Non-aqueous electrolyte and lithium secondary battery comprising same

By controlling the ratios and contents of organic solvents in the electrolyte, the electrolyte composition maintains lithium ion mobility and reduces resistance, improving battery performance across temperature variations.

WO2026235341A1PCT designated stage Publication Date: 2026-11-12LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/005838
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-04-28
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Lithium secondary batteries face performance degradation due to changes in lithium ion mobility and increased resistance at high or low temperatures, primarily due to the composition of the organic solvent in the electrolyte, affecting lifespan and charge/discharge performance.

Method used

The electrolyte composition is controlled by specific ratios and contents of cyclic and linear carbonate-based organic solvents, along with methyl acetate, to maintain lithium ion mobility and reduce resistance across varying temperatures.

Benefits of technology

The controlled electrolyte composition enhances battery lifespan and rapid charge/discharge performance by ensuring excellent ionic conductivity and stability at both high and low temperatures.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a non-aqueous electrolyte comprising: a lithium salt; and an organic solvent, wherein the organic solvent comprises a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent, and methyl acetate, the cyclic carbonate-based organic solvent comprises ethylene carbonate, the linear carbonate-based organic solvent comprises dimethyl carbonate and ethyl methyl carbonate, the volume ratio of the ethyl methyl carbonate to the dimethyl carbonate is 1:3 to 1:11, and the non-aqueous electrolyte satisfies the following formula 1. [Formula 1] 0.20 ≤ VDMC / (VMA + VEC) ≤ 1.65 (VDMC is a volume percentage (unit: vol%) of dimethyl carbonate relative to the volume of the organic solvent, VEC is a volume percentage (unit: vol%) of ethylene carbonate relative to the volume of the organic solvent, and VMA is a volume percentage (unit: vol%) of methyl acetate relative to the volume of the organic solvent.)
Need to check novelty before this filing date? Find Prior Art

Description

Non-aqueous electrolyte and lithium secondary battery containing the same

[0001] The present invention relates to a non-aqueous electrolyte and a lithium secondary battery containing the same.

[0002]

[0003] Recently, as the application areas of lithium-ion batteries have rapidly expanded to include not only power supply for electronic devices such as electrical, electronic, telecommunications, and computers, but also power storage for large-area devices such as automobiles and power storage systems, there is a growing demand for high-capacity, high-output, and high-stability secondary batteries.

[0004] In particular, with the growing interest in solving environmental problems and realizing a sustainable circular society, research on energy storage devices such as lithium-ion batteries and electric double-layer capacitors is being conducted extensively. Among these, lithium-ion batteries are receiving attention as battery systems that theoretically have the highest energy density within battery technology.

[0005] The aforementioned lithium secondary battery is largely composed of a positive electrode made of a transition metal oxide containing lithium, a negative electrode capable of storing lithium, an electrolyte that acts as a medium for transporting lithium ions, and a separator. Among these components, the electrolyte is known to have a significant impact on the battery's stability and safety, and as such, extensive research is being conducted on it.

[0006] In this regard, the electrolyte of a lithium secondary battery is generally a non-aqueous electrolyte containing lithium salts, organic solvents, etc., and the organic solvent used is a carbonate-based organic solvent. At this time, the freezing point, viscosity characteristics, and capacity characteristics of the electrolyte containing it may vary depending on the form and content of the compounds in the carbonate-based organic solvent. Meanwhile, the physical properties of the electrolyte can affect the battery's lifespan performance and output characteristics in relation to the operating temperature of the lithium secondary battery. For example, if a lithium secondary battery is exposed to high temperatures, decomposition of the materials constituting the electrolyte occurs, and the performance of the electrolyte may deteriorate due to the by-products generated as a result, and the resistance of the lithium secondary battery may increase. As another example, if a lithium secondary battery using an organic solvent with a high freezing point is operated in a low-temperature environment, the mobility characteristics of lithium ions within the electrolyte are poor, which may result in poor output characteristics and rapid charge / discharge performance of the lithium secondary battery.

[0007]

[0008] One objective of the present invention is to solve the above-mentioned problems by controlling the composition of the organic solvent included in the electrolyte so that the lithium ion mobility characteristics are not degraded even when the environment in which the lithium secondary battery is operated is high or low temperature, thereby providing a non-aqueous electrolyte with excellent battery life characteristics and reduced increase in resistance, resulting in excellent rapid charge / discharge performance.

[0009] In addition, another objective of the present invention is to provide a lithium secondary battery comprising the aforementioned non-aqueous electrolyte.

[0010]

[0011] [1] The present invention provides a non-aqueous electrolyte comprising a lithium salt; and an organic solvent; wherein the organic solvent comprises a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent and methyl acetate, wherein the cyclic carbonate-based organic solvent comprises ethylene carbonate, and the linear carbonate-based organic solvent comprises dimethyl carbonate and ethylmethyl carbonate, and the volume ratio of ethylmethyl carbonate and dimethyl carbonate is 1:3 to 1:11, and satisfies Formula 1 below.

[0012] [Equation 1]

[0013] 0.20 ≤ V DMC / (V MA + V EC ) ≤ 1.65

[0014] In the above Equation 1, V DMC is the volume percentage of the organic solvent volume of dimethyl carbonate (unit: volume%), V EC is the volume percentage of the organic solvent volume of ethylene carbonate (unit: volume%), V MA is the volume percentage (unit: volume%) of the organic solvent volume of methyl acetate.

[0015] [2] In the above [1], the ethylene carbonate may be included in the organic solvent in an amount of 20 volume% to 40 volume%.

[0016] [3] In one or more of [1] and [2] above, the organic solvent may satisfy Formula 2 below.

[0017] [Equation 2]

[0018] 0.25 ≤ V MA / V EC ≤ 1.50

[0019] In Equation 2 above, V EC is the volume percentage of the organic solvent volume of ethylene carbonate (unit: volume%), V MAis the volume percentage (unit: volume%) of the organic solvent volume of methyl acetate.

[0020] [4] In one or more of [1] to [3] above, the organic solvent may satisfy Formula 3 below.

[0021] [Equation 3]

[0022] 0.70 ≤ V DMC / V EC ≤ 2.00

[0023] In Equation 3 above, V DMC is the volume percentage of the organic solvent volume of dimethyl carbonate (unit: volume%), V EC is the volume percentage (unit: volume%) of the organic solvent volume of ethylene carbonate.

[0024] [5] In one or more of [1] to [4] above, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO2, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 It may include at least one selected from the group consisting of LiB(C2O4)2, LiCF3SO3, LiN(SO2F)2, LiCH3SO3, LiCF3CO2, LiCH3CO2, LiN(SO2CF3)2 and LiN(SO2CF2CF3)2.

[0025] [6] In the above [5], the lithium salt may include LiPF6 and LiN(SO2F)2.

[0026] [7] In one or more of [1] to [6] above, the linear carbonate-based organic solvent may be included in an amount of 20% to 67% by volume relative to 100% by volume of the organic solvent.

[0027] [8] In one or more of [1] to [7] above, the methyl acetate may be included in an amount of 5 to 45 volume% with respect to 100 volume% of the organic solvent.

[0028]

[0029] [9] According to another embodiment of the present invention, an electrode assembly comprising a positive electrode, a negative electrode opposite to the positive electrode, and a separator interposed between the positive electrode and the negative electrode; a non-aqueous electrolyte according to [1] above; and a battery case accommodating the electrode assembly and the non-aqueous electrolyte is provided.

[0030]

[0010] In the above [9], the cathode comprises a cathode active material layer, the cathode active material layer comprises a cathode active material, and the cathode active material may comprise a silicon-based active material.

[0031]

[0011] In the above

[0010] , the silicon-based active material is silicon (Si) and silicon oxide (SiO₂). x , 0 <x<2), 실리콘-금속 합금(Si-metal alloy) 및 실리콘-탄소 복합체(Si / C composite)로 이루어진 군에서 선택된 적어도 1종을 포함할 수 있다.

[0032]

[0012] In the above

[0010] and / or

[0011] , the silicon-based active material may be included in an amount of 0.1% to 30% by weight relative to 100% by weight of the negative electrode active material layer.

[0033]

[0013] In one or more of the above

[0010] to

[0012] , the battery case may be cylindrical or rectangular.

[0034]

[0035] The non-aqueous electrolyte according to the present invention is characterized by the fact that the content of a linear carbonate-based organic solvent containing dimethyl carbonate, a cyclic carbonate-based organic solvent containing ethylene carbonate, and methyl acetate in the organic solvent is controlled to satisfy a specific relationship, and the volume ratio of ethylmethyl carbonate and dimethyl carbonate contained in the linear carbonate-based organic solvent is controlled. Through the control of the content and ratio, the non-aqueous electrolyte exhibits excellent ionic conductivity even at high and low temperatures, which is desirable as it can improve the lifespan characteristics and rapid charge / discharge performance of the lithium secondary battery.

[0036]

[0037] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0038] In this specification, terms such as “comprising,” “comprising,” or “having” are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not excluding in advance the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0039]

[0040] The present invention will be described in detail below.

[0041] The non-aqueous electrolyte according to the present invention and the lithium secondary battery including the same comprise at least one of the configurations disclosed below, and may comprise any combination of technically feasible configurations among the configurations below.

[0042]

[0043] Non-aqueous electrolytes

[0044] The present invention relates to a non-aqueous electrolyte. More specifically, the non-aqueous electrolyte may be a non-aqueous electrolyte for a lithium secondary battery.

[0045] The non-aqueous electrolyte according to the present invention comprises a lithium salt; and an organic solvent; wherein the organic solvent comprises a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent, and methyl acetate, wherein the cyclic carbonate-based organic solvent comprises ethylene carbonate, and the linear carbonate-based organic solvent comprises dimethyl carbonate and ethylmethyl carbonate, and wherein the volume ratio of ethylmethyl carbonate and dimethyl carbonate included in the linear carbonate-based organic solvent is controlled to a specific level while satisfying Formula 1 below.

[0046] [Equation 1]

[0047] 0.20 ≤ V DMC / (V MA + V EC ) ≤ 1.65

[0048] In the above Equation 1, V DMC is the volume percentage of the organic solvent volume of dimethyl carbonate (unit: volume%), V EC is the volume percentage of the organic solvent volume of ethylene carbonate (unit: volume%), V MA is the volume percentage (unit: volume%) of the organic solvent volume of methyl acetate.

[0049] The non-aqueous electrolyte of the present invention is characterized by the fact that the content of a linear carbonate-based organic solvent containing dimethyl carbonate and ethyl methyl carbonate, a cyclic carbonate-based organic solvent containing ethylene carbonate, and methyl acetate in an organic solvent is controlled to satisfy a specific relationship (Equation 1), and the volume ratio of ethyl methyl carbonate and dimethyl carbonate contained in the linear carbonate-based organic solvent is controlled. Through the control of the content and ratio, the non-aqueous electrolyte exhibits excellent ionic conductivity even at high and low temperatures, which is desirable as it can improve the lifespan characteristics and rapid charge / discharge performance of the lithium secondary battery.

[0050]

[0051] (1) Lithium salt

[0052] As the lithium salt used in the present invention, various lithium salts commonly used in non-aqueous electrolytes for lithium secondary batteries may be used without limitation. For example, the lithium salt is Li as a cation. + It includes, and as anion, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , AlO4 - , AlCl4 - , PF6 - , SbF6 - , AsF6 - , B 10 Cl 10 - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P -, CF3SO3 - , C4F9SO3 - , CF3CF2SO3 - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CH3SO3 - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It may include at least one selected from a group consisting of

[0053] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO2, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 , may include at least one selected from the group consisting of LiB(C2O4)2, LiCF3SO3, LiN(SO2F)2 (lithium bis(fluorosulfonyl)imide; LiFSI), LiCH3SO3, LiCF3CO2, LiCH3CO2, LiN(SO2CF3)2 (lithium bis(trifluoromethanesulfonyl)imide; LiTFSI), and LiN(SO2CF2CF3)2 (lithium bis(perfluoroethanesulfonyl)imide; LiBETI). Specifically, the lithium salt may include LiBF4, LiClO4, LiPF6, LiBOB (LiB(C2O4)2), LiCF3SO3, LiN(SO2CF3)2, and LiN(SO2F). 2, It may include at least one selected from the group consisting of (LiFSI) and LiBETI (LiN(SO2CF2CF3)2). More specifically, the lithium salt may include LiPF6 and LiN(SO2F)2.

[0054] The above lithium salt may be included in the above-mentioned non-aqueous electrolyte at a concentration of 0.01M to 5M, specifically 0.05M to 3M, and more specifically 0.1M to 2.0M. When the concentration of the above-mentioned lithium salt satisfies the above range, the lithium ion yield (Li + The transference number and the degree of dissociation of lithium ions are improved, which can enhance the output characteristics of the battery.

[0055]

[0056] (2) Organic solvent

[0057] The organic solvent according to the present invention comprises a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent, and methyl acetate, wherein the cyclic carbonate-based organic solvent comprises ethylene carbonate, and the linear carbonate-based organic solvent comprises dimethyl carbonate and ethylmethyl carbonate, and the volume ratio of ethylmethyl carbonate and dimethyl carbonate included in the linear carbonate-based organic solvent is controlled to a specific level while satisfying the following Formula 1.

[0058] [Equation 1]

[0059] 0.20 ≤ V DMC / (V MA + V EC ) ≤ 1.65

[0060] In the above Equation 1, V DMC is the volume percentage of the organic solvent volume of dimethyl carbonate (unit: volume%), V EC is the volume percentage of the organic solvent volume of ethylene carbonate (unit: volume%), V MA is the volume percentage (unit: volume%) of the organic solvent volume of methyl acetate.

[0061] The organic solvent according to the present invention is an organic solvent capable of preventing degradation of lifespan performance even in various operating environments ranging from low to high temperatures, while ensuring output performance. By comprehensively considering the performance of each compound and the difficulties associated with excess or deficiency, the invention proposes a combination characteristic of the organic solvent that can take advantage of both the lifespan performance and output performance of the organic solvent.

[0062] In this regard, each of the specific types of compounds included in the organic solvent according to the present invention will be described first.

[0063] The organic solvent according to the present invention includes a cyclic carbonate-based organic solvent.

[0064] In addition, the above-mentioned cyclic carbonate-based organic solvent includes ethylene carbonate.

[0065] The above ethylene carbonate can be preferably used in terms of dissociating lithium salts and improving the mobility of lithium ions. In addition, the ethylene carbonate can improve the stability of the film formed on the surfaces of the cathode and anode, thereby contributing to the improvement of the battery's lifespan performance.

[0066] The organic solvent of the present invention may contain ethylene carbonate in an amount of 20 volume% or more, 22 volume% or more, 24 volume% or more, 25 volume% or more, 26 volume% or more, 27 volume% or more, 28 volume% or more, or 29 volume% or more. The organic solvent according to the present invention may contain ethylene carbonate in an amount of 40 volume% or less, 38 volume% or less, 36 volume% or less, 35 volume% or less, 34 volume% or less, 33 volume% or less, 32 volume% or less, or 31 volume% or less. The above numerical ranges may be combined with one another without limitation. Specifically, the organic solvent according to the present invention may contain ethylene carbonate in an amount of 20 volume% to 40 volume%. Specifically, the organic solvent according to the present invention may contain ethylene carbonate in an amount of 22 volume% to 38 volume%, more specifically 24 volume% to 36 volume%, and even more specifically 26 volume% to 34 volume%. Satisfying the above range is desirable in that it ensures the mobility of lithium ions in the organic solvent while simultaneously preventing an excessive increase in viscosity.

[0067] The above-mentioned cyclic carbonate-based organic solvent may further include at least one selected from the group consisting of fluoroethylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate.

[0068] Meanwhile, the above-mentioned cyclic carbonate-based organic solvent may not contain fluoroethylene carbonate (FEC). Fluoroethylene carbonate can cause a side reaction that generates hydrogen fluoride (HF) by reacting with moisture, and if included in excessive amounts, the stability of the SEI membrane may be reduced. Therefore, it is preferable to add fluoroethylene carbonate in small amounts even if it is added to the organic solvent.

[0069] Meanwhile, the above-mentioned cyclic carbonate-based organic solvent may not contain propylene carbonate (PC). This is because propylene carbonate can cause co-intercalation, a phenomenon in which it is simultaneously inserted into the negative electrode along with lithium ions during the charging and discharging process of the battery, which can lead to problems such as the promotion of dendrite formation or the unstable formation of the SEI film. Therefore, it is desirable to add a small amount of propylene carbonate to the organic solvent.

[0070] The organic solvent according to the present invention includes a linear carbonate-based organic solvent.

[0071] In addition, the linear carbonate-based organic solvent includes dimethyl carbonate and ethylmethyl carbonate.

[0072] The above-mentioned dimethyl carbonate is a solvent having low viscosity and low dielectric constant, and can be included for controlling the viscosity of organic solvents. Additionally, dimethyl carbonate is desirable in that it can improve oxidation stability during operation in high-voltage environments due to the high oxidation potential of the organic solvent, and contribute to reducing manufacturing costs.

[0073] The above-mentioned ethyl methyl carbonate has a relatively low freezing point, which has the effect of lowering the freezing point of the entire organic solvent, thereby preventing the degradation of lithium ion mobility characteristics even when the battery operating environment is at a low temperature. In addition, the above-mentioned ethyl methyl carbonate is a solvent with low viscosity characteristics; when used in combination with an organic solvent having a high dielectric constant, such as ethylene carbonate, it contributes to preventing the decomposition of the electrolyte at high temperatures, thereby improving stability. Furthermore, the above-mentioned ethyl methyl carbonate has excellent reactivity with the anode and cathode, allowing for the formation of a stable interface when forming the SEI film, and also has excellent compatibility with other types of solvents, providing flexibility in designing the electrolyte composition.

[0074] The organic solvent according to the present invention may contain dimethyl carbonate in an amount of 20 volume% or more, 21 volume% or more, 22 volume% or more, 23 volume% or more, 25 volume% or more, 27 volume% or more, 31 volume% or more, 33 volume% or more, or 34 volume% or more. The organic solvent according to the present invention may contain dimethyl carbonate in an amount of 65 volume% or less, 64 volume% or less, 62 volume% or less, 60 volume% or less, 58 volume% or less, or 56 volume% or less. The above numerical ranges may be combined with one another without limitation. Specifically, the organic solvent according to the present invention may contain dimethyl carbonate in an amount of 20 volume% to 65 volume%, specifically 21 volume% to 64 volume%, more specifically 22 volume% to 62 volume%, and even more specifically 23 volume% to 60 volume%. If the above range is satisfied, it may be desirable in terms of controlling the viscosity of the organic solvent and improving oxidation stability.

[0075] The organic solvent according to the present invention may contain ethyl methyl carbonate in an amount of 0.5 volume% or more, 1 volume% or more, 1.5 volume% or more, 2.0 volume% or more, 2.5 volume% or more, 3.0 volume% or more, 3.5 volume% or more, 4.0 volume% or more, or 4.5 volume% or more. The organic solvent according to the present invention may contain ethyl methyl carbonate in an amount of 20 volume% or less, 15 volume% or less, 12 volume% or less, 10 volume% or less, 9 volume% or less, 8 volume% or less, 7 volume% or less, or 6 volume% or less. The above numerical ranges may be combined without limitation. Specifically, the organic solvent according to the present invention may contain ethyl methyl carbonate in an amount of 0.5 volume% to 20 volume%, specifically 1 volume% to 15 volume%, and more specifically 2 volume% to 10 volume%. If the above range is satisfied, the stability of the organic solvent in a low-temperature operating environment can be improved.

[0076] The above linear carbonate-based organic solvent is an organic solvent having low viscosity and low dielectric constant, and may further include at least one selected from the group consisting of diethyl carbonate (DEC), dipropyl carbonate (DPC), ethylmethyl carbonate (EMC), methylpropyl carbonate (MPC), and ethylpropyl carbonate (EPC).

[0077] The linear carbonate-based organic solvent according to the present invention may be included in an amount of 20 volume% or more, 22 volume% or more, 24 volume% or more, 26 volume% or more, 28 volume% or more, 29 volume% or more, 30 volume% or more, 32 volume% or more, 34 volume% or more, 35 volume% or more, 38 volume% or more, or 39 volume% or more, based on 100 volume% of the organic solvent. The linear carbonate-based organic solvent according to the present invention may be included in an amount of 67 volume% or less, 65 volume% or less, 64 volume% or less, 63 volume% or less, 62 volume% or less, or 61 volume% or less, based on 100 volume% of the organic solvent. The above numerical ranges may be combined without limitation. Specifically, the linear carbonate-based organic solvent according to the present invention may be included in an amount of 20 to 67 volume%, specifically 22 to 65 volume%, more specifically 24 to 63 volume%, even more specifically 29 to 63 volume%, and even more specifically 35 to 62 volume%, based on 100 volume% of the organic solvent. When the content of the linear carbonate-based organic solvent included in the organic solvent satisfies the above range, it is possible to realize a non-aqueous electrolyte having excellent oxidation stability while appropriately controlling the viscosity of the organic solvent. For example, the linear carbonate-based organic solvent may be included as the remainder after excluding the volume of the cyclic carbonate-based organic solvent and methyl acetate from the organic solvent.

[0078] The above organic solvent includes methyl acetate.

[0079] The above methyl acetate is a low-viscosity solvent that can contribute to improving the mobility of lithium ions. It has a low freezing point, which has the effect of lowering the freezing point of the entire organic solvent, thereby preventing the degradation of lithium ion mobility characteristics even when the battery is operated in a low-temperature environment. In addition, methyl acetate can improve the lifespan performance of the battery by suppressing side reactions between the anode and the electrolyte through the formation of a stable SEI film on the surface of the anode.

[0080] Meanwhile, since methyl acetate can vaporize at a relatively low temperature due to its low boiling point, it may be preferable for the battery case into which the non-aqueous electrolyte containing an organic solvent containing methyl acetate is injected to be cylindrical or prismatic.

[0081] The above methyl acetate may be included in an amount of 5 vol% or more, 6 vol% or more, 7 vol% or more, 8 vol% or more, or 9 vol% or more with respect to 100 vol% of the organic solvent. The above methyl acetate may be included in an amount of 45 vol% or less, 43 vol% or less, 42 vol% or less, 41 vol% or less, 40 vol% or less, 38 vol% or less, 35 vol% or less, 33 vol% or less, 32 vol% or less, or 31 vol% or less with respect to 100 vol% of the organic solvent. The above numerical ranges may be combined with one another without limitation. Specifically, the methyl acetate may be included in an amount of 5 to 45 volume%, specifically 7 to 43 volume%, more specifically 8 to 42 volume%, even more specifically 9 to 41 volume%, and even more specifically 9 to 35 volume% with respect to 100 volume% of the organic solvent. When the content of methyl acetate included in the organic solvent satisfies the above range, the output characteristics at low temperatures and rapid charge / discharge performance of the lithium secondary battery can be improved to a desirable level without the viscosity of the non-aqueous electrolyte becoming too high.

[0082] The organic solvent according to the present invention satisfies Formula 1 below.

[0083] [Equation 1]

[0084] 0.20 ≤ V DMC / (V MA + V EC ) ≤ 1.65

[0085] In the above Equation 1, V DMC is the volume percentage of the organic solvent volume of dimethyl carbonate (unit: volume%), V EC is the volume percentage of the organic solvent volume of ethylene carbonate (unit: volume%), V MA is the volume percentage (unit: volume%) of the organic solvent volume of methyl acetate.

[0086] Satisfying the above Equation 1 means that dimethyl carbonate, ethylene carbonate, and methyl acetate contained in the organic solvent are included in a specific amount and satisfy a specific ratio. Specifically, if the content of dimethyl carbonate, ethylene carbonate, and methyl acetate contained in the organic solvent satisfies the above Equation 1, the lifespan performance and output performance at low to high temperatures can be improved.

[0087] The above V DMC / (V MA + V EC If the value of ) is less than 0.20, dimethyl carbonate is used in small quantities compared to ethylene carbonate and methyl acetate for viscosity control and oxidation stability improvement. This can lead to an increase in the viscosity of the non-aqueous electrolyte and a thickening of the SEI (Solid Electrolyte Interphase Layer) formed on the cathode surface, which may reduce lithium ion mobility. Consequently, this can degrade the battery's charge / discharge performance, leading to a decrease in lifespan. Additionally, ethylene carbonate may undergo side reactions with lithium ions at high temperatures, which can further degrade the battery's lifespan. Conversely, the above V DMC / (V MA + VEC If the value of ) exceeds 1.65, the dissociation of lithium salts does not proceed smoothly due to the insufficient addition of methyl acetate and ethylene carbonate relative to dimethyl carbonate, which may lead to a decrease in output performance. Additionally, the stability of the SEI film formed on the negative electrode surface may be reduced, resulting in a decrease in lifespan performance, and the output characteristics of the lithium secondary battery may deteriorate when operating in a low-temperature environment. Accordingly, the above V DMC / (V MA + V EC The value of ) may preferably be 0.22 or higher, 0.24 or higher, 0.26 or higher, 0.28 or higher, 0.30 or higher, 0.32 or higher, or 0.33 or higher. The above V DMC / (V MA + V EC The value of ) may be 1.60 or less, 1.55 or less, 1.50 or less, 1.45 or less, 1.43 or less, 1.41 or less, or 1.40 or less. The above numerical ranges may be combined with one another without limitation. For example, the above V DMC / (V MA + V EC ) may be 0.22 or more and 1.60 or less, specifically 0.24 or more and 1.55 or less, more specifically 0.26 or more and 1.50 or less.

[0088] Meanwhile, the lifespan performance and output performance improvement effect resulting from satisfying the above Equation 1 may be an effect that is manifested when the ratio of the volume of dimethyl carbonate to the volume of ethylmethyl carbonate is controlled to a specific level.

[0089] Specifically, the volume ratio of the ethylmethyl carbonate and dimethyl carbonate is 1:3 to 1:11. If the ratio of the volume of dimethyl carbonate to the volume of ethylmethyl carbonate is less than 3, the composition of the solvent deviates from the ability to stabilize the solvation structure of lithium ions in room temperature and high temperature environments, which may lead to a decrease in lithium ion mobility characteristics and disadvantages in terms of viscosity and interfacial stability with electrodes, resulting in a decrease in lifespan performance at room temperature and high temperature. Conversely, if the ratio of the volume of dimethyl carbonate to the volume of ethylmethyl carbonate exceeds 11, the dielectric properties of the organic solvent are difficult to maintain at low temperatures due to the relative excess of dimethyl carbonate. Consequently, the stability of the SEI film at the electrode interface is weakened, which may lead to a rapid decrease in lifespan and output performance at low temperatures.

[0090] The volume ratio of the ethylmethyl carbonate and dimethyl carbonate may specifically be 1:3.5 to 1:11, more specifically 1:5 to 1:11, and even more specifically 1:7 to 1:11. When the above range is satisfied, the dielectric constant of the electrolyte can be secured, and the decrease in the mobility of lithium ions can be prevented.

[0091] According to one embodiment of the present invention, the organic solvent may satisfy Formula 2 below.

[0092] [Equation 2]

[0093] 0.25 ≤ V MA / V EC ≤ 1.50

[0094] In Equation 2 above, V EC is the volume percentage of the organic solvent volume of ethylene carbonate (unit: volume%), V MA is the volume percentage (unit: volume%) of the organic solvent volume of methyl acetate.

[0095] V of the organic solvent according to the present invention MA / V EC The value may be 0.25 or higher, 0.27 or higher, 0.29 or higher, 0.30 or higher, 0.31 or higher, or 0.32 or higher. V of the organic solvent according to the present invention MA / V EC The value may be 1.50 or less, 1.47 or less, 1.45 or less, 1.43 or less, 1.41 or less, 1.39 or less, 1.37 or less, or 1.35 or less. The above numerical ranges may be combined with one another without limitation. For example, V of the organic solvent according to the present invention MA / V EC The value may be 0.25 or higher and 1.50 or lower, specifically 0.27 or higher and 1.47 or lower, more specifically 0.29 or higher and 1.45 or lower, and even more specifically 0.31 or higher and 1.39 or lower. When within the above range, the viscosity of the organic solvent is prevented from rising excessively without reducing the degree of dissociation of the lithium salt, thereby providing excellent rapid charge and discharge performance at high and low temperatures of the battery and improving lifespan performance.

[0096] According to one embodiment of the present invention, the organic solvent may satisfy Formula 3 below.

[0097] [Equation 3]

[0098] 0.70 ≤ V DMC / V EC ≤ 2.00

[0099] In Equation 3 above, V DMC is the volume percentage of the organic solvent volume of dimethyl carbonate (unit: volume%), V EC is the volume percentage (unit: volume%) of the organic solvent volume of ethylene carbonate.

[0100] V of the organic solvent according to the present invention DMC / V ECThe value of may be 0.70 or higher, 0.72 or higher, 0.74 or higher, 0.76 or higher, 0.78 or higher, 0.80 or higher, or 0.82 or higher. V of the organic solvent according to the present invention DMC / V EC The value of may be 2.00 or less, 1.97 or less, 1.94 or less, 1.92 or less, 1.90 or less, 1.88 or less, 1.86 or less, or 1.84 or less. The above numerical ranges may be combined with one another without limitation. For example, V of the organic solvent according to the present invention DMC / V EC The value of may be 0.70 or more and 2.00 or less, specifically 0.72 or more and 1.97 or less, more specifically 0.74 or more and 1.94 or less, and even more specifically 0.80 or more and 1.88 or less. The above V DMC / V EC If the value of is less than 0.70, the viscosity of the non-aqueous electrolyte increases, reducing the mobility of lithium ions, which may degrade the charge / discharge performance of the battery and reduce stability at high temperatures. The above V DMC / V EC If the value of is greater than 2.00, the dissociation of the lithium salt may not occur properly, the stability of the SEI film formed on the cathode surface may be reduced, and low-temperature output characteristics may be reduced.

[0101] Meanwhile, the above organic solvent may be used without limitation by adding organic solvents commonly used in non-aqueous electrolytes as needed. For example, the above organic solvent may additionally include at least one organic solvent selected from linear ester-based organic solvents, cyclic ester-based organic solvents, ether-based organic solvents, glycine-based solvents, and nitrile-based organic solvents.

[0102] The above linear ester-based organic solvent may specifically include at least one selected from the group consisting of ethyl acetate or propyl acetate. Meanwhile, linear ester-based organic solvents such as ethyl propionate may not be included or at least added in small amounts, as they have a low dielectric constant and may hinder the dissociation of the lithium salt.

[0103] In addition, the above-mentioned cyclic ester-based organic solvent may specifically include at least one selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.

[0104] As the above ether-based solvent, any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methylpropyl ether, ethyl propyl ether, 1,3-dioxolane (DOL), and 2,2-bis(trifluoromethyl)-1,3-dioxolane (TFDOL), or a mixture of two or more of these may be used, but is not limited thereto.

[0105] The above-mentioned glyme-based solvent has a high dielectric constant and low surface tension compared to linear carbonate-based organic solvents and is a solvent with low reactivity with metals. It may include at least one selected from the group consisting of dimethoxyethane (glyme, DME), diethoxyethane, diglyme, triglyme, and tetraglyme (TEGDME), but is not limited thereto.

[0106] The above nitrile-based solvent may be one or more selected from the group consisting of acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanitrile, cyclopentane carbonitrile, cyclohexane carbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, but is not limited thereto.

[0107]

[0108] (3) Additives

[0109] The above-mentioned non-aqueous electrolyte may further include additives along with the lithium salt and organic solvent described above.

[0110] The above additive may be included in the non-aqueous electrolyte to prevent the decomposition of the non-aqueous electrolyte in a high-power environment from causing cathode collapse, or to provide low-temperature high-rate discharge characteristics, high-temperature stability, prevention of overcharging, and suppression of battery expansion at high temperatures.

[0111] Specifically, the additive comprises lithium difluorophosphate (LiDFP), methyl propagyl carbonate, vinylene carbonate, vinylethylene carbonate, fluoroethylene carbonate, propane sultone, propene sultone, succinonitrile, succinic anhydride, adiponitrile, ethylene sulfate, LiBOB (Lithium bis-(oxalato)borate), LiBF4 (Lithium tetrafluoroborate), LiDFOB (Lithium difluoro(oxalato)borate), LiDFOP (Lithium difluoro bis(oxalato) phosphate), TMSPa (Tris(trimethylsilyl) phosphate), and It may include at least one selected from the group consisting of TMSPi (Tris(trimethylsilyl) Phosphite).

[0112] The above additive may be included in the above non-aqueous electrolyte in an amount of 0.1% to 15% by weight, more specifically, 0.3% to 12% by weight, and more specifically, 0.5% to 10% by weight.

[0113]

[0114] lithium secondary battery

[0115] In addition, the present invention provides a lithium secondary battery comprising the aforementioned non-aqueous electrolyte.

[0116] Specifically, the lithium secondary battery comprises: an electrode assembly including a positive electrode, a negative electrode facing the positive electrode, and a separator interposed between the positive electrode and the negative electrode; the aforementioned non-aqueous electrolyte; and a battery case accommodating the electrode assembly and the non-aqueous electrolyte.

[0117] As the description of the non-aqueous electrolyte has been provided above, it will be described below in the electrode assembly and battery case.

[0118]

[0119] (1) Electrode assembly

[0120] The electrode assembly can be inserted into a battery case and, after injecting the aforementioned non-aqueous electrolyte, sealed by the battery case.

[0121] The electrode assembly may include an anode, a cathode facing the anode, and a separator interposed between the anode and the cathode. For example, the electrode assembly may be formed by sequentially stacking an anode, a separator, and a cathode.

[0122] Types of electrode assemblies may include stack type, jelly roll type, stack and folding type, etc., but are not limited thereto.

[0123]

[0124] The anode, cathode, and separator are described in more detail below.

[0125]

[0126] anode

[0127] The above anode may include an anode active material.

[0128] The above-mentioned cathode active material is a compound capable of reversible intercalation and deintercalation, and is not particularly limited as long as it is a cathode active material used in the field. Specifically, the above-mentioned cathode active material is a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; lithium iron phosphate such as LiFePO4; and a compound with the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4 (0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7, etc.; chemical formula LiNi 1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, satisfying 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3 Lithium manganese composite oxides represented by O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, satisfying 0.01≤c3≤0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn); etc., but are not limited to these. The anode may also be a Li-metal anode.

[0129] More specifically, the positive electrode active material may include at least one selected from the group consisting of lithium cobalt oxide (LiCoO2), high-nickel lithium nickel-cobalt-manganese oxide, over-lithium manganese-rich oxide, and lithium iron phosphate.

[0130] The above high-nickel containing lithium nickel-cobalt-manganese oxide can be represented by the following chemical formula A.

[0131] [Chemical Formula A]

[0132] Li 1+x (Ni a Co b Mn c M d )O2

[0133] In the above chemical formula A, M is one or more selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and 1+x, a, b, c, and d are each atomic fractions of independent elements, where -0.2≤x≤0.2, 0.50≤a<1, 0 <b≤0.25, 0<c≤0.25, 0≤d≤0.1, a+b+c+d=1이다. 바람직하게는, 상기 a, b, c 및 d는 각각 0.70≤a≤0.95, 0.025≤b≤0.20, 0.025≤c≤0.20, 0≤d≤0.05일 수 있다. 또한, 상기 a, b, c 및 d는 각각 0.80≤a≤0.95, 0.025≤b≤0.15, 0.025≤c≤0.15, 0≤d≤0.05일 수 있다. 또한, 상기 a, b, c 및 d는 각각 0.85≤a≤0.90, 0.05≤b≤0.10, 0.05≤c≤0.10, 0≤d≤0.03일 수 있다.

[0134] The above-mentioned lithium manganese-rich oxide may include a compound represented by the following chemical formula B.

[0135] [Chemical Formula B]

[0136] Li 1+s [Ni t Co u Mn v M 1 w ]O 2+z

[0137] In the above chemical formula B, M 1... is one or more selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and 0.05≤s≤1, 0≤t≤0.5, 0≤u≤0.3, 0.5≤v<1.0, 0≤w≤0.2, 0≤z≤1. Preferably, in the above formula B, 0.05≤s≤1.0, 0.1≤t≤0.5, 0≤u≤0.1, 0.5≤v<1.0, 0≤w≤0.2, 0≤z≤1. More preferably, in the above formula B, 0.10≤s≤0.50, 0.1≤t≤0.5, 0≤u≤0.1, 0.6≤v<1.0, 0≤w≤0.1, and 0≤z≤0.50.

[0138] The above lithium iron phosphate may include a compound represented by the following chemical formula C.

[0139] [Chemical Formula C]

[0140] Li 1+e Fe 1-g M 2 g (PO 4-f )X f

[0141] In the above chemical formula C, M 2 is one or more elements selected from Co, Ni, Mn, Al, Mg, Ti, and V, X is F, S, or N, and 0≤g≤0.5; -0.5≤e≤+0.5; 0≤f≤0.1. The above chemical formula C can specifically be represented as LiFePO4 (g=0, e=0, and f=0).

[0142] The above positive electrode may include a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector.

[0143] The above positive current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. Specifically, the above positive current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, and aluminum-cadmium alloy, preferably aluminum.

[0144] The thickness of the above positive current collector can typically be 3㎛ to 500㎛, specifically 5㎛ to 50㎛.

[0145] The above positive current collector may form fine irregularities on its surface to strengthen the bonding force of the positive active material. For example, the above positive current collector can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0146] The positive active material layer may be disposed on at least one surface of the positive current collector. Specifically, the positive active material layer may be disposed on one or both surfaces of the positive current collector.

[0147] The above positive active material layer may include the aforementioned positive active material.

[0148] The above positive active material may be included in the above positive active material layer in an amount of 80% to 99% by weight, specifically 85% to 98% by weight.

[0149] The above positive active material layer may optionally further include a binder and / or a conductive material together with the aforementioned positive active material.

[0150] The above binder is a component that assists in the binding of active materials and conductive materials, and in binding to current collectors, and specifically may include at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene ter polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber, preferably polyvinylidene fluoride.

[0151] The above binder may be included in the positive active material layer in an amount of 1% to 20% by weight, preferably 1.2% to 10% by weight, in order to sufficiently secure binding strength between components such as the positive active material.

[0152] The above conductive material can be used to assist and enhance conductivity in a secondary battery, and is not particularly limited as long as it is conductive without causing chemical changes. Specifically, the above cathode conductive material may include at least one selected from the group consisting of graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, Farnes black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives, and preferably may include carbon nanotubes for the purpose of enhancing conductivity.

[0153] The above conductive material may be included in the above positive active material layer in an amount of 1% to 20% by weight, preferably 1.2% to 10% by weight, in order to sufficiently ensure electrical conductivity.

[0154] The thickness of the above positive active material layer may be 5㎛ to 500㎛, preferably 20㎛ to 200㎛.

[0155] The above anode can be manufactured by coating an anode slurry comprising an anode active material and optionally a binder, a conductive material, and a solvent for forming an anode slurry onto the above anode current collector, and then drying and rolling.

[0156]

[0157] cathode

[0158] The above cathode can be opposite to the above anode.

[0159] The above-mentioned cathode includes a cathode active material layer, and the cathode active material layer may include a cathode active material. The above-mentioned cathode may further include a cathode current collector.

[0160] The above negative electrode active material layer may be disposed on at least one surface of the negative electrode current collector, specifically on one or both surfaces of the negative electrode current collector.

[0161] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. Specifically, the above-mentioned negative current collector may be copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy.

[0162] The above-mentioned cathode current collector can typically have a thickness of 3 to 500 μm.

[0163] The above-mentioned negative current collector may form fine irregularities on its surface to strengthen the bonding force of the negative active material. For example, the above-mentioned negative current collector can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0164]

[0165] The above-mentioned negative electrode active material layer may include a negative electrode active material.

[0166] The above negative electrode active material may include at least one selected from carbon-based active materials and silicon-based active materials.

[0167] The carbon-based active material may include at least one selected from the group consisting of graphite, hard carbon, soft carbon, carbon black, graphene, and fibrous carbon, and preferably may include graphite. The graphite may be, for example, artificial graphite or natural graphite.

[0168] Average particle size (D of the above carbon-based active material) 50 ) may be 10㎛ to 30㎛, preferably 15㎛ to 25㎛, in terms of ensuring structural stability during charging and discharging and reducing adverse reactions with the electrolyte.

[0169] The above silicon-based active material is silicon (Si) and silicon oxide (SiO₂). x , 0 <x<2)로 표시될 수 있음), 실리콘-금속 합금(Si-metal alloy) 및 실리콘-탄소 복합체(Si / C Composite)로 이루어진 군에서 선택된 적어도 1종을 포함할 수 있다. 구체적으로, 실리콘계 활물질은 실리콘-탄소 복합체(Si-C Composite)일 수 있다.

[0170] The above silicon-carbon composite may be a composite of silicon and graphite, etc., and may form a structure in which graphene or amorphous carbon, etc. surrounds a core composed of silicon and graphite, etc. The size of the silicon dispersed in the above silicon-carbon composite may be at the nano level.

[0171] The above silicon oxide (SiO₂) x If ) is SiO2, it does not react with lithium ions and therefore cannot store lithium, so it is desirable that x be within the above range. Specifically, the silicon oxide may be SiO.

[0172] In the above silicon-metal alloy, the metal is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and specifically may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (Dudidum), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0173] Average particle size (D) of the above silicon-based active material 50 ) may be 0.01㎛ to 40㎛, specifically 1㎛ to 30㎛, more specifically 2㎛ to 15㎛ in terms of reducing adverse reactions with the electrolyte while ensuring structural stability during charging and discharging.

[0174] Specifically, the negative electrode active material may include at least one of a carbon-based active material and a silicon-based active material, and specifically, may include a carbon-based active material and a silicon-based active material. When the negative electrode active material includes a carbon-based active material and a silicon-based active material, the weight ratio of the carbon-based active material and the silicon-based active material may be 50:50 to 99:1, specifically 70:30 to 99:1, more specifically 85:15 to 99:1, and even more specifically 90:10 to 99:1.

[0175] When the above negative electrode active material includes the above silicon-based active material, the silicon-based active material may be included in an amount of 0.1% to 30% by weight, specifically 0.3% to 20% by weight, and more specifically 0.5% to 15% by weight relative to 100% by weight of the negative electrode active material layer. It is desirable that the content of the silicon-based active material included in the negative electrode active material layer satisfies the above range in terms of improving the capacity characteristics of the battery.

[0176] The above-mentioned negative electrode active material may be included in the negative electrode active material layer in an amount of 60% to 99% by weight, preferably 75% to 95% by weight.

[0177]

[0178] The above cathode active material layer may further include a binder and / or a conductive material together with the cathode active material.

[0179] The binder is used to improve the performance of the battery by enhancing the adhesion between the negative electrode active material layer and the negative electrode current collector, and may include, for example, at least one selected from the group consisting of polyvinylidenefluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidenefluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, and materials in which hydrogens thereof are substituted with Li, Na, or Ca, etc., and may also include various copolymers thereof. there is.

[0180] The above binder may be included in the cathode active material layer in an amount of 0.5% to 10% by weight, preferably 1% to 5% by weight.

[0181] The above conductive material is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, Farnes black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives may be used.

[0182] The above conductive material may be included in the above negative electrode active material layer in an amount of 0.5% to 10% by weight, preferably 1% to 5% by weight.

[0183] The thickness of the above negative electrode active material layer may be 10㎛ to 200㎛, preferably 20㎛ to 150㎛.

[0184] The above cathode can be manufactured by coating a cathode slurry comprising a cathode active material, a binder, a conductive material, and / or a solvent for forming a cathode slurry on at least one surface of a cathode current collector, and then drying and rolling.

[0185] The solvent for forming the cathode slurry may include, for example, at least one selected from the group consisting of distilled water, NMP (N-methyl-2-pyrrolidone), ethanol, methanol, and isopropyl alcohol, preferably distilled water, in order to facilitate the dispersion of the cathode active material, binder, and / or conductive material. The solid content of the cathode slurry may be 30% to 80% by weight, specifically 40% to 70% by weight.

[0186]

[0187] Separator

[0188] The above separator may be interposed between the anode and the cathode.

[0189] As the above separator, a conventional porous polymer film used as a separator, such as a polyolefin-based polymer film made of ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, may be used alone or in a laminate thereof, or a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc., may be used, but is not limited thereto. In addition, a coated separator containing a ceramic component or a polymer material may be used to ensure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.

[0190]

[0191] (2) Battery case

[0192] The battery case according to the present invention serves to accommodate the aforementioned electrode assembly and the aforementioned non-aqueous electrolyte.

[0193] The external shape of the battery case of the present invention is not particularly limited, but can be a cylindrical shape using a can, a rectangular shape, a pouch shape, or a coin shape.

[0194] Specifically, according to one embodiment of the present invention, the battery case may be cylindrical or prismatic. More specifically, the battery case may be a cylindrical or prismatic metal battery case. In the case of the non-aqueous electrolyte according to the present invention, the internal pressure of the battery case may increase due to the use of methyl acetate, so it may be preferable to apply it to a cylindrical or prismatic metal battery case.

[0195]

[0196] The present invention will be explained in more detail below through specific embodiments.

[0197]

[0198] Example 1

[0199] (Preparation of non-aqueous electrolytes)

[0200] As an organic solvent, a mixture of ethylene carbonate, ethylmethyl carbonate, dimethyl carbonate, and methyl acetate in a volume ratio of 30:5:55:10 was used. LiPF6 and LiN(SO2F)2 were dissolved in the above organic solvent to a concentration of 1.0 M and 0.25 M, respectively, and then vinylene carbonate (VC) was added as an additive to a concentration of 3.0 wt% to prepare a non-aqueous electrolyte.

[0201] (Manufacturing of lithium secondary batteries)

[0202] Li[Ni as positive electrode active material 0.95 Co 0.02 Mn 0.02 Al 0.01 An anode slurry was prepared by mixing O2, a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 97.60:1.57:0.83 in N-methylpyrrolidone. The anode slurry was applied to both sides of an aluminum (Al) current collector and dried, and then a roll press was performed to produce an anode (thickness: 103.2 μm).

[0203] A cathode slurry was prepared by mixing a cathode active material (graphite and Si / C, 85:13 weight ratio), a conductive material (carbon black), and a binder (styrene-butadiene rubber) in water in a weight ratio of 98.0:1.9:0.1. The cathode slurry was applied to both sides of a copper (Cu) current collector and dried, and then a roll press was performed to produce a cathode (thickness: 103.5 μm).

[0204] An electrode assembly was manufactured by interposing a polyethylene separator between the positive electrode and the negative electrode manufactured by the above-described method, and then the assembly was placed inside a battery case, and an electrolyte was injected into the battery case to manufacture a lithium secondary battery.

[0205]

[0206] Examples 2 to 4, Comparative Examples 1 to 6

[0207] A non-aqueous electrolyte and a lithium secondary battery were prepared in the same manner as in Example 1, except that the organic solvent composition was as shown in Table 1 below.

[0208] Organic solvent composition (volume%) Volume ratio of ethylmethyl carbonate and dimethyl carbonate V DMC / (V MA + V EC )V MA / V EC V DMC / V EC Ethylene Carbonate (EC) Fluoroethyl Carbonate Propylene Carbonate Ethyl Methyl Carbonate (EMC) Dimethyl Carbonate (DMC) Methyl Acetate (MA) Ethyl Propionate (EP) Example 1 30--555 10-1:111.38 0.33 1.83 Example 2 30--545 20-1:90.90 0.67 1.50 Example 3 30--535 30-1:70.58 1.00 1.17 Example 4 30--525 40-1:50.36 1.33 0.83 Comparative Example 1 30--600 10-1:000.330 Comparative Example 2 30--555 101:111.83 -1.83 Comparative Example 330--5605-1:121.710.172.00Comparative Example 4-30-55510-1:115.50--Comparative Example 5--3055510-1:115.50--Comparative Example 635--51050-1:20.121.430.29

[0209] Experimental Example 1: Life Performance Evaluation

[0210] The life characteristics of the lithium secondary batteries prepared according to Examples 1 to 4 and Comparative Examples 1 to 6 at 40°C, 24°C, and 10°C were measured.

[0211] Specifically, each of the lithium secondary batteries prepared according to Examples 1 to 4 and Comparative Examples 1 to 6 was charged to 4.2V and 0.05C under CC / CV and 1.0C conditions using an electrochemical charge / discharger at 40℃, 24℃, and 10℃, and then discharged to 2.5V under CC and 1.0C conditions, with 100 charge / discharge cycles performed as one cycle.

[0212] At this time, the above capacity retention rate was calculated using the following formula, and the results are shown in Table 2 below.

[0213]

[0214] Capacity Retention Rate (%) = {(Discharge Capacity after 100 Cycles / Discharge Capacity after 1 Cycle)} × 100

[0215] Volume Retention Rate (%, 100 cycles) 24℃ 40℃ 10℃ Example 1 82.49 75.39 76.82 Example 2 82.28 72.40 79.11 Example 3 82.23 71.39 79.37 Example 4 80.06 70.09 75.72 Comparative Example 181.25 70.42 70.48 Comparative Example 280.94 66.98 73.29 Comparative Example 3 79.68 69.36 41.62 Comparative Example 4 34.75 36.23 31.57 Comparative Example 5 77.84 67.43 33.09 Comparative Example 6 76.33 61.53 77.32

[0216] Referring to Table 2 above, Examples 1 to 4, which are lithium secondary batteries in which the composition of the organic solvent satisfies Formula 1 of the present invention while the ratio of the volume of dimethyl carbonate to the volume of ethylmethyl carbonate is controlled within the range according to the present invention, all show balanced and excellent capacity retention rates from low to high temperatures, whereas Comparative Examples 1 to 6, which are lithium secondary batteries that do not satisfy Formula 1 according to the present invention, show inferior performance in at least one of the capacity retention rates from low to high temperatures.

[0217] Specifically, V of Formula 1 of the present invention DMC / (V MA + V ECIt can be seen that the lithium secondary batteries of Comparative Examples 2 to 5, which fall outside the upper limit of the range, are inferior to the lithium secondary batteries of Examples 1 to 4 in at least one of the capacity retention rates at room temperature, high temperature, and low temperature.

[0218] Meanwhile, since dimethyl carbonate is not added, V of Formula 1 of the present invention DMC / (V MA + V EC Comparative Example 1, which falls outside the lower limit of the range, and Comparative Example 2, in which ethyl propionate was added instead of methyl acetate, showed that the lifespan performance at high and low temperatures was not significantly reduced compared to Examples 1 to 4 of the present invention; however, as will be described later, it was confirmed that the low-temperature growth rate was higher compared to Examples 1 to 4 of the present invention.

[0219] In addition, it can be confirmed that Comparative Example 6 does not satisfy Formula 1 of the present invention, and at the same time, the ratio of the volume of dimethyl carbonate to the volume of ethylmethyl carbonate is used at less than 3, resulting in a significant decrease in capacity retention rate at room temperature and high temperature. Similarly, it can be confirmed that Comparative Example 3 does not satisfy Formula 1 of the present invention, and at the same time, the ratio of the volume of dimethyl carbonate to the volume of ethylmethyl carbonate is used at more than 11, resulting in a problem where the capacity retention rate at low temperature decreases rapidly.

[0220]

[0221] Experimental Example 2: Evaluation of Resistance Increase Rate

[0222] The resistance increase rate at 10°C of the lithium secondary batteries prepared according to the above Examples 1 to 4 and Comparative Examples 1 to 6 was measured.

[0223] Specifically, each of the lithium secondary batteries prepared according to Examples 1 to 4 and Comparative Examples 1 to 6 was charged and discharged for one cycle using an electrochemical charge / discharger in the same manner as in Experimental Example 1, and then the discharge capacity after one cycle was measured using the electrochemical charge / discharger, the SOC was adjusted to 10%, and then a pulse of 0.5C was applied for 30 seconds, and the initial resistance was calculated through the difference between the voltage before the pulse application and the voltage after the pulse application.

[0224] After 100 cycles of charge and discharge, the resistance after 100 cycles was calculated using the same method as above, and the resistance increase rate was calculated using the following formula. The results are shown in Table 3 below.

[0225]

[0226] Resistance increase rate (%) = {(Resistance after 100 cycles - Resistance after 1 cycle) / Resistance after 1 cycle} × 100

[0227] Resistance Increase Rate (%) Example 1: 1146.09 Example 2: 128.60 Example 3: 134.30 Example 4: 152.39 Comparative Example 1: 296.84 Comparative Example 2: 198.68 Comparative Example 3: 327.26 Comparative Example 4: 408.41 Comparative Example 5: 340.96 Comparative Example 6: 155.20

[0228] Referring to Table 3 above, it can be seen that the resistance increase rate of Examples 1 to 4, which are lithium secondary batteries satisfying Formula 1 of the present invention with an organic solvent composition, is lower than the resistance increase rate of Comparative Examples 1 to 6.

[0229] Meanwhile, in the case of Comparative Example 6, although the resistance increase rate compared to Examples 1 to 4 of the present invention is not significantly large, as described above in Experimental Example 1, it can be seen that the capacity retention rate at high temperatures is inferior compared to Examples 1 to 4 of the present invention.

Claims

1. A lithium salt; and an organic solvent; comprising, The above organic solvent includes a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent, and methyl acetate, and The above-mentioned cyclic carbonate-based organic solvent includes ethylene carbonate, and The above linear carbonate-based organic solvent includes dimethyl carbonate and ethylmethyl carbonate, and The volume ratio of the above ethylmethyl carbonate and dimethyl carbonate is 1:3 to 1:11, and Non-aqueous electrolyte satisfying Equation 1 below: [Equation 1] 0.20 ≤ V DMC / (V MA + V EC ) ≤ 1.65 In the above Equation 1, V DMC is the volume percentage of the organic solvent volume of dimethyl carbonate (unit: volume%), V EC is the volume percentage of the organic solvent volume of ethylene carbonate (unit: volume%), V MA is the volume percentage (unit: volume%) of the organic solvent volume of methyl acetate.

2. In Claim 1, The above ethylene carbonate is a non-aqueous electrolyte contained in the above organic solvent at 20 volume% to 40 volume%.

3. In Claim 1, The above organic solvent is a non-aqueous electrolyte satisfying Formula 2 below: [Equation 2] 0.25 ≤ V MA / V EC ≤ 1.50 In Equation 2 above, V EC is the volume percentage of the organic solvent volume of ethylene carbonate (unit: volume%), V MA is the volume percentage (unit: volume%) of the organic solvent volume of methyl acetate.

4. In Claim 1, The above organic solvent is a non-aqueous electrolyte satisfying Formula 3 below: [Equation 3] 0.70 ≤ V DMC / V EC ≤ 2.00 In Equation 3 above, V DMC is the volume percentage of the organic solvent volume of dimethyl carbonate (unit: volume%), V EC is the volume percentage (unit: volume%) of the organic solvent volume of ethylene carbonate.

5. In Claim 1, The above lithium salts are LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO2, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 A non-aqueous electrolyte comprising at least one selected from the group consisting of LiB(C2O4)2, LiCF3SO3, LiN(SO2F)2, LiCH3SO3, LiCF3CO2, LiCH3CO2, LiN(SO2CF3)2 and LiN(SO2CF2CF3)2.

6. In Claim 5, The above lithium salt is a non-aqueous electrolyte containing LiPF6 and LiN(SO2F)2.

7. In Claim 1, The above linear carbonate-based organic solvent is a non-aqueous electrolyte contained in an amount of 20% to 67% by volume relative to 100% by volume of the organic solvent.

8. In Claim 1, The above methyl acetate is a non-aqueous electrolyte contained in an amount of 5 to 45 volume% relative to 100 volume% of an organic solvent.

9. An electrode assembly comprising an anode, a cathode opposite to the anode, and a separator interposed between the anode and the cathode; A non-aqueous electrolyte according to claim 1; and A lithium secondary battery comprising the above electrode assembly and a battery case accommodating the above non-aqueous electrolyte.

10. In Claim 9, The above cathode includes a cathode active material layer, and The above negative electrode active material layer includes a negative electrode active material, and The above negative electrode active material is a lithium secondary battery comprising a silicon-based active material.

11. In Claim 10, The above silicon-based active material is silicon (Si) and silicon oxide (SiO₂). x , 0 <x<2), 실리콘-금속 합금(Si-metal alloy) 및 실리콘-탄소 복합체(Si / C composite)로 이루어진 군에서 선택된 적어도 1종을 포함하는 리튬 이차전지.

12. In Claim 10, A lithium secondary battery comprising the above silicon-based active material in an amount of 0.1% to 30% by weight relative to 100% by weight of the above negative electrode active material layer.