Manufacturing method of antireflection film and antireflection film thereof
By using the same growth material to form multi-layer anti-reflection layers with different refractive indexes, the problem of high reflectivity of photodetectors in the CWDM4 band is solved, the process flow is simplified and the types of gas sources are reduced, achieving efficient reflectivity control and Transmitted light increases.
Patent Information
- Application Number
- CN202410904188.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
AI Technical Summary
The reflectivity of existing photodetectors in the CWDM4 band is high and the difference between bands is large. The preparation process of the multi-layer anti-reflection coating is complicated and requires a variety of materials and gas sources, which increases the difficulty of preparation and space occupation.
The same growth material (such as SiO) is used to form multi-layer anti-reflective layers with different refractive indexes through an epitaxial growth process. At least two anti-reflective layers are formed by adjusting deposition parameters to reduce reflected light and increase transmitted light, simplifying gas source types and processes. process.
It achieves similar reflectivity and reflectivity curves to those of anti-reflection coatings made by laminating multiple materials in the CWDM4 band, reducing gas source types and preparation costs, simplifying the process, reducing reflected light, and improving transmitted light. .
Smart Images

Figure CN118854441A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photoelectric detectors, and in particular to a method for manufacturing an anti-reflection film and the anti-reflection film. Background Art
[0002] At present, CWDM4 (4-wavelength sparse wavelength division multiplexer) is commonly used in optical communication and transmission. The 4 wavelengths are 1271nm, 1291nm, 1311nm and 1331nm, which requires the photodetector to have a high responsivity for the CWDM4 corresponding band, and the phase difference cannot be too large. Therefore, it is further required that the anti-reflection film on the surface of the photodetector has a low reflectivity for the CWDM4 corresponding wavelength, and the reflectivity curve in this band is relatively flat.
[0003] In order to optimize the anti-reflection film to reduce its reflectivity, common semiconductor processes generally use different materials (such as SiO, SiN, TiO, etc.) to form an anti-reflection film in a multi-layer alternating arrangement to achieve a higher transmittance and lower reflectivity in a certain band. However, since the above-mentioned anti-reflection film needs to use a variety of materials to make the film layer of the multi-layer anti-reflection film, it is necessary to provide a variety of different gas sources or gas source combinations to generate different film layers, which increases the difficulty of the preparation process and also increases the preparation space and operation area due to the storage and use of the gas source during the preparation process.
[0004] In view of this, there is a real need for a new type of anti-reflection film and a method for preparing the anti-reflection film. Summary of the invention
[0005] In order to solve at least one aspect of the above problems and defects in the prior art, the embodiments of the present invention provide a method for manufacturing an antireflection film and an antireflection film thereof, which uses the same growth material to form a multilayer antireflection layer with different refractive indices, thereby achieving the same antireflection effect as an antireflection film formed by stacking different materials, and reducing the types of gas sources used. The technical solution is as follows:
[0006] According to one aspect of the present invention, a method for manufacturing an antireflection film is provided.
[0007] The method for manufacturing the antireflection film comprises:
[0008] Providing growth materials for anti-reflection films;
[0009] Providing a gas source corresponding to the growth material of the antireflection film;
[0010] Using the same growth material to sequentially form at least two anti-reflection layers of an anti-reflection film on the substrate layer;
[0011] At least two anti-reflection layers and the substrate layer together form an anti-reflection film, which can be used to reduce reflected light and increase transmitted light.
[0012] Specifically, in the step of sequentially forming at least two anti-reflection layers of an anti-reflection film on a substrate layer using the same growth material, at least two anti-reflection layers are formed by an epitaxial growth process, and the refractive indices of two adjacent anti-reflection layers in the at least two anti-reflection layers are different by adjusting deposition parameters of the epitaxial growth.
[0013] In some embodiments, the substrate layer includes a SiO layer, a Si layer and an absorption layer in sequence along the film growth direction; and the growth material of the antireflection film is SiO.
[0014] Furthermore, the gas source corresponding to the growth material of the above antireflection film is a gas source combination of SiH4, N2O and N2.
[0015] In some embodiments, the at least two anti-reflection layers include two layers, including a first anti-reflection layer and a second anti-reflection layer.
[0016] In some embodiments, the epitaxial growth process uses plasma enhanced chemical vapor deposition (PECVD).
[0017] Specifically, the deposition parameters include any one of the following or any combination thereof:
[0018] The flow rates of Si H4, N2O and N2 are used to control the refractive index of each anti-reflection layer in at least two anti-reflection layers;
[0019] The film deposition time is used to control the thickness of each anti-reflection layer in at least two anti-reflection layers.
[0020] In some embodiments, the step of forming the anti-reflection film includes:
[0021] After the substrate layer is subjected to a semiconductor cleaning process, the substrate layer is placed on a CVD deposition device;
[0022] Control the upper electrode temperature of the CVD deposition equipment to 200-300°C and the lower electrode temperature to 250-350°C;
[0023] Adjusting a first deposition parameter of a CVD deposition device to grow a first anti-reflection layer;
[0024] A second deposition parameter of the CVD deposition equipment is adjusted to grow a second anti-reflection layer on the first anti-reflection layer.
[0025] In some embodiments,
[0026] When growing the first anti-reflection layer, the corresponding first deposition parameters include any one of the following or any combination thereof: first volume flow rates of Si H4, N2O and N2; first gas pressure; first radio frequency power of the CVD deposition equipment; first film deposition time;
[0027] When growing the second anti-reflection layer, the corresponding second deposition parameters include any one or any combination of the following: a second volume flow rate of Si H4, N2O and N2; a second gas pressure; a second RF power of the CVD deposition equipment; and a second thin film deposition time.
[0028] According to another aspect of the present invention, there is also provided an anti-reflection film, which is prepared by the method for manufacturing the anti-reflection film described in the above aspect, and the anti-reflection film comprises:
[0029] substrate layer;
[0030] A first anti-reflection layer is formed on the substrate layer from a growth material by an epitaxial growth process, the first anti-reflection layer has a thickness ranging from 10 to 200 nm and a refractive index ranging from 1.4 to 1.7;
[0031] A second anti-reflection layer is formed on the first anti-reflection layer from the same growth material through an epitaxial growth process, the second anti-reflection layer has a thickness ranging from 10 to 200 nm and a refractive index ranging from 1.4 to 1.7;
[0032] The application spectrum of the anti-reflection film is the CWDM4 band, with a wavelength range of 1270nm to 1331nm.
[0033] A method for manufacturing an anti-reflection film and an anti-reflection film thereof provided by an embodiment of the present invention have at least one or part of the following advantages:
[0034] (1) The method for manufacturing an antireflection film provided by the present invention uses the same growth material to form a multilayer antireflection layer with different refractive indices, thereby reducing reflected light while increasing transmitted light;
[0035] (2) The method for manufacturing the antireflection film provided by the present invention uses the same growth material. Compared with the manufacturing method using multiple growth materials, the types of gas sources corresponding to the growth materials are reduced, the space occupied by the gas source is reduced, the process flow is simplified, and the preparation cost is saved;
[0036] (3) The antireflection film prepared by the method for preparing the antireflection film provided by the present invention has the same or similar reflectivity value and reflectivity curve curvature as the antireflection film prepared by stacking multiple materials;
[0037] (4) The anti-reflection film prepared by the method for manufacturing the anti-reflection film provided by the present invention can be used in the CDWM4 band. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] These and / or other aspects and advantages of the present invention will become apparent and readily understood from the following description of the preferred embodiments in conjunction with the accompanying drawings, in which:
[0039] Figure 1 is a flow chart of a method for manufacturing an antireflection film according to an embodiment of the present invention;
[0040] Figure 2 is a schematic structural diagram of an antireflection film according to an embodiment of the present invention;
[0041] Figure 3 for Figure 1 A flow chart of an anti-reflection layer deposition process in a method for manufacturing an anti-reflection film shown;
[0042] Figure 4 A comparison diagram of a reflectivity curve of a double-layer anti-reflection film according to an embodiment of the present invention and reflectivity curves of double-layer anti-reflection films and a single-layer anti-reflection film made of different materials;
[0043] Figure 5 It is a comparison diagram of the reflectivity curves of the double-layer anti-reflection films according to Examples 1 and 2 of the present invention and the reflectivity curves of double-layer anti-reflection films made of different materials. DETAILED DESCRIPTION
[0044] The technical solution of the present invention is further specifically described below by examples and in conjunction with the accompanying drawings. In the specification, the same or similar reference numerals indicate the same or similar components. The following description of the embodiments of the present invention with reference to the accompanying drawings is intended to explain the overall inventive concept of the present invention and should not be construed as a limitation of the present invention.
[0045] Anti-reflection film, also known as anti-reflection film, has the main function of reducing or eliminating the reflected light from optical surfaces (such as lenses, prisms, plane mirrors, etc.), thereby increasing the light transmittance of the optical surface and reducing or eliminating stray light.
[0046] The working principle of the anti-reflection film is as follows: when light is incident on the anti-reflection film, on the one hand, the light forms the first reflection on the surface of the anti-reflection film; on the other hand, the light transmits through the anti-reflection film, forms the second reflection at the bottom of the anti-reflection film, and then emits from the surface of the anti-reflection film after transmission. At this time, interference will occur between the first reflected light and the second reflected light, thereby weakening the reflected light. According to the law of conservation of energy, the total energy of light remains unchanged, so when the reflected light decreases, the transmitted light increases.
[0047] In order to further reduce reflected light, it is common to use multi-layer materials with different anti-reflection films to reduce the reflectivity, and at the same time, the reflectivity curve can be flattened. Using a certain material to form a corresponding anti-reflection film requires a corresponding gas source or gas source combination, and different materials correspond to different gas sources or gas source combinations. Specifically, the corresponding gas source A1 of material A is used to form an anti-reflection layer 1, and the corresponding gas source B1 of material B is used to form an anti-reflection layer 2 on the anti-reflection layer 1, and so on. In order to eventually form N layers of anti-reflection layers, N types of materials are required, and accordingly, N types of gas sources or gas source combinations are required. This will result in the multi-layer superimposed anti-reflection film having a better effect in reducing the reflectivity, but the types of gas sources used are very many, which will increase the difficulty of controlling the preparation process. Storing or calling the gas source also requires a larger working space, occupying a larger area.
[0048] In order to reduce the use of gas sources and at the same time ensure that the anti-reflection film has a better anti-reflection effect, an embodiment of the present invention provides a novel method for manufacturing an anti-reflection film.
[0049] refer to Figure 1 The method for manufacturing the antireflection film comprises the following steps:
[0050] S101: providing growth materials for an antireflection film;
[0051] S102: providing a gas source corresponding to a growth material of the antireflection film;
[0052] S103: using the same growth material to sequentially form at least two anti-reflection layers of an anti-reflection film on the substrate layer;
[0053] S104: At least two anti-reflection layers and the substrate layer together form an anti-reflection film.
[0054] In one example, based on the wavelength range of CDWM4 (1271nm~1331nm), SiO material can be optionally used as the growth material of the anti-reflection film. In theory, in addition to SiO material, other materials can also be used as the growth material of the anti-reflection film, such as SiO2, Si N, ZnS, Ta2O3, TiO2, Al2O3, MgF2, etc. Different materials have different refractive indices, and different film growth parameters need to be adjusted during use. Of course, the choice of using SiO in this example is only an illustrative example, and those skilled in the art should not be understood as a limitation of the present invention.
[0055] In one example, after SiO is selected as the growth material of the anti-reflection film, a growth gas source corresponding to the SiO growth material can be further provided. This embodiment provides a gas source combination, specifically Si H4, N2O and N2. For the same growth material, the gas source or gas source combination that can be used is not unique. This example is only an illustrative example, and those skilled in the art should not be understood as a limitation of the present invention.
[0056] In one example, the at least two anti-reflection layers may be two, three or more layers. As the number of anti-reflection layers increases, although the anti-reflection performance within a specific wavelength range can be further improved, the difficulty of matching the thickness and refractive index of each anti-reflection layer will also increase. In the following embodiments provided by the present invention, two anti-reflection layers, namely the first anti-reflection layer and the second anti-reflection layer, are used under the premise of ensuring better anti-reflection performance. Of course, the design scheme of the number of anti-reflection layers involved in this example is only an illustrative example, and those skilled in the art should not be understood as a limitation of the present invention.
[0057] In one example, reference Figure 2 , shows a schematic diagram of the cross-sectional structure of an anti-reflection film 100 according to an embodiment of the present invention, the anti-reflection film 100 includes two parts, one part is a substrate layer 10, and the other part is an anti-reflection layer structure formed on the substrate layer 10, the anti-reflection layer structure includes a first anti-reflection layer 20 and a second anti-reflection layer 30 formed on the first anti-reflection layer 20.
[0058] In one example, specifically, the substrate layer 10 is a multilayer structure including multiple materials. After the growth material is selected, the multilayer structure of the substrate layer 10 is generally fixed. The substrate layer 10 of this embodiment is arranged along the film growth direction ( Figure 2 The first anti-reflection layer 20 and the second anti-reflection layer 30 are made of SiO.
[0059] In one example, two anti-reflection layers, namely the first anti-reflection layer 20 and the second anti-reflection layer 30, are formed by an epitaxial growth process, and the refractive indices of the adjacent first anti-reflection layer 20 and the second anti-reflection layer 30 are different by adjusting deposition parameters of the epitaxial growth.
[0060] Common epitaxial growth processes used for the preparation of antireflection films mainly include: sol-gel method (Sol-gel), chemical vapor deposition (CVD), sputtering method, etc., among which chemical vapor deposition (CVD) is a more commonly used one.
[0061] Chemical vapor deposition (CVD) is a thin film deposition technology that mainly uses one or more gas phase compounds or single substances containing thin film elements to chemically react on the substrate surface to form a thin film. Chemical vapor deposition technology is a new technology for preparing inorganic materials developed in recent decades. It has been widely used to purify substances, develop new crystals, and deposit various single crystal, polycrystalline or glassy inorganic thin film materials. These materials can be oxides, sulfides, nitrides, carbides, or binary or multi-element compounds in II IV, III V, IV-VI groups. The physical properties of these inorganic thin film materials can be precisely controlled through the deposition process of gas phase doping.
[0062] Chemical vapor deposition (CVD) has many advantages: small directionality of film formation, good microscopic uniformity; high film purity, small residual stress, strong ductility; and small radiation damage to the film. Therefore, for the anti-reflection film of this embodiment, a plasma enhanced chemical vapor deposition method (PECVD) can be optionally used for the epitaxial growth of the anti-reflection film.
[0063] In one example, reference Figure 3 The steps of forming the antireflection film of this embodiment by epitaxial growth using a CVD deposition device corresponding to a plasma enhanced chemical vapor deposition method (PECVD) include:
[0064] S301: After performing a semiconductor cleaning process on the substrate layer 10, the substrate layer 10 is placed on a CVD deposition device;
[0065] S302: Controlling the upper electrode temperature of the CVD deposition equipment to 200-300° C. and the lower electrode temperature to 250-350° C.;
[0066] S303: adjusting a first deposition parameter of a CVD deposition device to grow a first anti-reflection layer 20;
[0067] S304 : adjusting a second deposition parameter of the CVD deposition equipment to grow a second anti-reflection layer 30 on the first anti-reflection layer 20 .
[0068] In one example, specifically, the deposition parameters (ie, the first deposition parameters and the second deposition parameters) mainly include any one of the following or any combination thereof:
[0069] (1) The flow rates of SiH4, N2O and N2 are used to control the refractive index of each anti-reflection layer in each anti-reflection layer;
[0070] (2) Thin film deposition time is used to control the thickness of each anti-reflection layer in each anti-reflection layer. The shorter the epitaxial growth time, the thinner the anti-reflection layer; conversely, the longer the epitaxial growth time, the thicker the anti-reflection layer. Alternatively, the thin film deposition rate is controlled to be 40 nm / min, thereby controlling the overall time for forming the anti-reflection layer to be in the range of 0 to 10 min.
[0071] Specifically in this embodiment, the first anti-reflection layer 20 and the second anti-reflection layer 30 have different refractive indices and thicknesses, and together with the substrate layer 10 below the first anti-reflection layer 20, form an anti-reflection film 100 to reduce light reflection and increase light transmission.
[0072] In one example, by controlling the deposition parameters of the CVD deposition equipment, the structures and properties of the first anti-reflection layer 20 and the second anti-reflection layer 30 in the anti-reflection film obtained in this embodiment are as follows:
[0073] The first anti-reflection layer 20 has a thickness ranging from 10 to 200 nm and a refractive index ranging from 1.4 to 1.7;
[0074] The second anti-reflection layer 30 has a thickness ranging from 10 to 200 nm and a refractive index ranging from 1.4 to 1.7.
[0075] In one example, reference Figure 4 , shows the reflectivity curve of the anti-reflection film of the above example compared with the performance of a single-layer anti-reflection film and a double-layer anti-reflection film of different growth materials in the CWDM4 band range. Specifically, curve a in the figure is the reflectivity curve of the embodiment Figure 2 The reflectivity curve of the double-layer anti-reflection film of the same growth material is given, curve b is the reflectivity curve of the existing double-layer anti-reflection film of different growth materials, and curve c is the reflectivity curve of the single-layer anti-reflection film.
[0076] From the shapes of curves a, b and c, it can be seen that the reflectivity of a single-layer anti-reflection film fluctuates greatly with wavelength changes, ranging from 5% to 20%; in contrast, the reflectivity of a double-layer anti-reflection film fluctuates very little with wavelength changes, basically in the range of 10%±3%, and its maximum reflectivity (about 13%) is less than the maximum reflectivity of a single-layer anti-reflection film (about 20%).
[0077] Furthermore, by comparing curve a and curve b, the double-layer antireflection film made of the same growth material in this embodiment can achieve substantially the same reflective performance as the double-layer antireflection film made of different growth materials. Although there is a certain fluctuation in reflectivity, the fluctuation range does not exceed 2%, and the maximum reflectivity is 13%±1%. Since the double-layer antireflection film in this embodiment uses the same growth material, compared with the double-layer antireflection film made of different growth materials, the use of gas source is saved, thereby reducing the difficulty of preparation, reducing the preparation process space and the area occupied by the gas source.
[0078] In one example, two sets of antireflection films are formed using two sets of deposition parameters respectively. The formation process and performance parameters of the two sets of antireflection films are specifically described below through Example 1 and Example 2:
[0079] Embodiment 1:
[0080] After the substrate layer 10 is subjected to a semiconductor cleaning process, the substrate layer 10 is placed in a CVD deposition device;
[0081] The first deposition parameters of the CVD deposition equipment are adjusted to form the first anti-reflection layer 20, wherein the first deposition parameters include:
[0082] The first volume flow rate of Si H4 is 8 sccm, and the first gas pressure is 600 mTorr;
[0083] The first volume flow rate of N2O is 530 sccm;
[0084] The first volume flow rate of N2 is 625 sccm;
[0085] The first radio frequency power of the CVD deposition equipment is 60W;
[0086] The first film deposition time was 15 s;
[0087] The thickness of the first anti-reflection layer 20 obtained at this time is 10 nm, and the refractive index is 1.46;
[0088] On the basis of the first anti-reflection layer 20, the second deposition parameters of the CVD deposition equipment are adjusted to generate the second anti-reflection layer 30, wherein the second deposition parameters include:
[0089] The second volume flow rate of Si H4 is 8 sccm, and the second gas pressure is 600 mTorr;
[0090] The second volume flow rate of N2O is 50 sccm;
[0091] The second volume flow rate of N2 is 1105 sccm;
[0092] The second RF power of the CVD deposition equipment is 60W;
[0093] The second film deposition time was 278 s;
[0094] The thickness of the second anti-reflection layer 30 obtained at this time was 185 nm, and the refractive index was 1.65.
[0095] Embodiment 2:
[0096] After the substrate layer 10 is subjected to a semiconductor cleaning process, the substrate layer 10 is placed in a CVD deposition device;
[0097] The first deposition parameters of the CVD deposition equipment are adjusted to form the first anti-reflection layer 20, wherein the first deposition parameters include:
[0098] The first volume flow rate of Si H4 is 8 sccm, and the first gas pressure is 600 mTorr;
[0099] The first volume flow rate of N2O is 50 sccm;
[0100] The first volume flow rate of N2 is 1105 sccm;
[0101] The first radio frequency power of the CVD deposition equipment is 60W;
[0102] The first film deposition time was 285 s;
[0103] The thickness of the first anti-reflection layer 20 obtained at this time is 190 nm, and the refractive index is 1.65;
[0104] On the basis of the first anti-reflection layer 20, the second deposition parameters of the CVD deposition equipment are adjusted to generate the second anti-reflection layer 30, wherein the second deposition parameters include:
[0105] The second volume flow rate of Si H4 is 8 sccm, and the second gas pressure is 600 mTorr;
[0106] The second volume flow rate of N2O is 530 sccm;
[0107] The second volume flow rate of N2 is 625 sccm;
[0108] The second RF power of the CVD deposition equipment is 60W;
[0109] The second film deposition time is 15 s;
[0110] The thickness of the second antireflection layer obtained at this time was 10 nm, and the refractive index was 1.46.
[0111] Right now,
[0112] The combination of the double-layer antireflection film of the same growth material in Example 1 is: 10nm (refractive index 1.46) + 185nm (refractive index 1.65);
[0113] The combination of the double-layer antireflection film of the same growth material in Example 2 is: 190nm (refractive index 1.65)+10nm (refractive index 1.46).
[0114] Furthermore, the reflectivity curves of the anti-reflection films obtained in Example 1 and Example 2 can be plotted using simulation calculations, and compared with the reflectivity curves of double-layer anti-reflection films using different growth materials.
[0115] Specifically, refer to Figure 5 The reflectivity curve corresponding to Example 1 is curve a1, the reflectivity curve corresponding to Example 2 is curve a2, and the reflectivity curve corresponding to the double-layer anti-reflection film of different growth materials is curve b.
[0116] Compared with curve a1 and curve a2, the reflectivity curves are almost overlapped, the reflection effects are basically the same, and the reflectivity can be controlled within the range of 10%±3%.
[0117] Compared with curve b, curves a1 and a2 achieve similar reflection effects. Within the CDWM4 band, the reflectivity curvature changes of curves a1 and a2 can be relatively gentle, and the maximum reflectivity does not exceed 12% (the maximum reflectivity of curve b is about 11.5%).
[0118] A method for manufacturing an anti-reflection film and an anti-reflection film thereof provided by an embodiment of the present invention have at least one or part of the following advantages:
[0119] (1) The method for manufacturing an antireflection film provided by the present invention uses the same growth material to form a multilayer antireflection layer with different refractive indices, thereby reducing reflected light while increasing transmitted light;
[0120] (2) The method for manufacturing the antireflection film provided by the present invention uses the same growth material. Compared with the manufacturing method using multiple growth materials, the types of gas sources corresponding to the growth materials are reduced, the space occupied by the gas source is reduced, the process flow is simplified, and the preparation cost is saved;
[0121] (3) The antireflection film prepared by the method for preparing the antireflection film provided by the present invention has the same or similar reflectivity value and reflectivity curve curvature as the antireflection film prepared by stacking multiple materials;
[0122] (4) The anti-reflection film prepared by the method for manufacturing the anti-reflection film provided by the present invention can be used in the CDWM4 band.
[0123] Although some embodiments of the present general inventive concept have been shown and described, it will be appreciated by those skilled in the art that changes may be made to these embodiments without departing from the principles and spirit of the present general inventive concept, the scope of which is defined by the claims and their equivalents.
Claims
1. A method for manufacturing an antireflection film, comprising: Providing a growth material for the antireflection film; Providing a gas source corresponding to the growth material of the antireflection film; Using the same growth material to sequentially form at least two anti-reflection layers of the anti-reflection film on a substrate layer; The at least two anti-reflection layers and the substrate layer together form an anti-reflection film, and the anti-reflection film can be used to reduce reflected light and increase transmitted light.
2. The method for manufacturing an antireflection film according to claim 1, characterized in that: In the step of sequentially forming at least two anti-reflection layers of the anti-reflection film on the substrate layer using the same growth material, the at least two anti-reflection layers are formed by an epitaxial growth process, and the refractive indices of two adjacent anti-reflection layers in the at least two anti-reflection layers are different by adjusting deposition parameters of the epitaxial growth.
3. The method for manufacturing an antireflection film according to claim 1, characterized in that: The substrate layer includes a SiO layer, a Si layer and an absorption layer in sequence along the film growth direction; The growth material of the antireflection film is SiO.
4. The method for manufacturing an antireflection film according to claim 3, characterized in that: The gas source corresponding to the growth material of the anti-reflection film is a gas source combination of SiH4, N2O and N2.
5. The method for manufacturing an antireflection film according to any one of claims 1 to 4, characterized in that: The number of the at least two anti-reflection layers is two, and the at least two anti-reflection layers include a first anti-reflection layer and a second anti-reflection layer.
6. The method for manufacturing an antireflection film according to claim 5, characterized in that: The epitaxial growth process uses a plasma enhanced chemical vapor deposition method (PECVD).
7. The method for manufacturing an antireflection film according to claim 6, characterized in that: The deposition parameters include any one of the following or any combination thereof: The flow rates of SiH4, N2O and N2 are used to control the refractive index of each anti-reflection layer in the at least two anti-reflection layers; The thin film deposition time is used to control the thickness of each anti-reflection layer in the at least two anti-reflection layers.
8. The method for manufacturing an antireflection film according to claim 7, characterized in that: The steps of forming the antireflection film include: After performing a semiconductor cleaning process on the substrate layer, placing the substrate layer on a CVD deposition device; Controlling the upper electrode temperature of the CVD deposition equipment to be 200-300° C. and the lower electrode temperature to be 250-350° C.; Adjusting a first deposition parameter of the CVD deposition equipment to grow a first anti-reflection layer; A second deposition parameter of the CVD deposition equipment is adjusted to grow a second anti-reflection layer on the first anti-reflection layer.
9. The method for manufacturing an antireflection film according to claim 8, characterized in that: When growing the first anti-reflection layer, the first deposition parameter includes any one of the following or any combination thereof: a first volume flow rate of SiH4, N2O and N2; a first gas pressure; a first radio frequency power of a CVD deposition device; a first film deposition time; When growing the second anti-reflection layer, the second deposition parameters include any one of the following or any combination thereof: a second volume flow rate of SiH4, N2O and N2; a second gas pressure; a second RF power of the CVD deposition equipment; and a second thin film deposition time.
10. An anti-reflection film, prepared by the method for manufacturing an anti-reflection film according to any one of claims 1 to 9, the anti-reflection film comprising: substrate layer; A first anti-reflection layer is formed on the substrate layer from a growth material by an epitaxial growth process, wherein the first anti-reflection layer has a thickness ranging from 10 to 200 nm and a refractive index ranging from 1.4 to 1.7; a second anti-reflection layer, formed on the first anti-reflection layer from the same growth material through an epitaxial growth process, the second anti-reflection layer having a thickness ranging from 10 to 200 nm and a refractive index ranging from 1.4 to 1.7; The application spectrum of the antireflection film is the CWDM4 band, and the wavelength range is 1270nm to 1331nm.
Citation Information
Cited By
Optical waveguide structure, preparation method thereof and head-mounted display device
CN119535670A