Preparation method of polyvinylpyrrolidone coated magnetic ferrite adsorbent and application of polyvinylpyrrolidone coated magnetic ferrite adsorbent in uranium-containing wastewater

Through the dual function of polyvinylpyrrolidone coating magnetic ferrite adsorbent, the problems of low adsorption capacity and difficult treatment when treating uranium-containing wastewater are solved, and efficient and environmentally friendly uranium removal and regeneration are achieved. Suitable for the treatment of 0-200mg/L uranium-containing wastewater.

CN118988272APending Publication Date: 2024-11-22NUCLEAR POWER INSTITUTE OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411351161.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing adsorbents have low adsorption capacity, large reagent usage and difficult to process secondary waste when treating uranium-containing waste water. The introduction of metal magnetic materials may lead to weakening of acid and alkali resistance and increasing agglomeration, increasing post-treatment difficulty and being unfavorable to green production.

Method used

Polyvinylpyrrolidone coated with magnetic ferrite adsorbent, and by adjusting pH and temperature, the dual effects of complexation and electrostatic adsorption generated by the shared electron pair of amide groups and U(VI) in the carbon layer are significantly improved. , and achieve efficient adsorption and regeneration through magnetic separation.

Benefits of technology

The adsorption capacity of nanomagnetic ferrite to U(VI) is significantly improved, with a single adsorption rate greater than 80%, and a uranium removal rate ≥98%. The adsorption process is a spontaneous endothermic process, which simplifies the reaction conditions and achieves high efficiency. adsorption and recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005062397460000011
    Figure HDA0005062397460000011
  • Figure HDA0005062397460000012
    Figure HDA0005062397460000012
  • Figure HDA0005062397460000021
    Figure HDA0005062397460000021
Patent Text Reader

Abstract

The invention relates to the technical field of radioactive waste liquid treatment, and provides a preparation method of a polyvinylpyrrolidone coated magnetic ferrite adsorbent, which comprises the following steps: mixing FeSO4, FeS2 and PVP-K30, grinding the formed mixture, and carrying out gradient heating for a period of time to obtain the magnetic ferrite adsorbent. Gradually cooling, washing and drying to obtain the polyvinylpyrrolidone coated magnetic ferrite adsorbent. The invention further provides application of the adsorbent in uranium-containing wastewater, the pH value of the uranium-containing wastewater is adjusted to 6.0-8.0, then the adsorbent is added, and after adsorption is conducted for a period of time, the adsorbent and adsorption effluent are subjected to magnetic separation through a magnet; when the adsorbent is applied to U adsorption in uranium-containing wastewater, the reaction conditions are mild and easy to control, efficient adsorption can be achieved within a short time, after 100 mg / L of adsorption stock solution is continuously adsorbed for three times, the U concentration of adsorption effluent is smaller than or equal to 2 mg / L, and the uranium removal rate is larger than or equal to 98%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of radioactive waste liquid treatment, and in particular to a preparation method of a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent and application thereof in uranium-containing waste water. Background Art

[0002] Uranium has the dual hazards of heavy metal chemical toxicity and radioactive radiation. Improper discharge of uranium-containing wastewater will not only cause a waste of uranium resources, but will also be absorbed and accumulated by organisms along the food chain, eventually causing accumulation in the human body and chronic poisoning, endangering the ecological environment and human health. The composition of uranium-containing wastewater is complex. There have been a large number of research reports on the treatment of uranium-containing wastewater at home and abroad. The main methods include chemical precipitation, ion exchange, membrane separation, electrochemical, microbial, plant remediation, evaporation concentration and adsorption, among which adsorption is the most widely used. The adsorption method for removing uranium relies on high-performance adsorbents. The widely used adsorbents now include silica gel, activated carbon, ion exchange resins, etc., but they generally have many disadvantages such as low adsorption capacity, large reagent dosage and difficult secondary waste treatment. The industry is in urgent need of developing high-performance adsorbents with high adsorption capacity.

[0003] In recent years, the use of fixed nano-photocatalysts or added magnetic materials as adsorbents has been widely studied. In the additional magnetic method, magnetic nanomaterials such as Fe3O4 and FeO are combined with nano-photocatalytic materials to make the composite material have the characteristics of rapid magnetic separation. However, the introduction of metal magnetic materials may lead to a weakening of acid-base resistance and an increase in agglomeration, making the post-treatment of uranium-containing wastewater more difficult and not conducive to the green production of enterprises. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent and its application in uranium-containing wastewater, and specifically to a method for adsorbing U in uranium-containing wastewater by the above-mentioned adsorbent. The method can be applied to the treatment of uranium-containing waste liquid with a U(VI) concentration of 0 to 200 mg / L generated during the development and production of new fuel elements, and can also be applied to the treatment of waste liquid of other uranium-containing systems, thereby providing a guarantee for the development and production of fuel elements, providing technical support for the treatment of radioactive wastewater, and having important significance for environmental protection and the sustainable development of nuclear energy.

[0005] The embodiments of the present invention are implemented by the following technical solutions:

[0006] A method for preparing a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent comprises the following steps:

[0007] S1. Dry FeSO4·7H2O for a period of time to obtain FeSO4·H2O;

[0008] S2. Mix FeSO4·H2O, FeS2 and PVP-K30, and grind the resulting mixture for a period of time; wherein the mass ratio of FeSO4·H2O to FeS2 is 15-20:1; and the amount of PVP-K30 added is 5-10% of the total mass;

[0009] S3. The mixture ground from S2 is subjected to a gradient heating for a period of time under a protective atmosphere, and then gradually cooled, washed, and dried to obtain a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent.

[0010] The invention discloses an application of a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent in uranium-containing wastewater. The pH value of the uranium-containing wastewater is adjusted to 6.0-8.0, and then the adsorbent is added. After adsorption for a period of time, a magnet is used to magnetically separate the adsorbent from the adsorption effluent.

[0011] Furthermore, the method comprises the following steps: adjusting the pH value of the uranium-containing wastewater to 6.0-8.0, adding the above-mentioned adsorbent at a certain temperature, and stirring and mixing until the adsorption time is ≥60min or the U(VI) concentration of the reaction system solution does not change significantly after three consecutive analyses, and then the adsorption reaction ends.

[0012] Furthermore, the adsorption is repeated multiple times under the above conditions, preferably more than 3 times, to further improve the adsorption efficiency of U(VI).

[0013] Furthermore, the uranium-containing wastewater is uranium-containing waste liquid with a U(VI) concentration of 0 to 200 mg / L.

[0014] Furthermore, the temperature during adsorption is set to 30-60°C.

[0015] Furthermore, the solid-liquid ratio of the adsorbent to the uranium-containing wastewater is ≥1.0 g / L.

[0016] Furthermore, after the adsorption is completed, the adsorbent is soaked in a 0.05-0.15 mol / L hydrochloric acid solution for 30-60 min to desorb and regenerate the adsorbent.

[0017] Furthermore, during the stirring and mixing, the stirring time is controlled to be 5-20 min and the stirring speed is controlled to be 150-800 rpm / min.

[0018] The present invention uses polyvinyl pyrrolidone coated magnetic ferrite as an adsorbent to adsorb U(VI) in uranium-containing wastewater, which can significantly improve the adsorption capacity of nano magnetic ferrite such as Fe3O4 for U(VI), and the adsorption capacity can be as high as 185.8-291.0 mg / g, and has good recycling performance.

[0019] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:

[0020] 1. The amide groups in the carbon layer of the polyvinyl pyrrolidone-coated magnetic ferrite of the present invention share electron pairs with U(VI) to produce a dual effect of complexation and electrostatic adsorption. And its adsorption process is a spontaneous endothermic process, and the adsorption reaction is further promoted by heating. More importantly, the reaction system can reach adsorption equilibrium within 60 minutes under the condition of pH value of 6.0-7.0, and the single adsorption rate is greater than 80%. Therefore, the reaction conditions of the adsorbent of the present invention when used to adsorb U(VI) in uranium-containing wastewater are mild and easy to control, and efficient adsorption can be achieved in a short time. After 3 consecutive adsorptions of 100 mg / L adsorption stock solution, the U(VI) concentration of the adsorption effluent is ≤2 mg / L, and the uranium removal rate is ≥98%.

[0021] 2. The adsorbent of the present invention can be used for the treatment of uranium-containing wastewater (especially uranium-containing organic wastewater) with a U(VI) concentration of 0 to 200 mg / L generated during the development and production of new fuel elements and the recovery of uranium elements. It can also be used for the treatment of waste liquids from other uranium-containing systems, providing a guarantee for the development and production of fuel elements, providing technical support for the treatment of radioactive wastewater, and having important significance for environmental protection and the sustainable development of nuclear energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 It is a schematic diagram of the effect of solution pH on the adsorption effect of Fe3O4@PVP;

[0024] Figure 2 It is a schematic diagram of the effect of initial uranium concentration and adsorbent addition amount on the adsorption effect of Fe3O4@PVP;

[0025] Figure 3 It is a schematic diagram of the effect of temperature on the adsorption effect of Fe3O4@PVP;

[0026] Figure 4 Schematic diagram of the effect of ionic strength on the adsorption effect of Fe3O4@PVP. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0028] Example 1

[0029] This embodiment provides a method for preparing a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent, comprising the following steps:

[0030] First, FeSO4·7H2O was dried at 453K for 6 hours to obtain FeSO4·H2O;

[0031] Secondly, FeSO4·H2O, FeS2 and PVP-K30 were mixed in a certain mass ratio (PVP-K30 addition amount was 5wt.%, FeSO4 / FeS2 mass ratio was 15 / 1), and the resulting mixture was placed in an omnidirectional planetary ball mill and ground for 30 minutes to make it uniformly mixed;

[0032] Subsequently, the raw material mixture was placed in a tubular furnace under nitrogen protection, the heating rate was set to 10°C / min, the temperature was raised to 500°C, and the reaction was carried out for 30 minutes. Finally, the calcined product was cooled to ambient temperature under nitrogen protection, washed three times with deionized water and ethanol, and then vacuum dried at 80°C to constant weight to obtain a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent, i.e., PVP-coated nano-Fe3O4 adsorbent.

[0033] Example 2

[0034] This embodiment provides a method for applying the polyvinyl pyrrolidone-coated magnetic ferrite adsorbent prepared above in uranium-containing wastewater, comprising the following steps:

[0035] (1) Adsorbent selection: Select the above adsorbent with a size of 30 nm and a carbon layer thickness of 2 nm;

[0036] (2) Collecting uranium-containing waste liquid: collecting uranium-containing waste liquid with a U(VI) concentration of 100 mg / L and adding it to the reactor;

[0037] (3) Adjusting the pH value of the solution: using ammonia water, adjusting the pH value of the solution to 7.0, filtering and setting aside;

[0038] (4) Setting the adsorption temperature: Set the heating temperature to 30°C and turn on the heating to preheat the solution;

[0039] (5) Weighing the adsorbent: accurately calculate the required amount of adsorbent according to the solid-liquid ratio of 1.0 g / L, and weigh it accurately for use;

[0040] (6) Start adsorption: start the stirring system, add the adsorbent into the reactor, and start the adsorption reaction process;

[0041] (7) Completion of adsorption: The adsorption reaction is considered to be complete when the above state is maintained for more than 60 min or when the U(VI) concentration of the solution does not change significantly after three consecutive analyses;

[0042] (8) Repeated adsorption: Repeat the above process for more than 3 times to obtain a treated uranium solution with a U(VI) concentration of 1.7 mg / L. The calculated uranium removal rate is 98.3%;

[0043] (9) Adsorbent separation: magnetically separating the adsorbent from the adsorption effluent using a magnet;

[0044] (10) Adsorbent regeneration: The adsorbent can be regenerated by soaking it in 0.1 mol / L HCl solution for 30 min.

[0045] Example 3

[0046] This embodiment provides a method for applying the polyvinyl pyrrolidone-coated magnetic ferrite adsorbent prepared above in uranium-containing wastewater, which is different from Embodiment 2 in that the heating temperature in step (4) is 40°C.

[0047] Finally, a uranium solution with a U(VI) concentration of 0.87 mg / L was obtained, and a uranium removal rate of 99.1%.

[0048] Example 4

[0049] This embodiment provides a method for applying the polyvinyl pyrrolidone-coated magnetic ferrite adsorbent prepared above in uranium-containing wastewater, which differs from Example 2 in that: in step (1), the adsorbent size is 50 nm; in step (3), the pH value of the solution is adjusted to 8.0; and in step (4), the heating temperature is 50°C.

[0050] Finally, a uranium solution with a U(VI) concentration of 0.71 mg / L was obtained, and a uranium removal rate of 99.3%.

[0051] Example 5

[0052] This embodiment provides a method for applying the polyvinyl pyrrolidone-coated magnetic ferrite adsorbent prepared above in uranium-containing wastewater, which is different from that of embodiment 4 in that: the heating temperature in step (4) is 60° C.;

[0053] Finally, a uranium solution with a U(VI) concentration of 0.47 mg / L was obtained, and a uranium removal rate of 99.5%.

[0054] Example 6

[0055] This embodiment provides a method for applying the polyvinyl pyrrolidone-coated magnetic ferrite adsorbent prepared above in uranium-containing wastewater. The difference from Embodiment 1 is that in step (5), the solid-liquid ratio of the adsorbent to the uranium-containing wastewater is 1.5 g / L.

[0056] Finally, a uranium solution with a U(VI) concentration of 0.63 mg / L was obtained, and a uranium removal rate of 99.2%.

[0057] Experimental Example 1-Effect of Solution pH on Adsorption Effect

[0058] In order to explore the effect of solution pH on adsorption effect, this experiment measured the Zeta potential of Fe3O4@PVP, and then used Fe3O4@PVP as adsorbent, and used nitric acid and ammonia solution to adjust the initial pH value of the solution. Seven groups of solutions with different initial pH values, including pH = 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, and 8.0, were set to carry out experiments. After adsorption equilibrium, the pH value was tested. The results are shown in Table 1. Figure 1 ;in, Figure 1 (a) is the Zeta potential curve. Figure 1 (b) is the relationship between the solution adsorption equilibrium pH value and the adsorption capacity of Fe3O4@PVP for uranyl ions; ρ0 = 50 mg / L, adsorption temperature is 20 °C, solid-liquid ratio is 0.2 g / L, t = 120 min;

[0059] The pH test results showed that the pH value of the solution changed slightly after adsorption equilibrium, and the pH values ​​after adsorption equilibrium were 2.02, 3.11, 4.08, 5.12, 6.09, 6.97, and 7.88, respectively.

[0060] Depend on Figure 1 (a) The results show that the zero potential point of Fe3O4@PVP is pH = 9.25, that is, when pH < 9.25, the adsorbent surface is positively charged. When the pH value of the solution increases from 2.0 to 8.0, the positive charge on the surface of Fe3O4@PVP decreases continuously and gradually approaches zero potential. At the same time, the existence form of U(VI) changes from UO2 2+ Continuously add UO2(OH) + 、(UO2)3(OH)5 + 、UO2(OH)2、(UO2)3(OH)7 - With U2O7 2- The positive charge number decreases continuously, and finally U(VI) carries a negative charge. That is, when the pH value of the solution increases from 2.0 to 8.0, the electrostatic repulsion between Fe3O4@PVP and U(VI) decreases continuously and turns into electrostatic attraction. Therefore, the adsorption results are as follows: Figure 1As shown in (b), within the range of pH ≤ 6.0, the adsorption capacity increases with the increase of pH value. When the pH value increases to 6.0-8.0, the adsorption capacity of Fe3O4@PVP for U(VI) reaches the maximum value, so the suitable adsorption pH value is 6.0-7.0. From this phenomenon, it can also be inferred that the adsorption of U(VI) by Fe3O4@PVP mainly comes from the dual effects of complexation and electrostatic adsorption generated by the shared electron pairs between the amide groups in the Fe3O4@PVP carbon layer and U(VI).

[0061] Experimental Example 2-Effect of initial uranium concentration and adsorbent addition amount on adsorption effect

[0062] The initial uranium concentration of the solution and the amount of adsorbent added are closely related to the adsorption of uranyl ions by Fe3O4@PVP. The effect of initial uranium concentration on uranium adsorption was studied at 20-30°C, and the other conditions were preferred. Six groups of different adsorbent addition amounts (5-90 mg) were set to study the effect of adsorbent addition amount on adsorption. The results are shown in Figure 2 , where pH = 6.0, adsorption temperature is 25 °C, t = 120 min;

[0063] Depend on Figure 2 It can be seen that: when the adsorption amount is constant, with the increase of the initial uranium concentration, the adsorption capacity of Fe3O4@PVP gradually increases, and the rate of increase continues to slow down, and finally reaches saturation; when the initial uranium concentration is constant, with the increase of the amount of adsorbent added, the uranium adsorption rate continues to increase and reaches equilibrium. This is because as the initial uranium concentration increases, adsorption and desorption continue to occur on the active adsorption sites on the Fe3O4@PVP surface, but the total number of adsorption sites is constant, and finally the adsorption and desorption equilibrium is reached. Therefore, the adsorption capacity increases first and then reaches saturation. As the amount of adsorbent added increases, the active adsorption sites increase, and the adsorption rate increases. According to the curve, it is estimated that at 20-30°C, the saturated adsorption capacity of Fe3O4@PVP for adsorbing U(VI) is about 160-300 mg / g, and the final single adsorption uranium adsorption rate is greater than 75%.

[0064] Experimental Example 3-Effect of Temperature on Adsorption Effect

[0065] Adsorption temperature is an important parameter that affects the adsorption rate and adsorption capacity. When the initial uranium mass concentration was 9.7-96 mg / L and pH = 6.0, five different adsorption temperatures of 20, 30, 40, 50, and 60 °C were set to study the effects of adsorption time and adsorption temperature on the adsorption of U(VI) by Fe3O4@PVP. The results are shown in Figure 3 ; Wherein, ρ0 = 50 mg / L, pH = 6.0, m = 10 mg;

[0066] Depend on Figure 3It can be seen that heating can greatly promote the adsorption of uranyl ions on the surface of Fe3O4@PVP, increase the adsorption rate, and reduce the time to reach adsorption equilibrium. Taking the initial uranium mass concentration of 47 mg / L as an example, when the temperature rises from 20°C to 30, 40, 50, and 60°C, the saturated adsorption capacity increases from 120.7 mg / g to 123.7, 131.0, 135.2, and 141.1 mg / g, respectively. Because the increase in temperature accelerates the migration rate of uranyl ions in the solution and increases the effective collision probability between uranyl ions and Fe3O4@PVP adsorption sites, this shows that heating can significantly improve the adsorption efficiency. Therefore, the present invention sets the adsorption temperature to 30-60°C as a preferred adsorption temperature.

[0067] Experimental Example 4-Effect of ionic strength on adsorption

[0068] Ionic strength affects the double layer structure of the adsorbent surface, which is crucial to clarify the mechanism of Fe3O4@PVP adsorption of U(VI). In addition, different forms of salts also exist in actual uranium-containing wastewater, which also have different ionic strengths. This study used KCl as an ionic strength regulator and set 5 groups of ionic strengths (50, 70, 90, 120, 150 mg / L) to study the effect of ionic strength on Fe3O4@PVP adsorption of U(VI). The results are shown in Figure 4 , where pH = 6.0, 40 ° C, ρ0 = 50 mg / L, t = 120 min;

[0069] Depend on Figure 4 It can be seen that: with the increase of ionic strength, the adsorption rate of Fe3O4@PVP for U(VI) gradually decreases, which indicates that the increase of ionic strength induces the change of the double electric layer structure on the Fe3O4@PVP surface, resulting in the weakening of the adsorption of Fe3O4@PVP and U(VI) or the reduction of the number of active sites on the Fe3O4@PVP surface, thereby inhibiting the adsorption of Fe3O4@PVP for U(VI). This also verifies that the adsorption of U(VI) by Fe3O4@PVP is caused by the dual effects of amide complexation and electrostatic adsorption.

[0070] In summary, the Fe3O4@PVP prepared by the present invention has excellent adsorption effect on U(VI). Specifically, the suitable pH value for Fe3O4@PVP to adsorb U(VI) is 6.0-8.0, preferably 6.0-7.0, and adsorption equilibrium can be reached within 60 minutes. As the initial U(VI) concentration in the solution increases, the adsorption capacity of Fe3O4@PVP gradually increases, but the rate of increase slows down, and finally reaches adsorption saturation; the increase in the amount of adsorbent added will increase the adsorption rate, and it will continue to slow down, and the single adsorption rate is greater than 75%. Moreover, Fe3O4@PVP is a magnetic material that is easy to separate, and is expected to be used in the treatment of 0-200 mg / L uranium-containing wastewater (especially uranium-containing organic wastewater) and uranium recovery.

[0071] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent, characterized in that: By weight, the method comprises the following steps: S1. Dry FeSO4·7H2O for a period of time to obtain FeSO4·H2O; S2, mixing FeSO4·H2O, FeS2 and PVP-K30, and grinding the resulting mixture for a period of time; S3. The mixture ground from S2 is subjected to a gradient heating for a period of time under a protective atmosphere, and then gradually cooled, washed, and dried to obtain a polyvinyl pyrrolidone-coated magnetic ferrite adsorbent.

2. The method for preparing the polyvinyl pyrrolidone coated magnetic ferrite adsorbent according to claim 1, characterized in that: In S2, the mass ratio of FeSO4·H2O and FeS2 is 15-20:1; the addition amount of PVP-K30 is 5-10% of the total mass.

3. Use of an adsorbent prepared by the preparation method according to claim 1 or 2 in uranium-containing wastewater, characterized in that: After adjusting the pH value of the uranium-containing wastewater, the above-mentioned adsorbent is added, adsorbed for a period of time, and then the adsorbent and the adsorption effluent are magnetically separated by a magnet.

4. The use of the adsorbent prepared by the preparation method according to claim 3 in uranium-containing wastewater, characterized in that: The method comprises the following steps: adjusting the pH value of uranium-containing wastewater to 6.0-8.0, adding the above-mentioned adsorbent at a certain temperature, and stirring and mixing until the adsorption time is ≥60 minutes or the U(VI) concentration of the reaction system solution does not change significantly after three consecutive analyses, and then the adsorption reaction ends.

5. Use of the adsorbent prepared by the preparation method according to claim 3 in uranium-containing wastewater, characterized in that: The uranium-containing wastewater is a uranium-containing waste liquid with a U(VI) concentration of 0 to 200 mg / L.

6. Use of the adsorbent prepared by the preparation method according to claim 3 in uranium-containing wastewater, characterized in that: The adsorbent has a size of 10 to 100 nm, and a carbon layer thickness of ≥1 nm.

7. Use of the adsorbent according to claim 3 in uranium-containing wastewater, characterized in that: The solid-liquid ratio of adsorbent to uranium-containing wastewater is ≥1.0g / L.

8. Use of the adsorbent obtained by the preparation method according to claim 3 in uranium-containing wastewater, characterized in that: The temperature during adsorption was set at 30-60°C.

9. Use of the adsorbent obtained by the preparation method according to claim 3 in uranium-containing wastewater, characterized in that: After the adsorption is completed, the adsorbent is soaked in a 0.05-0.15 mol / L hydrochloric acid solution for 30-60 min to desorb and regenerate the adsorbent.