Lithium ferrous silicate positive electrode material and preparation method thereof
Through fluorine doping and carbon coating technology, high-performance lithium iron silicate cathode materials are prepared, which solves the problem of high cost and poor effect of metal ion doping in the existing technology, and realizes low-cost, high-performance silicon Lithium iron oxide cathode material improves electrochemical performance and conductivity.
Patent Information
- Application Number
- CN202411103904.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-13
AI Technical Summary
In the existing technology, metal ions such as Ni2+, Co2+, Mn2+, Cr3+, Zn2+, and Mg2+ are used to improve the ionic and electronic conductivity of lithium iron silicate cathode materials. The cost is high and the effect is not good, which limits the preparation of low-cost, high-performance Application of lithium iron silicate cathode material.
The preparation method of fluorine-doped lithium iron silicate cathode material is adopted. By adding lithium, iron, silicon and fluorine sources to the precursor, and calcining it under specific temperature and time conditions, a nanoparticle structure is formed and uniformly distributed on the surface of the material. Coated with carbon layer to improve electrochemical performance.
At a charge and discharge rate of 0.1C, the discharge specific capacity of the lithium iron silicate cathode material reaches 215.5mAh/g, which significantly improves the electrochemical performance, reduces the diffusion resistance and migration time of lithium ions, and enhances the conductivity and conductivity of the material. stability.
Smart Images

Figure CN118771399A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and more specifically, relates to a lithium ferrous silicate positive electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life, low self-discharge rate, and no pollution. They are widely used in the fields of power batteries and grid energy storage. The rapid development of lithium-ion batteries has increased the demand for high-performance, low-cost positive electrode materials. Lithium ferrous silicate positive electrode materials have the advantages of low cost, abundant raw materials, high theoretical specific capacity (330mAh / g), good thermal stability, and overcharge resistance. They are ideal positive electrode materials for lithium-ion batteries. However, the defects of lithium ferrous silicate positive electrode materials such as low ion and electronic conductivity limit its application in power batteries and energy storage. At present, researchers often use ion doping, nano-sizing, and carbon coating technologies to improve the ion and electronic conductivity of lithium ferrous silicate positive electrode materials. Carbon coating is the most commonly used modification method, which can not only improve the electronic conductivity of lithium ferrous silicate positive electrode materials, but also inhibit the grain growth of lithium ferrous silicate positive electrode materials, thereby achieving particle nano-sizing.
[0003] Fluorine has strong electronegativity. Fluorine doping can reduce the transfer impedance of lithium iron silicate cathode materials, thereby increasing their ion and electron conductivity and improving the electrochemical properties of electrode materials. Carbon coating can nanosize lithium iron silicate cathode materials, shorten the transmission distance of lithium ions in electrode materials, and further improve the rate performance of electrode materials.
[0004] Existing technology uses metal ions such as Ni 2+ 、Co 2+ , Mn 2+ Cr 3+ 、Zn 2+ Mg 2+ To improve the ionic and electronic conductivity of lithium iron silicate cathode materials. These technologies are not only costly, but also have unsatisfactory improvement effects, which is not conducive to the preparation of low-cost, high-performance lithium iron silicate cathode materials.
[0005] Chinese patent document 201010507828.8 discloses a method for preparing a lithium ferrous silicate positive electrode material doped with fluorine and zirconium at the same time. However, this method requires doping zirconium in the positive electrode material, which increases the production cost, and zirconium may affect the electrochemical properties of the positive electrode material, such as the stability. The comprehensive performance of the lithium ferrous silicate positive electrode material still has a lot of room for improvement. Summary of the invention
[0006] 1. Problem to be solved
[0007] The existing technology uses metal ions such as Ni 2+ 、Co2+ , Mn 2+ Cr 3+ 、Zn 2+ Mg 2+ To improve the ionic and electronic conductivity of lithium ferrous silicate positive electrode materials, there are problems of high cost and poor effect. The present invention provides a lithium ferrous silicate positive electrode material and a preparation method thereof.
[0008] 2. Technical solution
[0009] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0010] In a first aspect, the present invention provides a method for preparing a lithium iron silicate positive electrode material, comprising the following steps:
[0011] S1. Providing a precursor: providing a precursor containing a lithium source, an iron source, a silicon source, a fluorine source and a carbon source, wherein the lithium source, the iron source, the silicon source and the fluorine source are weighed according to a stoichiometric ratio of Li, Fe, Si, and F of 2:1:1:(0.01-0.04);
[0012] S2, calcination: in an inert gas atmosphere, the precursor is heated at a constant temperature of 300-400° C. for 3-4 hours, and then heated at a constant temperature of 700-750° C. for 5-6 hours, and then cooled to obtain a lithium iron silicate positive electrode material.
[0013] The reason for adopting the above technical solution is that compared with the prior art of adding metals such as Mg, Zn, Ni, Co, Nr, Cu, Ge, Ti, Cr or simultaneously adding fluorine and metal into the lithium ferrous silicate positive electrode material, the present invention only adds fluorine, which can maintain or even improve the electrochemical performance of the lithium ferrous silicate positive electrode material while saving costs.
[0014] In addition, the determination of the calcination temperature and calcination time in step S2 also has an influence on the electrochemical properties of the lithium ferrous silicate positive electrode material that cannot be ignored. In the two-stage calcination, there are several possibilities for designing the time and temperature conditions of each calcination to make it more conducive to improving the performance of the material. The present invention limits the temperature and time of the two calcinations to a smaller range. The performance of the lithium ferrous silicate positive electrode material prepared under this condition is better than that under other conditions. The reason may be that calcination involves heating the precursor material at a high temperature to induce phase change and crystal growth. By controlling the temperature and time of the two calcinations within a smaller range, the desired crystal phase can be obtained preferentially, the generation of undesirable phases can be reduced, the purity of the crystal phase can be increased, and the grain growth can be better controlled to form smaller and uniform nanoparticles.
[0015] Furthermore, in step S1, the lithium source includes one, two or more of lithium carbonate, lithium oxide, lithium hydroxide, lithium chloride, lithium oxalate, lithium acetate, lithium nitrate, lithium sulfate and lithium dihydrogen phosphate.
[0016] Further, in step S1, the iron source includes one, two or more of ferrous oxalate, ferrous acetate, ferrous chloride, ferrous sulfate, ferrous hydroxide, ferrous nitrate, ferrous citrate and ferrous oxide.
[0017] Furthermore, in step S1, the silicon source includes silicon dioxide.
[0018] Furthermore, in step S1, the silicon source is gas phase silicon dioxide with a size range of 20 to 30 nm.
[0019] The reason for adopting the above technical solution is that the selection of fumed silicon dioxide with a size range of 20 to 30 nm is conducive to controlling the particle size of the final lithium ferrous silica positive electrode material, making it smaller than non-fumed silicon dioxide with a larger size, specifically, making it in the range of 25 to 55 nm. In this way, the path for lithium ions to enter the active material from the electrolyte or return from the active material to the electrolyte will be shorter, which helps to reduce the diffusion resistance and migration time of lithium ions and improve the charge and discharge efficiency of lithium ion batteries. In contrast, the particle size of lithium ferrous silica positive electrode materials in the prior art is usually around 100 nm, and its overall conductivity is relatively poor.
[0020] Furthermore, in step S1, the fluorine source is selected from one, two or more of lithium fluoride, silicon fluoride, sodium fluoride, potassium fluoride and ammonium fluoride.
[0021] Furthermore, in step S1, the fluorine source is selected from one or both of lithium fluoride and silicon fluoride.
[0022] The reason for adopting the above technical solution is that: since lithium and silicon are components of the target product lithium ferrous silicate positive electrode material of the present invention, lithium fluoride or silicon fluoride will not introduce impurity elements compared with other fluorine sources.
[0023] Furthermore, in step S1, the carbon source is an organic carbon source.
[0024] The reason for adopting the above technical solution is that inorganic carbon sources are usually in an amorphous state after carbonization, and the coating uniformity is poor, while organic carbon sources can be more evenly coated on the surface of the target product after carbonization compared with inorganic carbon, thereby preventing the electrode material from being corroded in the electrolyte, better protecting the electrode material, and forming an effective conductive transmission channel on the surface of the material, thereby improving the electrochemical properties of the material.
[0025] Furthermore, the organic carbon source is selected from high molecular organic matter.
[0026] The reason for adopting the above technical solution is that the polymer organic carbon source has better flexibility and fluidity due to its macromolecular chain structure. During the carbonization process, this characteristic enables the polymer organic carbon source to be more evenly covered on the surface of the target product to form a continuous and dense coating layer. For example, the carbon source is polyvinyl pyrrolidone.
[0027] Furthermore, in step S1, the carbon layer formed after the carbon source is carbonized accounts for 3wt% to 10wt% of the lithium iron silicate positive electrode material.
[0028] The reason for adopting the above technical solution is that if the content of the carbon source is too low, effective coating of lithium ferrous silicate cannot be achieved; if the content of polyvinyl pyrrolidone is too high, the gaps originally provided for lithium ion transmission will be blocked in large quantities, greatly affecting the electrode reaction kinetics; therefore, the carbon layer formed after carbonization of the carbon source accounts for 3wt% to 10wt% of the lithium ferrous silicate positive electrode material, which is a reasonable range.
[0029] Furthermore, in step S1, the solvent is at least one of deionized water, distilled water, ethanol and acetone.
[0030] Further, step S1 is specifically as follows: weigh Li according to the stoichiometric ratio of Li, Fe, Si, and F being (2-x):1:1:x. 2 CO 3 , Fe 2 CO 4 ·4H 2 O、SiO 2 , LiF, and polyvinyl pyrrolidone are mixed in an ethanol solution and dried to obtain a precursor;
[0031] The value range of x is 0.01 to 0.04.
[0032] The reason for adopting the above technical solution is that: the above formula is selected as the positive electrode material of lithium ferrous silicate, lithium fluoride can not only provide lithium source but also provide fluorine source, will not introduce impurities and, at the same time, control Li 2 CO 3 The stoichiometric ratio of LiF to LiF is within a specific range, which can further improve the conductivity of the lithium iron silicate positive electrode material.
[0033] Furthermore, in step S2, the inert gas is selected from at least one of argon, nitrogen, carbon monoxide, carbon dioxide and hydrogen.
[0034] Furthermore, in step S2, the inert gas is argon and nitrogen.
[0035] Compared with carbon monoxide, carbon dioxide and hydrogen, argon and nitrogen are more advantageous in terms of safety and cost as inert gases.
[0036] Furthermore, the volume ratio of argon gas to nitrogen gas is (3-5):1.
[0037] Preferably, the volume ratio of argon to nitrogen is 4:1.
[0038] The reasons for adopting the above technical solution are: first, argon is completely inert, has a higher density, and can be used at extremely high temperatures without causing any risks; second, nitrogen is lower in cost than argon. Considering the combination of safety and cost advantages, the overall argon ratio is controlled at 80% and nitrogen at 20%.
[0039] Furthermore, in step S1, the mixing conditions include: mixing method: ball milling; ball mill speed: 400-500 r / min; ball-to-material ratio: (6-8):1.
[0040] For example, in step S1, the ball mill speed is 400 r / min and the ball-to-material ratio is 7:1.
[0041] In a second aspect, the present invention provides a lithium ferrous silicate positive electrode material, and the lithium ferrous silicate positive electrode material is prepared by the aforementioned method.
[0042] Furthermore, the particle size of the lithium iron silicate positive electrode material is 25 to 55 nm.
[0043] Furthermore, the surface of the lithium iron silicate positive electrode material is coated with a carbon layer.
[0044] 3. Beneficial effects
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] (1) The positive electrode material of the present invention is doped with fluorine only. Compared with the metal ion doping in the prior art, it can significantly improve the ionic and electronic conductivity of the lithium iron silicate positive electrode material while reducing the cost of raw materials. The electrochemical performance of the positive electrode material of the present invention is significantly improved compared with that of the positive electrode material without fluorine doping. At a charge and discharge rate of 0.1C, the discharge specific capacity can reach 215.5 mAh / g.
[0047] (2) The preparation method of the fluorine-doped nano-lithium ferrous silicate positive electrode material of the present invention is simple. The particle size of the prepared lithium ferrous silicate positive electrode material is about 25 to 55 nm, and a layer of carbon material is evenly coated on its surface. The effect of the uniform carbon coating layer is that the carbon layer can inhibit the growth of the grains of the material during the preparation process, prompting it to form nanoparticles with smaller particle size, shortening the Li + diffusion path; secondly, it can enhance the conductivity of the material and improve the Li+ finally, it can reduce the side reactions of electrode / solution and enhance the electrochemical stability of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is the SEM image of the lithium iron silicate positive electrode material in Example 1.
[0049] Figure 2 This is the charge and discharge curve of the lithium iron silicate positive electrode material in Example 1 at 0.1C. DETAILED DESCRIPTION
[0050] It should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the term "and / or" used herein includes any and all combinations of one or more related listed items.
[0051] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0052] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.
[0053] As used herein, "adjacent" refers to the proximity of two structures or elements. Specifically, elements identified as "adjacent" can be adjacent or connected. Such elements can also be close to or in proximity to each other without necessarily touching each other. In some cases, the precise degree of proximity can depend on the specific context.
[0054] As used herein, the term "at least one of" is intended to be synonymous with "one or more of." For example, "at least one of A, B, and C" expressly includes only A, only B, only C, and combinations of each thereof.
[0055] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.
[0056] Any steps described in any method or process claim (for example, steps S1, S2, S3... or steps (1), (2), (3)... or steps 1), 2), 3)...) may be performed in any order and are not limited to the order presented in the claims.
[0057] Method+function or step+function limitations shall only be adopted if all of the following conditions are present in a particular claim limitation: a) "a method for..." or "a step for..." are explicitly recited; b) the corresponding function is explicitly recited. The structure, material, or action that supports the method+function is explicitly recited in the description herein. Therefore, the scope of the present invention should be determined solely by the appended claims and their legal equivalents, rather than by the description and examples given herein.
[0058] The present invention is further described below in conjunction with specific embodiments.
[0059] Example 1
[0060] This embodiment provides a method for preparing a lithium iron silicate positive electrode material, comprising the following steps:
[0061] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, and F of 1.99:1:1:0.01, weigh 1.475 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2, 0.0052 g of LiF, and 2.117 g of polyvinyl pyrrolidone were ball-milled in an ethanol solution. The ball mill was a YXQM-1L model ball mill produced by Changsha Miqi Instrument Equipment Co., Ltd. The ball milling speed was 400 r / min; the ball milling time was 5 hours; the ball-to-material ratio was 7:1; and then dried at 85°C for 12 hours, and the mixed raw materials obtained a precursor.
[0062] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 1.99 FeSiO 4 F 0.01 / C, which is the target product fluorine-doped nano-Li 2 FeSiO 4 / C. Fluorine doped nano-Li 2 FeSiO 4 / C was assembled into a button half-cell and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that the discharge specific capacity was 215.5 mAh / g, 170.7 mAh / g, 165.6 mAh / g and 100.2 mAh / g at 0.1C, 0.5C, 1C and 5C charge and discharge rates. Figure 1 The fluorine-doped nano-Li 2 FeSiO 4 SEM image of / C, Figure 2 The fluorine-doped nano-Li 2 FeSiO 4 / C charge and discharge curve at 0.1C.
[0063] Example 2
[0064] This embodiment provides a method for preparing a lithium iron silicate positive electrode material, comprising the following steps:
[0065] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, and F of 1.98:1:1:0.02, and weigh 1.474 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , 0.01 g of LiF, and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0066] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 1.98 FeSiO 4 F 0.02 / C, which is the target product fluorine-doped nano-Li 2 FeSiO 4 / C. Fluorine doped nano-Li 2 FeSiO 4 / C was assembled into a button half-cell, and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that its discharge specific capacity was 223.5 mAh / g, 180.4 mAh / g, 175.8 mAh / g, and 105.3 mAh / g at 0.1C, 0.5C, 1C, and 5C charge and discharge rates.
[0067] Example 3
[0068] This embodiment provides a method for preparing a lithium iron silicate positive electrode material, comprising the following steps:
[0069] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, and F of 1.97:1:1:0.03, weigh 1.473 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , 0.016 g of LiF, and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0070] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 1.97 FeSiO 4 F 0.03 / C, which is the target product fluorine-doped nano-Li 2 FeSiO 4 / C. Fluorine doped nano-Li 2 FeSiO 4 / C was assembled into a button half-cell, and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that its discharge specific capacity was 213.8 mAh / g, 168.2 mAh / g, 160.4 mAh / g, and 96.5 mAh / g at charge and discharge rates of 0.1C, 0.5C, 1C, and 5C.
[0071] Example 4
[0072] This embodiment provides a method for preparing a lithium iron silicate positive electrode material, comprising the following steps:
[0073] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, and F of 1.96:1:1:0.04, and weigh 1.472 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , 0.021 g of LiF, and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0074] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 1.96 FeSiO 4 F 0.04 / C, which is the target product fluorine-doped nano-Li 2 FeSiO 4 / C. Fluorine doped nano-Li 2 FeSiO 4 / C was assembled into a button half-cell, and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that at 0.1C, 0.5C, 1C, and 5C charge and discharge rates, the discharge specific capacity was 205.7mAh / g, 157.6mAh / g, 142.8mAh / g, and 87.3mAh / g.
[0075] Comparative Example 1
[0076] This comparative example provides a method for preparing a lithium iron silicate positive electrode material, comprising the following steps:
[0077] (1) Weigh the raw materials according to the molar ratio of Li, Fe, and Si of 2:1:1, and weigh 1.478 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0078] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 2 FeSiO 4 / C, which is the target product nano-Li 2 FeSiO 4 / C. Nano-Li 2 FeSiO 4 / C was assembled into a button half-cell and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that the discharge specific capacity was 170.7 mAh / g, 120.6 mAh / g, 102.8 mAh / g and 47.3 mAh / g at 0.1C, 0.5C, 1C and 5C charge and discharge rates.
[0079] It can be seen from this comparative example that when the molar fractions of lithium, iron and silicon remain unchanged, if lithium carbonate is used as the lithium source without fluorine addition, the electrochemical performance of the positive electrode material will be significantly reduced, and the discharge specific capacity will decrease by about one-fourth.
[0080] Comparative Example 2
[0081] (1) Weigh the raw materials according to the molar ratio of Li, Fe, and Si being 2:1:1, weigh 1.04 g LiF, 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0082] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li2FeSiO 4 / C, which is the target product nano-Li 2 FeSiO 4 / C. Nano-Li 2 FeSiO 4 / C was assembled into a button half-cell, and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that its discharge specific capacity was 120.7 mAh / g, 70.6 mAh / g, 52.8 mAh / g, and 27.3 mAh / g at 0.1C, 0.5C, 1C, and 5C charge and discharge rates.
[0083] It can be seen from this comparative example that when the molar fractions of lithium, iron and silicon remain unchanged, if lithium fluoride is used as the entire lithium source, the molar fraction of fluorine is too much and exceeds the limit value by a large margin, the electrochemical performance of the positive electrode material will be significantly reduced, and the discharge specific capacity will drop by about one-half.
[0084] Comparative Example 3
[0085] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, and F of 1.995:1:1:0.005, weigh 1.4739 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , 0.0026 g of LiF, and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0086] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 1.995 FeSiO 4 F 0.005 / C, which is the target product nano-Li 1.995 FeSiO 4 F 0.005 / C. Nano-Li 1.995 FeSiO 4 F 0.005 / C was assembled into a button half-cell, and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that at 0.1C, 0.5C, 1C, and 5C charge and discharge rates, the discharge specific capacity was 180.5mAh / g, 131.4mAh / g, 106.8mAh / g, and 55.3mAh / g.
[0087] It can be seen from this comparative example that when the molar fractions of lithium, iron and silicon remain unchanged, if the molar fraction of fluorine is lower than the limit, the electrochemical performance of the positive electrode material will be significantly reduced, and the discharge specific capacity will decrease by about 10%.
[0088] Comparative Example 4
[0089] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, and F of 1.95:1:1:0.05, weigh 1.44 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2O, 1.2 g nano-SiO 2 , 0.026 g of LiF, and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0090] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 1.95 FeSiO 4 F 0.05 / C, which is the target product nano-Li 1.95 FeSiO 4 F 0.05 / C. Nano-Li 1.95 FeSiO 4 F 0.05 / C was assembled into a button half-cell, and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that at 0.1C, 0.5C, 1C, and 5C charge and discharge rates, the discharge specific capacity was 197.5mAh / g, 140.4mAh / g, 115.8mAh / g, and 65.2mAh / g.
[0091] It can be seen from this comparative example that when the amount fractions of lithium, iron and silicon remain unchanged, if the amount fraction of fluorine is higher than the limit,
[0092] The electrochemical performance of the positive electrode material will decline, and its discharge specific capacity at a 0.1C charge and discharge rate will drop below 200mAh / g.
[0093] Comparative Example 5
[0094] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, and F of 1.94:1:1:0.06, weigh 1.433 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , 0.0312 g of LiF, and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0095] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 1.94 FeSiO 4 F 0.06 / C, which is the target product nano-Li 1.94FeSiO 4 F 0.06 / C. Nano-Li 1.94 FeSiO 4 F 0.06 / C was assembled into a button half-cell, and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that its discharge specific capacity was 183.5 mAh / g, 134.4 mAh / g, 107.8 mAh / g, and 60.6 mAh / g at charge and discharge rates of 0.1C, 0.5C, 1C, and 5C.
[0096] A comprehensive analysis of this comparative example and comparative example 4 shows that when the molar fractions of lithium, iron and silicon remain unchanged, the more the molar fraction of fluorine exceeds the limit, the more obviously the electrochemical performance of the positive electrode material decreases, and its discharge specific capacity at a charge and discharge rate of 0.1C even drops to below 190 mAh / g.
[0097] Comparative Example 6
[0098] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, and Mg of 2:0.98:1:0.02, and weigh 1.478 g Li 2 CO 3 , 4.23 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , 0.033 g MgCO 3 , and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0099] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 2 Fe 0.98 Mg 0.02 SiO 4 / C, which is the target product nano-Li 2 Fe 0.98 Mg 0.02 SiO 4 / C. Nano-Li 2 Fe 0.98 Mg 0.02 SiO 4 / C was assembled into a button half-cell and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that at 0.1C, 0.5C, 1C, and 5C charge and discharge rates, the discharge specific capacity was 170.5mAh / g, 124.4mAh / g, 87.8mAh / g, and 53..6mAh / g.
[0100] It can be seen from this comparative example that if magnesium is used to replace fluorine in the positive electrode material and the amount fraction of silicon (one quarter) and the amount fraction of metal (including lithium, iron, and magnesium) (three quarters) remain unchanged, it can be seen that due to the lack of fluorine incorporation, its electrochemical performance is significantly reduced, and the discharge specific capacity decreases by about one quarter.
[0101] Comparative Example 7
[0102] (1) Weigh the raw materials according to the molar ratio of Li, Fe, Si, Mg, and F of 1.98:1:1:0.01:0.01, and weigh 1.462 g Li 2 CO 3 , 4.32 g FeC 2 O 4 ·4H 2 O, 1.2 g nano-SiO 2 , 0.016 g MgCO 3 , 0.0052 g of LiF, and 2.117 g of polyvinyl pyrrolidone were ball-milled and dried in an ethanol solution to obtain a precursor. The ball-milling and drying conditions were the same as those in Example 1.
[0103] (2) In an atmosphere of 80% argon and 20% nitrogen, the precursor was heated at 300°C for 4 hours and 700°C for 6 hours. After cooling to room temperature, Li 1.99 Fe 0.99 Mg 0.01 SiO 4 F 0.01 / C, which is the target product nano-Li 1.99 Fe 0.99 Mg 0.01 SiO 4 F 0.01 / C. Nano-Li 1.99 Fe 0.99 Mg 0.01 SiO 4 F 0.01 / C was assembled into a button half-cell, and its specific capacity was tested at different rates with a voltage range of 1.5 to 4.8 V. The test results showed that its discharge specific capacity was 183.5 mAh / g, 136.4 mAh / g, 97.8 mAh / g, and 63.7 mAh / g at 0.1C, 0.5C, 1C, and 5C charge and discharge rates.
[0104] It can be seen from this comparative example that replacing half of the lithium fluoride in the positive electrode material with other metals means that fluorine and metal are doped at the same time, and the amount fraction of silicon (one quarter) and the amount fraction of metal (including lithium, iron, and magnesium) (three quarters) are guaranteed to remain unchanged, and the amount fraction of fluorine is also within the limited range. The electrochemical performance of the positive electrode material will still decrease, and its discharge specific capacity at a charge and discharge rate of 0.1C will even drop to below 190 mAh / g. The effect of doping only with fluorine is better than doping with other metals or doping with metal and fluorine at the same time.
[0105] The above content is a schematic description of the present invention and its implementation methods, which is not restrictive. What is shown in the embodiment is only one of the implementation methods of the present invention, and the actual implementation method is not limited thereto. Therefore, if a person of ordinary skill in the art is inspired by it and designs implementation methods and embodiments similar to the technical solution without creative design without departing from the purpose of the invention, they should all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a lithium iron silicate positive electrode material, characterized in that: The following steps are involved: S1. Providing a precursor: providing a precursor containing a lithium source, an iron source, a silicon source, a fluorine source and a carbon source, wherein the lithium source, the iron source, the silicon source and the fluorine source are weighed according to a stoichiometric ratio of Li, Fe, Si, and F of 2:1:1:(0.01-0.04); S2, calcination: in an inert gas atmosphere, the precursor is heated at a constant temperature of 300-400° C. for 3-4 hours, and then heated at a constant temperature of 700-750° C. for 5-6 hours, and then cooled to obtain a lithium iron silicate positive electrode material.
2. The method for preparing the lithium iron silicate positive electrode material according to claim 1, characterized in that: In step S1, the lithium source includes one, two or more of lithium carbonate, lithium oxide, lithium hydroxide, lithium chloride, lithium oxalate, lithium acetate, lithium nitrate, lithium sulfate and lithium dihydrogen phosphate; The iron source includes one, two or more of ferrous oxalate, ferrous acetate, ferrous chloride, ferrous sulfate, ferrous hydroxide, ferrous nitrate, ferrous citrate and ferrous oxide; The silicon source includes silicon dioxide; The fluorine source is selected from one, two or more of lithium fluoride, silicon fluoride, sodium fluoride, potassium fluoride and ammonium fluoride.
3. The method for preparing the lithium iron silicate positive electrode material according to claim 2, characterized in that: In step S1, the silicon source is gas phase silicon dioxide with a size range of 20 to 30 nm.
4. The method for preparing the lithium iron silicate positive electrode material according to claim 2, characterized in that: In step S1, the fluorine source is selected from one or both of lithium fluoride and silicon fluoride.
5. The method for preparing the lithium iron silicate positive electrode material according to claim 1, characterized in that: In step S1, the carbon source is an organic carbon source.
6. The method for preparing the lithium iron silicate positive electrode material according to claim 5, characterized in that: In step S1, the carbon layer formed after the carbon source is carbonized accounts for 3wt% to 10wt% of the lithium iron silicate positive electrode material.
7. The method for preparing the lithium iron silicate positive electrode material according to claim 1, characterized in that: In step S2, the inert gas is selected from at least one of argon, nitrogen, carbon monoxide, carbon dioxide and hydrogen.
8. The method for preparing the lithium iron silicate positive electrode material according to claim 1, characterized in that: Step S1 specifically comprises: weighing Li2CO3, Fe2CO4·4H2O, SiO2, and LiF according to the stoichiometric ratio of Li, Fe, Si, and F being (2-x):1:1:x, mixing them with polyvinyl pyrrolidone in an ethanol solution, and drying them to obtain a precursor; The value range of x is 0.01 to 0.
04.
9. A lithium iron silicate positive electrode material, characterized in that: The lithium iron silicate positive electrode material is prepared by the method according to any one of claims 1 to 8.
10. The lithium iron silicate positive electrode material according to claim 9, characterized in that: The particle size of the lithium iron silicate positive electrode material is 25-55 nm.
Citation Information
Patent Citations
Preparation method for ferrous silicate lithium cathode material simultaneously doped with fluorine and zirconium
CN102013483A
Method for preparing ferrous silicate lithium of anode material of lithium ion battery
CN102219230A
Method for preparing lithium ferrous silicate or carbon ferrous silicate cathode material for lithium ion battery
CN102664262A
Carbon nitride and graphene cladded lithium iron phosphate composite anode material and preparation method thereof
CN104134801A
Preparation method of fluorine and yttrium-doped lithium ferrous silicate composite material for lithium-ion battery
CN108063227A
Cited By
Strontium-doped modified lithium ferrous silicate positive electrode material as well as preparation method and application thereof
CN121282132A
A strontium-doped modified lithium iron silicate cathode material, its preparation method and application
CN121282132B