Preparation method for tetrafluoro oxalate phosphate, and system and use, electrolyte and secondary battery

By reacting bioxalate and phosphorus pentafluoride in an inert organic solvent and combining with chlorosilane to isolate tetrafluorooxalate phosphate, the problem of low solvent and product recycling rate in the prior art is solved, and high purity is achieved and efficient preparation of tetrafluorooxalic acid phosphate, improving its application performance in secondary battery electrolytes.

WO2024244169A1PCT designated stage expired Publication Date: 2024-12-05GUANGZHOU TINCI MATERIALS TECH +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/112978
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2023-08-14
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

In the preparation of tetrafluorooxalic acid phosphate, it is difficult to efficiently recover solvents and products, resulting in high free acid and by-product residues, limiting its application in secondary battery electrolytes.

Method used

Bioxalate and phosphorus pentafluoride react in an inert organic solvent, followed by reaction with chlorosilane, separating tetrafluorooxalic acid phosphate and volatile by-products, and achieving high purity of tetrafluorooxalic acid phosphate by crystallization or other methods Extract and reuse the residual crystallization solvent into the production system.

Benefits of technology

It significantly improves the yield and product purity of tetrafluorooxalic acid phosphate, simplifies the post-treatment process, reduces the acidity and chloride ions residues, and improves the quality of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023112978_05122024_PF_FP_ABST
    Figure CN2023112978_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present application belongs to the field of new energy. Disclosed is a preparation method for a tetrafluoro oxalate phosphate for a secondary battery electrolyte. The preparation method comprises the following steps: step 1, by using a dioxalate and phosphorus pentafluoride as raw materials, performing a reaction in an inert organic solvent to obtain a solution containing an intermediate product; step 2, reacting the solution containing the intermediate product with chlorosilane to obtain a solution containing tetrafluoro oxalate phosphate and volatile by-products; and step 3, separating out the tetrafluoro oxalate phosphate from the solution. In addition to the solvent in the solution obtained in step 2 of the method, the products are the tetrafluoro oxalate phosphate and the volatile by-products, this means that the solvent can be recycled by means of a simple post-treatment; furthermore, the total yield of the tetrafluoro oxalate phosphate can be increased. Moreover, further disclosed in the present application are a production system suitable for the method, the use of the tetrafluoro oxalate phosphate prepared by using the method of the present application, and an electrolyte and a secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Preparation method, system, application, electrolyte and secondary battery of tetrafluorooxalophosphate

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on June 1, 2023, with application number 2023106434573 and application name “Preparation method, system, application, electrolyte and secondary battery of tetrafluorooxalate phosphate”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application belongs to the field of new energy, and specifically relates to a preparation method, system, application, electrolyte, and secondary battery of tetrafluorooxalophosphate for secondary battery electrolyte. Background Art

[0003] Lithium tetrafluorooxalophosphate (LiOTFP) is a new type of electrolyte lithium salt developed in recent years. Compared with lithium hexafluorophosphate, LiOTFP has better thermal stability and water tolerance. It can also form a more stable solid electrolyte interface film (CEI film) on the surface of the positive electrode material, effectively improving the high-temperature cycling and high-temperature storage performance of the battery. Therefore, it has been widely used in high-nickel and high-voltage fields. However, existing methods for preparing LiOTFP often only produce tetrafluorooxalophosphate solutions, making it difficult to precipitate high-purity tetrafluorooxalophosphate through crystallization. This easily leads to high free acid content, limiting its application in secondary battery electrolytes. Therefore, finding a safer, anhydrous method for preparing LiOTFP is one of the current research focuses on new electrolytes.

[0004] After searching, it can be generally known that the existing technology is divided into two main routes for preparing tetrafluorooxalophosphate.

[0005] Route 1: Preparation of tetrafluorooxalophosphate using oxalic acid and lithium hexafluorophosphate as raw materials;

[0006] Route 2: Prepare tetrafluorooxalophosphate using phosphorus pentafluoride and lithium oxalate as raw materials.

[0007] The following analyzes these two paths one by one:

[0008] Path 1

[0009] D1: CN113725430A discloses a preparation method, electrolyte, and secondary battery for lithium tetrafluorooxalate phosphate and its derivatives. In the preparation method for lithium tetrafluorooxalate phosphate and its derivatives, all reactants are mostly organic matter and lithium hexafluorophosphate, and the solvent is a non-aqueous solvent. High-purity lithium tetrafluorooxalate phosphate and its derivatives can be obtained by concentration and drying.

[0010] The specific preparation process is:

[0011] Providing oxalic acid, lithium hexafluorophosphate, a non-aqueous solvent and an organic auxiliary agent; the molar ratio of oxalic acid to the lithium hexafluorophosphate is 1:(1-2);

[0012] In the non-aqueous solvent, the oxalic acid, the lithium hexafluorophosphate and the organic auxiliary agent are mixed and reacted to obtain a solution containing lithium tetrafluorooxalophosphate;

[0013] The solution containing lithium tetrafluorooxalate phosphate is concentrated and dried to obtain the lithium tetrafluorooxalate phosphate.

[0014] D2: CN109850926A discloses a method for preparing lithium tetrafluorooxalophosphate and lithium difluorobisoxalophosphate. The method comprises preparing a titrant by dissolving lithium hexafluorophosphate in an organic solvent, adding trimethylsilyl chloride to the solution to prepare a base solution, dissolving oxalic acid in an organic solvent, preparing an organic base solution using the same method, adding the organic base to the oxalic acid solution, and stirring. The prepared titrant is slowly dripped into the reaction base solution. When the molar ratio of lithium hexafluorophosphate to oxalic acid is 1:1.8 to 1:2.5 and the reaction temperature is 15-40°C, lithium tetrafluorophosphate is produced. When the molar ratio of lithium hexafluorophosphate to oxalic acid is 1:1.8 to 1:2.5 and the reaction temperature is 15-40°C, lithium difluorobisoxalophosphate is produced. After the reaction is completed, the reaction system temperature is adjusted and stirring is continued for a period of time, followed by filtration and recrystallization to obtain the desired product.

[0015] D3: CN104334566B A method for safely producing a solution containing tetrafluoro(oxalato)phosphate, wherein the amount of chlorine compounds and free acid is so low that subsequent crystallization purification is unnecessary. The method comprises mixing hexafluorophosphate and oxalic acid in a non-aqueous solvent, and then adding silicon tetrachloride to the mixture and reacting the mixture, thereby producing a tetrafluoro(oxalato)phosphate solution. The ratio of hexafluorophosphate, oxalic acid, and silicon tetrachloride added is such that the hexafluorophosphate is at least 1.90 moles and the oxalic acid is between 1.90 and 2.10 moles per mole of silicon tetrachloride.

[0016] Through the above three technical documents, we can roughly draw the following conclusions:

[0017] 1. Analysis of D1 and D2 shows that when the ratio of lithium hexafluorophosphate to oxalic acid is different, lithium tetrafluorophosphate, lithium difluorobisoxalatophosphate, and lithium tetrafluorooxalatophosphate will be produced;

[0018] 2. In D1-D3, product extraction is mostly performed by crystallization. However, it is well known that no crystallization method can completely extract the product from the solution. 3-10% of the product always remains in the solution. These solutions require relatively complex post-processing methods for reuse, such as multi-stage distillation and vacuum distillation. In D1-D3, the raw materials used are lithium hexafluorophosphate, oxalic acid, and chlorosilane. Among these three raw materials, only chlorosilane is volatile. Given the reality that at least one raw material in the reaction cannot achieve 100% complete reaction (unless the material ratio is balanced and the process control accuracy is very high, so all substances react completely), not only the product but also the raw materials will remain in the solution, which places higher requirements on post-processing.

[0019] 3. Lithium hexafluorophosphate is expensive.

[0020] Path 2

[0021] D4: CN108808093A discloses a method for preparing lithium tetrafluorooxalophosphate, which comprises: (1) introducing phosphorus pentafluoride gas into a reactor to which lithium oxalate and dimethyl carbonate have been added, and carrying out sufficient reaction at 20-25°C for more than 5 hours, and filtering to obtain a lithium tetrafluorooxalophosphate solution; (2) adding dichloromethane dropwise until no crystals or precipitates are formed, and filtering to obtain a crude lithium tetrafluorooxalophosphate product; and (3) drying.

[0022] D5: CN109666046A discloses a method for preparing lithium tetrafluorooxalophosphate, which specifically includes the following steps: introducing phosphorus pentafluoride produced by the reaction of phosphorus element and fluorine gas into a reactor in which lithium oxalate and an organic solvent form a suspension for reaction through a buffer tank, and controlling the gas flow rate at 1 to 5 L / min, preferably 2 L / min. During the reaction, attention is paid to the pressure and temperature changes of the reactor. During this process, the temperature is controlled to be maintained between 10°C and 40°C, preferably 30°C, and the pressure is maintained at 0 to 0.5 MPa, preferably 0.1 MPa. The molar ratio of the obtained phosphorus pentafluoride to lithium oxalate is 2.2 to 2:1, preferably 2.05:1. The reaction is fully stirred for 1 to 3 hours, preferably 2 hours. After filtration, the desired product is obtained by concentration and crystallization, filtration, and drying.

[0023] D6: CN105218348B discloses a method for preparing lithium tetrafluorooxalophosphate, which specifically comprises the following steps: first, lithium oxalate is weighed and placed in a 316L stainless steel reactor A with a jacket and a filter, and stirred for 2 to 6 hours to fully dissolve it in anhydrous HF; then, phosphorus pentachloride and hydrogen fluoride are added to another 316L stainless steel reactor B with a jacket and a stirring device to carry out the reaction.

[0024] Through the above three technical documents, we can roughly draw the following conclusions:

[0025] 1. D6 uses HF as solvent, which has very high requirements for equipment corrosion protection and the reaction process is not gentle.

[0026] 2. D4 and D5 use lithium oxalate and phosphorus pentafluoride as raw materials to prepare lithium tetrafluorooxalophosphate. However, as is well known to those skilled in the art, lithium hexafluorophosphate will inevitably be produced (see paragraph 21 of the description of D5: Preferably, in the above-mentioned method for preparing lithium tetrafluorooxalophosphate, the main impurity in the obtained product is lithium hexafluorophosphate. By taking advantage of the difference in solubility of lithium hexafluorophosphate and lithium tetrafluorooxalophosphate in organic solvents, a pure lithium tetrafluorooxalophosphate product is obtained by concentration and crystallization).

[0027] The associated non-volatile lithium hexafluorophosphate product will still remain in the solvent after concentration and crystallization, resulting in the solvent inevitably containing products and by-products.

[0028] Therefore, from the above analysis, it can be seen that no matter whether path one or path two is adopted, the solvent after crystallization will contain product + non-volatile raw materials and / or by-products; this makes it very difficult to further recover these residual products.

[0029] Therefore, the technical problem to be solved in this project is: how to improve the recycling rate of substances in the reaction process, wherein the substances are solvents and / or products.

[0030] Summary of the Invention

[0031] In view of the shortcomings of the prior art, the purpose of the present application is to provide a method for preparing tetrafluorooxalophosphate for secondary battery electrolyte. In step 2 of the method, the solution obtained contains, in addition to the solvent, tetrafluorooxalophosphate and volatile by-products. This means that the solvent can be reused after simple post-treatment, and the solute in the solvent is almost entirely tetrafluorooxalophosphate, which can be directly reused in the production system without affecting the reaction. Alternatively, these solutions can be collected and concentrated again to precipitate tetrafluorooxalophosphate.

[0032] Although this case cannot achieve a high yield of the product in one step, through simple post-processing, the invisible yield can be significantly improved, thereby increasing the actual yield of the product.

[0033] The secondary purpose of the present application is to provide a production system for implementing the method, the use of the tetrafluorooxalophosphate prepared by the above method, an electrolyte, and a lithium secondary battery.

[0034] To achieve the purpose of this application, the present application adopts the following technical solution: a method for preparing tetrafluorooxalophosphate for secondary battery electrolyte, comprising the following steps:

[0035] Step 1: Using hydrogen oxalate and phosphorus pentafluoride as raw materials, reacting in an inert organic solvent to obtain a solution containing an intermediate product;

[0036] Step 2: reacting the solution containing the intermediate product with chlorosilane to obtain a solution containing tetrafluorooxalophosphate and volatile by-products;

[0037] Step 3: separating tetrafluorooxalophosphate from the solution containing tetrafluorooxalophosphate and volatile by-products.

[0038] It should be noted that:

[0039] The product and solution of step 3 can be separated by any method in the art, such as extraction, crystallization, vacuum distillation, etc. After the treatment in step 3, a solution containing tetrafluorooxalophosphate as the solute and a tetrafluorooxalophosphate solid of high purity can be obtained. This solution can be produced in any of the following directions:

[0040] Direction 1: Combine and concentrate the solutions produced multiple times, and then add a crystallization solvent to crystallize again;

[0041] Direction 2: After removing the crystallization solvent, directly recycle it to the reactor as the raw material solvent; it should be noted that although the raw material solvent contains the product, it has no effect on production.

[0042] The reaction equation of this application is: PF5+MHC2O4+Me x SiCl y →MPC2O4F4+Me x SiF y +HCl (M=Li,Na,K....;x+y=4)

[0043] Preferably, the present application recommends using a traditional crystallization operation to extract the product from the solution. Specifically, the step 3 includes the following sub-steps:

[0044] Sub-step 31: concentrating the solution containing tetrafluorooxalophosphate and volatile by-products to obtain an inert organic solvent concentrated solution containing tetrafluorooxalophosphate;

[0045] Sub-step 32: adding a crystallization solvent to the inert organic solvent concentrate to precipitate tetrafluorooxalate phosphate from the inert organic solvent concentrate to obtain tetrafluorooxalate phosphate solid and residual liquid.

[0046] In some implementation cases, the sub-step 32 further includes a sub-step 33: separating the crystallization solvent and the inert organic solvent in the residual liquid, and reusing the inert organic solvent as a raw material for step 1, wherein the inert organic solvent contains tetrafluorooxalate phosphate that has not been separated by crystallization.

[0047] As a further preferred embodiment of the present application, the molar ratio of hydrogen oxalate to phosphorus pentafluoride in step 1 is 1:0.9-1.1;

[0048] And / or, the molar ratio of hydrogen oxalate to chlorosilane in step 2 is 1:0.9-1.1.

[0049] Preferably, the molar ratio of hydrogen oxalate to phosphorus pentafluoride in step 1 is 1:1 to 1.1;

[0050] The molar ratio of hydrogen oxalate to chlorosilane in step 2 is 1:1 to 1.1.

[0051] In some embodiments of the present application, the molar ratio of hydrogen oxalate to phosphorus pentafluoride is 1:0.9, 1:0.91, 1:0.92, 1:0.93, 1:0.94, 1:0.95, 1:0.96, 1:0.97, 1:0.98, 1:0.99, 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09 or 1:1.1;

[0052] In some embodiments of the present application, the molar ratio of hydrogen oxalate to chlorosilane is 1:0.9, 1:0.91, 1:0.92, 1:0.93, 1:0.94, 1:0.95, 1:0.96, 1:0.97, 1:0.98, 1:0.99, 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09 or 1:1.1;

[0053] It needs further explanation:

[0054] 1. In the present application, more phosphorus pentafluoride can theoretically be used because more phosphorus pentafluoride will volatilize in the subsequent concentration step. However, more phosphorus pentafluoride, such as 1.5 times the molar ratio of phosphorus pentafluoride, will lead to a significant increase in the acidity of the solution, thereby hindering the reaction.

[0055] In the present application, more chlorosilane can be used, but more chlorosilane will not bring any benefit except increasing the loss of chlorosilane.

[0056] 2. In this application, if the molar ratio of phosphorus pentafluoride is less than 1.0, the hydrogen oxalate will not react completely. However, hydrogen oxalate is a solid in this system. Therefore, only an additional filter is required at the discharge port of the reactor to filter out the hydrogen oxalate before concentration. In other words, even if the amount of hydrogen oxalate is excessive, it will not result in residual raw material in the final recovered organic solvent.

[0057] In some embodiments of the present application, the inert organic solvent is 3 to 10 times the mass of the hydrogen oxalate; the reaction time of step 1 is 0.5 to 3 hours;

[0058] In the actual production process, the inert organic solvent is 3 times, 4 times, 5 times, 6 times, 7 times, 8 times, 9 times or 10 times the mass of hydrogen oxalate;

[0059] The reaction time of step 1 is 0.5h, 1h, 1.5h, 2h, 2.5h or 3h;

[0060] Step 2: Chlorosilane is added to the solution containing the intermediate product in batches. The addition time of chlorosilane is 1 to 5 hours. The reaction temperature is 10 to 90° C., and the reaction time is 1 to 6 hours after the addition of chlorosilane is completed.

[0061] The batch addition mentioned in this application is in the form of dropwise addition or addition in multiple batches;

[0062] It should be noted that if the chlorosilane is added in multiple batches, it should be added in small batches to stabilize the reaction, because adding all the chlorosilane at once will cause a violent reaction and a large amount of gas production.

[0063] In the actual production process, the addition time of chlorosilane is 1h, 2h, 3h, 4h or 5h;

[0064] The reaction temperature is 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C;

[0065] After the addition of chlorosilane is completed, the reaction time is 1 h, 2 h, 3 h, 4 h, 5 h or 6 h;

[0066] Preferably, the inert organic solvent is 4 to 9 times the mass of the hydrogen oxalate; the reaction time of step 1 is 1 to 2 hours;

[0067] Step 2: Chlorosilane is added to the solution containing the intermediate product in the form of dropwise addition or batch addition. The addition time of chlorosilane is 1 to 3 hours. The reaction temperature is 20 to 50° C., and the reaction time is 2 to 5 hours after the addition of chlorosilane is completed.

[0068] As a further preferred embodiment of the present application, in sub-step 31, the concentration of tetrafluorooxalate phosphate in the inert organic solvent concentrate is not less than 30 wt %; preferably, the concentration of tetrafluorooxalate phosphate in the inert organic solvent concentrate is not less than 35 wt %; preferably, the concentration of tetrafluorooxalate phosphate in the inert organic solvent concentrate is 30 wt % to 60 wt %; more preferably, the concentration of tetrafluorooxalate phosphate in the inert organic solvent concentrate is 30 wt % to 45 wt %;

[0069] Generally speaking, if the concentration is lower than 30 wt%, the crystallization efficiency is too low due to the low crystallization concentration; too high a concentration will cause precipitation before crystallization, so the optimal concentration is recommended to be within the above range.

[0070] The amount of the crystallization solvent added is more than 2 times the weight of the theoretical yield of tetrafluorooxalophosphate; preferably 2 to 5 times the weight, which can take into account both precipitation and reducing solvent recovery energy consumption;

[0071] Further preferably, in sub-step 31, the concentration method is reduced pressure concentration.

[0072] In practical applications, the concentration method can also be atmospheric pressure concentration.

[0073] In practical applications, the crystallization solvent can be selected from one or more of toluene, xylene, dichloromethane, chloroform, 1,2-dichloromethane, and ether;

[0074] The inert organic solvent is an ester solvent; the chlorosilane is one or more of trimethylchlorosilane, dimethyldichlorosilane, and monomethyltrichlorosilane;

[0075] The hydrogen oxalate is one or more of lithium hydrogen oxalate, sodium hydrogen oxalate, potassium hydrogen oxalate, and ammonium hydrogen oxalate;

[0076] Preferably, the ester solvent is one or more of propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl acetate, and ethyl acetate.

[0077] Before performing sub-step 31 , the solution containing tetrafluorooxalophosphate and volatile by-products is filtered, and the filtrate is subjected to sub-step 31 .

[0078] At the same time, the present application also discloses a production system for implementing any of the above methods, comprising a reaction unit, a concentration unit, a crystallization unit, a residual liquid collection unit, a distillation tower, a bottom liquid collection unit, and a first circulation pump connected in sequence; the outlet of the first circulation pump is connected to the reaction unit;

[0079] The reaction unit is used to implement step 1 and step 2, and transport the solution containing tetrafluorooxalophosphate and volatile by-products to the concentration unit;

[0080] The concentration unit is used to concentrate the solute in the solution containing tetrafluorooxalophosphate and volatile by-products to a preset concentration and volatilize the volatile by-products;

[0081] The crystallization unit is used to precipitate tetrafluorooxalophosphate from the concentrated solution, and discharge the residual liquid after crystallization to the residual liquid collection unit;

[0082] The distillation tower is used to remove light components from the residual liquid using the solution in the residual liquid collection unit as raw material. The bottom liquid after distillation is an inert organic solvent solution containing tetrafluorooxalophosphate that has not been crystallized. The bottom liquid is discharged into the bottom liquid collection unit and refluxed to the reaction unit through the first circulation pump.

[0083] The above production system further includes a tetrafluorooxalate phosphate post-treatment unit, wherein the tetrafluorooxalate phosphate post-treatment unit is located between the crystallization unit and the residual liquid collection unit;

[0084] The tetrafluorooxalate phosphate post-processing unit is used to separate the solution after crystallization in the crystallization unit into solid and liquid, and the tetrafluorooxalate phosphate remains in the tetrafluorooxalate phosphate post-processing unit, and the residual liquid is discharged into the residual liquid collection unit; the tetrafluorooxalate phosphate remaining is washed once or multiple times with a crystallization solvent, and dried to obtain a tetrafluorooxalate phosphate solid; the washed crystallization solvent is discharged into the residual liquid collection unit;

[0085] The reaction unit is connected to a first condensing unit and an exhaust gas treatment unit connected to the first condensing unit;

[0086] The concentrating unit is connected to a second condensing unit;

[0087] The tetrafluorooxalate phosphate post-treatment unit is connected to a third condensing unit;

[0088] The top of the distillation tower is connected in sequence with a fourth condensing unit and a crystallization solvent collecting unit; the crystallization solvent collecting unit is connected to the crystallization unit through a second circulation pump;

[0089] A filter is provided between the first circulation pump and the reaction unit.

[0090] In addition, the present application also discloses the use of the tetrafluorooxalophosphate prepared by any of the above preparation methods as an electrolyte in a secondary battery electrolyte or a functional additive in an electrolyte.

[0091] Preferably, the tetrafluorooxalophosphate is lithium tetrafluorooxalophosphate, sodium tetrafluorooxalophosphate or potassium tetrafluorooxalophosphate;

[0092] The secondary battery is a lithium ion battery, a sodium ion battery or a potassium ion battery.

[0093] More specifically, if the secondary battery is a lithium-ion battery, the tetrafluorooxalophosphate is lithium tetrafluorooxalophosphate;

[0094] If the secondary battery is a sodium ion battery, the tetrafluorooxalate phosphate is sodium tetrafluorooxalate phosphate;

[0095] If the secondary battery is a potassium ion battery, the tetrafluorooxalate phosphate is potassium tetrafluorooxalate phosphate;

[0096] At the same time, the present application also discloses an electrolyte, which contains tetrafluorooxalophosphate prepared by any of the above preparation methods.

[0097] In the above electrolyte, the content of tetrafluorooxalophosphate in the electrolyte is 0.01 wt% to 30 wt%.

[0098] Finally, the present application also discloses a secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte; the electrolyte contains tetrafluorooxalophosphate prepared by any of the above preparation methods.

[0099] Preferably, the content of the tetrafluorooxalophosphate in the electrolyte is 0.01 wt% to 30 wt%.

[0100] More specifically, if the content of tetrafluorooxalophosphate in the electrolyte is 0.01 wt% to 1 wt%, it is generally used as a functional additive;

[0101] If it exceeds 1 wt%, it is used as an electrolyte, if it is less than 5 wt%, it is used as a non-primary electrolyte, and if it is greater than 5 wt%, it is used as a primary additive;

[0102] Taking lithium secondary batteries as an example, if it is used as a non-primary electrolyte, the primary electrolyte may be lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, or the like.

[0103] Preferably, the secondary battery is a lithium ion battery, a sodium ion battery or a potassium ion battery; the tetrafluorooxalophosphate is lithium tetrafluorooxalophosphate, sodium tetrafluorooxalophosphate or potassium tetrafluorooxalophosphate;

[0104] More specifically, if the secondary battery is a lithium-ion battery, the tetrafluorooxalophosphate is lithium tetrafluorooxalophosphate;

[0105] If the secondary battery is a sodium ion battery, the tetrafluorooxalate phosphate is sodium tetrafluorooxalate phosphate;

[0106] If the secondary battery is a potassium ion battery, the tetrafluorooxalatophosphate is potassium tetrafluorooxalatophosphate.

[0107] Compared with the prior art, this application has the following beneficial effects:

[0108] (1) Tetrafluorooxalophosphate is synthesized from common non-aqueous solvents, phosphorus pentafluoride, hydrogen oxalate, and chlorosilane as raw materials without using hydrofluoric acid. The reaction equipment requirements are not high, the process is simple, the reaction conditions are mild, and the post-processing purification process adopts a double solvent recrystallization method to prepare a solid tetrafluorooxalophosphate, thereby ensuring a high product yield, better control of acidity and chloride ions, and good product quality;

[0109] (2) The raw materials of the present application are phosphorus pentafluoride, hydrogen oxalate and chlorosilane. Phosphorus pentafluoride and chlorosilane are both volatile raw materials. It is sufficient to ensure that the hydrogen oxalate reacts completely. The products of the present application, fluorosilane and hydrogen chloride, are also volatile products.

[0110] Furthermore, in the first step, lithium hydrogen oxalate is used as an example. It contains only one Li atom, so apart from the intermediate product, lithium hydrogen pentafluorooxalophosphate, no non-volatile by-products are generated. In the subsequent reaction with chlorosilane, the product is relatively pure, and the unreacted volatile raw materials can be volatilized, resulting in the final solvent containing almost only the product and no raw materials. This is the basis for the solvent in this case to be directly reused or secondary concentrated and precipitated.

[0111] Compared with the first and second paths described in the background art, the side reaction products and most of the raw materials in this application are volatile. BRIEF DESCRIPTION OF THE DRAWINGS

[0112] FIG1 is a flow chart of a system embodiment of the present application;

[0113] FIG2 is a nuclear magnetic 19F-NMR (CD3CN) spectrum of lithium tetrafluorooxalate phosphate of Example 1 of the present application;

[0114] FIG3 is a nuclear magnetic 31P-NMR (CD3CN) spectrum of lithium tetrafluorooxalophosphate of Example 1 of the present application. DETAILED DESCRIPTION

[0115] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.

[0116] Before describing the preparation process of the present application, the production system of the present application is first described. It should be emphasized that the production system of the present application is only a detailed description of the production scenario in which the solvent of the present application is directly recycled into the production system. Other utilization methods of the present application are not realized in this production system.

[0117] That is, the embodiment of the system of the present application does not represent any limitation on step 3 of the present application; it is only for enabling readers to understand the solution of the present application more clearly.

[0118] System Example

[0119] 1 , a production system of tetrafluorooxalophosphate includes a reaction unit, a concentration unit, a crystallization unit, a residual liquid collection unit 7, a distillation tower 1, a bottom liquid collection unit 8, and a first circulation pump 2 connected in sequence; the outlet of the first circulation pump 2 is connected to the reaction unit;

[0120] The complete reaction process is:

[0121] An inert organic solvent is added to the reaction unit; hydrogen oxalate and phosphorus pentafluoride are added to the inert organic solvent for reaction to obtain a solution containing an intermediate product; chlorosilane is added to the reaction unit for reaction to obtain a solution containing tetrafluorooxalophosphate and volatile byproducts;

[0122] After the reaction in the reaction unit is completed, the solution is discharged to the concentration unit, the solvent is evaporated, the solution is concentrated, and the concentrated solution is discharged to the crystallization unit;

[0123] The crystallization unit is filled with a crystallization solvent through a pipeline to precipitate tetrafluorooxalate phosphate. After the precipitation is completed, the liquid is discharged to the residual liquid collection unit 7 through solid-liquid separation, and the solid is tetrafluorooxalate phosphate;

[0124] The main function of the residual liquid collection unit 7 is liquid storage, which pumps the liquid into the distillation column 1;

[0125] Since the boiling point of the crystallization solvent is low and the boiling point of the inert organic solvent is high, the crystallization solvent can be easily discharged from the top of the distillation tower 1; the inert organic solvent solution containing tetrafluorooxalophosphate is retained in the bottom of the tower;

[0126] The tower bottom liquid is discharged into the bottom liquid collection unit 8 and pumped into the production unit through the first circulation pump.

[0127] As a further preferred embodiment of the present invention, a tetrafluorooxalate phosphate post-treatment unit is further included, and the tetrafluorooxalate phosphate post-treatment unit is located between the crystallization unit and the residual liquid collection unit 7;

[0128] The tetrafluorooxalate phosphate post-processing unit is used to separate the solution crystallized in the crystallization unit into solid and liquid, and the tetrafluorooxalate phosphate remains in the tetrafluorooxalate phosphate post-processing unit, and the residual liquid is discharged into the residual liquid collection unit 7; the tetrafluorooxalate phosphate remaining is washed once or multiple times with a crystallization solvent, and dried to obtain a tetrafluorooxalate phosphate solid; the washed crystallization solvent is discharged into the residual liquid collection unit 7; the tetrafluorooxalate phosphate post-processing unit is preferably a drying kettle 12, the bottom of the drying kettle 12 is provided with a drain pipe and a solid discharge port, the drain pipe is provided with a filter screen to prevent the solid product from entering the drain pipe; the drain pipe is connected to the residual liquid collection unit; the drying kettle 12 is provided with a heating jacket; the drying kettle 12 has a filling pipe for adding a crystallization solvent and an exhaust pipe, and the exhaust pipe is connected to the third condensing unit 13 described later;

[0129] More specifically, referring to FIG1 , the reaction unit is a reactor 3, preferably a high-pressure reactor; the concentration unit is a concentration tank 4; a filter 5 is provided between the reactor 3 and the concentration tank 4; the crystallization unit is a crystallization tank 6, and the residual liquid collection unit 7 and the bottom liquid collection unit 8 are both storage tanks;

[0130] As a further preference of this embodiment, the reaction unit is connected to a first condensing unit 9 and an exhaust gas treatment unit 10 connected to the first condensing unit 9;

[0131] The first condensing unit 9 includes one or more condensers, which can be horizontal or vertical condensers. The condensate produced by the condenser is collected by a collection tank 14; the non-condensable gas enters the tail gas treatment unit 10 for treatment;

[0132] The first condensation unit 9 mainly collects some volatilized by-products, fluorosilane, escaped phosphorus pentafluoride, and organic solvents;

[0133] The concentration unit is connected to a second condensing unit 11; the second condensing unit 11 is mainly used to collect organic solvents and by-product fluorosilane;

[0134] The tetrafluorooxalate phosphate post-treatment unit is connected to a third condensing unit 13 ; the third condensing unit 13 is mainly used to collect the gas generated during drying after washing, which is generally a crystallization solvent.

[0135] The second condensing unit 11 and the third condensing unit 13 include one or more condensers, which may be horizontal or vertical condensers; the condensate of the second condensing unit 11 is collected by a collection tank 14, and the condensate of the third condensing unit 13 may enter the residual liquid collection unit 7; the non-condensable gas of the second condensing unit 11 and the third condensing unit 13 enters the vacuum buffer tank 15, and the vacuum buffer tank 15 is connected to the vacuum pump 16; the vacuum pump 16 provides a negative pressure environment for the concentration unit and the tetrafluorooxalate phosphate post-treatment unit, thereby facilitating the negative pressure concentration operation of the concentration unit and promoting solvent volatilization in the tetrafluorooxalate phosphate post-treatment unit when drying the tetrafluorooxalate phosphate;

[0136] The top of the distillation tower 1 is connected in sequence with a fourth condensing unit 17 and a crystallization solvent collecting unit 18; the crystallization solvent collecting unit 18 is connected to the crystallization unit through a second circulation pump 19; the fourth condensing unit 17 is a condenser for condensing the crystallization solvent; the crystallization solvent is recycled to the crystallization kettle 6; as is well known in the art, the top of the distillation tower needs to reflux the condensate, so the crystallization solvent condensed by the fourth condensing unit 17 needs to be partially refluxed to the top of the distillation tower.

[0137] Preferably, a filter 5 is provided between the first circulation pump 2 and the reaction unit.

[0138] Implicitly, in this embodiment, valves should be installed on each pipeline, and the liquid flow between each kettle can be achieved by high and low liquid differentials or by pumps; observation holes, manholes, pressure gauges, thermometers, etc. can be installed on each kettle. This is common knowledge in the field and this embodiment does not impose too many restrictions on this; a feeding hopper, a feeding pipe, etc. are also required to be provided on the reactor 3.

[0139] The relevant implementation cases synthesized by this application are as follows:

[0140] Example 1

[0141] 96.0 g of lithium hydrogen oxalate (1.0 mol), 126.0 g of phosphorus pentafluoride (1.0 mol) and 800 g of ethyl methyl carbonate were added to an autoclave, stirred for 1 h, and then 114.1 g of trimethylsilyl chloride (1.05 mol) was added dropwise to start the reaction. The reaction was added dropwise for 2 h, the reaction temperature was 40 ° C, the reaction time was 4 h, and the reaction was cooled to 20 ° C after completion of the reaction. After sufficient stirring, the filtrate was concentrated at 30 ° C, -0.095 MPa for 2 h to obtain 420 g of a concentrated solution containing ethyl methyl carbonate. 600 g of dichloromethane was added dropwise, crystallized for 2 h, filtered twice, and the filter cake was dried at 60 ° C, -0.095 MPa for 4 h to obtain 183.8 g of lithium tetrafluorooxalophosphate, with a yield of 91.0%. The acidity of the 10% EMC solution was 11.7 ppm, and the chloride ion was 2.1 ppm. 2 and 3 , which are respectively the nuclear magnetic 19F-NMR (CD3CN) spectrum of lithium tetrafluorooxalate phosphate and the nuclear magnetic 31P-NMR (CD3CN) spectrum of lithium tetrafluorooxalate phosphate, it can be proved that the product of the present application is lithium tetrafluorooxalate phosphate.

[0142] In the above operation, the main components of the solution after crystallization were detected to be: dichloromethane, ethyl methyl carbonate, and lithium tetrafluorooxalate phosphate, and the concentration of lithium tetrafluorooxalate phosphate was about 2.3 wt%;

[0143] The above solution is fed into the distillation tower of the system embodiment. After fractionation in the distillation tower, dichloromethane (boiling point: 39.8°C) and ethyl methyl carbonate (boiling point: 107°C) can be separated relatively easily. The dichloromethane is separated at the top of the tower, and after condensation, part of the condensate is refluxed to the distillation tower, and part of the dichloromethane enters the crystallization process.

[0144] Example 2

[0145] 96.0 g of lithium hydrogen oxalate (1.0 mol), 113.4 g of phosphorus pentafluoride (0.9 mol) and 800 g of diethyl carbonate were added to an autoclave, stirred for 1 h, and then 108.6 g of trimethylsilyl chloride (1.0 mol) was added dropwise to start the reaction. The reaction was added dropwise for 2 h, the reaction temperature was 45 ° C, the reaction time was 3.5 h, and the temperature was lowered to 20 ° C after the reaction was completed. After sufficient stirring, the filtrate was filtered and concentrated at 40 ° C and -0.095 MPa for 2 h to obtain 400 g of concentrated solution containing ethyl methyl carbonate. 700 g of xylene was added dropwise and crystallized for 2 h. The mixture was filtered twice and the filter cake was dried at 60 ° C and -0.095 MPa for 4 h to obtain 166.3 g of lithium tetrafluorooxalophosphate with a yield of 91.5%. The acidity of the 10% EMC solution was 10.8 ppm and the chloride ion was 3.6 ppm.

[0146] Example 3

[0147] 96.0 g of lithium hydrogen oxalate (1.0 mol), 138.6 g of phosphorus pentafluoride (1.1 mol) and 800 g of ethyl acetate were added to a high-pressure reactor, stirred for 2 h, and then 119.5 g of trimethylchlorosilane (1.1 mol) was added dropwise to start the reaction. The reaction was added dropwise for 2 h, the reaction temperature was 45 ° C, the reaction time was 3.5 h, and the reaction was cooled to 20 ° C after completion of the reaction. After sufficient stirring, the filtrate was concentrated at 40 ° C, -0.095 MPa for 2 h to obtain 450 g of a concentrated solution containing ethyl methyl carbonate. 800 g of toluene was added dropwise, crystallized for 2 h, filtered twice, and the filter cake was dried at 60 ° C, -0.095 MPa for 4 h to obtain 183.2 g of lithium tetrafluorooxalophosphate, with a yield of 90.7%. The acidity of the 10% EMC solution was 12.6 ppm, and the chloride ion was 4.1 ppm.

[0148] The reaction equations of Examples 1-3 are: PF5+LiHC2O4+Me3SiCl→LiPC2O4F4+Me3SiF+HCl.

[0149] Example 4

[0150] 112.0 g of sodium hydrogen oxalate (1.0 mol), 126.0 g of phosphorus pentafluoride (1.0 mol) and 1000 g of dimethyl carbonate were added to a high-pressure reactor, stirred for 1.5 h, and then 68.4 g of dimethyldichlorosilane (0.53 mol) was added dropwise to start the reaction. The reaction was added dropwise for 1 h, the reaction temperature was 50 ° C, the reaction time was 3 h, and the reaction was cooled to 25 ° C after completion of the reaction. After sufficient stirring, the filtrate was concentrated at 40 ° C, -0.095 MPa for 2 h to obtain 500 g of a concentrated solution containing dimethyl carbonate. 660 g of 1,2-dichlorohexane was added dropwise, crystallized for 3 h, filtered twice, and the filter cake was dried at 50 ° C, -0.095 MPa for 5 h to obtain 194.0 g of sodium tetrafluorooxalophosphate with a yield of 89.2%. The acidity of the solution prepared into 10% EMC was 6.5 ppm and the chloride ion was 1.9 ppm.

[0151] The reaction equation of Example 4 is as follows: 2PF5+2NaHC2O4+Me2SiCl2→2NaPC2O4F4+Me2SiF2+2HCl.

[0152] Example 5

[0153] 128.0 g of potassium hydrogen oxalate (1.0 mol), 126.0 g of phosphorus pentafluoride (1.0 mol) and 1000 g of ethyl methyl carbonate were added to an autoclave, stirred for 2.5 h, and then 52.3 g of monomethyltrichlorosilane (0.35 mol) was added dropwise to start the reaction. The reaction was added dropwise for 1 h, the reaction temperature was 40 ° C, the reaction time was 3 h, and the reaction was cooled to 20 ° C after completion of the reaction. After sufficient stirring, the filtrate was concentrated at 40 ° C, -0.095 MPa for 2 h to obtain 900 g of a concentrated solution containing ethyl methyl carbonate. 800 g of ether was added dropwise, crystallized for 3 h, filtered twice, and the filter cake was dried at 60 ° C, -0.095 MPa for 5 h to obtain 203.6 g of potassium tetrafluorooxalophosphate, with a yield of 87.0%. The acidity of the solution prepared into 10% EMC was 5.9 ppm, and the chloride ion was 2.2 ppm.

[0154] The reaction equation of Example 5 is as follows: 3PF5+3KHC2O4+MeSiCl3→3KPC2O4F4+MeSiF3+3HCl.

[0155] Example 6

[0156] 107.0 g of ammonium hydrogen oxalate (1.0 mol), 126.0 g of phosphorus pentafluoride (1.0 mol) and 800 g of ethyl methyl carbonate were added to an autoclave, stirred for 3 h, and then 108.5 g of trimethylchlorosilane (1.0 mol) was added dropwise to start the reaction. The reaction was added dropwise for 2 h, the reaction temperature was 40 ° C, the reaction time was 3 h, and the reaction was cooled to 20 ° C after completion of the reaction. After sufficient stirring, the filtrate was concentrated at 30 ° C, -0.095 MPa for 2 h to obtain 420 g of a concentrated solution containing ethyl methyl carbonate. 600 g of dichloromethane was added dropwise, crystallized for 2 h, filtered twice, and the filter cake was dried at 60 ° C, -0.095 MPa for 3 h to obtain 188.7 g of lithium tetrafluorooxalophosphate with a yield of 88.6%. The acidity of the 10% EMC solution was 9.5 ppm, and the chloride ion was 3.6 ppm.

[0157] The reaction equation of Example 6 is as follows: PF5+NH4HC2O4+Me3SiCl→NH4PC2O4F4+Me3SiF+HCl.

[0158] Example 7

[0159] 96.0 g of lithium hydrogen oxalate (1.0 mol), 126.0 g of phosphorus pentafluoride (1.0 mol) and 300 g of ethyl methyl carbonate were added to an autoclave, stirred for 0.5 h, and then 114.1 g of trimethylchlorosilane (1.05 mol) was added dropwise to start the reaction. The reaction was added dropwise for 5 h, the reaction temperature was 40 ° C, the reaction time was 1 h, and the reaction was cooled to 20 ° C after completion of the reaction. After sufficient stirring, the filtrate was concentrated at 30 ° C, -0.095 MPa for 2 h to obtain 395 g of a concentrated solution containing ethyl methyl carbonate. 600 g of dichloromethane was added dropwise, crystallized for 2 h, filtered twice, and the filter cake was dried at 60 ° C, -0.095 MPa for 4 h to obtain 185.5 g of lithium tetrafluorooxalophosphate, with a yield of 91.8%. The acidity of the 10% EMC solution was 11.3 ppm, and the chloride ion was 2.2 ppm.

[0160] Example 8

[0161] 96.0 g of lithium hydrogen oxalate (1.0 mol), 126.0 g of phosphorus pentafluoride (1.0 mol) and 600 g of ethyl methyl carbonate were added to an autoclave, stirred for 3 h, and then 114.1 g of trimethylsilyl chloride (1.05 mol) was added dropwise to start the reaction. The reaction was added dropwise for 4 h, the reaction temperature was 40 ° C, the reaction time was 6 h, and the reaction was cooled to 20 ° C after completion of the reaction. After sufficient stirring, the filtrate was concentrated at 30 ° C, -0.095 MPa for 2 h to obtain 412 g of a concentrated solution containing ethyl methyl carbonate. 600 g of dichloromethane was added dropwise, crystallized for 2 h, filtered twice, and the filter cake was dried at 60 ° C, -0.095 MPa for 4 h to obtain 184.4 g of lithium tetrafluorooxalophosphate, with a yield of 91.3%. The acidity of the 10% EMC solution was 13.6 ppm, and the chloride ion was 2.9 ppm.

[0162] in conclusion:

[0163] 1. In the first path of the existing technology, the products are diverse, the raw materials are expensive, and the raw materials are non-volatile;

[0164] The product of this application is single, the raw materials are cheap, and most of the raw materials are volatile substances, which ensures that the solution after crystallization can be reused by simple distillation;

[0165] 2. In the second route of the prior art, lithium hexafluorophosphate is produced as a by-product, which makes it impossible to reuse the solvent after crystallization. This also means that it is more difficult to separate the residual product in the solution after crystallization.

[0166] The product of the present application is single and the solution after crystallization can be reused by simple distillation.

[0167] 3. The present application can recover the tetrafluorooxalophosphate that has not been crystallized by solvent recycling or solvent re-concentration and crystallization, which can indirectly increase the product yield.

[0168] The applicant declares that while the above-mentioned embodiments are used to illustrate the process of the present application, the present application is not limited to the above-mentioned process steps, nor does it mean that the present application must rely on the above-mentioned process steps in order to be implemented. Those skilled in the art should understand that any improvements to the present application, equivalent replacements of raw materials used in the present application, addition of auxiliary components, and selection of specific methods, etc., fall within the scope of protection and disclosure of the present application.

Claims

1. A method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte, wherein: The following steps are involved: Step 1: using hydrogen oxalate and phosphorus pentafluoride as raw materials, reacting in an inert organic solvent to obtain a solution containing an intermediate product; Step 2: reacting the solution containing the intermediate product with chlorosilane to obtain a solution containing tetrafluorooxalyl phosphate and volatile byproducts; Step 3: separating tetrafluorooxalate phosphate from the solution containing tetrafluorooxalate phosphate and volatile by-products.

2. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 1, wherein: The step 3 specifically includes the following sub-steps: Sub-step 31: concentrating the solution containing tetrafluorooxalate phosphate and volatile by-products to obtain an inert organic solvent concentrated solution containing tetrafluorooxalate phosphate; Sub-step 32: adding a crystallization solvent to the inert organic solvent concentrated solution to precipitate tetrafluorooxalate phosphate from the inert organic solvent concentrated solution to obtain tetrafluorooxalate phosphate solid and residual liquid.

3. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 2, wherein: Sub-step 32 also includes sub-step 33: separating the crystallization solvent and the inert organic solvent in the residual liquid, and recycling the inert organic solvent as a raw material for step 1.

4. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 1, wherein: In the step 1, the molar ratio of hydrogen oxalate to phosphorus pentafluoride is 1:0.9-1.

1.

5. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 1, wherein: The molar ratio of hydrogen oxalate to chlorosilane in step 2 is 1:0.9-1.

1.

6. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 4 or 5, wherein: In the step 1, the molar ratio of hydrogen oxalate to phosphorus pentafluoride is 1:1 to 1.

1.

7. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 4 or 5, wherein: The molar ratio of hydrogen oxalate to chlorosilane in step 2 is 1:1 to 1.

1.

8. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 1, wherein: The inert organic solvent is 3 to 10 times the mass of the hydrogen oxalate; and the reaction time of step 1 is 0.5 to 3 hours.

9. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 8, wherein: The inert organic solvent is 4 to 9 times the mass of hydrogen oxalate; and the reaction time of step 1 is 1 to 2 hours.

10. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 1, wherein: In step 2, chlorosilane is added to the solution containing the intermediate product in batches, and the addition time of chlorosilane is 1 to 5 hours; the reaction temperature is 10 to 90° C., and the reaction time is 1 to 6 hours after the addition of chlorosilane is completed.

11. The method for preparing tetrafluorooxalate phosphate according to claim 2, wherein: In sub-step 31, the concentration is carried out under reduced pressure, and the concentration of tetrafluorooxalate phosphate in the inert organic solvent concentrate is not less than 30 wt%.

12. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 11, wherein: The concentration of tetrafluorooxalate phosphate in the inert organic solvent concentrate is not less than 35 wt %.

13. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 11, wherein: The concentration of tetrafluorooxalate phosphate in the inert organic solvent concentrate is 30 wt % to 60 wt %.

14. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 13, wherein: The concentration of tetrafluorooxalate phosphate in the inert organic solvent concentrate is 30 wt % to 45 wt %.

15. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 2, wherein: The amount of the crystallization solvent added is more than twice the weight of the theoretical yield of tetrafluorooxalate phosphate.

16. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 15, wherein: The added amount of the crystallization solvent is 2 to 5 times by weight of the theoretical yield of tetrafluorooxalate phosphate.

17. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 2, wherein: The crystallization solvent is one or more of toluene, xylene, dichloromethane, chloroform, 1,2-dichloromethane and ether.

18. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 2, wherein: Before sub-step 31 is performed, the solution containing tetrafluorooxalate phosphate and volatile by-products is filtered, and the filtrate is subjected to sub-step 31.

19. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to any one of claims 1 to 18, wherein: The inert organic solvent is an ester solvent.

20. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to any one of claims 1 to 18, wherein: The chlorosilane is one or more of trimethylchlorosilane, dimethyldichlorosilane and monomethyltrichlorosilane.

21. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to any one of claims 1 to 18, wherein: The hydrogen oxalate is one or more of lithium hydrogen oxalate, sodium hydrogen oxalate, potassium hydrogen oxalate, and ammonium hydrogen oxalate.

22. The method for preparing tetrafluorooxalate phosphate for secondary battery electrolyte according to claim 19, wherein: The ester solvent is one or more of propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl acetate, and ethyl acetate.

23. A production system for implementing the method according to any one of claims 1 to 22, wherein: It includes a reaction unit, a concentration unit, a crystallization unit, a residual liquid collection unit, a distillation tower, a bottom liquid collection unit, and a first circulation pump connected in sequence; the outlet of the first circulation pump is connected to the reaction unit; The reaction unit is used to implement step 1 and step 2, and transport the solution containing tetrafluorooxalate phosphate and volatile by-products to the concentration unit; The concentration unit is used to concentrate the solute in the solution containing tetrafluorooxalate phosphate and volatile by-products to a preset concentration and volatilize the volatile by-products; The crystallization unit is used to precipitate tetrafluorooxalate phosphate from the concentrated solution, and discharge the residual liquid after crystallization to the residual liquid collection unit; The distillation tower is used to remove light components from the residual liquid using the solution in the residual liquid collection unit as raw material. The bottom liquid after distillation is an inert organic solvent solution containing tetrafluorooxalate phosphate that has not been crystallized. The bottom liquid is discharged into the bottom liquid collection unit and refluxed to the reaction unit through the first circulation pump.

24. The production system according to claim 23, wherein: It also includes a tetrafluorooxalate phosphate post-treatment unit, which is located between the crystallization unit and the residual liquid collection unit; The tetrafluorooxalate phosphate post-treatment unit is used to separate the solution after crystallization in the crystallization unit through solid-liquid separation, and the tetrafluorooxalate phosphate remains in the tetrafluorooxalate phosphate post-treatment unit, and the residual liquid is discharged into the residual liquid collection unit; the tetrafluorooxalate phosphate remaining is washed once or multiple times with a crystallization solvent, and dried to obtain a tetrafluorooxalate phosphate solid; the washed crystallization solvent is discharged into the residual liquid collection unit.

25. The production system according to claim 24, wherein: The reaction unit is connected to a first condensing unit and a tail gas treatment unit connected to the first condensing unit.

26. The production system according to claim 24, wherein: The concentration unit is connected to a second condensation unit.

27. The production system according to claim 24, wherein: The tetrafluorooxalate phosphate post-treatment unit is connected to a third condensing unit.

28. The production system of claim 24, wherein: The top of the distillation tower is sequentially connected with a fourth condensing unit and a crystallization solvent collecting unit, and the crystallization solvent collecting unit is connected to the crystallization unit through a second circulation pump.

29. The production system according to claim 23, wherein: A filter is provided between the first circulation pump and the reaction unit.

30. Use of the tetrafluorooxalate phosphate prepared by the preparation method according to any one of claims 1 to 22 as an electrolyte in an electrolyte of a secondary battery or a functional additive in an electrolyte.

31. The use according to claim 30, wherein The tetrafluorooxalate phosphate is lithium tetrafluorooxalate phosphate, sodium tetrafluorooxalate phosphate or potassium tetrafluorooxalate phosphate; The secondary battery is a lithium ion battery, a sodium ion battery or a potassium ion battery.

32. An electrolyte, wherein The electrolyte contains tetrafluorooxalate phosphate prepared by the preparation method according to any one of claims 1 to 22.

33. The electrolyte according to claim 32, wherein The content of tetrafluorooxalate phosphate in the electrolyte is 0.01 wt% to 30 wt%.

34. A secondary battery, wherein: It includes a positive electrode, a negative electrode, a separator, and an electrolyte as described in claim 32 or 33, wherein the secondary battery is a lithium ion battery, a sodium ion battery or a potassium ion battery; and the tetrafluorooxalate phosphate is lithium tetrafluorooxalate phosphate, sodium tetrafluorooxalate phosphate or potassium tetrafluorooxalate phosphate.

Citation Information

Patent Citations

  • Preparation method of lithium tetrafluoro (oxalato) phosphate and derivative thereof, electrolyte and secondary battery

    CN113725430A

  • Preparation method of oxalate phosphate, oxalate phosphate derivative and preparation method thereof, and electrolyte salt

    CN114075104A

  • Sodium ion electrolyte and application thereof, sodium ion battery and preparation method of sodium ion battery

    CN114497744A

  • Electrolyte additive, battery electrolyte and application thereof

    CN115312857A

  • Preparation method of electrolyte sodium salt of sodium-ion battery

    CN115676855A