Electrolyte and secondary battery
By using a specific electrolyte composition in lithium-ion batteries, a stable SEI film and coordination bonds on the surface of lithium cobalt oxide are formed, solving the problem of poor high-temperature storage performance of lithium-ion batteries and achieving good room-temperature cycling and high-temperature storage performance.
Patent Information
- Application Number
- PCT/CN2025/123720
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2025-09-24
- Publication Date
- 2026-11-12
AI Technical Summary
Lithium-ion batteries have good cycle performance at room temperature, but poor high-temperature storage performance and are prone to gas expansion and failure at 60°C.
An electrolyte composition with a specific ratio, including lithium salt, solvent and additives, is used to form a stable SEI film. The SEI film is formed by the nitrile groups forming stable coordination bonds with the cobalt active sites on the surface of lithium cobalt oxide, covering the catalytic active sites and inhibiting the oxidative decomposition of the electrolyte at high temperatures.
This technology improves the cycling performance of lithium-ion batteries at room temperature and their storage performance at high temperatures, reduces electrolyte gas production at high temperatures, and enhances battery stability and lifespan.
Smart Images

Figure PCTCN2025123720-FTAPPB-I100001 
Figure PCTCN2025123720-FTAPPB-I100002 
Figure PCTCN2025123720-FTAPPB-I100003
Abstract
Description
Electrolyte and secondary battery
[0001] This disclosure is based on and claims priority to Chinese Patent Application No. 202510597140.X, filed on May 9, 2025, entitled “Electrolyte and Secondary Battery”, the entire contents of which are incorporated herein by reference. Technical Field
[0002] This application relates to the field of battery technology, and in particular to an electrolyte and a secondary battery. Background Technology
[0003] In recent years, with the advancement of lithium-ion battery technology, lithium-ion batteries have been widely used in electric vehicles, drones, power tools and other fields.
[0004] Lithium-ion batteries in related technologies have good cycle performance at room temperature, but poor high-temperature storage performance. For example, they are prone to gas swelling and failure when fully charged and stored at 60°C for 7 days. Summary of the Invention
[0005] This application provides an electrolyte and a secondary battery, which enables the secondary battery to have both good room temperature cycling performance and good high-temperature storage performance. The technical solution is as follows:
[0006] On one hand, an electrolyte is provided, the electrolyte comprising: lithium salt, solvent and additives;
[0007] The lithium salt comprises the following components in the following mass fractions: lithium hexafluorophosphate 11.0%–17.0%, lithium difluorooxalate borate 0–0.5%, and lithium difluorophosphate 0–1.0%.
[0008] The solvent comprises the following components in the indicated mass fractions: ethylene carbonate 1.0%–5.0%, diethyl carbonate 8.0%–17.8%, propylene carbonate 7.0%–11.0%, propyl propionate 28.0%–49.0%, and fluoroethylene carbonate 6.0%–10.0%.
[0009] The additive comprises the following components in the indicated mass fractions: vinylene carbonate 0-0.2%, 1,3-propanesulfonate lactone 0.5%-3.0%, adiponitrile 0.5%-2.0%, 1,3,6-hexanetrionitrile 1.0%-3.5%, tris(trimethylsilyl)phosphate 0-0.5%, and tris(pentafluorophenyl)borane 0-1.2%.
[0010] The molar amount of nitrile groups in the electrolyte is greater than or equal to the molar amount of cobalt active sites on the surface of lithium cobalt oxide in the positive electrode.
[0011] In one possible implementation, the molar amount of adiponitrile in the electrolyte is n. ADN The molar amount of the 1,3,6-hexanetrionitrile is n. HTCN The molar amount of the lithium cobalt oxide is The actual specific capacity of the lithium cobalt oxide is The theoretical specific capacity of the lithium cobalt oxide is The molar amount of cobalt active sites on the lithium cobalt oxide surface relative to the total molar amount of active sites is η, n ADN n HTCN , And η satisfy the following relationship:
[0012] In another possible implementation, the mass of the lithium cobalt oxide is The electrolyte injection coefficient is d. 注液系数 The mass fraction of adiponitrile in the electrolyte is e. ADN质量分数 The molar mass of the adiponitrile is M. ADN Then n ADN , d 注液系数 e ADN质量分数 and M ADN The following relationship must be satisfied:
[0013] In another possible implementation, where half the average particle size of the lithium cobalt oxide is r, the radial number of layers of the lithium cobalt oxide octahedral crystal is x, the radial thickness of a single lithium cobalt oxide octahedral crystal is H, and half the radial thickness of a single lithium cobalt oxide octahedral crystal is h, then η, r, x, H, and h satisfy the following relationship:
[0014] Where rh-xh≥0, rh-(x+1)H<0.
[0015] In another possible implementation, the ethylene carbonate has a mass fraction of 2.0% to 5.0%.
[0016] The mass fraction of propyl propionate is 30.0% to 47.0%;
[0017] The mass fraction of the fluoroethylene carbonate is 6.0% to 9.6%;
[0018] The mass fraction of the tris(pentafluorophenyl)borane is 0.3% to 1.05%.
[0019] On the other hand, a secondary battery is provided, the secondary battery comprising: an electrolyte as described in any of the above, a negative electrode plate, a positive electrode plate disposed in the electrolyte, and a separator, wherein the negative electrode plate and the positive electrode plate are separated by the separator.
[0020] In one possible implementation, the ratio of the reversible surface capacity of the negative electrode to the reversible surface capacity of the positive electrode in the secondary battery is 1.10 to 1.25.
[0021] In another possible implementation, the positive electrode comprises lithium cobalt oxide, wherein the D50 of the lithium cobalt oxide is 4.0 μm to 7.0 μm;
[0022] The negative electrode sheet includes a silicon-carbon negative electrode material, wherein the D50 of the silicon-carbon negative electrode material is 2.0 μm to 15.0 μm.
[0023] In another possible implementation, the lithium cobalt oxide is doped with aluminum in an amount of 6000 ppm to 7000 ppm.
[0024] In another possible implementation, the silicon-carbon anode material has a silicon mass fraction of 20% to 75%.
[0025] This application provides an electrolyte comprising ethylene carbonate, propyl propionate, fluoroethylene carbonate, and tris(pentafluorophenyl)borane. These components synergistically form a stable SEI (Solid Electrolyte Interface) film on the negative electrode surface, thereby improving the cycle performance of the secondary battery at room temperature. Furthermore, the nitrile groups in adiponitrile and 1,3,6-hexanetrionitrile form stable coordination bonds with the cobalt active sites on the lithium cobalt oxide surface, covering the surface catalytic active sites and suppressing the oxidative decomposition and gas generation of the electrolyte at high temperatures. Simultaneously, the molar amount of the nitrile groups is greater than or equal to the molar amount of the cobalt active sites on the lithium cobalt oxide surface, ensuring that all cobalt in the lithium cobalt oxide is complexed with the nitrile groups, avoiding side reactions caused by residual active sites, thus improving the high-temperature storage performance of the secondary battery. Therefore, this electrolyte enables the secondary battery to possess both good room-temperature cycle performance and good high-temperature storage performance.
[0026] It should be understood that the above general description and the following detailed description are merely exemplary and do not limit this disclosure. Detailed Implementation
[0027] To make the technical solution and advantages of this application clearer, the embodiments of this application will be described in further detail below.
[0028] On one hand, embodiments of this application provide an electrolyte comprising: lithium salt, solvent, and additives;
[0029] The lithium salt comprises the following components in the following mass fractions: lithium hexafluorophosphate 11.0%–17.0%, lithium difluorooxalate borate 0–0.5%, and lithium difluorophosphate 0–1.0%.
[0030] The solvent comprises the following components in the indicated mass fractions: ethylene carbonate 1.0%–5.0%, diethyl carbonate 8.0%–17.8%, propylene carbonate 7.0%–11.0%, propyl propionate 28.0%–49.0%, and fluoroethylene carbonate 6.0%–10.0%.
[0031] The additives include the following components in the following mass fractions: vinylene carbonate 0-0.2%, 1,3-propanesulfonate lactone 0.5%-3.0%, adiponitrile 0.5%-2.0%, 1,3,6-hexanetrionitrile 1.0%-3.5%, tris(trimethylsilyl)phosphate 0-0.5%, and tris(pentafluorophenyl)borane 0-1.2%;
[0032] The molar amount of nitrile groups in the electrolyte is greater than or equal to the molar amount of cobalt active sites on the surface of lithium cobalt oxide in the positive electrode.
[0033] This application provides an electrolyte comprising ethylene carbonate, propyl propionate, fluoroethylene carbonate, and tris(pentafluorophenyl)borane. These components synergistically form a stable SEI (Solid Electrolyte Interface) film on the negative electrode surface, thereby improving the cycle performance of the secondary battery at room temperature. Furthermore, the nitrile groups in adiponitrile and 1,3,6-hexanetrionitrile form stable coordination bonds with the cobalt active sites on the lithium cobalt oxide surface, covering the surface catalytic active sites and suppressing the oxidative decomposition and gas generation of the electrolyte at high temperatures. Simultaneously, the molar amount of the nitrile groups is greater than or equal to the molar amount of the cobalt active sites on the lithium cobalt oxide surface, ensuring that all cobalt in the lithium cobalt oxide is complexed with the nitrile groups, avoiding side reactions caused by residual active sites, thus improving the high-temperature storage performance of the secondary battery. Therefore, this electrolyte enables the secondary battery to possess both good room-temperature cycle performance and good high-temperature storage performance.
[0034] For example, the mass fraction of lithium hexafluorophosphate (LiPF6) can be 11.0%, 11.5%, 12.0%, 12.5%, 13.0%, 13.5%, 14.0%, 14.5%, 15.0%, 15.5%, 16.0%, 16.5%, 17.0%, etc. Further, the mass fraction of lithium hexafluorophosphate can be from 13.0% to 16.5%.
[0035] In the embodiments of this application, LiPF6, as the main component in lithium salt, can provide high ionic conductivity and support lithium ion insertion / extraction.
[0036] For example, the mass fraction of lithium difluorooxalate borate (LiODFB) can be 0, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, etc. Further, the mass fraction of LiODFB can be from 0.1% to 0.5%.
[0037] In the embodiments of this application, LiODFB can form a strong SEI film on the negative electrode surface, preventing electrolyte decomposition on the cathode surface and corrosion of the carbon surface, thereby reducing side reactions and improving the cycle stability and durability of the battery. During charging, LiODFB can react with HF to generate stable LiDFB and LiBF4, reducing HF corrosion of the CEI and SEI films and decreasing the dissolution and redeposition of transition metals. LiODFB can also scavenge oxygen free radicals in the electrolyte, reducing the generation of oxygen and carbon dioxide and improving the electrochemical stability of the battery. In addition, LiODFB can also improve the high-temperature stability of the battery and the conductivity of the electrolyte.
[0038] For example, the mass fraction of lithium difluorophosphate (LiPO2F2) can be 0, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, etc. Further, the mass fraction of LiPO2F2 can be from 0.3% to 1.0%.
[0039] In the embodiments of this application, LiPO2F2 can significantly reduce interfacial impedance, increase electrolyte conductivity, improve battery low-temperature performance, reduce electrolyte decomposition and cathode decomposition, thereby improving battery cycle stability.
[0040] For example, the mass fraction of ethylene carbonate (EC) can be 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, etc. Further, the mass fraction of EC can be 2.0% to 5.0%.
[0041] In the embodiments of this application, EC plays an important role in the electrolyte solvent system, promoting the dissociation of metal salts and forming a stable SEI film on the negative electrode surface. This is indispensable for improving the cycle performance and cycle stability of the battery, and its reduction products can also enhance the stability of the electrolyte. However, due to the low oxidation potential of cyclic carbonates, a high content of EC will oxidize and decompose at the positive electrode to produce carbon dioxide (CO2) and carbon monoxide (CO) at a voltage of 4.45V, and will reductively decompose at the negative electrode to produce ethylene (CH2=CH2), carbon monoxide (CO), and methane (CH4). Therefore, this application limits the mass fraction of EC to no more than 5.0%.
[0042] For example, the mass fraction of diethyl carbonate (DEC) can be 8.0%, 9.0%, 10.0%, 11.0%, 12.0%, 13.0%, 14.0%, 15.0%, 16.0%, 17.0%, 17.5%, 17.75%, 17.8%, etc. Further, the mass fraction of DEC can be from 10.0% to 17.75%.
[0043] In the embodiments of this application, DEC can reduce the electrolyte concentration, improve the wettability of the electrode, and reduce concentration polarization.
[0044] For example, the mass fraction of propylene carbonate (PC) can be 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, 10.5%, 11.0%, etc. Further, the mass fraction of PC can be between 7.5% and 10.0%.
[0045] In the embodiments of this application, PC has a structure similar to EC and plays a certain role in negative electrode film formation, which contributes to improving the cycle performance of the battery.
[0046] For example, the mass fraction of propyl propionate (PP) can be 28.0%, 29.0%, 30.0%, 31.0%, 32.0%, 35.0%, 38.0%, 40.0%, 42.0%, 42.25%, 42.55%, 43.75%, 45.0%, 45.75%, 46%, 48.0%, 49.0%, etc. Further, the mass fraction of PP is between 30.0% and 47.0%.
[0047] In the embodiments of this application, PP can form a stable SEI film on the negative electrode surface, significantly improving the ionic conductivity of the electrolyte and reducing its viscosity. It also possesses a high oxidation potential and does not generate gas during full-charge storage at 60°C. Therefore, its content is relatively high (30.0%–47.0%).
[0048] For example, the mass fraction of fluoroethylene carbonate (FEC) can be 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, etc. Further, the mass fraction of FEC can be from 6.0% to 9.6%.
[0049] In the embodiments of this application, FEC is a negative electrode film-forming additive that can form a stable SEI film on the surface of the negative electrode, significantly improving the cycle performance and cycle stability of the silicon-carbon negative electrode.
[0050] For example, the mass fraction of vinylene carbonate (VC) can be 0, 0.04%, 0.05%, 0.08%, 0.1%, 0.12%, 0.15%, 0.18%, 0.2%, etc. Further, the mass fraction of VC can be from 0.04% to 0.2%.
[0051] In the embodiments of this application, VC is a negative electrode film-forming additive that can form a stable SEI film on the negative electrode surface, reduce the side reactions of the electrolyte on the negative electrode surface, and help improve the cycle stability of the battery and reduce the gas generation of the battery during charging and discharging.
[0052] For example, the mass fraction of 1,3-propanesulfonyl lactone (1,3-PS) can be 0.5%, 0.7%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 2.8%, 3.0%, etc. Further, the mass fraction of 1,3-PS can be from 0.7% to 2.5%.
[0053] In the embodiments of this application, 1,3-PS is a negative electrode film-forming additive that can form a stable SEI film on the negative electrode surface, suppress the reduction and gas generation of the electrolyte on the negative electrode surface, and help improve the cycle stability and high-temperature storage performance of the battery.
[0054] For example, the mass fraction of adiponitrile (ADN) can be 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, etc. Further, the mass fraction of ADN can be from 0.8% to 1.5%.
[0055] For example, the mass fraction of 1,3,6-hexanetrionitrile (HTCN) can be 1.0%, 1.2%, 1.5%, 1.6%, 1.8%, 2.0%, 2.2%, 2.5%, 2.8%, 3.0%, 3.2%, 3.5%, etc. Further, the mass fraction of HTCN can be from 1.5% to 3.0%.
[0056] In the embodiments of this application, both ADN and HTCN contain nitrile groups (-C≡N), which can complex with Co in lithium cobalt oxide (LiCoO2) to form stable coordination bonds, thereby suppressing gas generation during high-temperature storage of the battery.
[0057] For example, the mass fraction of tris(trimethylsilyl)phosphate (TMSP) can be 0, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, etc. Further, the mass fraction of TMSP can be from 0.05% to 0.5%.
[0058] In the embodiments of this application, TMSP is a positive electrode film-forming additive that can undergo PO-Co complexation on the positive electrode surface to generate a layer of silicate with good lithium conductivity and electrochemically stable inorganic lithium carbonate, while also having a partial dehydration effect.
[0059] For example, the mass fraction of tris(pentafluorophenyl)borane (TPFPB) can be 0, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.05%, 1.1%, 1.2%, etc. Further, the mass fraction of TFPB can be from 0.3% to 1.05%.
[0060] In the embodiments of this application, TFPB is a negative electrode film-forming additive that can significantly improve battery cycle performance in silicon-carbon negative electrode systems. In the electrolyte system, it can improve the poor battery cycle performance caused by insufficient FEC content.
[0061] In the embodiments of this application, the molar amount of nitrile groups in the electrolyte is greater than or equal to the molar amount of cobalt active sites on the surface of lithium cobalt oxide in the positive electrode.
[0062] The nitrile groups mainly come from adiponitrile and 1,3,6-hexanetrionitrile. Adiponitrile contains two nitrile groups (-C≡N), and 1,3,6-hexanetrionitrile contains three nitrile groups (-C≡N). Therefore, the molar amount of nitrile groups in the electrolyte can be expressed as 2n. ADN +3n HTCN , where n ADN n represents the molar amount of adiponitrile. HTCN This indicates the molar amount of 1,3,6-hexanetrionitrile.
[0063] The molar amount of cobalt active sites on the surface of lithium cobalt oxide can be expressed as: in, This indicates the molar amount of lithium cobalt oxide, expressed in mol. This indicates the actual specific capacity of lithium cobalt oxide, expressed in mAh / g. The theoretical specific capacity of lithium cobalt oxide is expressed in mAh / g; η represents the molar amount of cobalt active sites on the lithium cobalt oxide surface relative to the total molar amount of active sites, expressed in %.
[0064] in, This is the ratio of the amount of electricity released by a fully charged lithium cobalt oxide when discharged to the mass of the lithium cobalt oxide. It is a constant, 274 mAh / g.
[0065] Based on the above, the following relation (1) exists:
[0066] In one possible implementation, the molar amount n of adiponitrile ADN It can be expressed by the following relation (2):
[0067] Where, m ADN This indicates the mass of adiponitrile, expressed in grams (g). The mass of lithium cobalt oxide is expressed in grams (g); d 注液系数 This indicates the electrolyte injection coefficient, expressed in g / Ah; e ADN质量分数 The mass fraction of adiponitrile in the electrolyte is expressed in %; M ADN This indicates the molar mass of adiponitrile, expressed in g / mol.
[0068] In the embodiments of this application, The amount can be determined based on the mass of lithium cobalt oxide added in the actual application. ADN质量分数 The concentration ranges from 0.5% to 2.0%, M ADN The constant is 108.14 g / mol, and the electrolyte injection coefficient is 1.7 g / Ah to 2.1 g / Ah.
[0069] For example, the electrolyte injection coefficient can be 1.7 g / Ah, 1.75 g / Ah, 1.8 g / Ah, 1.85 g / Ah, 1.9 g / Ah, 1.95 g / Ah, 2.0 g / Ah, 2.05 g / Ah, 2.1 g / Ah, etc. Further, the electrolyte injection coefficient can be between 1.8 g / Ah and 2.0 g / Ah.
[0070] Similarly, the molar amount η of 1,3,6-hexanetrionitrile HTCN It can be expressed by the following relation (3):
[0071] Where, m HTCN This indicates the mass of 1,3,6-hexanetrionitrile, in grams; e HTCN质量分数 This indicates the mass fraction of 1,3,6-hexanetrionitrile in the electrolyte, expressed in %; M HTCNThis indicates the molar mass of 1,3,6-hexanetrionitrile, expressed in g / mol.
[0072] e HTCN质量分数 It ranges from 1.0% to 3.5%, M HTCN It is a constant, 161.20 g / mol.
[0073] molar amount of lithium cobalt oxide It can be expressed by the following relation (4):
[0074] in, This indicates the molar mass of lithium cobalt oxide, expressed in g / mol.
[0075] The molar amount of cobalt active sites on the lithium cobalt oxide surface relative to the total molar amount of active sites, η, can be expressed by the following equation (5):
[0076] Where rh-xH≥0, rh-(x+1)H<0.
[0077] In equation (5), r represents half of the average particle size of lithium cobalt oxide, in μm; x represents the radial number of layers of the lithium cobalt oxide octahedral crystal, which is a positive integer; H represents the radial thickness of a single lithium cobalt oxide octahedral crystal, in μm; h represents half of the radial thickness of a single lithium cobalt oxide octahedral crystal, in μm, and H = 2h.
[0078] In this embodiment, r can be determined based on the particle size of the lithium cobalt oxide added in the actual application, where H is a constant, approximately 7 × 10⁻⁶. 4 μm; x can be determined based on r and H, and thus η can be determined.
[0079] In the embodiments of this application, adiponitrile and 1,3,6-hexanetrionitrile in the electrolyte satisfy the above relationship (1), which is beneficial to improve the cycle stability of lithium cobalt oxide cathode material and suppress gas generation during high-temperature storage of battery.
[0080] On the other hand, embodiments of this application provide a method for preparing an electrolyte, which includes the following steps:
[0081] Add additives to the solvent according to the mass fraction of each component, stir or shake to mix evenly, then add lithium salt, stir or shake to mix evenly, and obtain electrolyte.
[0082] Solvents include ethylene carbonate, diethyl carbonate, propylene carbonate, propyl propionate, and fluoroethylene carbonate; additives include vinylene carbonate, 1,3-propanesulfonate lactone, adiponitrile, 1,3,6-hexanetrionitrile, tris(trimethylsilyl)phosphate, and tris(pentafluorophenyl)borane; and lithium salts include lithium hexafluorophosphate, lithium difluorooxalate borate, and lithium difluorophosphate.
[0083] In preparing the electrolyte, ethylene carbonate, diethyl carbonate, propylene carbonate, propyl propionate, and fluoroethylene carbonate can be mixed evenly first. Then, vinylene carbonate, 1,3-propanesulfonate lactone, adiponitrile, 1,3,6-hexanetrionitrile, tris(trimethylsilyl)phosphate, and tris(pentafluorophenyl)borane are added to the mixed solvent and stirred or shaken until evenly mixed. Then, lithium hexafluorophosphate, lithium difluorooxalate borate, and lithium difluorophosphate are added to the mixture and stirred or shaken until evenly mixed to obtain the electrolyte.
[0084] On the other hand, an embodiment of this application provides a secondary battery, which includes: any of the electrolytes described above, a negative electrode, a positive electrode, and a separator disposed in the electrolyte, wherein the negative electrode and the positive electrode are separated by the separator.
[0085] The secondary battery provided in this application embodiment has all the advantages of electrolyte. This secondary battery can be applied to fields such as high-power drones and power tools, without specific limitations.
[0086] In one possible implementation, the positive electrode includes: lithium cobalt oxide, wherein the D50 of the lithium cobalt oxide is 4.0 μm to 7.0 μm;
[0087] The negative electrode includes silicon-carbon negative electrode material, with a D50 of 2.0 μm to 15.0 μm.
[0088] For example, the D50 of lithium cobalt oxide can be 4.0 μm, 4.5 μm, 5.0 μm, 5.5 μm, 6.0 μm, 6.5 μm, 7.0 μm, etc., and the D50 of silicon-carbon anode materials can be 2.0 μm, 3.0 μm, 4.0 μm, 5.0 μm, 6.0 μm, 7.0 μm, 8.0 μm, 9.0 μm, 10.0 μm, 11.0 μm, 12.0 μm, 13.0 μm, 14.0 μm, 15.0 μm, etc. Further, the D50 of silicon-carbon anode materials is 4.0 μm to 10.0 μm.
[0089] In the embodiments of this application, lithium cobalt oxide with a D50 of 4.0 μm to 7.0 μm has a suitable specific surface area, which can ensure that the nitrile groups in the electrolyte can fully cover the cobalt active sites, suppress cobalt dissolution and oxygen release, thereby improving the battery's storage performance at high temperatures.
[0090] Silicon expands by up to 300% during lithium intercalation. Silicon-carbon anode materials with a D50 between 2.0 μm and 15.0 μm can alleviate expansion stress through the following mechanisms: (1) the internal pores of micron-sized silicon-carbon particles can accommodate part of the volume expansion; (2) severe agglomeration of nano-silicon (<1 μm) due to excessive surface energy is avoided. Furthermore, the multi-scale particle size distribution of silicon-carbon anode materials can form an interlocking structure, improving the mechanical integrity of the electrode.
[0091] In one possible implementation, lithium cobalt oxide is doped with aluminum at a concentration of 6000 ppm to 7000 ppm.
[0092] For example, the aluminum doping amounts are 6000ppm, 6100ppm, 6200ppm, 6300ppm, 6400ppm, 6500ppm, 6600ppm, 6700ppm, 6800ppm, 6900ppm, 7000ppm, etc. Further, the aluminum doping amounts are 6300ppm to 6800ppm.
[0093] In this embodiment, lithium cobalt oxide is doped with aluminum. Aluminum can replace some of the cobalt, forming strong Al-O bonds with O, significantly improving crystal field stability. Furthermore, aluminum doping can suppress the erosion of cobalt by HF generated from the decomposition of LiPF6 in the electrolyte, reducing cobalt leaching and thus improving the battery's storage performance at high temperatures. An aluminum doping level of 6000ppm to 7000ppm can balance battery cycle life and high-temperature storage performance.
[0094] In one possible implementation, the positive electrode further includes: a first conductive agent and a first binder; wherein the mass fraction of lithium cobalt oxide is 90% to 99%, the mass fraction of the first binder is 0.5% to 5%, and the mass fraction of the first conductive agent is 0.5% to 6%.
[0095] For example, the mass fraction of lithium cobalt oxide can be 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, etc. Further, the mass fraction of lithium cobalt oxide can be 93% to 97%.
[0096] The mass fraction of the first adhesive can be 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc. Further, the mass fraction of the first adhesive can be from 0.8% to 2.5%.
[0097] The mass fraction of the first conductive agent can be 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, etc. Further, the mass fraction of the first conductive agent can be 1% to 3%.
[0098] In one possible implementation, the first conductive agent is selected from at least one of conductive carbon black (SP), carbon nanotubes (CNTs), and carbon nanofibers (VGCF); the first binder is selected from polyvinylidene fluoride (PVDF).
[0099] In preparing the positive electrode sheet, lithium cobalt oxide, a first conductive agent, and a first binder can be added to the solvent. By adjusting the amount of solvent, the solid content of the positive electrode slurry can be made to be 50% to 70%. Then, the positive electrode slurry is coated on the positive electrode current collector and dried to obtain the positive electrode sheet.
[0100] For example, the solid content of the positive electrode slurry can be 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, etc.
[0101] In one possible implementation, the areal density of the positive electrode is 2.0 mg / cm³. 2 ~22.0 mg / cm 2 .
[0102] For example, the areal density of the positive electrode can be 2.0 mg / cm³. 2 3.0 mg / cm 2 5.0 mg / cm 2 6.0 mg / cm 2 8.0 mg / cm 2 10.0 mg / cm 2 12.0 mg / cm 2 13.0 mg / cm 2 15.0 mg / cm 2 18.0 mg / cm 2 19.0 mg / cm 2 20.0 mg / cm 2 21.0 mg / cm 2 22.0 mg / cm 2 Furthermore, the areal density of the positive electrode can be 10.0 mg / cm³. 2 ~18.0 mg / cm 2 .
[0103] In the embodiments of this application, setting the areal density of the positive electrode sheet in this way helps to improve the energy density of the battery.
[0104] In one possible implementation, the compaction density of the positive electrode sheet is 3.6 g / cm³. 3 ~3.9g / cm 3 .
[0105] For example, the compaction density of the positive electrode sheet can be 3.6 g / cm³.3 3.65g / cm 3 3.7g / cm 3 3.75g / cm 3 3.8g / cm 3 3.85g / cm 3 3.9g / cm 3 Furthermore, the compaction density of the positive electrode sheet can be 3.65 g / cm³. 3 ~3.85g / cm 3 .
[0106] In this embodiment, the compaction density is 3.6 g / cm³. 3 ~3.9g / cm 3 The positive electrode can increase the volumetric energy density of the battery.
[0107] In one possible implementation, the silicon mass fraction in the silicon-carbon anode material is 20% to 75%.
[0108] In silicon-carbon anode materials, the mass fraction of silicon refers to the value of the mass of silicon / (mass of silicon + mass of carbon).
[0109] For example, the mass fraction of silicon can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, etc. Further, the mass fraction of silicon can be 30% to 60%.
[0110] In the embodiments of this application, when the mass fraction of silicon is less than 20%, the battery capacity gain is not significant. When the mass fraction of silicon is greater than 75%, the carbon matrix cannot effectively buffer the expansion stress, leading to a surge in the electrode pulverization rate. Therefore, the mass fraction of silicon is limited to between 20% and 75%, which can both improve the battery capacity and effectively buffer the expansion stress.
[0111] In one possible implementation, the negative electrode further includes a second conductive agent and a second binder, wherein the mass fraction of the silicon-carbon negative electrode (SiC) is 89% to 97%, the mass fraction of the second conductive agent is 0.5% to 6%, and the mass fraction of the second binder is 0.5% to 5%.
[0112] For example, the mass fraction of the silicon-carbon anode can be 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, etc. Further, the mass fraction of the silicon-carbon anode can be 89% to 95%.
[0113] The mass fraction of the second conductive agent can be 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, etc. Further, the mass fraction of the second conductive agent can be from 1.5% to 4.5%.
[0114] The mass fraction of the second adhesive can be 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc. Further, the mass fraction of the second adhesive can be between 0.5% and 2%.
[0115] In one possible implementation, the second conductive agent is selected from at least one of conductive carbon black (SP), carbon nanotubes (CNTs), and graphene; the second binder is selected from polyacrylic acid (PAA).
[0116] In preparing the negative electrode sheet, silicon-carbon negative electrode, second conductive agent and second binder can be added to the solvent. By adjusting the amount of solvent, the solid content of the negative electrode slurry is made to be 5% to 25%. Then, the negative electrode slurry is coated on the negative electrode current collector and dried to obtain the negative electrode sheet.
[0117] For example, the solid content of the negative electrode slurry can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, etc.
[0118] The areal density of the negative electrode sheet can be the same as or different from that of the positive electrode sheet; there is no specific limitation on this. Similarly, the compacted density of the negative electrode sheet can be the same as or different from that of the positive electrode sheet; there is no specific limitation on this.
[0119] In one possible implementation, the ratio of the reversible surface capacity of the negative electrode to the reversible surface capacity of the positive electrode (reversible N / P) of the secondary battery is 1.10 to 1.25.
[0120] Among them, the reversible areal capacity of the negative electrode is used to represent the number of lithium ions that can be reversibly inserted and removed during the charging and discharging process of the negative electrode material, and the reversible areal capacity of the positive electrode is used to represent the number of lithium ions that can be reversibly inserted or removed from the positive electrode material.
[0121] The reversible areal capacity of the negative electrode can be expressed by the following formula (6): Anode single-sided areal density × specific charge capacity of silicon-carbon negative electrode material × mass fraction of silicon-carbon negative electrode material (6)
[0122] The reversible areal capacity of the positive electrode can be expressed by the following formula (7): Anode single-sided areal density × Lithium cobalt oxide discharge specific capacity × Lithium cobalt oxide mass fraction (7)
[0123] Accordingly, the reversible N / P can be expressed by the following formula (8):
[0124] Among them, the mass fraction of silicon-carbon anode material represents the mass fraction of silicon-carbon anode material in the anode sheet, and the mass fraction of lithium cobalt oxide represents the mass fraction of lithium cobalt oxide in the cathode sheet.
[0125] For example, the value of reversible N / P can be 1.10, 1.11, 1.12, 1.13, 1.15, 1.16, 1.18, 1.20, 1.22, 1.24, 1.25, etc. Further, the value of reversible N / P can be between 1.12 and 1.15.
[0126] In the embodiments of this application, when the reversible N / P value is in the range of 1.10 to 1.25, the negative electrode has enough lithium insertion sites to accommodate the lithium extracted from the positive electrode, which will not lead to lithium plating on the negative electrode, and the battery can be cycled and reversibly charged and discharged.
[0127] In the embodiments of this application, a certain preload is required during battery testing, and the preload can be 0.2 N·m to 0.8 N·m.
[0128] For example, the preload can be 0.2 N·m, 0.3 N·m, 0.4 N·m, 0.5 N·m, 0.6 N·m, 0.7 N·m, 0.8 N·m, etc. Further, the preload can be 0.3 N·m to 0.5 N·m.
[0129] In the embodiments of this application, the positive electrode, negative electrode and separator can be stacked in a "Z" shape using a stacking process, and then the secondary battery is obtained through processes such as tab welding, packaging, cell baking, liquid injection, sealing, resting and wetting, formation, second sealing and degassing, capacity testing, aging, DC internal resistance (DCIR) testing and sorting.
[0130] The secondary battery provided in this application has an upper operating voltage limit of 4.45V; its discharge capacity retention rate is ≥98% at 6C / 0.5C rates; its cycle count is >500 cycles with a capacity retention rate of 80% at room temperature (0.5C / 3C); it does not produce gas after 7 days of fully charged storage at 60℃; and it maintains a charge retention rate of ≥94% and a capacity recovery rate of ≥99% after 28 days of fully charged storage at room temperature. Therefore, the secondary battery provided in this application can simultaneously achieve both room temperature cycling performance and 7-day fully charged storage performance at 60℃.
[0131] The technical solution of this application will be described in detail below through specific embodiments.
[0132] In the following specific embodiments, unless otherwise specified, all operations shall be performed under normal conditions or conditions recommended by the manufacturer.
[0133] Example 1
[0134] Example 1 provides an electrolyte, as shown in Table 1, which comprises: 16.0% LiPF6, 0.4% LiODFB, 0.4% LiPO2F2, 4.5% EC, 14.0% DEC, 8.0% PC, 43.75% PP, 9.5% FEC, 0.05% VC, 0.8% 1,3-PS, 0.9% ADN, 1.6% HTCN, 0.10% TMSP, and 0.00% TFPPB.
[0135] The preparation method of this electrolyte is as follows:
[0136] Mix 4.5% EC, 14.0% DEC, 8.0% PC, 43.75% PP and 9.5% FEC thoroughly. Then add 0.05% VC, 0.8% 1,3-PS, 0.9% ADN, 1.6% HTCN and 0.10% TMSP, mix thoroughly, and then add 16.0% LiPF6, 0.4% LiODFB and 0.4% LiPO2F2. Mix thoroughly to obtain the electrolyte.
[0137] The secondary battery based on the electrolyte includes: the electrolyte, a positive electrode, a negative electrode, and a separator disposed in the electrolyte, wherein the positive electrode and the negative electrode are separated by the separator.
[0138] The positive electrode comprises: 95% rate-controlled lithium cobalt oxide, 2.5% PVDF, and 2.5% SP. The D50 of the lithium cobalt oxide is 6 μm, and the areal density of the positive electrode is 15.0 mg / cm³. 2 The compacted density is 3.8 g / cm³. 3 .
[0139] The negative electrode comprises 95% power-type silicon-carbon negative electrode material, 2% PAA and 3% CNTs. The D50 of the silicon-carbon negative electrode material is 8μm, and the silicon / (silicon + carbon) ratio is 50%.
[0140] The reversible N / P ratio is 1.13, and the ratio of the molar amount of nitrile groups in the electrolyte to the molar amount of cobalt active sites on the lithium cobalt oxide surface is 1.1.
[0141] Example 2
[0142] Example 2 provides an electrolyte, see Table 1. The formulation of this electrolyte is the same as that of Example 1, except that the mass fraction of PP is 45.75%, the mass fraction of FEC is 6.5%, and the mass fraction of TPPPB is 1.00%.
[0143] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0144] Example 3
[0145] Example 3 provides an electrolyte, see Table 1. The formulation of this electrolyte is the same as that of Example 1, except that the mass fraction of EC is 2.5% and the mass fraction of PP is 45.75%.
[0146] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0147] Example 4
[0148] Example 4 provides an electrolyte, see Table 1. The formulation of this electrolyte is the same as that of Example 1, except that the mass fraction of PP is 45.25% and the mass fraction of FEC is 8.0%.
[0149] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0150] Example 5
[0151] Example 5 provides an electrolyte, see Table 1. The formulation of this electrolyte is the same as that of Example 1, except that the mass fraction of PP is 42.55% and the mass fraction of HTCN is 2.8%.
[0152] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0153] The ratio of the molar amount of nitrile groups in the electrolyte to the molar amount of cobalt active sites on the lithium cobalt oxide surface is 1.3.
[0154] Example 6
[0155] Example 6 provides an electrolyte, see Table 1. The formulation of this electrolyte is the same as that of Example 1, except that the mass fraction of DEC is 17.75% and the mass fraction of PP is 40.00%.
[0156] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0157] Example 7
[0158] Example 7 provides an electrolyte, see Table 1. The formulation of this electrolyte is the same as that of Example 1, except that the mass fraction of PP is 46.75% and the mass fraction of FEC is 6.5%.
[0159] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0160] Comparative Example 1
[0161] Comparative Example 1 provides an electrolyte, as shown in Table 2. The formulation of this electrolyte can be found in Example 1, and will not be repeated here.
[0162] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, the difference being that the ratio of silicon to (silicon + carbon) is 76%.
[0163] Comparative Example 2
[0164] Comparative Example 2 provides an electrolyte, as shown in Table 2. The formulation of this electrolyte can be found in Example 1, and will not be repeated here.
[0165] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, the difference being that the reversible N / P value is 1.05.
[0166] Comparative Example 3
[0167] Comparative Example 3 provides an electrolyte, as shown in Table 2. The formulation of this electrolyte is the same as that in Example 1, except that the mass fraction of PP is 44.95%, the mass fraction of ADN is 0.4%, and the mass fraction of HTCN is 0.9%.
[0168] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1. The difference is that the ratio of the molar amount of nitrile groups to the molar amount of cobalt active sites on the surface of lithium cobalt oxide in the electrolyte is 0.8.
[0169] Comparative Example 4
[0170] Comparative Example 4 provides an electrolyte, as shown in Table 2. The formulation of this electrolyte is the same as that in Example 1, except that the mass fraction of EC is 0.5% and the mass fraction of PP is 47.75%.
[0171] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0172] Comparative Example 5
[0173] Comparative Example 5 provides an electrolyte, as shown in Table 2. The formulation of this electrolyte is the same as that in Example 1, except that the mass fraction of FEC is 5.0% and the mass fraction of PP is 48.25%.
[0174] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0175] Comparative Example 6
[0176] Comparative Example 6 provides an electrolyte, as shown in Table 2. The formulation of this electrolyte is the same as that in Example 1, except that the mass fraction of DEC is 8.25% and the mass fraction of PP is 49.5%.
[0177] The preparation method of the electrolyte and the secondary battery based on the electrolyte can be found in Example 1, and will not be repeated here.
[0178] Table 1
[0179] Table 2
[0180] This application conducted performance tests on the batteries prepared in Examples 1-7 and Comparative Examples 1-6. The test items are as follows:
[0181] (1) Rate performance at room temperature (6°C / 0.5°C):
[0182] At 25±2℃, place the battery in the test clamp, apply a certain pre-tightening force, connect it to the charge / discharge cabinet, charge it to 4.45V with a constant current of 0.5C, then charge it to 0.05C with a constant voltage, let it rest for 30 minutes, and then discharge it to 2.5V with a constant current of 0.5C. Record the 0.5C discharge capacity. Let it rest for 30 minutes, and finally charge it to 4.45V with a constant current of 0.5C, then charge it to 0.05C with a constant voltage, let it rest for 30 minutes, and then discharge it to 2.5V with a constant current of 6C. Record the 6C discharge capacity.
[0183] The capacity retention rate at room temperature (6C / 0.5C) = 6C discharge capacity / 0.5C discharge capacity.
[0184] (2) Cyclic performance at room temperature (0.5°C / 3°C):
[0185] At 25±2℃, place the battery in the test clamp, apply a certain pre-tightening force, connect it to the charge / discharge cabinet, charge at a constant current of 0.5C to 4.45V, then charge at a constant voltage to 0.05C, let it rest for 30 minutes, discharge at a constant current of 3C to 2.5V, let it rest for 30 minutes, and repeat the above steps. Record the discharge capacity of the first cycle as the initial discharge capacity Q1, and record the discharge capacity of the Nth cycle as Q. N Record the discharge capacity of the (N+1)th cycle as Q. N+1 When Q N / Q1≥80% and Q N+1 When / Q1 < 80%, record N as the number of battery cycles at room temperature (0.5C / 3C).
[0186] (3) Performance of 7 days of full-charge storage at 60℃:
[0187] At 25±2℃, place the battery in the test clamp, apply a certain pre-tightening force, connect it to the charge / discharge cabinet, let it rest for 10 minutes, discharge it at a constant current of 0.2C to 2.5V, let it rest for 30 minutes, charge it at a constant current of 0.2C to 4.45V, then charge it at a constant voltage to 0.02C, let it rest for 30 minutes, discharge it at a constant current of 0.2C to 2.5V, let it rest for 30 minutes, charge it at a constant current of 0.2C to 4.45V, then charge it at a constant voltage to 0.02C, and let it rest for 10 minutes. Remove the battery clamp, place it in a 60℃ oven, and leave it for 7 days. After 7 days, remove the battery from the oven and observe the battery swelling and bulging.
[0188] (4) Performance of 28 days of full-charge storage at room temperature:
[0189] At 25±2℃, place the battery in the test clamp, apply a certain pre-tightening force, connect it to the charge / discharge cabinet, let it rest for 10 minutes, discharge it at a constant current of 0.2C to 2.5V, let it rest for 30 minutes, charge it at a constant current of 0.2C to 4.45V, then charge it at a constant voltage to 0.02C, let it rest for 30 minutes, discharge it at a constant current of 0.2C to 2.5V, let it rest for 30 minutes, charge it at a constant current of 0.2C to 4.45V, then charge it at a constant voltage to 0.02C, let it rest for 10 minutes, and record the battery's initial discharge capacity at 0.2C. Remove the battery clamp, place it in a 25℃ oven, and leave it for 28 days. After 28 days, remove the battery from the oven.
[0190] Place the battery in the test clamp, apply a certain preload, connect it to the charge / discharge cabinet, let it rest for 30 minutes, then discharge it at a constant current of 0.2C to 2.5V, let it rest for 30 minutes, then charge it at a constant current of 0.2C to 4.45V, then charge it at a constant voltage to 0.02C, and let it rest for 30 minutes. Repeat this process 4 times. Record the discharge capacity of the first cycle as the remaining capacity, and the maximum value among the discharge capacities of the second, third, and fourth cycles as the recovered capacity.
[0191] Remaining capacity retention rate = (remaining capacity / initial discharge capacity) * 100%;
[0192] Recovery capacity retention rate = (recovery capacity / initial discharge capacity) * 100%.
[0193] The test results are shown in Table 3.
[0194] Table 3
[0195] According to the test results of Example 1 and Comparative Example 1, the higher the silicon / (silicon + carbon) ratio, the worse the battery's room temperature cycle performance. According to the test results of Example 1 and Comparative Example 2, when the reversible N / P value is below 1.10, the battery's room temperature cycle performance deteriorates. According to the test results of Example 5 and Comparative Example 3, when the molar amount of nitrile groups in the electrolyte is less than the molar amount of cobalt active sites on the lithium cobalt oxide surface, the battery will swell with gas after being fully charged and stored at 60°C for 7 days. According to the test results of Example 3 and Comparative Example 4, the lower the EC mass fraction, the worse the battery's room temperature cycle performance. According to the test results of Example 4 and Comparative Example 5, the lower the FEC mass fraction, the worse the battery's room temperature cycle performance. According to the test results of Example 2 and Example 7, the lower the TPPPB mass fraction, the worse the battery's room temperature cycle performance. According to the test results of Example 6 and Comparative Example 6, the higher the PP mass fraction, the worse the battery's room temperature cycle performance.
[0196] The above description is only for the purpose of enabling those skilled in the art to understand the technical solution of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. An electrolyte, characterized in that, The electrolyte comprises: lithium salt, solvent, and additives; The lithium salt comprises the following components in the following mass fractions: lithium hexafluorophosphate 11.0%–17.0%, lithium difluorooxalate borate 0–0.5%, and lithium difluorophosphate 0–1.0%. The solvent comprises the following components in the indicated mass fractions: ethylene carbonate 1.0%–5.0%, diethyl carbonate 8.0%–17.8%, propylene carbonate 7.0%–11.0%, propyl propionate 28.0%–49.0%, and fluoroethylene carbonate 6.0%–10.0%. The additive comprises the following components in the indicated mass fractions: vinylene carbonate 0-0.2%, 1,3-propanesulfonate lactone 0.5%-3.0%, adiponitrile 0.5%-2.0%, 1,3,6-hexanetrionitrile 1.0%-3.5%, tris(trimethylsilyl)phosphate 0-0.5%, and tris(pentafluorophenyl)borane 0-1.2%. The molar amount of nitrile groups in the electrolyte is greater than or equal to the molar amount of cobalt active sites on the surface of lithium cobalt oxide in the positive electrode.
2. The electrolyte according to claim 1, characterized in that, The molar amount of adiponitrile in the electrolyte is n. ADN The molar amount of the 1,3,6-hexanetrionitrile is n. HTCN The molar amount of the lithium cobalt oxide is The actual specific capacity of the lithium cobalt oxide is The theoretical specific capacity of the lithium cobalt oxide is The molar amount of cobalt active sites on the lithium cobalt oxide surface relative to the total molar amount of active sites is η, n ADN n HTCN , And η satisfy the following relationship:
3. The electrolyte according to claim 2, characterized in that, The mass of the lithium cobalt oxide is The electrolyte injection coefficient is d. 注液系数 The mass fraction of adiponitrile in the electrolyte is e. ADN质量分数 The molar mass of the adiponitrile is M. ADN Then n ADN , d 注液系数 e ADN质量分数 and M ADN The following relationship must be satisfied:
4. The electrolyte according to claim 2, characterized in that, The average particle size of the lithium cobalt oxide is 1 / 2 r, the radial number of layers of the lithium cobalt oxide octahedral crystal is x, the radial thickness of a single lithium cobalt oxide octahedral crystal is H, and 1 / 2 of the radial thickness of a single lithium cobalt oxide octahedral crystal is h. Then η, r, x, H, and h satisfy the following relationship: Where rh-xH≥0, rh-(x+1)H<0.
5. The electrolyte according to claim 1, characterized in that, The mass fraction of the ethylene carbonate is 2.0% to 5.0%; The mass fraction of propyl propionate is 30.0% to 47.0%; The mass fraction of the fluoroethylene carbonate is 6.0% to 9.6%; The mass fraction of the tris(pentafluorophenyl)borane is 0.3% to 1.05%.
6. A secondary battery, characterized in that, The secondary battery includes: an electrolyte as described in any one of claims 1 to 5, a negative electrode, a positive electrode, and a separator disposed in the electrolyte, wherein the negative electrode and the positive electrode are separated by the separator.
7. The secondary battery according to claim 6, characterized in that, The ratio of the reversible surface capacity of the negative electrode to the reversible surface capacity of the positive electrode in the secondary battery is 1.10 to 1.
25.
8. The secondary battery according to claim 6, characterized in that, The positive electrode includes lithium cobalt oxide, wherein the D50 of the lithium cobalt oxide is 4.0 μm to 7.0 μm; The negative electrode sheet includes a silicon-carbon negative electrode material, wherein the D50 of the silicon-carbon negative electrode material is 2.0 μm to 15.0 μm.
9. The secondary battery according to claim 8, characterized in that, The lithium cobalt oxide is doped with aluminum at a concentration of 6000 ppm to 7000 ppm.
10. The secondary battery according to claim 8, characterized in that, The silicon mass fraction in the silicon-carbon anode material is 20% to 75%.