Method for reducing hydrogen desorption temperature of solid solution type hydrogen storage alloy and application of method
By mixing titanium-vanadium hydrogen storage alloy and aluminum hydride through mechanical ball milling, composite hydrogen storage materials are prepared, which solves the problems of high crushing cost and high hydrogen release temperature platform of solid solution hydrogen storage alloy, and achieves lower hydrogen release temperature and improved activation. conditions, providing solutions for the commercial application of fuel cells.
Patent Information
- Application Number
- CN202310279080.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-09-24
AI Technical Summary
Solid solution hydrogen storage alloys have high costs and high hydrogen release temperature during the crushing process, which limits their application in the field of hydrogen economy.
Composite hydrogen storage materials are prepared by mixing titanium vanadium hydrogen storage alloy and aluminum hydride (AlH3) through mechanical ball milling (MA method), which reduces the hydrogen release temperature and improves the brittleness of the alloy.
It effectively reduces the hydrogen release temperature of the solid solution hydrogen storage alloy, reduces the crushing cost, and improves the activation conditions of the alloy, making it suitable for large-scale production and fuel cell applications.
Smart Images

Figure CN118682135A
Abstract
Description
Technical Field
[0001] The invention relates to a method for reducing the dehydrogenation temperature of a solid solution hydrogen storage alloy and application thereof, belonging to the technical field of hydrogen storage material preparation. Background Art
[0002] Hydrogen storage and transportation is a key link in the hydrogen economy. Solid solution hydrogen storage alloys have a strong appeal to the field of hydrogen storage and transportation in the current hydrogen economy. The main reason is that solid solution hydrogen storage alloys have a high weight hydrogen storage density (> 3.5wt.%) and volume hydrogen storage density (160kg / m 3 ) and excellent dynamic properties. There are two main problems that restrict the application of this type of alloy in the field of chemical hydrogen storage and physical hydrogen storage. First, it is difficult to crush and the crushing cost is high; second, the hydrogen decomposition temperature platform of the PCT curve of hydrogen decomposition is high. The existing technologies for solving the above problems mainly include: crushing using hydrogen charging and heating equipment, such as Chinese patent CN108766701A discloses a crushing process for NdFeB stripping pieces, which improves the crushing efficiency of NdFeB stripping pieces. And Chinese patents CN105074837B, CN113390011B, Japanese patents JP05103332, JP07188799A. JP06306413A, JP2005082891A, etc., all provide pulverizing equipment for improving the pulverizing efficiency of solid solution hydrogen storage alloys. However, since the radius of hydrogen molecules is extremely small, the metal materials used in the equipment are very demanding, and the metal will experience hydrogen embrittlement after long-term contact with hydrogen molecules. Once hydrogen leaks, it will cause great safety hazards. Therefore, the maintenance and maintenance of these equipment has caused huge cost expenditures.
[0003] Element substitution is one of the main methods to solve the high dehydrogenation temperature platform of solid solution hydrogen storage alloys. Other metal elements are used to replace elements in Ti-V-Cr, Ti-V-Mn, Ti-V-Ni and other system alloys. However, since precious metals have better substitution effects, it is difficult to achieve industrial production. For example, Chinese patent CN113528923A uses trace element doping technology to increase the hydrogen storage capacity of multi-principal element hydrogen storage alloys by up to 54.7%, and the activation performance is significantly improved; as well as Chinese patents CN115141965A, CN115612903A, CN115261677A, CN115141943A, etc.
[0004] In summary, for solid solution hydrogen storage alloys, the two major defects of the existing technology are difficulty in crushing and high crushing cost, as well as high hydrogen release temperature platform. Therefore, providing a solid solution hydrogen storage alloy that can make up for these two major defects at the same time is an urgent problem to be solved in order to realize the commercial application of fuel cells. Summary of the invention
[0005] Aiming at the problems that existing solid solution hydrogen storage alloys are difficult to crush, have high crushing costs, and have a high dehydrogenation temperature platform on the PCT curve of dehydrogenation, the present invention provides a method for reducing the dehydrogenation temperature of solid solution hydrogen storage alloys and its application.
[0006] The technical solution of the present invention:
[0007] One of the purposes of the present invention is to provide a method for reducing the dehydrogenation temperature of a solid solution hydrogen storage alloy, the method comprising: mixing a titanium-vanadium hydrogen storage alloy block and AlH3 by MA method to obtain a composite hydrogen storage material.
[0008] It is further defined that the mass of AlH3 is 1 to 10% of the mass of the composite hydrogen storage material.
[0009] It is further defined that the mass of AlH3 is 1 to 8% of the mass of the composite hydrogen storage material.
[0010] It is further defined that the mass of AlH3 is 3% of the mass of the composite hydrogen storage material.
[0011] It is further defined that the particle size of the titanium-vanadium hydrogen storage alloy block is 3 to 7 mm.
[0012] It is further defined that the titanium-vanadium hydrogen storage alloy block is:
[0013] TiV 2-x B x , 1.4≥x≥0.6, the B-side element is one or more of Mn, Cr, Ni, Zr, Fe, Cu, and Co;
[0014] Or Ti 1-y Re y V 2-x B x , 1.4≥x≥0.6, 0.4≥y≥0.1, Re is one or more elements selected from La, Ce, Pr, Nd, Sm, and Gd.
[0015] Further defined, the titanium vanadium hydrogen storage alloy block is TiV 1.1 Cr 0.3 Mn 0.6 .
[0016] Further defined, the MA method is mechanical ball milling, the rotation speed is 350-600rpm, the rotation speed is 350-600rpm, the ball-to-material ratio is (8-40):1, and the atmosphere is one or a mixture of nitrogen, argon, and hydrogen.
[0017] A second object of the present invention is to provide a solid solution hydrogen storage alloy prepared by the above preparation method.
[0018] The second purpose of the present invention is to provide an application of a solid solution hydrogen storage alloy prepared by the above method, specifically, the solid solution hydrogen storage alloy is used in the preparation of a fuel cell.
[0019] The present invention uses aluminum hydride and MA method (mechanical alloying) to prepare solid solution hydrogen storage alloys, which not only reduces the dehydrogenation temperature of solid solution hydrogen storage alloys, but also improves the brittleness of the alloy, making up for the defects of the existing solid solution hydrogen storage alloys that are difficult to crush, high crushing cost, and high dehydrogenation temperature platform, and provides a promising solution for the commercial application of fuel cells. In addition, compared with the prior art, the present invention also has the following beneficial effects:
[0020] (1) The advantages of using aluminum hydride as a catalyst promoter in the present invention are mainly: after it releases hydrogen, it can provide a hydrogen source for the hydrogen storage alloy, allowing the hydrogen storage alloy to undergo an autonomous hydrogen absorption and desorption process, thereby improving the activation conditions of the hydrogen storage alloy. In addition, the aluminum in aluminum hydride also has a heat conductive effect, which can transfer heat faster during the hydrogen absorption and desorption process. The interaction between the two reduces the temperature at which the alloy material completely desorbs hydrogen to about 100°C, and the activation energy of the desorption reaction is reduced by two times.
[0021] (2) The present invention adopts the MA method to synthesize the composite material, the process is easy to control, the conditions are simple, and it is suitable for large-scale production and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The hydrogen absorption kinetic curves of the composite hydrogen storage materials prepared in different embodiments;
[0023] Figure 2 This is a PCT test result diagram of the composite hydrogen storage material prepared in Example 2;
[0024] Figure 3 This is a PCT test result diagram of the hydrogen storage material prepared in Comparative Example 1;
[0025] Figure 4 These are DSC test result diagrams of composite hydrogen storage materials prepared in different embodiments. DETAILED DESCRIPTION
[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0027] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0028] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0029] Example 1
[0030] The composite hydrogen storage material prepared in this embodiment is expressed as 99wt.%TiV 1.1 Cr 0.3 Mn 0.6 +1wt.%AlH3, the preparation method is as follows:
[0031] (1) First, prepare a titanium-vanadium solid solution alloy, and the preparation method is as follows:
[0032] The vacuum arc melting furnace was evacuated to 2 × 10 -3 Pa was filled with 0.5 atmospheres of high-purity argon gas with a purity of 99.99% (volume percentage) as a protective gas, and Ti metal (purity 99.7%), V metal (purity 99.9%), Mn metal (purity 99.5%) and chromium metal (purity 99.9%) were placed in a TiV 1.1 Cr 0.3 Mn 0.6 After weighing the chemical formula, the alloy was placed in a vacuum arc furnace for smelting with an arc current of 300A, smelting was performed 4 times, each smelting was 2 minutes, and the alloy ingot was naturally cooled and taken out of the furnace to obtain the alloy ingot. The alloy ingot was broken into 3-7 mm alloy blocks to obtain titanium-vanadium hydrogen storage alloy blocks.
[0033] (2) Accurately weigh the TiV obtained in step (1) according to weight percentage. 1.1 Cr 0.3 Mn 0.6 1.98g of material powder and 0.02g of commercially available AlH3 material, with a total mass of 2.0g, were placed in a ball mill in a glove box filled with high-purity argon atmosphere, and zircon balls (total mass 40g) were added at a ball-to-material ratio of 20:1. Zircon balls of three sizes, large, medium and small, were selected, with diameters of 6mm, 4mm and 2mm respectively. The ball mill speed was 450rpm, and the ball milling time was 90min. The ball mill was removed from the ball mill, and the ball mill was opened in an argon atmosphere to obtain a composite hydrogen storage material, which was sealed and stored in a desiccator.
[0034] Example 2
[0035] The composite hydrogen storage material prepared in this embodiment is expressed as 97wt.%TiV 1.1 Cr 0.3 Mn 0.6+3wt.%AlH3, the preparation method is as follows:
[0036] (1) First, prepare a titanium-vanadium solid solution alloy, and the preparation method is as follows:
[0037] The vacuum arc melting furnace was evacuated to 2 × 10 -3 Pa was filled with 0.5 atmospheres of high-purity argon gas with a purity of 99.99% (volume percentage) as a protective gas, and Ti metal (purity 99.7%), V metal (purity 99.9%), Mn metal (purity 99.5%) and chromium metal (purity 99.9%) were placed in a TiV 1.1 Cr 0.3 Mn 0.6 After weighing the chemical formula, the alloy was placed in a vacuum arc furnace for smelting with an arc current of 300A, smelting was performed 4 times, each smelting was 2 minutes, and the alloy ingot was naturally cooled and taken out of the furnace to obtain the alloy ingot. The alloy ingot was broken into 3-7 mm alloy blocks to obtain titanium-vanadium hydrogen storage alloy blocks.
[0038] (2) Accurately weigh the TiV obtained in step (1) according to weight percentage. 1.1 Cr 0.3 Mn 0.6 1.94g of material powder and 0.06g of commercially available AlH3 material, with a total mass of 2.0g, were placed in a ball mill in a glove box filled with high-purity argon atmosphere, and zircon balls (total mass 40g) were added at a ball-to-material ratio of 20:1. Zircon balls of three sizes, large, medium and small, were selected, with diameters of 6mm, 4mm and 2mm respectively. The ball mill speed was 450rpm, and the ball milling time was 90min. The ball mill was removed from the ball mill, and the ball mill was opened in an argon atmosphere to obtain a composite hydrogen storage material, which was sealed and stored in a desiccator.
[0039] Example 3
[0040] The composite hydrogen storage material prepared in this embodiment is expressed as 95wt.%TiV 1.1 Cr 0.3 Mn 0.6 +5wt.%AlH3, the preparation method is as follows:
[0041] (1) First, prepare a titanium-vanadium solid solution alloy, and the preparation method is as follows:
[0042] The vacuum arc melting furnace was evacuated to 2 × 10 -3 Pa was filled with 0.5 atmospheres of high-purity argon gas with a purity of 99.99% (volume percentage) as a protective gas, and Ti metal (purity 99.7%), V metal (purity 99.9%), Mn metal (purity 99.5%) and chromium metal (purity 99.9%) were placed in a TiV 1.1 Cr 0.3 Mn0.6 After weighing the chemical formula, the alloy was placed in a vacuum arc furnace for smelting with an arc current of 300A, smelting was performed 4 times, each smelting was 2 minutes, and the alloy ingot was naturally cooled and taken out of the furnace to obtain the alloy ingot. The alloy ingot was broken into 3-7 mm alloy blocks to obtain titanium-vanadium hydrogen storage alloy blocks.
[0043] (2) Accurately weigh the TiV obtained in step (1) according to weight percentage. 1.1 Cr 0.3 Mn 0.6 1.90g of material powder and 0.1g of commercially available AlH3 material, with a total mass of 2.0g, were placed in a ball mill in a glove box filled with high-purity argon atmosphere, and zircon balls (total mass 40g) were added at a ball-to-material ratio of 20:1. Zircon balls of three sizes, large, medium and small, were selected, with diameters of 6mm, 4mm and 2mm respectively. The ball mill speed was 450rpm, and the ball milling time was 90min. The ball mill was removed from the ball mill, and the ball mill was opened in an argon atmosphere to obtain a composite hydrogen storage material, which was sealed and stored in a desiccator.
[0044] Comparative Example 1
[0045] This comparative example prepares a hydrogen storage material as a comparative sample, and its expression is TiV 1.1 Cr 0.3 Mn 0.6 , and its preparation method is as follows:
[0046] The vacuum arc melting furnace was evacuated to 2 × 10 -3 Pa was filled with 0.5 atmospheres of high-purity argon gas with a purity of 99.99% (volume percentage) as a protective gas, and Ti metal (purity 99.7%), V metal (purity 99.9%), Mn metal (purity 99.5%) and chromium metal (purity 99.9%) were placed in a TiV 1.1 Cr 0.3 Mn 0.6 After weighing the chemical formula, the alloy was placed in a vacuum arc furnace for smelting with an arc current of 300A, smelting was performed 4 times, each smelting was 2 minutes, and the alloy ingot was naturally cooled and taken out of the furnace to obtain the alloy ingot. The alloy ingot was broken into 3-7 mm alloy blocks to obtain titanium-vanadium hydrogen storage alloy blocks.
[0047] Comparative Example 2
[0048] This comparative example prepares a hydrogen storage material as a comparative sample, and its expression is BM-TiV 1.1 Cr 0.3 Mn 0.6 , and its preparation method is as follows:
[0049] (1) First, prepare a titanium-vanadium solid solution alloy, and the preparation method is as follows:
[0050] The vacuum arc melting furnace was evacuated to 2 × 10 -3 Pa was filled with 0.5 atmospheres of high-purity argon gas with a purity of 99.99% (volume percentage) as a protective gas, and Ti metal (purity 99.7%), V metal (purity 99.9%), Mn metal (purity 99.5%) and chromium metal (purity 99.9%) were placed in a TiV 1.1 Cr 0.3 Mn 0.6 After weighing the chemical formula, the alloy was placed in a vacuum arc furnace for smelting with an arc current of 300A, smelting was performed 4 times, each smelting was 2 minutes, and the alloy ingot was naturally cooled and taken out of the furnace to obtain the alloy ingot. The alloy ingot was broken into 3-7 mm alloy blocks to obtain titanium-vanadium hydrogen storage alloy blocks.
[0051] (2) Accurately weigh the TiV obtained in step (1) according to weight percentage. 1.1 Cr 0.3 Mn 0.6 2.0g of material powder was put into a ball mill in a glove box filled with high-purity argon atmosphere, and zircon balls (total mass 40g) were added at a ball-to-material ratio of 20:1. Three sizes of zircon balls were selected, large, medium and small, with diameters of 6mm, 4mm and 2mm respectively. The ball mill speed was 450rpm, and the ball milling time was 90min. The ball mill was removed from the ball mill, and the ball mill was opened in an argon atmosphere to obtain a composite hydrogen storage material, which was sealed and stored in a desiccator.
[0052] The solid solution alloy samples prepared in the above Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to performance test analysis. The specific experimental process and test results are as follows:
[0053] (1) The hydrogen storage material powders prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were placed in a reactor, and vacuumed for 30 minutes at 25°C. Then, 4 MPa of 99.99% (volume percentage) high-purity hydrogen was filled into the reactor at 25°C to measure the hydrogen absorption kinetics. The hydrogen absorption kinetics curves of each sample at 25°C were obtained, as shown in FIG. Figure 1 As shown (where the horizontal axis is time, expressed in minutes; the vertical axis is the amount of hydrogen absorption, expressed in mass percentage. Figure 1 It can be seen that the composite hydrogen storage materials of Examples 1, 2 and 3 doped with AlH3 can absorb hydrogen quickly after a short incubation period of about 10 seconds, and in the first 15 minutes, the hydrogen absorption rates of Comparative Examples 1 and 2 are only 0wt.%, while the hydrogen absorption rates of Examples 1, 2 and 3 are 1.46, 1.61 and 2.61wt.%, respectively. It can be seen that AlH3 has a certain modification effect on the alloy surface during the ball milling process, reduces the potential barrier on the alloy surface, and provides more channels for the diffusion of hydrogen molecules.
[0054] (2) In order to evaluate the hydrogen release capacity of the prepared composite hydrogen storage material, the samples prepared in Example 2 and Comparative Example 1 were subjected to PCT test. Specifically, the prepared hydrogen storage material powder samples were loaded into a reactor, and after the same activation treatment, PCT tests were performed at 25°C, 100°C, 150°C and 200°C, respectively, with a pressure range of 10 -4 Mpa~5Mpa, the test results are as follows Figure 2 and Figure 3 As shown, the results show that the effective hydrogen storage capacity of the sample prepared in Example 2 is higher than that of Comparative Example 1 at all temperatures, especially at 25°C, the effective hydrogen storage capacity of Example 2 is 1.096wt.%, while the effective hydrogen storage capacity of Comparative Example 1 is 0.297wt.%, indicating that the hydrogen evolution conditions of the composite material at room temperature are more conducive to practical applications.
[0055] (3) In order to evaluate the dehydrogenation temperature of the prepared hydrogen storage material, the ball-milled product of Example 2 and Comparative Examples 1 and 2 were subjected to DSC testing. Specifically, 5-10 mg of the hydrogen-saturated composite hydrogen storage material was placed in a differential scanning calorimeter at a temperature range of 25-700°C and a heating rate of 5°C / min. The results are shown in FIG. Figure 4 As shown, the results show that each sample has two endothermic peaks, corresponding to the two-step reaction stages of hydrogen atoms diffusing in the V-based solid solution. The first step is the decomposition of dihydride (VH2) into monohydride (VH). The second step is the transformation of monohydride (VH) to body-centered cubic phase. It can be clearly seen that the temperatures of the two decomposition steps of the composite hydrogen storage material are significantly affected by the presence of Al. 97wt.%TiV after ball milling 1.1 Cr 0.3 Mn 0.6 +3wt.%AlH3 composite hydrogen storage material has a lower first step decomposition temperature than TiV 1.1 Cr 0.3 Mn 0.6 The alloy temperature dropped by about 100°C, and the second step decomposition temperature dropped by about 120°C. The activation energy (Ea) of the distribution reaction was calculated according to the Kissinger equation. 1.1 Cr 0.3 Mn 0.6 +3wt.%AlH3 composite hydrogen storage material has an Ea value reduced to TiV 1.1 Cr 0.3 Mn 0.6 The decrease in dehydrogenation temperature and apparent activation energy indicates that Al doping reduces the barrier required for solid solution hydrogen desorption.
[0056] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for reducing the dehydrogenation temperature of a solid solution hydrogen storage alloy, characterized in that: The method comprises the following steps: mixing a titanium-vanadium hydrogen storage alloy block and AlH3 by using an MA method to obtain a composite hydrogen storage material.
2. The method according to claim 1, characterized in that The mass of AlH3 is 1 to 10% of the mass of the composite hydrogen storage material.
3. The method according to claim 2, characterized in that The mass of AlH3 is 1 to 8% of the mass of the composite hydrogen storage material.
4. The method according to claim 2 or 3, characterized in that: The mass of AlH3 is 3% of the mass of the composite hydrogen storage material.
5. The method according to claim 1, characterized in that The particle size of the titanium-vanadium hydrogen storage alloy block is 3 to 7 mm.
6. The method according to claim 1, characterized in that Titanium-vanadium hydrogen storage alloy block is: TiV 2-x B x , 1.4≥x≥0.6, the B-side element is one or more of Mn, Cr, Ni, Zr, Fe, Cu, and Co; Or Ti 1-y Re y V 2-x B x , 1.4≥x≥0.6, 0.4≥y≥0.1, Re is one or more elements selected from La, Ce, Pr, Nd, Sm, and Gd.
7. The method according to claim 1, characterized in that Titanium vanadium hydrogen storage alloy block is TiV 1.1 Cr 0.3 Mn 0.6 .
8. The method according to claim 1, characterized in that The MA method is mechanical ball milling with a rotation speed of 350-600 rpm, a ball-to-material ratio of (8-40):1, and an atmosphere of one or a mixture of nitrogen, argon, and hydrogen.
9. A solid solution hydrogen storage alloy, characterized in that: The method according to claim 1 is used to prepare the product.
10. An application of the solid solution hydrogen storage alloy according to claim 9, characterized in that: Used in the preparation of fuel cells.