Amino acid modified electrolyte for aqueous zinc ion battery and preparation method of amino acid modified electrolyte
By using amino acid electrolyte additives in aqueous zinc-ion batteries, the problems of zinc dendrite growth and side reactions are solved, long cycle life and high electrochemical performance of the battery are achieved, and the battery performance of zinc-ion batteries is significantly improved.
Patent Information
- Application Number
- CN202411042312.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-22
AI Technical Summary
During the use of aqueous zinc-ion batteries, there are problems such as zinc dendrite growth leading to battery short circuit, rapid capacity fading, and low Coulombic efficiency.
Using amino acid electrolyte additives, by adding leucine, lysine, valine or aspartic acid as electrolyte additives in the electrolyte, combined with weakly acidic soluble zinc salts and ultrapure water, an amino acid modified product is prepared. Resistant electrolyte for aqueous zinc-ion batteries. The electrolyte improves the wettability of the zinc anode, inhibits zinc dendrite growth, and adjusts the pH value to reduce side reactions.
It significantly extends the cycle life of aqueous zinc-ion batteries, improves the specific discharge capacity and charge-discharge cycle stability, and improves the electrochemical performance of the battery. The cycle life is increased from less than 100 hours to more than 2500 hours, and the capacity retention rate reaches 98.30%.
Smart Images

Figure CN118825439A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy materials, and in particular to an amino acid-modified electrolyte for an aqueous zinc ion battery and a preparation method thereof. Background Art
[0002] With the vigorous development of modern electronic products and energy automobile industries, people have put forward higher requirements for the energy storage industry. Traditional lithium-ion batteries have safety risks due to the high price and limited resources of lithium raw materials, and their electrolytes are organic solvents. Seeking energy storage materials that are abundant in resources, safe and reliable, clean and environmentally friendly is a new direction for the development of the energy storage industry. Aqueous zinc-ion batteries (AZIBs) have the advantages of low cost, high safety, and simple technology, and are considered to be extremely promising energy storage batteries. In addition, the theoretical specific capacity is high (820mAh·g -1 ), low redox potential (-0.76V vs. SHE), high ionic conductivity (>1S·m -1 ) is also an outstanding advantage of AZIBs. However, during the use of aqueous zinc-ion batteries, the uneven zinc deposition leads to the growth of zinc dendrites, which poses a risk of battery short circuit; in addition, side reactions such as hydrogen evolution (HER), corrosion, and passivation will inevitably occur in aqueous electrolytes, resulting in rapid battery capacity decay and low coulombic efficiency.
[0003] At present, researchers have proposed various strategies to modify the negative electrode of AZIBs, such as developing new electrolytes, adding additives to the electrolyte, designing 3D porous negative electrode materials, preparing artificial negative electrode protective layers (SEI), etc. Among them, introducing additives into the electrolyte of aqueous zinc-ion batteries is a simple and efficient modification method. The introduced electrolyte additives can play different roles in aqueous zinc-ion batteries, such as providing uniform and neat zinc deposition sites, regulating the zinc deposition crystal surface, and preferentially adsorbing on the anode surface to slow down water corrosion. Electrolytes with the addition of amino acid additives provide new ideas for the development and application of aqueous zinc-ion batteries. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides an amino acid-modified electrolyte for an aqueous zinc ion battery and a preparation method thereof. The amino acid-modified electrolyte achieves no dendrite growth at the anode of the aqueous zinc ion battery, obtains a long cycle life, and effectively solves the problems of rapid capacity decay, low coulombic efficiency and battery short circuit caused by zinc dendrite growth in aqueous zinc ion batteries.
[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention to solve the technical problem is: an amino acid-modified electrolyte for an aqueous zinc ion battery, comprising a weakly acidic soluble zinc salt, an amino acid electrolyte additive and ultrapure water.
[0006] The amino acid electrolyte additive is one of leucine, lysine, valine and aspartic acid.
[0007] The preparation method of the amino acid-modified electrolyte for aqueous zinc ion batteries comprises the following steps:
[0008] S1. Add a weakly acidic soluble zinc salt into ultrapure water and stir until fully dissolved to obtain a basic zinc sulfate electrolyte;
[0009] S2. Adding an amino acid electrolyte additive to the basic zinc sulfate electrolyte obtained in step S1, and then stirring until fully dissolved, to obtain an amino acid-modified electrolyte for an aqueous zinc ion battery.
[0010] Furthermore, in step S1, the weakly acidic soluble zinc salt is one of zinc sulfate heptahydrate, zinc chloride and zinc trifluoromethanesulfonate.
[0011] Furthermore, the concentration of the weakly acidic soluble zinc salt in the basic zinc sulfate electrolyte is 0.5-3 mol / L.
[0012] Furthermore, in step S2, the concentration of the amino acid electrolyte additive in the electrolyte is 0.01-5 mol / L.
[0013] An aqueous zinc ion battery comprises the amino acid-modified electrolyte for aqueous zinc ion batteries, a transition metal-based positive electrode material, a negative electrode material and a diaphragm.
[0014] Furthermore, the transition metal-based positive electrode material is one of manganese dioxide, vanadium oxide, vanadate, vanadium sulfide and vanadium-based phosphate.
[0015] Furthermore, the negative electrode material is one of zinc foil, zinc powder and zinc foam.
[0016] Furthermore, the diaphragm is a glass fiber diaphragm.
[0017] In summary, the present invention has the following beneficial effects:
[0018] 1. The present invention selects a series of amino acids as electrolyte additives for aqueous zinc ion batteries, uses a simple process flow to prepare aqueous zinc ion battery electrolytes with high cycle life, and effectively improves the electrochemical performance of aqueous zinc ion batteries. Amino acids have hydrophilic / zinc-philic groups such as -NH2 and -COOH, which can improve the wettability of the electrolyte on the zinc anode surface, provide more and more uniform zinc deposition sites, inhibit the generation of zinc dendrites, extend the cycle life of aqueous zinc ion batteries, and effectively improve the discharge specific capacity and charge-discharge cycle stability of zinc ion batteries. At the same time, good electrolyte wettability is conducive to ion conduction in the battery system, reduces interfacial impedance, and improves battery electrochemical performance. In addition, amino acids have different properties due to their different structures, R groups, etc., and introducing different amino acids into aqueous zinc ion battery electrolytes can also play a modification effect such as adjusting pH and inhibiting side reactions.
[0019] 2. During the operation of aqueous zinc-ion batteries, Zn will self-corrode when in contact with aqueous electrolyte, that is, water molecules undergo hydrolysis to produce H + With OH - Among them, H + The electrolyte / anode interface is unstable and a hydrogen evolution reaction occurs, generating hydrogen gas, and a large number of pores are generated on the anode surface, causing the anode structure to collapse. Amino acids contain hydrophilic groups -NH2 and -COOH, which cannot be converted into NH2 in acidic electrolytes. - ,COOH - Such anion groups can attract the hydrolysis product H+ and combine with it, thereby reducing the occurrence of hydrogen evolution reaction, inhibiting a series of side reactions, and maintaining a stable and smooth zinc anode interface.
[0020] 3. Compared with the unmodified aqueous zinc-ion battery electrolyte, the Zn||Zn symmetric battery assembled with the electrolyte containing amino acids as electrolyte additives has a higher conductivity than the unmodified aqueous zinc-ion battery at 1 mA / cm 2 The cycle life under current density is increased from less than 100 hours to more than 2500 hours.
[0021] 4. Button battery assembled with modified electrolyte (Zn||NH4V4O 10 ) at 1mA / cm 2 The maximum discharge capacity at the current density is about 143.36 mAh g -1 The average specific capacity is 137.56 mAh g -1 After 1000 cycles, the capacity retention rate is 98.30%. The average specific capacity of the unmodified electrolyte is 115.36 mAh g -1 , and the capacity retention rate is 62.33% after 1000 cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The contact angle test results between different electrolytes and zinc foil are shown in the figure;
[0023] Figure 2 It is a time-voltage curve of a Zn||Zn symmetric battery using zinc sulfate solution as the electrolyte;
[0024] Figure 3 The time-voltage curve of the Zn||Zn symmetric battery using the amino acid-modified electrolyte prepared in Example 1;
[0025] Figure 4 The charge and discharge performance results of full batteries with different electrolyte compositions within 1000 cycles;
[0026] Figure 5 Scanning electron microscope images of zinc sheets after immersion in different electrolytes. DETAILED DESCRIPTION
[0027] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0028] Example 1
[0029] The preparation method of the amino acid-modified electrolyte for aqueous zinc ion batteries comprises the following steps:
[0030] S1. At 25°C, add 2.875 g of zinc sulfate heptahydrate to 5 mL of ultrapure water and stir until fully dissolved to obtain a basic zinc sulfate electrolyte with a concentration of 2 mol / L;
[0031] S2. Add 65.59 mg of leucine to the basic zinc sulfate electrolyte obtained in step S1, and then stir until fully dissolved, wherein the concentration of leucine in the electrolyte is 0.1 mol / L, to obtain an amino acid-modified electrolyte (Leu+ZnSO4) for aqueous zinc ion batteries.
[0032] Example 2
[0033] The preparation method of the amino acid-modified electrolyte for aqueous zinc ion batteries comprises the following steps:
[0034] S1. At 25°C, add 2.875 g of zinc sulfate heptahydrate to 5 mL of ultrapure water and stir until fully dissolved to obtain a basic zinc sulfate electrolyte with a concentration of 2 mol / L;
[0035] S2. Add 73.10 mg of lysine to the basic zinc sulfate electrolyte obtained in step S1, and then stir until fully dissolved, wherein the concentration of lysine in the electrolyte is 0.1 mol / L, to obtain an amino acid-modified electrolyte (Lys+ZnSO4) for an aqueous zinc ion battery.
[0036] Example 3
[0037] The preparation method of the amino acid-modified electrolyte for aqueous zinc ion batteries comprises the following steps:
[0038] S1. At 25°C, add 2.875 g of zinc sulfate heptahydrate to 5 mL of ultrapure water and stir until fully dissolved to obtain a basic zinc sulfate electrolyte with a concentration of 2 mol / L;
[0039] S2. Add 58.57 mg of valine to the basic zinc sulfate electrolyte obtained in step S1, and then stir until fully dissolved, wherein the concentration of valine in the electrolyte is 0.1 mol / L, to obtain an amino acid-modified electrolyte (Val+ZnSO4) for an aqueous zinc ion battery.
[0040] Example 4
[0041] The preparation method of the amino acid-modified electrolyte for aqueous zinc ion batteries comprises the following steps:
[0042] S1. At 25°C, add 2.875 g of zinc sulfate heptahydrate to 5 mL of ultrapure water and stir until fully dissolved to obtain a basic zinc sulfate electrolyte with a concentration of 2 mol / L;
[0043] S2. Add 66.55 mg of aspartic acid to the basic zinc sulfate electrolyte obtained in step S1, and then stir until fully dissolved, wherein the concentration of aspartic acid in the electrolyte is 0.1 mol / L, to obtain an amino acid-modified electrolyte (Asp+ZnSO4) for an aqueous zinc ion battery.
[0044] Example 5
[0045] The preparation method of the amino acid-modified electrolyte for aqueous zinc ion batteries comprises the following steps:
[0046] S1. At 25°C, add 0.341 g zinc chloride to 5 mL ultrapure water and stir until fully dissolved to obtain a basic zinc chloride electrolyte with a concentration of 0.5 mol / L;
[0047] S2. Add 6.559 mg of leucine to the basic zinc chloride electrolyte obtained in step S1, and then stir until fully dissolved, wherein the concentration of leucine in the electrolyte is 0.01 mol / L, to obtain an amino acid-modified electrolyte (Leu+ZnCl2) for aqueous zinc ion batteries.
[0048] Example 6
[0049] The preparation method of the amino acid-modified electrolyte for aqueous zinc ion batteries comprises the following steps:
[0050] S1. At 25°C, add 5.453 g of zinc trifluoromethanesulfonate to 5 mL of ultrapure water and stir until fully dissolved to obtain a basic zinc trifluoromethanesulfonate electrolyte with a concentration of 3 mol / L;
[0051] S2. Add 3.279 g of leucine to the basic zinc trifluoromethanesulfonate electrolyte obtained in step S1, and then stir until fully dissolved, wherein the concentration of leucine in the electrolyte is 5 mol / L, to obtain an amino acid-modified electrolyte (Leu+Zn(CF3SO3)2) for aqueous zinc ion batteries.
[0052] Comparative Example
[0053] A method for preparing a zinc sulfate solution comprises the following steps:
[0054] S1. At 25°C, disperse 2.875 g of zinc sulfate heptahydrate in 5 mL of ultrapure water and stir to make it dispersed evenly and fully dissolved to obtain a zinc sulfate solution (2M ZnSO4) with a concentration of 2 mol / L.
[0055] Test Example 1
[0056] The contact angles between the zinc sulfate solution obtained in the comparative example and the amino acid-modified electrolyte for aqueous zinc ion batteries obtained in Examples 1-4 and the zinc foil were tested. The results are as follows: Figure 1 As shown, Figure 1 In the figure, (a) is the contact angle of the zinc sulfate solution obtained in the comparative example, and (b)-(e) are the contact angles of the amino acid-modified electrolytes obtained in Examples 1-4, respectively.
[0057] Depend on Figure 1 It can be seen that the contact angle of the zinc sulfate solution obtained in the comparative example is 111.4°, the contact angle of the amino acid modified electrolyte obtained in Example 1 is 97.0°, the contact angle of the amino acid modified electrolyte obtained in Example 2 is 89.8°, the contact angle of the amino acid modified electrolyte obtained in Example 3 is 94.7°, and the contact angle of the amino acid modified electrolyte obtained in Example 4 is 88.6°. Compared with the zinc sulfate solution obtained in the comparative example, the contact angles of the amino acid modified electrolytes obtained in Examples 1-4 are all reduced, which indicates that the electrolyte modified with amino acids as additives has a better wetting effect with the zinc sheet, and the electrolyte can be better spread on the surface of the zinc sheet, which is beneficial to the Zn in the battery system. 2+ transmission.
[0058] Test Example 2
[0059] The zinc sulfate solution obtained in the comparative example and the amino acid-modified electrolyte obtained in Example 1 were used to assemble a Zn||Zn symmetric battery.
[0060] Assemble Zn||Zn symmetrical battery: The positive and negative shells used are both CR2016, the positive and negative electrodes are both high-purity zinc foil (thickness 0.1mm, diameter 12mm), the diaphragm is a glass fiber diaphragm (diameter 19mm), and the electrolyte is 40μL. The battery assembly order is positive electrode shell-zinc foil-diaphragm-electrolyte-zinc foil-gasket-negative electrode shell, and then the battery is pressurized to 50MPa and maintained for 10-30s. The preparation of Zn||Zn symmetrical battery is completed.
[0061] At 1mA / cm 2 and 1mAh / cm 2 The assembled symmetrical battery was subjected to constant current charge and discharge tests at a current density of Figure 2 and Figure 3 As shown, Figure 2 The time-voltage curve of the Zn||Zn symmetric battery assembled using the zinc sulfate solution obtained in the comparative example as the electrolyte is shown in FIG. Figure 3 The time-voltage curve of the Zn||Zn symmetric battery assembled using the amino acid-modified electrolyte prepared in Example 1.
[0062] Depend on Figure 2 and Figure 3 It can be seen that the cycle life of the Zn||Zn symmetric battery using the zinc sulfate solution obtained in the comparative example as the electrolyte is less than 200h. The cycle life of the Zn||Zn symmetric battery using the amino acid modified electrolyte prepared in Example 1 reaches more than 2500h. This is because the use of the electrolyte modified by amino acids effectively improves the cycle life of the symmetric aqueous zinc ion battery of the basic electrolyte and effectively improves the charge and discharge stability of the battery. The hydrophilic groups -NH2 and -COOH contained in the amino acids cannot remain stable in the acidic electrolyte and are converted into NH2 - ,COOH - anionic groups, which can attract H products produced during the hydrolysis side reaction + The zinc anode interface is kept stable and smooth, thus extending the cycle life of the battery.
[0063] Test Example 3
[0064] The zinc sulfate solution obtained in the comparative example and the amino acid-modified electrolyte obtained in Example 1 were used to assemble a Zn||Zn full battery.
[0065] Assemble Zn||NH4V4O 10Full battery: The positive and negative shells used are both CR2016, the positive electrode base material is stainless steel mesh (pore size 250 mesh), and the coating material is NH4V4O 10 The negative electrode is a high-purity zinc foil (thickness 0.1mm, diameter 12mm), the diaphragm is a glass fiber diaphragm (diameter 19mm), and the electrolyte is 40μL. The battery assembly sequence is positive electrode shell-positive electrode-diaphragm-electrolyte-zinc foil-gasket-negative electrode shell, and then the battery is pressurized to 50MPa and maintained for 10-30s. Complete Zn||NH4V4O 10 Preparation of full cells.
[0066] The charge and discharge performance of the assembled full battery was tested within 1000 cycles. Figure 4 shown.
[0067] Depend on Figure 4 It can be seen that the Zn||NH4V4O 10 The average specific capacity of the full battery after 1000 charge and discharge cycles is 115.36 mAh g -1 , the maximum specific capacity is 158.39 mAh g -1 The capacity retention rate during the cycle was 62.33%, and the average coulombic efficiency during the cycle was 99.90%. Zn||NH4V4O 10 The average specific capacity of the full battery after 1000 charge and discharge cycles is 137.56 mAh g -1 , the maximum specific capacity is 143.36 mAh g -1 The capacity retention rate of the cycle process is 98.30%, and the average coulombic efficiency during the cycle process is 99.94%. Compared with the original electrolyte, the electrolyte with leucine added has better cycle performance, larger specific capacity, and better capacity retention in the full battery. This shows that amino acids as additives can improve the relatively stable electrochemical reaction environment for aqueous zinc-ion batteries.
[0068] Test Example 4
[0069] The zinc sheet was immersed in the zinc sulfate solution prepared in the comparative example and the amino acid-modified electrolyte prepared in Example 1. After 7 days, the surface morphology was observed using a scanning electron microscope (SEM). The results are as follows: Figure 5 As shown, Figure 5 In the figure, (a) is a SEM image of the zinc sheet after being immersed in the zinc sulfate solution prepared in the comparative example, and (b) is a SEM image of the zinc sheet after being immersed in the amino acid-modified electrolyte prepared in Example 1.
[0070] Depend on Figure 5It can be seen that the size and distribution of basic zinc sulfate on the zinc sheet after being soaked in the zinc sulfate solution prepared in the comparative example are uneven, and obvious gaps and cracks due to hydrogen evolution reaction appear. The zinc deposition on the zinc sheet after being soaked in the amino acid-modified electrolyte prepared in Example 1 is uniform and neat, without obvious gaps and cracks. This is because during the operation of the aqueous zinc ion battery, Zn contacts the aqueous electrolyte and self-corrodes water, that is, water molecules undergo hydrolysis reaction to produce H + With OH - Among them, H + The electrolyte / anode interface is unstable and a hydrogen evolution reaction occurs, producing hydrogen gas, which creates a large number of pores on the anode surface and causes the anode structure to collapse. - ,COOH - The anion group attracts the product H in the hydrolysis side reaction + approach and combine with it, thereby reducing the occurrence of hydrogen evolution reaction, inhibiting a series of side reactions, and forming a flat and dense zinc anode interface.
[0071] In summary, the use of amino acid-modified electrolyte can effectively improve the electrochemical performance of aqueous zinc-ion batteries, achieve dendrite-free anode of aqueous zinc-ion batteries, and obtain a long cycle life.
[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. Amino acid modified electrolyte for aqueous zinc ion batteries, It is characterized in that The invention comprises a weakly acidic soluble zinc salt, an amino acid electrolyte additive and ultrapure water, wherein the amino acid electrolyte additive is one of leucine, lysine, valine and aspartic acid.
2. The method for preparing the amino acid-modified electrolyte for aqueous zinc ion batteries according to claim 1, It is characterized in that The following steps are involved: S1. Add a weakly acidic soluble zinc salt into ultrapure water and stir until fully dissolved to obtain a basic zinc sulfate electrolyte; S2. Adding an amino acid electrolyte additive to the basic zinc sulfate electrolyte obtained in step S1, and then stirring until fully dissolved, to obtain an amino acid-modified electrolyte for an aqueous zinc ion battery.
3. The method for preparing an amino acid-modified electrolyte for an aqueous zinc ion battery as claimed in claim 2, It is characterized in that In step S1, the weakly acidic soluble zinc salt is one of zinc sulfate heptahydrate, zinc chloride and zinc trifluoromethanesulfonate.
4. The method for preparing an amino acid-modified electrolyte for an aqueous zinc ion battery as claimed in claim 2, It is characterized in that In step S1, the concentration of the weakly acidic soluble zinc salt in the basic zinc sulfate electrolyte is 0.5-3 mol / L.
5. The method for preparing an amino acid-modified electrolyte for an aqueous zinc ion battery as claimed in claim 2, It is characterized in that In step S2, the concentration of the amino acid electrolyte additive in the amino acid-modified electrolyte for an aqueous zinc ion battery is 0.01-5 mol / L.
6. An aqueous zinc ion battery, It is characterized in that The invention comprises the amino acid-modified electrolyte for aqueous zinc ion batteries as claimed in claim 1, a transition metal-based positive electrode material, a negative electrode material and a diaphragm.
7. The aqueous zinc ion battery according to claim 6, It is characterized in that The transition metal-based positive electrode material is one of manganese dioxide, vanadium oxide, vanadate, vanadium sulfide and vanadium-based phosphate.
8. The aqueous zinc ion battery according to claim 6, It is characterized in that The negative electrode material is one of zinc foil, zinc powder and foamed zinc.
9. The aqueous zinc ion battery according to claim 6, It is characterized in that The diaphragm is a glass fiber diaphragm.
Citation Information
Cited By
Free manganese (II) inhibited anion-rich water system electrochemical system
CN119764606A
A free manganese (II) inhibited anion-rich aqueous electrochemical system
CN119764606B
Self-adaptive active regeneration zinc negative electrode-electrolyte interface stabilization method
CN119812514A
An adaptive active regeneration zinc negative electrode-electrolyte interface stabilization method
CN119812514B
Combined negative electrode additive for zinc-bromine flow battery, negative electrode electrolyte, preparation method of combined negative electrode additive and negative electrode electrolyte, and zinc-bromine flow battery
CN122068075A