Silicon-carbon negative electrode material, preparation method therefor, and battery
By designing a hierarchical pore structure and gradient pore size in silicon-carbon anode materials, the problems of lithium-ion insertion/extraction difficulties and uneven silicon specific capacity were solved, achieving high initial efficiency and high specific capacity battery performance.
Patent Information
- Application Number
- PCT/CN2026/091583
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-08-26
- Filing Date
- 2026-04-20
- Publication Date
- 2026-11-12
AI Technical Summary
In existing technologies, lithium ions are difficult to intercalate and deintercalate in the ultra-micropores of silicon-carbon anode materials, resulting in reduced initial efficiency. Furthermore, the specific capacity of silicon varies in different pores, making it difficult to maximize its efficiency.
A multi-level porous silicon-carbon composite material was prepared by using a porous carbon matrix with a pore size gradient distribution that increases from the inside to the outside, and by coating a mesoporous silica layer on the surface of a MOF template using a sol-gel method, combined with chemical vapor deposition of silicon particles.
It improves silicon utilization and initial efficiency, enhances electrolyte wetting and diffusion, strengthens the structural stability of the porous carbon skeleton, and improves the battery's specific capacity and cycle performance.
Smart Images

Figure CN2026091583_12112026_PF_FP_ABST
Abstract
Description
A silicon-carbon anode material, its preparation method and battery
[0001] Cross-reference to related applications
[0002] This invention claims priority to Chinese Patent Application No. 202511199670.5, filed on August 26, 2025, entitled "A High Specific Capacity and High First-Efficiency Silicon-Carbon Anode Material, Its Preparation Method and Battery", the entire contents of which are incorporated herein by reference and constitute a part of this application for all purposes. Technical Field
[0003] This invention belongs to the technical field of silicon-carbon anode materials, specifically relating to a silicon-carbon anode material, its preparation method, and a battery. Background Technology
[0004] The statements in this section are merely background information related to this application and do not necessarily constitute prior art.
[0005] To improve battery energy density, silicon anodes can effectively replace traditional graphite due to their ultra-high capacity. Vapor-deposited silicon-carbon anodes have become a research hotspot due to their excellent properties such as low expansion and good cycle life. This technology uniformly deposits silicon particles within the pores of porous carbon to form a silicon-carbon composite material. The pore size, proportion, and distribution of the porous carbon are key factors determining the material's electrical properties (such as capacity, first-cycle efficiency, and cycle life), thus becoming a focus of research.
[0006] While existing porous carbon materials exhibit pore structures with varying pore sizes, such as micropores, micropores, and macropores, each pore size plays a different role and can improve the initial efficiency and safety performance of silicon-carbon anode materials to some extent. However, the utilization rate of silicon in micropores is low, making it difficult for lithium ions to be inserted and extracted during discharge, leading to a decrease in initial efficiency. Furthermore, the specific capacity of silicon varies at different locations within the same pore; without optimization of the pore structure, the specific capacity of silicon may not be maximized. Summary of the Invention
[0007] To overcome the shortcomings of the prior art, this application provides a silicon-carbon anode material, its preparation method, and a battery.
[0008] To achieve the above objectives, one or more embodiments of this application provide the following technical solutions:
[0009] In a first aspect, the present invention provides a silicon-carbon anode material, comprising a porous carbon matrix and silicon particles deposited within the porous carbon matrix;
[0010] The porous carbon matrix has a pore size gradient distribution, with the pore size increasing from the inside to the outside. The average pore size of the innermost region is 0.5-1 nm, the average pore size of the middle region is 1-5 nm, and the average pore size of the outermost region is 5-20 nm.
[0011] Secondly, the present invention provides a method for preparing the silicon-carbon anode material, comprising the following steps:
[0012] Metal-organic framework (MOF) particles were dispersed in a mesoporous silica precursor solution, and a mesoporous silica layer was coated on the MOF surface using the sol-gel method to obtain a MOF core-mesoporous shell composite template.
[0013] After the MOF core-mesoporous shell composite template is impregnated with a carbon source dispersion and dried, it is first carbonized at a low temperature at a first temperature and then carbonized at a high temperature at a second temperature.
[0014] After carbonization, the composite template is removed, resulting in porous carbon.
[0015] Silicon particles are deposited in porous carbon via chemical vapor deposition to obtain silicon-carbon composite materials.
[0016] Thirdly, the present invention provides a battery in which the active material of the negative electrode is the silicon-carbon negative electrode material.
[0017] The above one or more technical solutions have the following beneficial effects:
[0018] In the process of silicon delithiation, the further inside the silicon, the more difficult the delithiation becomes. The porous carbon in the silicon-carbon composite material of this invention has smaller pore sizes and less silicon deposition in the inner region. By reducing the amount of silicon deposited inside, the utilization rate of silicon can be effectively improved, thereby increasing the specific capacity and thus improving the first-efficiency performance.
[0019] The porous carbon in the silicon-carbon composite material of this invention has a larger pore size near the outer region, which not only helps to improve the wetting and diffusion of the electrolyte, but also allows the deposited silicon particles to have a larger particle size. Larger silicon particles have a smaller specific surface area, which can reduce the side reactions between silicon and electrolyte, thus improving the initial efficiency.
[0020] In addition, the innermost pore size of porous carbon is small, and the pore size increases from the inside to the outside, which can improve the strength and stiffness of the porous carbon skeleton and improve the structural stability of the porous carbon skeleton. Attached Figure Description
[0021] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments of this application and their descriptions are used to explain this application and do not constitute an undue limitation of this application.
[0022] Figure 1 is a schematic diagram of the material structure prepared in an embodiment of the present invention;
[0023] Figure 2 is an enlarged view of point A in Figure 1.
[0024] Wherein, 1-porous carbon framework; 2-porous carbon internal pores; 3-silicon particles; D1 is 5-20nm, D2 is 1-5nm, and D3 is 0.5-1nm. Detailed Implementation
[0025] It should be noted that the following detailed descriptions are exemplary and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.
[0026] It should be noted that the terminology used herein is for the purpose of describing particular implementations only and is not intended to limit the exemplary implementations according to this application.
[0027] Where there is no conflict, the embodiments and features described in this application may be combined with each other.
[0028] Methods for measuring each parameter:
[0029] The average pore size is determined by a combination of nitrogen adsorption-desorption and carbon dioxide adsorption. Nitrogen adsorption-desorption is used for micropores and mesopores, while carbon dioxide adsorption is used for ultramicropores D3. Both pore size measurement methods are well known in the testing field.
[0030] The particle size distribution of porous carbon matrix is measured by laser particle size analyzer. The porous carbon matrix is ultrasonically dispersed in the test solvent and the particle size distribution is measured by laser scattering. This is the most commonly used particle size distribution measurement method and is well known in the testing field.
[0031] The porosity is determined by testing the tap density and then applying the formula: porosity = 1 - tap density / true density. Porous carbon materials are non-metallic particulate materials. The tap density test follows the national standard GB / T 31057.2-2018. The true density of carbon materials is taken as 2.1 g / cm³. 3 ;
[0032] The method for measuring the hole depth is to prepare an electron microscope cross-sectional sample, observe the cross-sectional structure using a high-resolution electron microscope, and confirm the hole diameter depth and hole region length.
[0033] The method for determining the length of the borehole region is the same as the method for measuring the borehole depth;
[0034] The particle size testing method for silica particles is the same as that for porous carbon particles.
[0035] In a first aspect, the present invention provides a high specific capacity and high first-efficiency silicon-carbon anode material, comprising a porous carbon matrix and silicon particles deposited in the porous carbon matrix.
[0036] The porous carbon matrix has a pore size gradient distribution, with the pore size increasing sequentially from the inside to the outside and interconnected. The average pore size of the innermost region is 0.5-1 nm, the average pore size of the middle region is 1-5 nm, and the average pore size of the outermost region is 5-20 nm.
[0037] Type I pores (average pore size 5-20 nm) are larger, resulting in correspondingly larger silicon particle sizes and smaller specific surface areas. Being located on the outermost layer of the silicon + carbon material, they exhibit fewer side reactions with the electrolyte during battery formation, thus improving initial efficiency. Simultaneously, a larger outermost pore size facilitates electrolyte absorption and diffusion, enhancing cycle life and fast-charging capabilities. Average pore sizes can range from 5 nm to 20 nm.
[0038] Type III pores (average pore size 0.5-1 nm) have extremely small pore sizes and require the least amount of deposited silicon. Typically, the silicon in the innermost layer of silicon-carbon materials has a lower specific capacity than the outer layers; therefore, reducing the silicon content in the innermost layer reduces silicon waste and improves silicon utilization. Furthermore, the small pore size of the innermost layer in the pore structure results in higher rigidity and greater structural stability in the porous carbon. Average pore sizes can be 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, and 1 nm.
[0039] Type II pores (average pore size of 1-5 nm) have a suitable pore size and are the main active regions for silicon deposition, achieving optimal silicon particle utilization efficiency and the best electrical properties of silicon-carbon materials. Average pore sizes can be 1 nm, 2 nm, 3 nm, 4 nm, or 5 nm.
[0040] In some embodiments, the particle size of the porous carbon matrix is 3-15 μm, such as 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, or 15 μm.
[0041] In some embodiments, the porous carbon matrix has a porosity of 40-80% and a pore depth of 2.5-13 μm. The porosity can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or 80%; the pore depth can be 2.5 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, or 13 μm.
[0042] Preferably, the length of the pore region with an average pore size of 0.5-1 nm is 0.5-2.5 μm, and the length of the pore region with an average pore size of 5-20 nm is 0.5-3 μm.
[0043] The length of the pore region with an average pore size of 0.5-1 nm can be 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.5 μm, 2 μm, or 2.5 μm;
[0044] The length of the pore region with an average pore size of 5-20 nm can be 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, or 3 μm.
[0045] Secondly, the present invention provides a method for preparing the high-specific-capacity, high-efficiency silicon-carbon anode material, comprising the following steps:
[0046] MOF particles were dispersed in a mesoporous silica precursor solution, and a mesoporous silica layer was coated on the MOF surface using the sol-gel method to obtain a MOF core-mesoporous shell composite template.
[0047] After the MOF core-mesoporous shell composite template is impregnated with a carbon source dispersion and dried, it is first carbonized at a low temperature at a first temperature and then carbonized at a high temperature at a second temperature.
[0048] After carbonization, the composite template is removed, resulting in porous carbon.
[0049] Silicon particles are deposited in porous carbon via chemical vapor deposition to obtain silicon-carbon composite materials.
[0050] A two-step carbonization process helps maintain the original structure of the template. The first step, low-temperature carbonization, has minimal impact on the structure of MOF and mesoporous silica materials, avoiding the structural changes caused by direct high-temperature rapid carbonization that affect the pore structure. The second step, high-temperature carbonization, increases the degree of carbonization of the carbon material. A higher degree of carbonization results in better conductivity, but the temperature should not be too high, as excessively high temperatures can cause the carbon structure to collapse.
[0051] ZIF-8 (pore size approximately 0.4-0.5 nm) was used as the MOF template. Its framework channels provide ultra-micropores, while the intercrystalline gaps form micropores (1-5 nm). MOF particles were dispersed in a mesoporous silica precursor, and a layer of self-assembled mesoporous silica particles (particle size 5-20 nm) was coated on the MOF surface using a sol-gel method to form a MOF core-mesoporous shell composite template.
[0052] By constructing templates with multi-level pore structures or templates with varying pore sizes, carbon precursors form complementary multi-level carbon skeletons in the template pores. After removing the template, porous carbon materials are obtained with a continuous transition in pore size from macropores to mesopores / micropores / ultramicropores.
[0053] During high-temperature carbonization at 600-800℃, the impregnated carbon source is carbonized to form a carbon skeleton.
[0054] Silicon deposition is prepared using the most commonly used silane chemical vapor deposition method.
[0055] In some embodiments, the MOF is 2-methylimidazolium zinc MOF ZIF-8, zeolite imidazolium skeleton-67 ZIF-67, zeolite imidazolium ester skeleton-90 ZIF-90, or zeolite-type imidazolium zinc framework material MAF-6.
[0056] In some embodiments, the thickness of the mesoporous silica self-assembled particle layer is 0.5-3 μm, and the silica particle size is 5-20 nm.
[0057] The thickness of the mesoporous silica self-assembled particle layer can be 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, or 3μm; the particle size of the silica particles can be 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, or 20nm.
[0058] In some embodiments, the sol-gel method involves ultrasonically dispersing MOF ZIF8 particles uniformly in an ethanol solution, then slowly adding an ethanol solution containing tetraethyl orthosilicate and CTAB to the MOF dispersion, and finally slowly adding an ammonia solution to the mixed solution while stirring. The tetraethyl orthosilicate hydrolyzes on the MOF surface, forming a self-assembled mesoporous silica particle layer on the surface.
[0059] In some embodiments, the carbon source dispersion is a sucrose solution or a phenolic resin solution.
[0060] Preferably, the concentration of the sucrose solution is 1.0-1.5 g / mL; the concentration of the phenolic resin solution is 5-25 wt%, preferably a phenolic resin solution, which has a higher yield after carbonization.
[0061] The concentration of the sucrose solution can be 1.0 g / mL, 1.1 g / mL, 1.2 g / mL, 1.3 g / mL, 1.4 g / mL, or 1.5 g / mL; the concentration of the phenolic resin solution can be 5 wt%, 10 wt%, 15 wt%, 20 wt%, or 25 wt%.
[0062] In some embodiments, the drying temperature is 90-110°C, such as 90°C, 95°C, 100°C, 105°C, or 110°C.
[0063] In some embodiments, the first temperature is 300-400°C, and the second temperature is 600-800°C;
[0064] Preferably, the carbonization time at a low temperature of 300-400℃ is 1-2 hours. The low-temperature carbonization temperature can be 300℃, 310℃, 320℃, 330℃, 340℃, 350℃, 360℃, 370℃, 380℃, 390℃, or 400℃; the carbonization time can be 1 hour, 1.1 hours, 1.2 hours, 1.3 hours, 1.4 hours, 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours, or 2 hours.
[0065] In some embodiments, the carbonization time at 600-800℃ is 1-4 hours. The high-temperature carbonization temperature can be 600℃, 650℃, 700℃, 750℃, or 800℃; the high-temperature carbonization time can be 1 hour, 2 hours, 3 hours, or 4 hours.
[0066] Preferably, the silane flow rate for chemical vapor deposition of silicon particles in porous carbon is 2 L / min, the silane deposition temperature is 500 °C, and the deposition time is 60 min.
[0067] In some embodiments, the mesoporous silica layer is removed by dissolving in HF solution; and the organic residues remaining after the MOF template carbonization are extracted using N,N-dimethylformamide (DMF).
[0068] Thirdly, the present invention provides a battery in which the active material of the negative electrode is the high-capacity, high-efficiency silicon-carbon negative electrode material.
[0069] The present invention will be further described below with reference to the embodiments.
[0070] Example 1
[0071] A method for preparing a silicon-carbon anode material includes the following steps:
[0072] (1) Preparation of porous carbon framework materials with multi-level and continuous pore size distribution
[0073] ZIF-8 (pore size of about 0.4 nm) was used as the MOF template. Its framework channels provide ultra-micropores, while the intercrystalline gaps form micropores (1-5 nm).
[0074] MOF particles were first dispersed in deionized water. Then, a mixed solution of mesoporous silica precursor polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer P123 and tetraethyl orthosilicate TEOS was slowly added to the MOF dispersion. The mass ratio of TEOS to P123 was 2:1 and the concentration of P123 was 2wt%. A self-assembled mesoporous silica layer (pore size 5-10nm) with a thickness of 1-2μm was coated on the MOF surface by sol-gel method to form a MOF core-mesoporous shell composite template.
[0075] The composite template was impregnated with a 15wt% phenolic resin solution for 6 hours.
[0076] After impregnation, it is dried and cured at 100℃ for 2 hours;
[0077] After curing, it is carbonized in stages under an Ar atmosphere: low-temperature carbonization at 350℃ (preserving the MOF structure) for 2 hours; high-temperature carbonization at 700℃ (forming a carbon skeleton) for 2 hours.
[0078] After carbonization, the template is removed by dissolving the mesoporous silica layer with HF solution at a concentration of 30 wt%. After dissolution, the substrate is cleaned by rinsing with deionized water at least three times.
[0079] The MOF template was then extracted with DMF solvent. After extraction, the material was centrifuged and the solid and liquid were separated. The solid was washed with deionized water more than three times and dried to obtain three types of porous carbon materials with continuously distributed pore sizes (ultramicropores 0.5-1 nm, micropores 1-5 nm, and mesopores 5-20 nm continuously distributed).
[0080] (2) Preparation of silicon-carbon material: The porous carbon material prepared in step (1) is used as a precursor. Argon gas is introduced into the fluidized bed equipment, and silane gas is introduced into the fluidized bed. The silane flow rate is 2L / min, the silane deposition temperature is 500℃, and the deposition time is 60min to obtain silicon-carbon anode material.
[0081] Example 2
[0082] (1) Preparation of porous carbon framework materials with multi-level and continuous pore size distribution:
[0083] HKUST-1 (0.9 nm pore size) was used as the MOF template, and its framework channels provided ultrapores, while the intercrystalline gaps formed micropores (2-5 nm).
[0084] MOF particles were first dispersed in deionized water. Then, a mixed solution of mesoporous silica precursor P123 and TEOS was slowly added to the MOF dispersion. The mass ratio of TEOS to P123 was 2:1 and the concentration of P123 was 2 wt%. A self-assembled mesoporous silica layer (pore size 5-10 nm) with a thickness of 1-2 μm was coated on the MOF surface by sol-gel method to form a MOF core-mesoporous shell composite template.
[0085] The composite template was impregnated with a 15 wt% phenolic resin solution for 6 hours.
[0086] After impregnation, it is dried and cured at 100℃ for 2 hours;
[0087] After curing, it is carbonized in stages under an Ar atmosphere: low-temperature carbonization at 350℃ (preserving the MOF structure) for 2 hours; high-temperature carbonization at 700℃ (forming a carbon skeleton) for 2 hours.
[0088] After carbonization, the template is removed by dissolving the mesoporous silica layer with HF solution at a concentration of 30 wt%. After dissolution, the substrate is cleaned by rinsing with deionized water at least three times.
[0089] The MOF template was then extracted with DMF solvent. After extraction, the material was centrifuged and the solid and liquid were separated. The solid was washed with deionized water more than three times and then dried to obtain three types of continuously distributed porous carbon materials (ultramicropores 0.9-1 nm, micropores 1-5 nm, and mesopores 5-20 nm continuously distributed).
[0090] (2) Preparation of silicon-carbon material: The porous carbon material prepared in step (1) is used as a precursor. Argon gas is introduced into the fluidized bed equipment, and silane gas is introduced into the fluidized bed. The silane flow rate is 2L / min, the silane deposition temperature is 500℃, and the deposition time is 60min to obtain silicon-carbon anode material.
[0091] Example 3
[0092] (1) Preparation of porous carbon framework materials with multi-level and continuous pore size distribution:
[0093] HKUST-1 (0.9 nm pore size) was used as the MOF template, and its framework channels provided ultrapores, while the intercrystalline gaps formed micropores (2-5 nm).
[0094] MOF particles were first dispersed in deionized water. Then, a mixed solution of mesoporous silica precursor P123 and TEOS was slowly added to the MOF dispersion. The mass ratio of TEOS to P123 was 2:1 and the concentration of P123 was 2 wt%. A self-assembled mesoporous silica layer (pore size 5-10 nm) with a thickness of 1-2 μm was coated on the MOF surface by sol-gel method to form a MOF core-mesoporous shell composite template.
[0095] The composite template was impregnated with a 15wt% phenolic resin solution for 6 hours.
[0096] After impregnation, it is dried and cured at 110℃ for 1.5 hours.
[0097] After curing, it was carbonized in stages under an Ar atmosphere: low-temperature carbonization at 400℃ (preserving the MOF structure) for 1.5 hours; and high-temperature carbonization at 750℃ (forming a carbon skeleton) for 1.5 hours.
[0098] After carbonization, the template is removed by dissolving the mesoporous silica layer with HF solution at a concentration of 30 wt%. After dissolution, the substrate is cleaned by rinsing with deionized water at least three times.
[0099] The MOF template was then extracted with DMF solvent. After extraction, the material was centrifuged and the solid and liquid were separated. The solid was washed with deionized water more than three times and dried to obtain three types of porous carbon materials with continuously distributed pore sizes (ultramicropores 0.9-1 nm, micropores 1-5 nm, and mesopores 5-20 nm continuously distributed).
[0100] (2) Preparation of silicon-carbon material: The porous carbon material prepared in step (1) is used as a precursor. Argon gas is introduced into the fluidized bed equipment, and silane gas is introduced into the fluidized bed. The silane flow rate is 2L / min, the silane deposition temperature is 500℃, and the deposition time is 60min to obtain silicon-carbon anode material.
[0101] Example 4
[0102] The difference from Example 1 is that the MOF template is ZIF-67, while everything else is the same as in Example 1.
[0103] Example 5
[0104] The difference from Example 1 is that the MOF template is ZIF-90, while everything else is the same as in Example 1.
[0105] Example 6
[0106] The difference from Example 1 is that the MOF template is MAF-6, while everything else is the same as in Example 1.
[0107] Comparative Example 1
[0108] The difference from Example 1 is that silicon is deposited in conventional porous carbon: conventional porous carbon has been commercialized, while Comparative Example 1 of this invention uses porous carbon material developed by Shandong Shengquan New Energy Technology Co., Ltd. The pores in this porous carbon are mainly dominated by type II pores, with micropores of 1-2 nm accounting for nearly 90%. It is mainly obtained by carbonization of phenolic resin and alkali activation to create pores. The preparation method is already known in the industry.
[0109] Conventional porous carbon materials were introduced into a fluidized bed apparatus using argon as the carrier gas, and then silane gas was introduced into the fluidized bed at a flow rate of 2 L / min. The silane deposition temperature was 500℃ and the deposition time was 60 min, resulting in a silicon-carbon composite anode.
[0110] Comparative Example 2
[0111] (1) Preparation of porous carbon framework materials with different pore sizes:
[0112] The carbon precursor (sucrose precursor) is carbonized in an inert gas atmosphere to obtain carbonized material;
[0113] The carbonized material was then mixed with a pore-forming agent (potassium hydroxide) at a mass ratio of 1:1.2 to obtain a mixture.
[0114] The mixture was then activated in an inert atmosphere to obtain activated material. The activation method was as follows: the material was kept at 750°C for 0.6 hours, 850°C for 5 hours, and 950°C for 2 hours in sequence. The activated material was washed with water and acid in sequence and then filtered to obtain porous carbon material.
[0115] (2) Preparation of silicon-carbon materials: Same as in Example 1.
[0116] Comparative Example 3
[0117] The difference from Example 1 is that the step of coating the MOF surface with a mesoporous silica layer by the sol-gel method is omitted when preparing the porous carbon framework; otherwise, it is the same as Example 1.
[0118] Comparative Example 4
[0119] The difference from Example 1 is that the step of low-temperature carbonization at 350°C is omitted, while the rest is the same as Example 1.
[0120] Preparation of the positive electrode: Polyvinylidene fluoride (PVDF), conductive agent (SP), and positive electrode material (NCM811) were added to N-methylpyrrolidone (NMP) in a mass ratio of 1.2:1.5:97.3. The solid content of the slurry was 75%. The mixture was thoroughly stirred and homogenized. The slurry was then coated onto the surface of an aluminum current collector at a coating amount of 22 mg / cm². 2 The positive electrode sheet is obtained by drying, cold pressing, and punching.
[0121] Preparation of the negative electrode sheet: Sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber latex (SBR), conductive agent, and negative electrode active material (the negative electrode active material is composed of commercial graphite and silicon-carbon negative electrode materials prepared in Examples 1-3 or Comparative Examples 1-4 mixed at a mass ratio of 90:10) are added sequentially to deionized water at a mass ratio of 1.7:1.8:1.5:95, with a solid content of 50%. The mixture is thoroughly stirred and mixed to obtain a slurry. The slurry is coated onto a copper foil current collector, dried, cold-pressed, and die-cut to obtain the negative electrode sheet.
[0122] The PE separator is stacked in a "Z" shape with the prepared positive and negative electrode sheets, and packaged with aluminum-plastic film to obtain the cell to be injected with electrolyte. After baking, the electrolyte (the main component of the electrolyte is LiPF6 dissolved in a mixed solvent of EC:EMC = 3:7, and the concentration of LiPF6 is 1M) is injected to obtain a lithium-ion battery (soft pack battery) with a nominal capacity of 3Ah to be tested.
[0123] Lithium-ion battery performance testing:
[0124] 1. Battery internal resistance test: Use a battery internal resistance tester to test the resistance of the battery and obtain the DC internal resistance data of the battery;
[0125] 2. Battery first efficiency: first lithium delithiation capacity / first lithium insertion capacity (button cell, the electrode of which is composed of the above-coated negative electrode and lithium metal sheet, and the electrolyte and separator are the same as those of the above-mentioned soft pack battery);
[0126] 3. Negative electrode specific capacity test: Using button cells, the manufacturing method is the same as that used in the battery first-efficiency performance test, the specific capacity is measured by charging at 0.1C to 1.5V;
[0127] 4. Battery cycle test: 25℃ 1C / 1C cycle test, conducted using the Blue Electric test system.
[0128] Table 1 Battery internal resistance, initial battery efficiency, battery capacity, and cycle data
[0129] Test Result Analysis
[0130] In Table 1, the internal resistance of the batteries is generally similar. The internal resistance of silicon-carbon materials prepared from porous carbon with different pore sizes is likely mainly related to the relative amount of silicon. The total deposited silicon content is controlled similarly in the embodiments and comparative examples of this invention, hence the small difference in internal resistance. However, in terms of specific capacity, Example 1 has less deposited silicon due to the smaller pore size of the innermost layer, and the innermost silicon is more difficult to delithiate, thus limiting the specific capacity and making it difficult to achieve its full potential. Example 1 has the highest usable silicon content, resulting in the best specific capacity and initial efficiency. This is also due to the relatively larger size of the outermost silicon particles, which reduces side reactions with the electrolyte, leading to a higher initial efficiency.
[0131] In Example 2, the increased pore size of the innermost layer led to a higher silicon content deposited in the inner layer, but the lower silicon utilization rate in the innermost layer. Therefore, the specific capacity and initial efficiency were slightly lower than in Example 1. In Example 3, by appropriately increasing the carbonization temperature during carbonization, the carbonization time could be reduced accordingly, achieving the same technical effect.
[0132] Comparative Example 1 is a silicon-carbon material prepared using conventional porous carbon. The pore size of conventional porous carbon is mainly close to that of Class II pores, and the resulting silicon particle size is generally smaller than that of Class I pores. This leads to more side reactions with the electrolyte, resulting in lower initial efficiency and specific capacity of Comparative Example 1.
[0133] Comparative Example 2 uses publicly available technology. The pore structure of the three pore sizes is not designed to be continuously distributed from the outside in, and the smallest pore size is not explicitly placed in the innermost layer. This results in a higher silicon deposition amount in the micropores compared to Examples 1 and 2. Furthermore, the largest pore size is not positioned in the outer layer to reduce side reactions between silicon and the electrolyte. Therefore, the overall first-efficiency and specific capacity are lower than in Examples 1 and 2. Thus, although both examples have multi-level pore sizes, the location of the pores not only affects the silicon specific capacity but also the side reactions at the silicon-electrolyte interface.
[0134] Comparative Example 3 omits the step of preparing a self-assembled mesoporous silica particle layer using sol-gel. The resulting porous carbon structure only has three types of pores and two types of pores, lacking the outermost large-sized type one pores, which is not conducive to electrolyte wetting. At the same time, the larger specific surface area of the type two pores will lead to an increase in side reactions with the electrolyte. Therefore, the initial efficiency is significantly lower than that of Example 1.
[0135] Comparative Example 4 uses direct high-temperature carbonization, omitting the low-temperature carbonization process. This carbonization method is not conducive to maintaining the ordered pore structure, thus affecting silicon deposition and resulting in significantly lower first-efficiency and cycle performance in Comparative Example 4.
[0136] A well-designed and regionally distributed pore structure is beneficial for improving the overall specific capacity and first-efficiency of silicon-carbon. Cycling data shows that, overall, the cycling performance of vapor-deposited silicon-carbon is excellent with little difference. However, the hierarchical pore structure continuously distributed from the outside to the inside in this invention, with the inner layer designed with the smallest pore size, improves the structural stability of porous carbon, thus exhibiting a slight advantage.
Claims
1. A silicon-carbon anode material, characterized in that: This includes a porous carbon matrix and silicon particles deposited within the porous carbon matrix. The porous carbon matrix has a pore size gradient distribution, with the pore size increasing sequentially from the inside to the outside and interconnected. The average pore size of the innermost region is 0.5-1 nm, the average pore size of the middle region is 1-5 nm, and the average pore size of the outermost region is 5-20 nm.
2. The silicon-carbon anode material according to claim 1, characterized in that: The porous carbon matrix has a particle size of 3-15 μm; the porosity of the porous carbon matrix is 40-80%, and the pore depth is 2.5-13 μm.
3. The silicon-carbon anode material according to claim 1, characterized in that: The length of the pore region with an average pore size of 0.5-1 nm is 0.5-2.5 μm, and the length of the pore region with an average pore size of 5-20 nm is 0.5-3 μm.
4. The method for preparing the silicon-carbon anode material according to any one of claims 1-3, characterized in that: Includes the following steps: MOF particles were dispersed in a mesoporous silica precursor solution, and a mesoporous silica layer was coated on the MOF surface using the sol-gel method to obtain a MOF core-mesoporous shell composite template. After the MOF core-mesoporous shell composite template is impregnated with a carbon source dispersion and dried, it is first carbonized at a low temperature at a first temperature and then carbonized at a high temperature at a second temperature. After carbonization, the composite template is removed, resulting in porous carbon. Silicon particles are deposited in porous carbon via chemical vapor deposition to obtain silicon-carbon composite materials.
5. The preparation method according to claim 4, characterized in that: The MOF is ZIF-8, ZIF-67, ZIF-90, HKUST-1 or MAF-6.
6. The preparation method according to claim 4, characterized in that: According to the preparation method of claim 4, the thickness of the mesoporous silica layer is 0.5-3 μm, and the particle size of the silica particles is 5-20 nm.
7. The preparation method according to claim 4, characterized in that: The carbon source dispersion is a sucrose solution or a phenolic resin solution; the concentration of the sucrose solution is 1-1.5 g / mL; the concentration of the phenolic resin solution is 5-25 wt%.
8. The preparation method according to claim 4, characterized in that: The first temperature is 300-400℃, and the second temperature is 600-800℃; Preferably, the carbonization time at a low temperature of 300-400℃ is 1-2 hours; and the carbonization time at a high temperature of 600-800℃ is 1-4 hours. Preferably, the silane flow rate for chemical vapor deposition of silicon particles in porous carbon is 2 L / min, the silane deposition temperature is 500 °C, and the deposition time is 60 min.
9. The preparation method according to claim 4, characterized in that: The mesoporous silica layer was removed by dissolving in HF solution; the residual organic matter after the MOF template carbonization was extracted by N,N-dimethylformamide (DMF).
10. A battery, characterized in that: The active material of its negative electrode is the silicon-carbon negative electrode material according to any one of claims 1-3, or the silicon-carbon negative electrode material prepared by any one of claims 4-9.