Positive electrode active material, preparation method, positive electrode sheet, battery and electrical device
The secondary particle structure formed by spray drying solves the problem of capacity attenuation in the early cycle of lithium iron phosphate batteries. By increasing material polarization and forming ion channels, the active substances are activated, and the circulation performance and capacity retention rate of the battery are improved.
Patent Information
- Application Number
- PCT/CN2023/129150
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-11-01
- Publication Date
- 2024-12-05
AI Technical Summary
The problem of rapid capacity decay in the early cycle of lithium iron phosphate batteries.
By dispersing the primary particles of the lithium iron phosphate material and the binder in the solvent, the secondary particles are formed by spray drying, ensuring that at least part of the binder is located between adjacent primary particles, thereby forming a larger particle sized binary particle. Secondary particles increase the degree of polarization of the material, promote the formation of ion channels in the early stage of circulation, activate active substances that could not exert capacity, and improve the cycling performance of the battery.
It effectively alleviates the capacity attenuation of lithium iron phosphate positive electrode active material in the early stage of circulation, improves the initial and later stage capacity retention rate of the battery, and extends the cycle life of the battery.
Smart Images

Figure CN2023129150_05122024_PF_FP_ABST
Abstract
Description
Positive electrode active material, preparation method, positive electrode sheet, battery and electrical equipment
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 202310640920.9 filed on May 31, 2023, entitled “Positive electrode active material, preparation method, positive electrode sheet, battery and electrical equipment,” and the entire contents of that application are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to positive electrode active materials, preparation methods, positive electrode sheets, batteries and electrical equipment. Background Art
[0004] With the development of modern technology, lithium-ion batteries are considered the green and environmentally friendly battery of choice due to their high energy density, long cycle life, and environmental friendliness. Lithium-ion batteries are widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in electric vehicles, power tools, military equipment, and aerospace applications.
[0005] Lithium iron phosphate (LIFP) is a highly stable cathode material for lithium-ion batteries and is widely used in them. However, LFP batteries experience rapid capacity decay in the early stages of cycling, resulting in a poor user experience.
[0006] Summary of the Invention
[0007] In view of this, the main technical problem to be solved by this application is the problem of rapid capacity decay of lithium iron phosphate batteries in the early stage of cycling, thereby providing positive electrode active materials, preparation methods, positive electrode sheets, batteries and electrical equipment, which can improve the capacity decay in the early stage of cycling when lithium iron phosphate is used as the positive electrode active material.
[0008] In order to solve the above technical problems, a technical solution adopted in this application is: to provide a positive electrode active material, the positive electrode active material includes secondary particles, the secondary particles include primary particles and a binder, and the primary particles include lithium iron phosphate material; at least part of the binder is located between adjacent primary particles.
[0009] In the technical solution of the embodiment of the present application, the primary particles of the lithium iron phosphate material of the positive electrode active material are bonded by a binder to form secondary particles. The particle size of the lithium iron phosphate secondary particles increases relative to the particle size of the primary particles, resulting in a relatively large polarization of the positive electrode active material, a low initial charge and discharge efficiency of the positive electrode active material, and in the early stage of the cycle, some active materials cannot play their capacity. As the cycle progresses, after the binder between the primary particles is fully infiltrated by the electrolyte, ion channels are gradually formed. In addition, the expansion and contraction of the lithium iron phosphate material during the lithium intercalation and deintercalation process increases the gap between the originally tightly bonded primary particles, and some active materials that were originally unable to play their capacity are gradually activated, thereby compensating for the attenuation of the lithium iron phosphate positive electrode active material in the early stage of the cycle. On the other hand, due to the decrease in the overall polarization of the lithium iron phosphate positive electrode active material, the impedance of the battery cell formed by the positive electrode active material is relatively reduced, thereby showing a further increase in capacity, and the occurrence of small attenuation in the early stage of the cycle, no attenuation, or even an increase in capacity.
[0010] In the embodiments of the present application, the number of cycles in the initial cycle is smaller than the number of cycles in the early cycle. The initial cycle refers to the first 200 cycles, and the early cycle refers to the first 500 cycles. Of course, the number of cycles in the initial cycle and the early cycle also depends on the specific material of the positive electrode active material. The initial cycle can also be the first 200 cycles, or the first 300 cycles, or the first 150 cycles, etc. The early cycle can also be the first 400 cycles, or the first 600 cycles, etc.
[0011] In any embodiment, the volume average particle size Dv50 of the secondary particles is in the range of 2 μm to 50 μm. In the embodiment of the present application, by controlling the range of the volume average particle size Dv50 of the secondary particles of the positive electrode active material, the polarization degree of the positive electrode active material is optimized, so that the initial capacity of the battery is also maintained at an optimal state.
[0012] The volume average particle size Dv50 indicates that 50% of the particles in the total volume have a diameter greater than this value, and another 50% of the particles in the total volume have a diameter less than this value. Dv50 represents the median particle size of the powder.
[0013] In any embodiment, the volume average particle size Dv50 of the secondary particles is in the range of 10 μm to 30 μm. In the embodiment of the present application, the range of the volume average particle size Dv50 of the secondary particles of the positive electrode active material makes the polarization degree of the positive electrode active material better, so that the early capacity of the battery is also maintained in a better condition.
[0014] In any embodiment, the volume average particle size Dv50 of the primary particles is in the range of 0.1 μm to 2 μm. In the embodiment of the present application, the volume average particle size Dv50 of the primary particles of the positive electrode active material is within a range such that the polarization degree of the positive electrode active material is reduced during the later cycle, so that the capacity of the battery in the later period remains unchanged or has a small attenuation.
[0015] In any embodiment, the volume average particle size Dv50 of the primary particles is in the range of 0.2 μm to 1.5 μm. In the embodiment of the present application, the volume average particle size Dv50 of the primary particles of the positive electrode active material is within a range such that the positive electrode active material has a low degree of polarization during the later cycle, so that the capacity of the battery remains unchanged or increases in the later period.
[0016] In any embodiment, the mass fraction of the binder is 0.1%-2% based on the total mass of the positive electrode active material. In the embodiment of the present application, the final capacity and long-term performance of the positive electrode active material can be controlled by controlling the binder addition ratio: when the binder ratio is high, the prepared secondary particle material has greater polarization and lower initial capacity, but the capacity increases more significantly after the initial period; when the binder ratio is low, the final prepared lithium iron phosphate material has a higher initial capacity, but decays faster in the early stage of the cycle, and the degree of improvement in the capacity decay in the early stage of the cycle is small.
[0017] In any embodiment, the thickness of the binder between adjacent primary particles ranges from 0.1 μm to 1 μm. In the embodiment of the present application, by controlling the thickness of the binder, the cross-sectional area of the ion channel formed when the electrolyte infiltrates the binder of the positive electrode active material can be controlled, thereby effectively improving the early capacity decay of the battery.
[0018] In any embodiment, the binder comprises:
[0019] Wherein, R1, R2, and R3 each independently include hydrogen, an unsubstituted linear or branched alkyl group having 1 to 6 carbon atoms; R4 includes an unsubstituted linear or branched alkyl group having 1 to 6 carbon atoms; m has a numerical range of 100 to 3000; and n has a numerical range of 100 to 3000. In the embodiment of the present application, the binder includes a polymerized unit of a carbonate group, which can increase the molecular weight of the binder and improve the binding force of the binder, thereby effectively bonding the primary particles to form secondary particles.
[0020] In any embodiment, the unsubstituted linear or branched alkyl group having 1 to 6 carbon atoms includes methyl, ethyl, n-butyl or tert-butyl. In the embodiment of the present application, by further improving the binding force of the binder, the primary particles can be better bonded to form secondary particles.
[0021] In any embodiment, the binder comprises: Any one or more of the .
[0022] In any embodiment, the lithium iron phosphate material includes Li x Fe y M z PO4, wherein M includes any one or more of Mn, Cr, Co, Cu, Ni, V, Mo, Ti, Zn, Al, Ga, Mg, B and Nb, 0.05≦x≦1.2, 0.2≦y≦1, 0≦z≦0.8. In the embodiment of the present application, the lithium iron phosphate material includes lithium iron phosphate or lithium iron phosphate doped with metal elements. Lithium iron phosphate has strong stability during the charge and discharge process. Lithium iron phosphate is doped with the above-mentioned metal elements to improve the internal conductivity of the lithium iron phosphate primary particles. In the later stage of the battery cell in the embodiment of the present application, after formation or cycling, the atomic number ratio of the P element in the atomic number ratio of the constituent elements of the lithium iron phosphate material can be greater than 1, or less than 1 and greater than 0, and the atomic number ratio of the O element can be greater than 4, or less than 4 and greater than 0.
[0023] In any embodiment, the lithium iron phosphate material further includes a coating layer, and the coating layer includes a carbon layer. In the embodiment of the present application, the lithium iron phosphate has a coating layer on its surface, such as a carbon layer, which can improve the conductivity of the lithium iron phosphate.
[0024] In any embodiment, the thickness of the coating layer is greater than 0 and less than or equal to 20 nm. In the embodiment of the present application, the thickness of the coating layer is controlled to control the stability and conductivity of the lithium iron phosphate material within a preferred range.
[0025] The second aspect of the present application also provides a method for preparing a positive electrode active material, comprising: dispersing primary particles including lithium iron phosphate material and a binder in a solvent, and forming secondary particles by spray drying, wherein at least part of the binder is located between adjacent primary particles. In the embodiment of the present application, the primary particles and the binder are made into secondary particles by spray drying, so that the secondary particles have good uniformity, the size of the secondary particles is easy to control, and the uniformity of the bonding of the binder on the surface of the primary particles is easy to control. The primary particles in the secondary particles are in close contact with each other and with the bonding agent. The obtained lithium iron phosphate secondary particles are relatively polarized, the initial charge and discharge efficiency of the lithium iron phosphate secondary particles is low, and some active substances cannot exert their capacity in the early stage of the cycle; as the cycle proceeds, the binder between the primary particles is fully infiltrated by the electrolyte, and ion channels are gradually formed. Some active substances that were originally unable to exert their capacity are gradually activated, thereby compensating for the early attenuation of the lithium iron phosphate, making the early attenuation of the cycle small, no attenuation, and even increasing the capacity.
[0026] In any embodiment, the spray drying temperature range is 150° C. to 350° C. By controlling the spray drying temperature range, the particle size of the secondary particles and the thickness of the binder formed on the surface of the primary particles can be controlled.
[0027] The third aspect of the present application also provides a positive electrode plate, which includes the positive electrode active material of the first aspect of the present application or / and the positive electrode active material prepared by the preparation method of the positive electrode active material of the second aspect of the present application. Since the positive electrode plate of the present application includes the positive electrode active material provided in the present application and / or the positive electrode active material prepared by the preparation method of the positive electrode active material, it has at least the same advantages as a battery cell. On the other hand, the positive electrode active material used in the positive electrode plate of the embodiment of the present application includes lithium iron phosphate secondary particles, and there is a binder between the primary particles, so that the ability of the positive electrode active material in the embodiment of the present application to store electrolyte is enhanced, which is beneficial to improving the cycle performance of the battery.
[0028] The fourth aspect of the present application further provides a battery, comprising the positive electrode sheet of the third aspect of the present application. Since the battery of the present application comprises the positive electrode sheet provided by the present application, it has at least the same advantages as the positive electrode sheet.
[0029] The fifth aspect of the present application further provides an electrical device, comprising the battery according to the fourth aspect of the present application. Since the electrical device of the present application comprises the battery provided by the present application, it has at least the same advantages as the battery.
[0030] The beneficial effects of the present application are as follows: Different from the prior art, in the technical solution of the embodiment of the present application, the primary particles of the lithium iron phosphate material of the positive electrode active material are bonded by a binder to form secondary particles, and the particle size of the lithium iron phosphate secondary particles increases relative to the particle size of the primary particles, resulting in a relatively large polarization of the positive electrode active material, a low initial charge and discharge efficiency of the positive electrode active material, and in the early stage of the cycle, some active substances cannot exert their capacity. As the cycle proceeds, after the binder between the primary particles is fully infiltrated by the electrolyte, ion channels are gradually formed, and the expansion and contraction of the lithium iron phosphate material during the lithium insertion and extraction process increases the gap between the originally tightly bonded primary particles, and some active substances that were originally unable to exert their capacity are gradually activated, thereby compensating for the attenuation of the lithium iron phosphate positive electrode active material in the early stage of the cycle. On the other hand, due to the reduction in the overall polarization of the lithium iron phosphate positive electrode active material, the impedance of the battery formed by the positive electrode active material is relatively reduced, thereby showing a further increase in capacity, with a small early attenuation, no attenuation, or even a capacity increase. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] FIG1 is a schematic structural diagram of a vehicle according to an embodiment of the present application.
[0032] FIG2 is a schematic diagram of the exploded structure of a battery according to an embodiment of the present application.
[0033] FIG3 is a schematic diagram of the exploded structure of a battery cell according to an embodiment of the present application.
[0034] FIG4 is a schematic structural diagram of secondary particles according to an embodiment of the present application.
[0035] FIG5 a is a scanning electron microscope image of secondary particles according to one embodiment of the present application.
[0036] FIG5 b is another scanning electron microscope image of the secondary particles according to one embodiment of the present application.
[0037] FIG5 c is another scanning electron microscope image of the secondary particles according to one embodiment of the present application.
[0038] FIG5 d is another scanning electron microscope image of the secondary particles according to one embodiment of the present application.
[0039] FIG6 is a scanning electron microscope image of a cross section of a positive electrode sheet according to an embodiment of the present application.
[0040] FIG7 is a scanning electron microscope image of a cross section of the positive electrode sheet of Comparative Example 1.
[0041] FIG8 is an infrared spectrum of an example of an adhesive according to an embodiment of the present application. DETAILED DESCRIPTION
[0042] Below, the embodiments of the battery cells, batteries, and electrical equipment of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0043] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0044] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0045] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0046] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a method includes steps (a) and (b), which indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a method may further include step (c), which indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.
[0047] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may indicate that other components not listed may also be included or that only the listed components are included.
[0048] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0049] Lithium iron phosphate (LIFP) materials have a very stable structure, with little structural change during the initial charge and discharge process. This results in high initial charge and discharge efficiency, and the released active lithium essentially returns to the positive electrode after the initial discharge. However, during the initial use of the battery, active lithium is continuously consumed, forming a relatively stable SEI film, which results in a rapid capacity decay of LFP batteries in the early stages of cycling.
[0050] The battery disclosed in the embodiments of the present application can be used in electrical devices that use the battery as a power source or various energy storage systems that use the battery as an energy storage element. The electrical devices may be, but are not limited to, mobile phones, tablets, laptops, electric toys, power tools, battery cars, electric cars, ships, spacecraft, and the like. Among them, electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and the like, and spacecraft may include airplanes, rockets, space shuttles, and spacecraft, and the like.
[0051] For the convenience of description, the following embodiments are described by taking a vehicle 1000 as an example of an electrical device according to an embodiment of the present application.
[0052] Please refer to Figure 1, which is a schematic structural diagram of a vehicle 1000 provided in some embodiments of the present application. The vehicle 1000 can be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle can be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is provided inside the vehicle 1000, and the battery 100 can be provided at the bottom, head or tail of the vehicle 1000. The battery 100 can be used to power the vehicle 1000. For example, the battery 100 can serve as an operating power source for the vehicle 1000. The vehicle 1000 may also include a controller 200 and a motor 300. The controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the vehicle 1000.
[0053] In some embodiments of the present application, the battery 100 can serve not only as an operating power source for the vehicle 1000, but also as a driving power source for the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.
[0054] Please refer to Figure 2, which is a schematic diagram of the exploded structure of a battery 100 provided in some embodiments of the present application. The battery 100 includes a housing 10 and battery cells 20, with the battery cells 20 housed within the housing 10. The housing 10 provides a storage space for the battery cells 20 and can have various structures. In some embodiments, the housing 10 can include a first portion 11 and a second portion 12, which overlap each other and together define a storage space for the battery cells 20. The second portion 12 can be a hollow structure with one end open. The first portion 11 can be a plate-like structure, with the first portion 11 overlapping the open side of the second portion 12, so that the first portion 11 and the second portion 12 together define a storage space. Alternatively, the first portion 11 and the second portion 12 can each be a hollow structure with one end open, with the open side of the first portion 11 overlapping the open side of the second portion 12. Of course, the housing 10 formed by the first portion 11 and the second portion 12 can have various shapes, such as a cylinder or a rectangular parallelepiped.
[0055] In the battery 100, there may be multiple battery cells 20, and the multiple battery cells 20 may be connected in series, in parallel, or in a hybrid connection. A hybrid connection refers to a combination of series and parallel connections among the multiple battery cells 20. The multiple battery cells 20 may be directly connected in series, in parallel, or in a hybrid connection, and then the entire battery cell 20 may be housed within the housing 10. Alternatively, the battery 100 may be constructed by first connecting multiple battery cells 20 in series, in parallel, or in a hybrid connection to form a battery module, which is then connected in series, in parallel, or in a hybrid connection to form a complete battery module, and then housed within the housing 10. The battery 100 may also include other structures, such as a busbar assembly for electrically connecting the multiple battery cells 20.
[0056] Each battery cell 20 may be a secondary battery or a primary battery, and may also be a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, but is not limited thereto. The battery cell 20 may be cylindrical, flat, rectangular, or in other shapes.
[0057] Please refer to Figure 3, which is a schematic diagram of the exploded structure of a battery cell 20 provided in some embodiments of the present application. A battery cell 20 is the smallest unit that makes up a battery. As shown in Figure 3, a battery cell 20 includes an end cap 21, a housing 22, a cell assembly 23, and other functional components.
[0058] The end cap 21 is a component that covers the opening of the housing 22 to isolate the internal environment of the battery cell 20 from the external environment. The shape of the end cap 21 can be adapted to the shape of the housing 22 to match the housing 22. Optionally, the end cap 21 can be made of a material with a certain hardness and strength (such as an aluminum alloy). This prevents the end cap 21 from deforming when subjected to compression or collision, giving the battery cell 20 greater structural strength and improved safety. The end cap 21 can be provided with functional components such as electrode terminals 21a. The electrode terminals 21a can be used to electrically connect to the battery cell assembly 23 to output or input electrical energy to the battery cell 20. In some embodiments, the end cap 21 can also be provided with a pressure relief mechanism for relieving internal pressure when the internal pressure or temperature of the battery cell 20 reaches a threshold. The end cap 21 can also be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application are not particularly limited in this regard. In some embodiments, an insulating member may be provided inside the end cap 21 to isolate the electrical connection components in the housing 22 from the end cap 21 to reduce the risk of short circuit. For example, the insulating member may be made of plastic, rubber, or the like.
[0059] The housing 22 is a component that cooperates with the end cap 21 to form the internal environment of the battery cell 20. This internal environment can be used to accommodate the battery cell assembly 23, electrolyte, and other components. The housing 22 and end cap 21 can be separate components. An opening can be provided in the housing 22, and the end cap 21 is placed over the opening to form the internal environment of the battery cell 20. Alternatively, the end cap 21 and housing 22 can be integrated. Specifically, the end cap 21 and housing 22 can form a common connection surface before other components are inserted into the housing. When the interior of the housing 22 needs to be enclosed, the end cap 21 is placed over the housing 22. The housing 22 can have a variety of shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the housing 22 can be determined based on the specific shape and size of the battery cell assembly 23. The housing 22 can be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and this embodiment of the present application does not impose any specific limitations on this.
[0060] The cell assembly 23 is a component in the battery cell 100 where electrochemical reactions occur. One or more cell assemblies 23 may be contained in the housing 22. The cell assembly 23 is mainly formed by winding or stacking positive and negative electrode sheets, and a separator is usually provided between the positive and negative electrode sheets. The parts of the positive and negative electrode sheets with active materials constitute the main body of the cell assembly, and the parts of the positive and negative electrode sheets without active materials each constitute a tab 23a. The positive and negative electrode tabs may be located together at one end of the main body or respectively at both ends of the main body. During the charge and discharge process of the battery, the positive active material and the negative active material react with the electrolyte, and the tabs 23a connect the electrode terminals to form a current loop.
[0061] Some embodiments of the present application provide a positive electrode active material, as shown in FIG4 , the positive electrode active material includes secondary particles 30 , the secondary particles 30 include primary particles 31 and a binder 32 , the primary particles 31 include lithium iron phosphate material; at least part of the binder 32 is located between adjacent primary particles 31 .
[0062] In the technical solution of the embodiment of the present application, the primary particles 31 of the lithium iron phosphate material of the positive electrode active material are bonded by a binder 32 to form secondary particles 30. The particle size of the lithium iron phosphate secondary particles 30 is increased relative to the particle size of the primary particles 31, resulting in a relatively large polarization of the positive electrode active material, a low initial charge and discharge efficiency of the positive electrode active material, and the inability of some active materials to exert their capacity in the early stage of the cycle. As the cycle progresses, after the binder 32 between the primary particles 31 is fully infiltrated by the electrolyte, ion channels are gradually formed. In addition, the expansion and contraction of the lithium iron phosphate material during the lithium insertion and extraction process increases the gap between the originally tightly bonded primary particles 31, and some active materials that were originally unable to exert their capacity are gradually activated, thereby compensating for the attenuation of the lithium iron phosphate positive electrode active material in the early stage of the cycle. On the other hand, due to the reduction in the overall polarization of the lithium iron phosphate positive electrode active material, the impedance of the battery cell formed by the positive electrode active material is relatively reduced, thereby showing a further increase in capacity, with small early attenuation, no attenuation, or even increased capacity.
[0063] In any embodiment, the volume average particle size DV50 of the secondary particles 30 of the positive electrode active material is in the range of 2 μm to 50 μm. In the embodiment of the present application, by controlling the volume average particle size DV50 of the secondary particles 30 of the positive electrode active material to be in the range of 2 μm to 50 μm, the polarization degree of the positive electrode active material is improved, and the initial capacity of the battery is also maintained at an optimal level. Among them, the volume average particle size DV50 of the secondary particles 30 can be 2μm, 3μm, 5μm, 8μm, 10μm, 13μm, 15μm, 20μm, 22μm, 26μm, 28μm, 30μm, 35μm, 38μm, 40μm, 42μm, 45μm, 48μm, 50μm, etc., or a range consisting of any two of the above values, for example, 2μm-10μm, 10μm-22μm, 22μm-40μm, or 40μm-50μm, etc.
[0064] In any embodiment, the volume average particle size DV50 of the secondary particles 30 of the positive electrode active material is in the range of 10μm-30μm. In the embodiment of the present application, the volume average particle size DV50 of the secondary particles 30 of the positive electrode active material is in the range of 10μm-30μm, so that the polarization degree of the positive electrode active material is better, so that the early capacity of the battery is also maintained in a better state. Among them, the volume average particle size DV50 of the secondary particles 30 can be 10μm, 13μm, 15μm, 16μm, 18μm, 20μm, 22μm, 25μm, 26μm, 28μm, 30μm, etc., or a range consisting of any two of the above values, for example, 10μm-18μm, 16μm-30μm, or 25μm-30μm, etc.
[0065] In any embodiment, the volume average particle size DV50 of the primary particles 31 of the positive electrode active material body is in the range of 0.1 μm to 2 μm. In the embodiment of the present application, the volume average particle size DV50 of the primary particles 31 of the positive electrode active material is in the range of 0.1 μm to 2 μm, so that the polarization degree of the positive electrode active material is reduced during the later cycle process, so that the capacity of the battery in the later period of time remains unchanged or has a small attenuation. The volume average particle size DV50 of the primary particles 31 may be 0.1 μm, 0.2 μm, 0.3 μm, 0.5 μm, 0.6 μm, 0.8 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm or 2 μm, or a range consisting of any two of the above values, for example, 0.1 μm-0.8 μm, 0.8 μm-1.5 μm, or 1.5 μm-2 μm, etc.
[0066] In any embodiment, the volume average particle size DV50 of the primary particles 31 of the positive electrode active material body is in the range of 0.2μm-1.5μm. In the embodiment of the present application, the volume average particle size DV50 of the primary particles 31 of the positive electrode active material is in the range of 0.2μm-1.5μm, so that the polarization degree of the positive electrode active material is small during the later cycle, so that the capacity of the battery in the later stage remains unchanged or the capacity increases. Among them, the volume average particle size DV50 of the primary particles 31 can be 0.2μm, 0.3μm, 0.5μm, 0.6μm, 0.8μm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm or 1.5μm, etc., or a range composed of any two of the above values, for example, 0.2μm-0.6μm, 0.6μm-1.1μm, or 1.1μm-1.5μm, etc.
[0067] In any embodiment, the mass fraction of the binder 32 is 0.1%-2% based on the total mass of the positive electrode active material. In the embodiment of the present application, the final capacity and long-term performance of the positive electrode active material can be controlled by controlling the addition ratio of the binder 32: when the binder 32 ratio is high, the prepared secondary particles 30 material have greater polarization and lower initial capacity, but the capacity increases more significantly after the initial period; when the binder 32 ratio is low, the final prepared lithium iron phosphate material has a higher initial capacity, but decays faster in the early stages of the cycle, and the degree of improvement in the capacity decay in the early stages of the cycle is small. The mass fraction of the binder 32 based on the total mass of the positive electrode active material can be 0.1%, 0.2%, 0.3%, 0.5%, 0.6%, 0.7%, 0.8%, 1%, 1.1%, 1.2%, 1.3%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9% or 2%, or a range consisting of any two of the above values, for example, 0.1%-0.6%, 0.6%-1.2%, or 1.2%-2%, etc.
[0068] In any embodiment, the thickness of the binder 32 between adjacent primary particles 31 is in the range of 0.1 μm to 1 μm. In the embodiment of the present application, by controlling the thickness of the binder 32 to control the cross-sectional area of the ion channel formed when the electrolyte infiltrates the binder 32 of the positive electrode active material, the initial capacity attenuation of the battery can be better improved. Among them, the thickness of the binder 32 between the primary particles 31 is 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm or 1 μm, or a range consisting of any two of the above values, for example, 0.1 μm-0.4 μm, 0.4 μm-0.7 μm, or 0.7 μm-1 μm, etc.
[0069] In any embodiment, the adhesive 32 comprises:
[0070] Wherein, R1, R2, and R3 each independently include hydrogen, an unsubstituted straight-chain or branched alkyl group having 1 to 6 carbon atoms; R4 includes an unsubstituted straight-chain or branched alkyl group having 1 to 6 carbon atoms; the numerical range of m is 100-3000; the numerical range of n is 100-3000. In the embodiment of the present application, the binder 32 includes a carbonic acid group, which can increase the molecular weight of the binder 32, improve the bonding force of the binder 32, and better bond the primary particles 31 to form secondary particles 30. Wherein, the numerical value of m can be 100, 200, 500, 1000, 1500, 1800, 2000, 2500 or 3000, or a range consisting of any two of the above numerical values, such as 100-1000, 1000-2000 or 2000-3000, etc. The value of n is 100, 200, 500, 1000, 1500, 1800, 2000, 2500 or 3000, or a range consisting of any two of the above values, such as 100-1000, 1000-2000 or 2000-3000, etc.
[0071] In any embodiment, the unsubstituted linear or branched alkyl group having 1 to 6 carbon atoms includes methyl, ethyl, n-butyl or tert-butyl. In the embodiment of the present application, by further improving the bonding strength of the binder 32, the primary particles 31 can be better bonded to form the secondary particles 30.
[0072] In any embodiment, the adhesive 32 comprises: Any one or more of the .
[0073] In any embodiment, the lithium iron phosphate material includes Li x Fe y M z PO4, where M includes any one or more of Mn, Cr, Co, Cu, Ni, V, Mo, Ti, Zn, Al, Ga, Mg, B, and Nb, 0.05 ≤ x ≤ 1.2, 0.2 ≤ y ≤ 1, and 0 ≤ z ≤ 0.8. In the embodiments of the present application, the lithium iron phosphate material includes lithium iron phosphate or lithium iron phosphate doped with metal elements. Lithium iron phosphate has strong stability during the charge and discharge process. Doping the lithium iron phosphate with the above-mentioned metal elements can improve the internal conductivity of the lithium iron phosphate material primary particles 31.
[0074] In any embodiment, the lithium iron phosphate material further includes a coating layer, and the coating layer includes a carbon layer. In the embodiment of the present application, the lithium iron phosphate has a coating layer on its surface, such as a carbon layer, which can improve the conductivity of the lithium iron phosphate.
[0075] In any embodiment, the thickness of the coating layer is greater than 0 and less than or equal to 20 nm. In the embodiment of the present application, the thickness of the coating layer is controlled to control the stability and conductivity of the lithium iron phosphate material within a preferred range. The thickness of the coating layer can be 1 nm, 2 nm, 3 nm, 5 nm, 8 nm, 10 nm, 11 nm, 12 nm, 13 nm, 15 nm, 16 nm, 18 nm, 19 nm or 20 nm, or a range consisting of any two of the above values, such as 1-10, 10-15 or 15-20, etc.
[0076] A second aspect of the present application also provides a method for preparing a positive electrode active material, comprising: dispersing primary particles 31 comprising lithium iron phosphate material and a binder 32 in a solvent, and spray drying the resulting particles to form secondary particles 30, wherein at least a portion of the binder 32 is located between adjacent primary particles 31. In an embodiment of the present application, spray drying the primary particles 31 and the binder 32 to form the secondary particles 30 results in better uniformity of the secondary particles 30, easier control of the size of the secondary particles 30, and easier control of the uniformity of the binder 32 on the surface of the primary particles 31. This ensures close contact between the primary particles 31 and the binder 32 within the secondary particles 30. This results in relatively high polarization of the resulting lithium iron phosphate secondary particles 30, resulting in low initial charge and discharge efficiency, and in the early stages of cycling, some active materials are unable to fully utilize their capacity. As cycling progresses, the binder 32 between the primary particles 31 is fully infiltrated by the electrolyte, gradually forming ion channels and activating some of the active materials that were previously unable to fully utilize their capacity, thereby compensating for the initial attenuation of the lithium iron phosphate, resulting in minimal attenuation, no attenuation, or even increased capacity.
[0077] In any embodiment, the spray drying temperature range is 150° C. to 350° C. By controlling the spray drying temperature range, the particle size of the secondary particles 30 can be easily controlled. The spray drying temperature can be 150° C., 160° C., 180° C., 200° C., 210° C., 220° C., 240° C., 260° C., 300° C., 320° C., 340° C., 350° C., or a range consisting of any two of the foregoing values, such as 150° C. to 200° C., 200° C. to 260° C., or 260° C. to 350° C.
[0078] The third aspect of the present application further provides a positive electrode sheet, comprising the positive electrode active material of the first aspect of the present application and / or the positive electrode active material prepared by the method for preparing the positive electrode active material of the second aspect of the present application. Because the positive electrode sheet of the present application comprises the positive electrode active material and / or the positive electrode active material prepared by the method for preparing the positive electrode active material provided herein, it has at least the same advantages as a battery cell.
[0079] The fourth aspect of the present application further provides a battery, comprising the positive electrode sheet of the third aspect of the present application. Since the battery of the present application comprises the positive electrode sheet provided by the present application, it has at least the same advantages as the positive electrode sheet.
[0080] The fifth aspect of the present application further provides an electrical device, comprising the battery according to the fourth aspect of the present application. Since the electrical device of the present application comprises the battery provided by the present application, it has at least the same advantages as the battery.
[0081] Wherein, at 25°C, the solubility of the additive 222 in the electrolyte can be 0.01mmol / L, 0.05mmol / L, 0.08mmol / L, 0.1mmol / L, 0.15mmol / L, 0.2mmol / L, 0.3mmol / L, 0.5mmol / L, 1mmol / L, 2mmol / L, 3mmol / L, 5mmol / L, 8mmol / L, 10mmol / L, 12mmol / L, 15mmol / L, 18mmol / L, 20mmol / L, 30mmol / L, 35mmol / L, 40mmol / L, mmol / L, 46mmol / L, 50mmol / L, 54mmol / L, 60mmol / L, 65mmol / L, 70mmol / L, 75mmol / L, 80mmol / L, 87mmol / L, 90mmol / L, 95mmol / L, 98mmol / L or 100mmol / L, or a range consisting of any two of the above values, for example, 0.1mmol / L-80mmol / L, 15mmol / L-70mmol / L, 35mmol / L-60mmol / L, 46mmol / L-54mmol / L, etc.
[0082] In any embodiment, at 25°C, the solubility of the additive 222 in the electrolyte can be 100mmol / L, 105mmol / L, 110mmol / L, 120mmol / L, 125mmol / L, 130mmol / L, 140mmol / L, etc., or a range consisting of any two of the above values, for example, 100mmol / L-140mmol / L, above 140mmol / L, 105mmol / L-130mmol / L, etc.
[0083] In some embodiments, the electrolyte includes an electrolyte salt and a solvent, and the electrolyte serves to conduct ions between the positive electrode sheet and the negative electrode sheet.
[0084] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0085] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0086] [Positive electrode]
[0087] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, and the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.
[0088] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0089] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0090] In some embodiments, the positive electrode film layer may further optionally include a binder. For ease of distinction, the binder in the positive electrode active material may be referred to as a first binder, and the first binder is at least partially located between adjacent primary particles. The binder used in the positive electrode film layer may be referred to as a second binder. Preferably, the binder in the embodiment of the present application is different from the binder in the positive electrode active material. As an example, the second binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. The viscosity of the first binder is greater than the viscosity of the second binder.
[0091] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0092] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the second binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0093] [Negative electrode]
[0094] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0095] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0096] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0097] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0098] In some embodiments, the negative electrode film layer may further include a third binder. The third binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0099] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0100] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0101] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0102] [Isolation film]
[0103] In some embodiments, the battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0104] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0105] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be made into a battery cell assembly through a winding process or a lamination process.
[0106] In some embodiments, the housing 22 may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, or the like.
[0107] The present application has no particular limitation on the shape of the battery cell 20 , which may be cylindrical, square, or any other shape.
[0108] The beneficial effects of the present application are further illustrated below with reference to the examples.
[0109] In order to make the technical problems, technical solutions and beneficial effects solved by the embodiments of the present application clearer, the following will be further described in detail with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0110] Example 1
[0111]
Preparation of adhesive
[0112] Dissolve 1 mol of allyl methyl carbonate in 200 mL of tetrahydrofuran. After evacuation, continuously introduce N2 into a three-necked flask. Add 0.05 g of azobisisobutyronitrile as initiator, heat to 70°C, and stir to react for 12 hours. Pour the resulting crude product into 0°C ice ether for precipitation to obtain propylene carbonate polymer A.
[0113] Weigh 0.1 mol of propylene carbonate polymer A, add 1 mol of vinylidene fluoride, dissolve in 200 mL of tetrahydrofuran, evacuate, continuously introduce N2 into a three-necked flask, add 0.05 g of azobisisobutyronitrile initiator, heat to 70 ° C, stir and react for 12 hours, and then pour the obtained crude product into 0 ° C ice ether for sedimentation to obtain a binder, specifically a binder of formula (I) Among them, R1, R2, and R3 are all hydrogen, and R4 is methyl.
[0114] Specifically, in the embodiment of the present application, the binder is Among them, m is between 100-3000, and n is between 100-3000.
[0115] Preparation of positive electrode active materials
[0116] The primary particles of lithium iron phosphate material with a volume average particle size Dv50 of 0.6μm are mixed with the binder prepared above in a mass ratio of 99:1, dispersed in an organic solvent N-methylpyrrolidone, and spray-dried at 200°C to form secondary particles, thereby obtaining a positive electrode active material. The mass fraction of the binder is 1%, and the volume average particle size Dv50 of the secondary particles is 5.4μm. Specifically, as shown in Figures 5a-5d, the particle size distribution of the secondary particles is 2μm-20μm, the volume average particle size Dv50 of the secondary particles is 5.4μm, and the primary particles are bonded with a binder. Specifically, in the embodiment of the present application, the lithium iron phosphate material is LiFeMPO4. In the embodiment of the present application, the lithium iron phosphate material is lithium iron phosphate. In other embodiments, the lithium iron phosphate material may also be a lithium iron phosphate doped material LixFe1-yMyPO4, wherein M includes any one or more of Mn, Cr, Co, Cu, Ni, V, Mo, Ti, Zn, Al, Ga, Mg, B, and Nb, wherein the doped trace elements have little effect on the material properties. Alternatively, the lithium iron phosphate material may be a lithium iron phosphate coated with a carbon coating layer.
[0117]
Preparation of positive electrode sheet
[0118] The positive electrode active material, conductive carbon and polyvinylidene fluoride (PVDF) prepared above were mixed evenly in a mass ratio of 96:2.5:1.5, and then solvent N-methylpyrrolidone (NMP) was added to adjust the solid content to 70%-80%. After stirring evenly, the positive electrode slurry was obtained, which was then coated, dried, cold pressed and cut into positive electrode sheets.
[0119]
Preparation of negative electrode sheet
[0120] Graphite, conductive carbon SP, and binder SBR are dry-mixed at a ratio of 97:1:2, deionized water is added, and the solid content is adjusted to 45%-55%. After stirring evenly, the negative electrode slurry is obtained, which is then coated, dried, cold-pressed, and cut into negative electrode sheets.
[0121] Preparation of electrolyte
[0122] In an argon atmosphere glove box, ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 3 / 7 to obtain a solvent, LiPF6 was added to the solvent at a mass percentage of 12.5% and dissolved, and stirred to obtain an electrolyte.
[0123] [Diaphragm]
[0124] Polypropylene film is used as the isolation film.
[0125]
Battery preparation
[0126] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator positioned between the cathode and anode to provide isolation. The cells are then wound to form a bare cell. The bare cell is then placed in an outer package, injected with the prepared electrolyte, and packaged, injected, formed, and vented to produce a lithium-ion battery.
[0127] Example 2
[0128] The difference from Example 1 is that in the preparation of the positive electrode active material, the mass ratio of the lithium iron phosphate primary particles to the binder is 99.9:0.1, and the mass fraction of the binder is 0.1%. Other steps are the same as in Example 1 and will not be repeated here.
[0129] Example 3
[0130] The difference from Example 1 is that in the preparation of the positive electrode active material, the mass ratio of the lithium iron phosphate primary particles to the binder is 99.5:0.5, and the mass fraction of the binder is 0.5%. Other steps are the same as in Example 1 and will not be repeated here.
[0131] Example 4
[0132] The difference from Example 1 is that in the preparation of the positive electrode active material, the mass ratio of the lithium iron phosphate primary particles to the binder is 98.5:1.5, and the mass fraction of the binder is 1.5%. Other steps are the same as in Example 1 and will not be repeated here.
[0133] Example 5
[0134] The difference from Example 1 is that in the preparation of the positive electrode active material, the mass ratio of the lithium iron phosphate primary particles to the binder is 98:2, and the mass fraction of the binder is 2%. Other steps are the same as in Example 1 and will not be repeated here.
[0135] Example 6
[0136] The difference from Example 1 is that in the preparation of the binder, the reaction raw material is allyl ethyl carbonate, and the binder of formula (I) obtained is Wherein, R1 is hydrogen, R2 is methyl, R3 is hydrogen, and R4 is methyl. Other details are the same as those in Example 1 and will not be repeated here.
[0137] Example 7
[0138] The difference from Example 1 is that in the preparation of the binder, the reaction raw material is allyl ethyl carbonate, and the obtained binder is Wherein, R1 is hydrogen, R2 is methyl, R3 is tert-butyl, and R4 is methyl. Other details are the same as those in Example 1 and will not be repeated here.
[0139] Example 8
[0140] The difference from Example 1 is that in the preparation of the binder, 1 mol of allyl ethyl carbonate and 1 mol of vinylidene fluoride were dissolved in 200 mL of tetrahydrofuran, vacuumed, and under N2 atmosphere, 0.05 g of azobisisobutyronitrile initiator was added, heated to 70 ° C, stirred and reacted for 12 hours, and the resulting crude product was poured into 0 ° C ice ether for sedimentation to obtain the desired binder. The binder is Among them, R1 is hydrogen, R2 is methyl, R3 is hydrogen, and R4 is methyl. The obtained binder was subjected to infrared spectrum analysis, and the test results are shown in Figure 8. It can be seen from the infrared spectrum of Figure 8 that at 1183cm -1 The characteristic absorption peak of -CF2- appears at 1404cm-1, the characteristic absorption peak of -CH2- appears at 761cm-1, and the characteristic absorption peak of -CO3- appears near 761cm-1, indicating that the prepared binder contains functional groups -CF2- and -CO3-.
[0141] The rest is the same as in Example 1 and will not be described again here.
[0142] Example 9
[0143] The difference from Example 1 is that the preparation of the binder is not included. In the preparation of the positive electrode active material, the binder used is polyvinylidene fluoride (PVDF).
[0144] Example 10
[0145] The differences from Example 1 are that, in the preparation of the positive electrode active material, the volume average particle size (Dv50) of the primary particles of the lithium iron phosphate material is 0.1 μm; the spray drying temperature is 350°C; and the volume average particle size (Dv50) of the secondary particles is 2 μm. All other steps are the same as in Example 1 and are not further described here.
[0146] Example 11
[0147] The differences from Example 1 are that, in the preparation of the positive electrode active material, the volume average particle size (Dv50) of the primary particles of the lithium iron phosphate material is 0.2 μm; the spray drying temperature is 250°C; and the volume average particle size (Dv50) of the secondary particles is 5 μm. All other steps are the same as in Example 1 and are not further described here.
[0148] Example 12
[0149] The differences from Example 1 are that, in the preparation of the positive electrode active material, the volume average particle size (Dv50) of the primary particles of the lithium iron phosphate material is 1.5 μm; the spray drying temperature is 200°C; and the volume average particle size (Dv50) of the secondary particles is 20 μm. Other details are the same as in Example 1 and are not further described here.
[0150] Example 13
[0151] The differences from Example 1 are that, in the preparation of the positive electrode active material, the volume average particle size (Dv50) of the primary particles of the lithium iron phosphate material is 2 μm; the spray drying temperature is 150°C; and the volume average particle size (Dv50) of the secondary particles is 50 μm. All other steps are the same as in Example 1 and are not further described here.
[0152] Comparative Example 1
[0153] The difference from Example 1 is that the preparation of the binder and the preparation of the positive electrode active material are not included. In the preparation of the positive electrode sheet, the positive electrode active material used is lithium iron phosphate material primary particles, and the volume average particle size Dv50 of the lithium iron phosphate material primary particles is 0.6 μm.
[0154] The relevant parameter testing methods in the above embodiments and comparative examples are as follows:
[0155] 2.1) Volume average particle size Dv50 test
[0156] Equipment model: Malvern 2000 (MasterSizer 2000) laser particle size analyzer, reference standard process: GB / T19077-2016 / ISO 13320:2009, specific test process: Take an appropriate amount of the sample to be tested (the sample concentration is sufficient to ensure 8%-12% obscuration), add 20ml of deionized water, and simultaneously operate the external ultraviolet (53KHz / 120W) for 5 minutes to ensure that the sample is completely dispersed. Then, the sample is measured according to the GB / T19077-2016 / ISO 13320:2009 standard.
[0157] 2.2 Battery performance test
[0158] 2.21) DC resistance DCR test
[0159] The battery was left at rest at 25°C for 30 minutes, charged at a constant current of 0.33C to a voltage of 3.65V, and then charged at a constant voltage to a current at a cutoff current of 0.05C. The battery was then left at rest at 25°C for 5 minutes, discharged at 0.33C for 90 minutes, and discharged at a cutoff current of 0.5C. The battery was then left at rest at 25°C for 1 hour, discharged at 2C for 30 seconds, and left at rest at 25°C for another 5 minutes to measure the DC resistance (DCR).
[0160] 2.22) Capacity Test
[0161] The battery was allowed to stand at 25°C for 30 min, discharged at 0.33C to 2.5V, and allowed to stand at 25°C for 30 min; charged at 0.33C constant current to 3.65V, charged at constant voltage with a cutoff current of 0.05C; allowed to stand at 25°C for 30 min, then discharged at 0.33C to 2.5V, and allowed to stand at 25°C for 30 min, and the charge and discharge capacity of the Nth cycle was recorded.
[0162] 2.23) Cycle test
[0163] Step 1: Leave the battery at 25°C for 30 minutes, discharge at 0.33C to 2.5V, and leave it at 25°C for 30 minutes.
[0164] Step 2: Charge the battery at a constant current of 0.33C to 3.65V, then charge it at a constant voltage with a cutoff current of 0.05C and let it rest at 25°C for 30 minutes. Then, discharge it at 0.33C to 2.5V and let it rest at 25°C for 30 minutes. Repeat step 2 for 1000 cycles, and record the capacity retention rate after 1000 cycles.
[0165] Capacity retention rate CR (%) after battery cycle n times = discharge capacity at the nth cycle / discharge capacity at the first cycle × 100%.
[0166] Table 1 Process and cycle performance parameters of positive electrode active materials in various embodiments and comparative examples
[0167] Note: Formula II is a binder of formula (I), and R1, R2, and R3 are all hydrogen, and R4 is methyl; Formula III is a binder of formula (I), and R1 is hydrogen, R2 is methyl, R3 is hydrogen, and R4 is methyl; Formula IV is a binder of formula (I), and R1 is hydrogen, R2 is methyl, R3 is tert-butyl, and R4 is methyl; Formula V is a binder of formula (I), and R1 is hydrogen, R2 is methyl, R3 is hydrogen, and R4 is methyl; Temperature indicates the temperature of spray drying; Primary particles indicates the volume average particle size Dv50 of primary particles; Secondary particles indicates the volume average particle size Dv50 of secondary particles; Thickness indicates the thickness of the binder between adjacent primary particles.
[0168] Table 2 Performance parameters of positive electrode active materials in various examples
[0169] Note: Initial DCR means the first DC resistance DCR; 200-turn DCR means the DC resistance DCR at 200 turns; 500-turn DCR means the DC resistance DCR at 500 turns.
[0170] From the relevant data in Table 1, it can be seen that based on Comparative Example 1 and Examples 1-5, the volume average particle size Dv50 of the positive electrode active material of Comparative Example 1 is 0.6μm, and the volume average particle size Dv50 of the secondary particles of Examples 1-5 is in the range of 2.3μm-11.2μm. Based on Comparative Example 1, after 1000 cycles of Examples 1-5, the cycle capacity retention rate is significantly improved to 83.2%-93.7%, which is higher than 80% of Comparative Example 1. Specifically, this is because the positive electrode active materials of Examples 1-5 of the present application are formed into secondary particles by bonding the primary particles with a binder, which increases the particle size of the secondary particles, increases the initial polarization of the material, and the initial DC resistance DCR is large, resulting in a slight decrease in the initial gram capacity. As shown in Table 2, the polarization gradually decreases during the cycle. By comparing the DC resistance DCR at 200 cycles with the initial DC resistance DCR, it can be seen that the DC resistance DCR of Examples 1-5 has decreased, which causes the active lithium component contained in the lithium iron phosphate material in Examples 1-5 to be slowly released. Subsequently, ion channels are formed in the secondary particles. As the cycle progresses, the cathode polarization no longer decreases, and the DC resistance DCR begins to increase at 500 cycles. Among them, the growth rate of the DC resistance DCR of Examples 1-5 is relatively small, indicating that the overall growth rate of the DC resistance DCR of Examples 1-5 after 1000 cycles is also relatively small.
[0171] As shown in Tables 1 and 2, compared to Example 1, Examples 2-3 reduced the amount of binder added during the secondary granulation process of the lithium iron phosphate particles. The resulting secondary particles had a relatively small volume average particle size (D50), resulting in poor improvement in cycle capacity retention. In contrast, Examples 4-5 increased the amount of binder added, thereby increasing the D50 of the secondary particles and further increasing polarization. While the cycle capacity retention improved accordingly, the initial capacity decreased significantly. Therefore, by adjusting the amount of binder added, the size of the secondary particles can be controlled, thereby controlling the performance of the final battery and improving the cycle capacity retention.
[0172] Based on the adjustment of the synthetic raw materials to control the binder structure in Example 1 and Example 6-7, Example 8 controls the structure of the binder by adjusting the synthetic raw materials and the synthetic method, so that the structural formula of the binder of Example 6-8 conforms to Formula (I). Compared with Comparative Example 1, the obtained binder is used to bond the primary particles to form secondary particles, which can also improve the cycle capacity retention rate by as much as 91.3%-92.3%. The binder of Example 6-8 is used to bond the primary particles to form secondary particles, which can achieve the effect of increasing the initial polarization, increasing the initial DC resistance DCR, and improving the cycle capacity retention rate; the cycle capacity retention rate of Example 9 is also increased relative to Comparative Example 1. Example 9 uses PVDF to bond the primary particles to form secondary particles. Example 9 can also achieve the effect of some active materials being unable to exert capacity in the early stage of the cycle. As the cycle progresses, the binder PVDF between the primary particles is fully infiltrated by the electrolyte, and ion channels are gradually formed. In addition, the expansion and contraction of the lithium iron phosphate material during the lithium insertion and extraction process increase the gaps between the originally tightly bonded primary particles, and some active materials that were originally unable to exert capacity are gradually activated, thereby compensating for the attenuation of the lithium iron phosphate positive electrode active material in the early stage of the cycle.
[0173] The cycle capacity retention rate of Example 9 is less than that of Example 1 and Examples 6-8, indicating that the binder of formula (I) of Example 1 and Example 6-8 is better than that of PVDF of Example 9 in improving the cycle capacity retention rate of positive electrode active material as a binder. The main reason is that the binder of Example 1 and Example 6-8 has increased the carbonic acid group polymerization unit relative to the binder of Example 9, increased the molecular weight of the binder, improved the adhesive force of the binder, and can better bond the primary particles to form secondary particles. In addition, the carbonic acid group has better affinity with the electrolyte solvent in the battery due to similar miscible properties, and the swelling is more obvious. It can absorb electrolyte during the cycle, allowing the electrolyte to continuously infiltrate into the interior of the secondary particles, build ion paths, reduce polarization, and achieve the purpose of capacity sustained release, thereby improving the cycle capacity retention rate to a greater extent.
[0174] As shown in Figure 6, it is a scanning electron microscope image of the cross-section of the positive electrode piece of Example 1 of the present application, and Figure 7 is a scanning electron microscope image of the cross-section of the positive electrode piece of Comparative Example 1. It can be seen from Figure 6 that the primary particles of the lithium iron phosphate material in the secondary particles of the positive electrode active material of Example 1 of the present application are bonded by the binder (the first binder), and the primary particles are tightly bonded by the binder (the first binder), while the positive electrode active materials, conductive carbon and polyvinylidene fluoride binder (the second binder) in the positive electrode piece are loose and there are gaps between the positive electrode active materials, indicating that the first binder and the second binder in the positive electrode piece have different functions and different forms. The first binder can increase the initial polarization of the formed lithium iron phosphate secondary particles, and the second binder is used to bond the positive electrode active material to the current collector. As can be seen from Figure 7, in Comparative Example 1, lithium iron phosphate primary particles are used directly as the positive electrode active material, and in the positive electrode sheet formed with conductive carbon and polyvinylidene fluoride binder (second binder), the lithium iron phosphate primary particles positive electrode active materials are loose, and the second binder is used to bond the positive electrode active material to the current collector.
[0175] In summary, the cycle capacity retention rates of Examples 1 to 13 are all greater than the cycle capacity retention rate of Comparative Example 1, indicating that in the embodiment of the present application, the lithium iron phosphate positive electrode active material is bonded to the primary particles by a binder to form secondary granulation, which increases the particle size of the secondary particles, increases the initial polarization of the material, increases the initial DC resistance DCR, and some positive electrode active materials cannot play a capacity role, resulting in a slight decrease in the initial gram capacity. However, during the cycle, as the number of cycles increases, the DC resistance DCR shows a trend of first decreasing and then increasing, and the polarization of the positive electrode active material first decreases and then increases. The polarization of the positive electrode active material decreases. As the cycle proceeds, after the binder between the primary particles is fully infiltrated by the electrolyte, ion channels gradually form, and the expansion and contraction of the lithium iron phosphate material during the lithium intercalation and deintercalation process increases the gap between the originally tightly bonded primary particles. Part of the active material that was originally unable to play a capacity role is gradually activated, thereby compensating for the attenuation of the lithium iron phosphate positive electrode active material in the early stage of the cycle. As the cycle proceeds, ion channels are formed in the secondary particles, the positive electrode polarization no longer decreases, and an upward trend appears. At 500 cycles, the DC resistance DCR appears relative to the initial DCR, and the positive polarization is the same or increases.
[0176] The above is only an implementation method of the present application and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the description and drawings of this application, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A positive electrode active material, the positive electrode active material comprising secondary particles, the secondary particles comprising: primary particles, the primary particles comprising lithium iron phosphate material; A binder, at least part of which is located between adjacent primary particles.
2. The positive electrode active material according to claim 1, wherein The volume average particle size Dv50 of the secondary particles is in the range of 2 μm to 50 μm, and optionally in the range of 10 μm to 30 μm.
3. The positive electrode active material according to claim 1 or 2, wherein The volume average particle size Dv50 of the primary particles is in the range of 0.1 μm to 2 μm, and optionally in the range of 0.2 μm to 1.5 μm.
4. The positive electrode active material according to any one of claims 1 to 3, wherein Based on the total mass of the positive electrode active material, the mass fraction of the binder is 0.1%-2%.
5. The positive electrode active material according to any one of claims 1 to 4, wherein The thickness of the binder between adjacent primary particles is in the range of 0.1 μm to 1 μm.
6. The positive electrode active material according to any one of claims 1 to 5, wherein: The binder comprises: Wherein, R1, R2, and R3 each independently include hydrogen, an unsubstituted straight-chain or branched alkyl group having 1 to 6 carbon atoms; R4 includes an unsubstituted straight or branched alkyl group having 1 to 6 carbon atoms; The value range of m is 100-3000; The value range of n is 100-3000.
7. The positive electrode active material according to claim 6, wherein The unsubstituted straight-chain or branched alkyl group having 1 to 6 carbon atoms includes methyl, ethyl, n-butyl or tert-butyl.
8. The positive electrode active material according to any one of claims 1 to 7, wherein The binder comprises: Any one or more of the .
9. The positive electrode active material according to any one of claims 1 to 8, wherein The lithium iron phosphate material includes Li x Fe y M z PO4, wherein M includes any one or more of Mn, Cr, Co, Cu, Ni, V, Mo, Ti, Zn, Al, Ga, Mg, B and Nb, 0.05≦x≦1.2, 0.2≦y≦1, 0≦z≦0.
8.
10. The positive electrode active material according to any one of claims 1 to 9, wherein: The lithium iron phosphate material further includes a coating layer, and the coating layer includes carbon; optionally, the coating layer has a thickness greater than 0 and less than or equal to 20 nm.
11. A method for preparing a positive electrode active material, comprising: Primary particles including lithium iron phosphate material and a binder are dispersed in a solvent, and secondary particles are formed by spray drying, wherein at least a portion of the binder is located between adjacent primary particles.
12. The method for preparing the positive electrode active material according to claim 11, wherein: The spray drying temperature ranges from 150°C to 350°C.
13. A positive electrode sheet, comprising the positive electrode active material according to any one of claims 1 to 10 or / and a positive electrode active material prepared by the method for preparing a positive electrode active material according to claim 11 or 12.
14. A battery comprising the positive electrode sheet according to any one of claims 1 to 13.
15. An electrical device comprising the battery according to claim 14.
Citation Information
Patent Citations
Preparation method of micro-nano lithium ferric phosphate (LiFePO4) positive electrode material of lithium-ion battery
CN102173403A
Secondary battery positive electrode, secondary battery positive electrode current collector, and secondary battery
CN111656576A
Positive electrode active material, lithium iron phosphate thick electrode and preparation method and application of lithium iron phosphate thick electrode
CN115295799A
Lithium iron phosphate thick electrode and preparation method and application thereof
CN115394961A
Positive electrode material, positive electrode plate, lithium secondary battery, battery module, battery pack and device
CN116097468A
Cited By
Battery monomer, battery device and electric device
CN120413609A
Fluorine-containing copolymer, method for producing fluorine-containing polymer, particles, and aqueous dispersion
WO2025173785A1