Aluminum alloy plate and preparation method thereof
By adjusting the composition of aluminum alloy sheets and adopting dual-stage pre-aging treatment technology, the problems of insufficient forming performance, room temperature parking stability and paint hardening performance of aluminum alloy sheets are solved, achieving higher performance synergy and lightweight effects.
Patent Information
- Application Number
- CN202411169284.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
Existing aluminum alloy sheets have poor performance in forming performance, room temperature parking stability and paint hardening performance, especially in the problem of complex preparation processes and high cost after Sn and Cu microalloyization.
By adjusting the composition of aluminum alloy sheets, including Si, Fe, Cu, Mn, Mg, Cr, Ti and Sn, and using dual-stage pre-aging and solid solution treatment technology, the microstructure and performance of aluminum alloy sheets are optimized. .
It improves the room temperature parking stability and paint hardening performance of aluminum alloy sheets, meets the forming requirements of more complex parts, and realizes thinning of aluminum alloy sheets under equal strength, further improving the lightweight effect.
Smart Images

Figure BDA0005008707350000061 
Figure BDA0005008707350000062 
Figure BDA0005008707350000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to an aluminum alloy plate and a preparation method thereof. Background Art
[0002] Lightweighting of automobiles is an effective and economical means to achieve energy conservation and emission reduction, and it is also conducive to improving safety. Aluminum alloy sheets are considered to be ideal materials for lightweighting of automobiles due to their advantages of light weight, high specific strength and excellent comprehensive performance. 6xxx series aluminum alloys are the most widely used due to their excellent surface quality and heat-treatable strengthening properties. However, the current cost of aluminum alloy automobile sheets is much higher than that of traditional steel, and there is an urgent need to further reduce their costs. While ensuring the forming and stiffness requirements of parts, the improvement of the strength of 6xxx series aluminum alloys can reduce the use of aluminum materials, reduce the cost of parts and further improve the lightweight effect. In addition, while increasing the strength, the excellent forming performance and room temperature parking stability of the sheet should also be taken into account.
[0003] In recent years, some domestic universities and research institutes have conducted research on 6xxx series aluminum alloy automotive plates, such as:
[0004] The Chinese patent with the patent authorization announcement number CN112095039B proposes a two-stage pre-aging method to improve the performance of paint, but it does not pay attention to the stability of room temperature parking, especially after Sn and Cu micro-alloying, the preparation process is more complicated and its process is difficult to meet the needs.
[0005] The Chinese patent with the patent authorization announcement number CN103740988B proposes a method for preparing a high-performance aluminum alloy for automotive parts, but it adds elements such as Zr and Sr, which is more expensive.
[0006] The Chinese patent application with patent application publication number CN117467873A proposes an Al-Mg-Si-Sn-Sc alloy and a preparation method thereof, wherein the Sc element is added to the alloy and the alloy is supplied in T6 state. Summary of the invention
[0007] The main purpose of the present invention is to provide an aluminum alloy plate and a preparation method thereof, so as to solve the problems of poor forming performance, room temperature parking stability and paint hardening performance of the aluminum alloy plate in the prior art.
[0008] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided an aluminum alloy plate material, which comprises the following elements, measured in mass percentage: Si element content is 0.20-1.45wt%, Fe element content is ≤0.40wt%, Cu element content is 0.06-0.30wt%, Mn element content is 0.05-0.2wt%, Mg element content is 0.2-1.0wt%, Cr element content is ≤0.1wt%, Ti element content is 0.01-0.10wt%, Sn element content is 0.005-0.06wt%, the total content of unavoidable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
[0009] Furthermore, in terms of mass percentage, the above-mentioned aluminum alloy plate includes the following elements: the content of Si element is 0.40-1.25wt%, the content of Fe element is 0.1-0.3wt%, the content of Cu element is 0.15-0.25wt%, the content of Mn element is 0.10-0.18wt%, the content of Mg element is 0.4-0.8wt%, the content of Cr element is 0.01-0.05wt%, the content of Ti element is 0.02-0.04wt%, and the content of Sn element is 0.010-0.025wt%.
[0010] Furthermore, the mass ratio of the Sn element to the Cu element is 1:8-20.
[0011] Furthermore, the yield strength of the aluminum alloy plate after being placed at 25°C for 7 days is less than 100MPa; and / or, the increase in yield strength of the aluminum alloy plate after being placed at 25°C for 180 days is no more than 24MPa compared with that after being placed for 7 days; and / or, the aluminum alloy plate after being placed at 25°C for 7 days is sequentially subjected to a 2% pre-stretching treatment and a baking treatment at 185°C for 20min to obtain a treated aluminum alloy plate, and the yield strength of the treated aluminum alloy plate is greater than 220MPa, and the baking paint increase is greater than 140MPa.
[0012] According to another aspect of the present invention, there is provided a method for preparing the aforementioned aluminum alloy plate, the preparation method comprising: melting, refining and casting various raw materials including metals in accordance with a proportion to obtain an aluminum alloy ingot; subjecting the aluminum alloy ingot to a homogenization treatment, a hot rolling treatment, a cold rolling treatment, a solution treatment, a first-stage pre-aging treatment and a second-stage pre-aging treatment to obtain an aluminum alloy plate; wherein the temperature of the first-stage pre-aging treatment is greater than the temperature of the second-stage pre-aging treatment, and the cooling rate from the first-stage pre-aging treatment to the second-stage pre-aging treatment is ≥5°C / min.
[0013] Furthermore, the temperature of the first stage pre-aging treatment is 140-200° C.; and / or, the holding time of the first stage pre-aging treatment is 5-180s; and / or, the temperature of the second stage pre-aging treatment is 70-130° C.; and / or, the holding time of the second stage pre-aging treatment is 1-12h.
[0014] Further, the above-mentioned homogenization treatment includes a first-stage homogenization treatment and a second-stage homogenization treatment performed in sequence; wherein, the heating rate of the first-stage homogenization treatment is 30-80°C / h; and / or, the temperature of the first-stage homogenization treatment is 480-520°C; and / or, the holding time of the first-stage homogenization treatment is 4-10h; and / or, the heating rate from the first-stage homogenization treatment to the second-stage homogenization treatment is 20-40°C / h; and / or, the temperature of the second-stage homogenization treatment is 560-580°C; and / or, the holding time of the second-stage homogenization treatment is 6-10h.
[0015] Furthermore, an air cushion continuous annealing furnace is used for the above-mentioned solution treatment, and the solution treatment includes a heating process, a heat preservation process and a cooling process performed in sequence; and / or the heating rate of the heating process is ≥5°C / s; and / or the temperature of the heat preservation process is 565-585°C; and / or the heat preservation time of the heat preservation process is 0.5-5min; and / or the cooling rate of the cooling process is ≥30°C / s.
[0016] Further, the uncooled material after the homogenization treatment is directly subjected to the above-mentioned hot rolling treatment; and / or the thickness of the material after the hot rolling treatment is 3 to 8 mm.
[0017] Furthermore, the thickness of the material after the cold rolling treatment is 0.5 to 3.0 mm.
[0018] By applying the technical solution of the present application, compared with Mg and Si, Sn and Cu have stronger vacancy binding ability. The present application helps to improve the room temperature parking stability of the aluminum alloy sheet by adding Sn and Cu. Moreover, at high temperature, the release of vacancies in the aluminum alloy sheet and the precipitation of Sn phase and Cu phase help to improve the paint hardening performance of the aluminum alloy sheet. When the content of Sn is too little, the effect of improving the room temperature parking stability and paint hardening performance of the aluminum alloy sheet is not obvious. When the content of Sn is too much, it is not conducive to fully dissolving the Sn element back into the matrix, thereby not conducive to improving the uniformity of the microstructure distribution of the aluminum alloy sheet; when the content of Cu is too little, the effect of improving the room temperature parking stability and paint hardening performance of the aluminum alloy sheet is not obvious. When the content of Cu is too much, it is not conducive to improving the stamping performance and corrosion resistance of the aluminum alloy sheet. The addition of Si, Fe, Mn, Mg, Cr and Ti elements to the aluminum alloy plate helps to improve the comprehensive properties of the aluminum alloy plate, such as forming performance, baking performance and corrosion resistance. It is preferred to control the mass content of each element in the aluminum alloy plate within the above range, which helps to improve the synergistic effect between the components, thereby helping to improve the room temperature parking stability, paint hardening performance and stamping forming performance of the aluminum alloy plate, and further helps to make the aluminum alloy plate of the present application meet the forming requirements of more complex parts. In addition, since the aluminum alloy plate of the present application has high paint hardening performance, it can achieve thinning of the aluminum alloy plate at equal strength, reduce the amount of aluminum alloy plate used, and further improve the lightweight effect of the aluminum alloy plate. DETAILED DESCRIPTION
[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0020] It should be noted that mass percentage refers to the percentage of the mass (weight) of a certain alloy component in the total mass.
[0021] Yield strength: The yield limit of aluminum alloy when yielding occurs. The stress value that produces 0.2% residual deformation is stipulated as its yield limit. The stress-strain curve is obtained through a uniaxial tensile test, and the yield strength data is obtained through the curve.
[0022] Paint baking increment: The difference in yield strength of aluminum alloy plates before and after 2% pre-stretching treatment and baking treatment at 185℃ for 20 minutes.
[0023] As analyzed in the background technology of this application, the aluminum alloy sheets in the prior art have problems with poor forming performance, room temperature parking stability and paint hardening performance. In order to solve this problem, this application provides an aluminum alloy sheet and a preparation method thereof.
[0024] In a typical embodiment of the present application, an aluminum alloy plate is provided, which includes the following elements, measured in mass percentage: the content of Si element is 0.20-1.45wt%, the content of Fe element is ≤0.40wt%, the content of Cu element is 0.06-0.30wt%, the content of Mn element is 0.05-0.2wt%, the content of Mg element is 0.2-1.0wt%, the content of Cr element is ≤0.1wt%, the content of Ti element is 0.01-0.10wt%, the content of Sn element is 0.005-0.06wt%, the total content of unavoidable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
[0025] Compared with Mg and Si, Sn and Cu have stronger vacancy binding ability. The present application helps to improve the room temperature parking stability of the aluminum alloy sheet by adding Sn and Cu. Moreover, at high temperature, the release of vacancies in the aluminum alloy sheet and the precipitation of Sn phase and Cu phase help to improve the paint hardening performance of the aluminum alloy sheet. When the content of Sn is too little, the effect of improving the room temperature parking stability and paint hardening performance of the aluminum alloy sheet is not obvious. When the content of Sn is too much, it is not conducive to fully dissolving the Sn element back into the matrix, thereby not conducive to improving the uniformity of the organizational distribution of the aluminum alloy sheet; when the content of Cu is too little, the effect of improving the room temperature parking stability and paint hardening performance of the aluminum alloy sheet is not obvious. When the content of Cu is too much, it is not conducive to improving the stamping performance and corrosion resistance of the aluminum alloy sheet. The addition of Si, Fe, Mn, Mg, Cr and Ti elements to the aluminum alloy plate helps to improve the comprehensive properties of the aluminum alloy plate, such as forming performance, baking performance and corrosion resistance. It is preferred to control the mass content of each element in the aluminum alloy plate within the above range, which helps to improve the synergistic effect between the components, thereby helping to improve the room temperature parking stability, paint hardening performance and stamping forming performance of the aluminum alloy plate, and further helps to make the aluminum alloy plate of the present application meet the forming requirements of more complex parts. In addition, since the aluminum alloy plate of the present application has high paint hardening performance, it can achieve thinning of the aluminum alloy plate at equal strength, reduce the amount of aluminum alloy plate used, and further improve the lightweight effect of the aluminum alloy plate.
[0026] In order to further improve the synergistic effect between the components, thereby further reducing the yield strength of the aluminum alloy sheet, and improving the room temperature parking stability, paint hardening performance and stamping forming performance of the aluminum alloy sheet, in one embodiment of the present application, the above-mentioned aluminum alloy sheet preferably includes the following elements: the content of Si element is 0.40~1.25wt%, the content of Fe element is 0.1~0.3wt%, the content of Cu element is 0.15~0.25wt%, the content of Mn element is 0.10~0.18wt%, the content of Mg element is 0.4~0.8wt%, the content of Cr element is 0.01~0.05wt%, the content of Ti element is 0.02~0.04wt%, and the content of Sn element is 0.010~0.025wt%.
[0027] In one embodiment of the present application, the mass ratio of the Sn element to the Cu element is 1:8-20.
[0028] If the mass ratio of Sn element to Cu element is too large, the paint strength and paint increment of the plate will decrease. If the mass ratio of Sn element to Cu element is too small, the strength of the plate will be too high and the room temperature parking stability will decrease, which will lead to insufficient plate forming performance. It is preferred to control the mass ratio of Sn element to Cu element within the above range, which helps to give full play to the synergistic effect between Sn element and Cu element, thereby helping to further improve the room temperature parking stability and paint hardening performance of the aluminum alloy plate.
[0029] In one embodiment of the present application, the yield strength of the above-mentioned aluminum alloy plate after being placed at 25°C for 7 days is less than 100MPa; and / or, the increase in yield strength of the aluminum alloy plate after being placed at 25°C for 180 days compared with that after being placed for 7 days does not exceed 24MPa; and / or, the aluminum alloy plate placed at 25°C for 7 days is sequentially subjected to a 2% pre-stretching treatment and a baking treatment at 185°C for 20 minutes to obtain a treated aluminum alloy plate, and the yield strength of the treated aluminum alloy plate is greater than 220MPa, and the baking paint increase is greater than 140MPa.
[0030] The aluminum alloy sheet of the present application is an aluminum alloy sheet in T4P state, and the processed aluminum alloy sheet is an aluminum alloy sheet in T8X state. The aluminum alloy sheet having the above-mentioned yield strength and paint increment range helps to achieve thinning of the aluminum alloy sheet under equal strength and reduce the amount of aluminum alloy sheet, thereby helping to further improve the lightweight effect of the aluminum alloy sheet.
[0031] In another typical embodiment of the present application, a method for preparing the aforementioned aluminum alloy plate is provided, the preparation method comprising: melting, refining and casting various raw materials including metals in accordance with a proportion to obtain an aluminum alloy ingot; subjecting the aluminum alloy ingot to homogenization treatment, hot rolling treatment, cold rolling treatment, solution treatment, first-stage pre-aging treatment and second-stage pre-aging treatment to obtain an aluminum alloy plate; wherein the temperature of the first-stage pre-aging treatment is greater than the temperature of the second-stage pre-aging treatment, and the cooling rate from the first-stage pre-aging treatment to the second-stage pre-aging treatment is ≥5°C / min.
[0032] In the present application, the aluminum alloy ingot is subjected to homogenization treatment, which helps to effectively dissolve the alloy elements, especially the Sn element, so as to help improve the uniformity of the distribution of the alloy elements in the matrix, and then help to improve the room temperature parking stability and paint hardening performance of the aluminum alloy sheet. The alloy after the homogenization treatment is subjected to hot rolling treatment, which helps to improve the plasticity of the alloy, so that the alloy is easier to process, and the hot rolling treatment also helps to refine the grains, eliminate casting defects and improve the uniformity of the organization. The alloy after the hot rolling treatment is subjected to cold rolling treatment, which helps to improve the dimensional accuracy of the aluminum alloy sheet, eliminate the stress inside the material and improve the quality of the material surface. The alloy after the cold rolling treatment is subjected to solution treatment, which helps to dissolve the alloy elements, especially the Sn element, into the Al metal, so as to help improve the baking hardening performance of the aluminum alloy sheet. The use of a two-stage pre-aging treatment helps to further improve the bake hardening properties of the aluminum alloy sheet. Specifically, the first stage pre-aging treatment helps to precipitate clusters that are more conducive to conversion into a β" strengthening phase during the paint baking process, and the second stage pre-aging treatment helps to improve the room temperature parking stability of the aluminum alloy sheet, thereby helping to make the aluminum alloy sheet have both high room temperature parking stability and bake hardenability. It is preferred to control the cooling rate from the first stage pre-aging treatment to the second stage pre-aging treatment within the above range, which helps to reduce the risk of excessive precipitation or growth of clusters, resulting in excessive initial yield strength of the aluminum alloy sheet and decreased formability.
[0033] In one embodiment of the present application, the temperature of the first stage pre-aging treatment is 140-200° C.; and / or, the holding time of the first stage pre-aging treatment is 5-180s; and / or, the temperature of the second stage pre-aging treatment is 70-130° C.; and / or, the holding time of the second stage pre-aging treatment is 1-12h.
[0034] If the temperature of the first-stage pre-aging treatment is too high, a large number of clusters will be precipitated, which will lead to too high initial strength of the plate. If the temperature of the first-stage pre-aging treatment is too low, the effect of the first-stage pre-aging cannot be exerted, and the plate baking paint strength is insufficient. It is preferred to control the temperature and holding time of the first-stage pre-aging treatment within the above range, which is conducive to the precipitation of more clusters that are more conducive to conversion into β" strengthening phase during the baking paint process; if the temperature of the second-stage pre-aging treatment is too high, a large number of clusters will be precipitated, which will lead to too high initial strength of the plate. If the temperature of the second-stage pre-aging treatment is too low, the effect of pre-aging cannot be exerted, resulting in poor room temperature parking stability. It is preferred to control the temperature and holding time of the second-stage pre-aging treatment within the above range, which is conducive to further improving the room temperature parking stability of the aluminum alloy plate.
[0035] In one embodiment of the present application, the above-mentioned homogenization treatment includes a first-stage homogenization treatment and a second-stage homogenization treatment performed in sequence; wherein, the heating rate of the first-stage homogenization treatment is 30-80°C / h; and / or, the temperature of the first-stage homogenization treatment is 480-520°C; and / or, the holding time of the first-stage homogenization treatment is 4-10h; and / or, the heating rate from the first-stage homogenization treatment to the second-stage homogenization treatment is 20-40°C / h; and / or, the temperature of the second-stage homogenization treatment is 560-580°C; and / or, the holding time of the second-stage homogenization treatment is 6-10h.
[0036] If the temperature of the first-stage homogenization treatment is too high, it will cause overburning and material failure. If the temperature of the first-stage homogenization treatment is too low, it cannot ensure that the low-melting point phase is fully dissolved. It is preferred to control the temperature, holding time and heating rate of the first-stage homogenization treatment within the above range, which helps to ensure that the low-melting point phase of the material is fully dissolved and avoid overburning. In addition, the actual level of industrial production is also taken into consideration. If the temperature of the second-stage homogenization treatment is too high, it will cause overburning and material failure. When the temperature of the second-stage homogenization treatment is too low, the solubility of elements such as Sn is insufficient, which is not conducive to improving the room temperature parking stability of the aluminum alloy plate. It is preferred to control the temperature, holding time and heating rate of the second-stage homogenization treatment within the above range, which helps to avoid overburning while improving the room temperature parking stability and paint hardening performance of the aluminum alloy plate.
[0037] In order to further dissolve alloy elements, especially Sn elements, into Al metal, thereby improving the bake hardening performance of the aluminum alloy plate, in one embodiment of the present application, an air cushion continuous annealing furnace is preferably used for the above-mentioned solution treatment, and the solution treatment includes a heating process, a heat preservation process and a cooling process performed in sequence; and / or, the heating rate of the heating process is ≥5°C / s; and / or, the temperature of the heat preservation process is 565~585°C; and / or, the heat preservation time of the heat preservation process is 0.5~5min; and / or, the cooling rate of the cooling process is ≥30°C / s.
[0038] In order to further improve the plasticity of the alloy, refine the grains, eliminate casting defects and improve the uniformity of the structure, in one embodiment of the present application, it is preferred that the uncooled homogenized material is directly subjected to the above-mentioned hot rolling treatment; and / or, the thickness of the material after the hot rolling treatment is 3 to 8 mm.
[0039] In order to further improve the dimensional accuracy of the aluminum alloy plate, eliminate the stress inside the material and improve the surface quality of the material, in one embodiment of the present application, the thickness of the material after the above-mentioned cold rolling treatment is 0.5 to 3.0 mm.
[0040] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0041] Examples 1 to 8, Comparative Examples 1 to 3
[0042] Firstly, pure aluminum and various master alloys are melted according to the composition ratio shown in Table 1, and the melt is refined and then cast into an ingot using a semi-continuous casting device. After the ingot is headed and milled, it is placed in a heat treatment furnace for the first and second homogenization treatments. The heating rate of the first homogenization treatment is 50°C / h, and the heating rate from the first to the second homogenization treatment is 30°C / h. After the homogenization treatment, the ingot is directly taken out of the furnace for hot rolling. The thickness of the material after the hot rolling treatment is 5mm. After the hot rolling is completed, the obtained hot-rolled plate is cold-rolled. The material after the cold rolling treatment is The thickness is 2.0 mm; the obtained cold-rolled sheet is subjected to solution treatment, first-stage pre-aging treatment, and second-stage pre-aging treatment, and then trimming and blanking are performed to obtain an aluminum alloy sheet in T4P state, wherein the heating rate of the solution treatment is 5°C / s, and the cooling rate of the solution treatment is 30°C / s. The specific values of the temperature and holding time of the first-stage homogenization treatment and the second-stage homogenization treatment, the temperature and holding time of the solution treatment, the temperature and holding time of the first-stage pre-aging treatment and the second-stage pre-aging treatment, and the cooling rate from the first-stage pre-aging treatment to the second-stage pre-aging treatment are shown in Table 2.
[0043] Table 1
[0044]
[0045] Table 2
[0046]
[0047]
[0048] Example 9
[0049] The difference from Example 7 is that the content of Sn element is 0.025wt%, the content of Cu element is 0.20wt%, the mass ratio of Sn element to Cu element is 1:8, and finally an aluminum alloy plate in T4P state is obtained.
[0050] Example 10
[0051] The difference from Example 7 is that the content of Sn element is 0.010wt%, the content of Cu element is 0.20wt%, the mass ratio of Sn element to Cu element is 1:20, and finally an aluminum alloy plate in T4P state is obtained.
[0052] Embodiment 11
[0053] The difference from Example 7 is that the content of Sn element is 0.010wt%, the content of Cu element is 0.25wt%, the mass ratio of Sn element to Cu element is 1:25, and finally an aluminum alloy plate in T4P state is obtained.
[0054] Example 12
[0055] The difference from Example 7 is that the temperature of the first pre-aging treatment is 140°C, the holding time of the first pre-aging treatment is 180s, the temperature of the second pre-aging treatment is 70°C, the holding time of the second pre-aging treatment is 12h, and finally an aluminum alloy sheet in T4P state is obtained.
[0056] Example 13
[0057] The difference from Example 7 is that the temperature of the first pre-aging treatment is 200°C, the holding time of the first pre-aging treatment is 5s, the temperature of the second pre-aging treatment is 130°C, the holding time of the second pre-aging treatment is 1h, and finally an aluminum alloy sheet in T4P state is obtained.
[0058] Embodiment 14
[0059] The difference from Example 7 is that the temperature of the first pre-aging treatment is 205°C, the holding time of the first pre-aging treatment is 4s, the temperature of the second pre-aging treatment is 135°C, the holding time of the second pre-aging treatment is 0.5h, and finally an aluminum alloy sheet in T4P state is obtained.
[0060] Embodiment 15
[0061] The difference from Example 7 is that the heating rate of the first-stage homogenization treatment is 30°C / h, the temperature of the first-stage homogenization treatment is 480°C, and the holding time of the first-stage homogenization treatment is 10h; the heating rate from the first-stage homogenization treatment to the second-stage homogenization treatment is 20°C / h, the temperature of the second-stage homogenization treatment is 560°C, and the holding time of the second-stage homogenization treatment is 10h, and finally an aluminum alloy sheet in T4P state is obtained.
[0062] Example 16
[0063] The difference from Example 7 is that the heating rate of the first-stage homogenization treatment is 80°C / h, the temperature of the first-stage homogenization treatment is 520°C, and the holding time of the first-stage homogenization treatment is 4h; the heating rate from the first-stage homogenization treatment to the second-stage homogenization treatment is 40°C / h, the temperature of the second-stage homogenization treatment is 580°C, and the holding time of the second-stage homogenization treatment is 6h, and finally an aluminum alloy sheet in T4P state is obtained.
[0064] Embodiment 17
[0065] The difference from Example 7 is that the heating rate of the first-stage homogenization treatment is 85°C / h, the temperature of the first-stage homogenization treatment is 475°C, and the holding time of the first-stage homogenization treatment is 3h; the heating rate from the first-stage homogenization treatment to the second-stage homogenization treatment is 45°C / h, the temperature of the second-stage homogenization treatment is 555°C, and the holding time of the second-stage homogenization treatment is 5h, and finally an aluminum alloy sheet in T4P state is obtained.
[0066] Embodiment 18
[0067] The difference from Example 7 is that the temperature of the solution treatment is 565° C., the holding time of the solution treatment is 5 min, and finally an aluminum alloy plate in T4P state is obtained.
[0068] Embodiment 19
[0069] The difference from Example 7 is that the temperature of the solution treatment is 585° C., the holding time of the solution treatment is 0.5 min, and finally an aluminum alloy plate in T4P state is obtained.
[0070] Embodiment 20
[0071] The difference from Example 7 is that the temperature of the solution treatment is 555° C., the holding time of the solution treatment is 0.4 min, and finally an aluminum alloy plate in T4P state is obtained.
[0072] Performance Testing
[0073] The aluminum alloy sheets in the T4P state prepared in the above embodiments and comparative examples were tested for yield strength after being stored at 25°C for 7 days and 180 days. The baking performance adopts the evaluation standard of most OEMs, that is, the aluminum alloy sheets in the T4P state stored at 25°C for 7 days are pre-stretched by 2%, then kept in an oil bath furnace at 185°C for 20 minutes, and then quenched with water to room temperature to obtain the aluminum alloy sheets in the T8X state, and the yield strength and baking paint increment are tested. The above test results are shown in Table 3.
[0074] Table 3
[0075]
[0076]
[0077] As can be seen from Table 3, the cooling speed between the first and second stage pre-aging in Comparative Example 1 is too slow, resulting in a large number of clusters precipitating, the strength of the T4P state plate is too high, and the stamping performance is poor. In Comparative Example 2, insufficient Sn and Cu elements are added, resulting in insufficient room temperature parking stability in the T4P state and insufficient baking paint strength in the T8X state. In Comparative Example 3, the content of Cu and Sn elements is too high, resulting in too high yield strength of the T4P state plate.
[0078] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0079] Compared with Mg and Si, Sn and Cu have stronger vacancy binding ability. The present application helps to improve the room temperature parking stability of the aluminum alloy sheet by adding Sn and Cu. Moreover, at high temperature, the release of vacancies in the aluminum alloy sheet and the precipitation of Sn phase and Cu phase help to improve the paint hardening performance of the aluminum alloy sheet. When the content of Sn is too little, the effect of improving the room temperature parking stability and paint hardening performance of the aluminum alloy sheet is not obvious. When the content of Sn is too much, it is not conducive to fully dissolving the Sn element back into the matrix, thereby not conducive to improving the uniformity of the organizational distribution of the aluminum alloy sheet; when the content of Cu is too little, the effect of improving the room temperature parking stability and paint hardening performance of the aluminum alloy sheet is not obvious. When the content of Cu is too much, it is not conducive to improving the stamping performance and corrosion resistance of the aluminum alloy sheet. The addition of Si, Fe, Mn, Mg, Cr and Ti elements to the aluminum alloy plate helps to improve the comprehensive properties of the aluminum alloy plate, such as forming performance, baking performance and corrosion resistance. It is preferred to control the mass content of each element in the aluminum alloy plate within the above range, which helps to improve the synergistic effect between the components, thereby helping to improve the room temperature parking stability, paint hardening performance and stamping forming performance of the aluminum alloy plate, and further helps to make the aluminum alloy plate of the present application meet the forming requirements of more complex parts. In addition, since the aluminum alloy plate of the present application has high paint hardening performance, it can achieve thinning of the aluminum alloy plate at equal strength, reduce the amount of aluminum alloy plate used, and further improve the lightweight effect of the aluminum alloy plate.
[0080] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An aluminum alloy plate, characterized in that: In terms of mass percentage, the aluminum alloy plate includes the following elements: the content of Si element is 0.20-1.45wt%, the content of Fe element is ≤0.40wt%, the content of Cu element is 0.06-0.30wt%, the content of Mn element is 0.05-0.2wt%, the content of Mg element is 0.2-1.0wt%, the content of Cr element is ≤0.1wt%, the content of Ti element is 0.01-0.10wt%, the content of Sn element is 0.005-0.06wt%, the total content of inevitable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
2. The aluminum alloy sheet according to claim 1, characterized in that: In terms of mass percentage, the aluminum alloy plate includes the following elements: the content of Si element is 0.40-1.25wt%, the content of Fe element is 0.1-0.3wt%, the content of Cu element is 0.15-0.25wt%, the content of Mn element is 0.10-0.18wt%, the content of Mg element is 0.4-0.8wt%, the content of Cr element is 0.01-0.05wt%, the content of Ti element is 0.02-0.04wt%, and the content of Sn element is 0.010-0.025wt%.
3. The aluminum alloy sheet according to claim 1 or 2, characterized in that: The mass ratio of the Sn element to the Cu element is 1:8-20.
4. The aluminum alloy sheet according to any one of claims 1 to 3, characterized in that: The yield strength of the aluminum alloy plate after being placed at 25° C. for 7 days is less than 100 MPa; and / or the increment of the yield strength of the aluminum alloy plate after being placed at 25° C. for 180 days compared with that after being placed at 25° C. for 7 days does not exceed 24 MPa; And / or, the aluminum alloy plate, after being placed at 25° C. for 7 days, is subjected to a 2% pre-stretching treatment and a baking treatment at 185° C. for 20 minutes in sequence to obtain a treated aluminum alloy plate, wherein the treated aluminum alloy plate has a yield strength greater than 220 MPa and a baking paint increment greater than 140 MPa.
5. A method for preparing the aluminum alloy sheet according to any one of claims 1 to 4, characterized in that: The preparation method comprises: The raw materials including metals are sequentially melted, refined and cast according to the proportions to obtain aluminum alloy ingots; The aluminum alloy ingot is subjected to homogenization treatment, hot rolling treatment, cold rolling treatment, solution treatment, first-stage pre-aging treatment, and second-stage pre-aging treatment in sequence to obtain an aluminum alloy plate; The temperature of the first stage pre-aging treatment is greater than the temperature of the second stage pre-aging treatment, and the cooling rate from the first stage pre-aging treatment to the second stage pre-aging treatment is ≥5°C / min.
6. The preparation method according to claim 5, characterized in that: The temperature of the first stage pre-aging treatment is 140-200° C.; and / or, the holding time of the first stage pre-aging treatment is 5-180s; and / or, the temperature of the second stage pre-aging treatment is 70-130° C.; and / or, the holding time of the second stage pre-aging treatment is 1-12h.
7. The preparation method according to any one of claims 5 or 6, characterized in that The homogenization process includes a first-stage homogenization process and a second-stage homogenization process performed sequentially; Wherein, the heating rate of the first stage homogenization treatment is 30-80°C / h; and / or, the temperature of the first stage homogenization treatment is 480-520°C; and / or, the holding time of the first stage homogenization treatment is 4-10h; And / or, the heating rate from the first-stage homogenization treatment to the second-stage homogenization treatment is 20-40°C / h; and / or, the temperature of the second-stage homogenization treatment is 560-580°C; and / or, the holding time of the second-stage homogenization treatment is 6-10h.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The solid solution treatment is carried out in an air cushion continuous annealing furnace, and the solid solution treatment includes a heating process, a heat preservation process and a cooling process performed in sequence; and / or, the heating rate of the heating process is ≥5°C / s; and / or, the temperature of the heat preservation process is 565-585°C; and / or, the heat preservation time of the heat preservation process is 0.5-5min; and / or, the cooling rate of the cooling process is ≥30°C / s.
9. The preparation method according to any one of claims 5 to 8, characterized in that: The uncooled homogenized material is directly subjected to the hot rolling treatment; and / or the thickness of the material after the hot rolling treatment is 3 to 8 mm.
10. The preparation method according to any one of claims 5 to 9, characterized in that: The thickness of the material after the cold rolling treatment is 0.5 to 3.0 mm.
Citation Information
Cited By
Aluminum alloy plate, processing method of aluminum alloy plate, part comprising aluminum alloy plate and automobile
CN119351809A
Aluminum alloy sheet and preparation method therefor
EP4764017A1
Aluminum alloy sheet having high stability and high baking hardening performance, preparation method therefor and use thereof
WO2026012250A1
Aluminum alloy sheet and preparation method therefor
WO2026040835A1