Preparation method of consumable electrode for copper-chromium electric arc melting

Through the 'powder mixing-low-temperature sintering-crumbing' process, the problems of uneven composition and low density of copper-chromium contacts are solved, and the high density and uniformity of copper-chromium contacts are achieved, which simplifies the process and Reduces costs and improves the stability and yield of arc smelting.

CN119035550APending Publication Date: 2024-11-29GUILIN CONINST ELECTRICAL & ELECTRONIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191281.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

There are problems of uneven composition and low density in the existing copper-chrome contact self-consumable electrode preparation process, which leads to defects such as looseness and block loss during arc smelting, and the process is complex and costly.

Method used

Using the 'mixed powder-low-temperature sintering-crumbing' process, the powder separation and agglomeration problems are solved and the self-consumption is improved by performing low-temperature sintering at 300-550°C in a reducing atmosphere, and isostatic molding and vacuum sintering after crushing. Density and composition uniformity of electrodes.

Benefits of technology

The composition uniformity and high density of copper-chromium contacts are achieved, the stability of the arc smelting process is improved, the process complexity and cost are reduced, and the metallographic structure uniformity and yield of the product are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035550A_ABST
    Figure CN119035550A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a consumable electrode for copper-chromium electric arc melting, which comprises the following steps of: 1) weighing corresponding amounts of copper powder and chromium powder according to alloy components required by a process for later use; 2) uniformly mixing the weighed copper powder and chromium powder, performing low-temperature sintering on the obtained mixed powder in a reducing atmosphere, and crushing the obtained sintered material to obtain sintered powder; wherein the low-temperature sintering is carried out under the condition that the temperature is 300 to 550 DEG C; (3) an isostatic pressing forming die sleeve is filled with the obtained sintered powder, isostatic pressing forming is directly carried out or isostatic pressing forming is carried out after vibration compaction, and an electrode blank is obtained; and 4) carrying out vacuum sintering on the obtained electrode blank under a vacuum condition. The method is low in cost and simple in process, the prepared consumable electrode is high in density and uniform in component, when the consumable electrode is used for vacuum consumable electric arc melting, the stability of the melting process can be greatly improved, and the finished product rate of products is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy material preparation, and in particular to a method for preparing a consumable electrode for copper-chromium arc melting. Background Art

[0002] Copper-chromium contacts (CuCr contacts, chromium content is usually 25-55% by mass) have the characteristics of high voltage resistance, large breaking current capacity, low cutoff value, good anti-welding performance, etc. They are widely used in vacuum circuit breakers and are currently the main contact material for vacuum circuit breakers. There are four main methods for preparing copper-chromium contacts: solid phase sintering, infiltration, casting and vacuum consumable arc melting (arc melting for short). Among them, the copper-chromium contacts manufactured by arc melting have the best comprehensive performance and are currently recognized as the copper-chromium contacts with the best performance in the world.

[0003] The preparation technology of consumable electrodes is the key to the production of arc melting copper-chromium contact materials. The process of preparing consumable electrodes by conventional isostatic pressing is: mixing chromium powder and copper powder - isostatic pressing - vacuum sintering. Due to the difference in particle size and particle morphology between copper powder and chromium powder, powder separation and agglomeration are likely to occur when filling the mixed powder, resulting in uneven composition of the consumable electrode, and ultimately leading to local copper-rich / chromium-rich defects in the contact material; in addition, due to the poor sintering strength at the chromium powder aggregation site of the consumable electrode, the original particles of the powder are easy to fall off into the molten pool during arc melting, and even the powder blocks fall directly into the molten pool, causing defects such as looseness and falling blocks in the contact material.

[0004] The invention patent with publication number CN112481513A discloses a process for preparing a consumable electrode for a copper-chromium alloy electrical contact using CuCr metal powder. The technical route is to prepare a consumable electrode rod material using a conventional isostatic pressing process. Specifically, the copper-chromium mixed powder is cold isostatically pressed into a rod material and vacuum sintered. The obtained sintered blank is arc-melted in an arc melting furnace to form an ingot; the obtained ingot is thermally deformed into a rod material, which is then annealed and connected to an electrode rod of a certain length by electron beam welding. Finally, the electrode rod is placed in an arc melting furnace for consumable remelting. The number of non-metallic inclusion particles and gas content in the consumable electrode material described in the invention are both low, which can improve the stability of the copper-chromium alloy contact material during use. However, the consumable electrode needs to be arc-melted once in advance during the preparation process, and needs to be connected by electron beam welding, which is not only complex in process but also high in cost.

[0005] The invention patent with publication number CN111593224A discloses a method for preparing a consumable electrode rod for copper-chromium arc melting, including batching, ingot casting, powder making, blanking by cold pressing or cold spray deposition, degassing and hot isostatic pressing. The obtained consumable electrode rod has low gas content and ideal density. In the preparation of consumable electrodes, the invention uses copper plates and chromium blocks to melt into copper-chromium alloy ingots, and then makes spherical copper-chromium alloy powder by gas atomization to avoid the powder separation and agglomeration problems caused by the difference in particle size and particle morphology between copper powder and chromium powder in the conventional isostatic pressing process; on the other hand, the blanking process by cold pressing or cold spray deposition is combined with the hot isostatic pressing process to improve the density of the obtained consumable electrode rod. The process is relatively cumbersome and the cost is high. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a compact and uniformly composed consumable electrode for copper-chromium arc melting.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0008] A method for preparing a consumable electrode for copper-chromium arc melting comprises the following steps:

[0009] 1) Weigh the corresponding amount of copper powder and chromium powder according to the alloy composition required by the process and set aside;

[0010] 2) The weighed copper powder and chromium powder are mixed evenly, the obtained mixed powder is sintered at low temperature in a reducing atmosphere, and the obtained sintered material is crushed to obtain a sintered powder; wherein the low temperature sintering is carried out at a temperature of 300 to 550° C.;

[0011] 3) The obtained sintered powder is filled into an isostatic pressing mold sleeve, and isostatic pressing is performed directly or after vibration compaction, to obtain an electrode blank;

[0012] 4) The obtained electrode blank is vacuum sintered under vacuum conditions to obtain a consumable electrode for copper-chromium arc smelting.

[0013] In the industry, the composition of copper-chromium contact materials is usually 75-45% copper and 25-55% chromium by weight. Therefore, in step 1) of the method of the present invention, copper powder and chromium powder are weighed at 75-45% and 25-55% by weight, respectively. In the present invention, the copper powder is usually electrolytic copper powder, which has a dendritic shape and a particle size of ≤75μm (usually 200-mesh or 300-mesh sieve); the chromium powder is usually obtained by mechanical crushing of chromium blocks, has an irregular shape, and a particle size of 75-150μm (about 100-200 mesh).

[0014] In step 2) of the above preparation method, the copper powder and the chromium powder are mixed uniformly by conventional methods, such as placing the weighed copper powder and chromium powder in a mixer and mixing for 2 to 5 hours or even longer to achieve uniform mixing of the two. After low-temperature sintering, the sintered material is usually crushed to less than or equal to 40 mesh, preferably crushed to 40 to 60 mesh. The reducing atmosphere is usually a hydrogen atmosphere.

[0015] In step 2) of the above preparation method, the holding time during low-temperature sintering is preferably 0.5 to 2 hours. The applicant has found that low-temperature sintering of the mixed powder can give the copper powder and chromium powder in the mixed powder a certain bonding effect, thereby obtaining a sintered material (sintered block) with a certain sintering strength between the copper powder and the chromium powder. Since the copper powder and the chromium powder in the mixed powder are evenly mixed, the components of the sintered material obtained after sintering the mixed powder are also uniform; subsequently, the sintered material is crushed to break the irregular large-sized block-shaped sintered blocks into small-sized sintered powders of relatively uniform size. On the one hand, the small-sized sintered powders have better fluidity than the large-sized sintered blocks, thereby improving the filling of the sintered powders into the isostatic pressing process. On the other hand, even after crushing, since the sintered material itself has a certain sintering strength and is crushed to 40-60 meshes, the crushed particle size is much larger than the particle size of the copper powder and chromium powder raw materials themselves. Therefore, when the sintered powder obtained after crushing is filled into the isostatic pressing mold sleeve, it is not easy for the copper powder and chromium powder to separate, the copper powder to agglomerate or the chromium powder to agglomerate, thereby making the composition of the obtained consumable electrode uniform, and the vibration platform can be increased to increase the filling density of the consumable electrode, thereby improving the density and straightness of the electrode after isostatic pressing.

[0016] In step 3) of the above preparation method, the isostatic pressing operation is the same as the prior art. Specifically, the pressure during isostatic pressing is preferably 100-200 MPa, and the holding time is 1-2 min. The isostatic pressing die sleeve filled with sintered powder is vibrated and then isostatically pressed to further improve the density of the consumable electrode. The equipment for vibrating can be existing conventional equipment such as a vibration platform (also called a vibration platform).

[0017] In step 4) of the above preparation method, the vacuum sintering is carried out in a conventional vacuum sintering furnace, and the sintering parameters are the same as those in the prior art, preferably: the vacuum reading is ≤0.01Pa, and the vacuum sintering is carried out at 900-1050°C. Under the above conditions, the holding time of vacuum sintering is usually ≥1h, and the holding time is further preferably 1.5-6h.

[0018] Compared with the prior art, the present invention is characterized in that:

[0019] 1. The process of "powder mixing - low-temperature sintering - crushing" is combined to solve the problem of powder separation / aggregation in the prior art of directly filling the mixed powder into the isostatic pressing mold sleeve, so that the consumable electrode is dense and uniform in composition. When it is used for vacuum consumable arc melting, the stability of the melting process can be greatly improved, and the metallographic structure of the copper-chromium contact product is uniform.

[0020] 2. Compared with the existing technology, it does not require smelting and atomization, nor does it require the use of a combination of cold pressing and hot isostatic pressing processes. It can also obtain a dense and uniform copper-chromium consumable electrode with low cost and simple process.

[0021] 3. The consumable electrode prepared by the method of the present invention has uniform diameter and good straightness, and can be arc-melted without additional trimming. The copper-chromium contact product made by the consumable electrode of the present invention has uniform metallographic microstructure, no looseness, block drop, and copper-rich / chromium-rich defects of more than 100μm, and the product yield can reach more than 92%. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 25 consumable electrode prepared in Example 1 of the present invention.

[0023] Figure 2 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 40 consumable electrode prepared in Example 2 of the present invention.

[0024] Figure 3 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 40 consumable electrode prepared in Comparative Example 2 of the present invention.

[0025] Figure 4 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 55 consumable electrode prepared in Example 3 of the present invention.

[0026] Figure 5 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 55 consumable electrode prepared in Comparative Example 3-1 of the present invention.

[0027] Figure 6 This is the metallographic structure diagram of the contact product after arc melting of the copper-chromium 55 consumable electrode prepared in Comparative Example 3-2 of the present invention. DETAILED DESCRIPTION

[0028] In order to better explain the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments, but the embodiments of the present invention are not limited thereto.

[0029] Example 1

[0030] 1) Weigh 75% of copper powder and 25% of chromium powder by weight and set aside;

[0031] 2) The weighed copper powder and chromium powder are placed in a mixer and mixed for 4 hours. The obtained mixed powder is loaded into a stainless steel boat and placed in a sintering furnace for low-temperature sintering in a hydrogen atmosphere. The sintering parameters are: temperature 350°C, insulation time 2 hours; after sintering, the mixture is cooled with the furnace and taken out to obtain a sintered material; the obtained sintered material is crushed to 40-50 meshes using an ultrasonic vibrating screen machine to obtain a sintered powder;

[0032] 3) The obtained sintered powder is filled at a uniform speed until the diameter is The isostatic pressing mold sleeve is placed in the isostatic pressing mold sleeve, and the vibration platform (Xinxiang No. 1 Vibration Machinery Factory Co., Ltd., ZP-8-Ⅱ vibration platform) is started to vibrate the filled powder layer by layer, and after sealing, it is sent into the high-pressure chamber for isostatic pressing to obtain the electrode blank; wherein, the pressure during isostatic pressing is 100MPa, and the pressure holding time is 2min;

[0033] 4) The electrode blank obtained by isostatic pressing is placed in a vacuum furnace for vacuum sintering. The sintering parameters are: vacuum reading ≤ 0.01Pa, sintering temperature 900℃, and holding time 6h; after sintering, it is cooled in the furnace and taken out to obtain a dense and uniform electrode. Copper-chromium 25 consumable electrode. After testing, the relative density of the obtained copper-chromium 25 consumable electrode is 83%.

[0034] The copper-chromium 25 consumable electrode prepared in this example was used for vacuum consumable arc melting at a melting voltage of 23 V and a melting current of 2000 A to obtain Ingot, production The copper-chromium 25 contact product has a yield rate of 93%. The metallographic structure of the copper-chromium 25 contact product is as follows: Figure 1 shown.

[0035] Example 2

[0036] 1) Weigh 40% copper powder and 60% chromium powder by weight and set aside;

[0037] 2) The weighed copper powder and chromium powder are placed in a mixer and mixed for 3 hours. The obtained mixed powder is loaded into a stainless steel boat and placed in a sintering furnace for low-temperature sintering in a hydrogen atmosphere. The sintering parameters are: temperature 400°C, insulation time 1 hour; after sintering, the mixture is cooled with the furnace and taken out to obtain a sintered material; the obtained sintered material is crushed to 50-60 meshes using an ultrasonic vibrating screen machine to obtain a sintered powder;

[0038] 3) The obtained sintered powder is filled at a uniform speed until the diameter is The electrode blank is placed in an isostatic pressing mold sleeve, and a vibration platform (Xinxiang No. 1 Vibration Machinery Factory Co., Ltd., ZP-8-Ⅱ vibration platform) is started to compact the filled powder layer by layer, and after sealing, it is sent into a high-pressure chamber for isostatic pressing to obtain an electrode blank; wherein, the pressure during isostatic pressing is 180 MPa, and the holding time is 1.5 min;

[0039] 4) The electrode blank obtained by isostatic pressing is placed in a vacuum furnace for vacuum sintering. The sintering parameters are: vacuum reading ≤ 0.01Pa, sintering temperature 1000℃, and holding time 4h; after sintering, it is cooled in the furnace and taken out to obtain a dense and uniform electrode. Copper-chromium 40 consumable electrode. After testing, the relative density of the obtained copper-chromium 40 consumable electrode is 85%.

[0040] The copper-chromium 40 consumable electrode prepared in this example was used for vacuum consumable arc melting at a melting voltage of 24 V and a melting current of 2500 A to obtain Ingot, production The copper-chromium 40 contact product has a yield rate of 94%. The metallographic structure of the copper-chromium 40 contact product is as follows: Figure 2 shown.

[0041] Comparative Example 2

[0042] Example 2 was repeated, except that in step 2), the operation of sintering the mixed powder at low temperature and crushing the sintered material was omitted, that is, the mixed powder obtained by mixing the weighed copper powder and chromium powder in a mixer for 3 hours was directly subjected to step 3) and subsequent steps. After testing, the relative density of the obtained copper-chromium 40 consumable electrode was 75%.

[0043] The copper-chromium 40 consumable electrode prepared in this comparative example was used for vacuum consumable arc melting at a melting voltage of 24V and a melting current of 2500A to obtain Ingot, production The copper-chromium 40 contact product has a yield rate of 68%. The metallographic structure of the copper-chromium 40 contact product is as follows: Figure 3 As shown, the obtained electrode has obvious copper-rich (reddish) and chromium-rich (whiter) areas.

[0044] Example 3

[0045] 1) Weigh 45% copper powder and 55% chromium powder by weight and set aside;

[0046] 2) The weighed copper powder and chromium powder are placed in a mixer and mixed for 2 hours. The obtained mixed powder is loaded into a stainless steel boat and placed in a sintering furnace for low-temperature sintering in a hydrogen atmosphere. The sintering parameters are: temperature 500°C, insulation time 0.5h; after sintering, the mixture is cooled with the furnace and taken out to obtain a sintered material; the obtained sintered material is crushed to 40-60 meshes using an ultrasonic vibrating screen machine to obtain a sintered powder;

[0047] 3) The obtained sintered powder is filled at a uniform speed until the diameter is The isostatic pressing mold sleeve is placed in the isostatic pressing mold sleeve, and the vibration platform (Xinxiang No. 1 Vibration Machinery Factory Co., Ltd., ZP-8-Ⅱ vibration platform) is started to vibrate the filled powder layer by layer, and after sealing, it is sent into the high-pressure chamber for isostatic pressing to obtain the electrode blank; wherein, the pressure during isostatic pressing is 200MPa, and the pressure holding time is 1min;

[0048] 4) The electrode blank obtained by isostatic pressing is placed in a vacuum furnace for vacuum sintering. The sintering parameters are: vacuum reading ≤ 0.01Pa, sintering temperature 1050℃, and holding time 1.5h; after sintering, it is cooled in the furnace and taken out to obtain a dense and uniform electrode. Copper-chromium 55 consumable electrode. After testing, the relative density of the obtained copper-chromium 55 consumable electrode is 84%.

[0049] The copper-chromium 55 consumable electrode prepared in this embodiment is used for vacuum consumable arc melting at a melting voltage of 26V and a melting current of 2500A to obtain Ingot, production The copper-chromium 55 contact product has a yield rate of 93%. The metallographic structure of the copper-chromium 55 contact product is as follows: Figure 4 shown.

[0050] Comparative Example 3-1

[0051] Example 3 was repeated, except that in step 2), the sintering parameters were changed to: temperature 600° C., holding time 0.5 h. After testing, the relative density of the obtained copper-chromium 55 consumable electrode was 78%.

[0052] The copper-chromium 55 consumable electrode prepared in this comparative example was used for vacuum consumable arc melting at a melting voltage of 26V and a melting current of 2500A to obtain Ingot, production The copper-chromium 55 contact product has a yield rate of 70%. The metallographic structure of the copper-chromium 55 contact product is as follows: Figure 5 shown.

[0053] Comparative Example 3-2

[0054] Example 3 was repeated, except that in step 2), the sintering parameters were changed to: temperature 250° C., holding time 3 h. After testing, the relative density of the obtained copper-chromium 55 consumable electrode was 74%.

[0055] The copper-chromium 55 consumable electrode prepared in this comparative example was used for vacuum consumable arc melting at a melting voltage of 26V and a melting current of 2500A to obtain Ingot, production The copper-chromium 55 contact product has a yield rate of 68%. The metallographic structure of the copper-chromium 55 contact product is as follows: Figure 6 shown.

[0056] The gas content of the consumable electrodes prepared in the above-mentioned embodiments and comparative examples was tested, and the results are shown in the following Table 1.

[0057] Table 1:

[0058]

Claims

1. A method for preparing a consumable electrode for copper-chromium arc melting, The following steps are involved: 1) Weigh the corresponding amount of copper powder and chromium powder according to the alloy composition required by the process and set aside; 2) The weighed copper powder and chromium powder are mixed evenly, the obtained mixed powder is sintered at low temperature in a reducing atmosphere, and the obtained sintered material is crushed to obtain a sintered powder; wherein the low temperature sintering is carried out at a temperature of 300 to 550° C.; 3) The obtained sintered powder is filled into an isostatic pressing mold sleeve, and isostatic pressing is performed directly or after vibration compaction, to obtain an electrode blank; 4) The obtained electrode blank is vacuum sintered under vacuum conditions to obtain a consumable electrode for copper-chromium arc melting.

2. The preparation method according to claim 1, Its characteristics are: In step 2), the holding time of low temperature sintering is 0.5 to 2 hours.

3. The preparation method according to claim 1, Its characteristics are: In step 2), the sintered material is crushed to a size less than or equal to 40 mesh.

4. The preparation method according to any one of claims 1 to 3, Its characteristics are: In step 3), the pressure during isostatic pressing is 100-200 MPa, and the holding time is 1-2 min.

5. The preparation method according to any one of claims 1 to 3, Its characteristics are: In step 4), vacuum sintering is performed at 900-1050°C.

6. The preparation method according to claim 5, Its characteristics are: In step 4), the holding time of vacuum sintering is greater than or equal to 1 hour.

7. The preparation method according to claim 5, Its characteristics are: In step 4), the holding time of vacuum sintering is 1.5 to 6 hours.