Method for manufacturing patterned film substrate
By using specific fluorine-containing copolymers on the patterned film substrate and performing heat treatment, the problem of degradation of liquid repellency after cleaning is solved, the lyophilicity and liquid repellency of the patterned film are restored, and the inkjet method is improved Ink dropwise accuracy.
Patent Information
- Application Number
- CN202410951636.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-23
- Filing Date
- 2019-05-23
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, after UV ozone cleaning or oxygen plasma cleaning, the liquid repellency of the dam will decrease, resulting in the problem of ink crossing or dissolving the dam in ink.
UV ozone cleaning or oxygen plasma cleaning is used with a patterned film substrate containing a specific fluorine-containing copolymer, and the liquid repellency is restored by heating. The specific fluorine-containing copolymer is used to reduce the free energy of the film surface by heating after cleaning. The fluoroalkyl group moves toward the surface of the film to restore liquid repellency.
Effectively maintain the lyophilicity of the concave substrate surface of the pattern film, while restoring the liquid repellency, preventing the ink from crossing or dissolving in the ink dam, and improving the accuracy of ink dropping ink in the inkjet method.
Smart Images

Figure BDA0004947391820000061 
Figure BDA0004947391820000071 
Figure BDA0004947391820000072
Abstract
Description
[0001] The present invention is a divisional application of the Chinese patent application with application number 201980034770.9, application date May 23, 2019, and invention name “Method for manufacturing patterned film substrate”. This application claims the priority of Japanese Patent Application No. 2018-098679 filed in Japan on May 23, 2018. Technical Field
[0002] The present application relates to a method for manufacturing a patterned film substrate. The method for manufacturing a patterned film substrate in the present application can be used, for example, in the manufacture of a display element based on an inkjet method. As the display element, for example, an organic electroluminescent display (hereinafter, an organic EL display), a micro light emitting diode display (hereinafter, a micro LED display) or a quantum dot display can be listed. Background Art
[0003] It is well known to manufacture display elements such as organic EL displays, micro LED displays or quantum dot displays using an inkjet method.
[0004] As methods for manufacturing these display elements using an inkjet method, there can be listed: a method of dripping droplets of ink onto concave portions of a pattern formed on a substrate in the form of projections and recesses of the film through a nozzle and solidifying the resultant; or a method of dripping droplets of ink onto a pattern film pre-formed on a substrate as a lyophilic portion and a lyophobic portion, thereby causing the ink to adhere to the lyophilic portion, wherein the lyophilic portion is a portion that wets with ink and the lyophobic portion is a portion that repels ink.
[0005] In the method of dripping ink droplets to the depressions (concave parts) of the pattern film with concave and convex parts through a nozzle to solidify them, in order to prepare such a pattern film, the following methods can be used: a photolithography method in which a pattern consisting of an exposed part and an unexposed part is formed by exposing the surface of the resist film formed on the substrate in a patterned manner, dissolving any part in a developer, and forming concave and convex parts on the resist film; or an imprinting method in which a pattern film with concave and convex parts is formed on the substrate using a printing technique. In such a pattern film with concave and convex parts, the substrate surface of the concave parts is preferably exposed, and the exposed substrate surface is preferably lyophilic.
[0006] In the inkjet method, the convex parts of the pattern film having concavoconvexities are called banks. When ink is dropped into the concave parts of the pattern film by inkjet, the banks function as a barrier to prevent the mixing of ink.
[0007] For example, Patent Document 1 discloses a composition for an organic EL element used as ink in the manufacture of an organic EL display using an inkjet method. Patent Document 1 also describes that a bank is previously manufactured on a substrate, and an ink (composition for an organic EL element) for forming a light-emitting layer is dripped to manufacture a display element for an organic EL display.
[0008] Patent Document 2 discloses a method for manufacturing a color filter for liquid crystal, characterized in that a photosensitive compound layer is formed on a light-shielding portion on a light-transmitting substrate on which a light-shielding portion is formed by photolithography, and then an inkjet recording device is used to eject ink so that a colorant is arranged on the light-transmitting portion, wherein the photosensitive compound layer contains a surface tension or a critical surface tension of 2.5×10 -2 [N / m] or less. Patent Document 2 also states that when ink is dripped into the concave portion of the pattern film by inkjet, the photosensitive compound layer forming the dam contains a fluorine-based polymer or a fluorine-based surfactant, thereby improving the liquid repellency of the dam and preventing the ink from crossing the dam and invading the adjacent concave portion.
[0009] Patent document 3 discloses a lyophobic resist composition for obtaining a pattern consisting of a lyophobic region and a lyophilic region by photolithography. Patent document 3 also states that by using the lyophobic resist composition, a lyophobic-lyophilic pattern having a clear ink wetting contrast can be formed on a substrate by an inkjet method, and that when ink is dripped into a concave portion of a pattern film by an inkjet method, the surface of the substrate as the concave portion is made lyophilic and the surface of the dam is made lyophobic.
[0010] Patent Document 4 discloses a patterning substrate for inkjet method, which has a thin film on which a bank of a predetermined height and a coated area separated by the bank are formed. Patent Document 4 also states that the coated area as a concave portion is lyophilic, and the bank as a convex portion is lyophobic.
[0011] Patent Document 5 discloses a positive photosensitive resin composition that can form an image having high hydrophobicity and oleophobicity on the surface of a cured film. Patent Document 5 also states that the positive photosensitive resin composition is suitable for use as an interlayer insulating film in a liquid crystal display or an EL display, a light shielding material or a spacer material corresponding to an inkjet method.
[0012] In addition, Patent Documents 4 and 5 also record that when a pattern film is formed on a substrate by photolithography, the substrate surface as the concave portion of the pattern film is contaminated by organic matter, and when a pattern film is formed by an imprinting method, film residue occurs in the concave portion of the pattern film. Due to these defects, the concave portion of the pattern film becomes hydrophobic, so a hydrophilic treatment is performed on a substrate with a pattern film using a hydrophilic ink to make the concave portion of the pattern film hydrophilic. When the hydrophilic treatment is performed, the concave portion of the pattern film does not repel ink during inkjet printing, and ink can be dripped onto the substrate with the pattern film well.
[0013] Patent Document 4 also describes that by bringing a pattern film-attached substrate into contact with oxygen plasma gas and fluorine plasma gas, the substrate surface as the concave portion of the pattern film is made hydrophilic and the bank of the convex portion is made hydrophobic.
[0014] According to the positive photosensitive resin composition described in Patent Document 5, a substrate with a patterned film can be obtained in which the surface of the patterned film as a bank remains highly liquid-repellent after UV ozone cleaning during the hydrophilization treatment.
[0015] Prior art literature
[0016] Patent Literature
[0017] Patent Document 1: Japanese Patent Application Laid-Open No. 11-54270
[0018] Patent Document 2: Japanese Patent Application Laid-Open No. 10-197715
[0019] Patent Document 3: Japanese Patent Application Publication No. 2012-220860
[0020] Patent Document 4: Japanese Patent Application Publication No. 2000-353594
[0021] Patent Document 5: International Publication No. 2017 / 126610 Summary of the invention
[0022] 1. Technical issues to be resolved
[0023] As described in Patent Documents 4 and 5, in order to improve the lyophilicity of the substrate surface serving as the concave portion of the pattern film, when the substrate with the pattern film is subjected to UV ozone cleaning or oxygen plasma cleaning, the lyophobicity of the dam will decrease after cleaning, and when ink is dripped into the concave portion of the pattern film by an inkjet method, there is a problem of the ink crossing over the dam or the dam dissolving in the ink.
[0024] The present application provides a method for manufacturing a patterned film substrate that solves the above-mentioned problems.
[0025] (II) Technical solution
[0026] The inventors of the present application conducted in-depth research to solve the above-mentioned problems, and found that when a patterned film substrate containing a specific fluorinated copolymer is subjected to UV ozone cleaning or oxygen plasma cleaning, the liquid repellency of the patterned film will temporarily decrease, but the liquid repellency can be restored (the liquid repellency is restored) by subsequent heating.
[0027] For pattern films containing specific fluorinated copolymers, after UV ozone cleaning or oxygen plasma cleaning, it is observed that the lyophobicity to water and anisole used as an ink solvent in the inkjet method decreases, but by heating the pattern film, the decreased lyophobicity to water and anisole will be restored (see Table 2 and Table 4 of [Examples] of this specification). Similarly, for pattern films containing specific fluorinated copolymers, after UV ozone cleaning or oxygen plasma cleaning, it is observed that the lyophobicity to propylene glycol monomethyl ether acetate (PGMEA) and xylene decreases, but by heating the pattern film, the decreased lyophobicity to PGMEA and xylene will be restored (see Table 6 and Table 8 of [Examples] of this specification). In this way, the inventors of the present application unexpectedly found that for pattern films containing specific fluorinated copolymers, the lyophobicity is significantly restored by heating after UV cleaning.
[0028] It is speculated that the reason why the liquid repellency is restored by heating is that the membrane surface is oxidized and becomes liquid-philic by UV ozone cleaning or oxygen plasma cleaning, but because a special fluorinated copolymer that can inhibit the cleavage of the polymer main chain is used, the fluoroalkyl part with small surface free energy moves to the membrane surface due to the molecular movement caused by heating.
[0029] In the present application, UV ozone cleaning refers to a method of removing organic pollutants by irradiating a substrate with a patterned film with ultraviolet rays to break the chemical bonds of organic pollutants attached to the patterned film and the recessed portions of the substrate with the patterned film, and chemically bonding the active oxygen separated from the ozone generated by the ultraviolet irradiation with the organic pollutants to decompose them into volatile substances such as carbon dioxide and water. As an ultraviolet irradiation device, a low-pressure mercury lamp is generally used.
[0030] Oxygen plasma cleaning is a method of applying high pressure to a gas containing oxygen molecules to dissociate the oxygen molecules to generate active oxygen, thereby decomposing organic pollutants attached to the surface of the patterned film substrate into volatile substances such as carbon dioxide and water and removing them.
[0031] Hereinafter, Inventions 1 to 22 are disclosed.
[0032] [Invention 1]
[0033] A method for manufacturing a patterned film substrate, comprising:
[0034] A cleaning process of performing UV ozone cleaning or oxygen plasma cleaning on a patterned film substrate to obtain a first patterned film substrate, wherein the patterned film substrate has a patterned film formed on the substrate; and
[0035] a heating step of heating the first patterned film substrate to obtain a second patterned film substrate,
[0036] Through the cleaning step, the contact angle of the pattern film of the first pattern film-bearing substrate is reduced.
[0037] The contact angle of the pattern film of the second patterned film-attached substrate is restored by the heating step.
[0038] [Invention 2]
[0039] The manufacturing method according to Invention 1, wherein:
[0040] The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to anisole from the contact angle of the pattern film of the second pattern film substrate to anisole is recorded as D A1 When D A1 More than 10°.
[0041] [Invention 3]
[0042] The manufacturing method according to Invention 2, wherein:
[0043] The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to anisole from the contact angle of the pattern film to anisole before the cleaning step is recorded as D A0 When D A1 / D A0 It is above 0.30.
[0044] [Invention 4]
[0045] The production method according to any one of Inventions 1 to 3, wherein
[0046] The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to water from the contact angle of the pattern film of the second pattern film substrate to water is recorded as D. W1 When D W1 is 10° or more,
[0047] The value obtained by subtracting the contact angle of the pattern film on the first patterned film substrate to water from the contact angle of the pattern film on water before the cleaning step is recorded as D. W0 When D W1 / D W0 It is above 0.50.
[0048] [Invention 5]
[0049] The production method according to any one of Inventions 1 to 4, wherein
[0050] The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to propylene glycol monomethyl ether acetate from the contact angle of the pattern film of the second pattern film substrate to propylene glycol monomethyl ether acetate is recorded as D P1When D P1 More than 10°.
[0051] [Invention 6]
[0052] The manufacturing method according to Invention 5, wherein:
[0053] The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to propylene glycol monomethyl ether acetate from the contact angle of the pattern film to propylene glycol monomethyl ether acetate before the cleaning step is recorded as D P0 When D P1 / D P0 It is above 0.30.
[0054] [Invention 7]
[0055] The production method according to any one of Inventions 1 to 6, wherein
[0056] The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to xylene from the contact angle of the pattern film of the second pattern film substrate to xylene is recorded as D X1 When D X1 More than 15°.
[0057] [Invention 8]
[0058] The manufacturing method according to Invention 7, wherein:
[0059] The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to xylene from the contact angle of the pattern film to xylene before the cleaning step is recorded as D X0 When D X1 / D X0 It is above 0.80.
[0060] [Invention 9]
[0061] The production method according to any one of Inventions 1 to 8, wherein
[0062] The contact angle of the pattern film of the first pattern film substrate to water is greater than 50°, and the contact angle to anisole is greater than 30°;
[0063] The pattern film of the second patterned film substrate has a contact angle of 93° or more to water and a contact angle of 50° or more to anisole.
[0064] [Invention 10]
[0065] The production method according to any one of Inventions 1 to 9, wherein
[0066] The contact angle of the pattern film of the first pattern film substrate to propylene glycol monomethyl ether acetate is greater than 19°, and the contact angle to xylene is greater than 20°;
[0067] The pattern film of the second patterned film substrate has a contact angle of 40° or more with respect to propylene glycol monomethyl ether acetate, and a contact angle of 45° or more with respect to p-xylene.
[0068] [Invention 11]
[0069] The production method according to any one of Inventions 1 to 10, wherein
[0070] The pattern film includes a fluorine-containing copolymer having a repeating unit represented by formula (A).
[0071] [Chemical formula 1]
[0072]
[0073] In the formula, R 1 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X is a single bond or a divalent group. O is an oxygen atom.
[0074] [Invention 12]
[0075] The production method according to Invention 11, wherein the fluorinated copolymer is any one of the following fluorinated copolymers (1) to (3).
[0076] Fluorinated copolymer (1): contains both a repeating unit represented by the following formula (A) and a repeating unit represented by the following formula (B).
[0077] [Chemical formula 2]
[0078]
[0079] In the formula, R 1 , R 2 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X and Y are each independently a single bond or a divalent group. O is an oxygen atom, and H is a hydrogen atom.
[0080] Fluorinated copolymer (2): contains both a repeating unit represented by the following formula (A) and a repeating unit represented by the following formula (C).
[0081] [Chemical formula 3]
[0082]
[0083] In the formula, R 1 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted by fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X is a single bond or a divalent group. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups may be substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O is an oxygen atom.
[0084] Fluorinated copolymer (3): contains a repeating unit represented by the following formula (A), a repeating unit represented by the following formula (B), and a repeating unit represented by the following formula (C).
[0085] [Chemical formula 4]
[0086]
[0087] In the formula, R 1 , R 2 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted by fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X and Y are each independently a single bond or a divalent group. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups may be substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O is an oxygen atom and H is a hydrogen atom.
[0088] [Invention 13]
[0089] The production method according to any one of Inventions 1 to 12, wherein
[0090] In the heating step, the first patterned film substrate is heated at a temperature of 50° C. to 350° C. for 10 seconds or more.
[0091] [Invention 14]
[0092] The production method according to any one of Inventions 1 to 13, wherein
[0093] The second patterned film substrate is a substrate for forming a display element by an inkjet method.
[0094] [Invention 15]
[0095] The production method according to any one of Inventions 11 to 14, wherein
[0096] In the repeating unit represented by the formula (A), Q is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group.
[0097] [Invention 16]
[0098] The manufacturing method according to Invention 15, wherein
[0099] In the repeating unit represented by the formula (A), Q is a perfluorohexylethyl group, and X is a carbonyl group.
[0100] [Invention 17]
[0101] The manufacturing method according to Invention 15, wherein
[0102] In the repeating unit represented by the formula (A), Q is a hexafluoroisopropyl group, and X is a carbonyl group.
[0103] [Invention 18]
[0104] The production method according to any one of Inventions 11 to 14, wherein
[0105] The repeating unit represented by the formula (A) is a repeating unit represented by the formula (4).
[0106] [Chemical formula 5]
[0107]
[0108] In formula (4), R 4 , R 5 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 3 carbon atoms, wherein a part or all of the hydrogen atoms bonded to carbon atoms in the alkyl group may be substituted with fluorine atoms. O represents an oxygen atom, H represents a hydrogen atom, and F represents a fluorine atom.
[0109] [Invention 19]
[0110] The production method according to any one of Inventions 12 to 14, wherein
[0111] In the repeating unit represented by the formula (A), Q is a hexafluoroisopropyl group and X is a carbonyl group. In the repeating unit represented by the formula (B), Y is a p-phenylene group or a carboxyethylene group.
[0112] [Invention 20]
[0113] The production method according to any one of Inventions 12 to 14, wherein
[0114] The repeating unit represented by the formula (A) has Q that is hexafluoroisopropyl and X that is carbonyl, the repeating unit represented by the formula (B) has Y that is p-phenylene or carboxyethylene, and the repeating unit represented by the formula (C) has Z that is alkoxy, carboxyl, acetoxy or bistrifluoromethylvinyl.
[0115] [Invention 21]
[0116] The production method according to any one of Inventions 12 to 14, wherein
[0117] In the repeating unit represented by the formula (C), Z is a bistrifluoromethylvinyl group.
[0118] [Invention 22]
[0119] The production method according to any one of Inventions 12 to 14, wherein
[0120] In the repeating unit represented by the formula (A), Q is a fluoroalkyl group having 3 to 10 carbon atoms, X is a carbonyl group, in the repeating unit represented by the formula (B), Y is a p-phenylene group, a p-phenylenecarbonyl group or a p-phenylenehexafluoroisopropylidene group, and in the repeating unit represented by the formula (C), Z is a bistrifluoromethylvinyl group.
[0121] (III) Beneficial effects
[0122] As long as the manufacturing method of the patterned film substrate of the present application is used, the lyophilicity of the substrate surface serving as the concave portion of the pattern film can be maintained at all times, while the pattern film can be made sufficiently lyophobic. Even after the surface of the pattern film is subjected to UV ozone cleaning or oxygen plasma cleaning, the lyophobicity of the pattern film can be restored by heating the pattern film. DETAILED DESCRIPTION
[0123] The present invention is not limited to the following embodiments. It should be understood that appropriate changes and improvements to the following embodiments based on the general knowledge of those skilled in the art without departing from the scope of the present application fall within the scope of the present invention.
[0124] 1.Heat treatment after UV ozone cleaning or oxygen plasma cleaning
[0125] The method for manufacturing a patterned film substrate in the present application comprises: a cleaning step of performing UV ozone cleaning or oxygen plasma cleaning on the patterned film substrate to obtain a first patterned film substrate; and a heating step of heating the first patterned film substrate to obtain a second patterned film substrate.
[0126] The heating temperature in the heating step is preferably 50° C. to 350° C., more preferably 100° C. to 300° C., and even more preferably 150° C. to 250° C. If the heating temperature is lower than 50° C., it is difficult to obtain the following effect: the liquid repellency of the patterned film substrate that has decreased after UV ozone cleaning or oxygen plasma cleaning is restored to the same level as before UV ozone cleaning or oxygen plasma cleaning.
[0127] The upper limit of the heating time is not particularly limited, but it is preferably adjusted according to the heat resistance of the photoresist used in the pattern formation of the patterned film substrate. Although the upper limit is not particularly limited, it is substantially less than 1 hour. About the lower limit, it is preferably more than 10 seconds, more preferably more than 30 seconds. If the heating time is less than 10 seconds, it is difficult to obtain the following effect: the lyophobicity of the patterned film substrate that has decreased after UV ozone cleaning or oxygen plasma cleaning is restored to the same degree as before UV ozone cleaning or oxygen plasma cleaning.
[0128] As the heating method, a commonly used heating device can be used, for example, a hot plate or an oven.
[0129] The heating environment may be in nitrogen or under reduced pressure, but is preferably in atmospheric air (at normal pressure (101.325 kPa) because a commercially available heating device can be used.
[0130] According to the method for manufacturing a substrate with a pattern film of the present application, the contact angle of the pattern film of the first substrate with a pattern film decreases through the cleaning step, but the contact angle of the pattern film of the second substrate with a pattern film is restored through the heating step.
[0131] The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to anisole from the contact angle of the pattern film of the second pattern film substrate to anisole is recorded as D A1 When D A1 On the other hand, it is preferred that D A1 It is 70° or less, more preferably 65° or less, and particularly preferably 50° or less.
[0132] In addition, the contact angle of the pattern film of the first pattern film substrate to anisole is denoted as θ A1 The contact angle of the pattern film of the second pattern film substrate to anisole is denoted as θ A2 When θ A2 -θ A1 The value of A1 .
[0133] The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to anisole from the contact angle of the pattern film to anisole before the cleaning step is recorded as D A0When D A1 / D A0 On the other hand, D A1 / D A0 It is 1.20 or less, more preferably 1.15 or less, particularly preferably 1.10 or less.
[0134] In addition, the contact angle of the pattern film to anisole before the cleaning step is denoted as θ A0 When θ A0 -θ A1 The value of A0 .
[0135] Preferably, the contact angle θ of the pattern film of the first pattern film substrate to anisole is A1 On the other hand, the contact angle θ of the pattern film of the first pattern film substrate to anisole is preferably A1 It is 65° or less, and more preferably 63° or less.
[0136] It is preferred that the contact angle θ of the pattern film of the second pattern film substrate to anisole is A2 On the other hand, it is preferred that the contact angle θ of the pattern film of the second pattern film substrate to anisole is A2 It is 85° or less, and more preferably 83° or less.
[0137] The contact angle θ of the pattern film to anisole before the cleaning step is preferably A0 On the other hand, the contact angle θ of the pattern film to anisole before the cleaning step is preferably A0 It is 85° or less, and more preferably 83° or less.
[0138] The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to water from the contact angle of the pattern film of the second pattern film substrate to water is recorded as D. W1 When D W1 On the other hand, it is preferred that D W1 It is 90° or less, and more preferably 65° or less.
[0139] In addition, the contact angle of the pattern film of the first pattern film substrate to water is denoted as θ W1 The contact angle of the pattern film of the second pattern film substrate to water is denoted as θ W2 When θ W2 -θ W1 The value of W1 .
[0140] The value obtained by subtracting the contact angle of the pattern film on the first patterned film substrate from the contact angle of the pattern film on water before the cleaning step is recorded as D. W0 When DW1 / D W0 On the other hand, D W1 / D W0 It is 1.20 or less, more preferably 1.15 or less, particularly preferably 1.10 or less.
[0141] In addition, the contact angle of the pattern film to water before the cleaning step is denoted as θ W0 When θ W0 -θ W1 The value of W0 .
[0142] It is preferred that the contact angle θ of the pattern film of the first pattern film substrate to water is W1 On the other hand, it is preferred that the contact angle θ of the pattern film of the first pattern film substrate to water is W1 It is 100° or less, and more preferably 98° or less.
[0143] It is preferred that the contact angle θ of the pattern film of the second pattern film substrate to water is W2 On the other hand, it is preferred that the contact angle θ of the pattern film of the second pattern film substrate to water is W2 It is 120° or less, and more preferably 115° or less.
[0144] The contact angle θ of the pattern film to water before the cleaning step is preferably W0 On the other hand, it is preferred that the contact angle θ of the pattern film to water before the cleaning step is W0 It is 120° or less, and more preferably 115° or less.
[0145] It is particularly preferred that the contact angle θ of the pattern film of the first pattern film substrate to water is W1 The contact angle θ of anisole is 50° or more. A1 The contact angle θ of the pattern film of the second pattern film substrate to water is 30° or more. W2 The contact angle θ of anisole is 93° or more. A2 Above 50°.
[0146] The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to propylene glycol monomethyl ether acetate (PGMEA) from the contact angle of the pattern film of the second pattern film substrate to propylene glycol monomethyl ether acetate (PGMEA) is recorded as D P1 When D P1 On the other hand, it is preferred that D P1 It is 55° or less, and more preferably 40° or less.
[0147] In addition, the contact angle of the pattern film of the first pattern film-attached substrate to PGMEA is denoted as θP1 The contact angle of the pattern film of the second pattern film substrate to PGMEA is denoted as θ P2 When θ P2 -θ P1 The value of P1 .
[0148] The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to propylene glycol monomethyl ether acetate from the contact angle of the pattern film to propylene glycol monomethyl ether acetate before the cleaning step is recorded as D P0 When D P1 / D P0 On the other hand, D P1 / D P0 It is 1.20 or less, more preferably 1.18 or less, particularly preferably 1.15 or less.
[0149] In addition, the contact angle of the pattern film to PGMEA before the cleaning step is denoted as θ P0 When θ P0 -θ P1 The value of P0 .
[0150] It is preferred that the contact angle θ of the pattern film of the first pattern film substrate to PGMEA is P1 On the other hand, the contact angle θ of the pattern film of the first pattern film substrate to PGMEA is preferably P1 It is 45° or less, and more preferably 40° or less.
[0151] The contact angle θ of the pattern film of the second pattern film substrate to PGMEA is preferably P2 On the other hand, it is preferred that the contact angle θ of the pattern film of the second pattern film-attached substrate to PGMEA is P2 It is 70° or less, and more preferably 68° or less.
[0152] The contact angle θ of the pattern film to PGMEA before the cleaning step is preferably P0 On the other hand, the contact angle θ of the pattern film to PGMEA before the cleaning step is preferably P0 It is 70° or less, and more preferably 68° or less.
[0153] The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate with xylene from the contact angle of the pattern film of the second pattern film substrate with xylene is recorded as D X1 When D X1 On the other hand, it is preferred that D X1 It is 60° or less, and more preferably 50° or less.
[0154] In addition, the contact angle of the pattern film of the first pattern film substrate to xylene is denoted as θ X1 The contact angle of the pattern film of the second pattern film substrate to xylene is θ X2 When θ X2 -θ X1 The value of X1 .
[0155] The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to xylene from the contact angle of the pattern film to xylene before the cleaning step is recorded as D X0 When D X1 / D X0 On the other hand, D X1 / D X0 It is 1.20 or less, more preferably 1.18 or less, particularly preferably 1.15 or less.
[0156] In addition, the contact angle of the pattern film to xylene before the cleaning step is denoted as θ X0 When θ X0 -θ X1 The value of X0 .
[0157] It is preferred that the contact angle θ of the pattern film of the first pattern film substrate to xylene is X1 On the other hand, the contact angle θ of the pattern film of the first pattern film substrate to xylene is preferably X1 It is 50° or less, and more preferably 45° or less.
[0158] The contact angle θ of the pattern film of the second pattern film substrate to xylene is preferably X2 On the other hand, it is preferred that the contact angle θ of the pattern film of the second pattern film substrate to xylene is X2 It is 75° or less, and more preferably 73° or less.
[0159] The contact angle θ of the pattern film to xylene before the cleaning step is preferably X0 On the other hand, the contact angle θ of the pattern film to xylene before the cleaning step is preferably X0 It is 75° or less, and more preferably 73° or less.
[0160] It is particularly preferred that the contact angle θ of the pattern film of the first pattern film substrate to PGMEA is P1 The contact angle θ of xylene is 19° or more. X1 The contact angle θ of the pattern film of the second pattern film substrate to PGMEA is 20° or more. P2 The contact angle θ of xylene is 40° or more. X2 More than 45°.
[0161] According to the manufacturing method of the patterned film substrate in the present application, after UV ozone cleaning or oxygen plasma cleaning, the patterned film substrate with a patterned film formed on the substrate is heated, thereby preventing problems such as ink crossing over the dam or the dam dissolving in the ink when ink droplets are dripped into the concave portion of the patterned film of the patterned film substrate by an inkjet method.
[0162] 2. Fluorinated copolymers
[0163] In the method for producing a patterned film substrate of the present application, the patterned film substrate is obtained by forming a patterned film having a pattern on a substrate. Preferably, the patterned film comprises a fluorinated copolymer having a repeating unit represented by formula (A).
[0164] [Chemical formula 6]
[0165]
[0166] In the formula, R 1 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X is a single bond or a divalent group. O is an oxygen atom.
[0167] In the method for producing a patterned film substrate of the present invention, since the resist used for pattern formation is lyophobic to ink, the fluorinated copolymer having a repeating unit represented by formula (A) is preferably any one of the following fluorinated copolymers (1) to (3).
[0168] [Fluorinated copolymer (1)]
[0169] The fluorinated copolymer (1) contains both a repeating unit represented by the following formula (A) (hereinafter, sometimes referred to as repeating unit (A)) and a repeating unit represented by the following formula (B) (hereinafter, sometimes referred to as repeating unit (B)).
[0170] [Chemical formula 7]
[0171]
[0172] In the formula, R 1 , R 2 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X and Y are each independently a single bond or a divalent group. O is an oxygen atom, and H is a hydrogen atom.
[0173] In the fluorinated copolymer (1), it is preferred that Q in the repeating unit represented by the formula (A) is a hexafluoroisopropyl group (-CH(CF3)2), X is a carbonyl group (-C(=O)-), and Y in the repeating unit represented by the formula (B) is a carboxyethylene group (-C(=O)-O-CH2CH2-).
[0174] The following combinations of repeating units (A) and repeating units (B) are preferred.
[0175] [Chemical formula 8]
[0176]
[0177] <Content ratio of repeating units>
[0178] The content of the repeating unit (A) based on the total amount of the repeating units (A) and (B) contained in the fluorinated copolymer (1) is preferably from 5% to 90%, more preferably from 10% to 80%, by mol%.
[0179] In order to improve the solubility in organic solvents, the adhesion to the substrate during film formation or the hardness, the fluorinated copolymer (1) may contain repeating units other than repeating units (A) and (B) as required. In terms of mol%, the content of repeating units other than repeating units (A) and (B) is preferably 50% or less, more preferably 30% or less relative to the total amount of repeating units (A) and (B). If it is greater than 50%, it is difficult to obtain the effect of obtaining liquid repellency.
[0180] [Fluorinated copolymer (2)]
[0181] The fluorinated copolymer (2) contains both a repeating unit represented by the following formula (A) and a repeating unit represented by the following formula (C) (hereinafter, sometimes referred to as a repeating unit (C)).
[0182] [Chemical formula 9]
[0183]
[0184] In the formula, R 1 , R 3Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted by fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X is a single bond or a divalent group. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups may be substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O is an oxygen atom.
[0185] In the fluorinated copolymer (2), it is preferred that Q in the repeating unit represented by the formula (A) is a fluoroalkyl group having 3 to 10 carbon atoms, X is a carbonyl group (-C(=O)-), and Z in the repeating unit represented by the formula (C) is a bistrifluoromethylvinyl group (-CH=C(CF3)2).
[0186] The following combinations of repeating units (A) and repeating units (C) are preferred.
[0187] [Chemical formula 10]
[0188]
[0189] [Chemical formula 11]
[0190]
[0191] <Content ratio of repeating units>
[0192] The content of the repeating unit (A) based on the total amount of the repeating units (A) and (C) contained in the fluorinated copolymer (2) is preferably from 5% to 80%, more preferably from 10% to 60%, by mol%.
[0193] The content of the repeating unit (C) based on the total amount of the repeating units (A) and (C) contained in the fluorinated copolymer is preferably 3% to 90%, more preferably 5% to 80%, by mol%.
[0194] In order to improve the solubility in organic solvents, the adhesion to the substrate during film formation or the hardness, the fluorinated copolymer (2) may contain repeating units other than the repeating units (A) and (C) as required. In terms of mol%, the content of repeating units other than the repeating units (A) and (C) is preferably 50% or less, more preferably 30% or less relative to the total amount of the repeating units (A) and (C). If it is greater than 50%, it tends to be difficult to obtain liquid repellency.
[0195] [Fluorinated copolymer (3)]
[0196] The fluorinated copolymer (3) contains a repeating unit represented by the following formula (A), a repeating unit represented by the following formula (B) and a repeating unit represented by the following formula (C) at the same time.
[0197] [Chemical formula 12]
[0198]
[0199] In the formula, R 1 , R 2 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted by fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X and Y are each independently a single bond or a divalent group. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups may be substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O is an oxygen atom and H is a hydrogen atom.
[0200] In the fluorinated copolymer (3), it is preferred that Q in the repeating unit represented by the formula (A) is a hexafluoroisopropyl group (—CH(CF3)2), X is a carbonyl group (—C(═O)—), Y in the repeating unit represented by the formula (B) is a carboxyethylene group (—C(═O)—O—CH2CH2—), and R in the repeating unit represented by the formula (C) is 3 is a hydrogen atom or a methyl group, and Z is an alkylcarbonyloxy group having 1 to 4 carbon atoms.
[0201] The following combinations of repeating unit (A), repeating unit (B) and repeating unit (C) are preferred.
[0202] [Chemical formula 13]
[0203]
[0204] In the fluorinated copolymer (3), Q in the repeating unit represented by the formula (A) is a fluoroalkyl group having 3 to 10 carbon atoms, X is a carbonyl group (-C(=O)-), Y in the repeating unit represented by the formula (B) is a p-phenylene group (-C6H4-), a p-phenylenecarbonyl group (-C6H4-C(=O)-) or a p-phenylenehexafluoroisopropylidene group (-C6H4-C(CF3)2-), and R in the repeating unit represented by the formula (C) is 3 is a hydrogen atom or a methyl group, and Z is a bistrifluoromethylvinyl group (-CH=C(CF3)2).
[0205] The following combinations of repeating unit (A), repeating unit (B) and repeating unit (C) are preferred.
[0206] [Chemical formula 14]
[0207]
[0208] [Chemical formula 15]
[0209]
[0210] [Chemical formula 16]
[0211]
[0212] [Chemical formula 17]
[0213]
[0214] <Content ratio of repeating units>
[0215] The content of the repeating unit (A) based on the total amount of the repeating units (A), (B) and (C) contained in the fluorinated copolymer (3) is preferably from 5% to 80%, more preferably from 10% to 60%, by mol%.
[0216] The content of the repeating unit (B) based on the total amount of the repeating units (A), (B) and (C) contained in the fluorinated copolymer (3) is preferably from 10% to 85%, more preferably from 20% to 70%, by mol%.
[0217] The content of the repeating unit (C) based on the total amount of the repeating units (A), (B) and (C) contained in the fluorinated copolymer is preferably 3% to 90%, more preferably 5% to 80%, by mol%.
[0218] In order to improve solubility in organic solvents, adhesion to substrates during film formation, or hardness, the fluorinated copolymer (3) may contain repeating units other than repeating units (A), (B) and (C) as required. The content of repeating units other than repeating units (A), (B) and (C) is preferably 50% or less, more preferably 30% or less, relative to the total amount of repeating units (A), (B) and (C). If it is greater than 50%, it tends to be difficult to obtain liquid repellency.
[0219] [Molecular weight of fluorinated copolymer]
[0220] In the method for manufacturing a substrate with a patterned film of the present application, the number average molecular weight Mn of the fluorinated copolymers (1) to (3) contained in the patterned film is preferably 1,000 or more and 100,000 or less, more preferably 3,000 or more and 60,000 or less. In addition, the molecular weight distribution Mw / Mn defined by the ratio of the number average molecular weight Mn to the weight average molecular weight Mw is preferably 1 or more and 4 or less, more preferably 1 or more and 2.5 or less.
[0221] If the number average molecular weight Mn is 1,000 or more, the hardness of the pattern film containing the fluorinated copolymer is appropriate, and it is also easy to form a film of the desired thickness, so it is preferred. In addition, it is also preferred from the perspective of easy formation of a fine pattern consisting of a lyophobic portion and a lyophilic portion, and pattern durability. If the number average molecular weight Mn is 100,000 or less, when preparing a pattern-forming composition containing a fluorinated copolymer on a substrate, the fluorinated copolymer is easy to dissolve in a solvent, easy to apply, and is not easy to crack after film formation, so it is preferred.
[0222] The number average molecular weight Mn and weight average molecular weight Mw of the polymer are measured by using a high-speed gel permeation chromatograph (hereinafter sometimes referred to as GPC; manufactured by TOSOH CORPORATION, model HLC-8320GPC), connecting an ALPHA-M column and an ALPHA-2500 column (both manufactured by TOSOH CORPORATION) in series, and using tetrahydrofuran (THF) as a developing solvent. A detector for measuring a refractive index difference can be used as a detector.
[0223] 3. Repeating Unit
[0224] Hereinafter, the repeating unit (A) contained in the fluorinated copolymers such as the fluorinated copolymers (1) to (3), the repeating unit (B) contained in the fluorinated copolymer (1) or (3), and the repeating unit (C) contained in the fluorinated copolymer (2) or (3) will be described.
[0225] [Repeating unit (A)]
[0226] [Chemical formula 18]
[0227]
[0228] In the formula, R 1 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X is a single bond or a divalent group. O is an oxygen atom.
[0229] R 1Examples include a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a fluorine atom, a trifluoromethyl group, a trifluoroethyl group, a trifluoropropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group (-C(CF3)2H) or a heptafluoroisopropyl group. A hydrogen atom, a fluorine atom or a methyl group is particularly preferred.
[0230] Q is preferably a fluoroalkyl group having 3 to 10 carbon atoms, and examples thereof include trifluoromethyl, trifluoroethyl, trifluoropropyl, 1,1,1,3,3,3-hexafluoroisopropyl (-C(CF3)2H), heptafluoroisopropyl, pentafluoropropyl, perfluorohexylethyl, perfluorooctylethyl, perfluorodecylethyl, 1,2,2,3,3,4,4,5-octafluorocyclopentylmethyl, perfluorocyclopentyl, perfluorocyclohexyl or perfluoroadamantyl. Perfluorohexylethyl or hexafluoroisopropyl is particularly preferred.
[0231] X is a single bond or a divalent group, and the hydrogen atoms contained in the divalent group are optionally substituted by fluorine atoms. The divalent group is preferably a divalent group having 2 to 10 carbon atoms, and examples thereof include a methylene group, an alkylene group having 2 to 10 carbon atoms, an alkenylene group having 2 to 10 carbon atoms, a divalent aryl group having 6 to 10 carbon atoms, or a divalent alicyclic hydrocarbon group having 4 to 10 carbon atoms. An ether bond (-O-), a carbonyl group (-C(=O)-), a carboxyl group (-C(=O)-O-) or an oxycarbonyl group (-OC(=O)-) may be contained inside the alkylene group or the alkenylene group. If the aliphatic chain in the divalent group is long, the liquid repellency decreases, so more preferred examples include a single bond, a carbonyl group (-C(=O)-), an oxyethylene group (-O-CH2-CH2-), a carboxyethylene group (-C(=O)-O-CH2-CH2-), a carboxyphenylene group (-C(=O)-O-C6H4-), a phenylene group (-C6H4-) or a phenylene hexafluoroisopropylidene group (-C6H4-C(CF3)2-). A carbonyl group is particularly preferred.
[0232] Furthermore, as the repeating unit (A), a structure represented by formula (4) is also preferably mentioned.
[0233] [Chemical formula 19]
[0234]
[0235] In formula (4), R 4 , R 5 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 3 carbon atoms, wherein a part or all of the hydrogen atoms bonded to carbon atoms in the alkyl group may be substituted with fluorine atoms. O represents an oxygen atom, H represents a hydrogen atom, and F represents a fluorine atom.
[0236] [Repeating unit (B)]
[0237] [Chemical formula 20]
[0238]
[0239] In the formula, R 2 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Y is a single bond or a divalent group. O is an oxygen atom, and H is a hydrogen atom.
[0240] R 2 Preferred examples include a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a fluorine atom, a trifluoromethyl group, a trifluoroethyl group, a trifluoropropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group (-C(CF3)2H) or a heptafluoroisopropyl group. A hydrogen atom, a fluorine atom or a methyl group is particularly preferred.
[0241] Y is a single bond or a divalent group, and the divalent group is preferably a divalent group having 2 to 10 carbon atoms, and examples thereof include a methylene group, an alkylene group having 2 to 10 carbon atoms, an alkenylene group having 2 to 10 carbon atoms, an arylene group having 6 to 10 carbon atoms, or a divalent alicyclic hydrocarbon group having 4 to 10 carbon atoms. The alkylene group or the alkenylene group may contain an ether bond (—O—), a carbonyl group (—C(═O)—), a carboxyl group (—C(═O)—O—), or an oxycarbonyl group (—OC(═O)—). If the aliphatic chain in the divalent group is long, the liquid repellency decreases, so preferred examples include a single bond, a carbonyl group (-C(=O)-), an oxyethylene group (-O-CH2-CH2-), a carboxyethylene group (-C(=O)-O-CH2-CH2-), a carboxyphenylene group (-C(=O)-O-C6H4-), a phenylene group (-C6H4-), or a phenylene hexafluoroisopropylidene group (-C6H4-C(CF3)2-). Particularly preferred are p-phenylene and carboxyethylene groups.
[0242] [Repeating unit (C)]
[0243] [Chemical formula 21]
[0244]
[0245] In the formula, R 3 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms in these groups may be substituted with fluorine atoms, oxygen atoms or nitrogen atoms.
[0246] R 3Preferred examples include a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a fluorine atom, a trifluoromethyl group, a trifluoroethyl group, a trifluoropropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group (-C(CF3)2H) or a heptafluoroisopropyl group. A hydrogen atom, a fluorine atom or a methyl group is particularly preferred.
[0247] Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms, or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms, or nitrogen atoms. Since the effect of recovering the lyophobicity by heating is high, it is particularly preferred that Z is bistrifluoromethylvinyl (-CH=C(CF3)2).
[0248] 4. Synthesis of fluorinated copolymers (1) to (3)
[0249] 4-1. Monomer
[0250] The following lists the monomer (A1) that provides the repeating unit (A), the monomer (B1) that provides the repeating unit (B), and the monomer (C1) that provides the repeating unit (C).
[0251] The fluorinated copolymer (1) can be obtained by copolymerizing the monomer (A1) and the monomer (B1). The fluorinated copolymer (2) can be obtained by copolymerizing the monomer (A1) and the monomer (C1). The fluorinated copolymer (3) can be obtained by copolymerizing the monomer (A1) and the monomer (B1) and the monomer (C1).
[0252] [Monomer (A1)]
[0253] [Chemical formula 22]
[0254]
[0255] R 1 , X, Q and R shown in formula (A) 1 , X, and Q are the same.
[0256] [Monomer (B1)]
[0257] [Chemical formula 23]
[0258]
[0259] R 2 , Y and R shown in formula (B) 2 , Y are the same.
[0260] Examples of the monomer (B1) include the following monomers. 2 A hydrogen atom, a fluorine atom or a methyl group is particularly preferred.
[0261] [Chemical formula 24]
[0262]
[0263] [Monomer (C1)]
[0264] [Chemical formula 25]
[0265]
[0266] R 3 , Z and R shown in formula (C) 3 , Z are the same.
[0267] 4-2. Synthesis method of fluorinated copolymers (1) to (3)
[0268] In the synthesis method of the fluorinated copolymers (1) to (3), the above-mentioned monomers (A1), (B1), and (C1) are used as raw materials. The synthesis method can be selected from common polymerization methods. Free radical polymerization and ionic polymerization are preferred, and coordinated anionic polymerization, living anionic polymerization, and cationic polymerization can be selected according to the situation. In addition, a polymerization solvent can be used in the polymerization. The following is an explanation of free radical polymerization.
[0269] The radical polymerization can be carried out in the presence of a radical polymerization initiator or a radical polymerization initiation source by a known polymerization method such as bulk polymerization, solution polymerization, suspension polymerization or emulsion polymerization, in a batchwise, semi-continuous or continuous manner.
[0270] <Radical polymerization initiator>
[0271] As the free radical polymerization initiator, for example, azo compounds, peroxide compounds or redox compounds can be listed. As the azo compound, azobisisobutyronitrile can be exemplified. As the peroxide compound, tert-butyl peroxypivalate, di-tert-butyl peroxide, isobutyryl peroxide, didodecanol peroxide, peroxidated succinic acid, dicinnamyl peroxide, di-n-propyl peroxydicarbonate, allyl tert-butyl peroxycarbonate, benzoyl peroxide, hydrogen peroxide or ammonium persulfate can be exemplified. As the redox compound, a compound composed of an oxidant and a reductant can be used, such as a compound (Fenton's reagent) composed of a combination of a divalent iron ion and a hydrogen peroxide solution.
[0272] <Polymerization solvent>
[0273] As the polymerization solvent, a solvent that does not inhibit free radical polymerization is preferred, and examples thereof include ester solvents, ketone solvents, hydrocarbon solvents, and alcohol solvents. In addition, water, ethers, cyclic ethers, freons, or aromatic solvents may also be used.
[0274] Examples of the polymerization solvent include ethyl acetate or n-butyl acetate as an ester solvent, acetone or methyl isobutyl ketone as a ketone solvent, toluene or cyclohexane as a hydrocarbon solvent, and methanol, isopropanol or ethylene glycol monomethyl ether as an alcohol solvent.
[0275] These polymerization solvents may be used alone or in combination of two or more. In addition, a molecular weight modifier such as mercaptan may be used simultaneously.
[0276] <Polymerization conditions>
[0277] The polymerization temperature may be appropriately selected according to the type of the free radical polymerization initiator or the free radical polymerization initiation source. Preferably, the type of the free radical polymerization initiator or the free radical polymerization initiation source is appropriately selected so that the polymerization temperature is, for example, 20° C. to 200° C., preferably 30° C. to 140° C. The molecular weight of the fluorinated copolymers (1) to (3) can be controlled by selecting the free radical polymerization initiator or the free radical polymerization initiation source and adjusting the polymerization conditions.
[0278] As a method for removing the polymerization solvent such as an organic solvent or water from the solution or dispersion containing the polymerized fluorinated copolymers (1) to (3), a known method may be used, for example, reprecipitation, filtration or distillation under reduced pressure.
[0279] When the fluorinated copolymers (1) to (3) are used as resist components, the solubility of the fluorinated copolymers (1) to (3) in the developer solution varies depending on the molecular weight of the fluorinated copolymers (1) to (3), and the patterning conditions in lithography may change. If the molecular weight of the fluorinated copolymers (1) to (3) is high, the dissolution rate in the developer solution tends to decrease, and if the molecular weight is low, the dissolution rate tends to increase. The molecular weight of the fluorinated copolymers (1) to (3) can be controlled by adjusting the polymerization conditions.
[0280] 5. Resist pattern forming composition
[0281] A photosensitive agent or an acid generator, a basic compound and a solvent are added to a fluorinated copolymer such as fluorinated copolymers (1) to (3) to obtain a composition for forming a resist pattern. The obtained composition for forming a resist pattern is applied to a substrate and then patterned by photolithography to obtain a patterned film substrate used in the method for producing a patterned film substrate of the present application. Hereinafter, the composition for forming a resist pattern is sometimes referred to as a resist.
[0282] The above-mentioned resist can be prepared by the following method: (a) a fluorinated copolymer such as a fluorinated copolymer (1) to (3) is used as its essential component, and (b) an alkali-soluble resin, (c) a naphthoquinonediazide group-containing compound, (d) a solvent, (e) a photoacid generator, (f) a basic compound or (g) a cross-linking agent is added as needed.
[0283] 5-1. (b) Alkali-soluble resin
[0284] (b) The alkali-soluble resin includes, for example, an alkali-soluble novolac resin. The alkali-soluble novolac resin can be obtained by condensing phenols and aldehydes in the presence of an acid catalyst.
[0285] <Phenols>
[0286] Examples of phenols include phenol, o-cresol, m-cresol, p-cresol, 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, resorcinol, 2-methylresorcinol, 4-ethylresorcinol, hydroquinone, methylhydroquinone, catechol, 4-methylcatechol, pyrogallol, phloroglucinol, thymol, and isothymol. These phenols may be used alone or in combination of two or more.
[0287] <Aldehydes>
[0288] Examples of the aldehydes include formaldehyde, trioxymethylene, paraformaldehyde, benzaldehyde, acetaldehyde, propionaldehyde, phenylacetaldehyde, α-phenylpropionaldehyde, β-phenylpropionaldehyde, o-hydroxybenzaldehyde, m-hydroxybenzaldehyde, p-hydroxybenzaldehyde, o-tolualdehyde, m-tolualdehyde, p-tolualdehyde, nitrobenzaldehyde, furfural, glyoxal, glutaraldehyde, terephthalaldehyde, or isophthalaldehyde.
[0289] <Acid Catalyst>
[0290] Examples of the acid catalyst include hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, phosphorous acid, formic acid, oxalic acid, acetic acid, methanesulfonic acid, diethyl sulfate, and p-toluenesulfonic acid. These acid catalysts may be used alone or in combination of two or more.
[0291] The mass average molecular weight of the (b) alkali-soluble resin component is preferably 1,000 to 50,000 from the viewpoint of developability and resolution of the positive resist composition.
[0292] 5-2. (c) Naphthoquinone diazide compounds
[0293] (c) The naphthoquinonediazide group-containing compound is not particularly limited, and compounds that can be used as a photosensitive component of an i-line resist composition can be used, for example, naphthoquinone-1,2-diazide sulfonate compounds, o-benzoquinonediazide sulfonate, o-anthraquinonediazide sulfonate, and esters of naphthoquinone-1,2-diazide sulfonyl halides and hydroxyl compounds. Examples of the naphthoquinone-1,2-diazide sulfonyl halides include naphthoquinone-1,2-diazide-5-sulfonyl chloride, naphthoquinone-1,2-diazide-4-sulfonyl chloride, and naphthoquinone-1,2-diazide-6-sulfonyl chloride.
[0294] As the naphthoquinonediazide group-containing compound (c), naphthoquinonediazide-4-sulfonate, naphthoquinonediazide-5-sulfonate or naphthoquinonediazide-6-sulfonate is preferred because of its excellent solubility. These compounds may be used alone or in combination of two or more.
[0295] The amount of the naphthoquinonediazide-containing compound (c) added is preferably 10% by mass or more and 60% by mass or less, and more preferably 20% by mass or more and 50% by mass or less, relative to the total mass of the alkali-soluble resin (b) and the naphthoquinonediazide-containing compound (c). If the amount exceeds 60% by mass, the sensitivity as a resist cannot be obtained, and if the amount is less than 10% by mass, it is difficult to obtain a fine pattern due to the reduction of the film in the unexposed portion after photolithography.
[0296] 5-3.(d) Solvent
[0297] The (d) solvent contained in the resist may be any solvent selected from known resist solvents as long as it can dissolve (a) the fluorinated copolymers (1) to (3), (b) the alkali-soluble resin, and (c) the naphthoquinonediazide-containing compound to form a uniform solution. Two or more solvents may be mixed and used.
[0298] Examples of such solvents include ketones, alcohols, polyols, esters, aromatic solvents, ethers, fluorinated solvents, and turpentine-based naphtha solvents or paraffin solvents as high-boiling-point solvents for the purpose of improving coating properties.
[0299] Examples of ketones include acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl isobutyl ketone, methyl isoamyl ketone, and 2-heptanone. Examples of alcohols include isopropanol, butanol, isobutanol, n-pentanol, isopentanol, tert-pentanol, 4-methyl-2-pentanol, 3-methyl-3-pentanol, 2,3-dimethyl-2-pentanol, n-hexanol, n-heptanol, 2-heptanol, n-octanol, n-decanol, sec-pentanol, tert-pentanol, isopentanol, 2-ethyl-1-butanol, lauryl alcohol, hexyldecanol, and oleyl alcohol. As polyols, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, ethylene glycol monoacetate, ethylene glycol dimethyl ether (EDC), diethylene glycol monoacetate, propylene glycol monoacetate, dipropylene glycol monoacetate, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate (PGMEA) or propylene glycol monomethyl ether (PGME) and derivatives of these polyols can be illustrated. As esters, methyl lactate, ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate or ethyl ethoxypropionate or γ-butyrolactone (GBL) can be illustrated. As aromatic solvents, toluene or xylene can be illustrated. As ethers, diethyl ether, dioxane, anisole or diisopropyl ether can be illustrated. As fluorine-based solvents, hexafluoroisopropanol can be illustrated.
[0300] Preferred are ethylene glycol dimethyl ether (EDC), propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone, ethyl lactate (EL) or γ-butyrolactone (GBL).
[0301] The amount of the solvent (d) contained in the resist is preferably 1% by mass or more and 25% by mass or less, and more preferably 5% by mass or more and 15% by mass or less. The thickness of the formed resin film can be adjusted by adjusting the solid content concentration of the resist.
[0302] 5-4. (e) Photoacid generator
[0303] (e) The photoacid generator can be arbitrarily selected from compounds used as acid generators for chemically amplified resists and can be used, and examples thereof include sulfonates and sulfonate esters.
[0304] Examples of the sulfonates include iodonium sulfonate, sulfonium sulfonate, N-imide sulfonate, N-oxime sulfonate, o-nitrobenzyl sulfonate, trimesylate of pyrogallol, triphenylsulfonium trifluoromethane sulfonate, and triphenylsulfonium perfluoro-n-butane sulfonate.
[0305] These photoacid generators generate alkylsulfonic acid, aromatic sulfonic acid, or partially or fully fluorinated aromatic sulfonic acid or alkylsulfonic acid by exposure in photolithography. The photoacid generator that generates fully fluorinated alkylsulfonic acid is preferably triphenylsulfonium trifluoromethanesulfonate or triphenylsulfonium perfluorobutanesulfonate.
[0306] 5-5.(f) Basic compounds
[0307] The (f) basic compound plays a role in slowing down the diffusion rate of the acid generated by the (e) photoacid generator when diffusing in the resist film. The addition of the (f) basic compound can be expected to bring about the following effects: the shape of the resist pattern is improved by adjusting the acid diffusion distance; even if the exposure delay time after the formation of the resist film is long, the stability of forming the resist pattern with the required precision is improved.
[0308] Examples of such basic compounds include aliphatic amines, aromatic amines, heterocyclic amines, and aliphatic polycyclic amines, preferably aliphatic secondary amines, aliphatic tertiary amines, or alkanolamines. Examples of such amines include trimethylamine, triethylamine, tripropylamine, tributylamine, tripentylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, tridodecylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, dipentylamine, dihexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, didocylamine, dicyclohexylamine, methylamine, ethylamine, propylamine, butylamine, amylamine, hexylamine, heptylamine, octylamine, nonylamine, decylamine, dodecylamine, diethanolamine, triethanolamine, diisopropanolamine, triisopropanolamine, dioctanolamine, trioctanolamine, aniline, pyridine, picoline, lutidine, bipyridine, pyrrole, piperidine, piperazine, indole, or hexamethylenetetramine. These basic compounds may be used alone or in combination of two or more.
[0309] The amount of the basic compound (f) in the resist is preferably 0.001 to 2 parts by mass, more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of the fluorinated copolymer (a) such as the fluorinated copolymer (1) to (3). If the amount of the basic compound (f) is less than 0.001 parts by mass, the effect as an additive cannot be fully obtained, while if it is more than 2 parts by mass, there is a concern that the resolution or sensitivity may be reduced.
[0310] 5-6. (g) Cross-linking agent
[0311] (g) A crosslinking agent may be added to the above-mentioned resist as needed. As the (g) crosslinking agent, a known crosslinking agent may be used. As such a crosslinking agent, for example, 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine (hydroxymethyl melamine curing agent) and its derivatives, 1,3,4,6-tetrakis(methoxymethyl) glycoluril (glycoluril curing agent) and its derivatives, polyfunctional epoxides, polyfunctional oxetane compounds or polyfunctional isocyanate compounds may be cited. A variety of these crosslinking agents may be used.
[0312] 6. Pattern formation
[0313] The formation of a pattern in the method for manufacturing a patterned film substrate of the present application is described. The formation of the pattern includes: a film forming step of coating the resist on the substrate to form a film; an exposure step of irradiating an electromagnetic wave or an electron beam with a wavelength of 600 nm or less through a photomask to transfer the pattern of the photomask to the film; and a developing step of developing the film with a developer to obtain a pattern.
[0314] A pattern can be formed by using a resist containing a fluorinated copolymer such as fluorinated copolymers (1) to (3) and performing the following steps: (a) a film forming step of coating a substrate with the resist to form a resist film; (b) an exposure step of heating the resist film and then irradiating the resist film with an electromagnetic wave or electron beam having a wavelength of 600 nm or less through a photomask on which the pattern has been processed; and (c) a development step of developing the exposed resist film with an alkaline developer or an organic solvent to obtain a resist pattern having the pattern of the photomask transferred onto the substrate.
[0315] Hereinafter, each step will be described with reference to examples.
[0316] 6-1. (a) Film Forming Process
[0317] In the film forming step (a), the resist containing the fluorinated copolymers (1) to (3) is applied onto a silicon wafer or the like as a substrate by spin coating, and the silicon wafer is heated on a heating plate, for example, at a temperature of not less than 60° C. and not more than 200° C. for not less than 10 seconds and not more than 10 minutes, preferably at a temperature of not less than 80° C. and not more than 150° C. for not less than 30 seconds and not more than 2 minutes, to form a resist film on the substrate.
[0318] As the substrate, for example, a silicon wafer, a metal substrate or a glass substrate can be used. In addition, an organic or inorganic film can be provided on the substrate. For example, an anti-reflection film or a lower layer of a multilayer resist can be provided, and a pattern can also be formed thereon.
[0319] 6-2. (b) Exposure process
[0320] In the exposure step (b), a photomask is mounted on an exposure device so that the exposure dose is, for example, 1 mJ / cm 2 Above, 200mJ / cm 2 Below, preferably 10 mJ / cm 2 Above, 100mJ / cm 2 In the following manner, after irradiating the anti-etching film with an electromagnetic wave or electron beam with a wavelength of less than 600nm through a photomask, it is heated on a heating plate, for example, at a temperature of more than 60°C and less than 150°C for more than 10 seconds and less than 5 minutes, preferably at a temperature of more than 80°C and less than 130°C for more than 30 seconds and less than 3 minutes, to transfer the pattern of the photomask to the anti-etching film.
[0321] The wavelength of the electromagnetic wave is preferably 100 to 600 nm, more preferably 300 to 500 nm. It is particularly preferred to include light of i-line (365 nm), h-line (405 nm) or g-line (436 nm). In addition, light below 330 nm may be cut off as required.
[0322] Examples of the light source include KrF excimer laser (wavelength: 248 nm), ArF excimer laser (wavelength: 193 nm), and F2 excimer laser (wavelength: 157 nm).
[0323] 6-3. (c) Development process
[0324] In the (c) development process, as a developer, a concentration of tetramethylammonium hydroxide (TMAH) is used, for example, an aqueous solution of 0.1 mass % or more and 5 mass % or less, preferably an aqueous solution of 2 mass % or more and 3 mass % or less, or an organic solvent is used to dissolve any one of the exposed part or unexposed part of the resist film in the (b) exposure process to form a pattern, and obtain a pattern film on the substrate. As an organic solvent, propylene glycol monomethyl ether acetate (PGMEA), butyl acetate, etc. can be exemplified. In the development process, a known method such as an immersion method, a puddling method, and a spray method can be used to make the developer contact the resist film for example for more than 10 seconds and less than 3 minutes, preferably for more than 30 seconds and less than 2 minutes, thereby obtaining a patterned film substrate with a target pattern.
[0325] Example
[0326] The method for producing the patterned film substrate of the present application will be described in detail by the following examples. However, the present invention is not limited to the following examples.
[0327] 1. Synthesis of Monomers
[0328] The fluorinated monomers for obtaining the fluorinated copolymers (1) to (3) are synthesized.
[0329] 1-1. Synthesis of MA-CH2-OFCP
[0330] [Synthesis of 1,2,2,3,3,4,4,5-octafluorocyclopentylmethanol]
[0331] In a nitrogen atmosphere, 31.5 ml (0.75 mol) of methanol, 1.11 g (0.0045 mol) of benzoyl peroxide (BPO), and 31.2 g (0.12 mol) of octafluorocyclopentene (manufactured by Central Glass Co., Ltd.) were added to a 300 ml stainless steel pressure vessel at room temperature (20°C, the same below), the vessel was sealed, heated to 120°C, and stirred for 24 hours to carry out the following reaction. After the vessel was cooled, the contents were distilled under normal pressure to obtain 28.8 g of 1,2,2,3,3,4,4,5-octafluorocyclopentylmethanol, with a yield of 80%.
[0332] [Chemical formula 26]
[0333]
[0334] The results of nuclear magnetic resonance analysis (NMR) are shown below.
[0335] <NMR analysis results>
[0336] 1 H-NMR (CDCl3, TMS internal standard)
[0337] δ(ppm): 4.21-4.05(2H,m),5.22(1H,m)
[0338] [Synthesis of MA-CH2-OFCP]
[0339] 24.3 g (0.1 mol) of 1,2,2,3,3,4,4,5-octafluorocyclopentylmethanol obtained in the above synthesis, 15.1 g (0.15 mol) of triethylamine, and methoxyphenol (1000 ppm) as a polymerization inhibitor were weighed into a 300 ml glass flask with a stirrer, and 16.9 g (0.11 mol) of methacrylic anhydride was added dropwise to the reaction system at 30°C and stirred for 2 hours. After the stirring was completed, 40 ml of diisopropyl ether and 30 ml of pure water were added to separate the liquids. Then, 20 ml of 1 mass % sodium hydroxide aqueous solution was added, and after stirring for 1 hour, the mixture was transferred to a separating funnel to obtain an organic layer. After washing the organic layer twice with 30 ml of pure water, the mixture was subjected to reduced pressure distillation at a pressure of 1.0 kPa and a temperature of 70 to 72°C to obtain 26.5 g of MA-CH2-OFCP shown below, with a yield of 85%.
[0340] [Chemical formula 27]
[0341]
[0342] <NMR analysis results>
[0343] 1 H-NMR (Solvent: deuterated chloroform, internal standard: TMS)
[0344] δ(ppm): 1.92(3H,s),4.21-4.05(2H,m),5.22(1H,m),5.65(1H,q),6.12(1H,q)
[0345] 1-2. Synthesis of 1,1-Bistrifluoromethylbutadiene (BTFBE)
[0346] 400 g of concentrated sulfuric acid in a 1000 ml glass flask with a stirrer was heated to 100°C, and 300 g of 1,1,1-trifluoro-2-trifluoromethyl-4-pentene-2-ol was slowly added dropwise to the concentrated sulfuric acid over 1 hour to perform the following reaction. Sodium bicarbonate was added to the reaction system, and a fraction at 68 to 70°C was recovered by atmospheric distillation to obtain 1,1-bistrifluoromethylbutadiene (BTFBE) with a yield of 58%.
[0347] [Chemical formula 28]
[0348]
[0349] <NMR analysis results>
[0350] 1 H-NMR (solvent: deuterated chloroform, internal standard: TMS); δ (ppm): 5.95 (1H, dd), 6.05 (1H, dd), 6.85 (1H, m), 7.04 (1H, m)
[0351] 19 F-NMR (solvent: deuterated chloroform, internal standard: C6D6); δ (ppm): -58.4 (3F, m), -65.3 (3F, m)
[0352] 2. Polymer Synthesis
[0353] [Determination of the molar ratio of each repeating unit] NMR
[0354] According to the NMR 1 H-NMR and 19 The molar ratio of each repeating unit in the polymer was determined by measuring the value of F-NMR.
[0355] [Determination of polymer molecular weight] GPC
[0356] A high-speed gel permeation chromatograph (manufactured by TOSOH CORPORATION, model HLC-8320GPC) was used, and ALPHA-M columns and ALPHA-2500 columns (both manufactured by TOSOH CORPORATION) were connected in series one by one, and tetrahydrofuran (THF) was used as a developing solvent to measure the number average molecular weight Mn and weight average molecular weight Mw of the polymer. The detector can use a refractive index difference measurement detector. The molecular weight distribution Mw / Mn was calculated from the number average molecular weight Mn and the weight average molecular weight Mw.
[0357] 2-1. Synthesis of fluorinated copolymer 1
[0358] At room temperature, in a 300 ml glass flask with a stirrer, 62 g of THF was weighed as a solvent into 43.2 g (0.1 mol) of 2-(perfluorohexyl)ethyl methacrylate (MA-C6F) and 19.0 g (0.1 mol) of BTFBE, and 0.8 g (0.005 mol) of α,α-azobisisobutylcyanide (AIBN) was added as a polymerization initiator. The mixture was degassed while stirring, and then the inside of the flask was replaced with nitrogen. The temperature was raised to 75°C and reacted for 6 hours. The reaction system was decompressed, and after THF was distilled off, the reaction system was added dropwise to 300 g of n-heptane to precipitate a transparent viscous substance. The supernatant of the viscous substance was separated by decantation, and dried under reduced pressure at 60°C to obtain 22 g of fluorinated copolymer 1 as a transparent viscous substance, with a yield of 37%.
[0359] <NMR measurement results>
[0360] The content ratio of the repeating units in the fluorinated copolymer 1 was, in terms of molar ratio, repeating unit derived from MA-C6F:repeating unit derived from BTFBE=28:72.
[0361] [Chemical formula 29]
[0362]
[0363] <GPC measurement results>
[0364] Mw=7,300、Mw / Mn=1.4
[0365] 2-2. Synthesis of fluorinated copolymer 2
[0366] At room temperature, in a 300 ml glass flask equipped with a stirrer, 90 g of THF was added to 43.2 g (0.1 mol) of MA-C6F, 27.0 g (0.1 mol) of 1,1,1,3,3,3-hexafluoro-2-(4-vinylphenyl)propane-2-ol (4-HFA-St), and 19.0 g (0.1 mol) of BTFBE, and 0.8 g (0.005 mol) of AIBN was further added, and deaeration was performed while stirring. Then, the inside of the flask was replaced with nitrogen, and the temperature was raised to 75°C and reacted for 6 hours. After the reaction was completed, the solution was concentrated under reduced pressure to remove THF, and then 350 g of n-heptane was added dropwise to precipitate a transparent viscous substance. The supernatant of the viscous substance was separated by decantation and dried under reduced pressure at 60°C to obtain 48 g of fluorinated copolymer 2 as a transparent viscous substance, with a yield of 52%.
[0367] <NMR measurement results>
[0368] The content ratio of the repeating units in the fluorinated copolymer 2 was, in terms of molar ratio, repeating unit derived from MA-C6F:repeating unit derived from 4-HFA-St:repeating unit derived from BTFBE=17:37:46.
[0369] [Chemical formula 30]
[0370]
[0371] <GPC measurement results>
[0372] Mw = 13,300, Mw / Mn = 1.3
[0373] 2-3. Synthesis of fluorinated copolymer 3
[0374] At room temperature, 43.2 g (0.1 mol) of MA-C6F, 16.2 g (0.1 mol) of p-acetoxystyrene (AcO-St), 19.0 g (0.1 mol) of BTFBE, and 80 g of THF were weighed into a 300 ml glass flask equipped with a stirrer, and 0.8 g (0.005 mol) of AIBN was added. The mixture was deaerated while stirring, and then the inside of the flask was replaced with nitrogen. The temperature was raised to 75°C and the mixture was reacted for 6 hours. The reaction system was decompressed, and after THF was distilled off, 350 g of n-heptane was added dropwise to the reaction system to precipitate a transparent viscous substance. The supernatant of the viscous substance was separated by decantation, dissolved in 100 g of methanol, and 10.1 g (0.1 mol) of triethylamine (TEA) was added. In order to decompose the acetoxy solvent, the temperature was raised to 50°C and the mixture was stirred for 8 hours. After confirming the removal of the acetoxy group, the mixture was concentrated and then dried under reduced pressure at 60°C to obtain 35 g of fluorinated copolymer 3 as a white solid. The yield was 55%.
[0375] <NMR measurement results>
[0376] The content ratio of the repeating units in the fluorinated copolymer 3 was, in terms of molar ratio, repeating unit derived from MA-C6F:repeating unit derived from p-hydroxystyrene (p-HO-St):repeating unit derived from BTFBE=12:38:50.
[0377] [Chemical formula 31]
[0378]
[0379] <GPC measurement results>
[0380] Mw=17,500、Mw / Mn=1.4
[0381] 2-4. Synthesis of fluorinated copolymer 4
[0382] Fluorinated copolymer 4 having the following repeating units was synthesized by the same procedure as that of fluorinated copolymer 3 except that hexafluoroisopropyl methacrylate (HFIP-M) was used instead of MA-C6F used in the synthesis of the above fluorinated copolymer 3. Fluorinated copolymer 4 was obtained in a yield of 51%.
[0383] <NMR measurement results>
[0384] The content ratio of the repeating units in the fluorinated copolymer 4 was, in terms of molar ratio, repeating unit derived from HFIP-M:repeating unit derived from p-HO-St:repeating unit derived from BTFBE=15:39:46.
[0385] [Chemical formula 32]
[0386]
[0387] <GPC measurement results>
[0388] Mw=15,200、Mw / Mn=1.4
[0389] 2-5. Synthesis of fluorinated copolymer 5
[0390] Fluorinated copolymer 5 having the following repeating unit was synthesized by the same procedure as that of fluorinated copolymer 3 except that MA-CH2-OFCP was used instead of MA-C6F used in the synthesis of the above fluorinated copolymer 3. Fluorinated copolymer 5 was obtained in a yield of 54%.
[0391] <NMR measurement results>
[0392] The content ratio of the repeating units in the fluorinated copolymer 5 was, in terms of molar ratio, repeating unit derived from MA-CH2-OFCP:repeating unit derived from p-HO-St:repeating unit derived from BTFBE=13:38:49.
[0393] [Chemical formula 33]
[0394]
[0395] <GPC measurement results>
[0396] Mw=16,100、Mw / Mn=1.5
[0397] 2-6. Synthesis of fluorinated copolymer 6
[0398] Except for using 2-(perfluorohexyl)ethyl vinyl ether (V-C6F) instead of MA-C6F used in the synthesis of the above-mentioned fluorinated copolymer 3, the same steps as the synthesis of fluorinated copolymer 3 were used to synthesize fluorinated copolymer 6 containing the following repeating units, and fluorinated copolymer 6 was obtained in a yield of 41%.
[0399] <NMR measurement results>
[0400] The content ratio of the repeating units in the fluorinated copolymer 6 was, in terms of molar ratio, repeating unit derived from V-C6F:repeating unit derived from p-HO-St:repeating unit derived from BTFBE=10:38:52.
[0401] [Chemical formula 34]
[0402]
[0403] <GPC measurement results>
[0404] Mw=11,900、Mw / Mn=1.4
[0405] 2-7. Synthesis of fluorinated copolymer 7
[0406] At room temperature, in a 1000 ml glass flask with a stirrer, 200 g of 2-butanone as a solvent was weighed into 80.9 (0.34 mol) of HFIP-M and 19.1 g (0.14 mol) of 2-hydroxyethyl methacrylate (HEMA), and 1.6 g (0.01 mol) of AIBN was added, and deaeration was performed while stirring. Then, the inside of the flask was replaced with nitrogen, and the temperature was raised to 80°C and reacted for 6 hours. The reaction system was decompressed, 2-butanone was distilled off, and then added dropwise to 500 g of n-heptane to precipitate a white solid. After filtration, it was dried under reduced pressure at 60°C to obtain 80.1 g of fluorinated copolymer 7 as a white solid, with a yield of 80%.
[0407] <NMR measurement results>
[0408] The content ratio of the repeating units in the fluorinated copolymer 7 was, in terms of molar ratio, repeating units derived from HFIP-M:repeating units derived from HEMA=68:32.
[0409] [Chemical formula 35]
[0410]
[0411] <GPC measurement results>
[0412] Mw = 16,600, Mw / Mn = 1.7
[0413] 2-8. Synthesis of fluorinated copolymer 8
[0414] At room temperature, 74.1 (0.31 mol) of HFIP-M, 16.5 g (0.12 mol) of HEMA, 9.5 g (0.11 mol) of vinyl acetate (VAc), and 50 g of butyl acetate were weighed into a 1000 ml glass flask with a stirrer, and 1.6 g (0.01 mol) of AIBN was added, and deaeration was performed while stirring. Then, the inside of the flask was replaced with nitrogen, and the temperature was raised to 80°C and reacted for 6 hours. The reaction system was decompressed, and after butyl acetate was distilled off, it was added dropwise to 500 g of n-heptane to precipitate a white solid. After filtration, it was dried under reduced pressure at 60°C to obtain 85.7 g of fluorinated copolymer 8 as a white solid, with a yield of 78%.
[0415] <NMR measurement results>
[0416] The content ratio of the repeating units in the fluorinated copolymer 8 was, in terms of molar ratio, repeating unit derived from HFIP-M:repeating unit derived from HEMA:repeating unit derived from VAc=68:25:7.
[0417] [Chemical formula 36]
[0418]
[0419] <GPC measurement results>
[0420] Mw=55,500、Mw / Mn=2.1
[0421] 2-9. Synthesis of fluorinated copolymer 9
[0422] At room temperature, 84.6 g (0.2 mol) of MA-C6F, 31.7 g (0.2 mol) of p-acetoxystyrene (AcO-St), 11.2 g (0.06 mol) of BTFBE, and 127 g of THF were weighed into a 300 ml glass flask equipped with a stirrer, and 2.2 g (0.0135 mol) of AIBN was added. The mixture was deaerated while stirring, and then the inside of the flask was replaced with nitrogen. The temperature was raised to 70°C and the mixture was reacted for 6 hours. The reaction system was decompressed, and after THF was distilled off, 850 g of n-heptane was added dropwise to the reaction system to precipitate a transparent viscous substance. The supernatant of the viscous substance was separated by decantation, dissolved in 100 g of methanol, and 10.1 g (0.1 mol) of triethylamine (TEA) was added. In order to decompose the acetoxy solvent, the temperature was raised to 50°C and the mixture was stirred for 8 hours. After confirming the removal of the acetoxy group, the mixture was concentrated and then dried under reduced pressure at 60°C to obtain 95 g of fluorinated copolymer 9 as a white solid. The yield was 86%.
[0423] <NMR measurement results>
[0424] The content ratio of the repeating units in the fluorinated copolymer 9 was, in terms of molar ratio, repeating unit derived from MA-C6F:repeating unit derived from p-HO-St:repeating unit derived from BTFBE=30:50:20.
[0425] [Chemical formula 37]
[0426]
[0427] <GPC measurement results>
[0428] Mw=7,500、Mw / Mn=1.4
[0429] 2-10. Synthesis of fluorinated copolymer 10
[0430] At room temperature, 110.5 g (0.26 mol) of MA-C6F, 45.9 g (0.31 mol) of p-vinylbenzoic acid (VBA), 16.0 g (0.09 mol) of BTFBE, and 340 g of methyl ethyl ketone (MEK) were weighed into a 300 ml glass flask with a stirrer, and 10.8 g (0.065 mol) of AIBN was added. The mixture was deaerated while stirring, and then the inside of the flask was replaced with nitrogen. The temperature was raised to 75°C and reacted for 6 hours. The reaction system was decompressed, and after MEK was distilled off, 1350 g of n-heptane was added dropwise to the reaction system to obtain a white precipitate. After filtration, the mixture was dried under reduced pressure at 60°C to obtain 146.2 g of a thick white solid fluorinated copolymer 10 with a yield of 85%.
[0431] <NMR measurement results>
[0432] The content ratio of the repeating units in the fluorinated copolymer 10 was, in terms of molar ratio, repeating unit derived from MA-C6F:repeating unit derived from VBA:repeating unit derived from BTFBE=30:50:20.
[0433] [Chemical formula 38]
[0434]
[0435] <GPC measurement results>
[0436] Mw = 8,000, Mw / Mn = 1.4
[0437] 3. Synthesis of comparative polymers
[0438] 3-1. Synthesis of Comparative Polymer 1
[0439] At room temperature, 236.2 g (1 mol) of HFIP-M and 450 g of butyl acetate were weighed into a 300 ml glass flask with a stirrer, and 8 g (0.05 mol) of AIBN was added. The mixture was degassed while stirring, and then the inside of the flask was replaced with nitrogen. The temperature was raised to 80° C. and reacted for 6 hours. The reaction system was added dropwise to 500 g of n-heptane to obtain a white precipitate. After filtration, the mixture was dried under reduced pressure at 60° C. to obtain 165 g of comparative polymer 1 as a white solid containing only repeating units derived from HFIP-M, with a yield of 70%.
[0440] [Chemical formula 39]
[0441]
[0442] <GPC measurement results>
[0443] Mw=11,200、Mw / Mn=1.4
[0444] 3-2. Synthesis of comparative polymer 2
[0445] At room temperature, 43.2 g (0.1 mol) of MA-C6F and 85 g of butyl acetate were weighed into a 300 ml glass flask with a stirrer, and 0.8 g (0.005 mol) of AIBN was added. The mixture was degassed while stirring, and then the inside of the flask was replaced with nitrogen. The temperature was raised to 80°C and reacted for 6 hours. The contents were added dropwise to 500 g of n-heptane to obtain a white precipitate. The precipitate was filtered out and dried under reduced pressure at 60°C to obtain 32 g of comparative polymer 2 as a white solid containing repeating units derived from MA-C6F, with a yield of 74%.
[0446] [Chemical formula 40]
[0447]
[0448] <GPC measurement results>
[0449] Mw=13,800、Mw / Mn=1.6
[0450] 3-3. Synthesis of Comparative Polymer 3
[0451] At room temperature, 23.6 g (0.1 mol) of HFIP-M, 43.2 g (0.1 mol) of MA-C6F, and 130 g of butyl acetate were weighed into a 300 ml glass flask with a stirrer, and 0.8 g (0.005 mol) of AIBN was added. The mixture was degassed while being stirred, and then the inside of the flask was replaced with nitrogen. The temperature was raised to 80° C. and the reaction was carried out for 6 hours. The contents after the reaction were added dropwise to 500 g of n-heptane to obtain a white precipitate. The precipitate was filtered out and dried under reduced pressure at 60° C. to obtain 53 g of comparative polymer 3 as a white solid, with a yield of 80%.
[0452] <NMR measurement results>
[0453] In terms of molar ratio, the content ratio of the repeating units in the comparative polymer 3 was repeating units derived from HFIP-M:repeating units derived from MA-C6F=51:49.
[0454] [Chemical formula 41]
[0455]
[0456] <GPC measurement results>
[0457] Mw=14,700、Mw / Mn=1.7
[0458] 3-4. Synthesis of Comparative Polymer 4
[0459] According to Synthesis Example 6 of Patent Document 4, the following synthesis was carried out.
[0460] At room temperature, 2.50 g of a condensate of 4-hydroxyphenyl methacrylate and 1,2-naphthoquinone-2-diazide-5-sulfonyl chloride (HPMA-QD), 0.70 g of methacrylic acid (MAA), 5.26 g of MA-C6F, 2.58 g of methacryloyloxypropyl tris(trimethylsiloxy)silane (MA-P-TTMS), 1.46 g of N-cyclohexylmaleimide (N-CyM), and 51.3 g of cyclohexanone were weighed into a 300 ml glass flask with a stirrer, 0.33 g of AIBN was added, and the mixture was stirred at 110° C. for 20 hours to obtain a comparative polymer 4 having a solid content concentration of 20% by mass and containing the following repeating units.
[0461] [Compound 42]
[0462]
[0463] <GPC measurement results>
[0464] Mw = 11,000, Mw / Mn = 1.5
[0465] 3-5. Synthesis of Comparative Polymer 5
[0466] At room temperature, 7.2 g (0.083 mol) of methacrylic acid (MAA), 9.6 g (0.022 mol) of MA-C6F, 7.2 g (0.055 mol) of 2-hydroxyethyl methacrylate (HEMA), and 55 g of methyl ethyl ketone were weighed into a 300 ml glass flask equipped with a stirrer, and 0.6 g (0.004 mol) of AIBN was added, and stirred at 75° C. for 6 hours. After the reaction was completed, the contents were added dropwise to 500 g of n-heptane to obtain a white precipitate. The precipitate was filtered out and dried under reduced pressure at a temperature of 60° C. to obtain 19 g of comparative polymer 5 as a white solid, with a yield of 80%.
[0467] <NMR measurement results>
[0468] The content ratio of each repeating unit in the comparative polymer 5 was, in terms of molar ratio, repeating unit derived from MA-C6F:repeating unit derived from MAA:repeating unit derived from HEMA=14:52:34.
[0469] [Chemical formula 43]
[0470]
[0471] <GPC measurement results>
[0472] Mw = 5,000, Mw / Mn = 1.4
[0473] 3-6. Mole Ratio and Molecular Weight of Repeating Units of Fluorinated Copolymers 1 to 10 and Comparative Polymers 1 to 5
[0474] Table 1 shows the repeating units contained in the obtained fluorinated copolymers 1 to 10 and comparative polymers 1 to 5, their molar ratios, weight average molecular weight (Mw), molecular weight distribution (Mw / Mn) and yields.
[0475] [Table 1]
[0476]
[0477] MA-c6F: 2-(Perfluorohexyl)ethyl methacrylate [-] in the table means no
[0478] BTFBE: 11-Bis(trifluoromethyl)butadiene
[0479] 4-HFA-st: 1,1,1,3,3,3-hexafluoro-2-(4-vinylphenyl)propane-2-ol
[0480] HO-st: p-Hydroxystyrene
[0481] VBA: p-vinylbenzoic acid
[0482] HFIP-M: Hexafluoroisopropyl methacrylate
[0483] MA-CH2-OFCP: Synthesized in Example
[0484] V-C6F: 2-(Perfluorohexyl)ethyl vinyl ether
[0485] HEMA: 2-Hydroxyethyl Methacrylate
[0486] VAc: Vinyl acetate
[0487] MAA: Methacrylic acid
[0488] 4. Liquid repellency of each polymer film before and after UV ozone cleaning or oxygen plasma cleaning and after heating
[0489] After forming a film on a silicon wafer using the fluorinated copolymers 1 to 10 and the comparative polymers 1 to 5, the contact angles to water, anisole, propylene glycol monomethyl ether acetate (PGMEA) or xylene were measured before and after UV ozone cleaning or oxygen plasma cleaning and after heating. Water, anisole, PGMEA and xylene were used as ink solvents.
[0490] [Manufacturing of film-coated silicon wafers]
[0491] In addition, fluorinated copolymers 1 to 6, 9, 10 and comparative copolymers 1 to 5 were dissolved in propylene glycol monomethyl ether acetate (PGMEA) to form a predetermined film thickness, and applied on a silicon wafer using a spin coater to form a coating film. The film was then heated on a hot plate at 230° C. for 60 minutes to obtain a silicon wafer with a film.
[0492] Fluorinated copolymers 7 to 8 contain a large number of OH groups, and exhibit liquid repellency due to crosslinking of OH groups. Therefore, after preparing the following coating solution, a coating film was formed on a silicon wafer using a spin coater. Then, after pre-baking at 100°C for 150 seconds on a hot plate, the entire film surface was exposed and heated at 230°C for 60 minutes. In addition, the exposure device used a mask aligner MA6 manufactured by SUSSMICROTEC Co., Ltd.
[0493] [Preparation of coating liquid containing fluorinated copolymer 7 or fluorinated copolymer 8]
[0494] 0.2 g of 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine as a crosslinking agent and 0.01 g of a photoacid generator (2-[2-(4-methylphenylsulfonyloxyimino)thiophene-3(2H)-ylidene]-2-(2-methylphenyl)acetonitrile) were dissolved in 4 g of PGMEA with respect to 1 g of fluorinated copolymer 7 or fluorinated copolymer 8, and the mixture was stirred at room temperature for 3 hours to prepare a coating liquid containing either fluorinated copolymer 7 or fluorinated copolymer 8. The photoacid generator was decomposed by exposure after forming a coating film to generate an acid, and the OH group was reduced by crosslinking caused by the acid, thereby obtaining liquid repellency.
[0495] [Washing process and heating process]
[0496] Each silicon wafer with a film was subjected to UV ozone cleaning or oxygen plasma cleaning for 10 minutes using a UV ozone cleaning device, model PL17-110 manufactured by SEN LIGHTS CORPORATION, and a plasma cleaning device, model PDC210 manufactured by Yamato Scientific Co., Ltd. Then, the wafer was heated at 200° C. for 60 seconds.
[0497] [Measurement of contact angle]
[0498] The contact angle of the film surface on the silicon wafer before and after UV ozone cleaning or oxygen plasma cleaning and after subsequent heating to water, anisole, PGMEA or xylene was measured using a contact angle meter (DMs-601 manufactured by Kyowa Interface Science Co., Ltd.).
[0499] [Measurement of film thickness]
[0500] The film thickness of the film on the silicon wafer was measured before and after UV ozone cleaning or oxygen plasma cleaning and after subsequent heating using a contact-type film thickness meter.
[0501] [Determination of molecular weight]
[0502] The film on the silicon wafer before and after UV ozone cleaning or oxygen plasma cleaning and after subsequent heating was dissolved in THF and measured using the above-mentioned GPC.
[0503] Table 2 shows the results of measuring the contact angle to water or anisole and the film thickness before and after UV ozone cleaning and after subsequent heating.
[0504] [Table 2]
[0505]
[0506] As shown in Table 2, the contact angles of the films containing fluorinated copolymers 1 to 10 on silicon wafers to water and anisole decreased after UV ozone cleaning, but after heating, the contact angles recovered to almost the same values as before UV ozone cleaning. In contrast, the contact angles of comparative polymers 1 to 5 recovered only slightly by heating.
[0507] Table 3 shows the value D obtained by subtracting the contact angle of water before UV ozone cleaning from the contact angle of water after UV ozone cleaning. W0 , the value D obtained by subtracting the contact angle of water after UV ozone cleaning from the contact angle of water after heating W1 , the value D obtained by subtracting the contact angle of p-anisole before UV ozone cleaning from the contact angle of p-anisole after UV ozone cleaning A0 , the value D obtained by subtracting the contact angle of p-anisole after UV ozone cleaning from the contact angle of p-anisole after heating A1 Table 3 also shows D W1 / D W0 The value of D A1 / D A0 The value of .
[0508] [Table 3]
[0509]
[0510] Table 4 shows the measurement results of the contact angle to water or anisole and the film thickness before and after oxygen plasma cleaning and after subsequent heating.
[0511] [Table 4]
[0512]
[0513] As shown in Table 4, the contact angles of the films containing fluorinated copolymers 1 to 10 on the silicon wafer to water and anisole decreased after oxygen plasma cleaning, but after heating, the contact angles recovered to almost the same values as before oxygen plasma cleaning. In contrast, the contact angles of comparative polymers 1 to 5 recovered only slightly by heating.
[0514] Table 5 shows the value D obtained by subtracting the contact angle of water before oxygen plasma cleaning from the contact angle of water after oxygen plasma cleaning. W0 The value D is obtained by subtracting the contact angle of water after oxygen plasma cleaning from the contact angle of water after heating. W1 The value D is obtained by subtracting the contact angle of p-anisole before oxygen plasma cleaning from the contact angle of p-anisole after oxygen plasma cleaning. A0 The value D is obtained by subtracting the contact angle of p-anisole after oxygen plasma cleaning from the contact angle of p-anisole after heating. A1 Table 5 also shows DW1 / D W0 The value of D A1 / D A0 The value of .
[0515] [Table 5]
[0516]
[0517] Table 6 shows the measurement results of the contact angle and film thickness to PGMEA or xylene before and after UV ozone cleaning and after subsequent heating.
[0518] [Table 6]
[0519]
[0520] As shown in Table 6, the contact angles of the films containing fluorinated copolymers 1 to 10 on the silicon wafer to PGMEA and xylene decreased after UV ozone cleaning, but after heating, the contact angles recovered to almost the same values as before UV ozone cleaning. In contrast, the contact angles of comparative polymers 1 to 5 recovered only slightly by heating.
[0521] Table 7 shows the value D obtained by subtracting the contact angle for PGMEA before UV ozone cleaning from the contact angle for PGMEA after UV ozone cleaning. P0 , the value D obtained by subtracting the contact angle of PGMEA after UV ozone cleaning from the contact angle of water after heating P1 , the value D obtained by subtracting the contact angle of p-xylene before UV ozone cleaning from the contact angle of p-xylene after UV ozone cleaning X0 , the value D obtained by subtracting the contact angle of p-xylene after UV ozone cleaning from the contact angle of p-xylene after heating X1 Table 7 also shows D P1 / D P0 The value of D X1 / D X0 The value of .
[0522] [Table 7]
[0523]
[0524] Table 8 shows the measurement results of the contact angle and film thickness to PGMEA or xylene before and after oxygen plasma cleaning and after subsequent heating.
[0525] [Table 8]
[0526]
[0527] As shown in Table 8, the contact angles of the films containing fluorinated copolymers 1 to 10 on the silicon wafer to PGMEA and xylene decreased after oxygen plasma cleaning, but after heating, the contact angles recovered to almost the same values as before oxygen plasma cleaning. In contrast, the contact angles of comparative polymers 1 to 5 recovered only slightly by heating.
[0528] Table 9 shows the values obtained by subtracting the contact angle for PGMEA before oxygen plasma cleaning from the contact angle for PGMEA after oxygen plasma cleaning. P0 The value D is obtained by subtracting the contact angle of PGMEA after oxygen plasma cleaning from the contact angle of water after heating. P1 The value D is obtained by subtracting the contact angle of p-xylene before oxygen plasma cleaning from the contact angle of p-xylene after oxygen plasma cleaning. X0 , which is the difference D obtained by subtracting the contact angle of p-xylene after oxygen plasma cleaning from the contact angle of p-xylene after heating X1 Table 9 also shows D P1 / D P0 The value of D X1 / D X0 The value of .
[0529] [Table 9]
[0530]
[0531] Table 10 shows the results of dissolving the film on the silicon wafer before and after UV ozone cleaning, before and after oxygen plasma cleaning, and after subsequent heating in THF and measuring using the above-mentioned GPC.
[0532] [Table 10]
[0533]
[0534] As shown in Table 10, the molecular weights of the films containing the nitrogen-containing copolymers 1 to 10 on the silicon wafer were dissolved in THF and measured. After UV ozone cleaning and oxygen plasma cleaning, no significant change in the molecular weight was observed, indicating that the decomposition of the polymers was suppressed. In contrast, it was confirmed that the molecular weights of the comparative polymers 1 to 5 were greatly reduced.
[0535] 5. Evaluation of resist
[0536] Resists 2, 3, 7, 8 and comparative resist 4 were prepared using fluorinated copolymers 2, 3, 7, 8 and comparative polymer 4, and the resist performance of each resist was evaluated and compared.
[0537] 5-1. Preparation of resist
[0538] [Resist 2]
[0539] To 1.6 g of the fluorinated copolymer 2, 20 g of BMR C-1000 (solid content: 40 mass %) manufactured by TOKYO OHKA KOGYO CO., LTD. as a negative resist and 0.2 g of TPA-100 manufactured by Asahi Kasei Corporation as an isocyanate crosslinking agent were added to prepare a negative resist.
[0540] [Resist 3]
[0541] To 1.6 g of the fluorinated copolymer 3, 20 g of BMR C-1000 (solid content 40 mass %) manufactured by TOKYO OHKA KOGYO CO., LTD. as a negative resist, 0.2 g of 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine as a crosslinking agent, and 0.01 g of (2-[2-(4-methylphenylsulfonyloxyimino)thiophene-3(2H)-ylidene]-2-(2-methylphenyl)acetonitrile as a photoacid generator were added to prepare a negative resist.
[0542] [Resist 7, 8]
[0543] Relative to 1 g of fluorinated copolymer 7 or fluorinated copolymer 8, 0.2 g of 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine as a cross-linking agent and 0.01 g of a photoacid generator (2-[2-(4-methylphenylsulfonyloxyimino)thiophene-3(2H)-ylidene]-2-(2-methylphenyl)acetonitrile) were dissolved in 4 g of PGMEA, and the mixture was stirred at room temperature for 3 hours to prepare an anti-etching agent 7 containing fluorinated copolymer 7 or an anti-etching agent 8 containing fluorinated copolymer 8.
[0544] [Comparative resist 4]
[0545] Comparative Polymer 4 was used to prepare a positive photosensitive resin composition disclosed in Patent Document 4, and Comparative Resist 4 was obtained.
[0546] 5-2. Formation of resist film
[0547] Ultrapure water and then acetone were sprayed onto a silicon wafer having a diameter of 4 inches, and after cleaning by spin coating, UV ozone cleaning was performed for 5 minutes using the above-mentioned UV ozone cleaning device. Next, the above-mentioned resists 2, 3, 7, 8 and comparative resist 4 were filtered using a 0.2 μm membrane filter, and then the above-mentioned filtered resists were applied to the silicon wafer using a spinner at a rotation speed of 1,000 rpm, and heated and dried on a hot plate at 100°C for 150 seconds to form a resist film with a film thickness of 2 μm on the silicon wafer.
[0548] 5-3. Evaluation of resist solubility in developer and resolution of resist pattern
[0549] The resist film formed on the silicon wafer was evaluated for solubility in a developer and resolution of the resist pattern, and the contact angle was measured. The measurement method is shown below.
[0550] The resist film formed on the silicon wafer was exposed to i-line (wavelength 365 nm) through a mask with a line width / space of 5 μm using the above-mentioned mask aligner, and then "post-exposure baking" was performed at 120° C. for 60 seconds.
[0551] [Solubility in developer solution]
[0552] At room temperature, the resist film silicon wafer before and after exposure is immersed in alkaline developer or PGMEA for 60 seconds, and the solubility relative to developer or organic solvent is evaluated. As alkaline developer, 2.38% by mass of tetramethylammonium hydroxide aqueous solution (hereinafter, sometimes referred to as TMAH) is used. The film thickness of the resist film after immersion is measured using an optical interference film thickness meter, thus evaluating the solubility of the resist film. The situation in which the resist film is completely dissolved is recorded as "soluble", and the situation in which the resist film is not dissolved and has residues is recorded as "insoluble".
[0553] [Sensitivity]
[0554] The optimal exposure Eop (mj / cm2) for forming the pattern of the line width / line spacing is calculated. 2 ), which is used as an indicator of sensitivity.
[0555] [Resolution]
[0556] The resist pattern on the patterned silicon wafer was observed under a microscope. The case where no line edge roughness was observed was rated as "excellent", the case where some line edge roughness was observed was rated as "good", and the case where the line edge roughness was significant was rated as "failed".
[0557] Table 11 shows the evaluation results of the developer solubility of each resist and the sensitivity and resolution of the resist pattern.
[0558] [Table 11]
[0559]
[0560] PGMEA: Propylene glycol monomethyl ether acetate
[0561] <Evaluation of developer solubility>
[0562] As shown in Table 11, the unexposed parts of resists 2 and 3 are soluble in alkaline developer or PGMEA, and the exposed parts are insoluble. The unexposed parts of resists 7 and 8 are soluble in PGMEA, and the exposed parts are insoluble, and they can be used as negative resists. The exposed part of comparative resist 4 is soluble in alkaline developer, and it can be used as a positive resist.
[0563] <Sensitivity>
[0564] Resist 3 and comparative resist 4 showed the same degree of sensitivity. Compared with these resists, resists 7 and 8 were highly sensitive.
[0565] <Resolution>
[0566] The resist patterns using Resists 2, 3, 7, 8 and Comparative Resist 4 all transferred the 5 μm line width / line spacing of the mask with good resolution. In particular, no line edge roughness was observed in Resists 7 and 8, and the resolution was "excellent".
[0567] 5-4. Evaluation of liquid repellency of resist pattern before and after UV ozone cleaning and after heating
[0568] The contact angle of p-anisole was measured for the resist film on the silicon wafer using resists 2, 3, 7, 8 and comparative resist 4 before and after UV ozone cleaning and after subsequent heating. The silicon wafer with the resist film was UV ozone cleaned for 10 minutes using the above-mentioned UV ozone cleaning device, and then heated at 200°C for 60 seconds. The contact angle measuring instrument used was a contact angle measuring instrument manufactured by Kyowa InterfaceScience Co., Ltd.
[0569] [Table 12]
[0570]
[0571] [Contact angle measurement results]
[0572] As shown in Table 12, for Resists 2, 3, 7, and 8, the contact angle of anisole at the exposed portion constituting the bank during patterning decreased due to UV ozone cleaning, but increased due to heating, and the liquid repellency was restored.
[0573] 5-5. Evaluation of the liquid repellency of the resist pattern before and after oxygen plasma cleaning and after heating
[0574] The contact angle of p-anisole was measured for the resist film on the silicon wafer using resists 2, 3, 7, 8 and comparative resist 4 before and after oxygen plasma cleaning and subsequent heating. The resist-filmed silicon wafer was oxygen plasma cleaned for 10 minutes using the above-mentioned oxygen plasma cleaning apparatus, and then heated at 200° C. for 60 seconds. The contact angle measuring instrument used was a contact angle measuring instrument manufactured by Kyowa Interface Science Co., Ltd.
[0575] [Table 13]
[0576]
[0577] [Contact angle measurement results]
[0578] As shown in Table 13, for Resists 2, 3, 7, and 8, the contact angle of anisole in the exposed portion constituting the bank during patterning decreased due to oxygen plasma cleaning, but increased due to heating, thereby restoring the liquid repellency.
[0579] Industrial Applicability
[0580] The method for manufacturing a patterned film substrate of the present application can maintain the lyophilicity of the concave portion of the patterned film while making the dam sufficiently lyophobic. Therefore, the method for manufacturing a patterned film substrate of the present application can be applied not only to the manufacture of display elements using an inkjet method, but also to the manufacture of thin films such as organic semiconductor films or colored resin films, or to the manufacture of devices such as display wiring and thin film transistors.
Claims
1. A method for manufacturing a patterned film substrate, comprising: The patterned film substrate is cleaned by UV ozone cleaning or oxygen plasma cleaning to obtain a first patterned film substrate cleaning process. in, The patterned film substrate has a patterned film formed on the substrate; and a heating step of heating the first patterned film substrate to obtain a second patterned film substrate, Through the cleaning step, the contact angle of the pattern film of the first pattern film-bearing substrate is reduced. The contact angle of the pattern film of the second patterned film-attached substrate is restored by the heating step.
2. The manufacturing method according to claim 1, in, The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to anisole from the contact angle of the pattern film of the second pattern film substrate to anisole is recorded as D A1 When D A1 More than 10°.
3. The manufacturing method according to claim 2, in, The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to anisole from the contact angle of the pattern film to anisole before the cleaning step is recorded as D A0 When D A1 / D A0 It is above 0.
30.
4. The production method according to any one of claims 1 to 3, in, The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to water from the contact angle of the pattern film of the second pattern film substrate to water is recorded as D. W1 When D W1 is 10° or more; The value obtained by subtracting the contact angle of the pattern film on the first patterned film substrate to water from the contact angle of the pattern film on water before the cleaning step is recorded as D. W0 When D W1 / D W0 It is above 0.
50.
5. The production method according to any one of claims 1 to 3, in, The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to propylene glycol monomethyl ether acetate from the contact angle of the pattern film of the second pattern film substrate to propylene glycol monomethyl ether acetate is recorded as D P1 When D P1 More than 10°.
6. The manufacturing method according to claim 5, in, The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to propylene glycol monomethyl ether acetate from the contact angle of the pattern film to propylene glycol monomethyl ether acetate before the cleaning step is recorded as D P0 When D P1 / D P0 It is above 0.
30.
7. The production method according to any one of claims 1 to 3, in, The value obtained by subtracting the contact angle of the pattern film of the first pattern film substrate to xylene from the contact angle of the pattern film of the second pattern film substrate to xylene is recorded as D X1 When D X1 More than 15°.
8. The manufacturing method according to claim 7, in, The value obtained by subtracting the contact angle of the pattern film of the first patterned film substrate to xylene from the contact angle of the pattern film to xylene before the cleaning step is recorded as D X0 When D X1 / D X0 It is above 0.
80.
9. The production method according to any one of claims 1 to 3, in, The contact angle of the pattern film of the first pattern film substrate to water is greater than 50°, and the contact angle to anisole is greater than 30°; The pattern film of the second patterned film substrate has a contact angle of 93° or more to water and a contact angle of 50° or more to anisole.
10. The production method according to any one of claims 1 to 3, in, The contact angle of the pattern film of the first pattern film substrate to propylene glycol monomethyl ether acetate is greater than 19°, and the contact angle to xylene is greater than 20°; The pattern film of the second patterned film substrate has a contact angle of 40° or more with respect to propylene glycol monomethyl ether acetate, and a contact angle of 45° or more with respect to p-xylene.
11. The production method according to any one of claims 1 to 3, in, The pattern film comprises a fluorine-containing copolymer having a repeating unit represented by formula (A), [Chemical formula 1] In the formula, R 1 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted by fluorine atoms; Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom; X is a single bond or a divalent group; O is an oxygen atom.
12. The manufacturing method according to claim 11, in, The fluorinated copolymer is any one of the following fluorinated copolymers (1) to (3), The fluorinated copolymer (1) contains a repeating unit represented by the following formula (A) and a repeating unit represented by the following formula (B). [Chemical formula 2] In the formula, R 1 , R 2 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms; Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom; X and Y are each independently a single bond or a divalent group; O is an oxygen atom, and H is a hydrogen atom; The fluorinated copolymer (2) contains a repeating unit represented by the following formula (A) and a repeating unit represented by the following formula (C), [Chemical formula 3] In the formula, R 1 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms; Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom; X is a single bond or a divalent group; Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, wherein the hydrogen atoms in these groups may be substituted with fluorine atoms, oxygen atoms or nitrogen atoms; O is an oxygen atom; A fluorinated copolymer (3): comprising a repeating unit represented by the following formula (A), a repeating unit represented by the following formula (B), and a repeating unit represented by the following formula (C), [Chemical formula 4] In the formula, R 1 , R 2 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms; Q is a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom; X and Y are each independently a single bond or a divalent group; Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms; O is an oxygen atom and H is a hydrogen atom.
13. The production method according to any one of claims 1 to 3, in, In the heating step, the first patterned film substrate is heated at a temperature of 50° C. to 350° C. for 10 seconds or more.
14. The production method according to any one of claims 1 to 3, in, The second patterned film substrate is a substrate for forming a display element by an inkjet method.
15. The manufacturing method according to claim 11, in, In the repeating unit represented by the formula (A), Q is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group.
16. The manufacturing method according to claim 15, in, In the repeating unit represented by the formula (A), Q is a perfluorohexylethyl group, and X is a carbonyl group.
17. The manufacturing method according to claim 15, in, In the repeating unit represented by the formula (A), Q is a hexafluoroisopropyl group, and X is a carbonyl group.
18. The manufacturing method according to claim 11, in, The repeating unit represented by formula (A) is a repeating unit represented by formula (4), [Chemical formula 5] In formula (4), R 4 , R 5 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 3 carbon atoms, wherein a part or all of the hydrogen atoms bonded to carbon atoms in the alkyl group may be substituted with fluorine atoms; O represents an oxygen atom, H represents a hydrogen atom, and F represents a fluorine atom.
19. The manufacturing method according to claim 12, in, In the repeating unit represented by the formula (A), Q is a hexafluoroisopropyl group and X is a carbonyl group; and in the repeating unit represented by the formula (B), Y is a p-phenylene group or a carboxyethylene group.
20. The manufacturing method according to claim 12, in, The repeating unit represented by the formula (A) has Q that is hexafluoroisopropyl and X that is carbonyl; the repeating unit represented by the formula (B) has Y that is p-phenylene or carboxyethylene; and the repeating unit represented by the formula (C) has Z that is alkoxy, carboxyl, acetoxy or bistrifluoromethylvinyl.
21. The manufacturing method according to claim 12, in, In the repeating unit represented by the formula (C), Z is a bistrifluoromethylvinyl group.
22. The manufacturing method according to claim 12, in, In the repeating unit represented by the formula (A), Q is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group; in the repeating unit represented by the formula (B), Y is a p-phenylene group, a p-phenylenecarbonyl group, or a p-phenylenehexafluoroisopropylidene group; and in the repeating unit represented by the formula (C), Z is a bistrifluoromethylvinyl group.
Citation Information
Patent Citations
Production of color filter for liquid crystal, color filter for liquid crystal and liquid crystal panel produced by the same method
JP1998197715A
Positive liquid-repellent resist composition
JP2012220860A
Positive photosensitive resin composition
WO2017126610A1
Cited By
Broadband-gap perovskite thin film and preparation method and application thereof
CN122662565A
A wide band gap perovskite thin film, a preparation method and application thereof
CN122662565B