Electrolyte for lithium secondary battery, secondary battery, and electric device

By using a composite interface film formed by sulfate ester and fluorosulfonate ions in lithium secondary batteries, the problem of degradation of performance after circulation of lithium secondary batteries is solved, the DC internal resistance is reduced, and the storage performance is improved, and the use of batteries is extended life.

WO2024243966A1PCT designated stage expired Publication Date: 2024-12-05CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/097821
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

After multiple cycles of existing lithium secondary batteries, the storage performance and circulation performance are significantly reduced, and the DC internal resistance is significantly increased.

Method used

An electrolyte for lithium secondary batteries is used, which includes sulfate ester and fluorosulfonate ions. The molar ratio of sulfate ester and fluorosulfonate ions is (8-223): 1, and by forming a dense composite interface mask, Improve the thermal and mechanical stability of the interface mask, reduce DC internal resistance, and improve storage and cycling performance.

Benefits of technology

It significantly improves the cycle life of lithium secondary batteries, reduces DC internal resistance, improves storage performance and cycle performance, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023097821_05122024_PF_FP_ABST
    Figure CN2023097821_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present application are an electrolyte for a lithium secondary battery, a secondary battery, and an electric device. The electrolyte for a lithium secondary battery comprises sulfate and fluorosulfonate ions, wherein the molar ratio of the sulfate to the fluorosulfonate ions is (8-223) : 1.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte for lithium secondary batteries, secondary batteries and electrical equipment Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to an electrolyte for a lithium secondary battery, a secondary battery, and an electrical device. Background Art

[0002] Secondary batteries are not only used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, but are also widely used in electric vehicles such as electric bicycles, electric motorcycles, electric cars, as well as in military equipment, aerospace and other fields.

[0003] However, after multiple cycles, the storage performance and cycle performance of existing secondary batteries will be significantly reduced, and the DC internal resistance will also be significantly increased.

[0004] Public content

[0005] In view of the technical problems existing in the background technology, the present application provides an electrolyte for lithium secondary batteries, aiming to solve the problem that the storage performance and cycle performance of secondary batteries containing the electrolyte are significantly reduced and the DC internal resistance is significantly increased after multiple cycles.

[0006] In order to achieve the above object, the electrolyte for lithium secondary battery includes sulfate and fluorosulfonate ions, and the molar ratio of the sulfate to the fluorosulfonate ions is (8-223):1.

[0007] The present application includes at least the following beneficial effects: the electrolyte for lithium secondary batteries includes sulfate and fluorosulfonate ions, and the electrolyte for lithium secondary batteries includes sulfate and fluorosulfonate ions in the above-mentioned proportions, and the sulfate and fluorosulfonate ions jointly participate in forming the positive and negative electrode interface film to form a dense composite film, which can improve the thermal stability and mechanical stability of the interface film and play a role in significantly improving the cycle life of the secondary battery; in addition, the formed interface film has strong ionic conductivity, which reduces the DC internal resistance of the secondary battery. In this way, the simultaneous use of sulfate and fluorosulfonate ions can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.

[0008] In some embodiments of the present application, in the lithium secondary battery electrolyte, the molar ratio of the sulfate ester to the fluorosulfonate ion is (10-60):1, and can be optionally (16.7-50):1. This can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.

[0009] In some embodiments of the present application, the molar concentration of the sulfate ester in the lithium secondary battery electrolyte is 0.08 mol / L-0.2 mol / L, and optionally 0.1 mol / L-0.15 mol / L. Thus, the molar concentration of the sulfate ester in the lithium secondary battery electrolyte within the above range can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.

[0010] In some embodiments of the present application, the molar concentration of the fluorosulfonate ion in the lithium secondary battery electrolyte is 0.0009 mol / L-0.009 mol / L, and optionally 0.003 mol / L-0.006 mol / L. Thus, the molar concentration of the fluorosulfonate ion in the lithium secondary battery electrolyte within the above range can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.

[0011] In some embodiments of the present application, the sulfate ester includes at least one of vinyl sulfate, 4-methyl vinyl sulfate, 4-fluorovinyl sulfate, 4-n-propyl vinyl sulfate and 4,4'-disulfate.

[0012] In some embodiments of the present application, the fluorosulfonate ion is the following substance: ASO3F, where A includes at least one of Li, Na, K and H.

[0013] In some embodiments of the present application, the lithium secondary battery electrolyte further includes a positive electrode film-forming additive, whereby the positive electrode film-forming additive can participate in forming an interface film on the positive electrode surface of the secondary battery, thereby improving the storage performance and cycle performance of the secondary battery.

[0014] In some embodiments of the present application, the cathode film-forming additive includes at least one of fluoroethylene carbonate and 1,3-propane sultone. Thus, the cathode film-forming additive, which includes at least one of the aforementioned substances, can participate in film formation on the surface of the secondary battery's cathode, thereby improving the secondary battery's storage performance and cycling performance.

[0015] In some embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate ester and fluorosulfonate ions is (0.05-0.37):1, and can optionally be (0.06-0.3):1. Thus, when the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate ester and fluorosulfonate ions in the lithium secondary battery electrolyte is within the above range, the positive electrode film-forming additive can participate in forming an interface film on the surface of the positive electrode of the secondary battery, thereby improving the storage performance and cycle performance of the secondary battery.

[0016] In some embodiments of the present application, the molar concentration of the positive electrode film-forming additive in the lithium secondary battery electrolyte is 0.01 mol / L-0.03 mol / L. Thus, the concentration of the positive electrode film-forming additive in the lithium secondary battery electrolyte within the above range can participate in the formation of an interface film on the surface of the positive electrode of the secondary battery, thereby improving the storage performance and cycle performance of the secondary battery.

[0017] In some embodiments of the present application, the lithium secondary battery electrolyte further includes difluorophosphate ions. This can alter the solvation structure of the lithium secondary battery electrolyte, allowing more alkali metal ions to participate in film formation and improving the ionic conductivity of the interface film. Furthermore, the difluorophosphate ions, along with the fluorosulfonate ions and sulfate esters, contribute to the formation of the positive and negative electrode interface films, enhancing the thermal stability of the interface films, reducing the DC internal resistance of the secondary battery, and improving the storage and cycling performance of the secondary battery.

[0018] In some embodiments of the present application, the ratio of the molar amount of the difluorophosphate ion to the sum of the molar amounts of the sulfate ester and the fluorosulfonate ion is (0.048-1):1, and can optionally be (0.13-0.58):1. Thus, when the ratio of the molar amount of the difluorophosphate ion to the sum of the molar amounts of the sulfate ester and the fluorosulfonate ion in the lithium secondary battery electrolyte is within the above range, the DC internal resistance of the secondary battery can be reduced and the storage performance and cycle performance of the secondary battery can be improved.

[0019] In some embodiments of the present application, the molar concentration of the difluorophosphate ion is 0.01 mol / L-0.08 mol / L, and optionally 0.02 mol / L-0.06 mol / L. Thus, the molar concentration of the difluorophosphate ion in the lithium secondary battery electrolyte within the above range can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.

[0020] In some embodiments of the present application, the difluorophosphate ion adopts the following substance: MPO2F2, wherein M includes at least one of Li, Na, K and H.

[0021] In some embodiments of the present application, the lithium secondary battery electrolyte further comprises tetrafluoroborate ions. Tetrafluoroborate ions are compatible with the lithium secondary battery electrolyte system and can participate in forming the negative electrode interface film of the secondary battery, opening up ion channels and reducing the DC internal resistance of the secondary battery.

[0022] In some embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of the tetrafluoroborate ion to the sum of the molar amounts of the sulfate and fluorosulfonate ions is (0.0024-0.012):1, and can optionally be (0.0038-0.008):1. Thus, when the ratio of the molar amount of the tetrafluoroborate ion to the sum of the molar amounts of the sulfate and fluorosulfonate ions in the lithium secondary battery electrolyte is within the above range, the electrolyte can participate in forming the negative electrode interface film of the secondary battery, thereby reducing the DC internal resistance of the secondary battery.

[0023] In some embodiments of the present application, the molar concentration of the tetrafluoroborate ion in the lithium secondary battery electrolyte is 0.0005 mol / L-0.001 mol / L, and optionally 0.0006 mol / L-0.0008 mol / L. Thus, the molar concentration of the tetrafluoroborate ion in the lithium secondary battery electrolyte within the above range can participate in forming the negative electrode interface film of the secondary battery, thereby reducing the DC internal resistance of the secondary battery.

[0024] In some embodiments of the present application, the tetrafluoroborate ions are provided by at least one of the following substances: at least one of tetrafluoroboric acid, sodium tetrafluoroborate, potassium tetrafluoroborate and lithium tetrafluoroborate.

[0025] In some embodiments of the present application, the water content of the lithium secondary battery electrolyte is less than or equal to 20 ppm. Therefore, a water content within the above range can reduce water damage to the interfacial membrane, especially at high voltages, thereby improving the storage performance and cycle performance of the secondary battery.

[0026] In some embodiments of the present application, the HF content in the lithium secondary battery electrolyte is less than or equal to 150 ppm. Therefore, the HF content in the lithium secondary battery electrolyte within the above range can reduce HF damage to the interface film, especially at high voltages, thereby improving the storage performance and cycle performance of the secondary battery.

[0027] The second aspect of the present application provides a secondary battery comprising the electrolyte for lithium secondary batteries according to the first aspect of the present application, thereby providing the secondary battery with low DC internal resistance and excellent storage performance and cycle performance.

[0028] In some embodiments of the present application, the secondary battery includes a positive electrode active material, and the positive electrode active material includes Li x Ni (1-y-z) Co y M z O 2-b, wherein M includes at least one of Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.05≤y≤0.8, 0.01≤z≤0.5, 0≤b≤0.2.

[0029] In some embodiments of the present application, the BET specific surface area of ​​the positive electrode active material is less than or equal to 3 m 2 / g, optionally, the BET specific surface area of ​​the positive electrode active material is 1m 2 / g-2.5m 2 / g.

[0030] A third aspect of the present application provides an electrical device, which includes the secondary battery described in the second aspect.

[0031] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become obvious from the description below, or will be learned through practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0033] FIG1 is a schematic structural diagram of a secondary battery according to an embodiment of the present application;

[0034] FIG2 is a schematic structural diagram of a battery module according to an embodiment of the present application;

[0035] FIG3 is a schematic structural diagram of a battery pack according to an embodiment of the present application;

[0036] FIG4 is an exploded view of FIG3 ;

[0037] FIG. 5 is a schematic diagram of an embodiment of an electric device using a secondary battery as a power source.

[0038] Explanation of reference numerals: 1: secondary battery; 2: battery module; 3: battery pack; 4: upper case; 5: lower case. DETAILED DESCRIPTION

[0039] The following embodiments of the technical solution of the present application are described in detail. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only used as examples and are not intended to limit the scope of protection of the present application.

[0040] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0041] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.

[0042] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0044] Secondary batteries are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles such as electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. As the application areas of power secondary batteries continue to expand, their market demand is also growing.

[0045] During the initial charge and discharge process of a secondary battery, the electrode material (such as the negative electrode active material) reacts with the lithium secondary battery electrolyte at the solid-liquid interface, forming a passivation layer covering the surface of the electrode material. This passivation layer is an interfacial film that has the characteristics of a solid electrolyte: an electronic insulator but an excellent conductor of alkali metal ions. Alkali metal ions can freely embed and de-embedding through this passivation layer, hence the name "positive-negative electrode interface film."

[0046] However, existing secondary batteries have the following problems: on the one hand, as the secondary battery is charged and discharged, the interface film at the positive and negative electrode interfaces becomes unstable and easily damaged, and the transmission resistance of alkali metal ions also increases, thereby increasing the DC impedance of the secondary battery and deteriorating the storage performance and cycle performance; on the other hand, when the secondary battery is charged and discharged, under high temperature and high pressure, the positive electrode active material has strong oxidizing properties, which will oxidize the electrolyte for the lithium secondary battery, and the reaction will generate a large amount of gas, causing the loss of the lithium secondary battery electrolyte and the positive electrode active material, affecting the storage performance and cycle performance of the secondary battery.

[0047] In the present application, sulfate and fluorosulfonate ions jointly participate in forming the positive and negative electrode interface film to form a dense composite film, which can improve the thermal stability and mechanical stability of the interface film and play a role in significantly improving the cycle life of the secondary battery; in addition, the formed interface film has strong ionic conductivity, which reduces the DC internal resistance of the secondary battery. In this way, the simultaneous use of sulfate and fluorosulfonate ions can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery. On the other hand, the interface film has thermal stability and mechanical stability, which can reduce the probability of interface film rupture, thereby reducing the reaction between the positive electrode active material and the electrolyte for the lithium secondary battery, inhibiting the gas production of the secondary battery, reducing the loss of the electrolyte for the lithium secondary battery and the positive electrode active material, and improving the storage performance and cycle performance of the secondary battery.

[0048] The positive electrode active material disclosed in the embodiments of the present application is suitable for secondary batteries, and the secondary batteries disclosed in the embodiments of the present application can be used in electrical devices that use secondary batteries as power sources or various energy storage systems that use secondary batteries as energy storage elements. Electrical devices may include but are not limited to mobile phones, tablets, laptops, electric toys, power tools, battery cars, electric cars, ships, spacecraft, and the like. Among them, electric toys may include fixed or mobile electric toys, for example, game consoles, electric car toys, electric ship toys, and electric airplane toys, and the like, and spacecraft may include airplanes, rockets, space shuttles, and spacecraft, and the like.

[0049] In a first aspect, the present application provides an electrolyte for a lithium secondary battery, wherein the electrolyte for a lithium secondary battery comprises sulfate and fluorosulfonate ions, and the molar ratio of the sulfate to the fluorosulfonate ions is (8-223):1.

[0050] The present application includes at least the following beneficial effects: sulfate ester and fluorosulfonate ions are included in the electrolyte for lithium secondary batteries, and the electrolyte for lithium secondary batteries includes sulfate ester and fluorosulfonate ions in the above-mentioned proportion, and the two together participate in forming the positive and negative electrode interface film, forming a composite film, thereby improving the mechanical stability and thermal stability of the interface film; the ionic conductivity of the interface film can also be improved. In this way, the simultaneous use of sulfate ester and fluorosulfonate ions can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.

[0051] Direct current internal resistance (DCR) refers to the resistance to current flow within a battery cell. After a secondary battery's discharge, polarization causes the battery's voltage to rebound. DC impedance technology calculates the battery's internal resistance by measuring the difference between the battery's voltage immediately before the end of intermittent discharge and the voltage after the battery stabilizes.

[0052] In some embodiments of the present application, the sulfate ester may include at least one of vinyl sulfate, 4-methyl-vinyl sulfate, 4-fluorovinyl sulfate, 4-n-propyl vinyl sulfate, and 4,4'-vinyl bisulfate. Thus, by using the above-mentioned sulfate ester in the electrolyte for the lithium secondary battery of the present application, it can participate in the formation of the positive and negative electrode interface film, making the interface film flexible, adapting to the expansion and contraction of the secondary battery pole piece during the cycle, improving the mechanical stability of the interface film, and being able to improve the ion conductivity of the interface film, thereby improving the cycle performance of the secondary battery and reducing the DC internal resistance. In other embodiments of the present application, the sulfate ester includes 4,4'-vinyl bisulfate.

[0053] In some embodiments of the present application, the fluorosulfonate ions are in the form of ASO3F, where A comprises at least one of Li, Na, K, and H. Specifically, the fluorosulfonate ion-containing substance can provide fluorosulfonate ions. The interface formed by the fluorosulfonate ions is very dense and has good thermal stability, thereby reducing the DC impedance of the secondary battery while improving the storage performance of the secondary battery.

[0054] In some embodiments of the present application, the molar ratio of sulfate to fluorosulfonate ion can be (8.9-222):1, (10-200):1, (20-190):1, (30-180):1, (40-170):1, (50-160):1, (60-150):1, (70-140):1, (80-130):1, (90-120):1, (100-110):1, etc. In other embodiments of the present application, in lithium secondary batteries, In the electrolyte, the molar ratio of the sulfate to the fluorosulfonate ion is (10-60):1, for example (16.7-50):1. Specifically, the molar ratio of the sulfate to the fluorosulfonate ion is within the above range, which can reduce the reduction in thermal stability of the interface film caused by excessive sulfate, thereby improving the storage performance of the secondary battery. It can also reduce the defects of insufficient interface film formation and poor ion conductivity caused by too little sulfate, reduce the DC internal resistance of the secondary battery, and improve the storage performance and cycle performance of the secondary battery.

[0055] In some embodiments of the present application, in the electrolyte for lithium secondary batteries, the molar concentration of the sulfate ester is 0.08mol / L-0.2mol / L. For example, in the electrolyte for lithium secondary batteries, the molar concentration of the sulfate ester can be 0.04mol / L-0.18mol / L, 0.09mol / L-0.17mol / L, 0.1mol / L-0.16mol / L, 0.11mol / L-0.15mol / L, 0.12mol / L-0.14mol / L, etc. Therefore, the molar concentration of sulfate ester in the electrolyte for lithium secondary batteries is within the above range, which can reduce the thermal stability of the interface film caused by excessive sulfate ester, thereby improving the storage performance of the secondary battery, and can also reduce the defects of insufficient interface film formation and poor ion conductivity caused by too little sulfate ester, reduce the DC internal resistance of the secondary battery, and improve the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, in the electrolyte for lithium secondary batteries, the molar concentration of the sulfate ester is 0.1 mol / L-0.15 mol / L.

[0056] In some embodiments of the present application, the molar concentration of the fluorosulfonate ions in the lithium secondary battery electrolyte is 0.0009 mol / L-0.009 mol / L. For example, the molar concentration of the fluorosulfonate ions in the lithium secondary battery electrolyte can be 0.001 mol / L-0.009 mol / L, 0.002 mol / L-0.008 mol / L, 0.003 mol / L-0.007 mol / L, 0.004 mol / L-0.006 mol / L, etc. Specifically, the molar concentration of the fluorosulfonate ions in the lithium secondary battery electrolyte within the above range can reduce the problem of increased viscosity of the lithium secondary battery electrolyte caused by the addition of substances containing fluorosulfonate ions, thereby reducing the DC internal resistance of the secondary battery, while also being sufficient to improve the thermal stability of the interface film and enhance the storage performance of the secondary battery. In other embodiments of the present application, in the electrolyte for lithium secondary batteries, the molar concentration of fluorosulfonate ions is 0.003 mol / L-0.006 mol / L.

[0057] In some embodiments of the present application, the lithium secondary battery electrolyte further includes a positive electrode film-forming additive. Specifically, the positive electrode film-forming additive can participate in forming a stable positive electrode interface film, reduce the DC impedance of the secondary battery, and improve the cycle performance of the secondary battery.

[0058] In some embodiments of the present application, the cathode film-forming additive includes at least one of fluoroethylene carbonate and 1,3-propane sultone. Specifically, the cathode interface film formed with fluoroethylene carbonate and 1,3-propane sultone exhibits excellent performance, forming a tight interface film without increasing impedance. This interface film can prevent decomposition of the lithium secondary battery electrolyte, reduce the secondary battery's DC internal resistance, and improve the secondary battery's storage and cycling performance.

[0059] In some embodiments of the present application, in the electrolyte for the lithium secondary battery, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate and fluorosulfonate ions is (0.05-0.37):1. For example, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate and fluorosulfonate ions can be (0.05-0.36):1, (0.08-0.35):1, (0.1-0.33):1, (0.12-0.3):1, (0.15-0.29):1, (0.13-0.25):1, (0.15-0.22):1, (0.17-0.2):1, etc. Thus, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of sulfate and fluorosulfonate ions in the lithium secondary battery electrolyte is within the above range, which not only reduces the effect of the excessive amount of the positive electrode film-forming additive on the sulfate and fluorosulfonate ions, thereby increasing the DC impedance of the secondary battery, but also reduces the inability of the positive electrode film-forming additive to participate in the formation of the positive electrode interface film due to the insufficient amount of the positive electrode film-forming additive, thereby reducing the DC internal resistance of the secondary battery and improving the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of sulfate and fluorosulfonate ions is (0.06-0.3):1.

[0060] In some embodiments of the present application, in the electrolyte for lithium secondary batteries, the molar concentration of the positive electrode film-forming additive is 0.01mol / L-0.03mol / L. For example, in the electrolyte for lithium secondary batteries, the molar concentration of the positive electrode film-forming additive may be 0.01mol / L-0.025mol / L, 0.013mol / L-0.024mol / L, 0.015mol / L-0.023mol / L, 0.018mol / L-0.02mol / L, etc. Thus, the concentration of the positive electrode film-forming additive in the electrolyte for lithium secondary batteries is within the above range, which not only reduces the increase in the DC impedance of the secondary battery caused by an excessive amount of the positive electrode film-forming additive, but also reduces the inability of the positive electrode film-forming additive to participate in the formation of the positive electrode interface film due to an insufficient amount of the positive electrode film-forming additive, thereby reducing the DC internal resistance of the secondary battery and improving the storage performance and cycle performance of the secondary battery.

[0061] In some embodiments of the present application, the lithium secondary battery electrolyte further comprises difluorophosphate ions. The difluorophosphate ions can change the solvation structure of the lithium secondary battery electrolyte, allowing more alkali metal ions to participate in film formation, improving the ionic conductivity of the interface film and the transport resistance of the alkali metal ions. Furthermore, the difluorophosphate ions can participate in the formation of the positive and negative electrode interface films, enhancing the thermal stability of the interface films, thereby reducing the DC impedance of the secondary battery while improving the storage performance of the secondary battery.

[0062] In some embodiments of the present application, in the electrolyte for lithium secondary batteries, the ratio of the molar amount of the difluorophosphate ion to the sum of the molar amounts of the sulfate and fluorosulfonate ions is (0.048-1):1. For example, in the electrolyte for lithium secondary batteries, the ratio of the molar amount of the difluorophosphate ion to the sum of the molar amounts of the sulfate and fluorosulfonate ions can be (0.048-0.95):1, (0.05-0.9):1, (0.1-0.8):1, (0.2-0.7):1, (0.3-0.6):1, (0.4-0.5):1, etc. Specifically, the ratio of the molar amount of difluorophosphate ions to the sum of the molar amounts of sulfate and fluorosulfonate ions in the lithium secondary battery electrolyte is within the above range, which can change the solvation structure of the lithium secondary battery electrolyte, allowing more alkali metal ions to participate in film formation, improving the ionic conductivity of the interface film, and improving the transmission resistance of alkali metal ions. In addition, difluorophosphate ions can also participate in the formation of the positive and negative electrode interface films, improving the thermal stability of the interface film, thereby reducing the DC impedance of the secondary battery while improving the storage performance of the secondary battery. In other embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of difluorophosphate ions to the sum of the molar amounts of sulfate and fluorosulfonate ions is (0.13-0.58):1.

[0063] In some embodiments of the present application, in the lithium secondary battery electrolyte, the molar concentration of the difluorophosphate ion is 0.01mol / L-0.08mol / L. For example, in the lithium secondary battery electrolyte, the molar concentration of the difluorophosphate ion is 0.01mol / L-0.07mol / L, 0.02mol / L-0.06mol / L, 0.03mol / L-0.05mol / L, 0.04mol / L-0.05mol / L, etc. Specifically, the concentration of the difluorophosphate ion in the lithium secondary battery electrolyte is within the above range, which can reduce the effect of excessive addition of difluorophosphate ions on the fluorosulfonate ions and sulfate esters, and is sufficient to allow the difluorophosphate ions to play a role, thereby reducing the DC internal resistance of the secondary battery and improving the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, in the lithium secondary battery electrolyte, the molar concentration of the difluorophosphate ion is 0.02mol / L-0.06mol / L.

[0064] In some embodiments of the present application, the difluorophosphate ion is in the form of the following substance: MPO2F2, wherein M comprises at least one of Li, Na, K, and H. Specifically, the above-mentioned substance containing difluorophosphate ions can provide difluorophosphate ions, change the solvation structure of the electrolyte for lithium secondary batteries, allow more alkali metal ions to participate in film formation, improve the ionic conductivity of the interface film, and improve the transmission resistance of alkali metal ions. In addition, the difluorophosphate ions can also participate in the formation of the positive and negative electrode interface film, enhance the thermal stability of the interface film, thereby reducing the DC impedance of the secondary battery while improving the storage performance of the secondary battery.

[0065] In some embodiments of the present application, the lithium secondary battery electrolyte further includes tetrafluoroborate ions. Tetrafluoroborate ions are compatible with the lithium secondary battery electrolyte system and can participate in forming the negative electrode interface film of the secondary battery, opening up ion channels and reducing the DC internal resistance of the secondary battery.

[0066] In some embodiments of the present application, the substance containing the tetrafluoroborate ion may be at least one of tetrafluoroboric acid, sodium tetrafluoroborate, potassium tetrafluoroborate and lithium tetrafluoroborate.

[0067] In some embodiments of the present application, in the electrolyte for the lithium secondary battery, the ratio of the molar amount of the tetrafluoroborate ion to the sum of the molar amounts of the sulfate and fluorosulfonate ions is (0.0024-0.012):1, for example, the ratio of the molar amount of the tetrafluoroborate ion to the sum of the molar amounts of the sulfate and fluorosulfonate ions can be (0.0024-0.011):1, (0.003-0.01):1, (0.004-0.009):1, (0.005-0.008):1, (0.006-0.007):1, etc. Thus, the ratio of the molar amount of tetrafluoroborate ions to the molar amount of sulfate and fluorosulfonate ions in the lithium secondary battery electrolyte is within the above range, which not only reduces the effect of excessive tetrafluoroborate ions on sulfate and fluorosulfonate ions, thereby increasing the DC impedance of the secondary battery, but also reduces the effect of too little tetrafluoroborate ions on the formation of the negative electrode interface film, thereby reducing the DC internal resistance of the secondary battery and improving the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, in the lithium secondary battery electrolyte, the ratio of the molar amount of tetrafluoroborate ions to the molar amount of sulfate and fluorosulfonate ions is (0.0038-0.008):1.

[0068] In some embodiments of the present application, the molar concentration of the tetrafluoroborate ions in the lithium secondary battery electrolyte is 0.0005mol / L-0.001mol / L. For example, the molar concentration of the tetrafluoroborate ions in the lithium secondary battery electrolyte can be 0.0005mol / L-0.0009mol / L, 0.0006mol / L-0.0008mol / L, 0.0007mol / L-0.0008mol / L, etc. Thus, the molar concentration of the tetrafluoroborate ions in the lithium secondary battery electrolyte is within the above range, which reduces the deterioration of the DC impedance of the secondary battery caused by excessive tetrafluoroborate ions. At the same time, the tetrafluoroborate ions can play a role in participating in the formation of the negative electrode interface film, thereby reducing the DC internal resistance of the secondary battery and improving the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, in the electrolyte for lithium secondary batteries, the molar concentration of tetrafluoroborate ions is 0.0006 mol / L-0.0008 mol / L.

[0069] In some embodiments of the present application, the water content in the lithium secondary battery electrolyte is less than or equal to 20 ppm. For example, the water content in the lithium secondary battery electrolyte may be 1 ppm-19 ppm, 2 ppm-18 ppm, 3 ppm-17 ppm, 4 ppm-16 ppm, 5 ppm-15 ppm, 6 ppm-14 ppm, 7 ppm-13 ppm, 8 ppm-12 ppm, 9 ppm-11 ppm, etc. Therefore, when the water content in the lithium secondary battery electrolyte is within the above range, it is possible to reduce water damage to the secondary battery interface membrane, especially at high voltage, thereby reducing the DC internal resistance of the secondary battery and improving the storage performance and cycle performance of the secondary battery.

[0070] In some embodiments of the present application, the HF content in the lithium secondary battery electrolyte is less than or equal to 150 ppm. For example, the HF content in the lithium secondary battery electrolyte can be 10 ppm-140 ppm, 20 ppm-130 ppm, 30 ppm-120 ppm, 40 ppm-110 ppm, 50 ppm-100 ppm, 60 ppm-90 ppm, 70 ppm-80 ppm, etc. Therefore, when the HF content in the lithium secondary battery electrolyte is within the above range, it can reduce HF damage to the secondary battery interface film, especially at high voltage. This can reduce the DC internal resistance of the secondary battery and improve the storage performance and cycle performance of the secondary battery.

[0071] It is understandable that the control of the water content and HF content in the lithium secondary battery electrolyte can be achieved by using molecular sieves to remove water and HF. Specifically, molecular sieves can be added to the lithium secondary battery electrolyte to ensure that the molecular sieves and the lithium secondary battery electrolyte are in full contact, so as to adsorb water and HF in the lithium secondary battery electrolyte, and then the molecular sieves and the lithium secondary battery electrolyte can be separated by filtration, centrifugation, etc.

[0072] It is understood that the water content and HF content in the electrolyte for lithium secondary batteries can be measured by the following method:

[0073] Water content test: inject the electrolyte for lithium secondary battery into the electrolytic cell that has reached equilibrium, and after the indicator electrode detects H2O, electrode oxidation occurs. - I2 is a quantitative chemical reaction between I2 and H2O, so the water content is calculated. According to HG / T4067-2015 Determination of Water in Hexafluorophosphate Electrolyte 5.9, the quantitative reaction formula of I2 and H2O is: H2O+I2+SO2+3C5H5N=2C5H5N·HI+C5H5N·SO3. The amount of water is calculated by the amount of iodine consumed.

[0074] Test of hydrofluoric acid content: In a dry environment, titrate the free acid in the electrolyte with a standard triethylamine solution and calculate the HF content;

[0075] HG / T4067-2015 Lithium hexafluorophosphate electrolyte 5.10 Determination of free acid content;

[0076] HF(ppm)=(V2-V1) / 1000×C×20 / m×1000000=(V2-V1)×C / m×20000;

[0077] Where: 0.01——concentration of standard solution, 0.02mol / L;

[0078] V1 - the volume reading of the burette before starting the titration, ml;

[0079] V2——The volume reading of the burette after adding the electrolyte sample and titrating to the endpoint, ml;

[0080] 20 – molar molecular weight of HF, g / mol;

[0081] m——the amount of electrolyte weighed, g;

[0082] 20000——The coefficient for conversion to ug / g.

[0083] In some embodiments of the present application, the electrolyte for a lithium secondary battery may further include an electrolyte salt and a solvent.

[0084] When the secondary battery is a lithium ion battery, as an example, the electrolyte salt may include at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0085] As an example, the solvent may include at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0086] In some embodiments, the electrolyte for lithium secondary batteries may further include additives. For example, the additives may include additives that can improve certain properties of the secondary battery, such as additives that improve the overcharge performance of the secondary battery, additives that improve the high temperature performance of the secondary battery, and additives that improve the low temperature performance of the secondary battery.

[0087] The second aspect of the present application provides a secondary battery comprising the electrolyte for lithium secondary batteries according to the first aspect of the present application, thereby providing the secondary battery with low DC internal resistance, excellent storage performance and cycle performance.

[0088] A secondary battery is a battery that can be recharged after discharge to activate the active materials and continue to be used.

[0089] Typically, a secondary battery consists of a positive electrode, a negative electrode, a separator, and an electrolyte. During the charge and discharge process, active ions (alkali metal ions) are inserted and removed between the positive and negative electrodes. The separator is placed between the positive and negative electrodes to isolate them. The electrolyte conducts ions between the positive and negative electrodes.

[0090] In some embodiments of the present application, the secondary battery may be a lithium-ion battery.

[0091] [Positive electrode]

[0092] In a secondary battery, the positive electrode sheet generally includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material.

[0093] The positive electrode current collector may be a conventional metal foil or a composite current collector (a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the positive electrode current collector may be an aluminum foil.

[0094] The specific type of the positive electrode active material is not limited, and any active material known in the art that can be used for the positive electrode of a secondary battery can be used. Those skilled in the art can select it according to actual needs.

[0095] For example, when the secondary battery is a lithium-ion battery, as an example, the positive electrode active material may include, but is not limited to, at least one of a lithium transition metal oxide, an olivine-structured lithium-containing phosphate, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their modified compounds. These materials can all be obtained through commercial channels.

[0096] In some embodiments of the present application, the positive electrode active material includes Li x Ni (1-y-z) Co y M z O 2-b , wherein M includes at least one of Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.05≤y≤0.8, 0.01≤z≤0.5, 0≤b≤0.2.

[0097] For example, x can satisfy: 0.2≤x≤1.2, 0.4≤x≤1.1, 0.5≤x≤1.0, 0.6≤x≤0.9, 0.7≤x≤0.8, etc.; y can satisfy: 0.05≤y≤0.7, 0.1≤y≤0.6, 0.2≤y≤0.5, 0.3≤y≤0.4, etc.; z can satisfy: 0.01≤z≤0.45, 0.1≤z≤0.4, 0.2≤z≤0.3, etc.; b can satisfy: 0≤b≤0.15, 0.02≤b≤0.13, 0.05≤b≤0.1, 0.07≤b≤0.09, etc.

[0098] It should be noted that in the positive electrode sheet, secondary battery, or electrical device, lithium ions are consumed during the formation and cycling of the secondary battery, resulting in the measured lithium content x in the positive electrode active material being less than 1. Furthermore, if a lithium supplement is used in the positive and negative electrode sheets, the measured lithium content x in the positive electrode active material may be greater than 1 after the secondary battery undergoes formation and cycling.

[0099] In addition, as the secondary battery undergoes processes such as formation and cycling, the positive electrode active material may release oxygen from the lattice, causing oxygen loss. Therefore, the oxygen content in the positive electrode active material may be less than 2.

[0100] In some embodiments of the present application, the BET specific surface area of ​​the positive electrode active material is less than or equal to 3 m 2 / g, for example, the BET specific surface area of ​​the positive electrode active material can be 0.3 m 2 / g-3m 2 / g,1m 2 / g-2.5m 2 / g,1.2m 2 / g-2.3m 2 / g,1.5m 2 / g-2m 2 / g, etc. Specifically, the BET specific surface area of ​​the positive electrode active material is within the above range, which can reduce the side reaction of the positive electrode active material under high voltage and improve the storage performance and cycle performance of the secondary battery. In other embodiments of the present application, the BET specific surface area of ​​the positive electrode active material is 1m 2 / g-2.5m 2 / g.

[0101] It can be understood that the BET specific surface area of ​​the positive electrode active material can be tested by referring to the following method: using the American Microelectronics multi-station fully automatic BET specific surface area and pore analyzer GeminiVII2390, take about 7g of sample and put it into a 9cc long tube with a bulb, degas at 200℃ for 2h, and then put it into the main unit for testing to obtain the BET (specific surface area) data of the positive electrode active material.

[0102] The positive electrode active material layer may also optionally include a binder, a conductive agent, and other optional auxiliary agents.

[0103] As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene, and carbon nanofibers.

[0104] As an example, the binder may include at least one of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), and polyvinyl butyral (PVB).

[0105] [Negative electrode]

[0106] In a secondary battery, the negative electrode sheet generally includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.

[0107] The negative electrode current collector may be a conventional metal foil or a composite current collector (for example, a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the negative electrode current collector may be a copper foil.

[0108] The specific type of the negative electrode active material is not limited, and active materials that can be used for the negative electrode of a secondary battery known in the art can be used, and those skilled in the art can make a choice according to actual needs. As an example, the negative electrode active material may include but is not limited to at least one of artificial graphite, natural graphite, hard carbon, soft carbon, silicon-based materials and tin-based materials. The silicon-based material may include at least one of elemental silicon, silicon oxide (such as silicon monoxide), silicon-carbon composite, silicon-nitrogen composite, and silicon alloy. The tin-based material may include at least one of elemental tin, tin oxide, and tin alloy. These materials can all be obtained commercially.

[0109] In some embodiments, to further improve the energy density of the secondary battery, the negative electrode active material may include a silicon-based material.

[0110] The negative electrode active material layer may also optionally include a binder, a conductive agent, and other optional auxiliary agents.

[0111] As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0112] As an example, the binder may include at least one of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA), and polyvinyl butyral (PVB).

[0113] As examples, other optional additives may include thickening and dispersing agents (eg, sodium carboxymethyl cellulose CMC-Na), and PTC thermistor materials.

[0114] As the above-mentioned isolation membrane, the present application has no special restrictions and any known porous structure isolation membrane with electrochemical stability and mechanical stability can be selected according to actual needs. For example, it can include a single-layer or multi-layer film containing at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride.

[0115] The embodiment of the present application has no particular limitation on the shape of the secondary battery, which can be cylindrical, square, or any other shape. FIG1 shows a secondary battery 1 with a square structure as an example.

[0116] In some embodiments, the secondary battery may include an outer packaging for encapsulating the positive electrode sheet, the negative electrode sheet, and the electrolyte.

[0117] In some embodiments, the outer packaging may include a housing and a cover. The housing may include a bottom plate and side plates connected to the bottom plate, with the bottom plate and side plates enclosing a receiving cavity. The housing may have an opening communicating with the receiving cavity, and the cover may be positioned over the opening to seal the receiving cavity.

[0118] The positive electrode sheet, negative electrode sheet, and separator can be wound or laminated to form an electrode assembly. The electrode assembly is encapsulated in the housing. The number of electrode assemblies in a secondary battery can be one or more, and can be adjusted according to demand.

[0119] In some embodiments, the outer package of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell.

[0120] The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0121] In some embodiments, secondary batteries may be assembled into a battery module. The battery module may contain multiple secondary batteries, and the specific number may be adjusted according to the application and capacity of the battery module.

[0122] Figure 2 shows an example battery module 2. Referring to Figure 2 , within the battery module 2, multiple secondary batteries 1 may be arranged sequentially along the length of the battery module 2. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 1 may be secured together using fasteners.

[0123] The battery module 2 may further include a housing having a housing space, wherein the housing space accommodates a plurality of secondary batteries 1. In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0124] Figures 3 and 4 illustrate an example battery pack 3. Referring to Figures 3 and 4 , the battery pack 3 may include a battery box and multiple battery modules 2 disposed within the battery box. The battery box comprises an upper case 4 and a lower case 5. The upper case 4 can be placed over the lower case 5 to form an enclosed space for accommodating the battery modules 2. The multiple battery modules 2 can be arranged in any manner within the battery box.

[0125] In a third aspect, the present application provides an electrical device comprising the secondary battery described in the second aspect. Specifically, the secondary battery can serve as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks), electric trains, ships, satellites, and energy storage systems.

[0126] FIG5 shows an example of an electric device, which includes a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.

[0127] As another example, electric devices may include mobile phones, tablet computers, and laptop computers. These electric devices are generally required to be lightweight and thin, and may use secondary batteries as power sources.

[0128] In order to make the technical problems, technical solutions and beneficial effects solved by the embodiments of the present application clearer, the following will be further described in detail with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0129] Example 1

[0130] Preparation of secondary battery containing electrolyte for lithium secondary battery

[0131] 1. Preparation of electrolyte for lithium secondary batteries

[0132] Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of 30:70 to obtain an organic solvent, and fully dried electrolyte salt LiPF6, sulfate, lithium fluorosulfonate, positive electrode film-forming additive, lithium difluorophosphate and lithium tetrafluoroborate are dissolved in the above solvent, and the mixture is evenly mixed to obtain an electrolyte for lithium secondary batteries.

[0133] Molecular sieves are added to the electrolyte for lithium secondary batteries to fully contact the molecular sieves and the electrolyte for lithium secondary batteries to adsorb water and HF in the electrolyte for lithium secondary batteries. The molecular sieves and the electrolyte for lithium secondary batteries are then filtered to separate the molecular sieves and remove water and HF in the electrolyte for lithium secondary batteries.

[0134] 2. Preparation of secondary batteries

[0135] Preparation of positive electrode

[0136] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), conductive agent carbon black (Super P), and binder polyvinylidene fluoride (PVDF) are mixed evenly in an appropriate amount of solvent N-methylpyrrolidone (NMP) in a mass ratio of 96.2:2.7:1.1 to obtain a positive electrode slurry. The positive electrode slurry is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained through drying, cold pressing, slitting, and cutting processes.

[0137] Preparation of negative electrode sheet

[0138] The negative electrode active material artificial graphite, conductive agent carbon black (Super P), binder styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC-Na) are mixed evenly in a proper amount of solvent deionized water at a mass ratio of 96.4:0.7:1.8:1.1 to obtain a negative electrode slurry. The negative electrode slurry is coated on the negative electrode current collector copper foil, and the negative electrode sheet is obtained through the processes of drying, cold pressing, slitting and cutting.

[0139] The isolation film is made of polyethylene film.

[0140] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation, and then wound to obtain an electrode assembly; the electrode assembly is placed in an outer package, and the above-mentioned lithium secondary battery electrolyte is injected into the dried secondary battery. After vacuum packaging, standing, formation, and shaping processes, a secondary battery is obtained.

[0141] The secondary batteries of Examples 2-49 and Comparative Examples 1-2 are the same as those of Example 1 except for the different parameters (see Table 1).

[0142] The compositions of the gel polymer electrolytes in the secondary batteries of Examples 1-49 and Comparative Examples 1-2 of the present application are shown in Table 1.

[0143] Table 1

[0144] In Table 1, “ / ” indicates that the corresponding substance was not added or the added amount was 0.

[0145] Secondary battery performance test:

[0146] 1. Secondary battery capacity and cycle performance

[0147] Taking Example 1 as an example, at 25°C, the secondary battery was charged at a constant current rate of 0.5C to a charge cutoff voltage of 4.2V. It was then charged at a constant voltage to a current of ≤0.05C and allowed to stand for 5 minutes. The battery was then discharged at a constant current rate of 0.33C to a discharge cutoff voltage of 2.8V and allowed to stand for 5 minutes. The discharge capacity (C0) of the secondary battery at this point was recorded as the initial capacity of the secondary battery. This method was used to cycle the secondary battery 200 times. The discharge capacity after 200 cycles was recorded as C1, which was the capacity of the secondary battery after 200 cycles.

[0148] Cycle capacity retention rate of secondary battery = C1 / C0×100%

[0149] The testing process of the capacity of the secondary batteries of Example 2-49 and Comparative Example 1-2 is the same as above.

[0150] 2. Secondary battery DC internal resistance

[0151] Taking Example 1 as an example, the secondary battery is charged to 4.15V at a constant current of 1C at 25°C, then charged at a constant voltage of 4.15V until the current drops to 0.05C, and then discharged to 2.5V at a constant current of 1C. After that, it is left for 5 minutes (stabilization time) and the next cycle is continued. In each cycle, the secondary battery voltage before discharge termination and the secondary battery voltage after stabilization are recorded, and then the DC impedance R = ΔU / I (wherein: ΔU is the voltage difference, R is the DC resistance, and I is the discharge current) is calculated using the following formula.

[0152] Secondary battery internal resistance growth rate = (secondary battery internal resistance after 200 cycles - secondary battery initial internal resistance) / secondary battery initial internal resistance × 100%

[0153] The testing process of the DC internal resistance of the secondary batteries of Example 2-49 and Comparative Example 1-2 is the same as above.

[0154] The performance test results of the secondary batteries of various embodiments and comparative examples are shown in Table 2.

[0155] Table 2

[0156] As can be seen from Table 2, in Examples 1-49 of the present application, sulfate and fluorosulfonate ions were added to the lithium secondary battery electrolyte, and the lithium secondary battery electrolyte included sulfate and fluorosulfonate ions in the aforementioned ratios. Their simultaneous use reduced the DC internal resistance of the secondary battery and improved its storage and cycling performance. Compared to Examples 1-49, the molar ratios of sulfate to fluorosulfonate ions in Comparative Examples 1 and 2 were outside the scope of this application, resulting in significantly reduced storage and cycling performance of the secondary battery and a significant increase in DC internal resistance.

[0157] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. An electrolyte for a lithium secondary battery, in, The electrolyte for lithium secondary batteries includes sulfate and fluorosulfonate ions, and the molar ratio of the sulfate to the fluorosulfonate ions is (8-223):

1.

2. The electrolyte for lithium secondary battery according to claim 1, in, The molar ratio of the sulfate ester to the fluorosulfonate ion is (10-60):1, and can be optionally (16.7-50):

1.

3. The electrolyte for lithium secondary battery according to claim 1 or 2, in, In the electrolyte for lithium secondary batteries, the molar concentration of the sulfate ester is 0.08 mol / L-0.2 mol / L, and can be optionally 0.1 mol / L-0.15 mol / L.

4. The electrolyte for lithium secondary battery according to any one of claims 1 to 3, in, In the electrolyte for lithium secondary batteries, the molar concentration of the fluorosulfonate ions is 0.0009 mol / L-0.009 mol / L, and can be optionally 0.003 mol / L-0.006 mol / L.

5. The electrolyte for lithium secondary battery according to any one of claims 1 to 4, in, The sulfate ester includes at least one of vinyl sulfate, 4-methyl-vinyl sulfate, 4-fluorovinyl sulfate, 4-n-propyl vinyl sulfate and 4,4'-bisulfate.

6. The electrolyte for lithium secondary battery according to any one of claims 1 to 5, in, The fluorosulfonate ion is the following: ASO 3 F, A includes at least one of Li, Na, K and H.

7. The electrolyte for lithium secondary battery according to any one of claims 1 to 6, in, The electrolyte for lithium secondary batteries further includes a positive electrode film-forming additive.

8. The electrolyte for lithium secondary battery according to claim 7, in, The positive electrode film-forming additive includes at least one of fluoroethylene carbonate and 1,3-propane sultone.

9. The electrolyte for lithium secondary battery according to claim 7 or 8, in, In the electrolyte for lithium secondary batteries, the ratio of the molar amount of the positive electrode film-forming additive to the sum of the molar amounts of the sulfate ester and the fluorosulfonate ion is (0.05-0.37):1, and can be optionally (0.06-0.3):

1.

10. The electrolyte for lithium secondary battery according to any one of claims 7 to 9, in, In the electrolyte for lithium secondary batteries, the molar concentration of the positive electrode film-forming additive is 0.01 mol / L-0.03 mol / L.

11. The electrolyte for lithium secondary battery according to any one of claims 1 to 10, in, The electrolyte for lithium secondary batteries further includes difluorophosphate ions.

12. The electrolyte for lithium secondary battery according to claim 11, in, In the electrolyte for lithium secondary batteries, the ratio of the molar amount of the difluorophosphate ions to the sum of the molar amounts of the sulfate ester and the fluorosulfonate ions is (0.048-1):1, and can be optionally (0.13-0.58):

1.

13. The electrolyte for lithium secondary battery according to claim 11 or 12, in, In the electrolyte for lithium secondary batteries, the molar concentration of difluorophosphate ions is 0.01 mol / L-0.08 mol / L, and can be optionally 0.02 mol / L-0.06 mol / L.

14. The electrolyte for lithium secondary battery according to any one of claims 11 to 13, in, The difluorophosphate ion adopts the following substances: MPO 2 F 2 , wherein M includes at least one of Li, Na, K and H.

15. The electrolyte for lithium secondary battery according to any one of claims 1 to 14, in, The electrolyte for lithium secondary batteries also includes tetrafluoroborate ions.

16. The electrolyte for lithium secondary battery according to claim 15, in, In the electrolyte for lithium secondary batteries, the ratio of the molar amount of the tetrafluoroborate ions to the sum of the molar amounts of the sulfate and fluorosulfonate ions is (0.0024-0.012):1, and can be optionally (0.0038-0.008):

1.

17. The electrolyte for lithium secondary battery according to claim 15 or 16, in, In the electrolyte for lithium secondary batteries, the molar concentration of tetrafluoroborate ions is 0.0005 mol / L-0.001 mol / L, and can be optionally 0.0006 mol / L-0.0008 mol / L.

18. The electrolyte for lithium secondary battery according to any one of claims 15 to 17, in, The tetrafluoroborate ions are provided by at least one of the following substances: at least one of tetrafluoroboric acid, sodium tetrafluoroborate, potassium tetrafluoroborate and lithium tetrafluoroborate.

19. The electrolyte for lithium secondary battery according to any one of claims 1 to 18, in, The lithium secondary battery electrolyte satisfies at least one of the following conditions: The water content of the electrolyte for lithium secondary battery is less than or equal to 20 ppm; The HF content in the electrolyte for lithium secondary batteries is less than or equal to 150 ppm.

20. A secondary battery, in, The secondary battery comprises the electrolyte for a lithium secondary battery according to any one of claims 1 to 19.

21. The secondary battery according to claim 20, in, The secondary battery includes a positive electrode active material, wherein the positive electrode active material includes Li x Ni (1-y-z) Co y M z O 2-b , wherein M includes at least one of Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.05≤y≤0.8, 0.01≤z≤0.5, 0≤b≤0.

2.

22. The secondary battery according to claim 21, in, The BET specific surface area of ​​the positive electrode active material is less than or equal to 3 m 2 / g, optionally, the BET specific surface area of ​​the positive electrode active material is 1m 2 / g-2.5m 2 / g.

23. An electrical device, in, A secondary battery comprising the secondary battery according to any one of claims 20 to 22.

Citation Information

Patent Citations

  • High-voltage electrolyte and lithium ion battery based on same

    CN111883839A

  • Electrolyte and lithium ion battery

    CN112736285A

  • Secondary battery, method for manufacturing secondary battery, battery module, battery pack, and power device

    CN116111177A

  • Nonaqueous electrolyte secondary battery module

    JP2011082033A