Non-aqueous electrolyte secondary battery
The non-aqueous electrolyte secondary battery addresses capacity degradation issues by employing a through-holed current collector, fibrous PTFE binder, and a specific particle size and ratio mix of lithium manganese and transition metal oxides, enhancing adhesion and reducing manganese leaching to maintain battery performance.
Patent Information
- Application Number
- PCT/JP2026/015731
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-20
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional lithium-ion batteries face issues with capacity degradation due to charge-discharge cycles, particularly when using spinel-type lithium manganese oxide as the positive electrode active material, which leads to delamination and manganese leaching, especially under high-temperature conditions.
A non-aqueous electrolyte secondary battery design utilizing a positive electrode current collector with through holes, a fibrous polytetrafluoroethylene (PTFE) binder, and a combination of large-particle spinel-type lithium manganese oxide and small-particle lithium transition metal oxide with a layered rock salt structure, optimized in terms of mixing ratio and particle size, to enhance adhesion and minimize manganese leaching.
The design effectively suppresses capacity degradation by improving adhesion and reducing resistance, thereby maintaining battery performance over charge-discharge cycles.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000017_0000 
Figure 00000017_0001
Abstract
Description
Non-aqueous electrolyte secondary battery
[0001] This invention relates to a non-aqueous electrolyte secondary battery, and more particularly to the configuration of a positive electrode current collector and a positive electrode mixture.
[0002] Traditionally, lithium cobalt oxide and nickel-cobalt-manganese composite oxides have been commonly used as positive electrode active materials in lithium-ion batteries. Cobalt, used in these positive electrode active materials, is a rare metal and contributes to the high cost of batteries. Therefore, research and development are underway to reduce the amount of cobalt used, and among these, materials mainly composed of inexpensive manganese are attracting attention as positive electrode active materials.
[0003] Furthermore, in the positive electrode of a lithium-ion battery, a positive electrode mixture layer containing positive electrode active material and a binder is typically provided on the surface of a positive electrode current collector made of metal foil. This positive electrode mixture layer is manufactured by a wet process in which a highly fluid slurry or paste-like positive electrode mixture with a solid content of approximately 60% to 40% by mass is applied. This wet process requires a drying step to evaporate and remove the solvent from the coating obtained by application, which has been a factor in increasing the cost of batteries.
[0004] In response to this, in recent years, dry methods have been proposed for manufacturing electrodes using positive electrode mixtures with a solid content of 80% by mass or more, or powdered positive electrode mixtures that do not use solvents. For example, Patent Document 1 (U.S. Patent Application Publication No. 2007 / 0042274) describes a method for manufacturing electrodes in which a paste-like electrode mixture is supplied to the surface of a current collector to be deposited, and the resulting deposited layer is heated and then pressurized (rolled) in the thickness direction. Separately, a method has also been proposed in which a paste-like positive electrode mixture is compressed into a sheet, and the resulting positive electrode mixture sheet is laminated onto a current collector.
[0005] U.S. Patent Application Publication No. 2007 / 0042274
[0006] However, in the above-described dry method for manufacturing electrodes, it is not possible to use a slurry in which polyvinylidene fluoride (PVdF), which is used as a binder, is dissolved in N-methylpyrrolidone (NMP), and therefore the adhesive and bonding properties of such a slurry cannot be utilized.
[0007] Furthermore, spinel-type lithium manganese oxide, which is the positive electrode active material, exhibits a larger change in lattice constant during charging and discharging compared to lithium cobalt oxide and lithium nickelate, which have a layered rock salt structure. Therefore, when aluminum foil or the like is used as the current collector, the change in lattice volume during the charge-discharge cycle can easily cause delamination at the interface between the positive electrode mixture layer and the positive electrode current collector, leading to a decrease in initial performance and rapid degradation due to increased resistance during the charge-discharge cycle.
[0008] Furthermore, even when using a positive electrode current collector with through holes, when spinel-type lithium manganese oxide was used as the positive electrode active material, manganese leached out due to changes in the crystal structure associated with the charge-discharge cycle, and the degradation of the charge-discharge cycle was particularly pronounced under high-temperature environments.
[0009] In view of the above-mentioned problems of the conventional battery, the object of the present invention is to provide a non-aqueous electrolyte secondary battery that can suppress capacity degradation due to charge-discharge cycles.
[0010] The inventors of the present invention have conducted numerous experiments and studies to determine the details of the constituent materials of a non-aqueous electrolyte secondary battery. As a result, they have found that a non-aqueous electrolyte secondary battery that can suppress capacity degradation due to charge-discharge cycles can be realized mainly by (1) using fibrous polytetrafluoroethylene (PTFE) as a binder, (2) using a positive electrode current collector with through holes as the positive electrode current collector, and (3) using a combination of large-particle and small-particle positive electrode active material. This has led to the completion of the present invention.
[0011] In other words, the non-aqueous electrolyte secondary battery according to the present invention comprises a positive electrode having a positive electrode mixture layer and a positive electrode current collector, a negative electrode having a negative electrode mixture layer and a negative electrode current collector, and a non-aqueous electrolyte, wherein the positive electrode current collector has a plurality of through holes, the positive electrode mixture constituting the positive electrode mixture layer contains at least a binder comprising a fibrous polymer material made of polytetrafluoroethylene, and a first positive electrode active material (large particles) comprising spinel-type lithium manganese oxide having a first average particle size of 15 μm to 25 μm and a second positive electrode active material (small particles) comprising lithium transition metal oxide having a layered rock salt structure with a second average particle size smaller than the first average particle size of 3 μm to 10 μm, and the mixed volume ratio of the first positive electrode active material to the second positive electrode active material is 90 / 10 to 60 / 40.
[0012] Furthermore, in the non-aqueous electrolyte secondary battery of the present invention described above, it is preferable that the lithium transition metal oxide having the layered rock salt structure contains nickel, manganese, and cobalt, and that the molar ratio of nickel is 60% or less.
[0013] According to the present invention, it is possible to provide a non-aqueous electrolyte secondary battery that can suppress capacity degradation due to charge-discharge cycles.
[0014] This is a schematic plan view illustrating the openings that constitute the through-holes of the positive electrode current collector. This is a schematic diagram illustrating the structure of the aluminum laminate battery (lithium secondary battery) fabricated in the embodiment.
[0015] Hereinafter, the non-aqueous electrolyte secondary battery according to the present invention will be described using a lithium-ion secondary battery as a representative embodiment, but the present invention is not limited to this embodiment. The lithium-ion secondary battery of this embodiment has a configuration in which an electrode body having a structure in which the positive electrode comprising a positive electrode mixture layer and a positive electrode current collector, a negative electrode comprising a negative electrode mixture layer and a negative electrode current collector, and a non-aqueous electrolyte, with the positive electrode and negative electrode stacked via a separator, is housed together with the non-aqueous electrolyte in a battery case.
[0016] (1) Positive electrode The positive electrode of this embodiment comprises a positive electrode mixture layer and a positive electrode current collector. As the positive electrode current collector, for example, a long conductive sheet can be used, and the conductive sheet has regularly spaced holes (through holes) that penetrate from the front and back (from the first surface to the second surface). As the conductive sheet, a metal sheet mainly made of aluminum can be used, for example, expanded metal, perforated metal, or metal foil with partially formed through holes. Alternatively, a conductive sheet having a three-dimensional structure in the thickness direction (for example, a three-dimensional solid structure) may be used. Examples of aluminum foil include 1085, 1N30, 3003 series, 8000 series, and so on.
[0017] Here, there are no particular limitations on the shape or aperture ratio of the opening(s) that constitute the through-hole, but it is preferable that the shortest distance of the opening be at least D90 or greater, which is the average particle size of the first positive electrode active material (large particles). This is because a shorter opening distance of this magnitude makes it easier to improve the adhesion between the positive electrode mixture layers on the front and back. On the other hand, the optimal longest distance of the opening depends on the thickness, material, and strength of the positive electrode current collector (e.g., aluminum), but for example, in the case of high-purity aluminum expanded metal with a thickness of 30 μm, it is preferable that the longest distance be 2 mm or less. If the longest distance is 2 mm or less, the distribution of the distance from the positive electrode current collector (e.g., aluminum) to the positive electrode active material does not become too wide, which makes it less likely for uneven reactions to occur during charging and discharging, and may suppress the deterioration of battery performance. Figure 1 is a schematic plan view illustrating the opening of the positive electrode current collector.
[0018] Furthermore, the aperture ratio is preferably between 30% and 70%. A higher aperture ratio allows for a reduction in the volume of the current collector, enabling the inclusion of more positive electrode active material and thus increasing the battery capacity. On the other hand, by not increasing the aperture ratio too much, the decrease in strength that is proportional to the aperture ratio can be suppressed, and the risk of the positive electrode current collector fracturing during the electrode manufacturing process is also reduced.
[0019] The positive electrode mixture layer is provided on both sides of the positive electrode current collector, and the positive electrode mixture constituting the positive electrode mixture layer contains at least a binder, and a first positive electrode active material (large particles) having a first average particle size and a second positive electrode active material (small particles) having a second average particle size smaller than the first average particle size. The binder of the positive electrode in this embodiment is a fibrous polymer material made of fibrous polytetrafluoroethylene (PTFE) or a modified version thereof. The three-dimensional structure of fine fibers improves the adhesion between positive electrode active material particles, including the first and second positive electrode active materials, in the positive electrode mixture. In particular, by using a positive electrode current collector having through holes as described above, even if the electrodes are manufactured by a dry method, for example, the presence of fibril portions of the fibrous PTFE binder, which will be described later, allows the positive electrode mixture layers on both sides to adhere firmly to the positive electrode current collector through the through holes.
[0020] Furthermore, the positive electrode mixture of this embodiment contains, in addition to the binder, a first positive electrode active material (large particles) made of spinel-type lithium manganese oxide having a first average particle size of 15 μm to 25 μm, and a second positive electrode active material (small particles) made of lithium transition metal oxide having a layered rock salt structure and a second average particle size smaller than the first average particle size of 3 μm to 10 μm. In other words, the first average particle size D1 of the first positive electrode active material and the second average particle size D2 of the second positive electrode active material have the same unit and the relationship D1 > D2.
[0021] Examples of spinel-type lithium manganese oxides that constitute the large-particle first positive electrode active material include LiMn 2 O 4 Examples include those shown, where some of the Mn sites may be occupied by metallic elements such as Al, Mg, Ti, and Li. When using spinel-type lithium manganese oxide, it is possible to minimize the surface area of the positive electrode active material by increasing the particle size of the positive electrode active material, thereby minimizing manganese elution.
[0022] Furthermore, examples of lithium transition metal oxides having a layered rock salt structure that constitute the second positive electrode active material, which consists of small particles, include composite metal oxides of Li and at least one transition metal selected from Ba, Mn, Fe, Co, and Ni. In particular, from the viewpoint of effectively suppressing the decrease in initial capacity and the increase in resistance associated with charge-discharge cycles even when placed in a moisture-containing environment during the electrode manufacturing process, examples include lithium transition metal oxides with a Ni content (molar ratio) of more than 0 mol% to less than 90 mol% (preferably 60 mol% or less).
[0023] One challenge when using large-particle positive electrode active materials is that the contact area between positive electrode active materials decreases, making it difficult to maintain adhesion between positive electrode active materials using fibrous PTFE. This can lead to a significant increase in the initial resistance of the positive electrode and a corresponding increase in resistance with each charge-discharge cycle, potentially causing a decrease in initial capacity and degradation with each charge-discharge cycle. However, in this embodiment, the contact area between positive electrode active materials can be increased by arranging small particles between large particles, thus eliminating the aforementioned concerns. Since lithium transition metal oxides with a layered rock salt structure, which are small particles, have a stable crystal structure and are less prone to metal leaching, they can significantly suppress capacity degradation with each charge-discharge cycle compared to using only spinel-type lithium manganese oxide.
[0024] The mixing volume ratio of the first positive electrode active material (large particles) to the second positive electrode active material (small particles) is 90 / 10 to 60 / 40. From the viewpoint of increasing the filling rate and improving the charge-discharge cycle characteristics, it is generally preferable to be around 70 / 30 to 80 / 20. In addition, the average particle size D50 (first average particle size D1) of the first positive electrode active material (large particles) is in the range of 15 μm to 25 μm, and the average particle size D50 (second average particle size D2) of the second positive electrode active material (small particles) is 3 μm to 10 μm.
[0025] By satisfying these relationships between mixing volume ratio and average particle size, manganese leaching from the positive electrode active material can be suppressed, while conventional peeling between the positive electrode mixture layer and the positive electrode current collector, a decrease in initial performance, and rapid degradation due to resistance increase during cycles can be reduced, thereby suppressing a rapid decrease in capacity due to charge-discharge cycles. In particular, if the average particle size of the first positive electrode active material (large particles) is 25 μm or less, the solid-phase diffusion resistance within the particles does not increase easily, and a decrease in electrical performance can also be suppressed.
[0026] The average particle size (D50) of the positive electrode active material, including the first and second positive electrode active materials described above, can be defined as the particle size at 50% of the volume-cumulative particle size distribution of the particles. In the case of single particles, it refers to the average particle size of primary particles, and in the case of secondary particles, it refers to the average particle size of secondary particles. The particles may be single crystals. The average particle size (D50) can be measured, for example, using the laser diffraction method. After dispersing the powder to be measured in a dispersion medium, a volume-cumulative particle size distribution graph can be created using a commercially available laser diffraction particle size analyzer, and the particle size corresponding to 50% of the volume-cumulative amount can be determined.
[0027] Furthermore, the positive electrode mixture may contain, for example, a conductive material, as long as it does not impair the effects of the present invention. Examples of such conductive materials include carbon materials such as carbon black, acetylene black, Ketjen black, and graphite, and one of these may be used, or two or more may be used in combination.
[0028] (2) Negative electrode The negative electrode of this embodiment comprises a negative electrode mixture layer and a negative electrode current collector. As the negative electrode current collector, for example, a long conductive sheet can be used, and examples include stainless steel, nickel, copper, etc. Among these, copper is preferred from the viewpoint of material cost and chemical stability in the battery. Also, similar to the positive electrode, it may be expanded metal, perforated metal, metal foil with partially formed through holes, etc., or a conductive sheet having a three-dimensional structure in the thickness direction (for example, a three-dimensional structure).
[0029] The negative electrode mixture layer is provided on both sides of the negative electrode current collector, and the negative electrode mixture constituting the negative electrode mixture layer contains at least a binder and a negative electrode active material.
[0030] As the binder for the negative electrode in the present embodiment, conventionally known binders can be used. For example, similarly to the positive electrode, polytetrafluoroethylene (PTFE), other fluororesins, PAN, polyimide resins, polyethylene oxide, acrylic resins, polyolefin resins and the like can be used. In addition, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt may be present), polyvinyl alcohol (PVA), etc. may also be used. Furthermore, two or more types of binders may be included.
[0031] As the negative electrode active material, for example, a carbon-based active material that reversibly occludes and releases lithium ions can be used. Suitable carbon-based active materials include natural graphite such as flake graphite, massive graphite, and earthy graphite, artificial graphite such as massive artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB), silicon (Si), metals that form alloys with lithium such as tin (Sn), or alloys containing metal elements such as Si and Sn, composite oxides, and the like can be used.
[0032] (3) Separator As the separator interposed between the positive electrode and the negative electrode, for example, a porous sheet having ion permeability and insulating properties is used. Specific examples of the form of the porous sheet include, for example, microporous thin films, woven fabrics, non-woven fabrics and the like. Examples of the material of the separator include polyolefin, polyvinylidene fluoride, polytetrafluoroethylene, polyimide, polyamide, polyamideimide, polyethersulfone, polyetherimide, aramid and the like.
[0033] The above porous sheet may have a multilayer structure such as polypropylene / polyethylene / polypropylene, and a filler layer (heat-resistant layer) containing an inorganic filler may be formed at the interface between the separator and at least one of the positive electrode and the negative electrode.
[0034] (4) Non-aqueous electrolyte The non-aqueous electrolyte is obtained by dissolving an electrolyte in a non-aqueous solvent, and examples of the electrolyte include LiPF 6 , LIFSI(F 2 LiNO 4 S 2 ), LiBF 4 , LiClO 4 , LiCF 2 SO 3 , LiCF 3 CO 2 , LiN(CF 3 SO 2 ) 2 , LiN(C 3 F 5 SO 2 ) and the like. Each of these may be used alone, or a plurality of types may be used in combination. Among them, LIFSI is preferable because decomposition of the electrolyte hardly occurs particularly during high-temperature use, generation of hydrofluoric acid accompanying decomposition of the electrolytic solution is suppressed, and thus cycle deterioration of the battery can be significantly reduced. The concentration of the electrolyte in the non-aqueous electrolyte may be, for example, 0.5 to 2 mol / L.
[0035] Further, as the non-aqueous solvent, for example, cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, and vinylene carbonate, chain carbonates such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, formic acid, methyl methyl methyl, trimethyl phosphate, trimethoxymethane, sulfolane, 3-methyl-2-oxazolidinone, diethyl ether, 1,3-propane sultone and the like can also be used.
[0036] (5) The lithium-ion secondary battery of this embodiment has a configuration in which an electrode body, in which a positive electrode and a negative electrode are stacked with a separator as described above, is housed in an external case together with a non-aqueous electrolyte. The electrode body may be of other forms such as a wound type in addition to the stacked type, and the external case can be a metal case, a resin case formed by laminating a resin sheet (laminated battery), etc.
[0037] The lithium-ion secondary battery and its components according to this embodiment can be manufactured by conventionally known methods. In particular, the positive electrode mixture is preferably manufactured by a mixing step in which a positive electrode active material, a binder, and a conductive material are mixed, and then an appropriate amount of water is added to obtain a predetermined solid content, and a sizing and drying step in which the positive electrode mixture obtained in the mixing step is subjected to first sizing, drying, and second sizing in this order.
[0038] In this manufacturing method, the positive electrode mixture obtained in the grain sizing and drying process may be further rolled between two rolls with different peripheral speed ratios to produce a positive electrode mixture sheet, and the positive electrode mixture sheet and the core material may be laminated and pressed.
[0039] Although typical embodiments of the present invention have been described above, the present invention is not limited to these, and various design modifications are possible, all of which fall within the technical scope of the present invention. Furthermore, the present invention will be specifically described below based on examples, but the present invention is not limited to these examples.
[0040] <Example 1> In this example, an aluminum laminate battery with the structure shown in Figure 2 was fabricated. Figure 2 is a schematic diagram of a partially disassembled part to explain the structure of the aluminum laminate battery (lithium secondary battery) 1 fabricated in this example. This aluminum laminate battery 1 is constructed by housing an electrode body, which is a laminate of a positive electrode 2 with a positive electrode terminal 2a, a separator 4, and a negative electrode 6 with a negative electrode terminal 6a, in a bag 8 made of aluminum laminate film, injecting a non-aqueous electrolyte (not shown), and sealing it. [Fabrication of the positive electrode] First, spinel-type lithium manganese oxide (chemical formula LiMn) with an average particle size of 18 μm was prepared as the first positive electrode active material (large particle).2 O 4 ) and LiNi with an average particle size of 6 μm as the second positive electrode active material (small particles) 0.6 Co 0.2 Mn 0.2 O 2 A mixture was prepared by mixing the materials in a volume ratio of 70 / 30. Next, this mixture, acetylene black as a conductive material, and water-dispersed polytetrafluoroethylene (PTFE) with a solid content of 50% by mass as a binder were mixed in a mass ratio of 91:5:4. After that, the solid content was adjusted with water to 95%, and the mixture was put into a granulator and mixed (wet granulation) was performed at room temperature, at a rotation speed of 14,000 rpm for 2 minutes. The cathode mixture obtained by wet granulation in this way was sized using a sizing machine with a mesh of 6 to 12 mesh. The sized cathode mixture was dried in a dryer to a predetermined moisture content, and then sized again using a sizing machine with a mesh of 24 mesh. Through this process, the PTFE particles were fibrous, and a cathode mixture was obtained in which the first cathode active material, second cathode active material, fibrous PTFE, and acetylene black were uniformly dispersed.
[0041] The obtained positive electrode mixture was rolled by passing it between two rolls to produce a positive electrode mixture sheet. The peripheral speed ratio of the two rolls was set to 1:3, and the positive electrode mixture sheet was adjusted by performing multiple stretching processes. The obtained positive electrode mixture sheet was placed on both sides of the positive electrode current collector, and the laminate of the positive electrode mixture sheet and the positive electrode current collector was compressed in a press with a roll diameter of 350 mm. This compression resulted in a positive electrode in which the positive electrode mixture sheet was firmly bonded to both sides of the current collector. As the positive electrode current collector, expanded metal with an opening ratio of 50% was used, which was obtained by making staggered cuts in a 30 μm thick high-purity aluminum sheet using an expander and simultaneously pushing it open from side to side.
[0042] [Preparation of the negative electrode] First, flake-shaped artificial graphite was crushed and classified so that the average particle size was approximately 20 μm. Next, 100 parts by mass of flake-shaped artificial graphite was mixed with 1 part by mass of styrene / butadiene rubber (binder) and 100 parts by mass of an aqueous solution containing 1% by mass of carboxymethylcellulose to obtain a negative electrode mixture slurry. Then, this negative electrode mixture slurry was applied to both sides of an 8 μm thick copper foil (negative electrode current collector) and dried. Finally, it was compressed to a predetermined thickness to obtain the negative electrode.
[0043] [Preparation of Non-Aqueous Electrolyte] 1% by mass of vinylene carbonate was added to a mixed solvent in which the volume ratio of ethylene carbonate and ethyl methyl carbonate was 3:7. 1.2 mol / m³ 3 LiPF at this concentration 6 A non-aqueous electrolyte was prepared by dissolving the substance.
[0044] [Fabrication of Laminated Battery] A negative electrode was laminated to both sides of the positive electrode obtained as described above, with a separator (16 μm thick, porous polyethylene film with 42% porosity) in between, to create a laminated electrode body. Next, the electrode body and electrolyte (LiPF) were placed on an aluminum laminate film. 6 After inserting and housing 1.2M [EC / EMC = 30 / 70 volume%] VC2 mass), an aluminum laminate film was sealed to create a laminate battery for evaluation testing with a design capacity of 100 mAh.
[0045] <Examples 2-7 and Comparative Examples 1-8> Laminate batteries for evaluation testing were prepared in the same manner as in Example 1, except that the average particle size of the first positive electrode active material (large particles) and the second positive electrode active material (small particles), the presence or absence of an opening in the positive electrode current collector, and the nickel ratio of the second positive electrode active material were changed to the conditions shown in Table 1.
[0046] [Charge and Discharge Test] The laminated batteries prepared as described above were evaluated for their initial capacity and cycle characteristics under the following test conditions. Initial capacity and capacity retention rate in the cycle test were measured under the following conditions. The results of the initial capacity measurement and the capacity retention rate at 500 cycles in the cycle test are shown in Table 1. (1) Initial capacity measurement Charging CCCV / 0.2C / 4.2V Discharge CC / 0.2C / 2.75Vcut Temperature 25℃ (2) Capacity retention rate measurement in cycle test Charging CCCV / 0.5C / 4.2V Discharge CC / 0.5C / 2.75Vcut Temperature 40℃
[0047] [Overall Assessment] <Comparison of Example 1 and Comparative Example 1> Since the battery of Comparative Example 1 did not have an opening in the core material, the positive electrode mixture layer and the core material could not adhere to each other, making it impossible to evaluate the battery.
[0048] <Comparison of Examples 1, 2, and 3 and Comparative Examples 2 and 3> In the batteries of Examples 1, 2, and 3, the mixing ratio of small particles was in the range of 10 to 40 vol. Therefore, the small particles were optimally filled between the large particles, improving the contact area between the active materials. By increasing the contact area between the positive electrode active materials, it was possible to improve the electrical contact between the active materials and the holding force between the active materials by the PTFE fibers, thereby improving the initial capacity and cycle performance. On the other hand, in Comparative Examples 2 and 3, the mixing ratio of large and small particles was outside the range of 10 to 40 vol. Therefore, the contact area between the large and small particles could not be sufficiently increased, resulting in insufficient electrical contact between the active materials and insufficient holding force between the active materials by the PTFE fibers, leading to a decrease in initial capacity and cycle performance.
[0049] <Comparison of Examples 1, 4, 5, 6, 7 and Comparative Examples 4, 5, 6, 7> In Examples 1, 4, 5, 6, and 7, the average particle diameter of the large particles was in the range of 15 to 25 μm. As small particles were optimally filled between the large particles, the contact area between the active materials was improved. By increasing the contact area between the positive electrode active materials, it was possible to improve the electrical contact between the active materials and the holding force between the active materials by the PTFE fibers, thereby improving the initial capacity and cycle performance. On the other hand, in Comparative Examples 4 and 5, the average particle diameter of the small particles was outside the range of 3 to 10 μm. As a result, the contact area between the large and small particles could not be sufficiently increased, resulting in insufficient electrical contact between the active materials and insufficient holding force between the active materials by the PTFE fibers, leading to a decrease in initial capacity and cycle performance. Furthermore, in the battery of Comparative Example 6, the average particle diameter of the large particles was 25 μm or more, which resulted in high solid-phase diffusion resistance and a decrease in initial capacity and cycle characteristics. On the other hand, in Comparative Example 7, the average particle size of the large particles was 15 μm or less, which increased the surface area of the spinel-type lithium manganese oxide, accelerating manganese leaching and leading to cycle degradation.
[0050] <Comparison of Example 1 and Comparative Example 8> Compared to the battery of Example 1, the battery of Example 8 has a molar ratio of small nickel particles of 0.8, which causes the surface of the positive electrode active material to react with water during the electrode manufacturing process, degrading the active material and accelerating the decrease in initial capacity and the deterioration of cycle performance.
Claims
1. A non-aqueous electrolyte secondary battery comprising a positive electrode having a positive electrode mixture layer and a positive electrode current collector, a negative electrode having a negative electrode mixture layer and a negative electrode current collector, and a non-aqueous electrolyte, wherein the positive electrode current collector has a plurality of through holes, and the positive electrode mixture constituting the positive electrode mixture layer contains at least a binder comprising a fibrous polymer material made of polytetrafluoroethylene, and a first positive electrode active material comprising a spinel-type lithium manganese oxide having a first average particle size of 15 μm to 25 μm and a second positive electrode active material comprising a lithium transition metal oxide having a layered rock salt structure with a second average particle size smaller than the first average particle size of 3 μm to 10 μm, and the mixed volume ratio of the first positive electrode active material to the second positive electrode active material is 90 / 10 to 60 / 40.
2. The non-aqueous electrolyte secondary battery according to claim 1, characterized in that the lithium transition metal oxide having a layered rock salt structure contains nickel, manganese, and cobalt, and the molar ratio of nickel is 60% or less.