Electrolyte additive, electrolyte containing same, and lithium-ion secondary battery

By using pyridine-sulfonate-based or pyridine-sulfonate-based electrolyte additives in lithium-ion batteries, the problems of discoloration and increased impedance caused by electrolyte acid degradation have been solved, thereby improving the structural stability and cycle performance of the battery.

WO2026233095A1PCT designated stage Publication Date: 2026-11-12MURATA MFG CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/091770
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2026-04-20
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

In existing technologies, lithium-ion battery electrolytes are prone to discoloration and increased impedance during acid degradation, which affects cycle performance.

Method used

Electrolyte additives containing pyridine-sulfonyl groups or pyridine-sulfonate groups are used to suppress electrolyte discoloration and form low-resistance SEI and CEI films at the positive and negative electrodes by regulating the electron cloud density on the pyridine ring, thereby improving the structural stability and cycle performance of the battery.

Benefits of technology

It effectively suppresses electrolyte discoloration, reduces the rise in battery impedance during cycling, and significantly improves cycle discharge capacity and capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026091770_12112026_PF_FP_ABST
    Figure CN2026091770_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present application are an electrolyte additive, an electrolyte containing same, and a lithium-ion secondary battery. The electrolyte additive comprises any one of the following substances (I), wherein R1 is substituted or unsubstituted C1-7 alkyl, -CN, -TMS, or substituted or unsubstituted C2-3 alkenyl; R2 is each independently substituted or unsubstituted C1-7 alkyl, -CN, substituted or unsubstituted C2-3 alkenyl, -TMS, (II) or (III); R3 is substituted or unsubstituted phenyl, substituted or unsubstituted C1-7 alkyl, -CN, -TMS, or substituted or unsubstituted C2-3 alkenyl; and R4 is independently substituted or unsubstituted C1-7 alkyl, -CN, substituted or unsubstituted C2-3 alkenyl, -TMS, (II) or (III); R5 and R6 is each independently substituted or unsubstituted C1-3 alkyl, -CN, -TMS, or substituted or unsubstituted C2-3 alkenyl; and n is an integer among 0-4. Using the electrolyte additive of the present invention can inhibit the discoloration of electrolytes, significantly suppress the impedance increase of batteries during cycling processes, and greatly improve the cycle discharge capacity and capacity retention rate.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte additives, electrolytes containing them, and lithium-ion secondary batteries Technical Field

[0001] This invention relates to the field of lithium-ion batteries, and more specifically, to electrolyte additives for lithium-ion secondary batteries, electrolytes containing the electrolyte additives, and lithium-ion secondary batteries. Background Technology

[0002] The widespread use of mobile phones and other electronic devices has created a strong demand for miniaturization, weight reduction, and long lifespan. Therefore, the development of small, lightweight rechargeable batteries with high energy density is underway as a power source.

[0003] Secondary batteries are not limited to applications in electronic devices; research is also underway for other uses. Examples include battery packs that can be detachably installed in electronic devices, electric vehicles such as electric cars, power storage systems such as home power servers, and power tools such as electric drills.

[0004] Compared to traditional lead-acid and zinc-manganese batteries, lithium-ion batteries offer advantages such as longer lifespan, higher output voltage, higher energy density, lower self-discharge, less environmental pollution, and no memory effect. They are now widely used in portable electronic devices, electric vehicles, and power tools. The electrolyte, as a crucial component of lithium-ion batteries, significantly impacts the overall battery performance.

[0005] Therefore, various studies have been conducted in this field regarding the composition of electrolytes. CN 116053587A discloses an electrolyte for lithium-ion batteries, which includes an electrolyte salt, a non-aqueous solvent, additive A, and additive B. Additive B includes a positive electrode film-forming additive and a negative electrode film-forming additive. The positive electrode film-forming additive includes one or more of propane sulpholactone, vinyl sulfate, and methane disulfonate, while the negative electrode film-forming additive includes one or two of vinylene carbonate and fluoroethylene carbonate. The most significant inventive point of CN 116053587A is the inclusion of cyclic heterocyclic fluorosulfonates, which necessarily contain F substituents with unchanged sites. The design does not consider the different characteristics of different functional groups, resulting in a relatively simplistic approach.

[0006] CN 113948775B discloses an electrolyte for lithium-ion batteries containing two additives: Additive A is selected from 2-ethynyl-1,3-dioxolane compounds, a bifunctional additive. Its lone pair of electrons, when added in small amounts to the electrolyte, exhibits weak Lewis basicity, allowing it to form complexes (e.g., hexaligand complexes) with other components in the electrolyte (e.g., PF5), thereby reducing the acidity and reactivity of the electrolyte and suppressing the increase of free acid in the electrolyte. Simultaneously, the carbon-carbon triple bonds present in Additive A readily undergo oxidation on the positive electrode surface to generate a low-impedance interfacial film. Additive B is selected from sulfate ester compounds, which preferentially form a low-impedance interfacial protective film on the negative electrode surface compared to the electrolyte solvent, thus improving the high-temperature performance of the electrolyte. CN 113948775B aims to mitigate the acid degradation caused by the reaction of Additive B in the electrolyte through the combined action of the two additives, utilizing the Lewis basicity of Additive A. Summary of the Invention

[0007] The main objective of this invention is to provide an electrolyte additive, an electrolyte containing the additive, and a lithium-ion secondary battery, in order to solve the problem in the prior art that specific F-containing additives or combinations of two additives are required to suppress electrolyte discoloration and impedance increase caused by electrolyte acid degradation, while improving cycle performance.

[0008] To achieve the above objectives, according to one aspect of the present invention, an electrolyte additive is provided, the electrolyte additive comprising any one of the following substances:

[0009] Where R1 is substituted or unsubstituted C 1-7 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl;

[0010] R2 is independently either substituted or unsubstituted C. 1-7 Alkyl, -CN, substituted or unsubstituted C 2- 3-Alkenyl, -TMS,

[0011] R3 is a substituted or unsubstituted phenyl group, or a substituted or unsubstituted C group. 1-7 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl;

[0012] R4 is independently either substituted or unsubstituted C. 1-7 Alkyl, -CN, substituted or unsubstituted C 2- 3-Alkenyl, -TMS,

[0013] R5 and R6 are independently substituted or unsubstituted C. 1-3 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl;

[0014] n is an integer between 0 and 4.

[0015] Furthermore, in the above-mentioned electrolyte additives, the group It is located in the ortho or meta position of the nitrogen atom in pyridine.

[0016] Furthermore, in the above electrolyte additives, n is 0 or 1.

[0017] Furthermore, in the above-mentioned electrolyte additives, R2 and R4 are located at the ortho position of the pyridine nitrogen atom, or R2 and R4 are located at the group. The neighboring position.

[0018] Furthermore, in the above-mentioned electrolyte additives, R1 is -CN, substituted or unsubstituted C. 1-3 Alkyl, -TMS, or substituted or unsubstituted C 2-3 Alkenyl group, R3 is a substituted or unsubstituted phenyl group, -CN group, substituted or unsubstituted C group. 1-3 Alkyl, -TMS, or substituted or unsubstituted C 2-3 Alkenyl group.

[0019] Furthermore, in the above-mentioned electrolyte additives, R2 and R4 are each independently substituted or unsubstituted C. 1-3 Alkyl, -CN, substituted or unsubstituted C 2-3 alkenyl, -TMS or

[0020] Furthermore, in the above-mentioned electrolyte additives, R2 and R4 are each independently methyl, ethyl, propyl, -CN, -CH2=CH3, -CH2=CH2-CH3, -TMS, or...

[0021] Furthermore, in the above-mentioned electrolyte additives, the electrolyte additives include any one of the following substances:

[0022] According to another aspect of the invention, an electrolyte is provided comprising an organic solvent, a lithium salt, and the electrolyte additives described in the invention.

[0023] Furthermore, in the above electrolyte, the electrolyte additive is present in an amount of 0.05wt%-2.0wt% based on the total weight of the organic solvent and lithium salt.

[0024] Furthermore, in the above-mentioned electrolyte, the organic solvent includes linear carbonates, cyclic carbonates, or combinations thereof.

[0025] According to another aspect of the present invention, a lithium-ion secondary battery is provided, comprising: a positive electrode, a negative electrode, a separator, and an electrolyte as described in the present invention.

[0026] The electrolyte additive of this invention has a core structure of pyridine-sulfonyl or pyridine-sulfonate groups. The lone pair of electrons on the nitrogen atom of pyridine can accept protons, exhibiting basicity. Introducing sulfonyl or sulfonate groups, which are electron-withdrawing groups and rich in sulfur, can introduce sulfur while regulating the electron cloud density on the pyridine ring. This is beneficial for suppressing the rise in battery impedance. Furthermore, the interaction between pyridine-sulfonyl or pyridine-sulfonate groups can reduce the electron richness and basicity of the pyridine ring, thereby suppressing electrolyte discoloration. Moreover, by introducing neutral or electron-withdrawing structures onto the pyridine ring or sulfonyl or sulfonate groups, the additive of this invention can further disperse the electron cloud density on the pyridine ring, thereby reducing the basicity of the pyridine ring, achieving structural stability, suppressing electrolyte discoloration, and forming low-resistivity SEI and CEI films at the positive and negative electrodes. This significantly suppresses the rise in battery impedance during cycling, while greatly improving cycle discharge capacity and capacity retention. Attached Figure Description

[0027] Figure 1 shows the color changes of the base electrolyte, the electrolytes prepared in Examples 1-10, after 30 days of storage compared to fresh electrolyte. Detailed Implementation

[0028] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0029] As explained in the background section, existing electrolyte additives suffer from problems such as requiring specific fluoride-containing additives or combinations of both to suppress electrolyte discoloration and impedance increase caused by electrolyte acid degradation, while simultaneously improving cycle performance. Therefore, there is still a need to develop an electrolyte additive that can overcome the problems of the prior art. To address the problems of the prior art, according to a typical embodiment of the present invention, an electrolyte additive is provided, comprising any one of the following substances:

[0030] Where R1 is substituted or unsubstituted C 1-7 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl;

[0031] R2 is independently either substituted or unsubstituted C.1-7 Alkyl, -CN, substituted or unsubstituted C 2- 3-Alkenyl, -TMS,

[0032] R3 is a substituted or unsubstituted phenyl group, or a substituted or unsubstituted C group. 1-7 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl;

[0033] R4 is independently either substituted or unsubstituted C. 1-7 Alkyl, -CN, substituted or unsubstituted C 2- 3-Alkenyl, -TMS,

[0034] R5 and R6 are independently substituted or unsubstituted C. 1-3 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl;

[0035] n is an integer between 0 and 4.

[0036] The electrolyte additive of this invention has a core structure of pyridine-sulfonyl or pyridine-sulfonate groups. The lone pair of electrons on the nitrogen atom of pyridine can accept protons and exhibits basicity. Introducing sulfonyl or sulfonate groups, which are electron-withdrawing groups and are also rich in sulfur, can introduce sulfur while regulating the electron cloud density on the pyridine ring. This is beneficial for suppressing the rise in battery impedance. Furthermore, the interaction between pyridine-sulfonyl or pyridine-sulfonate groups can reduce the electron richness and basicity of the pyridine ring, thereby suppressing electrolyte discoloration. Moreover, by introducing neutral or electron-withdrawing structures onto the pyridine ring or sulfonyl or sulfonate groups, the additive of this invention can further disperse the electron cloud density on the pyridine ring, thereby reducing the basicity of the pyridine ring, achieving structural stability, suppressing electrolyte discoloration, and forming low-resistivity SEI and CEI films at the positive and negative electrodes. This significantly suppresses the rise in battery impedance during cycling, while greatly improving cycle discharge capacity and capacity retention.

[0037] In this application, the term "substituted" means substituted with an alkyl group or C, wherein the alkyl group refers to C. 1-6 Alkyl groups, especially C 1-3 alkyl.

[0038] Preferably, in the above-mentioned electrolyte additives, the group Located at the ortho or meta position of the nitrogen atom in pyridine. This is controlled by the group... The electrolyte additive of the present invention can better regulate the electron cloud density on the pyridine ring, and through the interaction of pyridine-sulfonyl groups or pyridine-sulfonate groups, it can more advantageously reduce the electron-richness and alkalinity of the pyridine ring, thereby more advantageously suppressing electrolyte discoloration, suppressing the rise in battery impedance during cycling, and greatly improving cycle discharge capacity and capacity retention.

[0039] For example, in the above-mentioned electrolyte additive, n can be 0, 1, 2, 3, or 4; preferably, n can be 0 or 1. When n is within this range, the electrolyte additive of the present invention can improve the activity and reactivity of the electrolyte additive in the battery environment, thereby better suppressing electrolyte discoloration, suppressing the rise in battery impedance during cycling, and greatly improving cycle discharge capacity and capacity retention.

[0040] Preferably, in the above-mentioned electrolyte additive, R2 and R4 can be located at the ortho position of the pyridine nitrogen atom, or R2 and R4 can be located at the group. The adjacent positions of R2 and R4 can further disperse the electron cloud density on the pyridine ring, thereby better reducing the basicity of the pyridine ring, achieving structural stability, suppressing electrolyte discoloration, and better forming low-resistivity SEI and CEI films on the positive and negative electrodes. This more significantly suppresses the impedance rise of the battery during cycling, while greatly improving the cycle discharge capacity and capacity retention.

[0041] Preferably, in the above-mentioned electrolyte additive, R1 can be -CN, substituted or unsubstituted C. 1- 3-alkyl, -TMS, or substituted or unsubstituted C 2-3 Alkenyl, R3 can be a substituted or unsubstituted phenyl, -CN, substituted or unsubstituted C 1-3 Alkyl, -TMS, or substituted or unsubstituted C 2-3 Alkenyl groups. When R1 and R3 are selected from these groups, the electrolyte additive of the present invention can further reduce the electron-richness and alkalinity of the pyridine ring, thereby better suppressing electrolyte discoloration, suppressing the rise in battery impedance during cycling, and greatly improving cycle discharge capacity and capacity retention.

[0042] More preferably, in the above-mentioned electrolyte additive, R1 can be methyl, ethyl, propyl, -CH2-CN, -CH2-CH2-CN, -CH2-CH2-CH2-CN, -TMS, -CH2=CH3, -CH2=CH2-CH3, and R3 can be methyl, ethyl, propyl, phenyl, methyl-substituted phenyl, ethyl-substituted phenyl, -CH2-CN, -CH2-CH2-CN, or -CH2-CH2-CH2-CN. When R1 and R3 are selected from these groups, the electrolyte additive of the present invention can further reduce the electron-richness and alkalinity of the pyridine ring, thereby more effectively suppressing electrolyte discoloration, suppressing the rise in battery impedance during cycling, and greatly improving cycle discharge capacity and capacity retention.

[0043] Preferably, in the above-mentioned electrolyte additives, R2 and R4 can each be independently substituted or unsubstituted C. 1-3 Alkyl, -CN, substituted or unsubstituted C 2-3 alkenyl, -TMS or When R2 and R4 are selected from these groups, the electrolyte additive of the present invention can further reduce the electron-richness and alkalinity of the pyridine ring, thereby making it more effective in suppressing electrolyte discoloration, suppressing the rise in battery impedance during cycling, and greatly improving cycle discharge capacity and capacity retention.

[0044] Preferably, in the above-mentioned electrolyte additives, R2 and R4 can each independently be methyl, ethyl, propyl, -CN, -CH2=CH3, -CH2=CH2-CH3, -TMS, or... When R2 and R4 are selected from these groups, the electrolyte additive of the present invention can further reduce the electron-richness and alkalinity of the pyridine ring, thereby making it more effective in suppressing electrolyte discoloration, suppressing the rise in battery impedance during cycling, and greatly improving cycle discharge capacity and capacity retention.

[0045] Most preferably, R2 and R4 can each be -CN independently. When R2 and R4 are selected from this group, the electrolyte additive of the present invention can further reduce the electron-richness and alkalinity of the pyridine ring, thereby better suppressing electrolyte discoloration, suppressing the rise in battery impedance during cycling, and greatly improving cycle discharge capacity and capacity retention.

[0046] Preferably, in the above-mentioned electrolyte additive, the electrolyte additive comprises any one of the following substances:

[0047] According to another aspect of the invention, an electrolyte is provided comprising an organic solvent, a lithium salt, and the electrolyte additives described in the invention.

[0048] The electrolyte of the present invention contains the electrolyte additives described herein. Therefore, the electrolyte of the present invention can suppress electrolyte discoloration, significantly suppress the rise in battery impedance during cycling, and greatly improve cycle discharge capacity and capacity retention.

[0049] Preferably, in the above-mentioned electrolyte, the electrolyte additive may be present in an amount of 0.05 wt% to 2.0 wt% based on the total weight of the organic solvent and lithium salt. When the electrolyte additive is present in an amount within this range, the electrolyte of the present invention can further suppress the rise in battery impedance during cycling and greatly improve the cycle discharge capacity and capacity retention.

[0050] For example, based on the total weight of the organic solvent and lithium salt, the amount of electrolyte additive present can be 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, or 2.0 wt%.

[0051] Preferably, in the electrolyte, the organic solvent includes linear carbonates, cyclic carbonates, or combinations thereof. More preferably, in the electrolyte, the organic solvent is selected from one or more of ethylene carbonate, propylene carbonate, butyl carbonate, fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, dihexyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, and propyl propionate. The above are merely examples of organic solvents used in this invention, and are not intended to limit the invention. Those skilled in the art can select suitable organic solvents according to actual needs.

[0052] This invention does not impose any limitations on lithium salts; any lithium salts commonly used in the art can be used in this invention.

[0053] According to another aspect of the present invention, a lithium-ion secondary battery is provided, comprising: a positive electrode, a negative electrode, a separator, and an electrolyte as described in the present invention. The present invention does not impose any limitations on the positive electrode, negative electrode, or separator; commonly used positive electrodes, negative electrodes, and separators in the art can all be used in the present invention.

[0054] Since the lithium-ion secondary battery of the present invention uses the electrolyte described above, the lithium-ion secondary battery of the present invention can suppress electrolyte discoloration, significantly suppress the rise in battery impedance during cycling, and greatly improve cycle discharge capacity and capacity retention.

[0055] The present application is described in further detail below in conjunction with specific examples, which shall not be construed as limiting the scope of protection claimed by the present application.

[0056] Examples

[0057] Preparation of positive electrode plate

[0058] 95.5 g of positive electrode active material lithium nickel cobalt aluminate NCA (specifically Li[Ni 0.8 Co 0.1 Al 0.1 O₂), 2.5 g of conductive carbon black, 1.9 g of polyvinylidene fluoride and 0.1 g of dispersant are mixed to obtain a positive electrode mixture, and the obtained mixture is dispersed in N-methylpyrrolidone to obtain a positive electrode mixture slurry. Subsequently, the positive electrode mixture slurry is coated on an aluminum foil to obtain a positive electrode current collector, the positive electrode current collector is dried, and a stamping forming process is used to form the positive electrode plate.

[0059] Preparation of negative electrode plate

[0060] 95.85 g of a mixture of silicon monoxide (SiOₓ, 1<x<2) and graphite powder at a weight ratio of 1:11, 1 g of Super P, 3.15 g of a binder mixture of carboxymethyl cellulose (CMC) and styrene-butadiene latex (SBR) at a weight ratio of 1:1, and an appropriate amount of water are stirred to prepare a negative electrode slurry. Then, the obtained negative electrode slurry is uniformly coated on a copper foil to obtain a negative electrode current collector, the negative electrode current collector is dried, and a stamping forming process is used to form the negative electrode plate.

[0061] Preparation of base electrolyte

[0062] 20.8 g of ethylene carbonate, 56.7 g of dimethyl carbonate, 3.5 g of ethyl methyl carbonate (at a weight ratio of 6:16:1), 0.4 g of lithium tetrafluoroborate and 18.6 g of lithium hexafluorophosphate (1.5 M) are mixed and stirred uniformly to prepare the base electrolyte.

[0063] Preparation of electrolytes of Examples 1-17

[0064] 0.5 g (0.5 wt%) of each of the electrolyte additives (1)-(10) and (12)-(18) is added to the base electrolyte respectively. The mixture is homogenized and set aside for later use.

[0065] Preparation of electrolyte of Example 18

[0066] The preparation of the electrolyte of Example 18 is the same as the preparation of the electrolyte of Example 1, except that the amount of the electrolyte additive in Example 1 is changed to 0.025 g (0.025 wt%).

[0067] Preparation of electrolyte of Example 19

[0068] Except for changing the amount of electrolyte additive in Example 6 to 0.025 g (0.025 wt%), the preparation of the electrolyte in Example 19 is the same as that in Example 6.

[0069] Preparation of electrolyte in Example 20

[0070] Except for changing the amount of electrolyte additive in Example 7 to 0.025 g (0.025 wt%), the preparation of the electrolyte in Example 20 is the same as that in Example 7.

[0071] Preparation of electrolyte in Example 21

[0072] Except for changing the amount of electrolyte additive in Example 1 to 0.05 g (0.05 wt%), the preparation of the electrolyte in Example 21 is the same as that in Example 1.

[0073] Preparation of electrolyte in Example 22

[0074] Except for changing the amount of electrolyte additive in Example 3 to 0.05 g (0.05 wt%), the preparation of the electrolyte in Example 22 is the same as that in Example 3.

[0075] Preparation of electrolyte in Example 23

[0076] Except for changing the amount of electrolyte additive in Example 6 to 0.05 g (0.05 wt%), the preparation of the electrolyte in Example 23 is the same as that in Example 6.

[0077] Preparation of electrolyte in Example 24

[0078] Except for changing the amount of electrolyte additive in Example 7 to 0.05 g (0.05 wt%), the preparation of the electrolyte in Example 24 is the same as that in Example 7.

[0079] Preparation of electrolyte in Example 25

[0080] Except for changing the amount of electrolyte additive in Example 1 to 0.1 g (0.1 wt%), the preparation of the electrolyte in Example 25 is the same as that in Example 1.

[0081] Preparation of electrolyte in Example 26

[0082] Except for changing the amount of electrolyte additive in Example 6 to 0.1 g (0.1 wt%), the preparation of the electrolyte in Example 26 is the same as that in Example 6.

[0083] Preparation of electrolyte in Example 27

[0084] Except for changing the amount of electrolyte additive in Example 1 to 1.0 g (1.0 wt%), the preparation of the electrolyte in Example 27 is the same as that in Example 1.

[0085] Preparation of electrolyte in Example 28

[0086] Except for changing the amount of electrolyte additive in Example 6 to 1.0 g (1.0 wt%), the preparation of the electrolyte in Example 28 is the same as that in Example 6.

[0087] Preparation of electrolyte in Example 29

[0088] Except for changing the amount of electrolyte additive in Example 1 to 3.0 g (3.0 wt%), the preparation of the electrolyte in Example 29 is the same as that in Example 1.

[0089] Preparation of the electrolyte in Example 30

[0090] Except for changing the amount of electrolyte additive in Example 6 to 3.0 g (3.0 wt%), the preparation of the electrolyte in Example 30 is the same as that in Example 6.

[0091] Preparation of electrolyte in Example 31

[0092] Except for changing the amount of electrolyte additive in Example 7 to 3.0 g (3.0 wt%), the preparation of the electrolyte in Example 31 is the same as that in Example 7.

[0093] Preparation of electrolyte in Example 32

[0094] Except for changing the amount of electrolyte additive in Example 3 to 2.0 g (2.0 wt%), the preparation of the electrolyte in Example 32 is the same as that in Example 3.

[0095] Preparation of electrolyte in Example 33

[0096] Except for changing the amount of electrolyte additive in Example 6 to 2.0 g (2.0 wt%), the preparation of the electrolyte in Example 33 is the same as that in Example 6.

[0097] Preparation of electrolyte in Example 34

[0098] Except for changing the amount of electrolyte additive in Example 7 to 2.0 g (2.0 wt%), the preparation of the electrolyte in Example 34 is the same as that in Example 7.

[0099] Preparation of electrolytes in Comparative Examples 1-4

[0100] The electrolyte for Comparative Example 1 is the basic electrolyte prepared above.

[0101] Except that the electrolyte additives of the present invention are replaced with electrolyte additives A, B and C respectively, the preparation of the electrolytes in Comparative Examples 2-4 is the same as that in Examples 1-17, wherein:

[0102] Battery assembly

[0103] CR2016 coin cells were assembled in a dry laboratory. The positive electrode sheet prepared in the above steps was used as the positive electrode, the negative electrode sheet as the negative electrode, and the electrolyte prepared in the examples and comparative examples was used as the electrolyte. The positive electrode, negative electrode, separator, and coin cell casing were assembled, and the electrolyte was injected. After assembly, the cells were allowed to stand for 12 hours to age, thus obtaining the coin cell.

[0104] Battery performance testing

[0105] 1. Use a charge / discharge tester to test the battery's cycle performance and impedance.

[0106] The batteries in the above embodiments and comparative examples were first subjected to a 0.1C cycle test once at 23°C between OCV and 4.2V, and the initial discharge capacity (discharge capacity of the first cycle) and impedance (initial impedance) were measured. Then, at 60°C, a 0.5C charge and 5C discharge cycle test was performed 100 times between 2.5V and 4.2V, and the discharge capacity of the 100th cycle was measured. Based on the following formula: Capacity retention rate after 100 cycles [%] = (Discharge capacity of the 100th cycle / Discharge capacity of the first cycle) × 100%, the capacity retention rate (%) after 100 cycles was calculated using the discharge capacity of the first cycle and the discharge capacity of the 100th cycle. Finally, a 0.5C charge test was performed once at 60°C, and the battery impedance value (final impedance) was measured. The impedance growth rate was calculated using the following formula: Impedance growth rate [%] = [(Final impedance - Initial impedance) / Initial impedance] × 100%.

[0107] The performance test results of the batteries in Examples 1-34 and Comparative Examples 1-4 are shown in Table 1 below.

[0108] Table 1

[0109] As can be seen from the test results in Table 1, the above embodiments of the present invention achieve the following technical effects:

[0110] Compared with Comparative Example 1, which did not have electrolyte additives, the batteries (Examples 1-34) containing the electrolyte additives (1)-(10) and (12)-(18) of the present invention showed a significantly reduced impedance growth rate during cycling. Except for the discharge capacity of Example 29, which was comparable to that of Comparative Example 1, the discharge capacity of the 100th cycle was significantly increased, and the capacity retention rate was significantly increased.

[0111] Compared with Comparative Examples 2-4, which contain the same amount of electrolyte additives A, B and C respectively, the batteries (Examples 1-17) containing the electrolyte additives (1)-(10) and (12)-(18) of the present invention showed a significantly lower impedance growth rate during cycling, a significantly higher discharge capacity at the 100th cycle, and a significantly increased capacity retention rate.

[0112] Comparing Examples 3, 6, and 7 with Example 1, it is evident that the batteries containing the same amounts of electrolytes from Examples 3, 6, and 7 exhibit a significantly lower impedance growth rate during cycling, a more significantly higher discharge capacity at the 100th cycle, and a more significantly increased capacity retention. Similar results are demonstrated by comparing Examples 19 and 20 with Example 18, Examples 22-24 with Example 21, Examples 26 with Example 25, Examples 28 with Example 27, and Examples 30-31 with Example 29.

[0113] 2. Color change of electrolyte

[0114] This invention uses a DR2800 Hazen spectrophotometer to detect the color of the electrolyte. According to SJ / T 11723-2018 "Electrolytes for Lithium-ion Batteries," the color of the electrolyte for lithium-ion batteries should be tested according to GB / T3143 "Determination of Color of Liquid Chemical Products - Hazen Units - Platinum-Cobalt Color." Firstly, the appearance should be a liquid without sediment, suspended matter, or stratification, and the color index should be ≤50 HAZEN.

[0115] The color of the base electrolyte, vinyl sulfate (DTD) and electrolyte containing the electrolyte additives (1)-(10) of the present invention (Examples 1-10) is shown in Figure 1 and Table 2 below, both when freshly prepared and after being stored at 25-30°C for 30 days in an environment isolated from water and oxygen.

[0116] Table 2

[0117] Referring to Figure 1 and Table 2, it can be seen that the electrolytes containing the electrolyte additives (1)-(10) of the present invention (Examples 1-10) showed no significant color change after 30 days of storage compared to fresh electrolytes. Therefore, the electrolyte additives of the present invention are stable and easy to transport and store. In contrast, vinyl sulfate (DTD) itself is unstable, and transportation and storage require an environment below 15°C; otherwise, it is prone to deterioration, which can lead to discoloration of the electrolyte.

[0118] The battery performance test results above show that by using the electrolyte additive of the present invention, electrolyte discoloration can be suppressed, the impedance rise of the battery during cycling can be significantly suppressed, and the cycle discharge capacity and capacity retention rate can be greatly improved.

[0119] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An electrolyte additive, characterized in that, The electrolyte additive comprises any one of the following substances: Where R1 is substituted or unsubstituted C 1-7 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl; R2 is independently either substituted or unsubstituted C. 1-7 Alkyl, -CN, substituted or unsubstituted C 2-3 alkenyl, -TMS, R3 is a substituted or unsubstituted phenyl group, or a substituted or unsubstituted C group. 1-7 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl; R4 is independently either substituted or unsubstituted C. 1-7 Alkyl, -CN, substituted or unsubstituted C 2-3 alkenyl, -TMS, R5 and R6 are independently substituted or unsubstituted C. 1-3 Alkyl, -CN, -TMS, or substituted or unsubstituted C 2-3 alkenyl; n is an integer between 0 and 4.

2. The electrolyte additive according to claim 1, characterized in that, Group It is located in the ortho or meta position of the nitrogen atom in pyridine.

3. The electrolyte additive according to claim 1 or 2, characterized in that, n is 0 or 1.

4. The electrolyte additive according to claim 1 or 2, characterized in that, R2 and R4 are located either adjacent to the nitrogen atom of pyridine or located in the group. The neighboring position.

5. The electrolyte additive according to claim 1 or 2, characterized in that, R1 is -CN, substituted or unsubstituted C. 1-3 Alkyl, -TMS, or substituted or unsubstituted C 2-3 Alkenyl group, R3 is a substituted or unsubstituted phenyl group, -CN group, substituted or unsubstituted C group. 1-3 Alkyl, -TMS, or substituted or unsubstituted C 2-3 Alkenyl group.

6. The electrolyte additive according to claim 1 or 2, characterized in that, R2 and R4 are each independently substituted or unsubstituted C. 1-3 Alkyl, -CN, substituted or unsubstituted C 2-3 alkenyl, -TMS or 7. The electrolyte additive according to claim 1 or 2, characterized in that, R2 and R4 can each be independently methyl, ethyl, propyl, -CN, -CH2=CH3, -CH2=CH2-CH3, -TMS, or 8. The electrolyte additive according to claim 1 or 2, characterized in that, The electrolyte additive comprises any one of the following substances:

9. An electrolyte comprising an organic solvent, a lithium salt, and an electrolyte additive according to any one of claims 1 to 8.

10. The electrolyte according to claim 9, characterized in that, The electrolyte additive is present in an amount of 0.05 wt% to 2.0 wt% based on the total weight of the organic solvent and the lithium salt.

11. The electrolyte according to claim 9 or 10, characterized in that, The organic solvent includes linear carbonates, cyclic carbonates, or combinations thereof.

12. A lithium-ion secondary battery, characterized in that, include: positive electrode, negative electrode, Diaphragm, and The electrolyte according to any one of claims 9 to 11.