first layer of acrylic resin: the thickness of (the second layer of urethane resin + the third layer).
[0237] Experimental Example 4) Life Evaluation
[0238] The all-solid-state batteries manufactured according to the above Examples 1 to 6 and Comparative Examples 1 to 4 were placed in a test module and fixed with a force of 5000 gf, and then charged at a constant current of 0.1 C at 45°C to an upper limit voltage of 4.25 V, and then discharged at 0.1 C to an end voltage of 2.5 V to perform initial charge-discharge.
[0239] The battery, which had undergone initial charge and discharge, was subjected to 300 cycles of charge and discharge at 0.33 C in a voltage range of 2.5 V to 4.25 V at 45°C, and the number of cycles at which the ratio of discharge capacity to initial discharge capacity fell below 90% was defined as the lifespan. The results are shown in Table 1 below.
[0240] CFD70 / CFD50 Stress Relaxation Rate (%) Recovery Rate (%) Life (Cycle) Example 1 2.513 / 1.062 = 2.37 10.47 3.3 > 300 Example 2 3.527 / 1.532 = 2.30 9.1% 80.1% > 300 Example 3 3.015 / 1.133 = 2.67 9.0% 80.9% > 300 Example 4 2.059 / 0.918 = 2.24 13.8% 74.2% > 300 Example 5 2.213 / 0.950 = 2.33 12.5% 67.0% > 300 Example 6 4.447 / 1.804 = 2.47 10.4% 73.3% > 300 Comparison Example 13.080 / 1.184=2.601.591.7~100 Comparison Example 21.022 / 0.568=1.811.370.5~190 Comparison Example 312.747 / 2.082=6.1214.872.4~70 Comparison Example 44.911 / 1.119=4.3912.866.4~220
[0241]
[0242] As shown in Table 1 above, it can be seen that the all-solid-state batteries of Examples 1 to 5, which include an acrylic binder, hollow particles, and glass filler, and include an elastic sheet satisfying the conditions of Equation 1, have excellent stress relaxation rate, recovery rate, and lifespan characteristics.
[0243] In this regard, in the case of Comparative Example 1 that does not include hollow particles, the stress relaxation rate is significantly low and the life characteristics are also low, and in the case of Comparative Example 2 that does not include glass bubbles, the stress relaxation rate and recovery rate are low and the life characteristics are not high.
[0244] In addition, it can be seen that comparative examples 3 and 4 using conventional urethane-based elastic sheets exhibit low recovery rate and life characteristics.
[0245] Although the preferred embodiments of the present invention have been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the patent claims, the detailed description of the invention, and the attached drawings, and it is obvious that this also falls within the scope of the present invention.
Claims
1. Contains acrylic binder, hollow particles and glass filler, An elastic sheet for an all-solid-state battery satisfying the following equation 1. [Formula 1] 2≤CFD70 / CFD50≤4 (In the above equation 1, CFD (compression force deflection) 50 is the compressive strength (MPa) measured at the point where the thickness becomes 50% of the thickness of the elastic sheet, CFD70 is the compressive strength (MPa) measured at a point where the thickness is 30% of the thickness of the elastic sheet.
2. In paragraph 1, The above CFD50 is an elastic sheet for an all-solid-state battery having a strength of 0.5 MPa to 4 MPa.
3. In paragraph 1, The above CFD70 is an elastic sheet for an all-solid-state battery having a strength of 2 MPa to 6 MPa.
4. In paragraph 1, An elastic sheet for an all-solid-state battery having a slope of 4 to 30 when the above CFD70 and the above CFD50 are on the y-axis and the elastic sheet strain is on the x-axis.
5. In paragraph 1, An elastic sheet for an all-solid-state battery, wherein the content of the acrylic binder is 85 wt% to 98.5 wt% based on 100 wt% of the total elastic sheet.
6. In paragraph 1, An elastic sheet for an all-solid-state battery, wherein the content of the hollow particles is 0.5 wt% to 5 wt% based on 100 wt% of the entire elastic sheet.
7. In paragraph 1, An elastic sheet for an all-solid-state battery, wherein the content of the glass filler is 1 wt% to 10 wt% based on 100 wt% of the entire elastic sheet.
8. In paragraph 1, The above acrylic binder is an all-solid-state elastic sheet for batteries which is a (meth)acrylic copolymer.
9. In paragraph 8, The above (meth)acrylic copolymer is an elastic sheet for an all-solid-state battery, which is a ternary copolymer comprising a first repeating unit derived from a linear alkyl (meth)acrylate having a glass transition temperature (Tg) of -30°C or lower, a second repeating unit derived from a cyclic alkyl (meth)acrylate having a Tg of 50°C or higher, and a third repeating unit derived from an alkyl (meth)acrylate containing a hydroxyl group.
10. In paragraph 9, An elastic sheet for an all-solid-state battery, wherein the ternary copolymer comprises 10 to 40 wt% of the first repeating unit, 20 to 50 wt% of the second repeating unit, and 10 to 50 wt% of the third repeating unit, based on the total weight of the ternary copolymer.
11. In paragraph 1, The above hollow particles are elastic sheets for all-solid-state batteries that are polymer hollow particles.
12. In paragraph 11, The above polymer is an elastic sheet for an all-solid-state battery, wherein the polymer is polyacrylonitrile, polymethyl methacrylate polymer, silicon-containing polymer, or a combination thereof.
13. In paragraph 1, An elastic sheet for an all-solid-state battery, wherein the size of the hollow particles is 10 μm to 90 μm.
14. In paragraph 1, An elastic sheet for an all-solid-state battery, wherein the size of the above glass filler is 10㎛ to 90㎛.
15. Bipolar; cathode; A solid electrolyte layer positioned between the anode and the cathode; and An elastic sheet according to any one of claims 1 to 14, positioned on the outer side of at least one of the positive and negative electrodes. An all-solid-state battery comprising:
Citation Information
Patent Citations
All solid thin film laminated battery
JP2004273436A
Ultraviolet deodorization sterilization module using uva light and UVC light
KR1020230053800A
Secondary battery having venting part
KR1020230122563A
Antimicrobial oil stain paint composition having fast dry, torsional supression and humidity prevention feature and manufacturing the same, wood material coated with the same
KR102256036B1
Solid-state battery
US20210020995A1