Curable composition, cured film, and display device
A curable composition with controlled weight loss and polymerizable compounds stabilizes semiconductor particles, addressing luminescence intensity loss in exposure processes, enhancing the performance of wavelength conversion films.
Patent Information
- Application Number
- PCT/JP2026/017334
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-05-01
- Publication Date
- 2026-11-12
AI Technical Summary
Exposure processes such as photolithography can reduce the emission intensity of wavelength-converted light in curable films containing semiconductor particles, leading to a decrease in luminescence intensity.
A curable composition comprising semiconductor particles with specific weight loss ratios and polymerizable compounds, optionally including resins, light scattering agents, and polymerization initiators, which suppress the decrease in luminescence intensity before and after exposure.
The composition effectively maintains luminescence intensity by stabilizing semiconductor particles and enhancing their dispersibility, thereby improving the performance of wavelength conversion films.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Curable composition, cured film, and display device
[0001] This disclosure relates to a curable composition containing semiconductor particles, a cured film, and a display device containing the cured film.
[0002] A curable resin composition containing semiconductor particles such as semiconductor quantum dots is known for forming curable films such as wavelength conversion films included in display devices such as image display devices (Patent Document 1).
[0003] Japanese Patent Publication No. 2021-105108
[0004] One example of a method for forming the cured film such as the wavelength conversion film described above is the photolithography method. In the photolithography method, a curable composition containing semiconductor particles is applied to a substrate, dried (pre-baked) to remove volatile components such as solvents to obtain a composition layer, the composition layer is exposed to air through a photomask, and the exposed composition layer is brought into contact with a developer solution to develop it, thereby obtaining a patterned cured film. It is preferable to further heat (post-bake) the patterned film obtained by development.
[0005] Cured films, such as wavelength-converting films, formed from curable compositions containing semiconductor particles, are films that absorb primary light from a primary light source and emit light that has been wavelength-converted (color-converted). Our investigations revealed that exposure processes such as photolithography can sometimes reduce the emission intensity of the wavelength-converted light.
[0006] Therefore, the present disclosure aims to provide a curable composition containing semiconductor particles that can be applied to a method for obtaining a cured film by exposure such as photolithography, and which can suppress the decrease in luminescence intensity before and after the exposure process (hereinafter also referred to as "process tolerance").
[0007] The contents of this disclosure that have achieved the above objectives are as follows: [1] A curable composition comprising semiconductor particles (A) and a polymerizable compound (D), wherein the semiconductor particles (A) comprises an organic ligand (G), and the weight loss ratio X above 300°C, calculated by formula (1) when the semiconductor particles (A) comprising the organic ligand (G) are heated from 25°C to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min by thermogravimetric analysis, is 35% or less, and the clogP of the polymerizable compound (D) is 3.5 or more. Weight loss ratio above 300°C X (%) = {T1 / (T0+T1)} × 100 … (1) [In formula (1), T 0 This is the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight, and T 1 [1] is the weight loss rate from 300°C to 600°C, based on the weight of semiconductor particles (A) containing an organic ligand (G) at 100°C. [2] The curable composition according to [1], further comprising a resin (C). [3] The curable composition according to [1] or [2], further comprising a light scattering agent (B). [4] The curable composition according to any one of [1] to [3], wherein the weight loss ratio X at 300°C or higher is 5 to 25%, and the clogP of the polymerizable compound (D) is 3.8 to 7.0. [5] The curable composition according to any one of [1] to [4], wherein the content of the polymerizable compound (D) is 4% by mass or more and 70% by mass or less, based on 100% by mass of the total amount of solids in the curable composition. [6] The curable composition according to any one of [1] to [5], wherein the polymerizable compound (D) comprises at least one selected from the group consisting of dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, di(meth)acrylate of ethoxylated bisphenol A, and di(meth)acrylate of ethoxylated bisphenol F. [7] The curable composition according to any one of [1] to [6], further comprising a polymerization initiator (E), wherein the polymerization initiator (E) comprises an oxime compound. [8] A cured film formed from the curable composition according to any one of [1] to [7]. [9] A display device comprising the cured film according to [8].
[0008] The curable composition of this disclosure makes it possible to suppress the decrease in the luminescence intensity of a cured film containing semiconductor particles before and after exposure.
[0009] <<Curable Composition>> The curable composition comprises semiconductor particles (A) and polymerizable compounds (D), wherein the semiconductor particles (A) contain organic ligands (G) and, if necessary, preferably at least one selected from light scattering agents (B), resins (C), polymerization initiators (E), antioxidants (Fa), leveling agents (H), and solvents (J).
[0010] In this specification, unless otherwise specified, the compounds exemplified as components may be used individually or in combination of two or more. Furthermore, when using multiple types of components, unless otherwise specified, the content should be adjusted by the total amount of all components used.
[0011] <Semiconductor Particle (A)> Semiconductor particle (A) is preferably a light-emitting inorganic semiconductor particle that absorbs primary light and emits light of a different wavelength than the primary light, and more preferably the light-emitting inorganic semiconductor particle absorbs primary light and emits green or red light, and even more preferably it converts the wavelength of blue light, which is the primary light, to the wavelength of red light or the wavelength of green light.
[0012] In this specification, "blue" refers to all light that is perceived as blue (all light with intensity in the blue wavelength range, for example, 380 nm to 495 nm), and is not limited to light of a single wavelength. "Green" refers to all light that is perceived as green (all light with intensity in the green wavelength range, for example, 495 nm to 585 nm), and is not limited to light of a single wavelength. "Red" refers to all light that is perceived as red (all light with intensity in the red wavelength range, for example, 585 nm to 780 nm), and is not limited to light of a single wavelength.
[0013] Examples of semiconductor particles (A) include quantum dots and particles composed of compounds having a perovskite crystal structure (hereinafter also referred to as "perovskite compounds"), with quantum dots being preferred. Quantum dots are luminescent inorganic semiconductor nanoparticles with a particle diameter of 1 nm to 100 nm (preferably 1 nm to 50 nm, more preferably 1 nm to 30 nm), which utilize the band gap of the semiconductor to absorb ultraviolet light or visible light (e.g., blue light) and emit light.
[0014] Examples of quantum dots include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, HgS, HgSe, HgTe, CdHgTe, CdSeS, CdSeTe, CdSte, ZnSeS, ZnSeTe, ZnSte, HgSeS, HgSeTe, HgSte, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSte, CdHgSeS, CdHgSte, CdHgSte, HgZnSeS, HgZn Examples include compounds of group 12 elements and group 16 elements such as SeTe and HgZnSte; compounds of group 13 elements and group 15 elements such as GaN, GaP, GaAs, AlN, AlP, AlAs, InN, InP, InAs, GaNP, GaNAs, GaPAs, AlNP, AlNAs, AlPAs, InNP, InNAs, InPAs, GaAlNP, GaAlNAs, GaAlPAs, GaInNP, GaInNAs, GaInPAs, InAlNP, InAlNAs, InAlPAs; and compounds of group 14 elements and group 16 elements such as PdS and PbSe. Among these, quantum dots are preferably compounds of group 12 elements and group 16 elements, or compounds of group 13 elements and group 15 elements.
[0015] If the quantum dots contain sulfur (S) or senium (Se), quantum dots that have been surface-modified with metal oxides or organic materials may be used. By using surface-modified quantum dots, it is possible to prevent the extraction of S or Se by reactive components contained in or that may be contained in the curable composition.
[0016] Furthermore, the quantum dots may form a core-shell structure by combining the above-mentioned compounds. From the viewpoint of luminescence intensity, the core and shell are preferably selected from the group consisting of compounds of group 12 and group 16 elements and compounds of group 13 and group 15 elements. More preferably, the core is selected from the group consisting of compounds of group 12 and group 16 elements and compounds of group 13 and group 15 elements, and the shell is more preferably a compound of group 12 and group 16 elements. It is even more preferably that the core is selected from the group consisting of CdS, CdSe, CdTe, InN, InP, and InAs, and it is even more preferably that the shell is selected from the group consisting of ZnS, ZnSe, ZnTe, ZnSeS, ZnSeTe, and ZnSTe. Among these, examples include fine particles in which the core is CdSe and the shell is ZnS, fine particles in which the core is InP and the shell is ZnSeS, and fine particles in which the core is InP and the shells are ZnSe and ZnS.
[0017] Since the energy state of a quantum dot depends on its size, the emission wavelength can be freely selected by changing the particle size. Furthermore, because the light emitted from quantum dots has a narrow spectral width, it is advantageous for widening the color gamut of display devices. In addition, quantum dots have high responsiveness, which is advantageous in terms of primary light utilization efficiency.
[0018] Examples of perovskite compounds include those described in Japanese Patent Publication No. 2024-61630.
[0019] The curable composition may contain one or more types of semiconductor particles (A). The curable composition may contain only semiconductor particles that emit light of a specific wavelength, or it may contain two or more types of semiconductor particles that emit light of different wavelengths.
[0020] From the viewpoint of luminescence intensity, the content of semiconductor particles (A) in the curable composition is preferably 3% to 60% by mass, more preferably 10% to 55% by mass, even more preferably 20% to 50% by mass, even more preferably 20% to 45% by mass, and particularly preferably 20% to 40% by mass, based on 100% by mass of the solid content of the curable composition.
[0021] In the present specification, the total amount of solids in the curable composition means the sum of components excluding the solvent (J) among the components contained in the curable composition. The content ratio in the solids of the curable composition can be measured by a known analysis means such as liquid chromatography or gas chromatography. The content ratio of each component in the solids of the curable composition may be calculated from the formulation at the time of preparing the curable composition.
[0022] <Organic Ligand (G)> The semiconductor particles (A) preferably contain an organic ligand (G), and the semiconductor particles (A) are present in the curable composition in a state where the organic ligand (G) is coordinated (hereinafter sometimes referred to as coordinated semiconductor particles (AG)). The organic ligand (G) is, for example, an organic compound having a polar group exhibiting coordination ability to the semiconductor particles (A) and an organic group. The organic ligand (G) can coordinate to the surface of the semiconductor particles (A), for example. The curable composition may contain one or two or more kinds of organic ligands (G).
[0023] It is preferable that at least some of the molecules of the organic ligand (G) are coordinated to the semiconductor particles (A), and all or almost all of the molecules may be coordinated to the semiconductor particles (A). Including the organic ligand (G) coordinated to the semiconductor particles (A) can be advantageous from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A), as well as the emission intensity when the cured film is used as a wavelength conversion layer.
[0024] The aforementioned polar group of the organic ligand (G) is, for example, a phosphine group (-PR a 2 , R a represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms.), a phosphine oxide group (-PR b 2 O, R b represents a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms), a thiol group (-SH), a carboxy group (-COOH) and an amino group (-NH 2The group consists of at least one group selected from the group consisting of thiol groups and carboxyl groups. A polar group selected from this group may be advantageous in enhancing the coordination to the semiconductor particle (A). High coordination can contribute to improved stability and dispersibility of the semiconductor particle (A) in the curable composition, as well as improved luminescence intensity when the cured film is used as a wavelength conversion layer. In particular, from the viewpoint of increasing luminescence intensity, it is more preferable that the polar group is at least one group selected from the group consisting of thiol groups and carboxyl groups. The organic ligand (G) may have one or more polar groups.
[0025] The organic group of the organic ligand (G) is preferably a hydrocarbon group. The hydrocarbon group may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The hydrocarbon group is preferably an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, or an aromatic hydrocarbon group.
[0026] Examples of aliphatic hydrocarbon groups include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, hentriacontyl, dotriacontyl, tritriacontyl, tetratriacontyl, pentatriacontyl, hexatriacontyl, heptatriacontyl, octatriacontyl, nonatriacontyl, and tetracontyl; Isopropyl group, isobutyl group, sec-butyl group, tert-butyl group, 2-ethylbutyl group, 3,3-dimethylbutyl group, 1,1,3,3-tetramethylbutyl group, 1-methylbutyl group, 1-ethylpropyl group, 3-methylbutyl group, neopentyl group, 1,1-dimethylpropyl group, 2-methylpentyl group, 3-ethylpentyl group, 1,3-dimethylbutyl group, 2-propylpentyl group, 1-ethyl-1,2-dimethylpropyl group, 1-methylpentyl group, 4-methylpentyl group, 4-methylpentyl group Branched alkyl groups such as hexyl group, 5-methylhexyl group, 2-ethylhexyl group, 1-methylhexyl group, 1-ethylpentyl group, 1-propylbutyl group, 3-ethylheptyl group, 2,2-dimethylheptyl group, 1-methylheptyl group, 1-ethylhexyl group, 1-propylpentyl group, 1-methyloctyl group, 1-ethylheptyl group, 1-propylhexyl group, 1-butylpentyl group, 1-methylnonyl group, 1-ethyloctyl group, 1-propylheptyl group, and 1-butylhexyl group;Ethenyl group (vinyl group), propenyl group (e.g., 1-propenyl group, 2-propenyl group (allyl group)), 1-methylethenyl group, butenyl group (e.g., 1-butenyl group, 2-butenyl group, 3-butenyl group), 3-methyl-1-butenyl group, 1,3-butadienyl group, 1-(2-propenyl)ethenyl group, 1-(1-methylethenyl)ethenyl group, 1,2-dimethyl-1-propenyl group, pentenyl group (e.g., 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group), 1-(1,1-dimethylethyl)ethenyl group, 1,3-dimethyl-1-butenyl group, hexenyl group (e.g., Alkenyl groups such as 1-hexenyl group, 5-hexenyl group, heptenyl group (e.g., 1-heptenyl group, 6-heptenyl group), octenyl group (e.g., 1-octenyl group, 7-octenyl group), nonenyl group (e.g., 1-nonenyl group, 8-nonenyl group), decenyl group (e.g., 1-decenyl group, 9-decenyl group), undecenyl group, dodecenyl group, tridecenyl group, tetradecenyl group, pentadecenyl group, hexadecenyl group, heptadecenyl group, octadecenyl group, nonadecenyl group, icocenyl group, 1,1-dimethyl-2-propenyl group, 1-ethyl-2-propenyl group, and 1-methyl-1-butenyl group; Examples include ethylyl groups, propynyl groups (e.g., 1-propynyl, 2-propynyl), octinyl groups (e.g., 1-octinyl, 7-octinyl), butynyl, pentynyl, hexynyl, heptynyl, noninyl, desinyl, undecynyl, dodecynyl, tridecynyl, tetradecynyl, pentadecynyl, hexadecinyl, heptadecynyl, octadecynyl, nonadecinyl, and icosinyl groups; and other alkynyl groups.
[0027] The number of carbon atoms in the aliphatic hydrocarbon group is preferably 1 to 40, more preferably 2 to 30, and even more preferably 3 to 20.
[0028] Examples of alicyclic hydrocarbon groups include cyclopropyl group, 1-methylcyclopropyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, 1-methylcyclohexyl group, 2-methylcyclohexyl group, 3-methylcyclohexyl group, 4-methylcyclohexyl group, 1,2-dimethylcyclohexyl group, 1,3-dimethylcyclohexyl group, 1,4-dimethylcyclohexyl group, 2,3-dimethylcyclohexyl group, 2,4-dimethylcyclohexyl group, 2,5-dimethylcyclohexyl group, 2,6-dimethylcyclohexyl group, 3,4-dimethylcyclohexyl group, 3,5-dimethylcyclohexyl group, 2,2-dimethylcyclohexyl group, 3,3-dimethylcyclohexyl group, and 4,4 Examples include cycloalkyl groups such as dimethylcyclohexyl group, cyclooctyl group, 2,4,6-trimethylcyclohexyl group, 2,2,6,6-tetramethylcyclohexyl group, 3,3,5,5-tetramethylcyclohexyl group, 4-pentylcyclohexyl group, 4-octylcyclohexyl group, and 4-cyclohexylcyclohexyl group; cycloalkenyl groups such as cyclohexenyl group (e.g., cyclohexa-1-en-1-yl group, cyclohexa-2-en-1-yl group, cyclohexa-3-en-1-yl group), cycloheptenyl group, and cyclooctenyl group; saturated or unsaturated polycyclic hydrocarbon groups such as norbornyl group, norborneyl group, adamantyl group, and bicyclo[2.2.2]octyl group; and so on.
[0029] The number of carbon atoms in the alicyclic hydrocarbon group is preferably 3 to 40, more preferably 3 to 30, and even more preferably 3 to 20.
[0030] Aromatic hydrocarbon groups include phenyl group, o-tolyl group, m-tolyl group, p-tolyl group, 2-ethylphenyl group, 3-ethylphenyl group, 4-ethylphenyl group, 2,3-dimethylphenyl group, 2,4-dimethylphenyl group, 2,5-dimethylphenyl group, 2,6-dimethylphenyl group, 3,4-dimethylphenyl group, 3,5-dimethylphenyl group, 4-vinylphenyl group, o-isopropylphenyl group, m-isopropylphenyl group, p-isopropylphenyl group, o-tert-butylphenyl group, m-tert-butylphenyl group, p-tert-butylphenyl group, 3,5-di(tert-butyl)phenyl group, 3,5-di(tert-butyl)-4-methylphenyl group, and 4-butyl Aromatic hydrocarbon groups such as phenyl group, 4-pentylphenyl group, 2,6-bis(1-methylethyl)phenyl group, 2,4,6-tris(1-methylethyl)phenyl group, 4-cyclohexylphenyl group, 2,4,6-trimethylphenyl group, 4-octylphenyl group, 4-(1,1,3,3-tetramethylbutyl)phenyl group, 1-naphthyl group, 2-naphthyl group, 6-methyl-2-naphthyl group, 5,6,7,8-tetrahydro-1-naphthyl group, 5,6,7,8-tetrahydro-2-naphthyl group, fluorenyl group, phenanthryl group, anthryl group, 2-dodecylphenyl group, 3-dodecylphenyl group, 4-dodecylphenyl group, perilenyl group, chrysenyl group, and pyrenyl group; and the like.
[0031] The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 40, more preferably 6 to 30, and even more preferably 6 to 20.
[0032] The hydrocarbon group may further have hydrophilic functional groups. The hydrophilic functional groups are preferably hydroxyl groups, carboxyl groups, carbonyl groups, thiol groups, amino groups, ether bonds, ester bonds, and siloxane bonds. If the hydrocarbon group has an ether bond, the hydrocarbon group is composed of -CH 2 The - may be replaced by -O-. If the hydrocarbon group has an ester bond, the -CH constituting the hydrocarbon group 2 -CH 2 -CH 2The - may be replaced by -C(=O)-O- or -O-C(=O)-. When the hydrocarbon group has a siloxane bond, the -CH constituting the hydrocarbon group 2 -CH 2 The - may be replaced by -Si-O-. Also, the methylene group contained in the hydrocarbon group may be replaced by -S-, -C(=O)-, -C(=O)-NH-, -NH-, etc.
[0033] The organic ligand (G) preferably contains at least one selected from the group consisting of a hydrophobic organic ligand (G1) and a hydrophilic organic ligand (G2). The hydrophobic organic ligand (G1) is preferably a compound having the above-mentioned polar group and the above-mentioned hydrocarbon group (preferably a hydrocarbon group without a hydrophilic functional group). The hydrophilic organic ligand (G2) is preferably a compound having the above-mentioned polar group and a hydrocarbon group having a hydrophilic functional group. The presence of a hydrophilic functional group in the organic group enables dispersion in a polar dispersion medium. The organic ligand (G) may contain one or more hydrophobic organic ligands (G1) and hydrophilic organic ligands (G2).
[0034] A hydrophobic organic ligand (G1) is, for example, given by the following formula (x): X A -R X It is preferable that the organic compound is represented by (x). In the formula, X A R is the polar group described above, X It is preferable that the hydrocarbon group is a monovalent hydrocarbon group which may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The hydrocarbon group may have one or more unsaturated bonds, such as carbon-carbon double bonds. The hydrocarbon group may have a linear, branched, or cyclic structure. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 40, and may be 1 to 30. XIt is more preferable that the ligand is a monovalent aliphatic hydrocarbon group. The monovalent aliphatic hydrocarbon group may be the same as the aliphatic hydrocarbon group described above. In particular, the hydrocarbon group is preferably an alkyl group, alkynyl group, or alkenyl group having 1 to 40 carbon atoms (preferably 1 to 30 carbon atoms). The organic group of the hydrophobic organic ligand (G1) may also contain substituents such as halogen atoms or heteroatoms (N, O, S).
[0035] X A The polar group represented is preferably at least one group selected from the group consisting of a phosphine group, a phosphine oxide group, a thiol group, a carboxyl group, and an amino group. There may be one or more polar groups.
[0036] polar group A Specific examples of organic ligands having a carboxyl group include saturated or unsaturated fatty acids. Specific examples of saturated or unsaturated fatty acids include saturated fatty acids such as propionic acid, butyric acid, pentanoic acid, caproic acid, caprylic acid, capric acid, lauric acid, myristic acid, pentadecyl acid, palmitic acid, margaric acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid; monounsaturated fatty acids such as myristoleic acid, palmitoleic acid, oleic acid, eicosenoic acid, erucic acid, and nervonic acid; and polyunsaturated fatty acids such as linoleic acid, alpha-linolenic acid, gamma-linolenic acid, stearic acid, dihomo-gamma-linolenic acid, arachidonic acid, eicosatetraenoic acid, docosadienoic acid, and adrenaline (docosatetraenoic acid).
[0037] polar group A Specific examples of organic ligands having a thiol group or an amino group include the polar group X exemplified above. A This includes organic ligands in which the carboxyl group of an organic ligand having a carboxyl group is replaced by a thiol group or an amino group. Polar group X A Specific examples of organic ligands having a thiol group include hexanethiol, octanthiol, decanethiol, and 1-dodecanethiol. Polar group X A Examples of organic ligands having an amino group include oleylamine. Polar group X AExamples of organic ligands having a phosphine group or a phosphine oxide group include trioctylphosphine and trioctylphosphine oxide.
[0038] From the viewpoint of improving the stability and dispersibility of semiconductor particles, the molecular weight of the hydrophobic organic ligand (G1) is preferably 1500 or less, more preferably 1000 or less, and even more preferably 800 or less. The molecular weight of the hydrophobic organic ligand (G1) is usually 100 or more. That is, the molecular weight of the hydrophobic organic ligand (G1) is preferably 100 to 1500, 100 to 1000, or 100 to 800. The above molecular weight may be the number average molecular weight or the weight average molecular weight. In this case, the number average molecular weight and the weight average molecular weight are the number average molecular weight and the weight average molecular weight on a standard polystyrene basis measured by gel permeation chromatography (GPC), respectively.
[0039] Examples of hydrophilic organic ligands (G2) include compound (G2-1) and compound (G2-2).
[0040] [Compound (G2-1)] Compound (G2-1) is preferably a compound having a first functional group, a second functional group, and a divalent organic group. The first functional group is preferably a carboxyl group (-COOH) or a hydroxyl group (-OH), and the second functional group is preferably a carboxyl group or a thiol group (-SH). The first and second functional groups correspond to the hydrophilic functional group and the polar group, respectively. There may be one or more first and second functional groups. Since compound (G2-1) has a carboxyl group, a thiol group, and a hydroxyl group, it can be a ligand that coordinates to semiconductor particles (A). The curable composition may contain only one compound (G2-1) or two or more. The divalent organic group may be any hydrocarbon group that is divalent as described above.
[0041] An example of compound (G2-1) is the compound represented by the following formula (G2-1a). Compound (G2-1) may also be the acid anhydride of the compound represented by formula (G2-1a).
[0042]
[0043] [In the formula, R B R represents a divalent hydrocarbon group. B If present, they may be the same or different. The hydrocarbon group may have one or more substituents. If multiple substituents are present, they may be the same or different, and they may be bonded to each other, forming a ring with the atom to which each substituent is bonded. The hydrocarbon group contains -CH 2 - is -O-, -S-, -SO 2 It may be replaced by at least one of -, -CO-, and -NH-. p represents an integer from 1 to 10.
[0044] R B Examples of divalent hydrocarbon groups represented by this symbol include chain hydrocarbon groups, alicyclic hydrocarbon groups, aromatic hydrocarbon groups, and groups that combine these.
[0045] Examples of linear hydrocarbon groups include linear or branched alkanediyl groups, which typically have 1 to 40 carbon atoms, preferably 1 to 20, and more preferably 1 to 10. Examples of alicyclic hydrocarbon groups include monocyclic or polycyclic cycloalkanediyl groups, which typically have 3 to 40 carbon atoms, preferably 3 to 20, and more preferably 3 to 10. Examples of aromatic hydrocarbon groups include monocyclic or polycyclic arenediyl groups, which typically have 6 to 20 carbon atoms.
[0046] Examples of substituents that the hydrocarbon group may have include C1-C40 alkyl groups, C3-C40 cycloalkyl groups, C6-C20 aryl groups, carboxyl groups, amino groups, and halogen atoms. Preferably, the substituents that the hydrocarbon group may have are carboxyl groups, amino groups, or halogen atoms.
[0047] The above hydrocarbon group contains -CH 2 If - is replaced by at least one of -O-, -CO-, and -NH-, then -CH 2 The hyphen is preferably replaced by at least one of -CO- and -NH-, and more preferably by -NH-. p is preferably 1 or 2.
[0048] Examples of compounds represented by formula (G2-1a) include those represented by the following formulas (1-1) to (1-9).
[0049]
[0050] Specific examples of compounds represented by formula (G2-1a), listed by their chemical names, include, for example, mercaptoacetic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutanoic acid, 4-mercaptobutanoic acid, mercaptohexanoic acid, mercaptooctanoic acid, mercaptoundecanoic acid, mercaptosuccinic acid, mercaptostearic acid, 4-mercaptobenzoic acid, 2,3,5,6-tetrafluoro-4-mercaptobenzoic acid, L-cysteine, N-acetyl-L-cysteine, 3-methoxybutyl 3-mercaptopropionic acid, and 3-mercapto-2-methylpropionic acid. Among these, 3-mercaptopropionic acid and mercaptosuccinic acid are preferred.
[0051] Another example of compound (G2-1) is a polycarboxylic acid compound, preferably a compound (G2-1b) in which the -SH in formula (G2-1a) is replaced with a carboxyl group (-COOH).
[0052] Examples of compounds (G2-1b) include the following:
[0053] Succinic acid, glutaric acid, adipic acid, octafluoroadipic acid, azelaic acid, dodecanediic acid, tetradecanediic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanediic acid, nonadecanedioic acid, dodecafluoroseveric acid, 3-ethyl-3-methylglutaric acid, hexafluoroglutaric acid, trans-3-hexenodioic acid, sebacic acid, hexadecafluorosebacic acid, acetylenedicarboxylic acid, trans-aconitic acid, 1,3-adamantanedicarboxylic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, cis-4-silicon Chlohexene-1,2-dicarboxylic acid, 1,1-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, cis- or trans-1,3-cyclohexanedicarboxylic acid, cis- or trans-1,4-cyclohexanedicarboxylic acid, 1,1-cyclopentanediacetic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, decahydro-1,4-naphthalenedicarboxylic acid, 2,3-norbornanedicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid, phthalic acid, 3-fluorophthalic acid, isophthalic acid, tetrafluoroiso Phthalic acid, terephthalic acid, tetrafluoroterephthalic acid, 2,5-dimethylterephthalic acid, 2,6-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,1'-ferrocenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 2,5-franzicarboxylic acid, benzophenone-2,4'-dicarboxylic acid monohydrate, benzophenone-4,4'-dicarboxylic acid, 2,3-pyrazinedicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 3,5-Pyridinedicarboxylic acid, 2,5-Pyridinedicarboxylic acid, 2,6-Pyridinedicarboxylic acid, 3,4-Pyridinedicarboxylic acid, Pyrazole-3,5-dicarboxylic acid monohydrate, 4,4'-Stilbenidicarboxylic acid, Anthraquinone-2,3-dicarboxylic acid, 4-(carboxymethyl)benzoic acid, Cheridonic acid monohydrate, Azobenzene-4,4'-dicarboxylic acid, Azobenzene-3,3'-dicarboxylic acid, Chlorendic acid, 1H-Imidazole-4,5-dicarboxylic acid, 2,2-Bis(4-carboxyphenyl)hexafluoropropane, 1,10-Bis(4-carboxyphenoxy)decane, dipropylmalonic acid, dithiodiglycolic acid, 3,3'-dithiodipropionic acid, 4,4'-dithiodibutanoic acid, 4,4'-dicarboxydiphenyl ether, 4,4'-dicarboxydiphenyl sulfone, ethylene glycol bis(4-carboxyphenyl) ether, 3,4-ethylenedioxythiophene-2,5-dicarboxylic acid, 4,4'-isopropylidenediphenoxyacetic acid, 1,3-acetonedicarboxylic acid, methylenedisalicylic acid, 5,5'-thiodisalicylic acid, tris(2-carboxyethyl) isocyanurate, tetrafluorosuccinic acid, α,α,α',α'-tetramethyl-1,3-benzenedipropionic acid, 1,3,5-benzenetricarboxylic acid, etc.
[0054] From the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer, the molecular weight of compound (G2-1) is preferably 3,000 or less, more preferably 2,500 or less, even more preferably 2,000 or less, still more preferably 1,000 or less, particularly preferably 800 or less, and most preferably 500 or less. The molecular weight of compound (G2-1) is usually 100 or more. That is, the molecular weight of compound (G2-1) is preferably 100 to 3,000, 100 to 2,500, 100 to 2,000, 100 to 1,000, 100 to 800, or 100 to 500.
[0055] The above molecular weight may be either the number-average molecular weight Mn or the weight-average molecular weight Mw. In this case, Mn and Mw are standard polystyrene equivalent values measured by gel permeation chromatography (GPC).
[0056] The content ratio of compound (G2-1) to semiconductor particles (A) in the curable composition is preferably 0.001 to 1 by mass, more preferably 0.01 to 0.5, and even more preferably 0.02 to 0.45. Having this content ratio within this range is advantageous in terms of the stability and dispersibility of the semiconductor particles (A), as well as improving the luminescence intensity when the cured film is used as a wavelength conversion layer.
[0057] The content of compound (G2-1) in the curable composition is preferably 0.1% to 20% by mass, more preferably 0.2% to 20% by mass, even more preferably 0.2% to 10% by mass, even more preferably 0.5% to 10% by mass, and particularly preferably 0.5% to 8% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.
[0058] [Compound (G2-2)] Compound (G2-2) is a compound different from compound (G2-1), containing a polyalkylene glycol structure and having polar groups at its molecular ends. Preferably, the molecular end is the end of the longest carbon chain in compound (G2-2) (the carbon atoms in the carbon chain may be replaced by other atoms such as oxygen atoms).
[0059] The semiconductor particle (A) may contain only one compound (G2-2) or two or more compounds. The semiconductor particle (A) may contain compound (G2-1) or compound (G2-2), or may contain compound (G2-1) and compound (G2-2).
[0060] Compounds containing a polyalkylene glycol structure and having the above-mentioned first functional group, second functional group, and divalent organic group shall be classified as compound (G2-1).
[0061] The structure of polyalkylene glycol is as follows:
[0062]
[0063] This refers to a structure represented by (n is an integer greater than or equal to 2). In the formula, R C This is an alkylene group, such as an ethylene group or a propylene group.
[0064] A specific example of compound (G2-2) is a polyalkylene glycol compound represented by the following formula (G2-2a).
[0065]
[0066] In formula (G2-2a), X is a polar group, Y is a monovalent group, and Z C R is a divalent or trivalent base. n is an integer greater than or equal to 2. m is 1 or 2. C This is an alkylene group.
[0067] Polar group X is a phosphine group (-PR a 2 , R a ) represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms (preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms). ), phosphine oxide group (-PR b 2 O, R b (wherein represents a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms), a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH 2 It is preferable that the polar group X is at least one group selected from the group consisting of thiol groups and carboxyl groups. A polar group selected from this group may be advantageous in improving coordination to semiconductor particles (A). In particular, from the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer, it is more preferable that the polar group X is at least one group selected from the group consisting of thiol groups and carboxyl groups, and even more preferable that it is a thiol group.
[0068] Group Y is a monovalent organic group. Group Y is not particularly limited and may include monovalent hydrocarbon groups that have substituents (such as N, O, S, halogen atoms, etc.). The hydrocarbon group contains -CH 2 The hyphen may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. The number of carbon atoms in the hydrocarbon group is, for example, 1 to 12. The hydrocarbon group may have an unsaturated bond.
[0069] Examples of group Y include alkyl groups having 1 to 12 carbon atoms and having a linear, branched, or cyclic structure; and alkoxy groups having 1 to 12 carbon atoms and having a linear, branched, or cyclic structure. The number of carbon atoms in the alkyl and alkoxy groups is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 4. The alkyl and alkoxy groups contain -CH 2 The - may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. In particular, group Y is preferably a linear or branched alkoxy group having 1 to 4 carbon atoms, and more preferably a linear alkoxy group having 1 to 4 carbon atoms.
[0070] Group Y may contain a polar group. The polar group may be a phosphine group (-PR a 2 , R a ) represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms (preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms). ), phosphine oxide group (-PR b 2 O, R b (wherein represents a hydrocarbon group having 1 to 10 carbon atoms, preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms), a thiol group (-SH), a carboxyl group (-COOH), and an amino group (-NH 2 A maximum of one group selected from the group consisting of ) is mentioned. However, as described above, compounds containing a polyalkylene glycol structure and having the first and second functional groups are considered to belong to compound (G2-2). The polar group is preferably located at the terminal end of group Y.
[0071] Base Z C It is a divalent or trivalent group. Group Z C Examples include divalent or trivalent hydrocarbon groups, which are not particularly limited and may contain heteroatoms (such as N, O, S, halogen atoms, etc.). The number of carbon atoms in the hydrocarbon group is, for example, 1 to 24. The hydrocarbon group may have unsaturated bonds.
[0072] The divalent group Z CExamples include alkylene groups having a linear, branched, or cyclic structure with 1 to 24 carbon atoms; and alkenylene groups having a linear, branched, or cyclic structure with 1 to 24 carbon atoms. The number of carbon atoms in the alkyl and alkenylene groups is preferably 1 to 12, more preferably 1 to 8, and even more preferably 1 to 4. The alkyl and alkenylene groups contain -CH 2 The hyphen may be substituted with -O-, -S-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -C(=O)-NH-, -NH-, etc. The trivalent group Z C An example of this is the divalent group Z mentioned above. C We can give an example of a group obtained by removing one hydrogen atom from the same group.
[0073] Base Z C The group Z may have a branched structure. C In a branch chain separate from the branch chain containing the polyalkylene glycol structure shown in formula (G2-2a) above, the branch chain may have a polyalkylene glycol structure separate from the polyalkylene glycol structure shown in formula (G2-2a) above.
[0074] In particular, Base Z C It is preferably a linear or branched alkylene group having 1 to 6 carbon atoms, and more preferably a linear alkylene group having 1 to 4 carbon atoms.
[0075] R C The group is an alkylene group, preferably a linear or branched alkylene group having 1 to 6 carbon atoms, and more preferably a linear alkylene group having 1 to 4 carbon atoms.
[0076] In formula (G2-2a), n is an integer of 2 or more, preferably 2 to 540, more preferably 2 to 120, even more preferably 2 to 60, even more preferably 2 to 30, even more preferably 2 to 15, and particularly preferably 2 to 10.
[0077] Specific examples of compound (G2-2) include, but are not limited to, HS-PEG-COOH, PEG-SH, polyethylene glycol monomethyl ether thiol, polypropylene glycol monomethyl ether thiol, 3-mercaptopropionic acid-PEG ester, and preferably polyethylene glycol monomethyl ether thiol and polypropylene glycol monomethyl ether thiol, and more preferably HS-(CH2CH2O) k It is a compound represented as -CH3 (where k is an integer between 2 and 10).
[0078] The molecular weight of compound (G2-2) may be, for example, 150 to 10,000, but from the viewpoint of improving the stability and dispersibility of semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer, it is preferably 150 to 5,000, more preferably 150 to 4,000, even more preferably 150 to 1,500, even more preferably 150 to 1,000, and particularly preferably 150 to 800. The molecular weight may be a number-average molecular weight or a weight-average molecular weight. In this case, the number-average molecular weight and the weight-average molecular weight are standard polystyrene equivalent values measured by GPC.
[0079] The content ratio of compound (G2-2) to semiconductor particles (A) in the curable composition is preferably 0.001 to 2 by mass, more preferably 0.01 to 1.5, and even more preferably 0.1 to 1. Having this content ratio within this range is advantageous in terms of the stability and dispersibility of the semiconductor particles (A), as well as improving the luminescence intensity when the cured film is used as a wavelength conversion layer.
[0080] The content of compound (G2-2) in the curable composition is preferably 0.1% to 40% by mass, more preferably 0.1% to 20% by mass, even more preferably 1% to 15% by mass, and still more preferably 2% to 12% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.
[0081] To improve the dispersion of semiconductor particles (A) and thus enhance luminescence intensity, the composition ratio of hydrophilic organic ligands (G2) is preferably 60% or more, more preferably 62% or more, even more preferably 65% or more, even more preferably 80% or more, and 85% or more, relative to all organic ligands (G) coordinating to the semiconductor particles. Furthermore, the composition ratio is preferably 95% or less, and more preferably 90% or less. That is, the composition ratio of hydrophilic organic ligands (G2) is preferably 60-95%, 62-95%, 65-90%, 80-90%, or 85-90%. The composition ratio of hydrophilic organic ligands (G2) relative to all organic ligands (G) coordinating to the semiconductor particles (A) can be determined from {T0 / (T0+T1)} × 100 (T0 and T1 are the same as above). Specifically, it can be determined by the method described in the examples.
[0082] The semiconductor particle (A) preferably contains a hydrophobic organic ligand (G1) and a hydrophilic organic ligand (G2) as an organic ligand (G), more preferably contains a compound represented by formula (x) and a polyalkylene glycol compound represented by formula (G2-2a), and even more preferably contains oleic acid, 1-dodecanethiol, trioctylphosphine and triethylene glycol monomethyl etherthiol.
[0083] The ratio of the content of organic ligands (G) to semiconductor particles (A) in the curable composition is preferably 0.001 or more and 1 or less by mass, more preferably 0.01 or more and 0.8 or less, and even more preferably 0.02 or more and 0.5 or less. Having this content ratio within this range can be advantageous in terms of the stability and dispersibility of the semiconductor particles (A), and in improving the luminescence intensity when the cured film is used as a wavelength conversion layer. The content of organic ligands (G) as used herein refers to the total content of all organic ligands contained in the curable composition.
[0084] When semiconductor particles (A) or coordination semiconductor particles (AG) containing an organic ligand (G) are heated from 25°C to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min by thermogravimetric analysis, the weight loss ratio X above 300°C, as determined by formula (1), is 35% or less. By using such semiconductor particles (A) and a polymerizable compound (D) with a clogP of 3.5 or higher, as described later, the decrease in luminescence intensity before and after exposure in the manufacturing process of a cured film using a curable composition can be suppressed. The weight loss ratio X above 300°C of semiconductor particles (A) or coordination semiconductor particles (AG) containing an organic ligand (G) is preferably more than 0% and 35% or less, more preferably 1% or more and 35% or less, even more preferably 1% or more and 30% or less, even more preferably 3% or more and 20% or less, and even more preferably 5% or more and 14% or less. The reason why the curable composition of this disclosure provides the above effects is not necessarily clear, but the inventors speculate as follows. In other words, when the weight loss ratio X of semiconductor particles (A) or coordination semiconductor particles (AG) containing organic ligands (G) above 300°C is within the aforementioned range, the balance between hydrophobicity and hydrophilicity is appropriately controlled. This allows the semiconductor particles (A) to be well dispersed even during exposure. Furthermore, when clogP is within the aforementioned range, the polymerizable compound (D) has a high affinity for semiconductor particles (A) or coordination semiconductor particles (AG) containing organic ligands (G), resulting in good solubility and dispersibility. This appropriately maintains the polymerization reaction rate and makes it easier to disperse the semiconductor particles (A). As a result, aggregation of semiconductor particles (A) is suppressed even in the cured film after exposure, and the decrease in luminescence intensity can be suppressed. Weight loss ratio X above 300°C (%) = {T1 / (T 0+T1)}×100...(1) [In formula (1), T 0 This is the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight, and T 1 This is the weight loss rate between 300°C and 600°C, relative to the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C. In other words, the weight loss ratio above 300°C represents the proportion of the hydrophobic organic ligand (G1) to all the organic ligands (G) coordinating to the semiconductor particle (A).
[0085] The weight loss ratio of semiconductor particles (A) or coordination-type semiconductor particles (AG) containing an organic ligand (G) at temperatures above 300°C can be adjusted, for example, in a semiconductor particle preparation method in which semiconductor particles are mixed with an organic ligand described later, and then the semiconductor particles are washed one or more times, by adjusting the type, number, and amount of organic ligand (G), or by adjusting the type and amount of solvent, washing temperature, and washing time in the washing process.
[0086] The content of semiconductor particles (A) containing an organic ligand (G) in the curable composition is preferably 10% to 75% by mass, more preferably 12% to 70% by mass, and even more preferably 25% to 60% by mass, relative to the total amount of solids in the curable composition, from the viewpoint of improving the stability and dispersibility of the semiconductor particles (A) and the luminescence intensity when the cured film is used as a wavelength conversion layer.
[0087] <Polymerizable Compound (D)> Polymerizable compound (D) is a compound that can be polymerized by active radicals, acids, etc., generated from the polymerization initiator (E) described later. The logP of polymerizable compound (D) is 3.5 or higher. A high logP results in an appropriate polymerization reaction rate for polymerizable compound (D), which makes it easier for semiconductor particles (A) to maintain dispersion during exposure, thereby suppressing the decrease in luminescence intensity before and after exposure. The logP is obtained by dividing the chemical structure into substructures (fragments) and estimating the logP value of the compound by summing the logP contributions assigned to each fragment. For example, Daylight Chemical Information System, Inc. The calculations are performed using programs such as "CLOGP," MOLINSPIRATION CHEMINFORMATICS (http: / / www.molinspiration.com), or ChemDraw 22.0 (manufactured by Cambridge Soft), which are available from [source].
[0088] Furthermore, when using two or more polymerizable compounds (D), the clogP of polymerizable compounds (D) shall be a weighted average value calculated based on the mass-based content ratio.
[0089] The clogP of polymerizable compound (D) is preferably 3.5 to 10.0, more preferably 3.8 to 8.0, even more preferably 3.8 to 7.0, even more preferably 3.8 to 6.0, and most preferably 3.8 to 5.0 or less. When the clogP of polymerizable compound (D) is within the above range, the dispersibility of semiconductor particles (A) or coordination semiconductor particles (AG) containing the organic ligand (G) is good, and the decrease in luminescence intensity before and after exposure in the manufacturing process of a cured film using the curable composition can be suppressed.
[0090] Furthermore, the molecular weight or weight-average molecular weight Mw of the polymerizable compound (D) having a clogP of 3.5 or higher is preferably 250 to 1000, more preferably 350 to 900, and even more preferably 450 to 850. Note that the weight-average molecular weight Mw should be used only when the polymerizable compound (D) is a mixed component and it is difficult to calculate the molecular weight.
[0091] Polymerizable compounds (D) having a clogP of 3.5 or higher include polymerizable compounds having one or more groups with ethylenically unsaturated bonds in the molecule (hereinafter sometimes referred to as ethylenically unsaturated groups), where the number of ethylenically unsaturated groups is preferably 2 to 10, more preferably 2 to 8, and even more preferably 2 to 6.
[0092] The ethylenically unsaturated group may be, for example, a vinyl group, a (meth)acryloyl group, or other groups that constitute an α-olefin, or a hydrocarbon group in which carbon atoms are bonded to both carbon atoms of a double bond. However, groups that constitute an α-olefin are preferred, (meth)acryloyl groups are more preferred, and acryloyl groups are even more preferred.
[0093] When the molecule contains two or more ethylenically unsaturated groups, it is preferable that the compound is one in which two or more ethylenically unsaturated groups are bonded to a single linking group. For example, when the ethylenically unsaturated group is a (meth)acryloyl group, a compound can be given in which two or more (meth)acrylic acid groups are bonded to a polyhydric alcohol by an ester bond, or a compound in which two or more (meth)acrylic acid groups are bonded to a polyhydric alcohol via a polyoxyalkylene glycol. The (meth)acryloyl group is preferably an acryloyl group.
[0094] The polyhydric alcohol may be an aliphatic polyhydric alcohol or an aromatic polyhydric alcohol. Examples of aliphatic polyhydric alcohols include trivalent or higher aliphatic alcohols such as pentaerythritol, dipentaerythritol, tripentaerythritol, and tetrapentaerythritol, with dipentaerythritol being preferred. The aliphatic polyhydric alcohol is preferably 3 to 10 valency, more preferably 4 to 8 valency, and even more preferably 5 to 6 valency. Examples of aromatic polyhydric alcohols include polyhydric alcohols having an aromatic ring, such as bisphenols such as bisphenol A, B, C, S, and F, and compounds having a cardi structure such as 4,4'-(9H-fluorene-9,9-diyl)diphenol, with bisphenol A or 4,4'-(9H-fluorene-9,9-diyl)diphenol being preferred. The aromatic polyhydric alcohol is preferably 2 to 6 valency, more preferably 2 to 4 valency, and even more preferably 2 valency.
[0095] The number of repeating oxyalkylene groups in polyoxyalkylene glycol is, for example, 1 to 6, preferably 1 to 4, and more preferably 1 to 2. Examples of polyoxyalkylene glycols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol. Polyoxyalkylene glycol forms ester bonds with (meth)acrylic acid and ether bonds with polyhydric alcohols. When two or more (meth)acrylic acid molecules are bonded to a polyhydric alcohol via polyoxyalkylene glycol, the polyoxyalkylene glycol may be different depending on the (meth)acrylic acid, or it may be the same, but it is preferable that it be the same.
[0096] The number of ethylenically unsaturated groups may be the same as the number of hydroxyl groups in the polyhydric alcohol, or it may be one or two fewer than the number of hydroxyl groups.
[0097] Examples of polymerizable compounds (D) with a clogP of 3.5 or higher include pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, tetrapentaerythritol nona(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, and propoxylated bisphenol Examples include di(meth)acrylate of bisphenol A, di(meth)acrylate of ethoxylated bisphenol F, di(meth)acrylate of propoxylated bisphenol F, di(meth)acrylate of ethoxylated bisphenol fluorene, and di(meth)acrylate of propoxylated bisphenol fluorene, among which dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, di(meth)acrylate of ethoxylated bisphenol A, and di(meth)acrylate of ethoxylated bisphenol F are preferred.
[0098] The content of polymerizable compound (D) in the curable composition (total amount if multiple types are included) is preferably 3% to 80% by mass, more preferably 4% to 70% by mass, even more preferably 5% to 25% by mass, or 6% to 20% by mass, based on 100% by mass of the total solid content of the curable composition. Process resistance can be improved when the content of polymerizable compound (D) is within the above range. It is also preferable that the curable composition contains resin (C) when the content of polymerizable compound (D) is 5% to 25% by mass, or 6% to 20% by mass, based on 100% by mass of the total solid content of the curable composition.
[0099] In particular, from the viewpoint of process tolerance, it is preferable that the weight loss ratio X at 300°C or higher for the semiconductor particle (A) containing the organic ligand (G) is 5 to 25%, and the clogP of the polymerizable compound (D) is 3.8 to 7.0; more preferably that the weight loss ratio X at 300°C or higher for the semiconductor particle (A) containing the organic ligand (G) is 8 to 20%, and the clogP of the polymerizable compound (D) is 3.8 to 6.0; and even more preferably that the weight loss ratio X at 300°C or higher for the semiconductor particle (A) containing the organic ligand (G) is 13 to 20%, and the clogP of the polymerizable compound (D) is 3.8 to 5.0.
[0100] <Resin (C)> Resin (C) is preferably an alkali-soluble resin. Resin (C) is preferably having at least one structural unit selected from the group consisting of at least one selected from the group consisting of unsaturated carboxylic acids and unsaturated carboxylic acid anhydrides (hereinafter also referred to as "(a)"), a structural unit selected from the group consisting of a monomer (b) having a cyclic ether structure with 2 to 4 carbon atoms and an ethylenically unsaturated bond (hereinafter also referred to as "(b)"), and a structural unit selected from the group consisting of a monomer (c) copolymerizable with (a) (however different from (a) and (b)) (hereinafter also referred to as "(c)"). Resin (C) may have an ethylenically unsaturated bond and may have a carboxyl group.
[0101] Examples of resin (C) include the following resin [K6]. Examples of other resins include the compounds described in Japanese Patent Application Publication No. 2024-61630.
[0102] Resin [K6]: A copolymer having a structural unit derived from (b) to which (a) is added, and a structural unit to which a carboxylic acid anhydride is further ester-bonded, and a structural unit derived from (c).
[0103] (a) includes, for example, unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, o-, m-, p-vinylbenzoic acid; and unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, itaconic acid, 3-vinylphthalic acid, 4-vinylphthalic acid, 3,4,5,6-tetrahydrophthalic acid, 1,2,3,6-tetrahydrophthalic acid, dimethyltetrahydrophthalic acid, and 1,4-cyclohexenedicarboxylic acid; Bicyclounsaturated compounds containing carboxyl groups, such as methyl-5-norbornene-2,3-dicarboxylic acid, 5-carboxybicyclo[2.2.1]hept-2-ene, 5,6-dicarboxybicyclo[2.2.1]hept-2-ene, 5-carboxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-carboxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-carboxy-6-methylbicyclo[2.2.1]hept-2-ene, and 5-carboxy-6-ethylbicyclo[2.2.1]hept-2-ene; Examples include unsaturated dicarboxylic acid anhydrides such as maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, and 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride; unsaturated mono[(meth)acryloyloxyalkyl] esters of divalent or higher polycarboxylic acids such as succinate mono[2-(meth)acryloyloxyethyl] and phthalate mono[2-(meth)acryloyloxyethyl]; and unsaturated (meth)acrylates containing both a hydroxyl group and a carboxyl group in the same molecule, such as α-(hydroxymethyl)(meth)acrylic acid.
[0104] Of these, (meth)acrylic acid, mono[2-(meth)acryloyloxyethyl] succinate, maleic anhydride, etc. are preferred from the viewpoint of copolymerization reactivity, etc.
[0105] In this specification, (meth)acrylic acid means acrylic acid and / or methacrylic acid. The same applies to "(meth)acryloyl," "(meth)acrylate," etc.
[0106] (b) is a monomer having, for example, a cyclic ether structure with 2 to 4 carbon atoms (for example, at least one selected from the group consisting of an oxirane ring, an oxetane ring, and a tetrahydrofuran ring) and an ethylenically unsaturated bond. Preferably, (b) is a monomer having a cyclic ether structure with 2 to 4 carbon atoms and a (meth)acryloyloxy group.
[0107] Examples of (b) include monomers having an oxyranyl group and an ethylenically unsaturated bond (b1) (hereinafter sometimes referred to as "(b1)"), monomers having an oxetanyl group and an ethylenically unsaturated bond (b2) (hereinafter sometimes referred to as "(b2)"), monomers having a tetrahydrofuryl group and an ethylenically unsaturated bond (b3) (hereinafter sometimes referred to as "(b3)"), and so on.
[0108] Examples of (b1) include monomers having a linear or branched aliphatic unsaturated hydrocarbon structure that has been epoxidized (b1-1) (hereinafter sometimes referred to as "(b1-1)") and monomers having a cyclic unsaturated hydrocarbon structure that has been epoxidized (b1-2) (hereinafter sometimes referred to as "(b1-2)").
[0109] (b1-1) includes, for example, glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, β-ethylglycidyl (meth)acrylate, glycidyl vinyl ether, o-vinylbenzylglycidyl ether, m-vinylbenzylglycidyl ether, p-vinylbenzylglycidyl ether, α-methyl-o-vinylbenzylglycidyl ether, α-methyl-m-vinylbenzylglycidyl ether, α-methyl-p-vinylbenzylglycidyl ether, 2,3-bis(glycidyl Examples include (zyloxymethyl)styrene, 2,4-bis(glycidyloxymethyl)styrene, 2,5-bis(glycidyloxymethyl)styrene, 2,6-bis(glycidyloxymethyl)styrene, 2,3,4-tris(glycidyloxymethyl)styrene, 2,3,5-tris(glycidyloxymethyl)styrene, 2,3,6-tris(glycidyloxymethyl)styrene, 3,4,5-tris(glycidyloxymethyl)styrene, and 2,4,6-tris(glycidyloxymethyl)styrene.
[0110] Examples of (b1-2) include vinylcyclohexene monooxide, 1,2-epoxy-4-vinylcyclohexane (e.g., Celoxide 2000; manufactured by Daicel Corporation), 3,4-epoxycyclohexylmethyl (meth)acrylate (e.g., Cyclomer A400; manufactured by Daicel Corporation), 3,4-epoxycyclohexylmethyl (meth)acrylate (e.g., Cyclomer M100; manufactured by Daicel Corporation), compounds represented by formula (BI), and compounds represented by formula (BII).
[0111]
[0112] [In formulas (BI) and (BII), R e and R f X represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and the hydrogen atom contained in the alkyl group may be substituted with a hydroxyl group. e and X f This is a single bond, *-R g -, *-R g -O-, *-R g -S- or *-R g Represents -NH-. g * represents an alkanediyl group with 1 to 6 carbon atoms. * represents a bond with oxygen.
[0113] Examples of alkyl groups having 1 to 4 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, sec-butyl group, and tert-butyl group. Examples of alkyl groups in which hydrogen atoms are substituted with hydroxyl include hydroxymethyl group, 1-hydroxyethyl group, 2-hydroxyethyl group, 1-hydroxypropyl group, 2-hydroxypropyl group, 3-hydroxypropyl group, 1-hydroxy-1-methylethyl group, 2-hydroxy-1-methylethyl group, 1-hydroxybutyl group, 2-hydroxybutyl group, 3-hydroxybutyl group, and 4-hydroxybutyl group. e and R fPreferably, the group is a hydrogen atom, a methyl group, a hydroxymethyl group, a 1-hydroxyethyl group, or a 2-hydroxyethyl group, and more preferably, a hydrogen atom or a methyl group.
[0114] Examples of alkanediyl groups include methylene, ethylene, propane-1,2-diyl, propane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, and hexane-1,6-diyl groups. e and X f Preferably, the components are a single bond, a methylene group, an ethylene group, and *-CH 2 -O- and *-CH 2 CH 2 -O- is a possible example, more preferably a single bond, *-CH 2 CH 2 -O- is one example (* represents a bonding with O).
[0115] Compounds represented by formula (BI) include compounds represented by any of formulas (BI-1) to (BI-15). Among these, compounds represented by formulas (BI-1), (BI-3), (BII-5), (BI-7), (BI-9), or (BI-11) to (BI-15) are preferred, and compounds represented by formulas (BI-1), (BI-7), (BI-9), or (BI-15) are more preferred.
[0116]
[0117] Compounds represented by formula (BII) include compounds represented by any of formulas (BII-1) to (BII-15). Among these, compounds represented by formulas (BII-1), (BII-3), (BII-5), (BII-7), (BII-9), or (BII-11) to (BII-15) are preferred, and compounds represented by formulas (BII-1), (BII-7), (BII-9), or (BII-15) are more preferred.
[0118]
[0119] The compound represented by formula (BI) and the compound represented by formula (BII) may be used individually or in combination of two or more. When the compound represented by formula (BI) and the compound represented by formula (BII) are used in combination, their content ratio [compound represented by formula (BI):compound represented by formula (BII)] is preferably 5:95 to 95:5, more preferably 20:80 to 80:20, on a molar basis.
[0120] For (b2), monomers having an oxetanyl group and a (meth)acryloyloxy group are more preferred. Examples of (b2) include 3-methyl-3-methacryloyloxymethyl oxetane, 3-methyl-3-acryloyloxymethyl oxetane, 3-ethyl-3-methacryloyloxymethyl oxetane, 3-methyl-3-methacryloyloxyethyl oxetane, 3-methyl-3-acryloyloxyethyl oxetane, 3-ethyl-3-methacryloyloxyethyl oxetane, and 3-ethyl-3-acryloyloxyethyl oxetane.
[0121] For (b3), monomers having a tetrahydrofurfuryl group and a (meth)acryloyloxy group are more preferred. Specifically for (b3), examples include tetrahydrofurfuryl acrylate (e.g., Viscoat V#150, manufactured by Osaka Organic Chemical Industry Co., Ltd.) and tetrahydrofurfuryl methacrylate.
[0122] (b) is preferable because it allows for higher reliability in terms of chemical resistance, etc.
[0123] Because the resin [K6] has high reactivity during production and unreacted (b) is less likely to remain, a monomer having an oxirane ring and an ethylenically unsaturated bond is preferred for (b).
[0124] (c) For example, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, tricyclo[5.2.1.0 2,6 ] Decane-8-yl (meth)acrylate (in the relevant technical field, it is commonly called "dicyclopentanyl (meth)acrylate". It is also sometimes called "tricyclodecyl (meth)acrylate"), tricyclo[5.2.1.0 2,6(Meth)acrylic acid esters such as decen-8-yl (meth)acrylate (commonly known as "dicyclopentenyl (meth)acrylate" in the relevant technical field), dicyclopentanyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, allyl (meth)acrylate, propargyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, and benzyl (meth)acrylate; hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; dicarboxylic acid diesters such as diethyl maleate, diethyl fumarate, and diethyl itaconate;Bicyclo[2.2.1]hept-2-ene, 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxybicyclo[2.2.1]hept-2-ene, 5-hydroxymethylbicyclo[2.2.1]hept-2-ene, 5-(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5-methoxybi Cyclo[2.2.1]hept-2-ene, 5-ethoxybicyclo[2.2.1]hept-2-ene, 5,6-dihydroxybicyclo[2.2.1]hept-2-ene, 5,6-di(hydroxymethyl)bicyclo[2.2.1]hept-2-ene, 5,6-di(2'-hydroxyethyl)bicyclo[2.2.1]hept-2-ene, 5,6-dimethoxybicyclo[2.2.1]hept-2-ene To-2-ene, 5,6-diethoxybicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-methylbicyclo[2.2.1]hept-2-ene, 5-hydroxy-5-ethylbicyclo[2.2.1]hept-2-ene, 5-hydroxymethyl-5-methylbicyclo[2.2.1]hept-2-ene, 5-tert-butoxycarbonylbicyclo[2.2.1]hept-2 Bicyclounsaturated compounds such as -ene, 5-cyclohexyloxycarbonylbicyclo[2.2.1]hept-2-ene, 5-phenoxycarbonylbicyclo[2.2.1]hept-2-ene, 5,6-bis(tert-butoxycarbonyl)bicyclo[2.2.1]hept-2-ene, 5,6-bis(cyclohexyloxycarbonyl)bicyclo[2.2.1]hept-2-ene; dicarbonylimide derivatives such as N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, N-succinimidyl-3-maleimide benzoate, N-succinimidyl-4-maleimide butyrate, N-succinimidyl-6-maleimide caproate, N-succinimidyl-3-maleimide propionate, and N-(9-acridinyl)maleimide;Examples include styrene, α-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, p-methoxystyrene, acrylonitrile, methacrylonitrile, vinyl chloride, vinylidene chloride, acrylamide, methacrylamide, vinyl acetate, 1,3-butadiene isoprene, 2,3-dimethyl-1,3-butadiene, etc.
[0125] Of the above, methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, styrene, vinyltoluene, N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, bicyclo[2.2.1]hept-2-ene, etc. are preferred from the viewpoint of copolymerization reactivity.
[0126] Resin [K6] is a resin obtained by reacting a cyclic ether derived from (b) in a copolymer of (b) and (c) with a carboxylic acid or carboxylic acid anhydride from (a), and then reacting it with a carboxylic acid anhydride. The hydroxyl group generated by the reaction of the cyclic ether with the carboxylic acid or carboxylic acid anhydride is reacted with the carboxylic acid anhydride.
[0127] The ratio of structural units derived from (b) and (c) is preferably such that, with respect to the total number of moles of all structural units constituting the copolymer, the ratio of structural units derived from (b) is 5 mol% to 95 mol%, and the ratio of structural units derived from (c) is 5 mol% to 95 mol%, and it is more preferably such that the ratio of structural units derived from (b) is 10 mol% to 90 mol%, and the ratio of structural units derived from (c) is 10 mol% to 90 mol%.
[0128] The amount of (a) used to react with the copolymer is preferably 5 moles to 120 moles, and more preferably 20 moles to 110 moles, per 100 moles of (b).
[0129] Examples of carboxylic acid anhydrides include succinic anhydride, maleic anhydride, citraconic anhydride, itaconic anhydride, 3-vinylphthalic anhydride, 4-vinylphthalic anhydride, 3,4,5,6-tetrahydrophthalic anhydride, 1,2,3,6-tetrahydrophthalic anhydride, dimethyltetrahydrophthalic anhydride, and 5,6-dicarboxybicyclo[2.2.1]hept-2-ene anhydride.
[0130] The amount of carboxylic acid anhydride used is preferably 0.1 to 1 mole, more preferably 0.2 to 1 mole, and even more preferably 0.3 to 1 mole, per 1 mole of the amount of (a) used.
[0131] Examples of resins [K6] include resins obtained by adding (meth)acrylic acid to a tricyclodecyl (meth)acrylate / glycidyl (meth)acrylate copolymer and further esterifying it with tetrahydrophthalic anhydride or succinic anhydride, and resins obtained by adding (meth)acrylic acid to a dicyclopentanyl (meth)acrylate / 2-ethylhexyl (meth)acrylate / glycidyl (meth)acrylate copolymer and further esterifying it with tetrahydrophthalic anhydride or succinic anhydride. Other resins may be used, for example, the resins described in Japanese Patent Application Publication No. 2024-61630 and Japanese Patent Application Publication No. 2018-123274.
[0132] The resin (C) has a standard polystyrene equivalent Mw measured by GPC, for example, 1,000 to 100,000, preferably 2,000 to 50,000, more preferably 3,000 to 20,000, and even more preferably 5,000 to 8,000, from the viewpoint of developability and luminescence intensity of the curable composition. The Mw of resin (C) can be adjusted by appropriately combining reaction conditions such as the selection of raw materials used, the preparation method, the reaction temperature and time. The Mw of resin (C) can be measured according to the measurement method described in the Examples section below. Alternatively, the Mw of resin (C) contained in the curable composition may be measured using GPC.
[0133] The acid value of resin (C) is preferably 1 mg KOH / g or more and 150 mg KOH / g or less, more preferably 20 mg KOH / g or more and 110 mg KOH / g or less, and even more preferably 30 mg KOH / g or more and 80 mg KOH / g or less, from the viewpoint of the developability and solvent resistance of the curable composition. The acid value of resin (C) can be adjusted by the content of monomer components having acid groups and the content of carboxylic acid anhydrides.
[0134] The acid value of resin (C) is measured as the amount of potassium hydroxide (mg) required to neutralize 1 g of resin (C), and can be determined, for example, by titration using an aqueous potassium hydroxide solution. Specifically, it can be measured according to the measurement method described in the Examples section below. Alternatively, the acid value of resin (C) contained in the composition may be determined, for example, by performing a structural analysis of it.
[0135] Resin (C) preferably contains a resin with a double bond equivalent of 1500 g / eq or less, more preferably a resin with a double bond equivalent of 1000 g / eq or less, even more preferably a resin with a double bond equivalent of 500 g / eq or less, and even more preferably a resin with a double bond equivalent of 450 g / eq or less. In the preferred embodiment, the lower limit of the double bond equivalent of these resins may be 200 g / eq. That is, the double bond equivalent of resin (C) is preferably 200 to 1500 g / eq, 200 to 1000 g / eq, 200 to 500 g / eq, or 200 to 450 g / eq. Examples of resins having the above-mentioned double bond equivalent include (meth)acrylic resins. Resin (C) preferably consists of a (meth)acrylic resin.
[0136] The resin (C) content in the curable composition is, for example, 5% by mass or more and 80% by mass or less, preferably 10% by mass or more and 70% by mass or less, more preferably 13% by mass or more and 60% by mass or less, and even more preferably 17% by mass or more and 55% by mass or less, based on the total amount of solids in the curable composition.
[0137] The mass ratio of the resin (C) to the semiconductor particles (A) containing the organic ligand (G), i.e., C / (A+G), is preferably 0.1 or more and less than 3, more preferably 0.3 or more and 2 or less, and even more preferably 0.3 or more and 1 or less, from the viewpoint of developability.
[0138] <Light Scattering Agent (B)> Examples of the light scattering agent (B) include inorganic particles such as metal or metal oxide particles and glass particles. Examples of the metal oxide include TiO 2 , SiO 2 , BaTiO 3 , ZnO and the like. From the viewpoint of efficiently scattering light and increasing emission intensity, the particles are preferably TiO 2 particles. The particle diameter of the light scattering agent (B) is, for example, about 0.03 μm to 20 μm, preferably 0.05 μm to 1 μm, more preferably 0.05 μm to 0.5 μm.
[0139] As the light scattering agent (B), a product obtained by previously dispersing the light scattering agent in part or all of the solvent (J) using the dispersant (I) may be used. Examples of the dispersant (I) include the compounds described in JP 2024-61630 A.
[0140] The content of the light scattering agent (B) in the curable composition is, for example, 0.001 mass% to 50 mass% relative to the total solid content of the curable composition. From the viewpoint of improving the light scattering performance and emission intensity when the cured film is used as a wavelength conversion layer, the content is preferably 1 mass% to 40 mass%, more preferably 2 mass% to 30 mass%, still more preferably 5 mass% to 30 mass%, and even more preferably 5 mass% to 15 mass%.
[0141] <Polymerization Initiator (E)> The polymerization initiator (E) is a compound capable of generating active radicals, acids and the like under the action of light or heat to initiate the polymerization of the polymerizable compound (D). The curable composition may contain one or more polymerization initiators (E).
[0142] The polymerization initiator (E) preferably contains an oxime compound.
[0143] Including an oxime compound as a polymerization initiator (E) can be advantageous from the viewpoint of improving luminescence intensity. One reason for this effect is presumed to be that, due to the unique molecular structure of the oxime compound, the absorption wavelength of the oxime compound changes significantly before and after cleavage (decomposition) of the oxime compound, which is necessary for the oxime compound to initiate photopolymerization. Therefore, oxime compounds have a high photoradical polymerization initiation ability.
[0144] Examples of oxime compounds include those having a substructure represented by the following formula (da1) or formula (da2). * and ** represent bonding sites.
[0145]
[0146] The oxime compound preferably has at least one substructure selected from those represented by the following formulas (d-1) to (d-4). If the oxime compound has these substructures, a curable composition that can form a cured film with good surface properties can be easily provided. The oxime compound more preferably has the substructure represented by formula (d-1) or the substructure represented by formula (d-3), and even more preferably has the substructure represented by formula (d-1). In particular, if the oxime compound has the substructure represented by formula (d-1) (carbazole skeleton), a curable composition with excellent patternability is obtained. In formulas (d-1) to (d-4), * and ** represent bonding. In the following substructures represented by formulas (d-1) to (d-3), * bonds with a structure other than the substructure represented by formula (da1) or formula (da2). The substructures represented by the following formulas (d-1) to (d-4) are combined with the substructures represented by the aforementioned formula (da1) or formula (da2).
[0147]
[0148] The polymerization initiator (E) preferably contains a compound represented by formula (EA).
[0149] [In the formula, R ea1 R represents a branched hydrocarbon group having 3 to 20 carbon atoms, which may have substituents.ea2 ~R ea5 Each of these independently represents a hydrocarbon group having 1 to 20 carbon atoms, which may have substituents. n represents an integer from 0 to 4. The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-.
[0150] R ea1 Examples of branched hydrocarbon groups having 3 to 20 carbon atoms, represented by , include branched saturated hydrocarbon groups having 3 to 20 carbon atoms and branched unsaturated hydrocarbon groups having 3 to 20 carbon atoms.
[0151] R ea1Examples of branched saturated hydrocarbon groups having 3 to 20 carbon atoms, represented by , include 1-methylethyl group (isopropyl group), 1-methylpropyl group (sec-butyl group), 2-methylpropyl group (isobutyl group), 1,1-dimethylethyl group (tert-butyl group), 1,1-dimethylpropyl group, 2,2-dimethylpropyl group, 1,2-dimethylpropyl group, 1-ethylpropyl group, 1-methylbutyl group, 2-methylbutyl group, 3-methylbutyl group, 1,1-dimethylbutyl group, and 2,2-dimethylbutyl group. ,3,3-dimethylbutyl group, 1,2-dimethylbutyl group, 1,3-dimethylbutyl group, 2,3-dimethylbutyl group, 1-ethylbutyl group, 2-ethylbutyl group, 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 4-methylpentyl group, 1,1-dimethylpentyl group, 2,2-dimethylpentyl group, 3,3-dimethylpentyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 2,3-dimethylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3 - Ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 4-methylhexyl group, 1,1-dimethylhexyl group, 2,2-dimethylhexyl group, 3,3-dimethylhexyl group, 1,2-dimethylhexyl group, 1,3-dimethylhexyl group, 2,3-dimethylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 4-methylheptyl group, 1,1-dimethylheptyl Butyl group, 2,2-dimethylheptyl group, 3,3-dimethylheptyl group, 1,2-dimethylheptyl group, 1,3-dimethylheptyl group, 2,3-dimethylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, 3-ethylheptyl group, 1-methyloctyl group, 2-methyloctyl group, 3-methyloctyl group, 4-methyloctyl group, 1,1-dimethyloctyl group, 2,2-dimethyloctyl group, 3,3-dimethyloctyl group, 1,2-dimethyloctyl group, 1,3-dimethyloctyl group, 2,3-dimethyloctyl group, 1-ethyloctyl group, 2-ethyloctyl group, 3-ethyloctyl group, 1-methylnonyl group, 2-methylnonyl group, 3-methylnonyl group, 4-methylnonyl group, dimethylnonyl group, ethylnonyl group, methyldecyl group, dimethyldecyl group, ethyldecyl group, methylundecyl group, dimethylundecyl group, ethylundecyl group, methyldodecyl group and other branched alkyl groups; and the like. R, ea1 The branched alkyl group represented by may be any of a primary branched alkyl group, a secondary branched alkyl group, or a tertiary branched alkyl group. R ea1 The number of carbon atoms of the branched saturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, and is preferably 16 or less, more preferably 12 or less, still more preferably 10 or less (that is, 4 to 16, 4 to 12, or 5 to 10 is preferable).
[0152] R ea1 Examples of the branched unsaturated hydrocarbon group represented by include the aforementioned R ea1 Groups in which at least one carbon-carbon single bond contained in the branched saturated hydrocarbon group represented by is replaced with a carbon-carbon double bond or a carbon-carbon triple bond, and the like are exemplified. R ea1 Examples of the branched unsaturated hydrocarbon group represented by include alkenyl groups such as isopropenyl group, isobutenyl group, isopentenyl group, isohexenyl group, isoheptenyl group, isooctenyl group, isononenyl group and isodecenyl group; alkynyl groups such as isopropynyl group, isobutynyl group, isopentynyl group, isohexynyl group, isoheptynyl group, isooctynyl group, isononynyl group and isodecynyl group; and the like. R ea1 The number of carbon atoms of the branched unsaturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, and is preferably 16 or less, more preferably 12 or less, still more preferably 10 or less (that is, 4 to 16, 4 to 12, or 5 to 10 is preferable).
[0153] R ea2 , R ea3 , R ea4 and R ea5Examples of hydrocarbon groups having 1 to 20 carbon atoms represented by include saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, and aromatic hydrocarbon groups having 6 to 20 carbon atoms. ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon groups represented by may be the same or different.
[0154] Examples of the saturated hydrocarbon groups having 1 to 20 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, hexadecyl, and eicosyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and tricyclodecyl groups. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 18, more preferably 1 to 15, even more preferably 1 to 10, and even more preferably 1 to 8.
[0155] Examples of the carbon-2 to carbon-20 unsaturated hydrocarbon groups include alkenyl groups such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, hexadecenyl, octadecenyl, and eicosenyl groups; alkynyl groups such as ethynyl, propynyl, hexynyl, desinyl, and eicosinyl groups; and cycloalkenyl groups such as cyclopentenyl, cyclohexenyl, and cycloheptenyl groups. The carbon number of the unsaturated hydrocarbon group is preferably 2 to 18, more preferably 2 to 15, and even more preferably 2 to 10.
[0156] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include phenyl group, xylyl group, trimethylphenyl group, dipropylphenyl group, di(2,2-dimethylpropyl)phenyl group, naphthyl group, benzyl group, phenylethyl group, and phenylbutyl group. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 15, and even more preferably 6 to 12.
[0157] R ea1 , R ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon group represented by may have substituents such as halogen atoms, cyano groups, and nitro groups. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom.
[0158] The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-, and adjacent -CH2- will not be substituted with the same type of group at the same time, nor will terminal -CH2- be substituted.
[0159] n represents an integer from 0 to 4, preferably an integer from 0 to 3, more preferably an integer from 0 to 2, even more preferably an integer of 0 or 1, and even more preferably 0.
[0160] *-OCO-R ea4 The bond position of the group (* represents the bond with the phenyl group) is *-OCO-R ea4 The group may be attached to the 2nd, 3rd, or 4th position of the phenyl group, but is preferably at the 3rd or 4th position, and more preferably at the 4th position.
[0161] R ea1The branched hydrocarbon group having 3 to 20 carbon atoms represented by is preferably a branched saturated hydrocarbon group having 3 to 20 carbon atoms, more preferably a branched alkyl group having 3 to 20 carbon atoms, even more preferably a branched alkyl group having 3 to 10 carbon atoms, and preferably one or more selected from the group consisting of 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, and 3-ethylheptyl group.
[0162] R ea2 , R ea3 , R ea4 and R ea5 The hydrocarbon group having 1 to 20 carbon atoms represented by is preferably a saturated hydrocarbon group having 1 to 20 carbon atoms, an unsaturated hydrocarbon group having 2 to 20 carbon atoms, more preferably a saturated hydrocarbon group having 1 to 20 carbon atoms, even more preferably a chain-like saturated hydrocarbon group having 1 to 10 carbon atoms, and even more preferably a chain-like alkyl group having 1 to 8 carbon atoms. ea2 A chain-like alkyl group having 1 to 8 carbon atoms is preferred, and a chain-like alkyl group having 1 to 6 carbon atoms is more preferred. ea3 A chain-like alkyl group having 1 to 8 carbon atoms is preferred, and a chain-like alkyl group having 1 to 3 carbon atoms is more preferred. ea4 A chain-like alkyl group having 1 to 8 carbon atoms is preferred, and a chain-like alkyl group having 1 to 3 carbon atoms is more preferred. ea5 The alkyl group is preferably a chain-like or branched alkyl group having 1 to 8 carbon atoms, and more preferably a chain-like or branched alkyl group having 1 to 6 carbon atoms.
[0163] Furthermore, the polymerization initiator (E) preferably contains a compound represented by formula (EB).
[0164] [In the formula, R eb1 R represents a branched hydrocarbon group having 3 to 20 carbon atoms, which may have substituents. eb2 ~R eb4Each of these independently represents a hydrocarbon group having 1 to 20 carbon atoms, which may have substituents. m represents an integer from 0 to 4. The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-.
[0165] R eb1 Examples of branched hydrocarbon groups having 3 to 20 carbon atoms, represented by , include branched saturated hydrocarbon groups having 3 to 20 carbon atoms and branched unsaturated hydrocarbon groups having 3 to 20 carbon atoms.
[0166] R eb1 As a branched saturated hydrocarbon group having 3 to 20 carbon atoms, R ea1 Examples of branched saturated hydrocarbon groups having 3 to 20 carbon atoms, as represented by R, are similar to those exemplified above. eb1 The branched alkyl group represented by may be a primary branched alkyl group, a secondary branched alkyl group, or a tertiary branched alkyl group. eb1 The number of carbon atoms in the branched saturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less (i.e., 4 to 16, 4 to 12, or 5 to 10 are preferred).
[0167] R eb1 The branched unsaturated hydrocarbon group represented by the above-mentioned R is eb1 Examples include groups in which at least one carbon-carbon single bond in a branched saturated hydrocarbon group represented by is replaced by a carbon-carbon double bond or a carbon-carbon triple bond. eb1 Examples of branched unsaturated hydrocarbon groups represented by include alkenyl groups such as isopropenyl, isobutenyl, isopentenyl, isohexenyl, isoheptenyl, isooctenyl, isononyl, and isodecenyl groups; alkynyl groups such as isopropynyl, isobutynyl, isopentinyl, isohexynyl, isoheptynyl, isooctynyl, isononinyl, and isodesynyl groups; and so on. eb1The number of carbon atoms in the branched unsaturated hydrocarbon group represented by is preferably 4 or more, more preferably 5 or more, preferably 16 or less, more preferably 12 or less, and even more preferably 10 or less (i.e., 4 to 16, 4 to 12, or 5 to 10 are preferred).
[0168] R eb2 , R eb3 and R eb4 Examples of hydrocarbon groups having 1 to 20 carbon atoms represented by include saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, and aromatic hydrocarbon groups having 6 to 20 carbon atoms. eb2 , R eb3 and R eb4 The hydrocarbon groups represented by may be the same or different.
[0169] Examples of the saturated hydrocarbon groups having 1 to 20 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, hexadecyl, and eicosyl groups; branched alkyl groups such as isopropyl, isobutyl, isopentyl, neopentyl, and 2-ethylhexyl groups; and alicyclic saturated hydrocarbon groups having 3 to 20 carbon atoms such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and tricyclodecyl groups. The number of carbon atoms in the saturated hydrocarbon group is preferably 1 to 18, more preferably 1 to 15, even more preferably 1 to 10, and even more preferably 1 to 8.
[0170] Examples of the carbon-2 to carbon-20 unsaturated hydrocarbon groups include alkenyl groups such as vinyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, hexadecenyl, octadecenyl, and eicosenyl groups; alkynyl groups such as ethynyl, propynyl, hexynyl, desinyl, and eicosinyl groups; and cycloalkenyl groups such as cyclopentenyl, cyclohexenyl, and cycloheptenyl groups. The carbon number of the unsaturated hydrocarbon group is preferably 2 to 18, more preferably 2 to 15, and even more preferably 2 to 10.
[0171] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include phenyl group, xylyl group, trimethylphenyl group, dipropylphenyl group, di(2,2-dimethylpropyl)phenyl group, naphthyl group, benzyl group, phenylethyl group, and phenylbutyl group. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 15, and even more preferably 6 to 12.
[0172] R eb1 , R eb2 , R eb3 and R eb4 The hydrocarbon group represented by may have substituents such as halogen atoms, cyano groups, and nitro groups. The halogen atom is preferably a fluorine atom, a bromine atom, a chlorine atom, or an iodine atom, and more preferably a fluorine atom.
[0173] The -CH2- contained in the hydrocarbon group may be replaced with -O-, -S-, -CO-, or -OCO-, and in particular may be replaced with -O-, and adjacent -CH2- will not be simultaneously replaced with the same type of group, and terminal -CH2- will not be replaced.
[0174] m represents an integer from 0 to 4, preferably an integer from 1 to 3, more preferably an integer from 2 to 3, and even more preferably 3.
[0175] If m is 1 or greater, *-R eb4 At least one of the 2nd, 4th, and 6th positions of the phenyl group to which it is attached contains *-R eb4 (* represents a bond with a phenyl group) It is preferable that *-R is bonded, eb4 *-R is attached to at least two positions (2, 4, and 6) of the phenyl group to which it is bonded. eb4 It is more preferable that *-R is bonded. eb4 *-R is attached to all of the phenyl groups at positions 2, 4, and 6. eb4 It is even more preferable that they are bonded together.
[0176] R eb1The branched hydrocarbon group having 3 to 20 carbon atoms represented by is preferably a branched saturated hydrocarbon group having 3 to 20 carbon atoms, more preferably a branched alkyl group having 3 to 20 carbon atoms, even more preferably a branched alkyl group having 3 to 10 carbon atoms, and more preferably one or more selected from the group consisting of 1-methylpentyl group, 2-methylpentyl group, 3-methylpentyl group, 1-ethylpentyl group, 2-ethylpentyl group, 3-ethylpentyl group, 1-methylhexyl group, 2-methylhexyl group, 3-methylhexyl group, 1-ethylhexyl group, 2-ethylhexyl group, 3-ethylhexyl group, 1-methylheptyl group, 2-methylheptyl group, 3-methylheptyl group, 1-ethylheptyl group, 2-ethylheptyl group, and 3-ethylheptyl group.
[0177] R eb2 The hydrocarbon group having 1 to 20 carbon atoms represented by is preferably an aromatic hydrocarbon group having 6 to 20 carbon atoms, more preferably an aromatic hydrocarbon group having 6 to 17 carbon atoms, even more preferably an aromatic hydrocarbon group having 7 to 15 carbon atoms, and particularly preferably an aromatic hydrocarbon group having 8 to 13 carbon atoms. In any of these preferred embodiments, it is preferable to have a structure in which 1 to 8 (particularly 1 to 5) fluorine atoms as substituents, and 1 to 2 -CH2- are replaced by -O-.
[0178] R eb2 The preferred embodiment of the aromatic hydrocarbon group having 8 to 13 carbon atoms is preferably one of the following (eb2-1) to (eb2-6).
[0179]
[0180] R eb3 and R eb4 The hydrocarbon groups having 1 to 20 carbon atoms represented by the formula are, independently, preferably saturated hydrocarbon groups having 1 to 20 carbon atoms, unsaturated hydrocarbon groups having 2 to 20 carbon atoms, more preferably saturated hydrocarbon groups having 1 to 20 carbon atoms, even more preferably linear saturated hydrocarbon groups having 1 to 10 carbon atoms, even more preferably linear alkyl groups having 1 to 8 carbon atoms, and particularly preferably linear alkyl groups having 1 to 3 carbon atoms.
[0181] In formula (EB), if the -CH2- contained in the hydrocarbon group is replaced with -O-, -S-, -CO-, or -OCO-, the number of carbon atoms in the replaced portion shall be counted as the number of carbon atoms of the -CH2- before the replacement.
[0182] Furthermore, the polymerization initiator (E) preferably contains a compound represented by formula (EC). [In the formula, R ec1 and R ec2 Each of them is independent of R ec11 , OR ec11 COR ec11 , SR ec11 CONR ec12 R ec13 Or it represents CN. R ec11 , R ec12 and R ec13 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec11 , R ec12 or R ec13 The hydrogen atom of the group represented by OR ec21 COR ec21 , SR ec21 , NR ec22 R ec23 CONR ec22 R ec23 , -NR ec22 -OR ec23 , -N(COR ec22 )-OCOR ec23 , -C(=N-OR ec21 )-R ec22 , -C(=N-OCOR ec21 )-R ec22 , CN, halogen atom, or COOR ec21 It may be replaced with R. ec21 , R ec22 and R ec23 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec21 , R ec22 or R ec23The hydrogen atoms of the group represented by may be substituted with CN, halogen atoms, hydroxyl groups, or carboxyl groups. ec11 , R ec12 , R ec13 , R ec21 , R ec22 or R ec23 When the group represented by has an alkylene portion, the alkylene portion is -O-, -S-, -COO-, -OCO-, -NR ec24 -, -NR ec24 CO-, -NR ec24 COO-,-OCONR ec24 It may be interrupted 1 to 5 times by -, -SCO-, -COS-, -OCS-, or -CSO-. ec24 R represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ec11 , R ec12 , R ec13 , R ec21 , R ec22 or R ec23 When the group represented by has an alkyl moiety, the alkyl moiety may be branched, cyclic, or R ec12 and R ec13 and R ec22 and R ec23 They may each form a ring together. ec4 is a hydroxyl group, a carboxyl group, or the following formula (2-2)
[0183]
[0184] (In formula (2-2), L ec11 * represents *-O- or *-OCO-, where * is L ec12 This represents a bonding with L ec12 R represents an alkylene group having 1 to 20 carbon atoms, and the alkylene group may be interrupted by 1 to 3 -O- atoms. ec44a OR ec55 or COOR ec55 Represents R ec55 ) represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0185] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of alkyl groups having 1 to 20 carbon atoms represented by include methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, isopentyl group, tert-pentyl group, hexyl group, heptyl group, octyl group, isooctyl group, 2-ethylhexyl group, tert-octyl group, nonyl group, isononyl group, decyl group, isodecyl group, undecyl group, dodecyl group, tetradecyl group, hexadecyl group, octadecyl group, eicosyl group, cyclopentyl group, cyclohexyl group, cyclohexylmethyl group, cyclohexylethyl group, and the like.
[0186] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of aryl groups having 6 to 30 carbon atoms represented by the formula include phenyl, tolyl, xylyl, ethylphenyl, naphthyl, anthryl, phenanthryl, phenyl, biphenylyl, naphthyl, and anthryl groups substituted with one or more of the above alkyl groups.
[0187] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and R ec24 Examples of aralkyl groups having 7 to 30 carbon atoms, represented by the formula, include benzyl group, α-methylbenzyl group, α,α-dimethylbenzyl group, and phenylethyl group.
[0188] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 , R ec23 and Rec24 Examples of heterocyclic groups having 2 to 20 carbon atoms represented by include pyridyl group, pyrimidyl group, furyl group, thienyl group, tetrahydrofuryl group, dioxolanyl group, benzoxazole-2-yl group, tetrahydropyranyl group, pyrrolidyl group, imidazolidyl group, pyrazolidyl group, thiazolidyl group, isothiazolidyl group, oxazolidyl group, isoxazolidyl group, piperidyl group, piperadyl group, morpholinyl group, and the like, and are preferably 5 to 7 membered heterocyclic groups.
[0189] R in equation (EC) ec12 and R ec13 and R ec22 and R ec23 The statement that they may each form a ring together means that R ec12 and R ec13 and R ec22 and R ec23 This means that each atom may form a ring with the nitrogen, carbon, or oxygen atoms it connects to.
[0190] R in equation (EC) ec12 and R ec13 and R ec22 and R ec23 Examples of rings that can be formed by these rings together include cyclopentane rings, cyclohexane rings, cyclopentene rings, benzene rings, piperidine rings, morpholine rings, lactone rings, lactam rings, and the like, and are preferably 5 to 7 membered rings.
[0191] R in equation (EC) ec11 , R ec12 , R ec13 , R ec21 , R ec22 and R ec23 Examples of halogen atoms that may be present as substituents include fluorine, chlorine, bromine, and iodine atoms.
[0192] R in equation (EC) ec1 Preferably R ec11 The alkyl group is more preferably a C1 to C20 alkyl group, even more preferably a C1 to C10 alkyl group, and still more preferably a C1 to C6 alkyl group.
[0193] Rec4 Preferably, the group is represented by formula (2-2). In this case, it is advantageous in terms of the solubility of the oxime compound in solvent (J) and the developability of the curable composition.
[0194] L ec12 The number of carbon atoms in the alkylene group represented by is preferably 1 to 10, and more preferably 1 to 4.
[0195] R ec44a This is preferably a hydroxyl group or a carboxyl group, and more preferably a hydroxyl group.
[0196] Furthermore, the polymerization initiator (E) preferably contains a compound represented by formula (ED). [In the formula, R ed1 This represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or CN, and the hydrogen atoms of the alkyl group, aryl group, and arylalkyl group are further OR ed21 COR ed21 , SR ed21 , NR ed22 R ed23 ,-NCOR ed22 -OCOR ed23 CN, halogen atom, -CR ed21 =CR ed22 R ed23 or -CO-CR ed21 =CR ed22 R ed23 It may be replaced with R ed21 , R ed22 and R ed23 Each of these independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 2 to 20 carbon atoms. ed2 R ed11 OR ed11 Represents R ed11 R represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms, and the hydrogen atoms of the alkyl group, aryl group, and arylalkyl group may be further substituted with halogen atoms. ed3R represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms. ed1 , R ed3 , R ed21 , R ed22 and R ed23 The methylene group in the alkyl group represented by may be interrupted 1 to 5 times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds, or urethane bonds. ed3 It may form a ring together with an adjacent benzene ring. ed4 and R ed5 Each of them independently, R ed11 , OR ed11 , represents a CN or halogen atom. a and b are each independently between 0 and 3.
[0197] In the above formula (ED), R ed1 , R ed11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of alkyl groups represented by include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, s-butyl, t-butyl, pentyl, 1-methylbutyl, hexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, t-octyl, nonyl, isononyl, decyl, isodecyl, undecyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, cyclopentyl, cyclohexyl, cyclohexylmethyl, vinyl, allyl, butenyl, ethinyl, propynyl, methoxyethyl, ethoxyethyl, propoxyethyl, pentyloxyethyl, octyloxyethyl, methoxyethoxyethyl, ethoxyethoxyethyl, propoxyethoxyethyl, methoxypropyl, 2-methoxy-1-methylethyl, and the like. The number of carbon atoms in the alkyl group is preferably 1 to 15, more preferably 1 to 10, even more preferably 1 to 8, and even more preferably 1 to 6. In particular, the alkyl group is preferably methyl, ethyl, propyl, or 1-methylbutyl.
[0198] R ed1 , Red11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of aryl groups represented by include phenyl, tolyl, xylyl, ethylphenyl, chlorophenyl, naphthyl, anthuryl, phenanthrenyl, and phenyl, biphenylyl, naphthyl, and anthuryl groups substituted with one or more of the above alkyl groups. The number of carbon atoms in the aryl group is preferably 6 to 20, more preferably 6 to 15, even more preferably 6 to 12, and even more preferably 6 to 10. Among these, tolyl is preferred, o-tolyl and m-tolyl are more preferred, and o-tolyl is even more preferred.
[0199] R ed1 , R ed11 , R ed21 , R ed22 , R ed23 , R ed3 Examples of arylalkyl groups represented by include benzyl, chlorobenzyl, α-methylbenzyl, α,α-dimethylbenzyl, phenylethyl, and phenylethenyl. The number of carbon atoms in the arylalkyl group is preferably 7 to 20, more preferably 7 to 15, and even more preferably 7 to 12.
[0200] R ed21 , R ed22 and R ed23 Examples of heterocyclic groups represented by include, for example, 5- to 7-membered heterocycles such as pyridyl, pyrimidyl, furyl, thienyl, tetrahydrofuryl, dioxolanil, benzoxazole-2-yl, tetrahydropyranil, pyrrolidyl, imidazolidyl, pyrazolidyl, thiazolidyl, isothiazolidyl, oxazolidyl, isoxazolidyl, piperidyl, piperadyl, and morpholinil. The number of carbon atoms in the heterocyclic group is preferably 2 to 15, more preferably 3 to 12, and even more preferably 3 to 9.
[0201] Together with the adjacent benzene ring, R ed3Examples of rings formed by the nitrogen atom to which it is bonded include 5- to 7-membered rings such as cyclopentane rings, cyclohexane rings, cyclopentene rings, benzene rings, piperidine rings, morpholine rings, lactone rings, and lactam rings.
[0202] R ed1 , R ed11 , R ed21 , R ed22 and R ed23 Halogen atoms and R that may be substituted ed4 , R ed5 Examples of halogen atoms represented by this formula include fluorine, chlorine, bromine, and iodine.
[0203] The methylene group contained in the alkyl group described above may be interrupted one to five times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds, or urethane bonds. In this case, the interrupting group may be one or two or more types of groups, and if the group can be interrupted consecutively, it may be interrupted two or more times consecutively. Furthermore, the alkyl group may have branched side chains, may be a cyclic alkyl group, and the alkyl group terminus may be an unsaturated bond. Among these, it is preferable that the methylene group is interrupted by an ether bond.
[0204] Examples of alkyl groups interrupted by ether bonds include the following:
[0205]
[0206] In particular, in the above formula (ED), R ed1 This represents an aryl group with 6 to 20 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 It is replaced with R ed21 R represents an alkyl group having 1 to 15 carbon atoms. ed21 The methylene group in the alkyl group is interrupted 1 to 5 times by ether bonds, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 15 carbon atoms. ed3 However, it is preferable that it represents an alkyl group having 1 to 15 carbon atoms, and that a and b are 0.
[0207] Red1 This represents an aryl group with 6 to 15 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 It is replaced with R ed21 R represents an alkyl group having 1 to 10 carbon atoms. ed21 The methylene group in the alkyl group is interrupted 1 to 3 times by ether bonds, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 10 carbon atoms. ed3 However, it is more preferable that the alkyl group has 1 to 10 carbon atoms, and that a and b are 0.
[0208] R ed1 This represents an aryl group with 6 to 12 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 It is replaced with R ed21 R represents an alkyl group having 1 to 8 carbon atoms. ed21 The methylene group in the alkyl group is interrupted once or twice by an ether bond, R ed2 However, R ed11 Represents R ed11 However, R represents an alkyl group with 1 to 8 carbon atoms. ed3 However, it is more preferable that it represents an alkyl group having 1 to 8 carbon atoms, and that a and b are 0.
[0209] R ed1 This represents an aryl group with 6 to 10 carbon atoms, and the hydrogen atoms of this aryl group are OR ed21 It is replaced with R ed21 R represents an alkyl group having 1 to 6 carbon atoms. ed21 The methylene group in the alkyl group is interrupted once by an ether bond, R ed2 However, R ed11 Represents R ed11 However, it represents an alkyl group with 1 to 3 carbon atoms, R ed3 However, it is even more preferable that it represents an alkyl group having 1 to 3 carbon atoms, and that a and b are 0.
[0210] The polymerization initiator (E) preferably contains at least one compound represented by formulas (EA) to (ED), more preferably contains a compound represented by formula (EA) or formula (ED) from the viewpoint of process tolerance, and even more preferably contains a compound represented by formula (EA).
[0211] Examples of oxime compounds include acetophenone O-benzoyl oxime, N-benzoyloxy-1-(4-phenylsulfanylphenyl)butan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropane-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethane-1-imine, and N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2,4-dioxacyclopentanylmethyl Examples include compounds described in Japanese Patent Publication No. 2011-132215, International Publication Nos. 2008 / 78678, 2008 / 78686, 2012 / 132558, 2017 / 051680, and 2020 / 004601. Commercially available products such as Irgacure OXE01 (N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine), OXE02 (N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethane-1-imine), OXE03 (all manufactured by BASF), N-1919, NCI-930, NCI-831 (all manufactured by ADEKA) may also be used.
[0212] Other polymerization initiators (E) include photopolymerization initiators such as alkylphenone compounds, biimidazole compounds, triazine compounds, and acylphosphine compounds, and thermal polymerization initiators such as azo compounds and organic peroxides.
[0213] The content of the polymerization initiator (E) in the curable composition is preferably 0.1 parts by mass or more and 80 parts by mass or less, more preferably 0.1 parts by mass or more and 30 parts by mass or less, per 100 parts by mass of the polymerizable compound (D). Furthermore, the content of the polymerization initiator (E) in the curable composition is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 20 parts by mass or less, per 100 parts by mass of the total amount of resin (C) and polymerizable compound (D).
[0214] From the viewpoint of process tolerance, the content of the polymerization initiator (E) in the curable composition is, for example, 0.01% by mass or more and 20% by mass or less, preferably 0.1% by mass or more and 15% by mass or less, more preferably 0.2% by mass or more and 10% by mass or less, even more preferably 0.3% by mass or more and 8% by mass or less, even more preferably 0.5% by mass or more and 5% by mass or less, and particularly preferably 0.5% by mass or more and 3% by mass or less.
[0215] <Antioxidant (Fa)> The curable composition may contain an antioxidant (Fa). The antioxidant (Fa) is not particularly limited as long as it is an antioxidant commonly used in industry, and phenolic antioxidants, phosphorus-based antioxidants, phosphorus / phenol complex antioxidants, and sulfur-based antioxidants can be used, but from the viewpoint of luminescence intensity, phenolic antioxidants and phosphorus / phenol complex antioxidants are preferred, and phosphorus / phenol complex antioxidants are more preferred. The curable composition may contain two or more antioxidants.
[0216] Examples of phosphorus / phenol complex antioxidants include Sumirizer® GP (6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1.3.2]dioxaphosfepine) (manufactured by Sumitomo Chemical Co., Ltd.). Other antioxidants include, for example, the compounds described in Japanese Patent Application Publication No. 2024-61630.
[0217] The content of antioxidants (Fa) in the curable composition (total amount in the case of multiple types) is, for example, 1 part by mass or more and 50 parts by mass or less per 100 parts by mass of resin (C), and from the viewpoint of luminescence intensity, it is preferably 5 parts by mass or more and 40 parts by mass or less, and more preferably 7 parts by mass or more and 30 parts by mass or less.
[0218] <Leveling agent (H)> Examples of leveling agent (H) include silicone-based surfactants, fluorine-based surfactants, and silicone-based surfactants having a fluorine atom. These may have polymerizable groups in their side chains. It is preferable that the leveling agent (H) includes a silicone-based surfactant. The curable composition may contain two or more types of leveling agent (H).
[0219] Examples of silicone-based surfactants include surfactants having siloxane bonds in their molecules. Examples of such surfactants include the compounds described in Japanese Patent Application Publication No. 2024-61630.
[0220] Examples of fluorine-based surfactants include surfactants having fluorocarbon chains in their molecules. Examples of such surfactants include the compounds described in Japanese Patent Application Publication No. 2024-61630.
[0221] When the curable composition contains a leveling agent (H), the content of the leveling agent (H) in the curable composition is, for example, 0.001% by mass or more and 1.0% by mass or less, preferably 0.005% by mass or more and 0.75% by mass or less, and more preferably 0.01% by mass or more and 0.5% by mass or less, relative to the total amount of solids in the curable composition. When the content of the leveling agent (H) is within the above range, the flatness of the cured film when used as a wavelength conversion layer can be improved.
[0222] <Solvent (J)> Solvent (J) dissolves the polymerizable compound (D) and the resin (C) and polymerization initiator (E) used in a preferred embodiment. Examples of solvent (J) include the solvent described in Japanese Patent Application Publication No. 2024-61630.
[0223] The solvent (J) preferably contains one or more selected from the group consisting of propylene glycol monomethyl ether acetate, ethyl lactate, propylene glycol monomethyl ether, cyclohexyl acetate, ethyl 3-ethoxypropionate, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, 4-hydroxy-4-methyl-2-pentanone, and aromatic hydrocarbon solvents.
[0224] Solvent (J) is a component other than the solid content, and includes, for example, solvents contained in dispersions of semiconductor particles (A) or solutions of resins (C).
[0225] The solvent (J) content in the curable composition is the ratio of the total mass of all solvents contained in the curable composition to the total amount of the curable composition, and is, for example, 40% by mass or more and 95% by mass or less, preferably 40% by mass or more and 80% by mass or less, relative to the total amount of the curable composition. In other words, the solid content of the curable composition is, for example, 5% by mass or more and 60% by mass or less, preferably 20% by mass or more and 60% by mass or less. When the solvent (J) content is within the above range, the flatness of the curable composition layer during application is improved, and it tends to be easier to form a wavelength conversion layer of appropriate thickness.
[0226] <Other components> The curable composition may further contain additives known in the art, such as polymerization inhibitors, fillers, other polymer compounds, adhesion promoters, and chain transfer agents, as needed.
[0227] <<Cured Film>> This disclosure includes cured films formed from curable compositions. A cured film containing semiconductor particles (A) can emit light of a different wavelength from the irradiated light when irradiated with ultraviolet or visible light. Therefore, a cured film containing semiconductor particles (A) can be used as a wavelength conversion film.
[0228] The thickness of the cured film is, for example, 0.5 μm or more and 10 μm or less, preferably 1 μm or more and 9 μm or less, more preferably 1.5 μm or more and 7 μm or less, and even more preferably 2 μm or more and 5 μm or less.
[0229] <<Method for Manufacturing a Curable Composition>> A curable composition can be manufactured by a method that includes mixing predetermined components and other components used as needed. The method for manufacturing a curable composition may further include a step of preparing a resin (C). Among the components contained in the curable composition, semiconductor particles (A) and light scattering agents (B) may be mixed with some or all of the solvent (J) beforehand before being mixed with the other components.
[0230] <<Method for Manufacturing a Cured Film>> The cured film of this disclosure can be obtained by performing the following steps: applying a curable composition to a substrate, which includes semiconductor particles (A) containing an organic ligand (G) and a polymerizable compound (D), and optionally other components; an exposure step of curing the coated layer of the curable composition (hereinafter also referred to as the "composition layer") by irradiating it with light; and a heating step (post-bake) of the composition layer (cured layer) after exposure. Further steps may include a drying (pre-bake) step in which the composition layer, which is the coated layer of the curable composition, is dried (pre-bake) before the exposure step to remove volatile components such as solvents, and a developing step performed after the exposure step and before the post-bake, and it is preferable to include at least a pre-bake step.
[0231] The curable composition of this disclosure uses semiconductor particles (A) containing an organic ligand (G) that satisfies a predetermined weight loss ratio of 300°C or more, and a polymerizable compound (D) that satisfies a predetermined clogP. Therefore, the decrease in luminescence intensity after exposure relative to the luminescence intensity before exposure can be suppressed, and more preferably, the decrease in luminescence intensity of the cured layer after exposure and heating (post-bake) relative to the luminescence intensity of the composition layer before exposure after drying (pre-bake) can be suppressed. The process resistance evaluated in the examples described later is, for example, 75 to 100%, preferably 77 to 100%, more preferably 80 to 100%, even more preferably 83% to 100%, even more preferably 85 to 100%, and even more preferably 87 to 100%.
[0232] The cured film may be formed over the entire surface of the substrate, or it may be formed as a cured pattern on a part of the substrate surface. In this specification, a cured pattern is one aspect of the cured film, and refers to a cured film formed in a pattern.
[0233] The curable composition used for forming the cured film comprises semiconductor particles (A) containing an organic ligand (G) and a polymerizable compound (D), an example of which is the curable composition described above.
[0234] The coating process involves applying a curable composition to a substrate to form a composition layer. Coating methods include spin coating, slit coating, and slit-and-spin coating.
[0235] Examples of substrates include glass plates such as quartz glass, borosilicate glass, aluminasilate glass, and soda-lime glass with a silica coating on the surface; resin plates such as polycarbonate, polymethyl methacrylate, and polyethylene terephthalate; silicon; and substrates on which aluminum, silver, or silver / copper / palladium alloy thin films are formed. Preferably, the substrate is a glass plate or a silicon substrate.
[0236] The substrate may be pre-treated to adjust the wettability of the substrate surface. Examples of pre-treatment include solvent cleaning with alcohol or acetone, acid treatment, alkali treatment, plasma treatment, and corona treatment. By selecting an appropriate pre-treatment for the substrate on which the cured film is to be laminated, the applicability of the curable composition can be improved compared to an untreated substrate.
[0237] The pre-bake temperature is preferably 30°C to 130°C, and more preferably 50°C to 120°C. The heating time is preferably 10 seconds to 60 minutes, and more preferably 30 seconds to 30 minutes.
[0238] The thickness of the composition layer after the coating or drying process is not particularly limited and can be appropriately selected according to the desired thickness of the cured film. For example, it is 0.5 μm or more and 10 μm or less, preferably 1 μm or more and 9 μm or less, more preferably 1.5 μm or more and 7 μm or less, and even more preferably 2 μm or more and 5 μm or less. The thickness of the final cured film may also be the same as described above.
[0239] In a preferred embodiment, an exposure step is performed on the composition layer after the drying step. The exposed composition layer hardens due to polymerization of polymerizable compounds (D) and the like contained in the composition layer. A light source that generates light with a wavelength of 250 nm to 450 nm is preferred for exposure. If the curable composition contains a photopolymerization initiator (E), light around 436 nm, 408 nm, or 365 nm may be selectively extracted from the above wavelengths using a bandpass filter, depending on the absorption wavelength of the polymerization initiator (E). Specific examples of light sources include mercury lamps, light-emitting diodes, metal halide lamps, halogen lamps, and the like.
[0240] The exposure amount in the exposure process is preferably 50 mJ / cm². 2 More preferably, 80 mJ / cm 2 More preferably 100 mJ / cm 2 More preferably, the concentration is 150 mJ / cm². 2 That's all. The exposure dose is typically 1000 mJ / cm². 2The following, preferably 800 mJ / cm² 2 More preferably, 700 mJ / cm 2 The following (i.e., 50–1000 mJ / cm²) 2 , 80-800mJ / cm 2 , 100-700mJ / cm 2 , or 150-700 mJ / cm² 2 (Preferably) The exposure amount in the exposure process is 1000 mJ / cm 2 The following conditions prevent excessive shrinkage of the cured film, thereby preventing the semiconductor particles (A) from coming into close proximity within the film due to shrinkage and preventing a decrease in emitted light intensity. The exposure amount is the exposure amount based on a wavelength of 365 nm and can be measured using an ultraviolet integrated light meter (UIT-250, manufactured by Ushio Inc.).
[0241] One example of a method for forming a cured pattern, which is a form of a cured film, is photolithography. Photolithography is a method of exposing a composition layer through a photomask for forming the desired cured pattern and then developing it. In this case, it is preferable to use an exposure apparatus such as a mask aligner and a stepper, as this allows for uniform irradiation of the entire exposure surface with parallel light and enables precise alignment between the photomask and the substrate on which the composition layer is formed.
[0242] By subjecting the composition layer after the exposure process to a developing process in which it is brought into contact with a developer, the unexposed parts of the composition layer are dissolved and removed in the developer, thereby imparting a pattern to the composition layer. Examples of the developer include aqueous solutions of alkaline compounds such as potassium hydroxide, sodium bicarbonate, sodium carbonate, and tetramethylammonium hydroxide, or organic solvents. The concentration of the alkaline compound in the aqueous solution is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.03% by mass or more and 5% by mass or less. Examples of organic solvents include those similar to solvent (J) described above. The developer may also contain a surfactant. The developing method may be any of the following: the paddle method, the dipping method, or the spray method. Furthermore, the substrate may be tilted at any angle during development.
[0243] The composition layer after the exposure step or after the development step is thermally cured (post-baked) in the thermal curing step. Through the thermal curing step, the polymerization of the resin (C), the polymerizable compound (D) and the like including preferred embodiments can be further advanced, and the resistance to solvents is improved compared to before post-baking.
[0244] The thermal curing temperature in the thermal curing step performed after the exposure step or after the development step is preferably 100°C or higher and 250°C or lower, more preferably 150°C or higher and 200°C or lower. The heating time is preferably 1 minute or more and 120 minutes or less, more preferably 10 minutes or more and 60 minutes or less. By performing heating after development, the polymerization of the unreacted polymerizable compound (D) and the like contained in the cured pattern can be advanced, so that a cured pattern with further excellent chemical resistance can be obtained. Even when development is not performed, heating (post-baking) is further performed on the exposed composition layer.
[0245] The thermal curing step is preferably performed under an air atmosphere.
[0246] <<Display Device>> Since the cured film has a function of converting the wavelength of irradiation light, it can be used as a color conversion layer (wavelength conversion film) of a display device. Examples of such a display device include the display devices described in JP-A-2006-309219, JP-A-2006-310303, JP-A-2013-15812, JP-A-2009-251129, JP-A-2014-2363, and the like. The cured film according to the present disclosure is useful as a color conversion layer (wavelength conversion film) for display devices, particularly liquid crystal display devices, organic EL display devices, or inorganic EL display devices.
[0247] This application claims the benefit of priority based on Japanese Patent Application No. 2025-078615 filed on May 9, 2025. The entire content of the specification of Japanese Patent Application No. 2025-078615 filed on May 9, 2025 is incorporated herein by reference in its entirety.
[0248] Hereinafter, the present disclosure will be described in further detail by way of Examples. "%" and "part" in the examples mean mass% and mass parts, respectively, unless otherwise specified.
[0249] (1) Measurement of the weight loss ratio above 300°C and the composition ratio of organic ligands of semiconductor particles (A) containing organic ligand (G) The weight loss ratio above 300°C of semiconductor particles (A) containing organic ligand (G) was measured under the following conditions. 0.1 g of semiconductor particles (A) containing organic ligand (G) was redispersed in 1 mL of toluene, 9 mL of poor solvent was added to precipitate, and then the mixture was centrifuged at 4000 G for 20 minutes. The precipitated semiconductor particles (A) containing organic ligand (G) was redispersed in 0.5 mL of toluene. The resulting dispersion was dried at 110°C for 10 minutes to prepare a dry powder. The dry powder was heated from 25°C to 600°C at a heating rate of 10°C / min under a nitrogen atmosphere using thermogravimetric analysis (Bruker TG-DTA2000SA). Here, using the TG graph obtained by thermogravimetric analysis, the weight loss rate from 100°C to 300°C and from 300°C to 600°C were calculated, with the 100°C value (weight) as the baseline. The ratio of the weight loss rate from 300°C to 600°C to the sum of these was defined as the weight loss rate above 300°C (%). In other words, the weight loss rate above 300°C (%), calculated using equation (1), was measured when semiconductor particles (A) containing each organic ligand (G) were heated from 25°C to 600°C under a nitrogen atmosphere at a heating rate of 10°C / min using thermogravimetric analysis. Note that the weight loss rate above 300°C (%) refers to a simple ratio. Weight loss rate above 300°C X (%) = {T1 / (T 0+ T1)}×100...(1) [In formula (1), T 0 This is the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight, and T 1is the weight reduction rate from 300°C to 600°C based on the weight of the semiconductor particles (A) containing the organic ligand (G) at 100°C.] Further, when the TG graphs from thermogravimetric analysis of the purified semiconductor particles (A) containing the organic ligand (G) of Preparation Example 1 are compared with the TG graphs of the purified semiconductor particles (A) containing the organic ligand (G) of Preparation Examples 2 to 4, a mass reduction behavior in the temperature range of 100°C to 300°C was observed only in the TG graphs of the semiconductor particles (A) containing the organic ligand (G) of Preparation Examples 2 to 4. This mass reduction behavior at 100°C to 300°C is presumed to originate from the hydrophilic organic ligand coordinated by ligand exchange. Therefore, the composition ratio of each organic ligand was calculated with the ratio T0 / (T0+T1) defined as the composition ratio of the hydrophilic organic ligand, and the ratio T1 / (T0+T1) defined as the composition ratio of the hydrophobic organic ligand. The composition ratio of each organic ligand means a simple proportion.
[0250] (2) clogP of Polymerizable Compound (D) Using ChemDraw 22.0 (manufactured by CambridgeSoft), the clogP of the polymerizable compound (D) was determined.
[0251] (3) Measurement of Process Resistance On a 5 cm square glass substrate ("Eagle XG" manufactured by Corning Inc.), the curable compositions 1 to 12 described later were applied by spin coating so that the thickness of the layer after post-baking would be 5 μm, followed by pre-baking at 100°C for 3 minutes to form a composition layer. For the substrate on which this composition layer was formed, using an exposure apparatus ("TME-150RSK" manufactured by Topcon Corporation) under an air atmosphere, 200 mJ / cm 2A cured film was formed by irradiating with light at an exposure level (based on 365 nm) and performing post-bake at 180°C for 10 minutes. The luminescence intensity of the composition layer after pre-baking and the cured film after post-baking was measured using the following method. A surface-emitting backlight (OPSM series: manufactured by Optex FA Co., Ltd.) equipped with an LED lamp and diffuser plate with an emission peak wavelength of 450 nm was prepared as the backlight. The backlight was installed with the diffuser plate facing upwards, and a spectroradiometer (SR-UL1R: manufactured by Topcon Techno House Co., Ltd.) was placed at a height of 60 cm from the surface of the diffuser plate. A glass substrate (Eagle 2000: manufactured by Corning Corporation) was placed on the surface of the diffuser plate of the backlight as a reference. With the backlight turned on in this state, the integrated spectral irradiance value in the wavelength range of 380 nm to 480 nm of the backlight was measured through the reference glass substrate at 3.15 W·sr. -1 ・m -2 The backlight intensity was adjusted to achieve the desired result. Next, the reference glass substrate was removed, and a 5 cm square substrate having the pre-baked composition layer formed on the glass substrate, and a 5 cm square substrate having the post-baked cured film formed on the glass substrate were placed on the surface of the backlight diffuser plate as measurement samples. With the backlight turned on in this state, the light emitted from the composition layer and the cured film was measured as the integrated spectral irradiance in the wavelength range of 480 nm to 780 nm, and the luminous intensity (unit: mW・sr) was measured. -1 ・m -2 The luminescence intensity of the cured film formed on the glass substrate was taken as EIa, and the luminescence intensity of the composition layer formed on the glass substrate was taken as EIb. Process resistance was determined according to the following formula: Process resistance (%) = [EIa / EIb] × 100
[0252] [Solid Content] Approximately 1 g of resin (C) solution was weighed into an aluminum cup, dried at 180°C for 1 hour, and then its mass was measured. The solid content (mass %) of resin (C) solution was calculated from the amount of mass loss.
[0253] [Weight-average molecular weight] The weight-average molecular weight (Mw) of resin (C) was measured by the GPC method under the following conditions: Apparatus: K2479 (Shimadzu Corporation) Column: SHIMADZU Shim-pack GPC-80M Column temperature: 40°C Solvent: Tetrahydrofuran Flow rate: 1.0 mL / min Detector: RI Calibration standards: TSK STANDARD POLYSTYRENE F-40, F-4, F-288, A-2500, A-500 (Tosoh Corporation)
[0254] [Acid Value] 3 g of resin (C) solution was accurately weighed and dissolved in a mixed solvent of 90 g of acetone and 10 g of water. Using a 0.1 N KOH aqueous solution as the titrant, the acid value of resin (C) solution was measured using an automatic titrator (manufactured by Hiranuma Sangyo Co., Ltd., product name: COM-555). The acid value per gram of solids was determined from the acid value of the solution and the solids content of the solution.
[0255] Preparation Example 1: Preparation of semiconductor particles (A) containing organic ligand (G) (hydrophobic organic ligand (G1)) <Production of core particles> Indium acetate (0.3 mmol) and zinc oleate (0.05 mmol) were added to a mixture of oleic acid (0.9 mmol), 1-dodecanethiol (0.1 mmol), and octadecene (10 mL), and the mixture was heated from room temperature to 120°C at a heating rate of 10°C per minute under vacuum (<20 Pa) and reacted for 1 hour. Next, the mixture reacted under vacuum (<20 Pa) was heated to 25°C under a nitrogen atmosphere, and tris(trimethylsilyl)phosphine (0.15 mmol) was added, followed by heating to 300°C at a heating rate of 10°C per minute and reacting for 10 minutes. Furthermore, the reaction mixture was cooled to 25°C, octanoic acid chloride (0.60 mmol) was injected, and the mixture was heated to 250°C at a rate of 10°C per minute. After reacting for 30 minutes, it was cooled to 25°C to obtain a dispersion solution of core particles.
[0256] <Preparation of Precursor Solution for Shell Formation> 40 mmol of zinc oleate and 75 mL of octadecene were mixed and heated under vacuum at 110°C for 1 hour to prepare a Zn precursor solution with [Zn] = 0.4 M. Separately, 22 mmol of selenium powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain selenide trioctylphosphine with [Se] = 2.2 M. Furthermore, 22 mmol of sulfur powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain sulfide trioctylphosphine with [S] = 2.2 M.
[0257] <Shell Formation> The core particle dispersion solution was heated to 250°C. At 250°C, 4.3 mL of Zn precursor solution and 1.5 mL of selenite trioctylphosphine were added and reacted for 30 minutes to form a ZnSe shell on the surface of the InP-based semiconductor nanoparticles. Furthermore, 3.8 mL of Zn precursor solution and 0.5 mL of sulfide trioctylphosphine were added, the temperature was raised to 280°C, and the reaction was allowed to proceed for 1 hour to form a ZnS shell.
[0258] <Purification of Core-Shell Particles> The reaction solution of the obtained core-shell particles was added to acetone, mixed well, and then centrifuged. The centrifugal acceleration was set to 4000 G. The precipitate was collected, and n-hexane was added to the precipitate to prepare a dispersion. This operation was repeated several times to obtain purified core-shell particles (semiconductor particles (A) containing organic ligand (G) (hydrophobic organic ligand (G1))).
[0259] Preparation Example 2: Preparation of semiconductor particles (A1) containing organic ligands (Ga) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2)) In a flask, semiconductor particles (A) containing organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene at a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, and 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare the mixture. The mixture was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. Centrifugation at 4000 G for 20 minutes separated the mixture into a clear 1-octadecene phase and a phase containing semiconductor particles (A1) containing organic ligands (Ga). The 1-octadecene phase was removed, and the phase containing semiconductor particles (A1) containing organic ligands (Ga) was recovered.
[0260] 5.0 mL of acetone was added to the obtained phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A1) containing purified organic ligands (Ga) ((hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2))). The weight loss ratio above 300°C of the semiconductor particles (A1) containing organic ligand (Ga), as determined by the above measurement method, was 32.0%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A1) containing organic ligand (Ga), as determined by the above measurement method, were 68.0% and 32.0%, respectively.
[0261] Preparation Example 3: Preparation of semiconductor particles (A2) containing organic ligand (Gb) (hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2)) In a flask, semiconductor particles (A) containing organic ligand (G) obtained in Preparation Example 1 were dispersed in 1-octadecene at a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, and 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare mixture 1. Mixture 1 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating into a clear 1-octadecene phase and a phase containing semiconductor particles (A) containing organic ligand (G). The 1-octadecene phase was removed, and the phase containing semiconductor particles (A) containing organic ligand (G) was recovered.
[0262] Propylene glycol monomethyl ether acetate (hereinafter also referred to as "PGMEA") (dispersion medium) was added to the semiconductor particle (A) phase containing the remaining organic ligand (G) to prepare a PGMEA dispersion so that the semiconductor particle (A) containing the organic ligand (G) was 10% by mass. The prepared PGMEA dispersion was placed in a flask, and 1.0 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.1 g of zinc acetate were added to prepare mixture 2. Mixture 2 was stirred at 110°C for 60 minutes under a nitrogen atmosphere and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the phase containing the semiconductor particle (A2) containing the organic ligand (Gb).
[0263] 5.0 mL of acetone was added to the obtained phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A2) containing purified organic ligand (Gb) ((hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2))). The weight loss ratio above 300°C of the semiconductor particles (A2) containing organic ligand (Gb), as determined by the above measurement method, was 18.3%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A2) containing organic ligand (Gb), as determined by the above measurement method, were 81.7% and 18.3%, respectively.
[0264] Preparation Example 4: Preparation of semiconductor particles (A3) containing organic ligands (Gc) (hydrophobic organic ligands and hydrophilic organic ligands) In a flask, semiconductor particles (A) containing organic ligands (G) obtained in Preparation Example 1 were dispersed in 1-octadecene at a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in a flask, and 1.2 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.12 g of zinc acetate were added to prepare mixture 3. The mixture 3 was stirred at 110°C for 60 minutes under a nitrogen atmosphere, cooled to 25°C, and then transferred to a centrifuge tube. It was centrifuged at 4000 G for 20 minutes, separating into a clear 1-octadecene phase and a phase containing semiconductor particles (A) containing organic ligands (G). The 1-octadecene phase was removed, and the phase containing semiconductor particles (A) containing organic ligands (G) was recovered.
[0265] PGMEA (dispersion medium) was added to the remaining semiconductor particle (A) phase containing the organic ligand (G) to prepare a PGMEA dispersion so that the semiconductor particle (A) containing the organic ligand (G) was 10% by mass. The prepared PGMEA dispersion was placed in a flask, and 1.2 g of triethylene glycol monomethyl ether thiol (molecular weight 180) and 0.12 g of zinc acetate were added to prepare mixture 4. The mixture 4 was stirred at 110°C for 60 minutes under a nitrogen atmosphere and cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, 50 mL of n-hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes to recover the phase containing the semiconductor particle (A3) containing the organic ligand (Gc).
[0266] 5.0 mL of acetone was added to the obtained phase to prepare a dispersion. 50 mL of n-hexane was added to the obtained dispersion and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed and the precipitate was collected. This procedure was repeated several times to obtain semiconductor particles (A3) containing purified organic ligands (Gc) ((hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2))). The weight loss ratio above 300°C of the semiconductor particles (A3) containing organic ligands (Gc), as determined by the above measurement method, was 13.8%. The composition ratios of hydrophilic organic ligand (G2) and hydrophobic organic ligand (G1) in the semiconductor particles (A3) containing organic ligands (Gc), as determined by the above measurement method, were 86.2% and 13.8%, respectively.
[0267] Preparation Example 5: Preparation of dispersion c of light scattering agent (B) To 70 parts of titanium dioxide nanoparticles (B1), 3 parts of BYK-LPN21116 (manufactured by Bic Chemie Japan) and PGMEA were added so that the total amount was 100 parts. The mixture was then stirred in a paint shaker until it was thoroughly dispersed to obtain dispersion c of light scattering agent (B1) (solid content 73%).
[0268] Synthesis Example 1: Synthesis of Resin (C1) 276.8 parts of propylene glycol monomethyl ether acetate were placed in a flask equipped with a stirring device, dropping funnel, condenser, thermometer, and gas inlet tube, and stirred while purging with nitrogen, and the temperature was raised to 120°C. Next, a monomer mixture consisting of 92.4 parts of 2-ethylhexyl acrylate, 184.9 parts of glycidyl methacrylate, and 12.3 parts of dicyclopentanyl methacrylate was mixed with 35.3 parts of t-butyl peroxy-2-ethylhexanoate (polymerization initiator), and this mixture was added dropwise to the flask from the dropping funnel over a period of 2 hours. After the addition was complete, the mixture was stirred at 120°C for a further 30 minutes to carry out the copolymerization reaction and produce an addition copolymer.
[0269] Subsequently, the flask was purged with air, and 93.7 parts of acrylic acid, 1.5 parts of triphenylphosphine (catalyst), and 0.8 parts of methoquinone (polymerization inhibitor) were added to the above addition copolymer solution. The reaction was continued at 110°C for 10 hours, during which the epoxy groups derived from glycidyl methacrylate reacted with acrylic acid to cleave the epoxy groups and simultaneously introduce polymerizable unsaturated bonds into the polymer side chains. Next, 24.2 parts of succinic anhydride were added to the reaction system, and the reaction was continued at 110°C for 1 hour, during which the hydroxyl groups generated by the cleavage of the epoxy groups reacted with succinic anhydride to introduce carboxyl groups into the side chains, yielding polymer (resin (C1)). Finally, 383.3 parts of propylene glycol monomethyl ether acetate were added to the reaction solution to obtain a resin (C1) solution with a polymer solids content of 40%. The Mw of the resulting copolymer was 6.2 × 10⁻⁶. 3 The acid value, calculated on a solid content basis, was 35 mg KOH / g.
[0270] Comparative Examples 1-2, Examples 1-10: Preparation of Curable Compositions 1-12 The semiconductor particles (A) obtained in the above preparation examples, the dispersion c of the light scattering agent (B), and each component were mixed to prepare curable compositions 1-12 having the compositions shown in Table 1. In Table 1, the amounts of components other than the solvent (J) are shown as solid content equivalents.
[0271]
[0272] (A1) + (Ga): Semiconductor particle (A1) containing the hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 2 (A2) + (Gb): Semiconductor particle (A2) containing the hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 3 (A3) + (Gc): Semiconductor particle (A3) containing the hydrophobic organic ligand (G1) and hydrophilic organic ligand (G2) prepared in Preparation Example 4 Resin (C1): Resin (C1) prepared in Synthesis Example 1 Polymerizable compound (D1): 1,6-hexanediol diacrylate (clogP is 3.0) Polymerizable compound (D2): Dipropylene glycol diacrylate (clogP is 2.0) Polymerizable compound (D3): Ethylene oxide-modified bisphenol A diacrylate (manufactured by Daicel Ornex, EBECRYL150, clogP 5.2) Polymerizable compound (D4): Dipentaerythritol polyacrylate (manufactured by Shin Nakamura Kogyo Co., Ltd., "A-9570W", clogP 3.8) Polymerizable compound (D5): Ethoxylated bisphenol fluorene diacrylate (clogP 7.5) Polymerization initiator (E1): Compound represented by the following formula (EA-1) Light scattering agent (B1): Dispersion of the light scattering agent (B1) prepared in Preparation Example 5 Antioxidant (Fa1): Product name "SumiLizer® GP" manufactured by Sumitomo Chemical Co., Ltd. Leveling agent (H1): Polyether-modified silicone oil (product name "Toray Silicone SH8400" manufactured by Toray Dow Corning Co., Ltd.)
[0273]
[0274] Solvent (J1): PGMEA (Propylene glycol monomethyl ether acetate)
[0275] Table 2 shows the results of process resistance measurements for curable compositions 1 to 12, as measured according to (3) above.
[0276]
Claims
1. A curable composition comprising semiconductor particles (A) and a polymerizable compound (D), wherein the semiconductor particles (A) contain an organic ligand (G), and the weight loss ratio X above 300°C, calculated by formula (1) when the semiconductor particles (A) containing the organic ligand (G) are heated from 25°C to 600°C in a nitrogen atmosphere at a heating rate of 10°C / min by thermogravimetric analysis, is 35% or less, and the clogP of the polymerizable compound (D) is 3.5 or more. Weight loss ratio above 300°C X (%) = {T1 / (T0+T1)} × 100 …(1) [In formula (1), T 0 This is the weight loss rate from 100°C to 300°C, with the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C as the reference weight, and T 1 This is the weight loss rate from 300°C to 600°C, relative to the weight of the semiconductor particle (A) containing the organic ligand (G) at 100°C.
2. The curable composition according to claim 1, further comprising resin (C).
3. The curable composition according to claim 1 or 2, further comprising a light scattering agent (B).
4. The curable composition according to claim 1 or 2, wherein the weight loss ratio X at 300°C or higher is 5 to 25%, and the clogP of the polymerizable compound (D) is 3.8 to 7.
0.
5. A cured film formed from the curable composition according to claim 1 or 2.
6. A display device comprising the cured film according to claim 5.