A UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material and its preparation method and application
By preparing UIO-66-NH2/CNTs/TiO2 ternary composite materials, combining MOF with carbon nanotubes and titanium dioxide, the problem of low activity of TiO2 photocatalytic materials is solved, and efficient photocatalytic degradation of organic dyes is achieved, providing high efficiency dye wastewater treatment plan.
Patent Information
- Application Number
- CN202410108482.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-01-26
AI Technical Summary
The existing TiO2 photocatalytic materials have low activity under ultraviolet light, low utilization rate, and low degradation efficiency of organic dyes, making it difficult to effectively degrade dye pollution in water under natural conditions.
The UIO-66-NH2/CNTs/TiO2 ternary composite material was prepared by sol-gel method. By combining MOF with carbon nanotubes and titanium dioxide, a narrow bandgap semiconductor coupling was used to form a heterojunction, which improved the photocatalytic performance and adsorption capacity of the material. , a new type of porous carbon adsorption-photocatalyst was prepared.
It significantly improves the photocatalytic degradation efficiency of the organic dye methyl orange, realizes efficient industrial wastewater treatment, and provides dye wastewater treatment technology with low energy consumption and high removal rate.
Smart Images

Figure CN117816133B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an organic dye adsorption-photocatalytic material, and relates to a UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, and a preparation method and application thereof. Specifically, it relates to the preparation and application of a material for adsorbing and degrading methyl orange. Background Art
[0002] In recent years, with the rapid development of the textile industry, the problem of water pollution caused by dyes has become increasingly serious. In the textile industry, nearly 10,000 dyes are put into use. In the dyeing process, only about 40% of the dyes are colored on textiles, and the remaining 60% of the dyes are discharged into the natural environment in the form of wastewater. According to the literature, more than 7,105 tons of dyes are discharged into aquatic ecosystems every year. They are highly toxic to aquatic organisms and humans, and are mutagenic and even carcinogenic. However, since dyes have good chemical stability to light and heat, they are difficult to degrade under natural conditions. Therefore, it is urgent to find an efficient way to degrade dyes.
[0003] The main methods for dye wastewater treatment include physical methods, chemical methods, biological methods and some combined processes. As the difficulty of dye wastewater treatment becomes increasingly greater and the emission standards become higher and higher, traditional treatment methods have been difficult to meet the emission standards. Therefore, it is necessary to further research and develop dye wastewater treatment technologies with low energy consumption and high removal rate. In recent years, the wastewater treatment methods that have been studied more and have better treatment effects mainly include electrochemical methods and photocatalytic oxidation methods.
[0004] TiO2 is recognized as the most promising environmentally friendly semiconductor photocatalytic material in the field of environmental pollution control due to its high efficiency, safety and non-toxicity, stable chemical properties, low cost and wide distribution. It can completely degrade organic dye pollutants in water and completely mineralize them into harmless inorganic substances such as CO2 and H2O, so it can avoid secondary pollution. However, pure TiO2 has some disadvantages in the degradation of organic dyes: (1) TiO2 is only active under ultraviolet light (UV), and ultraviolet light only accounts for 4% of sunlight, so the utilization rate of sunlight is not high; (2) TiO2 has a wide band gap; (3) The recombination rate of TiO2 photogenerated electron-hole pairs is high. Therefore, the photocatalytic efficiency of TiO2 is low. Therefore, it is necessary to modify TiO2 to improve its photocatalytic efficiency. The common modification methods currently include: non-metallic ion doping method, metal ion doping method, semiconductor composite method, precious metal deposition method, etc.
[0005] MOFs, as an organic-inorganic hybrid material, is a new type of porous compound. UiO-66-NH2 is a Zr-based MOFs with high thermal and mechanical stability. However, the band gap of UiO-66-NH2 is about 3.6eV, which limits its optical adsorption in the visible light region. To achieve this, the use of narrow bandgap semiconductor coupling to form a heterojunction method is an ideal choice.
[0006] MOF@CNTs materials have the characteristics of high mechanical and elastic strength, excellent chemical and thermal stability, excellent electronic and optical properties, low weight, low toxicity and some low cost, so they have been widely used. Therefore, integrating MOFs with carbon-based materials not only helps to transform the weaknesses of MOFs into advantages, but also surprisingly brings many new functions, such as enhanced stability, improved conductivity, template effect, etc. MOF@CNTs, as electron acceptors, delay the recombination of electron-hole pairs and increase the surface area and number of active sites of TiO2.
[0007] The present invention utilizes a sol-gel method to prepare titanium dioxide, and simultaneously composites TiO2 with metal organic framework materials UIO-66-NH2 and CNTs having a large specific surface area through a solvent synthesis method, combines the excellent adsorption properties of UIO-66-NH2 and CNTs with the photocatalytic degradation performance of TiO2, and prepares a novel derivative porous carbon adsorption-photocatalyst based on an amino-modified Zr-MOF composite with carbon nanotubes and titanium dioxide, and applies it to the photocatalytic degradation of the organic dye methyl orange, showing an excellent catalytic degradation effect, providing a new treatment idea for treating organic pollutants in industrial wastewater, and having a good application prospect. Summary of the invention
[0008] The invention provides a UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material and a preparation method and application thereof. The composite material is easy to prepare and has high degradation performance.
[0009] The technical solution adopted by the present invention to solve the technical problem is: a UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, the preparation method of which includes the following steps:
[0010] 1) Preparation of UIO-66-NH2 / CNTs / TiO2 ternary composite material:
[0011] Zirconium tetrachloride and 2-aminoterephthalic acid are added to NN dimethylformamide and glacial acetic acid, followed by the addition of carbon nanotubes, ultrasonication at room temperature to form a mixed solution, TiO2 is added, ultrasonication at room temperature, stirring to form an off-white mixed solution, and the solution is placed in a stainless steel high-pressure reactor for reaction, and the off-white solid in the reactor is taken out, washed, centrifuged, dried, and ground to obtain a UIO-66-NH2 / CNTs / TiO2 ternary composite material;
[0012] 2) Preparation of UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon materials
[0013] The UIO-66-NH2 / CNTs / TiO2 ternary composite material is calcined to obtain a UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material.
[0014] In the above-mentioned UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, in step 1), the mass ratio of zirconium tetrachloride: 2-aminoterephthalic acid: NN dimethylformamide: glacial acetic acid is 130-140: 95-100: 60-70: 10-14.
[0015] In the above-mentioned UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, in step 1), the mass ratio of zirconium tetrachloride: carbon nanotubes: TiO2 is 250:10-20:240-260.
[0016] In the above-mentioned UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, in step 1), the preparation method of TiO2 comprises the following steps:
[0017] (a) Preparation of Solution A: Slowly add tetrabutyl titanate into 2-propanol and stir evenly;
[0018] Prepare Solution B: Mix distilled water, acetic acid, and nitric acid;
[0019] (b) Liquid B is slowly dripped into Liquid A and stirred vigorously until the color changes from milky white to light yellow. The mixture is sealed and placed in a dark place to form a soft elastic solid gel.
[0020] (c) drying the sealed solid gel to form yellow granular crystals, preparing a xerogel, and grinding to obtain a powder;
[0021] (d) The ground powder is calcined, naturally cooled, and sieved to obtain TiO2.
[0022] In the above-mentioned UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, in step (d), the calcination temperature is 350-450°C and the calcination time is 5-7h.
[0023] In the above-mentioned UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, in step 1), the reaction is kept at 120°C for 24 hours.
[0024] In the above-mentioned UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, in step 2), the calcination temperature is 650-850°C, the calcination time is 1h, and the heating rate is 5°C·min -1 .
[0025] The above-mentioned UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material is used in photocatalytic degradation of organic dyes.
[0026] In the above application, the organic pollutant is methyl orange.
[0027] In the above application, the above UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material is added to a solution containing methyl orange, and the methyl orange is degraded under light conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the XRD diagram of the UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material prepared in Example 1.
[0029] Figure 2 This is the infrared spectrum of the UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material obtained in Example 1.
[0030] Figure 3 This is the effect of the initial concentration of methyl orange on the catalytic efficiency in Example 2.
[0031] Figure 4 This is the effect of the amount of catalyst used in Example 2 on the catalytic efficiency.
[0032] Figure 5 This is the effect of different catalysts on the adsorption-degradation of methyl orange in Example 2.
[0033] Figure 6 It is the degradation rate of methyl orange of the UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material prepared at different calcination temperatures. DETAILED DESCRIPTION
[0034] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.
[0035] The carbon nanotubes involved in the following examples were all purchased from Sinopharm Chemical Reagent Co., Ltd.
[0036] Example 1 A UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material
[0037] (I) The preparation method is as follows:
[0038] (1) Preparation of TiO2:
[0039] (a) Preparation of Solution A: Slowly add 17.20 mL of tetrabutyl titanate into 57.65 mL of 2-propanol, stir evenly, and stir magnetically for 20-30 min;
[0040] Prepare Solution B: Mix 1.8 mL of distilled water, 5.66 mL of acetic acid, and 2.7 mL of nitric acid;
[0041] (b) Liquid B is slowly dripped into Liquid A and stirred vigorously for 1-3 hours. The color changes from milky white to light yellow. The sol is sealed in a beaker and placed in a dark place for 18-30 hours to form a soft elastic solid gel.
[0042] (c) removing the sealing film from the solid gel, placing it in a vacuum drying oven at 80-120° C. and drying it for 18-36 h to form yellow granular crystals to prepare a xerogel, and placing the xerogel in a mortar and grinding it into powder;
[0043] (d) The ground powder is placed in a porcelain boat, and the porcelain boat containing the sample is placed in a tube furnace and calcined at 350-450° C. for 5-7 h, cooled naturally, and passed through a 150-300 mesh sieve;
[0044] (2) Preparation of UIO-66-NH2 / CNTs / TiO2 ternary composite material:
[0045] 0.25 g zirconium tetrachloride and 0.268 g 2-aminoterephthalic acid were added to 50 mL N-N dimethylformamide and 4 mL glacial acetic acid, followed by the addition of 0.02072 g carbon nanotubes, ultrasonicated at room temperature for 15 min, magnetically stirred for 30 min, and 0.25 g TiO2 prepared as described above was added, ultrasonicated and stirred to form an off-white mixed solution, which was placed in a stainless steel high-pressure reactor and kept warm at 120°C in a forced air drying cabinet for 24 h. The off-white solid in the reactor was taken out, washed, centrifuged, dried and ground to obtain the UIO-66-NH2 / CNTs / TiO2 ternary composite material.
[0046] (3) Preparation of UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon materials:
[0047] The prepared UIO-66-NH2 / CNTs / TiO2 ternary composite material was placed in a tubular furnace and calcined at a heating rate of 5°C·min -1 , and kept warm at 650℃ for 1h, and finally the derived porous carbon material was obtained.
[0048] Comparative Example 1 Preparation of UIO-66-NH2
[0049] Dissolve 0.250g zirconium tetrachloride and 0.268g ligand 2-aminoterephthalic acid in 50mL N-N dimethylformamide, add 4mL glacial acetic acid, and stir well at room temperature for 1h. Then transfer the solution to a reactor. React at 120℃ for 24h. The synthesized product is washed several times with N-N dimethylformamide and methanol, and finally dried under vacuum at 120℃ for 12h to obtain UIO-66-NH2.
[0050] Example 2 Characterization
[0051] Figure 1 The powder X-ray diffraction (PXRD) of the synthesized UIO-66-NH2, UIO-66-NH2 / CNTs / TiO2 ternary composite material and the derived carbon material of the UIO-66-NH2 / CNTs / TiO2 ternary composite and CNTs showed that the derived carbon material of the UIO-66-NH2 / CNTs / TiO2 ternary composite had good crystallinity during the synthesis and preparation process.
[0052] Figure 2 The infrared spectra (FT-IR) of the synthesized UIO-66-NH2, UIO-66-NH2 / CNTs / TiO2 ternary composite material and the derived carbon material of the UIO-66-NH2 / CNTs / TiO2 ternary composite and CNTs indicate that the derived carbon material of the UIO-66-NH2 / CNTs / TiO2 ternary composite was successfully prepared.
[0053] Example 3 Photocatalytic degradation of organic dye methyl orange solution by UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material
[0054] The UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material prepared in Example 1 was used to photocatalytically degrade the methyl orange solution.
[0055] Activation treatment of photocatalyst: Take a certain amount of UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material and vacuum dry it at 363K for 12h.
[0056] A ZF-1 three-purpose UV analyzer and a 365nm spot lamp were used as the UV light source. 3 mg of the activated UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material in Example 1 was weighed, 4 mL of 10 mg / L methyl orange solution was added into a weighing bottle, and the mixture was placed on a magnetic stirrer. The mixture was stirred for 30 min in a dark environment to allow the sample to reach adsorption equilibrium and avoid adsorption affecting the photocatalytic effect. After 30 min of dark reaction, the spot lamp was turned on, and photocatalytic degradation was carried out at intervals of 30 min. After the reaction was completed, the sample was aspirated into a centrifuge tube with a pipette, and the sample was centrifuged (2500 rpm) for 15 min. The supernatant was taken for wavelength testing. The wavelength testing instrument was a Puxi universal visible light photometer, and the absorbance was measured to calculate the photocatalytic efficiency.
[0057] Example 4 Effect of initial concentration of methyl orange solution on degradation rate
[0058] In order to explore the catalyst activity, the effect of the initial concentration of methyl orange on the degradation rate of methyl orange was studied. A ZF-1 three-purpose UV analyzer and a 365nm spot lamp were used as the UV light source. 3 mg of the activated UIO-66-NH2 / CNTs / TiO2 ternary composite derivative carbon material in Example 1 was weighed and added to 4 mL of methyl orange solution in a weighing bottle, which was then placed on a magnetic stirrer. The sample was stirred in a dark environment for 30 minutes to allow the sample to reach adsorption equilibrium to avoid adsorption affecting the photocatalytic effect. After 30 minutes of dark reaction, the spot lamp was turned on, and photocatalytic degradation was performed at intervals of 30 minutes. After the reaction was completed, the sample was aspirated into a centrifuge tube with a pipette, and centrifuged (2500 rpm) for 15 minutes. The supernatant was taken for wavelength testing. The wavelength testing instrument used a Puxi universal visible light photometer to measure the absorbance and calculate the photocatalytic efficiency. The initial concentrations of methyl orange were set to 10 mg / L, 20 mg / L, 30 mg / L, 40 mg / L, and 50 mg / L, respectively. From Figure 3 It can be seen that the degradation efficiency of MO depends on its initial concentration, and when the dye concentration is 10 mg / L, its photodegradation efficiency reaches 100%. As the dye concentration increases, the degradation rate of the dye decreases. This is because in high-concentration dye solutions, less UV light is irradiated through the solution, so the efficiency of the photodegradation process decreases. As the methyl orange concentration changes from 10 mg / L to 50 mg / L, the removal rate decreases from 100% to 57%.
[0059] Example 5 Effect of the amount of UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material added on the degradation rate of methyl orange
[0060] In order to explore the catalyst activity, the effect of the amount of UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material added on the degradation rate of methyl orange was studied. A ZF-1 three-purpose ultraviolet analyzer was used, and a 365nm spot lamp was used as an ultraviolet light source. A certain mass of the UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material activated in Example 1 was weighed and added to a weighing bottle with 4mL of 10mg / L methyl orange solution, and placed on a magnetic stirrer; stirred in a dark environment for 30 minutes so that the sample reached adsorption equilibrium to avoid adsorption affecting the photocatalytic effect; after 30 minutes of dark reaction, the spot lamp was turned on, and photocatalytic degradation was performed at intervals of 30 minutes. After the reaction was completed, it was aspirated into a centrifuge tube with a pipette, centrifuged (2500rpm) for 15 minutes, and the supernatant was taken for wavelength testing. The wavelength testing instrument selected a general visible light photometer from Puxi to measure the absorbance and calculate the photocatalytic efficiency. The addition amounts of derived carbon materials of the UIO-66-NH2 / CNTs / TiO2 ternary composite were set to 1 mg, 2 mg, 3 mg, and 4 mg, respectively. Figure 4 The results show that the degree of dye degradation increases with the increase in the amount of photocatalyst in the solution. Obviously, the rate of photodegradation reaction increases with the increase in the amount of photocatalyst, but this lasts until the maximum amount is used. As the amount of photocatalyst increases, the removal rate decreases. This is because the photocatalyst blocks the irradiation of ultraviolet light and limits the oxidation reaction.
[0061] Example 6 Effect of different photocatalysts on the degradation rate of methyl orange
[0062] The effects of different catalysts on the degradation rate of methyl orange were studied. Pure TiO2, UiO-66-NH2 and CNTs, UIO-66-NH2 / CNTs / TiO2 ternary composite materials and UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon materials were used to degrade methyl orange. A ZF-1 three-purpose UV analyzer was used, and a 365nm spot lamp was used as the UV light source. 3 mg of pure TiO2, UiO-66-NH2 and CNTs, as well as UIO-66-NH2 / CNTs / TiO2 ternary composite materials and UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon materials were weighed respectively, added into a weighing bottle with 4 mL of 10 mg / L methyl orange solution, and placed on a magnetic stirrer; stirred for 30 minutes in a dark environment to allow the sample to reach adsorption equilibrium to avoid adsorption affecting the photocatalytic effect; after 30 minutes of dark reaction, the spot lamp was turned on, and photocatalytic degradation was carried out at intervals of 30 minutes. After the reaction was completed, the sample was aspirated into a centrifuge tube with a pipette, centrifuged (2500 rpm) for 15 minutes, and the supernatant was taken for wavelength testing. The wavelength testing instrument used was a Puxi universal visible light photometer to measure the absorbance and calculate the photocatalytic efficiency.
[0063] Figure 5 It can be seen that the adsorption effect of TiO2 on MO is very low in the dark reaction stage, while UiO-66-NH2 and CNTs have strong adsorption capacity for MO. In the photocatalytic stage, the catalytic ability of TiO2 is much greater than that of UiO-66-NH2 and CNTs (as can be seen from the slope of the curve). Under ultraviolet light irradiation, the adsorption and degradation efficiency of pure TiO2, UiO-66-NH2 and CNTs within 120 minutes were 47%, 59% and 52%, respectively. In the absence of a catalyst, after 120 minutes, the degradation rate of MO was less than 5%. From Figure 5 It can be seen that the degradation efficiency of MO by UIO-66-NH2 / CNTs / TiO2 ternary composite material is 76%, while the degradation efficiency of MO by UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material is 100%, which is much higher than pure TiO2, UiO-66-NH2 and CNTs. The addition of TiO2 and CNTs can greatly improve the degradation efficiency of MO.
[0064] Example 7 Effect of different calcination temperatures on the degradation rate of methyl orange
[0065] The effect of UIO-66-NH2 / CNTs / TiO2 ternary composite materials obtained at different calcination temperatures on the degradation rate of methyl orange was studied. UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon materials were obtained by calcination at 650°C, 800°C, and 850°C, respectively, and the remaining steps were the same as in Example 1.
[0066] The UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon materials obtained at different calcination temperatures were used to photocatalytically degrade methyl orange. Figure 6 It can be seen that the UIO-66-NH2 / CNTs / TiO2 ternary composite material calcined at 650℃ has the best degradation effect on methyl orange, with a degradation rate of 100%. The degradation rate gradually decreases with the increase of calcination temperature.
[0067] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material, characterized in that: The preparation method comprises the following steps: 1) Preparation of UIO-66-NH2 / CNTs / TiO2 ternary composite material: Zirconium tetrachloride and 2-aminoterephthalic acid are added to NN dimethylformamide and glacial acetic acid, followed by the addition of carbon nanotubes, ultrasonication at room temperature to form a mixed solution, TiO2 is added, ultrasonication at room temperature, stirring to form an off-white mixed solution, and the solution is placed in a stainless steel high-pressure reactor for reaction, and the off-white solid in the reactor is taken out, washed, centrifuged, dried, and ground to obtain a UIO-66-NH2 / CNTs / TiO2 ternary composite material; the mass ratio of zirconium tetrachloride: carbon nanotubes: TiO2 is 250:10-20:240-260; 2) Preparation of UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon materials The UIO-66-NH2 / CNTs / TiO2 ternary composite material was calcined at 650°C for 1 h to obtain the UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material.
2. A UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material according to claim 1, characterized in that: In step 1), the mass ratio of zirconium tetrachloride: 2-aminoterephthalic acid: NN dimethylformamide: glacial acetic acid is 130-140: 95-100: 60-70: 10-14.
3. The UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material according to claim 1, characterized in that: In step 1), the preparation method of TiO2 comprises the following steps: (a) Preparation of Solution A: Slowly add tetrabutyl titanate into 2-propanol and stir evenly; Prepare Solution B: Mix distilled water, acetic acid, and nitric acid; (b) Liquid B is slowly dripped into Liquid A and stirred vigorously until the color changes from milky white to light yellow. The mixture is sealed and placed in a dark place to form a soft elastic solid gel. (c) drying the sealed solid gel to form yellow granular crystals, preparing a xerogel, and grinding the xerogel to obtain a powder; (d) The ground powder is calcined, naturally cooled, and sieved to obtain TiO2.
4. The UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material according to claim 3, characterized in that: In step (d), the calcination temperature is 350-450° C. and the calcination time is 5-7 hours.
5. The UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material according to claim 1, characterized in that: In step 1), the reaction is carried out at 120°C for 24 hours.
6. Use of the UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material as described in claim 1 in photocatalytic degradation of organic dyes.
7. The use according to claim 6, characterized in that: The organic dye is methyl orange.
8. The use according to claim 7, characterized in that: The UIO-66-NH2 / CNTs / TiO2 ternary composite derived carbon material according to claim 1 is added to a solution containing methyl orange, and the methyl orange is degraded under light conditions.