Photosensitive resin composition, cured film, and display device using the same

By using a photosensitive resin composition containing amide or urethane groups and heat treatment technology, the problem of insufficient durability of organic EL light-emitting elements under high temperature, high humidity and light irradiation conditions is solved, and high durability and low display are achieved Unhealthy effects.

CN112889002BActive Publication Date: 2024-11-19TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980064350.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-12
Filing Date
2019-10-02
Publication Date
2024-11-19
Estimated Expiration
2039-10-02

AI Technical Summary

Technical Problem

The existing organic EL light-emitting elements are not durable under high temperature, high humidity and light irradiation conditions, and are prone to overflow when adding functional materials by inkjet, resulting in poor luminescence. The phenol compounds in the used resin composition lead to degassing components and damage Component life.

Method used

The photosensitive resin composition using an amide group or a urethane group, an alkali-soluble resin and a photosensitive agent is used to form a functional layer in the partition pattern by inkjet method, and a partition wall is formed by heat treatment to improve the ink wetting property. and liquid repellency, reduce display defects and enhance durability.

Benefits of technology

High durability under high temperature, high humidity and light irradiation conditions are achieved, display defects are reduced, ink wetting and film thickness uniformity are improved, and the life of organic EL light-emitting elements is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002998498480000051
    Figure BDA0002998498480000051
  • Figure BDA0002998498480000052
    Figure BDA0002998498480000052
  • Figure BDA0002998498480000053
    Figure BDA0002998498480000053
Patent Text Reader

Abstract

The object of the present invention is to provide a photosensitive resin composition having excellent ink wettability at the opening and sufficient liquid repellency in the cured film. In addition, the object of the present invention is to provide a display device with less occurrence of display failure and high durability for subsequent heat treatment. One mode of the photosensitive resin composition of the present invention for achieving the above-mentioned object is a photosensitive resin composition containing a liquid repellent material (A) having at least an amide group or a carbamate group, an alkali-soluble resin (B) and a photosensitive agent (E), wherein the alkali-soluble resin (B) comprises at least one alkali-soluble resin selected from the group consisting of polyimide, polybenzoxazole, polyamide-imide, their precursors and their copolymers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photosensitive resin composition, a cured film, and a display device using the cured film. Background Art

[0002] In display devices with thin displays such as smart phones, tablet PCs, and televisions, many products using organic electroluminescent (hereinafter referred to as "organic EL") light-emitting elements have been developed. Typically, an organic EL light-emitting element has a driving circuit, a planarization layer, a first electrode, an insulating layer, a light-emitting layer, and a second electrode on a substrate, and emits light by applying a voltage between the opposing first electrode and the second electrode. Among these, as a material for a planarization layer and a material for an insulating layer, a photosensitive resin composition that can be patterned by ultraviolet irradiation is generally used. Among them, for a photosensitive resin composition using a polyimide-based or polybenzoxazole-based resin, the resin has high heat resistance, and the gas component generated from the cured film is small, so it is possible to provide a highly durable organic EL display device, which can be suitably used from this aspect (patent document 1).

[0003] In recent years, printing methods represented by inkjet method have been gradually used in the formation of light-emitting layers. Specifically, for example, the following method is known: after forming a partition wall pattern on a substrate, a functional material solution such as a light-emitting material, a hole transport material, and an electron transport material is dripped into the opening between the partition walls by inkjet method to form an organic EL light-emitting element having a functional layer.

[0004] In order to drop a functional material solution into a predetermined region of a partition wall pattern by inkjet method, the partition wall pattern needs to be rendered liquid-repellent. To achieve this purpose, a method of rendering the upper surface of the partition wall pattern on the substrate liquid-repellent by fluorination treatment based on plasma irradiation has been studied (Patent Document 2).

[0005] In addition, a method of forming a partition wall by adding a photosensitive resin composition having a liquid-repellent compound is also studied. For example, a resist composition containing a specific fluorine-based polymer (Patent Document 3) and a photosensitive resin composition having a fluorine-containing compound having a silane compound and a Novolac-type phenolic resin as main components (Patent Document 4) are studied.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2002-91343

[0009] Patent Document 2: Japanese Patent No. 4612773

[0010] Patent Document 3: Japanese Patent Application Publication No. 2012-220860

[0011] Patent Document 4: Japanese Patent No. 6098635 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, demands for high durability such as longer driving life are becoming increasingly stringent for organic EL light-emitting elements, and they are required to maintain performance as light-emitting elements even after durability tests under accelerated conditions such as high temperature, high humidity, and light irradiation.

[0014] In the technology of Patent Document 1, since the formed partition walls are not liquid-repellent, there is a problem that the functional material solution dropped by the inkjet method goes over the partition walls and mixes into nearby pixels, causing light emission failure.

[0015] The technology of Patent Document 2 has a problem in that the liquid-repellent component also adheres to the openings between the partition walls due to the fluorination treatment, and the ink wettability of the openings becomes insufficient.

[0016] In addition, with regard to the technologies of Patent Documents 3 and 4, although they have sufficient liquid repellency and can form patterns as photosensitive resin compositions, since phenol compounds are used as the main component of the resin, they are prone to display defects due to outgassing components from the resin composition that constitutes the partition pattern, thereby greatly damaging the driving life of the organic EL element.

[0017] Therefore, the object of the present invention is to solve the problems associated with the above-mentioned prior art and provide a photosensitive resin composition having excellent ink wettability in an opening portion and having a cured film having sufficient liquid repellency. In addition, the object of the present invention is to provide a display device having a cured film of the photosensitive resin composition, which has little occurrence of display failure and has high durability against subsequent heat treatment.

[0018] Means for solving problems

[0019] In order to solve the above problems, the present invention has the following configuration.

[0020] A first embodiment of the photosensitive resin composition of the present invention is a photosensitive resin composition comprising a lyophobic material (A) having at least an amide group or a urethane group, an alkali-soluble resin (B) and a photosensitizer (E), wherein the alkali-soluble resin (B) comprises at least one alkali-soluble resin selected from the group consisting of polyimide, polybenzoxazole, polyamide-imide, their precursors and their copolymers.

[0021] Moreover, the 1st aspect of the cured film of this invention contains the hardened|cured material of the 1st aspect of the photosensitive resin composition of this invention.

[0022] Moreover, the 1st aspect of the display device of this invention is a display device which has a grid-shaped partition formed on a substrate, and this partition consists of the 1st aspect of the cured film of this invention.

[0023] A first aspect of the method for producing a substrate with partition walls according to the present invention includes the following steps (1) to (4) in order.

[0024] Step (1), coating the first embodiment of the photosensitive resin composition of the present invention on a substrate having a first electrode to form a photosensitive resin film;

[0025] Step (2), exposing the photosensitive resin film;

[0026] Step (3), developing the exposed photosensitive resin film;

[0027] In step (4), the developed photosensitive resin film is subjected to a heat treatment to form a partition wall.

[0028] Furthermore, a first aspect of the method for manufacturing a display device of the present invention includes the following steps (5) to (6) in order.

[0029] Step (5) of forming a functional layer by inkjet coating a functional ink in a region surrounded by a partition wall on a substrate having a partition wall comprising a cured product of the first embodiment of the photosensitive resin composition of the present invention.

[0030] Step (6), forming a second electrode on the functional layer.

[0031] Effects of the Invention

[0032] The present invention can provide a photosensitive resin composition having excellent ink wettability at an opening and having a cured film having sufficient liquid repellency. In addition, the present invention can provide a display device having a cured film of the photosensitive resin composition, which has little occurrence of display failure and has high durability against subsequent heat treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] [ Figure 1 ] is an example of a cross-section obtained by cutting a grid-shaped partition wall formed on a substrate perpendicularly relative to the length direction of the partition wall and the surface of the substrate.

[0034] [ Figure 2 ] is a schematic diagram of the substrate used in the evaluation of the embodiment. DETAILED DESCRIPTION

[0035] Embodiments of the present invention will be described in detail.

[0036] A first embodiment of the photosensitive resin composition of the present invention is a photosensitive resin composition comprising a lyophobic material (A) having at least an amide group or a urethane group, an alkali-soluble resin (B) and a photosensitizer (E), wherein the alkali-soluble resin (B) comprises at least one alkali-soluble resin selected from the group consisting of polyimide, polybenzoxazole, polyamide-imide, their precursors and their copolymers.

[0037] In the first embodiment of the photosensitive resin composition of the present invention, in order to impart liquid repellency to the surface of the cured film, a liquid repellent material (A) having at least an amide group or a carbamate group is contained. It should be noted that in the first embodiment of the photosensitive resin composition of the present invention, "the liquid repellent material (A) having at least an amide group or a carbamate group" is sometimes referred to as "(A) component" or "liquid repellent material (A)". By making the (A) component have an amide group or a carbamate group, it has the effect of improving the compatibility with the alkali-soluble resin (B) described later, reducing defects such as shrinkage, and improving the uniformity of the film thickness of the cured film, and as a result, reducing the display defects of the display device. In particular, in the first embodiment of the photosensitive resin composition of the present invention, the alkali-soluble resin (B) contains at least one alkali-soluble resin selected from the group consisting of polyimide, polybenzoxazole, polyamide-imide, their precursors and their copolymers, so that the effect of significantly improving compatibility can be obtained.

[0038] The liquid-repellent material (A) having at least an amide group or a urethane group preferably contains a compound having a structural unit represented by the following general formula (1) or the following general formula (11).

[0039] [Chemical formula 1]

[0040]

[0041] In the general formula (1), R 1 , R 2 and R 3 The monovalent organic groups representing hydrogen atoms or carbon 1 to 4 atoms may be the same or different.

[0042] [Chemical formula 2]

[0043]

[0044] In the general formula (11), R 18 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 19 represents an aliphatic group having 1 to 6 carbon atoms. A represents a carbamate group of (A-1) or (A-2) described below.

[0045] [Chemical formula 3]

[0046]

[0047] The compound having the structural unit represented by the general formula (1) or (11) can be obtained, for example, by (co)polymerizing a (meth)acrylamide monomer represented by the following general formula (3) or a (meth)acrylate monomer represented by the following general formula (12).

[0048] [Chemical formula 4]

[0049]

[0050] In the general formula (3), R 1 , R 2 and R 3 The monovalent organic groups representing hydrogen atoms or carbon 1 to 4 atoms may be the same or different.

[0051] [Chemical formula 5]

[0052]

[0053] In the general formula (12), R 18 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 19 represents an aliphatic group having 1 to 6 carbon atoms. A represents a carbamate group represented by the following formula (A-1) or (A-2).

[0054] [Chemical formula 6]

[0055]

[0056] Preferred examples of the (meth)acrylamide monomer represented by the general formula (3) include N,N-dimethylacrylamide and N,N-diethylacrylamide.

[0057] Moreover, as a preferable example of the (meth)acrylic acid ester monomer represented by General formula (12), the following structures are mentioned.

[0058] [Chemical formula 7]

[0059]

[0060] From the perspective of improving compatibility with the alkali-soluble resin (B), the total amount of the structural units represented by the general formula (1) or the general formula (11) is preferably 15 mol% or more, more preferably 30 mol% or more, of the total amount of the structural units constituting the lyophobic material (A). In order to further improve the lyophobicity, the total amount is preferably 85 mol% or less, more preferably 70 mol% or less.

[0061] In the first embodiment of the photosensitive resin composition of the present invention, from the viewpoint of improving alkali solubility, the lyophobic material (A) having at least an amide group or a carbamate group preferably contains a compound having a carbamate group, and more preferably contains a compound having a structural unit represented by the general formula (11). By improving alkali solubility, the residue in the opening portion during alkali development is reduced, and thus the wettability of the functional ink applied to the opening portion can be further improved. As a result, the uniformity of the film thickness of the functional layer formed by the functional ink is easily improved, the display defects of the display device are easily reduced, and the durability is easily further improved.

[0062] The liquid-repellent material (A) having at least an amide group or a carbamate group preferably contains a compound having a structural unit represented by the general formula (2) or a structure represented by the general formula (13). By having a structural unit represented by the general formula (2) or a structure represented by the general formula (13), liquid repellency can be easily imparted to the surface of the cured film.

[0063] [Chemical formula 8]

[0064]

[0065] In the general formula (2), R 4 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 5 represents an aliphatic group having 1 to 6 carbon atoms, R 6 It represents a perfluoroalkyl group having 3 to 6 carbon atoms.

[0066] [Chemical formula 9]

[0067]

[0068] In the general formula (13), X is selected from the following structural formulae (a) to (e), and all X may have the same structure or may have multiple structures present randomly or in blocks. m is an integer of 1 to 100 indicating the number of repeating units.

[0069] [Chemical formula 10]

[0070]

[0071] The compound having the structural unit represented by the general formula (2) or the structure represented by the general formula (13) can be obtained, for example, by (co)polymerizing a (meth)acrylate monomer represented by the general formula (4) or a monomer having a structure represented by the general formula (13).

[0072] [Chemical formula 11]

[0073]

[0074] In the general formula (4), R 4represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 5 represents an aliphatic group having 1 to 6 carbon atoms, R 6 It represents a perfluoroalkyl group having 3 to 6 carbon atoms.

[0075] Preferred examples of the (meth)acrylate monomer having a perfluoroalkyl group represented by the general formula (4) include 2-(perfluorobutyl)ethyl (meth)acrylate and 2-(perfluorohexyl)ethyl (meth)acrylate.

[0076] Preferred examples of the monomer having a structure represented by the general formula (13) include monomers having the following structures.

[0077] [Chemical formula 12]

[0078]

[0079] [Chemical formula 13]

[0080]

[0081] In the first embodiment of the photosensitive resin composition of the present invention, from the viewpoint of further improving the alkali solubility, the lyophobic material (A) having at least an amide group or a carbamate group preferably contains a compound having a structure represented by the general formula (13). By further improving the alkali solubility, the residue in the opening portion during alkali development is reduced, and thus the wettability of the functional ink applied to the opening portion can be further improved. As a result, the uniformity of the film thickness of the functional layer formed by the functional ink is improved, and it is easy to obtain a reduction in display defects and an improvement in durability of the display device.

[0082] In the first embodiment of the photosensitive resin composition of the present invention, the lyophobic material (A) having at least an amide group or a carbamate group contains a compound having a carbamate group and a structure represented by the general formula (13). By containing this compound, it is easy to further improve the alkali solubility of the component (A). The first embodiment of the photosensitive resin composition of the present invention more preferably contains a compound having a structural unit represented by the general formula (11) and a structure represented by the general formula (13).

[0083] Commercially available products of liquid-repellent materials comprising a compound having a structural unit represented by the general formula (11) and a structure represented by the general formula (13) (which belongs to a compound containing a carbamate group and a structure represented by the general formula (13)) include "Megafac (registered trademark)" RS-72-K, RS-72-A, RS-75, RS-76-E, RS-76-NS, RS-78, and RS-90 (manufactured by DIC Corporation).

[0084] The lyophobic material (A) having at least an amide group or a carbamate group preferably also has an epoxy group. By having an epoxy group, it is easy to further improve the durability as a light-emitting element by condensation with the alkali-soluble resin (B). The (A) component more preferably also has a structural unit represented by the general formula (5). The component (A) having a structural unit represented by the general formula (5) can be obtained, for example, by copolymerizing an epoxy-containing (meth)acrylate monomer represented by the general formula (6) as one of the copolymerization components.

[0085] [Chemical formula 14]

[0086]

[0087] [Chemical formula 15]

[0088]

[0089] In the general formulas (5) and (6), R 7 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 8 It represents a monovalent organic group having 2 to 16 carbon atoms and having an epoxy group.

[0090] Preferred examples of the epoxy group-containing (meth)acrylate monomer represented by the general formula (6) include glycidyl acrylate, glycidyl methacrylate, 4-hydroxybutyl acrylate glycidyl ether (4-HBAGE), 4-hydroxybutyl methacrylate glycidyl ether, acrylates having an alicyclic epoxy group, and methacrylates having an alicyclic epoxy group.

[0091] In addition, the structural unit represented by the general formula (5) is preferably 10 mol% or more of the structural unit constituting the lyophobic material (A), and more preferably 20 mol% or more. If it is within this range, when forming a cured film of the photosensitive resin composition, it is polycondensed with the alkali-soluble resin (B) to form a cured film with high heat resistance, the heat resistance of the cured film of the photosensitive resin composition is increased, and the durability of the display device is improved. In addition, in order to obtain the effect of improving the lyophobicity and compatibility with the alkali-soluble resin (B), it is preferably 50 mol% or less, and more preferably 40 mol% or less.

[0092] The lyophobic material (A) having at least an amide group or a carbamate group may also be a copolymer further copolymerized with a (meth) acrylic monomer substituted with different functional groups. By further copolymerizing with a (meth) acrylic monomer substituted with different functional groups, it is possible to easily obtain a balance between lyophobicity and solubility. For example, there may be mentioned (meth) acrylic esters containing hydroxyl groups, (meth) acrylamides containing hydroxyl groups, (meth) acrylic esters containing alkoxy groups, (meth) acrylic esters containing blocked isocyanate groups, (meth) acrylic esters containing phenoxy groups, (meth) acrylic alkyl esters, compounds containing vinyl groups, and the like.

[0093] Examples of the (meth)acrylates containing a hydroxyl group include 2-hydroxyethyl (meth)acrylate and the like.

[0094] Examples of the (meth)acrylamides containing a hydroxyl group include N-hydroxymethacrylamide and the like.

[0095] As (meth)acrylates which have an alkoxy group, 3-methacryloxypropylmethyldimethoxysilane etc. are mentioned, for example.

[0096] Examples of the blocked isocyanate group-containing (meth)acrylates include 2-(0-[1′-methylpropyleneamino]carboxyamino)ethyl methacrylate (Karenz MOI-BM: manufactured by Showa Denko K.K.; registered trademark).

[0097] Examples of the phenoxy group-containing (meth)acrylates include 2-phenoxybenzyl acrylate and 3-phenoxybenzyl acrylate.

[0098] The alkyl (meth)acrylates include diluent monomers such as unsubstituted or substituted alkyl (meth)acrylates, such as alkyl acrylates, which have a linear, branched and / or cyclic alkyl group having 1 to 12 carbon atoms and which is unsubstituted or substituted with at least one of an amino group, a monoalkylamino group, a dialkylamino group, a hydrocarbon aromatic ring, and a heterocyclic ring, or to which a hydroxyl group can be cleaved and added with an acid anhydride, and the like.

[0099] Examples of the vinyl group-containing compounds include n-butyl vinyl ether and the like.

[0100] The compound contained in the lyophobic material (A) having at least an amide group or a carbamate group is usually a (co)polymer. The (co)polymer of the compound contained in the lyophobic agent (A) can be obtained by a known polymerization method. The (co)polymer can be obtained, for example, by ionic polymerization such as free radical polymerization and anionic polymerization. In addition, it can be any of a random copolymer, a block copolymer, a graft (co)polymer, or an alternating copolymer. Here, a free radical (co)polymerization method is cited as an example. For example, component (A) can be obtained by the following method: random copolymerization of a predetermined amount of dimethyl (meth) acrylamide, a predetermined amount of fluorine-containing (meth) acrylate monomer, and a predetermined amount of epoxy-containing (meth) acrylates, hydroxyl-containing (meth) acrylates, hydroxyl-containing (meth) acrylamides, alkoxy-containing (meth) acrylates, blocked isocyanate-containing (meth) acrylates, phenoxy-containing (meth) acrylates, (meth) alkyl esters, and vinyl-containing compounds in an appropriate solvent in the presence of a free radical polymerization initiator and a chain transfer agent added as needed. As a free radical polymerization initiator, for example, tert-butyl peroxy 2-ethylhexanoate can be used. As a chain transfer agent, for example, dodecyl mercaptan can be used. In addition, as a solvent, for example, an inactive solvent such as cyclohexanone can be used.

[0101] The weight average molecular weight of the lyophobic material (A) having at least an amide group or a carbamate group is preferably in the range of 1500 to 50000. By making the molecular weight within this range, it can be more easily dissolved in the solvent used in the photosensitive resin composition. In addition, by making the molecular weight within this range, it is easy to improve the defoaming property of the photosensitive resin composition solution.

[0102] From the viewpoint that the obtained cured film is easy to fully exhibit liquid repellency, the liquid repellent material (A) having at least an amide group or a carbamate group is preferably 0.1 parts by mass or more, and more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the alkali-soluble resin (B). In addition, from the viewpoint that liquid repellency is not easily generated in the pixel and high durability is easily obtained, it is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less.

[0103] The first embodiment of the photosensitive resin composition of the present invention contains an alkali-soluble resin (B) (hereinafter, sometimes referred to as component (B)). In the first embodiment of the photosensitive resin composition of the present invention, the alkali-soluble resin refers to a resin having a dissolution rate of 50 nm / min or more as defined below. Specifically, it refers to the following resin: a solution obtained by dissolving the resin in γ-butyrolactone is applied to a silicon wafer, pre-baked at 120°C for 4 minutes to form a pre-baked film with a film thickness of 10 μm±0.5 μm, the pre-baked film is immersed in a 2.38 mass% tetramethylammonium hydroxide aqueous solution at 23±1°C for 1 minute, and then rinsed with pure water, and the dissolution rate calculated based on the reduction in film thickness at this time is 50 nm / min or more.

[0104] In the first embodiment of the photosensitive resin composition of the present invention, the alkali-soluble resin (B) preferably has an alkali-soluble group in the structural unit of the resin and / or at the end of its main chain in order to impart alkali solubility. The alkali-soluble group refers to a functional group that increases solubility in an alkaline solution by interacting or reacting with a base, and specifically, an acidic group and the like can be cited. Preferred alkali-soluble groups include carboxyl groups, phenolic hydroxyl groups, sulfonic acid groups, thiol groups, and the like.

[0105] The alkali-soluble resin (B) in the first embodiment of the present invention comprises at least one alkali-soluble resin selected from the group consisting of polyimide, polybenzoxazole, polyamide-imide, their precursors and their copolymers. These alkali-soluble resins can be used alone, or a plurality of alkali-soluble resins can be used in combination. These alkali-soluble resins have high heat resistance, so when used in a display device, the amount of outgassing at a high temperature of more than 200°C after heat treatment decreases, which can improve the durability of the display device.

[0106] For preferred embodiments of polyimide, polybenzoxazole, polyamideimide, precursors thereof, and copolymers thereof used as the alkali-soluble resin (B), see the description of the alkali-soluble resin (BI) in the second embodiment of the photosensitive resin composition of the present invention described later.

[0107] The first mode of the photosensitive resin composition of the present invention preferably further contains at least one resin (C) selected from the group consisting of phenolic resins and polyhydroxystyrene resins (hereinafter, sometimes referred to as component (C). These resins have the function of a compatibilizer. By mixing them, the compatibility of component (A) and component (B) can be further improved, which helps to stabilize the solubility of each component in the developer and easily improves the straightness of the pattern. As a result, it is expected that the display defect of the display device will be reduced. In addition, when a positive photosensitizer is used as the photosensitive agent (E) described later, by containing component (C), the film loss amount in the development process can be reduced, so it is easy to make component (A) stay on the surface of the film after development, and the process margin for obtaining good liquid repellency can be improved.

[0108] In the first embodiment of the photosensitive resin composition of the present invention, the sum of at least one resin (C) selected from the group consisting of the above-mentioned phenolic resin and polyhydroxystyrene resin is preferably 10 to 100 parts by mass relative to 100 parts by mass of the above-mentioned alkali-soluble resin (B). From the viewpoint of improving the compatibility of the components (A) and (B) so that the straightness of the pattern is good and the display failure of the display device is easily reduced, the sum of the components (C) is preferably 10 parts by mass or more, and more preferably 30 parts by mass or more. In addition, from the viewpoint of not easily reducing the durability of the cured film of the photosensitive resin composition, it is preferably 100 parts by mass or less, and more preferably 80 parts by mass or less.

[0109] For preferred embodiments of at least one resin (C) selected from the group consisting of phenolic resins and polyhydroxystyrene resins, see the description of at least one resin (CI) among phenolic resins and polyhydroxystyrene resins in the second embodiment of the photosensitive resin composition of the present invention described later.

[0110] The first embodiment of the photosensitive resin composition of the present invention preferably further contains a thermal crosslinking agent (D). By containing a thermal crosslinking agent (D), the durability of the display device is easily further improved. For preferred embodiments of the thermal crosslinking agent (D), see the description of the thermal crosslinking agent (DI) in the second embodiment of the photosensitive resin composition of the present invention described later.

[0111] The first embodiment of the photosensitive resin composition of the present invention contains a photosensitive agent (E). The photosensitive agent (E) may be a negative type that is cured by light, or a positive type that is solubilized by light. As the photosensitive agent (E), it is preferred to contain (e-1) a polymerizable unsaturated compound and a photopolymerization initiator, or (e-2) a quinonediazide compound, etc. In the first embodiment of the photosensitive resin composition of the present invention, from the viewpoint of forming a step-shaped partition wall described later by halftone processing and one photolithography, it is preferably a positive type. For the preferred embodiment of the photosensitive agent (E), please refer to the description of the photosensitive agent (EI) in the second embodiment of the photosensitive resin composition of the present invention described later.

[0112] The first embodiment of the photosensitive resin composition of the present invention preferably further contains a colorant (F). Specific examples of the colorant (F) include known organic pigments, inorganic pigments or dyes commonly used in the field of electronic information materials. The colorant (F) is preferably an organic pigment and / or an inorganic pigment. For preferred embodiments of the colorant (F), see the description of the colorant (FI) in the second embodiment of the photosensitive resin composition of the present invention described later.

[0113] The first embodiment of the photosensitive resin composition of the present invention preferably contains an organic solvent (G). As the organic solvent (G), for example, ethers, acetates, esters, ketones, aromatic hydrocarbons, amides or alcohols can be cited. For preferred embodiments of the organic solvent (G), see the description of the organic solvent (GI) in the second embodiment of the photosensitive resin composition of the present invention described later.

[0114] The first embodiment of the photosensitive resin composition of the present invention may contain an adhesion improver. Preferred embodiments of the adhesion improver are as described for the adhesion improver in the second embodiment of the photosensitive resin composition of the present invention described later.

[0115] Next, the method for manufacturing the photosensitive resin composition of the present invention is described. The first embodiment of the photosensitive resin composition of the present invention can be obtained, for example, by dissolving the above-mentioned (A) component to the colorant (F) in an organic solvent (G). As the dissolution method, stirring, heating, etc. can be mentioned. When heating, the heating temperature is preferably set within a range that does not damage the performance of the resin composition, usually 20°C to 80°C. In addition, the dissolution order of each component is not particularly limited, for example, there is a method of dissolving in order from compounds with low solubility.

[0116] The obtained photosensitive resin composition is preferably filtered using a filter to remove dust and particles. For preferred embodiments of the filter, see the description of the filter in the second embodiment of the photosensitive resin composition of the present invention described later.

[0117] The first aspect of the cured film of the present invention is formed from the cured product of the first aspect of the photosensitive resin composition of the present invention.

[0118] The description of the method for producing the cured film of the first embodiment of the present invention corresponds to the method for producing a cured film of the second embodiment of the photosensitive resin composition of the present invention described later.

[0119] The first embodiment of the cured film of the present invention can be used for electronic components such as organic EL display devices, semiconductor devices, and multilayer wiring boards. Specifically, it is preferably used for the partition wall of an organic EL element, the flattening layer of a substrate with a drive circuit of a display device using an organic EL element, the interlayer insulating film between the rewiring of a semiconductor device or a semiconductor component, the passivation film of a semiconductor, the protective film of a semiconductor element, the interlayer insulating film of a multilayer wiring for high-density packaging, the wiring protective insulating layer of a circuit substrate, the on-chip microlens of a solid-state imaging element, and the flattening layer for various displays and solid-state imaging elements. As an electronic device having a surface protective film, an interlayer insulating film, etc. configured with the first embodiment of the cured film of the present invention, for example, a magnetoresistive memory (hereinafter referred to as MRAM) with low heat resistance can be cited. That is, the first embodiment of the cured film of the present invention is suitable for use as a surface protective film of an MRAM. In addition, it can be used for the partition wall and insulating layer of a display device (specifically, for example, LCD, ECD, ELD, organic EL, etc.) comprising a first electrode formed on a substrate and a second electrode arranged opposite to the first electrode. More preferably, it can be used as a partition wall of the following display device, in which a functional layer is formed by applying a functional ink by inkjet in an area (pixel) surrounded by a grid-shaped partition wall formed on a substrate. The first embodiment of the cured film of the present invention has good liquid repellency, and can prevent the ink applied by inkjet from penetrating into adjacent pixels, thereby reducing the occurrence of display defects. In addition, the first embodiment of the cured film of the present invention has a small amount of outgassing at high temperature, and therefore, it can be preferably used in an organic EL display device containing at least one selected from the group consisting of an organic EL light-emitting material, a hole injection material, and a hole transport material in the functional layer.

[0120] In the first embodiment of the cured film of the present invention, the contact angle of the surface of the cured film when propylene glycol monomethyl ether acetate is dropped by the sessile drop method according to JIS-R3258 is preferably 30° or more, more preferably 40° or more. The contact angle of the surface of the cured film, for example, increases when the content of the lyophobic material (A) having at least an amide group or a carbamate group is increased, and decreases when the content of the lyophobic material (A) is reduced. Therefore, for example, the above range can be achieved by adjusting the content of the lyophobic material (A) having at least an amide group or a carbamate group.

[0121] The first embodiment of the display device of the present invention is a display device having a grid-shaped partition wall formed on a substrate, and the partition wall includes the first embodiment of the cured film of the present invention. By including the first embodiment of the cured film of the present invention, the occurrence of display defects of the display device can be reduced. In addition, the amount of outgassing at a high temperature of 200°C or more after heat treatment is reduced, and the durability of the display device can be improved. In addition, the first embodiment of the cured film of the present invention has good liquid repellency, so that the ink applied to the pixel surrounded by the grid-shaped partition wall by inkjet can be prevented from penetrating into the adjacent pixel, thereby reducing the occurrence of display defects.

[0122] In the first mode of the display device of the present invention, the lattice-shaped partition walls formed on the substrate have a stepped shape including a first partition wall portion (a cross section of which is a trapezoidal shape when cut vertically relative to the length direction of the partition wall and the surface of the substrate) and a second partition wall portion (which is located on the upper part of the first partition wall portion and has a trapezoidal cross section). In the cross section, when the width of the upper surface of the first partition wall portion is set to A and the width of the bottom surface of the second partition wall portion is set to B, the relationship A>B is preferably satisfied. Figure 1 2 shows an example of a schematic diagram of a cross section of a grid-shaped partition wall formed on a substrate cut perpendicularly to the longitudinal direction of the partition wall and the surface of the substrate. The partition wall is formed on a substrate 8 having a first electrode 2 . Figure 1 In the example, the partition wall has a stepped shape having a second partition wall portion 10 having a trapezoidal cross section on an upper portion of a first partition wall portion 9, and satisfies the relationship A>B.

[0123] Usually, in a region (pixel) surrounded by a lattice-shaped partition wall formed on a substrate, when a functional ink is applied by inkjet to form a functional layer, after the functional ink is applied, the solvent contained in the functional ink is dried to form the functional layer. The drying of the ink droplets starts near the partition wall, so there is a tendency that the viscosity of the ink near the partition wall increases as the drying proceeds. Therefore, it is known that the film thickness of the functional layer is thicker at the end than at the center. In the case of an organic EL display device, this is the cause of the problem that the brightness of the central and peripheral portions of the pixel is different.

[0124] In the first mode of the display device of the present invention, in the area surrounded by the above-mentioned grid-shaped partitions with a step shape, when the functional ink is applied by inkjet, an end of the functional layer with a thicker film thickness can be formed on the upper surface of the first partition portion. That is, in the surface cut in the direction perpendicular to the substrate, the end of the functional layer can be made to be located on the side surface of the above-mentioned second partition portion. In such a structure, the end of the functional layer with a thicker film thickness does not emit light due to the first partition portion, and only the area of ​​the functional layer with a uniform film thickness can emit light. As a result, the problem of different brightness at the center and end of the pixel can be eliminated. Figure 1In one example of a schematic diagram of a cross section of a partition wall, a functional layer 11 and an end portion 12 of the functional layer are shown.

[0125] In the first embodiment of the display device of the present invention, the film thickness of the partition wall is preferably 0.5 to 5.0 μm. When it is 0.5 μm or more, the functional ink can be easily retained in the pixel. From the viewpoint of facilitating the processing of the photosensitive resin composition by photolithography, the film thickness of the partition wall is preferably 5.0 μm or less. In addition, the film thickness of the first partition wall portion is preferably 0.1 to 1.0 μm. When the film thickness of the first partition wall portion is 0.1 μm or more, the insulation required for the partition wall can be maintained. When the film thickness of the first partition wall portion is 1.0 μm or less, a thicker functional layer end portion can be formed on the upper part of the first partition wall portion. In the first embodiment of the display device of the present invention, it is more preferred that the film thickness of the partition wall is 0.5 to 5.0 μm and the film thickness of the first partition wall portion is 0.1 to 1.0 μm.

[0126] In the first embodiment of the display device of the present invention, it is preferred that the first partition wall portion and the second partition wall portion are formed of a cured film of the same material. In the present invention, the so-called "same material" means formed of the same photosensitive resin composition. If it is the first embodiment of the photosensitive resin composition of the present invention, a step difference shape can be easily formed by half exposure described later and one photolithography.

[0127] The first mode of the display device of the present invention preferably forms a functional layer in the area surrounded by the partition wall of the above-mentioned display device. For example, by forming a coloring layer that colors the transmitted light and configuring a plurality of coloring layers with different colors in each pixel, it can be used as a color filter. Alternatively, by forming an organic EL light-emitting layer containing at least one selected from an organic EL light-emitting material, a hole injection material, and a hole transport material, it can be used as an organic EL display device.

[0128] In the first embodiment of the display device of the present invention, it is preferred that, in a cross section cut vertically relative to the length direction of the partition wall and the surface of the substrate, the end of the functional layer is located on the side of the second partition wall. If the end of the functional layer is located on the side of the second partition wall, the end of the thicker functional layer does not emit light due to the first partition wall, and only the region of the functional layer with uniform film thickness can emit light. As a result, the problem of different brightness between the center and the end of the pixel can be eliminated.

[0129] The first embodiment of the organic EL display device of the present invention comprises at least one selected from the group consisting of an organic EL light-emitting material, a hole injection material, and a hole transport material in the functional layer of the above-mentioned display device. By comprising at least one selected from the group consisting of an organic EL light-emitting material, a hole injection material, and a hole transport material in the functional layer, an organic EL light-emitting layer can be formed.

[0130] The first mode of the organic EL display device of the present invention has a driving circuit, a planarization layer, a first electrode, a partition wall, an organic EL light-emitting layer and a second electrode on a substrate, and the partition wall is formed by the first mode of the cured film of the present invention. Taking an active matrix display device as an example, a TFT and wiring located on the side of the TFT and connected to the TFT are provided on a substrate such as glass or a resin film, and a planarization layer is provided in a manner covering the concavoconvexity thereon, and a display element is further provided on the planarization layer. The display element and the wiring are connected via a contact hole formed in the planarization layer.

[0131] By using the first embodiment of the cured film of the present invention for partition walls, the film has liquid repellency, and the discharge liquid used in the inkjet method is prevented from penetrating into adjacent pixels, thereby providing an organic EL display device with less display failure and excellent durability.

[0132] Next, a first embodiment of the method for manufacturing a substrate with partition walls of the present invention and a first embodiment of the method for manufacturing a display device of the present invention will be described.

[0133] A first aspect of the method for producing a substrate with partition walls of the present invention includes the following steps (1) to (4) in order.

[0134] Step (1), coating the first embodiment of the photosensitive resin composition of the present invention on a substrate having a first electrode to form a photosensitive resin film;

[0135] Step (2), exposing the photosensitive resin film;

[0136] Step (3), developing the exposed photosensitive resin film;

[0137] In step (4), the developed photosensitive resin film is subjected to a heat treatment to form a partition wall.

[0138] First, the step (1) of applying a photosensitive resin composition on a substrate having a first electrode to form a photosensitive resin film will be described.

[0139] As a method for coating the photosensitive resin composition on the substrate having the first electrode, spin coating, slit coating, dip coating, spray coating, printing and the like can be cited. Before coating, the substrate to be coated with the photosensitive resin composition can be pre-treated with the above-mentioned adhesion improver. For example, the following method can be cited: using a solution in which 0.5 to 20% by mass of the adhesion improver is dissolved in a solvent such as isopropanol, ethanol, methanol, water, tetrahydrofuran, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, diethyl adipate, etc., to treat the surface of the substrate. As a method for treating the surface of the substrate, spin coating, slit die coating, rod coating, dip coating, spray coating, steam treatment and the like can be cited.

[0140] Next, for example, the applied photosensitive resin film is subjected to reduced pressure drying treatment as necessary, and then heat-treated at 50° C. to 180° C. for 1 minute to several hours using a hot plate, an oven, infrared rays, etc., to obtain a dried photosensitive resin film.

[0141] Next, the step (2), that is, exposing the photosensitive resin film, will be described.

[0142] On the photosensitive resin film, chemical rays are irradiated through a photomask having a desired pattern. As chemical rays used in exposure, there are ultraviolet rays, visible rays, electron rays, X-rays, etc. In the present invention, it is preferred to use i-line (365nm), h-line (405nm), and g-line (436nm) of a mercury lamp. After irradiation with chemical rays, post-exposure baking can be performed. By performing post-exposure baking, effects such as improved resolution after development or expanded allowable range of development conditions can be expected. Post-exposure baking can use an oven, a hot plate, infrared rays, a flash annealing device, or a laser annealing device. The post-exposure baking temperature is preferably 50 to 180°C, and more preferably 60 to 150°C. The post-exposure baking time is preferably 10 seconds to several hours. When the post-exposure baking time is within the above range, there is a case where the reaction proceeds well and the development time can be shortened.

[0143] In the present invention, through "half exposure", the following step difference shape can be easily formed: it is a step difference shape having a first partition wall portion with a trapezoidal cross-section, and a second partition wall portion located on the upper part of the first partition wall portion and with a trapezoidal cross-section. In the surface cut in the direction perpendicular to the substrate, when the width of the upper surface of the first partition wall portion is set to A and the width of the bottom surface of the second partition wall portion is set to B, the relationship A>B is satisfied.

[0144] “Half exposure” refers to a process in which the base of the photosensitive resin film in the exposed portion remains to a certain extent when development is completed. In other words, it refers to a process in which the first partition wall portion of the photosensitive resin film is exposed so as not to be photosensitive.

[0145] Next, the step (3), that is, developing the exposed photosensitive resin film, will be described.

[0146] In the developing step of developing the exposed photosensitive resin film, the exposed photosensitive resin film is developed using a developer to remove the portion other than the exposed portion. The developer is preferably an aqueous solution of an alkaline compound such as tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and hexamethylenediamine. In addition, depending on the situation, the following can be added to these alkaline aqueous solutions alone or in combination: polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, γ-butyrolactone, dimethylacrylamide, etc., alcohols such as methanol, ethanol, isopropanol, etc., esters such as ethyl lactate, propylene glycol monomethyl ether acetate, cyclopentanone, cyclohexanone, isobutyl ketone, methyl isobutyl ketone, etc. Ketones, etc., etc. As the developing method, spraying, puddle, dipping, ultrasonic waves, etc. can be used.

[0147] Next, the pattern formed by development is preferably rinsed with distilled water. Here, alcohols such as ethanol and isopropyl alcohol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, etc. may be added to distilled water for rinsing.

[0148] Next, the step (4) of forming the partition wall by heat-treating the developed photosensitive resin film will be described.

[0149] A cured film is obtained by a process of heat-treating the developed photosensitive resin film. In the present invention, the cured film of the photosensitive resin composition can be suitably used for the partition of an organic EL display device. By heat treatment, residual solvents and components with low heat resistance can be removed, so that heat resistance and chemical resistance can be improved. In addition, when a thermal crosslinking agent (D) is contained, a thermal crosslinking reaction can be carried out by heat treatment, which can improve heat resistance and chemical resistance. For the heat treatment, a temperature is selected and the temperature is raised in stages, or a certain temperature range is selected and the temperature is continuously raised for 5 minutes to 5 hours. As an example, a method of heat treatment at 150°C and 250°C for 30 minutes each can be cited. Alternatively, a method of linearly raising the temperature from room temperature to 300°C over 2 hours can be cited. As the heat treatment conditions in the present invention, it is preferably above 180°C, more preferably above 200°C, further preferably above 230°C, and particularly preferably above 250°C. The heat treatment conditions are preferably 400° C. or lower, more preferably 350° C. or lower, and even more preferably 300° C. or lower.

[0150] A first aspect of the method for manufacturing a display device of the present invention includes the following steps (5) to (6) in order.

[0151] Step (5) of forming a functional layer by inkjet coating a functional ink in a region surrounded by a partition wall in a substrate having a partition wall comprising a cured product of the first embodiment of the photosensitive resin composition of the present invention;

[0152] Step (6), forming a second electrode on the functional layer.

[0153] First, step (5) of forming a functional layer by inkjet coating a functional ink in a region surrounded by a partition wall in a substrate having a partition wall including a cured product of the first embodiment of the photosensitive resin composition of the present invention will be described.

[0154] In the area (pixel) surrounded by the grid-shaped partition walls formed on the substrate, the functional ink is applied by inkjet to form a functional layer. For example, in the case of an organic EL display device, a composition comprising at least one selected from the group consisting of an organic EL luminescent material, a hole injection material, and a hole transport material can be dropped into the pixel as a functional ink and dried to form an organic EL luminescent layer. It is preferred to use a hot plate or an oven for drying at 150°C to 250°C for 0.5 to 120 minutes.

[0155] Next, step (6), that is, forming a second electrode on the functional layer, will be described.

[0156] The second electrode is formed so as to cover the entire partition wall and the functional layer. Examples of the method for forming the second electrode include sputtering and vapor deposition. It should be noted that it is preferred that the second electrode be formed with a uniform layer thickness without disconnection.

[0157] The first aspect of the method for manufacturing a display device of the present invention preferably includes the following steps (1) to (6) in order.

[0158] Step (1), coating the first embodiment of the photosensitive resin composition of the present invention on a substrate having a first electrode to form a photosensitive resin film;

[0159] Step (2), exposing the photosensitive resin film;

[0160] Step (3), developing the exposed photosensitive resin film;

[0161] Step (4), forming partition walls by heating the developed photosensitive resin film;

[0162] Step (5), forming a functional layer by applying a functional ink by inkjet in the area surrounded by the partition wall;

[0163] Step (6), forming a second electrode on the functional layer.

[0164] The second embodiment of the photosensitive resin composition of the present invention comprises: a compound (AI) having at least a structural unit represented by the general formula (1) and the general formula (2) (hereinafter, sometimes referred to as compound (AI)); and an alkali-soluble resin (BI) selected from polyimide, polybenzoxazole, polyamide-imide, a precursor of any of them, and a copolymer thereof. In this specification, the photosensitive resin composition in the second embodiment of the photosensitive resin composition of the present invention is sometimes referred to as photosensitive resin composition (I).

[0165] [Chemical formula 16]

[0166]

[0167] In the general formula (1), R 1 , R 2 and R 3 The monovalent organic groups representing hydrogen atoms or carbon 1 to 4 atoms may be the same or different.

[0168] [Chemical formula 17]

[0169]

[0170] In the general formula (2), R 4 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 5 represents an aliphatic group having 1 to 6 carbon atoms, R 6 It represents a perfluoroalkyl group having 3 to 6 carbon atoms.

[0171] The compound (AI) is a compound obtained by copolymerizing at least a (meth)acrylamide monomer represented by the general formula (3) and a (meth)acrylate monomer having a perfluoro group represented by the general formula (4), and is a liquid repellent material that is compatible with the photosensitive resin composition (I) and is added to impart liquid repellency to the surface of the cured film.

[0172] [Chemical formula 18]

[0173]

[0174] In the general formula (3), R 1 , R 2 and R 3 The monovalent organic groups representing hydrogen atoms or carbon 1 to 4 atoms may be the same or different.

[0175] [Chemical formula 19]

[0176]

[0177] In the general formula (4), R 4 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 5 represents an aliphatic group having 1 to 6 carbon atoms, R 6 It represents a perfluoroalkyl group having 3 to 6 carbon atoms.

[0178] Preferred examples of the (meth)acrylamide monomer represented by the general formula (3) include N,N-dimethylacrylamide and N,N-diethylacrylamide. Preferred examples of the (meth)acrylate monomer having a perfluoro group represented by the general formula (4) include 2-(perfluorobutyl)ethyl (meth)acrylate and 2-(perfluorohexyl)ethyl (meth)acrylate.

[0179] Compound (AI) has a structural unit represented by the general formula (1) obtained by copolymerizing the (meth)acrylamide monomer represented by the general formula (3). The structural unit represented by the general formula (1) has the effect of improving compatibility with the alkali-soluble resin (B) described later, reducing defects such as shrinkage, and improving the uniformity of the film thickness of the cured film, and as a result, the display defects of the organic EL display device are reduced. From the perspective of reducing the display defects of the organic EL display device, the structural unit represented by the general formula (1) is preferably 35 mol% or more of the structural unit constituting the compound (AI), and further preferably 40 mol% or more and the molar ratio of the largest number of the multiple structural units constituting the compound (AI). In addition, in order to impart liquid repellency, it is preferably 85 mol% or less, and more preferably 70 mol% or less.

[0180] For the purpose of further improving the durability of the light-emitting element by condensation polymerization with the alkali-soluble resin (B) when forming a cured film of the photosensitive resin composition (I), the compound (AI) preferably has a structural unit represented by the general formula (5), and is more preferably a copolymer formed by copolymerization with an epoxy group-containing (meth)acrylate monomer represented by the general formula (6).

[0181] [Chemical formula 20]

[0182]

[0183] [Chemical formula 21]

[0184]

[0185] In the general formulas (5) and (6), R 7 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 8It represents a monovalent organic group having 2 to 16 carbon atoms and having an epoxy group.

[0186] Preferred examples of the epoxy group-containing (meth)acrylate monomer represented by the general formula (6) include glycidyl acrylate, glycidyl methacrylate, 4-hydroxybutyl acrylate glycidyl ether (4-HBAGE), and an acrylate monomer having an alicyclic epoxy group.

[0187] In addition, if the structural unit represented by the general formula (5) is in an equimolar or higher molar ratio with the structural unit represented by the general formula (2), it undergoes condensation polymerization with the alkali-soluble resin (B) when forming a cured film of the photosensitive resin composition (I) to form a cured film with high heat resistance. The heat resistance of the cured film of the photosensitive resin composition (I) is improved, and the durability of the organic EL display device is improved, which is further preferred.

[0188] For the purpose of obtaining a balance between liquid repellency and solubility, compound (AI) may be a copolymer further copolymerized with a (meth)acrylic monomer substituted with a different functional group. For example, hydroxyl-containing (meth)acrylates, hydroxyl-containing (meth)acrylamides, alkoxy-containing (meth)acrylates, blocked isocyanate-containing (meth)acrylates, phenoxy-containing (meth)acrylates, (meth)acrylic acid alkyl esters, and vinyl-containing compounds may be cited.

[0189] Examples of the (meth)acrylates containing a hydroxyl group include 2-hydroxyethyl (meth)acrylate and the like.

[0190] Examples of the (meth)acrylamides containing a hydroxyl group include N-hydroxymethacrylamide and the like.

[0191] As (meth)acrylates which have an alkoxy group, 3-methacryloxypropylmethyldimethoxysilane etc. are mentioned, for example.

[0192] Examples of the blocked isocyanate group-containing (meth)acrylates include 2-(0-[1′-methylpropyleneamino]carboxyamino)ethyl methacrylate (Karenz MOI-BM: manufactured by Showa Denko K.K.; registered trademark).

[0193] Examples of the phenoxy group-containing (meth)acrylates include 2-phenoxybenzyl acrylate and 3-phenoxybenzyl acrylate.

[0194] The alkyl (meth)acrylates include diluent monomers such as unsubstituted or substituted alkyl (meth)acrylates, such as alkyl acrylates, which have a linear, branched and / or cyclic alkyl group having 1 to 12 carbon atoms and which is unsubstituted or substituted with at least one of an amino group, a monoalkylamino group, a dialkylamino group, a hydrocarbon aromatic ring, and a heterocyclic ring, or to which a hydroxyl group can be cleaved and added with an acid anhydride, and the like.

[0195] Examples of the vinyl group-containing compounds include n-butyl vinyl ether and the like.

[0196] The copolymer of compound (AI) can be obtained by ionic polymerization such as free radical polymerization and anionic polymerization, and can be obtained by known polymerization methods. In addition, it can be any of random copolymers, block copolymers, graft copolymers, or alternating copolymers. Here, a free radical polymerization method is cited as an example. For example, compound (AI) can be obtained by the following method: a specified amount of dimethyl (meth) acrylamide, a specified amount of fluorine-containing (meth) acrylate monomer, and a specified amount of epoxy-containing (meth) acrylates, hydroxyl-containing (meth) acrylates, hydroxyl-containing (meth) acrylamides, alkoxy-containing (meth) acrylates, blocked isocyanate-containing (meth) acrylates, phenoxy-containing (meth) acrylates, (meth) alkyl esters, and vinyl-containing compounds are randomly copolymerized in a suitable solvent in the presence of a free radical polymerization initiator and a chain transfer agent added as needed. As a free radical polymerization initiator, for example, tert-butyl peroxy 2-ethylhexanoate can be used, and as a chain transfer agent, for example, dodecyl mercaptan can be used. In addition, as the solvent, for example, an inert solvent such as cyclohexanone can be used.

[0197] The weight average molecular weight of the compound (AI) is preferably in the range of 1,500 to 50,000. A molecular weight in this range is preferred because the compound (AI) can be easily dissolved in a solvent used for the photosensitive resin composition (I) and the defoaming property of the photosensitive resin composition solution is high.

[0198] From the viewpoint that the obtained cured film fully exhibits lyophobicity, the compound (AI) in the present invention is preferably 0.1 mass parts or more relative to 100 mass parts of alkali-soluble resins (B) selected from polyimide, polybenzoxazole or polyamide-imide described later, the precursor of any of them and their copolymers, in addition, it is further preferred when it is 0.3 mass parts or more. In addition, from the viewpoint of not causing lyophobicity to be generated in the pixel and obtaining high durability, it is preferably 10 mass parts or less, and more preferably 5 mass parts or less. It should be noted that, with respect to the appropriate addition amount of compound (AI), the contact angle when propylene glycol monomethyl ether acetate is dripped on the cured film surface of the photosensitive resin composition (I) can be used to judge, according to JIS-R3258, the contact angle when measured by the sessile drop method is preferably 40 ° or more.

[0199] The photosensitive resin composition (I) has an alkali-soluble resin (BI) selected from polyimide, polybenzoxazole, polyamide-imide, a precursor of any of them, and a copolymer thereof (hereinafter, sometimes referred to as (BI) component). In addition, it may contain two or more selected from polyimide, polybenzoxazole, polyamide-imide, and a precursor of any of them, and may also contain a copolymer having the above two or more repeating units.

[0200] The alkali solubility in the second embodiment of the photosensitive resin composition of the present invention means that a solution prepared by dissolving a resin in γ-butyrolactone is applied on a silicon wafer, pre-baked at 120° C. for 4 minutes to form a pre-baked film having a film thickness of 10 μm±0.5 μm, the pre-baked film is immersed in a 2.38 mass % tetramethylammonium hydroxide aqueous solution at 23±1° C. for 1 minute, and then rinsed with pure water, and the dissolution rate obtained based on the reduction in film thickness at this time is 50 nm / minute or more.

[0201] Polyimide can be obtained by reacting tetracarboxylic acid or tetracarboxylic dianhydride, tetracarboxylic diester dichloride, etc. with diamine or diisocyanate compound, trimethylsilylated diamine, etc. Polyimide has a tetracarboxylic acid residue and a diamine residue. In addition, polyimide can also be obtained, for example, by the following method: using heat treatment, dehydration and ring closure of polyamic acid, which is one of the polyimide precursors, obtained by reacting tetracarboxylic dianhydride with diamine. During the heat treatment, a solvent that azeotropes with water, such as m-xylene, can also be added. Alternatively, a dehydration condensation agent such as carboxylic anhydride, dicyclohexylcarbodiimide, a base such as triethylamine, etc. can also be added as a ring closure catalyst, and dehydration and ring closure can be obtained by chemical heat treatment. Alternatively, it can also be obtained by adding a weakly acidic carboxylic acid compound and dehydration and ring closure at a low temperature below 100°C by heat treatment.

[0202] Polybenzoxazole can be obtained, for example, by reacting a bisaminophenol compound with a dicarboxylic acid or dicarboxylic acid chloride, a dicarboxylic acid active ester, etc. Polybenzoxazole has a dicarboxylic acid residue and a bisaminophenol residue. In addition, polybenzoxazole can also be obtained, for example, by the following method: utilizing heat treatment to dehydrate and ring-close the polyhydroxyamide obtained as one of the polybenzoxazole precursors by reacting the bisaminophenol compound with the dicarboxylic acid. Alternatively, it can also be obtained by adding phosphoric anhydride, alkali, carbodiimide compounds, etc., utilizing chemical treatment to dehydrate and ring-close the polyhydroxyamide.

[0203] As polyimide precursors, polyamic acid, polyamic acid ester, polyamide amide, polyisoimide, etc. can be cited. For example, polyamic acid can be obtained by reacting tetracarboxylic acid or tetracarboxylic dianhydride, tetracarboxylic acid diester dichloride, etc. with diamine or diisocyanate compound, trimethylsilylated diamine. Polyimide can be obtained, for example, by the following method: dehydration and ring closure of the polyamic acid obtained by the above method by heating or chemical treatment such as acid and alkali.

[0204] As the polybenzoxazole precursor, polyhydroxyamide and the like can be cited. For example, polyhydroxyamide can be obtained by reacting bisaminophenol with dicarboxylic acid or dicarboxylic acid chloride, dicarboxylic acid active ester, etc. Polybenzoxazole can be obtained, for example, by dehydrating and ring-closing the polyhydroxyamide obtained by the above method by heating or chemical treatment with phosphoric anhydride, alkali, carbodiimide compounds, etc.

[0205] The polyamideimide precursor can be obtained, for example, by reacting tricarboxylic acid, the corresponding tricarboxylic anhydride, tricarboxylic anhydride halide, etc. with diamine or diisocyanate. Polyamideimide can be obtained, for example, by dehydrating and ring-closing the precursor obtained by the above method by heating or chemical treatment with acid, alkali, etc.

[0206] As the copolymer of polyimide, polybenzoxazole, polyamide-imide, it can be any or a combination of block copolymerization, random copolymerization, alternating copolymerization, graft copolymerization. For example, a block copolymer can be obtained by reacting tetracarboxylic acid, corresponding tetracarboxylic dianhydride, tetracarboxylic acid diester dichloride, etc. with polyhydroxyamide. In addition, dehydration and ring closure can also be performed by heating or chemical treatment such as acid and alkali.

[0207] The component (BI) preferably has a structural unit represented by any one of the general formulae (7) to (10), and more preferably has a structural unit represented by (10). Two or more resins having these structural units may be contained, or two or more structural units may be copolymerized. The resin of the component (BI) preferably contains 3 to 1000 structural units represented by any one of the general formulae (7) to (10) in the molecule, and more preferably contains 20 to 200 structural units.

[0208] [Chemical formula 22]

[0209]

[0210] In the general formulas (7) to (10), R 9 and R 12 Represents a 4-valent organic group, R 10 , R 11 and R 14 Represents a divalent organic group, R 13 Represents a trivalent organic group, R 15 Represents a 2- to 4-valent organic group, R 16 represents a 2- to 12-valent organic group. 17 represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms. p represents an integer of 0 to 2, q represents an integer of 0 to 10. n represents an integer of 0 to 2.

[0211] Preferred R 9 ~R 16 All of them have an aromatic ring and / or an aliphatic ring.

[0212] In the general formulas (7) to (10), R 9 represents a tetracarboxylic acid derivative residue, R 11 represents a dicarboxylic acid derivative residue, R 13 represents a tricarboxylic acid derivative residue, R 15 represents a di-, tri- or tetra-carboxylic acid derivative residue. 9 , R 11 , R 13 , R 15 (COOR 17 ) n (OH) pExamples of the acid component include terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, bis(carboxyphenyl)hexafluoropropane, biphenyl dicarboxylic acid, benzophenone dicarboxylic acid, and triphenyl dicarboxylic acid. Examples of tricarboxylic acids include trimellitic acid, trimesic acid, diphenyl ether tricarboxylic acid, and biphenyl trimaric acid. Examples of tetracarboxylic acids include pyromellitic acid, 3,3',4,4'-biphenyl tetracarboxylic acid, 2,3,3',4'-biphenyl tetracarboxylic acid, 2,2',3,3'-biphenyl tetracarboxylic acid, 3,3',4,4'-benzophenone tetracarboxylic acid, 2,2',3,3'-benzophenone tetracarboxylic acid, 2,2-bis(3, 4-dicarboxyphenyl)hexafluoropropane, 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(3,4-dicarboxyphenyl)methane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)ether, aromatic tetracarboxylic acids such as 1,2,5,6-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, and 3,4,9,10-perylenetetracarboxylic acid, and aliphatic tetracarboxylic acids such as butanetetracarboxylic acid and 1,2,3,4-cyclopentanetetracarboxylic acid. Among these, in the general formula (10), one or two carboxyl groups of each of the tricarboxylic acid and the tetracarboxylic acid correspond to COOR 15 These acid components can be used directly or in the form of anhydrides, active esters, etc. In addition, two or more acid components among these can also be used in combination.

[0213] In the general formulas (7) to (10), R 10 , R 12 , R 14 and R 16 represents a diamine derivative residue. 10 , R 12 , R 14 , R 16Examples of the diamine component of (OH)q include bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)methylene, bis(3-amino-4-hydroxyphenyl)ether, bis(3-amino-4-hydroxy)biphenyl, bis(3-amino-4-hydroxyphenyl)fluorene and other hydroxyl group-containing diamines, 3-sulfonic acid-4,4'-diaminodiphenyl ether Diamines containing sulfonic acid, diamines containing thiol groups such as dithiophenylene diamine, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylene diamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxyphenyl)sulfone, bis(3-aminophenoxyphenyl)sulfone, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-di Aromatic diamines such as ethyl-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, compounds obtained by replacing a part of the hydrogen atoms of these aromatic rings with an alkyl group having 1 to 10 carbon atoms, a fluoroalkyl group, a halogen atom, etc., alicyclic diamines such as cyclohexanediamine and methylenebiscyclohexylamine, etc. These diamines can be used directly or in the form of corresponding diisocyanate compounds or trimethylsilylated diamines. In addition, two or more diamine components among these can be used in combination. In applications requiring heat resistance, it is preferred to use aromatic diamines in an amount of 50 mol% or more of the total diamine.

[0214] R in the general formulas (7) to (10) 9 ~R 16 The skeleton may contain a phenolic hydroxyl group, a sulfonic acid group, a thiol group, etc. By using a resin having an appropriate amount of a phenolic hydroxyl group, a sulfonic acid group, or a thiol group, a positive photosensitive resin composition having an appropriate alkali solubility is obtained.

[0215] In addition, it is preferred that the structural unit of the (BI) component contains fluorine atoms. The fluorine atoms impart hydrophobicity to the surface of the film during alkali development, which can inhibit penetration from the surface. In order to fully obtain the effect of preventing penetration from the interface, the fluorine atom content in the (BI) component is preferably 10% by mass or more, and in terms of solubility in alkaline aqueous solutions, it is preferably 20% by mass or less.

[0216] In addition, in order to improve the storage stability of the resin composition, the resin of the (BI) component preferably uses a known monoamine, anhydride, monocarboxylic acid, monoacyl chloride compound, monoactive ester compound and other end-capping agents to end-cap the main chain. The introduction ratio of the monoamine used as an end-capping agent is preferably 0.1 mol% or more relative to the total amine components, and is particularly preferably 5 mol% or more, preferably 60 mol% or less, and particularly preferably 50 mol% or less. The introduction ratio of the anhydride, monocarboxylic acid, monoacyl chloride compound or monoactive ester compound used as an end-capping agent is preferably 0.1 mol% or more relative to the diamine component, and is particularly preferably 5 mol% or more, preferably 100 mol% or less, and particularly preferably 90 mol% or less. By reacting multiple end-capping agents, multiple different terminal groups can be introduced.

[0217] In the resin having a structural unit represented by any one of the general formulae (7) to (9), the number of repetitions of the structural unit is preferably 3 to 200. In addition, in the resin having a structural unit represented by the general formula (10), the number of repetitions of the structural unit is preferably 10 to 1000. Within this range, a thick film can be easily formed.

[0218] The (BI) component may be composed of only the structural unit represented by any one of the general formulae (7) to (10), or may be a copolymer or a mixture with other structural units. In this case, the structural unit represented by any one of the general formulae (7) to (10) is preferably contained in an amount of 10% by mass or more of the total resin, more preferably 30% by mass or more. The type and amount of the structural unit used in the copolymerization or mixing can be selected within the range that does not impair the mechanical properties of the film obtained by the final heat treatment.

[0219] The photosensitive resin composition (I) preferably also contains at least one of phenolic resin and polyhydroxystyrene resin (CI) (hereinafter, sometimes referred to as (CI) component.). These resins have the function of a compatibilizer. By mixing them, the compatibility of the compound (AI) and the (BI) component is further improved, which helps to stabilize the solubility of each component in the developer and improve the straightness of the pattern. As a result, it is expected to reduce the poor display of the organic EL display device. In addition, when the photosensitive agent (EI) described later is a positive type, by containing the (CI) component, the film loss amount of the developing process can be reduced, so that the compound (AI) has the effect of staying on the film surface after development, and the process margin for obtaining good liquid repellency can be improved.

[0220] The phenolic resin includes Novolac phenolic resin and Resol phenolic resin, which can be obtained by polycondensing various phenols alone or a mixture of multiple phenols using aldehydes such as formalin by a known method.

[0221] Examples of the phenols constituting the Novolac phenolic resin and the Resol phenolic resin include phenol, p-cresol, m-cresol, o-cresol, 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,3,4-trimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, 2,4,5-trimethylphenol, methylenediamine, 1,2-dimethylphenol ... bisphenol, methylenebis-p-cresol, resorcinol, catechol, 2-methylresorcinol, 4-methylresorcinol, o-chlorophenol, m-chlorophenol, p-chlorophenol, 2,3-dichlorophenol, m-methoxyphenol, p-methoxyphenol, p-butoxyphenol, o-ethylphenol, m-ethylphenol, p-ethylphenol, 2,3-diethylphenol, 2,5-diethylphenol, p-isopropylphenol, α-naphthol, β-naphthol, etc., which can be used alone or as a mixture of a plurality of them. In addition, as aldehydes, in addition to formalin, paraformaldehyde, acetaldehyde, benzaldehyde, hydroxybenzaldehyde, chloroacetaldehyde, etc. can also be mentioned, which can be used alone or as a mixture of a plurality of them.

[0222] As the polyhydroxystyrene resin, a homopolymer of vinylphenol or a copolymer with styrene may be used.

[0223] The preferred weight average molecular weight of the phenol resin and the polyhydroxystyrene resin is 2,000 to 20,000, preferably 3,000 to 10,000, in terms of polystyrene based on GPC (gel permeation chromatography). Within this range, a resin composition having a high concentration and a low viscosity can be obtained.

[0224] From the viewpoint of improving the compatibility of the compound (AI) and the component (BI) so as to improve the straightness of the pattern and reduce the display failure of the organic EL display device, the total content of the phenolic resin and the polyhydroxystyrene resin in the photosensitive resin composition (I) is preferably 20 parts by mass or more, and more preferably 30 parts by mass or more, relative to 100 parts by mass of the component (BI). In addition, in order not to reduce the durability of the cured film of the photosensitive resin composition, it is preferably 50 parts by mass or less, and more preferably 40 parts by mass or less.

[0225] The photosensitive resin composition (I) preferably further contains a thermal crosslinking agent (DI) for the purpose of easily obtaining a cured film.

[0226] The so-called thermal crosslinking agent refers to a compound having at least two thermally reactive functional groups represented by hydroxymethyl, alkoxymethyl, epoxy, and oxetanyl in the molecule. The (DI) thermal crosslinking agent crosslinks the (BI) component or other added components to improve the durability of the cured film.

[0227] Preferred examples of the compound having at least two alkoxymethyl groups or hydroxymethyl groups include DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DML-MBPC, DML-MTrisPC, DML-BisOC-Z, DML-BisOCHP-Z, DML-BPC, DML-BisOC-P, DMOM-PC, DMOM-PTBP, DMOM -MBPC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TML-BPA, TML-BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP (these are trade names, manufactured by Honshu Chemical Industry Co., Ltd.), NIKALAC (registered trademark) MX-290, NIKALAC MX-280, NIKALAC MX-270, NIKALACMX-279, NIKALAC MW-100LM, NIKALAC MX-750LM (these are trade names, manufactured by Sanwa Chemical Co., Ltd.), each of which can be obtained from the above-mentioned companies.

[0228] Regarding the compound having an epoxy group or an oxetane group, examples of the compound having two epoxy groups in one molecule include "Epikote" (registered trademark) 807, "Epikote" 828, "Epikote" 1002, "Epikote" 1750, "Epikote" 1007, YX8100-BH30, E1256, E4250, and E4275 (the above are trade names, Japan Epoxy Co., Ltd.), "Epiclon" (registered trademark) EXA-4880, "Epiclon" EXA-4822, "Epiclon" EXA-9583, HP4032 (the above are trade names, manufactured by Dainippon Ink & Chemicals Co., Ltd.), "EPOLIGHT" (registered trademark) 40E, "EPOLIGHT" 100E, "EPOLIGHT" 200E, "EPOLIGHT" 400E, "EPOLIGHT" 70P, "EPOLIGHT" 200P, " "EPOLIGHT" 400P, "EPOLIGHT" 1500NP, "EPOLIGHT" 80MF, "EPOLIGHT" 4000, "EPOLIGHT" 3002 (these are trade names, manufactured by Kyoeisha Chemical Co., Ltd.), "Denacol" (registered trademark) EX-212L, "Denacol" EX-214L, "Denacol" EX-216L, "Denacol" EX-252, "Denacol" EX-850L (these are trade names, manufactured by Nagase ChemteX Co., Ltd.), GAN, GOT (these are trade names, manufactured by Nippon Kayaku Co., Ltd.), "Celloxide" (registered trademark) 2021P (trade name, manufactured by Daicel Co., Ltd.), "RIKARESIN" (registered trademark) DME-100, "RIKARESIN" BEO-60E (these are trade names, manufactured by Shin Nippon Chemical Co., Ltd.), etc., each of which can be obtained from the respective companies.

[0229] Examples of compounds having three or more epoxy groups include VG3101L (trade name, manufactured by Printec Co., Ltd.), "TEPIC" (registered trademark) S, "TEPIC" G, "TEPIC" P (these are trade names, manufactured by Nissan Chemical Industries, Ltd.), "Epiclon" N660, "Epiclon" N695, HP7200 (these are trade names, manufactured by Dainippon Ink and Chemicals Co., Ltd.), "Denacol" EX-321L (trade name, manufactured by Nagase ChemteX Co., Ltd.), NC6000, EPPN502H, NC3000 (the above are trade names, manufactured by Nippon Kayaku Co., Ltd.), "Epotohto" (registered trademark) YH-434L (trade name, manufactured by Tohto Kasei Co., Ltd.), EHPE-3150 (trade name, manufactured by Daicel Co., Ltd.), as compounds having two or more oxetane groups, OXT-121, OXT-221, OX-SQ-H, OXT-191, PNOX-1009, RSOX (the above are trade names, manufactured by Toagosei Co., Ltd.), "ETERNACOLL" (registered trademark) OXBP, "ETERNACOLL" OXTP (the above are trade names, manufactured by Ube Industries, Ltd.), etc., each of which can be obtained from each company.

[0230] As the (DI) thermal crosslinking agent, it is preferred to have a phenolic hydroxyl group in one molecule and a methylol and / or alkoxymethyl group at two adjacent positions of the phenolic hydroxyl group. By making the methylol and / or alkoxymethyl group adjacent to the phenolic hydroxyl group, the durability of the cured film can be further improved. As the alkoxymethyl group, for example, methoxymethyl, ethoxymethyl, propoxymethyl, butoxymethyl can be cited, but it is not limited to these.

[0231] The content of the (DI) thermal crosslinking agent is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and further preferably 15 parts by mass or more relative to 100 parts by mass of the (BI) alkali-soluble resin. In addition, it is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and further preferably 30 parts by mass or less. By making the content of the (DI) thermal crosslinking agent 5 parts by mass or more, the heat resistance of the cured film is improved, and by making it 50 parts by mass or less, the elongation of the cured film can be prevented from decreasing.

[0232] The photosensitive resin composition (I) preferably contains a photosensitizer (EI). The photosensitizer (EI) may be a negative type that is cured by light or a positive type that is solubilized by light, and may preferably contain (e-1) a polymerizable unsaturated compound and a photopolymerization initiator, or (e-2) a quinonediazide compound.

[0233] As the polymerizable unsaturated compound in (e-1), for example, known compounds such as compounds having unsaturated double bond functional groups such as vinyl, allyl, acryloyl, methacryloyl and / or unsaturated triple bond functional groups such as propargyl can be cited. Among them, from the perspective of polymerizability, conjugated vinyl, acryloyl, and methacryloyl are preferred. In addition, as the number of functional groups contained, from the perspective of stability, it is preferably 1 to 4, and each group may not be the same. In addition, the compound referred to herein is preferably a substance with a molecular weight of 30 to 800. When the molecular weight is within the range of 30 to 800, the compatibility with the polymer and the reactive diluent is good. Specific examples include 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, dihydroxymethyl-tricyclodecane diacrylate, isobornyl acrylate, isobornyl methacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, methylenebisacrylamide, N,N-dimethylacrylamide, Olefinamide, N-methylol acrylamide, 2,2,6,6-tetramethylpiperidinyl methacrylate, 2,2,6,6-tetramethylpiperidinyl acrylate, N-methyl-2,2,6,6-tetramethylpiperidinyl methacrylate, N-methyl-2,2,6,6-tetramethylpiperidinyl acrylate, ethylene oxide-modified bisphenol A diacrylate, ethylene oxide-modified bisphenol A dimethacrylate, N-vinyl pyrrolidone, N-vinyl caprolactam, etc. These can be used alone or in combination of two or more.

[0234] The photopolymerization initiator in (e-1) refers to a substance that mainly generates free radicals by irradiating light in the ultraviolet to visible light region to initiate polymerization. From the perspective of being able to use commonly used light sources and rapid curing properties, it is preferably selected from known photopolymerization initiators in acetophenone derivatives, benzophenone derivatives, benzoin ether derivatives, and xanthone derivatives. As examples of preferred photopolymerization initiators, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxy-cyclohexyl phenyl ketone, isobutylbenzoin ether, benzoin methyl ether, thioxanthone, isopropylthioxanthone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, etc. can be cited, but are not limited to these.

[0235] As the (e-2) quinonediazide compound, there can be mentioned known substances such as the product obtained by bonding the sulfonic acid of quinonediazide with a polyhydroxy compound by an ester bond, the product obtained by bonding the sulfonic acid of quinonediazide with a polyamino compound by a sulfonamide bond, and the product obtained by bonding the sulfonic acid of quinonediazide with a polyhydroxypolyamino compound by an ester bond and / or a sulfonamide bond. Not all functional groups in these polyhydroxy compounds, polyamino compounds, and polyhydroxypolyamino compounds may be substituted with quinonediazide, and preferably, an average of more than 40 mol% of all functional groups are substituted with quinonediazide. By using such a quinonediazide compound, a positive photosensitive resin composition that is sensitive to the i-line (wavelength 365nm), h-line (wavelength 405nm), and g-line (wavelength 436nm) of a mercury lamp, which are common ultraviolet rays, can be obtained.

[0236] The polyhydroxy compound includes Bis-Z, BisP-EZ, TekP-4HBPA, TrisP-HAP, TrisP-PA, TrisP-SA, TrisOCR-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, Methylenetris-FR-CR, BisRS-26X, DML-MBPC, DML-MBOC, DML-OCHP, DML-PCHP, DML-PC, DML-PTBP, DML-34X, DML-EP, DML-POP, Dimethylol-BisOC-P, DML-PFP, DML-PSBP, DML-MTrisPC, TriML-P, TriML -35XL, TML-BP, TML-HQ, TML-pp-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP (these are trade names, manufactured by Honshu Chemical Industry), BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-BIPC-F, TEP-BIP-A, 46DMOC, 46DMOEP, TM-BIP-A (these are trade names, manufactured by Asahi Organic Materials Industries), 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, naphthol, tetrahydroxybenzophenone, methyl gallate, bisphenol A, bisphenol E, methylene bisphenol, BisP-AP (trade name, manufactured by Honshu Chemical Industry), Novolac resin, etc., but are not limited to these.

[0237] Examples of the polyamino compound include 1,4-phenylenediamine, 1,3-phenylenediamine, 4,4′-diaminodiphenyl ether, 4,4′-diaminodiphenylmethane, 4,4′-diaminodiphenyl sulfone, and 4,4′-diaminodiphenyl sulfide, but are not limited thereto.

[0238] Moreover, as a polyhydroxypolyamino compound, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 3,3'-dihydroxybenzidine, etc. are mentioned, but it is not limited to these.

[0239] Among them, the (e-2) quinonediazide compound more preferably comprises an ester of a phenol compound and naphthoquinonediazide-5-sulfonyl group. Thus, high sensitivity and higher resolution can be obtained by i-line exposure.

[0240] The content of the quinonediazide compound (e-2) is preferably 1 to 50 parts by mass, more preferably 10 to 40 parts by mass, relative to 100 parts by mass of the resin of the component (BI). By setting the content of the quinonediazide compound within this range, higher sensitivity can be achieved, and photosensitivity can be obtained without impairing liquid repellency.

[0241] The photosensitive resin composition (I) may contain a colorant (FI). The colorant (FI) refers to a known organic pigment, inorganic pigment or dye commonly used in the field of electronic information materials. The colorant (FI) may preferably be an organic pigment and / or an inorganic pigment.

[0242] Examples of organic pigments include diketopyrrolopyrrole pigments, azo pigments such as azo, disazo or polyazo, phthalocyanine pigments such as copper phthalocyanine, halogenated copper phthalocyanine or non-metallic phthalocyanine, anthraquinone pigments such as aminoanthraquinone, diaminodianthraquinone, anthrapyrimidine, flavanthrone, anthraquinone, indanthrone, pyranthrone or anthrone violet, quinacridone pigments, bisoxizone pigments, pyrenone pigments, perylene pigments, thioindigo pigments, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, threne pigments, benzofuranone pigments or metal complex pigments.

[0243] Examples of the inorganic pigment include black iron oxide, cadmium red, red iron oxide, molybdenum red, molybdate orange, chrome vermilion, yellow lead, cadmium yellow, yellow iron oxide, titanium yellow, chromium oxide, chrome green, titanium cobalt green, cobalt green, cobalt chrome green, Victoria green, ultramarine, Prussian blue, cobalt blue, cerulean blue, cobalt silicon blue, cobalt zinc silicon blue, manganese violet, and cobalt violet.

[0244] Examples of the dye include azo dyes, anthraquinone dyes, condensed polycyclic aromatic carbonyl dyes, indigo dyes, carbocation dyes, phthalocyanine dyes, methine or polymethine dyes.

[0245] Examples of the red pigment include Pigment Red 9, 48, 97, 122, 123, 144, 149, 166, 168, 177, 179, 180, 192, 209, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240 and 254 (all numerical values ​​are color indexes (hereinafter referred to as "CI" numbers)).

[0246] Examples of the orange pigment include Pigment Orange 13, 36, 38, 43, 51, 55, 59, 61, 64, 65, and 71 (all numerical values ​​are CI numbers).

[0247] Examples of the yellow pigment include Pigment Yellow 12, 13, 17, 20, 24, 83, 86, 93, 95, 109, 110, 117, 125, 129, 137, 138, 139, 147, 148, 150, 153, 154, 166, 168, and 185 (all values ​​are CI numbers).

[0248] Examples of the violet pigment include Pigment Violet 19, 23, 29, 30, 32, 37, 40, and 50 (all numerical values ​​are CI numbers).

[0249] Examples of the blue pigment include Pigment Blue 15, 15:3, 15:4, 15:6, 22, 60, and 64 (all numerical values ​​are CI numbers).

[0250] Examples of green pigments include Pigment Green 7, 10, 36, and 58 (all numerical values ​​are CI numbers).

[0251] As black pigment, for example, black organic pigment and black inorganic pigment etc. can be mentioned. As black organic pigment, for example, carbon black, benzofuranone black pigment (International Publication No. 2010 / 081624 record), perylene black pigment, aniline black pigment or anthraquinone black pigment can be mentioned. Among them, from the aspect of obtaining a negative photosensitive resin composition with better sensitivity, benzofuranone black pigment or perylene black pigment are particularly preferred. The reason is that benzofuranone black pigment and perylene black pigment can achieve high light-shielding property with low transmittance in the visible light region, and the transmittance in the ultraviolet region is relatively high, so that the chemical reaction during exposure is carried out efficiently. It is also possible to contain benzofuranone black pigment and perylene black pigment at the same time. Examples of the black inorganic pigment include graphite, or fine particles, oxides, composite oxides, sulfides, nitrides, or oxynitrides of metals such as titanium, copper, iron, manganese, cobalt, chromium, nickel, zinc, calcium, or silver. Carbon black or titanium nitride having high light-shielding properties is preferred.

[0252] Examples of the dye include Sumilan, Lanyl (registered trademark) series (all manufactured by Sumitomo Chemical Co., Ltd.), Orasol (registered trademark), Oracet (registered trademark), Filamid (registered trademark), Irgasperse (registered trademark), ZapoN, NeozapoN, Neptune, and Acidol series (all manufactured by BASF Corporation), Kayaset (registered trademark), Kayakalan (registered trademark) series (all manufactured by Nippon Kayaku Co., Ltd.), Valifast (registered trademark) Colors series (manufactured by Orient Chemical Industry Co., Ltd.), Savinyl, Sandoplast, Polysynthren (registered trademark), and Lanasyn (registered trademark) series (all manufactured by Clariant Japan Co., Ltd.), Aizen (registered trademark), and Spilon (registered trademark) series (all manufactured by Hodogaya Chemical Industry Co., Ltd.), functional pigments (manufactured by Yamada Chemical Industry Co., Ltd.), and Plast Color and Oil Color series (manufactured by Arimoto Chemical Industry Co., Ltd.).

[0253] For the purpose of improving the contrast of the organic EL display device, the color of the colorant is preferably black that can shield visible light in the entire wavelength region, and at least one selected from organic pigments, inorganic pigments and dyes can be used, and a colorant that is black when made into a cured film can be used. Therefore, the above-mentioned black organic pigments and black inorganic pigments can be used, and blackening can also be simulated by mixing two or more organic pigments and dyes. When simulating blackening, it can be obtained by mixing two or more of the above-mentioned red, orange, yellow, purple, blue, green and other organic pigments and dyes. It should be noted that the photosensitive resin composition (I) itself does not necessarily need to be black, and a colorant that changes color during heat curing so that the cured film is black can be used.

[0254] Among these, from the viewpoint of ensuring high heat resistance, it is preferred to use a colorant that contains an organic pigment and / or an inorganic pigment and is black when formed into a cured film. In addition, from the viewpoint of ensuring high insulation, it is preferred to use a colorant that contains an organic pigment and / or a dye and is black when formed into a cured film. That is, from the viewpoint of being able to simultaneously achieve high heat resistance and high insulation, it is preferred to use a colorant that contains an organic pigment and is black when formed into a cured film.

[0255] The content of the colorant (FI) is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, further preferably 30 parts by mass or more, preferably 300 parts by mass or less, more preferably 200 parts by mass or less, further preferably 150 parts by mass or less, relative to 100 parts by mass of the component (BI). By making the content of the colorant 10 parts by mass or more, the colorability required for the cured film can be obtained, and by making it 300 parts by mass or less, the storage stability becomes good.

[0256] When a pigment is used as a colorant (FI), the photosensitive resin composition (I) preferably contains a dispersant. By containing a dispersant, the colorant can be uniformly and stably dispersed in the resin composition. The dispersant is not particularly limited, and a polymer dispersant is preferred. As a polymer dispersant, for example, a polyester polymer dispersant, an acrylic polymer dispersant, a polyurethane polymer dispersant, a polyallylamine polymer dispersant or a carbodiimide dispersant can be cited. More specifically, the so-called polymer dispersant refers to a polymer compound whose main chain is formed by polyamino, polyether, polyester, polyurethane, polyacrylate, etc., and has polar groups such as amines, carboxylic acids, phosphoric acid, amine salts, carboxylates, and phosphates at the side chains or the ends of the main chains. The polar group is adsorbed on the pigment and plays a role in stabilizing the dispersion of the pigment through the steric hindrance of the main chain polymer.

[0257] Dispersants are classified into (polymer) dispersants having only an amine value, (polymer) dispersants having only an acid value, (polymer) dispersants having both an amine value and an acid value, or (polymer) dispersants having neither an amine value nor an acid value. Preferred are (polymer) dispersants having both an amine value and an acid value, and (polymer) dispersants having only an amine value. More preferred are (polymer) dispersants having only an amine value.

[0258] Specific examples of polymer dispersants having only an amine value include DISPERBYK (registered trademark) 102, 160, 161, 162, 2163, 164, 2164, 166, 167, 168, 2000, 2050, 2150, 2155, 9075, 9077, BYK-LP N6919, BYK-LP N21116, and BYK-LP N21234 (all manufactured by BYK-Chemie), EFKA (registered trademark) 4015, 4020, 4046, 4047, 4050, 4055, 4060, 4080, 4300, 4330, 4340, 4400, 4401, 4402, 4403 or 4800 (all manufactured by BASF), Ajisper (registered trademark) PB711 (manufactured by Ajinomoto Fine-Techno Co., Inc.) or SOLSPERSE (registered trademark) 13240, 13940, 20000, 71000 or 76500 (all manufactured by Lubrizol).

[0259] In order to improve dispersion stability while maintaining heat resistance, the ratio of the dispersant to the colorant is preferably 1% by mass or more, more preferably 3% by mass or more, and is preferably 100% by mass or less, more preferably 50% by mass or less.

[0260] The photosensitive resin composition (I) preferably contains an organic solvent (GI). Examples of the organic solvent (GI) include ethers, acetates, esters, ketones, aromatic hydrocarbons, amides, and alcohols.

[0261] More specifically, for example, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, dipropylene glycol dimethyl ether, dipropylene glycol methyl-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, di ... Ethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether or tetrahydrofuran ethers, butyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, 3-methoxybutyl acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, cyclohexanol acetate, propylene glycol diacetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate (hereinafter referred to as "PGMEA"), dipropylene glycol methyl ether acetate, 3-methoxy-3-methyl-1-butyl acetate, 1,4-dimethoxy-3-methyl-1-butyl acetate, Acetic esters such as 1,3-butanediol diacetate, 1,6-hexanediol diacetate, etc., methyl ethyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, etc., alkyl lactates such as methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, etc., ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxylate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutyrate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, ethyl acetate , n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-amyl formate, isoamyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate or ethyl 2-oxobutyrate or other esters, toluene or xylene or other aromatic hydrocarbons, N-methylpyrrolidone, N,N-dimethylformamide or N,N-dimethylacetamide or other amides, or butanol, isobutanol, amyl alcohol, 4-methyl-2-pentanol, 3-methyl-2-butanol, 3-methyl-3-methoxybutanol or diacetone alcohol or other alcohols.

[0262] When a pigment is used as a colorant (FI), an acetate compound is preferably used as an organic solvent (GI) in order to stabilize the dispersion of the pigment. The proportion of the acetate compound in the total organic solvent (GI) contained in the photosensitive resin composition (I) is preferably 50% by mass or more, more preferably 70% by mass or more. In addition, it is preferably 100% by mass or less, more preferably 90% by mass or less.

[0263] The amount of the solvent used is not particularly limited because it varies depending on the desired film thickness and the coating method to be used, but is preferably 50 to 2000 parts by mass, particularly preferably 100 to 1500 parts by mass, based on 100 parts by mass of the resin of the component (BI).

[0264] The photosensitive resin composition (I) may contain surfactants, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, alcohols such as ethanol, ketones such as cyclohexanone and methyl isobutyl ketone, and ethers such as tetrahydrofuran and dioxane, if necessary, for the purpose of improving wettability with the substrate.

[0265] The photosensitive resin composition (I) may contain a close fit improver. As a close fit improver, silane coupling agents such as vinyl trimethoxy silane, vinyl triethoxy silane, epoxy cyclohexyl ethyl trimethoxy silane, 3-glycidoxy propyl trimethoxy silane, 3-glycidoxy propyl triethoxy silane, p-phenyl trimethoxy silane, 3-aminopropyl trimethoxy silane, 3-aminopropyl triethoxy silane, N-phenyl-3-aminopropyl trimethoxy silane, titanium chelate, aluminum chelate, and compounds obtained by reacting aromatic amine compounds with alkoxy-containing silicon compounds, etc., may be cited. Two or more of them may be contained. By containing these close fit improvers, when developing the photosensitive resin film, the close fit with base substrates such as silicon wafer, ITO, SiO2, silicon nitride, etc. may be improved. In addition, the tolerance to oxygen plasma and UV ozone treatment used in washing, etc. may be improved. The content of the adhesion improver is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, based on 100 parts by mass of the component (BI).

[0266] For the purpose of improving wettability with the substrate, the photosensitive resin composition (I) may contain a surfactant as needed. The surfactant may be a commercially available compound, and specifically, as a silicone surfactant, SH series, SD series, ST series of Toray Dow Corning Silicone, BYK series of BYK-Chemie Japan, KP series of Shin-Etsu Silicone, TSF series of Toshiba Silicone, etc. may be cited, as a fluorine-based surfactant, "Megafac (registered trademark)" series of Dainippon Ink Industries, FLUORAD series of Sumitomo 3M, "SURFLON (registered trademark)" series of Asahi Glass, "AsahiGuard (registered trademark)" series of Shin-Akita Chemical, EF series of Omnova Solution, PolyFox series of Omnova Solution, etc. may be cited, as a surfactant containing an acrylic acid and / or methacrylic acid polymer, Polyflow series of Kyoeisha Chemical, "DISPARLON (registered trademark)" series of Kusumoto Chemical, etc. may be cited, but it is not limited to these.

[0267] The content of the surfactant is preferably 0.001 parts by mass or more, more preferably 0.002 parts by mass or more, and preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, based on 100 parts by mass of the component (BI).

[0268] Next, the method for producing the photosensitive resin composition (I) is described. For example, by dissolving the above-mentioned components (AI) to (EI) in an organic solvent (GI), a photosensitive resin composition (I) can be obtained. As a dissolving method, stirring and heating can be mentioned. In the case of heating, the heating temperature is preferably set within a range that does not damage the performance of the resin composition, usually room temperature to 80°C. In addition, the dissolution order of each component is not particularly limited, for example, there is a method of dissolving in order from compounds with low solubility.

[0269] The obtained photosensitive resin composition (I) is preferably filtered using a filter to remove dust and particles. The filter pore size is, for example, 0.5 μm, 0.2 μm, 0.1 μm, 0.05 μm, etc., but is not limited to these. The filter material includes polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc., and polyethylene and nylon are preferably used for filtering.

[0270] Next, the method for producing a cured film using the photosensitive resin composition (I) will be described in detail.

[0271] The method for producing a cured film comprises the following steps in sequence:

[0272] Step (1), coating the photosensitive resin composition (I) on a substrate to form a photosensitive resin film;

[0273] A pre-baking step (2) to dry the photosensitive resin film;

[0274] An exposure step (3) of irradiating the dried photosensitive resin film with chemical radiation through a photomask;

[0275] A developing step (4) of developing the exposed photosensitive resin film; and

[0276] In step (5), the developed photosensitive resin film is heated to form a cured film.

[0277] In the process of forming a photosensitive resin film, the photosensitive resin composition (I) is applied by spin coating, slit coating, dip coating, spray coating, printing, etc. to obtain a photosensitive resin film of the photosensitive resin composition (I). Before coating, the substrate to which the photosensitive resin composition (I) is applied may be pre-treated with the above-mentioned adhesion improver. For example, the following method may be cited: using a solution in which 0.5 to 20% by mass of the adhesion improver is dissolved in a solvent such as isopropanol, ethanol, methanol, water, tetrahydrofuran, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, diethyl adipate, etc., to treat the surface of the substrate. As a method for treating the surface of the substrate, methods such as spin coating, slit die coating, rod coating, dip coating, spray coating, and steam treatment may be cited.

[0278] In the pre-baking step of drying the photosensitive resin film, the coated photosensitive resin film is subjected to reduced pressure drying treatment as needed, and then heat-treated at 50° C. to 180° C. for 1 minute to several hours using a hot plate, an oven, infrared rays, etc., to obtain a dried photosensitive resin film.

[0279] Next, the process of exposing the dried photosensitive resin film through a photomask is described. On the photosensitive resin film, chemical rays are irradiated through a photomask having a desired pattern. As chemical rays used in exposure, there are ultraviolet rays, visible rays, electron rays, X-rays, etc. In the present invention, it is preferred to use i-line (365nm), h-line (405nm), and g-line (436nm) of a mercury lamp. After irradiation with chemical rays, post-exposure baking can be performed. By performing post-exposure baking, effects such as improved resolution after development or a wider allowable range of development conditions can be expected. Post-exposure baking can use an oven, a hot plate, infrared rays, a flash annealing device, or a laser annealing device. As the post-exposure baking temperature, 50 to 180°C is preferred, and 60 to 150°C is more preferred. The post-exposure baking time is preferably 10 seconds to several hours. When the post-exposure baking time is within the above range, the reaction proceeds well, and there is a case where the development time can be shortened.

[0280] In the developing process of developing the exposed photosensitive resin film, the exposed photosensitive resin film is developed using a developer to remove the portion other than the exposed portion. As the developer, aqueous solutions of alkaline compounds such as tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and hexamethylenediamine are preferred. In addition, depending on the circumstances, the following can be added to these alkaline aqueous solutions alone or in combination: polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, γ-butyrolactone, dimethylacrylamide, alcohols such as methanol, ethanol, and isopropanol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, and methyl isobutyl ketone, etc. The developing method may be spraying, puddle, dipping, ultrasonic wave or the like.

[0281] Next, the pattern formed by development is preferably rinsed with distilled water. Here, alcohols such as ethanol and isopropyl alcohol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, etc. may be added to distilled water for rinsing.

[0282] Next, a cured film is obtained by subjecting the developed photosensitive resin film to a heat treatment process. By heat treatment, residual solvents and components with low heat resistance can be removed, thereby improving heat resistance and chemical resistance. In addition, when a thermal crosslinking agent (DI) is contained, a thermal crosslinking reaction can be performed by heat treatment, which can improve heat resistance and chemical resistance. For the heat treatment, a temperature is selected and the temperature is raised in stages, or a certain temperature range is selected and the temperature is continuously raised for 5 minutes to 5 hours. As an example, heat treatment at 150°C and 250°C for 30 minutes each can be cited. Alternatively, a method of linearly heating from room temperature to 300°C over 2 hours can be cited. As the heat treatment conditions in the present invention, it is preferably above 180°C, more preferably above 200°C, more preferably above 230°C, and particularly preferably above 250°C. In addition, the heat treatment conditions are preferably below 400°C, more preferably below 350°C, and more preferably below 300°C.

[0283] Next, a method for producing a cured film using a photosensitive sheet formed from the photosensitive resin composition (I) is described. Note that the photosensitive sheet herein is defined as a sheet obtained by coating the photosensitive resin composition (I) on a releasable substrate and drying it.

[0284] When a photosensitive sheet formed of the photosensitive resin composition (I) is used, if a protective film is present on the photosensitive sheet, it is peeled off, and the photosensitive sheet and the substrate are placed opposite to each other and bonded by thermal compression to obtain a photosensitive resin film. The photosensitive sheet can be obtained by coating the photosensitive resin composition (I) on a support film made of polyethylene terephthalate or the like as a removable substrate and drying it.

[0285] Thermocompression bonding can be performed by heat pressing, heat lamination, heat vacuum lamination, etc. From the perspective of adhesion and embedding properties with the substrate, the lamination temperature is preferably 40° C. or higher. In addition, when the photosensitive sheet is photosensitivity, the lamination temperature is preferably 140° C. or lower in order to prevent the photosensitive sheet from being cured during lamination and the resolution of pattern formation in the exposure and development process from being reduced.

[0286] The photosensitive resin film obtained by laminating a photosensitive sheet to a substrate can be formed into a cured film by the following steps: exposing the photosensitive resin film; developing the exposed photosensitive resin film; and curing by heating.

[0287] The cured film (hereinafter, sometimes referred to as the second embodiment of the cured film of the present invention) formed by curing the photosensitive resin composition (I) or the photosensitive sheet can be used for electronic components such as organic EL display devices, semiconductor devices, and multilayer wiring boards. Specifically, it is preferably used for the insulating layer of an organic EL element, the planarization layer of a substrate with a drive circuit of a display device using an organic EL element, the interlayer insulating film between the rewiring of a semiconductor device or a semiconductor component, the passivation film of a semiconductor, the protective film of a semiconductor element, the interlayer insulating film of a multilayer wiring for high-density mounting, the wiring protection insulating layer of a circuit substrate, the on-chip microlens of a solid-state imaging element, and the planarization layer for various displays and solid-state imaging elements. As an electronic device having a surface protective film, an interlayer insulating film, etc. configured with the second embodiment of the cured film of the present invention, for example, an MRAM with low heat resistance can be cited. That is, the second embodiment of the cured film of the present invention is suitable for use as a surface protective film of an MRAM. In addition, it can be used as an insulating layer of a display device (specifically, for example, LCD, ECD, ELD, organic EL, etc.) including a first electrode formed on a substrate and a second electrode disposed opposite to the first electrode.

[0288] The organic EL display device having a cured film of the photosensitive resin composition (I) has a driving circuit, a planarization layer, a first electrode, an insulating layer, a light-emitting layer, and a second electrode on a substrate, wherein the insulating layer is formed by the second embodiment of the cured film of the present invention. Taking an active matrix display device as an example, a TFT and wiring located on the side of the TFT and connected to the TFT are provided on a substrate such as glass or a resin film, and a planarization layer is provided in a manner covering the concavoconvexity thereon, and a display element is further provided on the planarization layer. The display element and the wiring are connected via contact holes formed in the planarization layer.

[0289] The organic EL display device having a cured film of the photosensitive resin composition (I) is preferably used in the case of using the following manufacturing method, that is, forming at least a portion of the pixel surrounded by the cured film by an inkjet method. By using a cured film formed by curing the photosensitive resin composition (I) or the photosensitive resin sheet, it has liquid repellency, and the discharge liquid used in the inkjet method is prevented from penetrating into adjacent pixels, thereby obtaining an organic EL display device with less display failure and excellent durability.

[0290] Example

[0291] Hereinafter, the present invention will be described with reference to Examples, but the present invention is not limited to these Examples. First, the measurement method and the evaluation method will be described.

[0292] (1) Average molecular weight determination

[0293] The molecular weights of (a1) to (a8) and (c1) to (c2) used in the examples were measured using a GPC (gel permeation chromatography) apparatus Waters 2690-996 (manufactured by Waters Corporation, Japan) with tetrahydrofuran (hereinafter referred to as THF) as the eluting solvent, and the weight average molecular weight (Mw) was calculated in terms of polystyrene.

[0294] The molecular weights of (b1) to (b4) used in the examples were measured using the above-mentioned GPC apparatus with N-methyl-2-pyrrolidone (hereinafter referred to as NMP) as an eluting solvent, and the number average molecular weight (Mn) was calculated in terms of polystyrene.

[0295] (2) Film thickness measurement

[0296] The film thickness after prebaking, development and curing was measured using a surface roughness and profile measuring machine (SURFCOM1400D; Tokyo Seimitsu Co., Ltd.) at a measurement magnification of 10,000 times, a measurement length of 1.0 mm and a measurement speed of 0.30 mm / s.

[0297] (3) Evaluation of contact angle

[0298] In the measurement of the contact angle, 1 μL of propylene glycol monomethyl ether acetate (hereinafter referred to as PGMEA) was dropped onto the partition pattern formed on the substrate by the method described below, and the contact angle was measured. The measurement was performed using a contact angle measuring apparatus DMs-401 (manufactured by Kyowa Interface Science Co., Ltd.) and a sessile drop method was used at 23° C. in accordance with JIS-R3257.

[0299] The results of the measurement of the PGMEA contact angle on the cured film were judged as follows, and the contact angle was 60° or more (A+), the contact angle was 50° or more and less than 60° (A), and the contact angle was 40° or more and less than 50° (B) as excellent, the contact angle was 30° or more and less than 40° (C) as good, and the contact angle was less than 30° (D) as poor.

[0300] A+: contact angle is 60° or more

[0301] A: The contact angle is 50° or more and less than 60°

[0302] B: The contact angle is 40° or more and less than 50°

[0303] C: The contact angle is 30° or more and less than 40°

[0304] D: The contact angle is less than 30°.

[0305] (4) Evaluation of ink wettability at the opening

[0306] Using a substrate formed with a partition wall pattern 5 described later, as a hole injection layer, an inkjet device (Litlex142 manufactured by ULVAC) was used to drop an ink of a compound (HT-1) using methyl benzoate as a solvent into the area surrounded by the partition wall, and the number of ink droplets required for coating the entire opening at this time was counted. The volume of each drop of ink used in this evaluation was 15 pl.

[0307] (5) Evaluation of the incidence rate of adverse reactions

[0308] At 10mA / cm 2 The organic EL display device produced by the method described later is driven by DC to emit light under conditions, and the display defects such as whether there are non-luminous areas in the center of the pixel are observed. The display defect incidence rate is calculated based on the number of normally luminous organic EL display devices among 20 organic EL display devices.

[0309] The judgment is made in the following manner: the case where the defect incidence rate is greater than 30% and less than 40% (C) is qualified, the case where the defect incidence rate is greater than 20% and less than 30% (B) is good, and the case where the defect incidence rate is less than 20% (A and A+) is excellent.

[0310] A+: The defect rate is 0% or more and less than 10%

[0311] A: Display defect rate is more than 10% and less than 20%

[0312] B: Display defect rate is 20% or more and less than 30%

[0313] C: Display defect rate is 30% or more and less than 40%

[0314] D: Display defect rate is 40% or more and less than 70%

[0315] E: Display defect rate is 70% or more and less than 100%

[0316] (6) Evaluation of durability

[0317] The organic EL display device prepared by the method described below was kept at 80°C for 100 hours and then 2 Under the conditions of , it is driven by DC to make it emit light, and the display defects such as non-luminous area in the center of the pixel are observed. The display defect incidence rate is calculated in the same way as above to determine the durability.

[0318] A+: The defect rate is 0% or more and less than 10%

[0319] A: Display defect rate is more than 10% and less than 20%

[0320] B: Display defect rate is 20% or more and less than 30%

[0321] C: Display defect rate is 30% or more and less than 40%

[0322] D: Display defect rate is 40% or more and less than 70%

[0323] E: Display defect rate is 70% or more and less than 100%

[0324] The compounds used in Examples and Comparative Examples are shown below.

[0325] Synthesis Example 1 Synthesis of Compound (AI) and Liquid-Repellent Material (A)

[0326] In a 1000mL reaction vessel equipped with a stirring device, a reflux condenser, a dropping funnel, a thermometer and a nitrogen blowing port, 100 parts by mass of cyclohexanone were added, and the temperature was raised to 110°C under a nitrogen atmosphere. The temperature of cyclohexanone was maintained at 110°C, and the monomer mixed solution shown in Table 1 was dripped at a constant rate of 2 hours using a dropping funnel to prepare each monomer solution. After the dropwise addition was completed, the monomer solution was heated to 115°C and reacted for 2 hours to obtain copolymers (a1) to (a9). GPC was used to determine the weight average molecular weight. The results are shown in Table 1.

[0327] The abbreviations in Table 1 are shown below.

[0328] DMAA: N,N-dimethylacrylamide

[0329] FAMAC-6: 2-(Perfluorohexyl)ethyl methacrylate

[0330] GMA: Glycidyl Methacrylate

[0331] Karenz MOI-BM: 2-(0-[1'-methylpropyleneamino]carboxyamino)ethyl methacrylate

[0332] [Table 1]

[0333]

[0334] Synthesis Example 2 Synthesis of a hydroxyl-containing diamine compound

[0335] 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (hereinafter referred to as BAHF) was dissolved in 100 mL of acetone and 17.4 g (0.3 mol) of propylene oxide, and the mixture was cooled to -15°C. A solution of 20.4 g (0.11 mol) of 3-nitrobenzoyl chloride dissolved in 100 mL of acetone was added dropwise thereto. After the addition was completed, the mixture was reacted at -15°C for 4 hours, and then returned to room temperature. The precipitated white solid was filtered and vacuum dried at 50°C.

[0336] 30 g of the solid was added to a 300 mL stainless steel autoclave, dispersed in 250 mL of methyl cellosolve, and 2 g of 5% palladium-carbon was added. Hydrogen was introduced into the mixture using a balloon, and the reduction reaction was carried out at room temperature. After about 2 hours, it was confirmed that the balloon no longer softened, and the reaction was terminated. After the reaction was completed, the palladium compound used as a catalyst was removed by filtration, and concentrated using a rotary evaporator to obtain a hydroxyl-containing diamine compound represented by the following formula.

[0337] [Chemical formula 23]

[0338]

[0339] Synthesis Example 3 Synthesis of alkali-soluble resin (b1)

[0340] Under a dry nitrogen stream, 62.0 g (0.20 mole) of 3,3',4,4'-diphenylether tetracarboxylic dianhydride (hereinafter referred to as ODPA) was dissolved in 500 g of N-methyl-2-pyrrolidone (hereinafter referred to as NMP). 96.7 g (0.16 mole) of the hydroxyl-containing diamine compound obtained in Synthesis Example 2 was added together with 100 g of NMP, and reacted at 20°C for 1 hour, and then at 50°C for 2 hours. Next, 8.7 g (0.08 mole) of 3-aminophenol as a capping agent was added together with 50 g of NMP, and reacted at 50°C for 2 hours. Then, 47.7 g (0.40 mole) of N,N-dimethylformamide dimethyl acetal was added. After the addition, it was stirred at 50°C for 3 hours. After the stirring was completed, the solution was cooled to room temperature, and then the solution was added to 5 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and then dried in a vacuum dryer at 80° C. for 24 hours to obtain the target polyimide precursor (b1). The number average molecular weight of the polyimide precursor (b1) was 11,000.

[0341] Synthesis Example 4 Synthesis of Alkali-Soluble Resin (b2)

[0342] Under a dry nitrogen stream, BAHF58.6g (0.16 mol) and 3-aminophenol 8.7g (0.08 mol) as a capping agent were dissolved in N-methyl-2-pyrrolidone (NMP) 300g. ODPA 62.0g (0.20 mol) was added together with 100g NMP, stirred at 20°C for 1 hour, and then stirred at 50°C for 4 hours. Then, 15g of xylene was added, and water and xylene were azeotroped together while stirring at 150°C for 5 hours. After stirring, the solution was put into 5L of water and a white precipitate was collected. The precipitate was collected by filtration, washed three times with water, and dried in a vacuum dryer at 80°C for 24 hours to obtain the target polyimide (b2). The number average molecular weight of polyimide (b2) is 8200.

[0343] Synthesis Example 5 Synthesis of Alkali-Soluble Resin (b3)

[0344] Under a dry nitrogen stream, 0.16 mol of a mixture of dicarboxylic acid derivatives obtained by reacting 41.3 g (0.16 mol) of diphenyl ether-4,4'-dicarboxylic acid with 43.2 g (0.32 mol) of 1-hydroxy-1,2,3-benzotriazole and 73.3 g (0.20 mol) of BAHF were dissolved in 570 g of NMP, and then reacted at 75°C for 12 hours. Next, 13.1 g (0.08 mol) of 5-norbornene-2,3-dicarboxylic anhydride dissolved in 70 g of NMP was added, and the mixture was further stirred for 12 hours to terminate the reaction. After filtering the reaction mixture, the reaction mixture was put into a solution of water / methanol = 3 / 1 (volume ratio) to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and then dried in a vacuum dryer at 80°C for 24 hours to obtain the target polybenzoxazole (PBO) precursor (b3). The number average molecular weight of the PBO precursor (b3) was 8,500.

[0345] Synthesis Example 6 Synthesis of Alkali-Soluble Resin (b4)

[0346] A methyl methacrylate / methacrylic acid / styrene copolymer (mass ratio 30 / 40 / 30) was synthesized by a known method (Japanese Patent No. 3120476, Example 1). 40 parts by mass of glycidyl methacrylate was added to 100 parts by mass of the copolymer, and the mixture was reprecipitated with purified water, filtered, and dried to obtain an acrylic resin (b4) as a polymer containing a radical polymerizable monomer having a number average molecular weight of 10,000 and an acid value of 110 (mgKOH / g).

[0347] Synthesis Example 7 Synthesis of phenolic resin (c1)

[0348] Under a dry nitrogen stream, 108.0 g (1.00 mol) of m-cresol, 75.5 g (0.93 mol of formaldehyde) of 37% by mass aqueous solution, 0.63 g (0.005 mol) of oxalic acid dihydrate, and 264 g of methyl isobutyl ketone were added, and then immersed in an oil bath, and the reaction solution was refluxed while polycondensation reaction was carried out for 4 hours. Then, the temperature of the oil bath was increased over 3 hours, and then the pressure in the flask was reduced to 4.0 kPa to 6.7 kPa, and the volatile components were removed. The dissolved resin was cooled to room temperature to obtain Novolac type phenolic resin (c1). From GPC, it was found that the weight average molecular weight was 3,500.

[0349] Synthesis Example 8 Synthesis of Quinonediazide Compound (e2)

[0350] Under a dry nitrogen stream, 21.22 g (0.05 mol) of TrisP-PA (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) and 36.27 g (0.135 mol) of naphthoquinone diazide 5-sulfonyl chloride were dissolved in 450 g of 1,4-dioxane and the mixture was brought to room temperature. 15.18 g of triethylamine mixed with 50 g of 1,4-dioxane was added dropwise so that the temperature in the system did not exceed 35°C. After the addition, the mixture was stirred at 30°C for 2 hours. The triethylamine salt was filtered and the filtrate was put into water. The precipitate was then collected by filtration. The precipitate was dried using a vacuum dryer to obtain a quinone diazide compound (e2) represented by the following formula.

[0351] [Chemical formula 24]

[0352]

[0353] The abbreviations of the components used in the examples are shown below.

[0354] <(A) Liquid-repellent material>

[0355] "Megafac (registered trademark)" RS-72-K (a liquid-repellent material containing a polymer of the following chemical formula as a compound having a carbamate group and a structure represented by the general formula (13), manufactured by DIC Corporation)

[0356] [Chemical formula 25]

[0357]

[0358] <(DI) and (D) thermal crosslinking agent>

[0359] HMOM-TPHAP (a compound represented by the following chemical formula having a phenolic hydroxyl group and substituents having a molecular weight of 40 or more at both ortho positions of the phenolic hydroxyl group, manufactured by Honshu Chemical Industry Co., Ltd.)

[0360] [Chemical formula 26]

[0361]

[0362] VG3101L: "Techmore" (registered trademark) VG3101L (a compound represented by the following chemical formula, manufactured by Printec Co., Ltd.).

[0363] [Chemical formula 27]

[0364]

[0365] <Solvents>

[0366] PGMEA: Propylene glycol monomethyl ether acetate

[0367] PGME: Propylene glycol monomethyl ether

[0368] GBL: gamma-butyrolactone.

[0369] Examples 1 to 27, Comparative Examples 1 to 7

[0370] Figure 2 A schematic diagram of the substrate used in the evaluation is shown. First, on a 38×46 mm alkali-free glass plate 1, a 10 nm ITO transparent conductive film is formed on the entire surface of the alkali-free glass plate by sputtering to form a first electrode 2, and then etched. In addition, in order to take out the second electrode, an auxiliary electrode 3 is also formed at the same time. The obtained substrate is ultrasonically cleaned for 10 minutes using "Semico Clean" (registered trademark) 56 (manufactured by Furuuchi Chemical Co., Ltd.), then washed with ultrapure water, and dried to form a substrate.

[0371] Next, under a yellow light, the components were mixed at the mixing ratios shown in Tables 2 and 3, and stirred sufficiently at room temperature to dissolve. The resulting solution was then filtered with a filter having a pore size of 1 μm to obtain photosensitive resin compositions W1 to W34. The obtained photosensitive resin composition was applied on the substrate by spin coating, pre-baked on a heating plate at 120°C for 4 minutes to form a dry coating film, and then patterned exposure was performed through a photomask having a specified pattern. Then, development was performed with a 2.38% TMAH aqueous solution for 60 seconds or 120 seconds to dissolve unnecessary parts, and then rinsed with pure water to produce: an object having a partition wall pattern 4 formed on the substrate, wherein the partition wall pattern 4 has an opening with a width of 70 μm and a length of 260 μm arranged in the center; and, similarly, an object having a partition wall pattern 5 formed on the substrate, wherein the partition wall pattern 5 has openings with a width of 70 μm and a length of 260 μm arranged at intervals of 155 μm in the width direction and at intervals of 465 μm in the length direction, and each opening is shaped to expose the first electrode.

[0372] Next, the substrate having the partition wall pattern 4 and the partition wall pattern 5 with an opening at the center was heated in a nitrogen atmosphere at 250° C. for 1 hour to solidify the substrate, and the substrate having the partition wall pattern 4 with an opening at the center was used to evaluate the contact angle (3). The results are shown in Tables 4 and 5.

[0373] Next, the substrate was developed with a 2.38% TMAH aqueous solution for 60 seconds, and as a hole injection layer, an inkjet device (Litlex142 manufactured by ULVAC) was used to drip the ink of the compound (HT-1) with methyl benzoate as a solvent into the area surrounded by the partition walls, and the ink wettability of the opening (4) was evaluated. Then, the film was fired at 200°C to form a hole injection layer. Next, as a hole transport layer, an inkjet device was used to drip the compound (HT-2) with 4-methoxytoluene as a solvent into the area surrounded by the partition walls, and then fired at 190°C to form a hole transport layer. Furthermore, as a light-emitting layer, an inkjet device was used to drip a mixture of the compound (GH-1) and the compound (GD-1) with 4-methoxytoluene as a solvent into the area surrounded by the partition walls, and then fired at 130°C to form a light-emitting layer. Then, as an electron transport material, the compound (ET-1) and the compound (LiQ) were sequentially stacked at a volume ratio of 1:1 by vacuum evaporation to form an organic EL layer 6. Next, after evaporating 2 nm of the compound (LiQ), Mg and Ag were evaporated at a volume ratio of 10:1 for 10 nm to form a second electrode 7. Finally, a cover glass plate was bonded using an epoxy resin adhesive in a low-humidity nitrogen atmosphere to seal the substrate, thereby manufacturing four 5 mm square light-emitting devices on one substrate.

[0374] [Chemical formula 28]

[0375]

[0376] At 10mA / cm 2 The organic EL display device prepared by the above method was driven by direct current to emit light, and (5) the occurrence rate of display failure was evaluated. Then, the device was kept at 80°C for 100 hours and then again at 10 mA / cm 2 Under the conditions of , it was made to emit light by direct current drive, and (6) durability evaluation was carried out to confirm whether there was any change in the luminescence characteristics. The results are shown in Tables 4 and 5.

[0377] Thus, it was confirmed that the organic EL light-emitting element had little occurrence of display failure, could maintain its performance as a light-emitting element even after the durability test under accelerated conditions, and had high durability.

[0378] [Table 2]

[0379] [Table 2]

[0380]

[0381] [Table 3]

[0382] [Table 3]

[0383]

[0384] [Table 4]

[0385] [Table 4]

[0386]

[0387] [Table 5]

[0388] [Table 5]

[0389]

[0390] Embodiments 28 to 34

[0391] Figure 2 A schematic diagram of the substrate used in the evaluation is shown. First, on a 38×46 mm alkali-free glass plate 1, a 10 nm ITO transparent conductive film is formed on the entire surface of the alkali-free glass plate by sputtering to form a first electrode 2, and then etched. In addition, in order to take out the second electrode, an auxiliary electrode 3 is also formed at the same time. The obtained substrate is ultrasonically cleaned for 10 minutes using "Semico Clean" (registered trademark) 56 (manufactured by Furuuchi Chemical Co., Ltd.), then washed with ultrapure water, and dried to form a substrate.

[0392] Next, a photosensitive resin composition W21 is applied to the substrate by spin coating, and pre-baked on a heating plate at 120°C for 4 minutes to form a dry coating. Then, patterned exposure is performed through a photomask having a specified pattern. At this time, exposure is performed by "half exposure" in a manner to form the following step difference shape: the step difference shape is a step difference shape having a first partition wall portion (whose cross section is a trapezoid) and a second partition wall portion (which is located on the upper part of the first partition wall portion and has a trapezoidal cross section), and in the surface cut in a direction perpendicular to the substrate, when the width of the upper surface of the first partition wall portion is set to A and the width of the bottom surface of the second partition wall portion is set to B, the relationship A>B is satisfied.

[0393] Next, the substrate was developed with a 2.38% TMAH aqueous solution for 60 seconds to dissolve the unnecessary part, and then rinsed with pure water to prepare two partition walls having the following partition wall pattern 5 formed on the substrate, wherein the partition wall pattern 5 was provided with openings of 70 μm in width and 260 μm in length at a pitch of 155 μm in the width direction and at a pitch of 465 μm in the length direction, and each opening was in a shape that exposed the first electrode. The film thickness of the prepared partition wall is shown in Table 6.

[0394] Next, using the substrate with the partition wall pattern 5 formed thereon, as a hole injection layer, an inkjet device (Litlex142 manufactured by ULVAC) was used to drop an ink of the compound (HT-1) using methyl benzoate as a solvent into the area surrounded by the partition walls. At this time, it was confirmed whether the ink leaked out of the opening and evaluated as follows.

[0395] A: No ink leakage

[0396] B: Ink leaks

[0397] Next, the hole injection layer was formed by firing at 200° C. Then, the cross section of the opening was observed by SEM using the first substrate to confirm the position of the end of the hole injection layer. Evaluation was performed as follows.

[0398] A: The end portion of the hole injection layer is located on the side surface of the second partition wall portion.

[0399] B: The end portion of the hole injection layer is located on the side surface of the first partition wall portion.

[0400] Next, on another substrate, as a hole transport layer, a compound (HT-2) with 4-methoxytoluene as a solvent was dropped into the area surrounded by the partition wall using an inkjet device, and then fired at 190°C to form a hole transport layer. Furthermore, as a light-emitting layer, a mixture of a compound (GH-1) and a compound (GD-1) with 4-methoxytoluene as a solvent was dropped into the area surrounded by the partition wall using an inkjet device, and then fired at 130°C to form a light-emitting layer. Then, as an electron transport material, a compound (ET-1) and a compound (LiQ) were stacked in a volume ratio of 1:1 by vacuum evaporation to form an organic EL layer 6. Next, a 2nm compound (LiQ) was vapor-deposited, and then Mg and Ag were vapor-deposited at a volume ratio of 10:1 for 10nm to form a second electrode 7. Finally, a cover glass plate was bonded with an epoxy resin adhesive in a low-humidity nitrogen atmosphere to seal the substrate, thereby manufacturing four 5 mm square light-emitting devices on one substrate.

[0401] At 10mA / cm 2 Under the conditions of , the organic EL display device produced by the above method is driven by DC to emit light, and the center and periphery of the pixel are compared to observe whether there is uneven brightness within the pixel and evaluate it.

[0402] A: There is no display defect when comparing the center and periphery of the pixel.

[0403] B: There is display failure when comparing the center and the periphery of the pixel.

[0404] [Table 6]

[0405] [Table 6]

[0406]

[0407] Description of Reference Numerals

[0408] 1 Alkali-free glass plate

[0409] 2. First electrode

[0410] 3 Auxiliary electrode

[0411] 4 The partition pattern with an opening in the center

[0412] 5 Next door pattern

[0413] 6 Organic EL layer

[0414] 7 Second electrode

[0415] 8 substrate

[0416] 9 First adjacent part

[0417] 10 Second adjacent part

[0418] 11 Functional layer

[0419] 12 Functional layer end

Claims

1. A photosensitive resin composition comprising a lyophobic material (A) having at least an amide group or a urethane group, an alkali-soluble resin (B), at least one resin (C) selected from the group consisting of a phenolic resin and a polyhydroxystyrene resin, and a photosensitizer (E), The alkali-soluble resin (B) comprises at least one alkali-soluble resin selected from the group consisting of polyimide, polybenzoxazole, polyamide-imide, precursors thereof, and copolymers thereof, and The lyophobic material (A) having at least an amide group or a carbamate group comprises a compound having a structural unit represented by the following general formula (2) or a structure represented by the following general formula (13); In the general formula (2), R 4 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 5 represents an aliphatic group having 1 to 6 carbon atoms, R 6 represents a perfluoroalkyl group having 3 to 6 carbon atoms; In the general formula (13), X is selected from the following structural formulas (a) to (e), all Xs may have the same structure, or may have multiple structures that exist randomly or in blocks; m is an integer of 1 to 100 indicating the number of repeating units; 2. The photosensitive resin composition according to claim 1, wherein The liquid-repellent material (A) having at least an amide group or a carbamate group comprises a compound having a structural unit represented by the following general formula (1) or the following general formula (11), In the general formula (1), R 1 , R 2 and R 3 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, each of which may be the same or different; In the general formula (11), R 18 represents a hydrogen atom or a monovalent organic group having 1 to 4 carbon atoms, R 19 represents an aliphatic group having 1 to 6 carbon atoms; A represents a carbamate group represented by the following formula (A-1) or (A-2); 3. The photosensitive resin composition according to claim 2, wherein The liquid-repellent material (A) having at least an amide group or a urethane group includes a compound having a structural unit represented by the general formula (11) and a structure represented by the general formula (13).

4. The photosensitive resin composition according to claim 2 or 3, wherein In the lyophobic material (A) having at least an amide group or a urethane group, the total amount of the structural units represented by the general formula (1) or (11) is in the range of 15 to 85 mol % of all the structural units constituting the lyophobic material (A).

5. The photosensitive resin composition according to any one of claims 1 to 3, wherein The liquid-repellent material (A) having at least an amide group or a urethane group further has an epoxy group.

6. The photosensitive resin composition according to any one of claims 1 to 3, wherein The content of the liquid-repellent material (A) having at least an amide group or a urethane group is 0.1 to 10 parts by mass based on 100 parts by mass of the alkali-soluble resin (B).

7. The photosensitive resin composition according to any one of claims 1 to 3, wherein The total amount of at least one resin (C) selected from the group consisting of phenolic resins and polyhydroxystyrene resins is 10 to 100 parts by mass based on 100 parts by mass of the alkali-soluble resin (B). 8 . The photosensitive resin composition according to claim 1 , further comprising a thermal crosslinking agent (D). 9 . The photosensitive resin composition according to claim 1 , further comprising a colorant (F). 10 . A cured film formed from a cured product of the photosensitive resin composition according to claim 1 . 11 . A display device comprising lattice-shaped partition walls formed on a substrate, wherein the partition walls comprise the cured film according to claim 10 .

12. The display device according to claim 11, wherein: The lattice-shaped partition wall formed on the substrate is a step-difference shape having a first partition wall portion and a second partition wall portion, wherein the first partition wall portion is a partition wall portion having a trapezoidal cross section and is cut vertically relative to the length direction of the partition wall and the surface of the substrate, and the second partition wall portion is a partition wall portion located above the first partition wall portion and having a trapezoidal cross section, In the cross section, when the width of the upper surface of the first partition wall portion is represented by A and the width of the bottom surface of the second partition wall portion is represented by B, a relationship of A>B is satisfied.

13. The display device according to claim 12, wherein: The film thickness of the partition wall is 0.5 to 5.0 μm, and the film thickness of the first partition wall portion is 0.1 to 1.0 μm.

14. The display device according to claim 12 or 13, wherein: The first partition wall portion and the second partition wall portion are formed of a cured film of the same material. 15 . A display device, wherein a functional layer is formed in a region surrounded by the partition wall of the display device according to claim 11 . 16 . A display device according to claim 12 , wherein a functional layer is formed in a region surrounded by the partition wall.

17. The display device according to claim 16, wherein: In a cross section cut perpendicularly to the longitudinal direction of the partition wall and the surface of the substrate, an end portion of the functional layer is located on a side surface of the second partition wall portion.

18. An organic EL display device, wherein the functional layer of the display device according to any one of claims 15 to 17 contains at least one selected from the group consisting of an organic EL light-emitting material, a hole injection material, and a hole transport material.

19. A method for producing a substrate with partition walls, comprising the following steps (1) to (4) in sequence: Step (1), coating the photosensitive resin composition according to any one of claims 1 to 9 on a substrate having a first electrode to form a photosensitive resin film; Step (2), exposing the photosensitive resin film; Step (3), developing the exposed photosensitive resin film; In step (4), the developed photosensitive resin film is subjected to a heat treatment to form a partition wall.

20. A method for manufacturing a display device, comprising the following steps (5) to (6) in sequence: Step (5), in the substrate with partition walls, in the region surrounded by the partition walls, coating the functional ink by inkjet to form a functional layer, The substrate with partition walls has partition walls comprising a cured product of the photosensitive resin composition according to any one of claims 1 to 9; Step (6), forming a second electrode on the functional layer.