Preparation method and application of carbon nanosphere modified biomass monolithic composite porous carbon
By adopting the preparation method of biomass monolithic composite porous carbon modified by nano-carbon balls and utilizing hydrothermal carbonization and thermochemical conversion technology, a microporous-mesoporous-macroporous hierarchical pore structure is constructed, which solves the pore clogging problem of traditional powdered carbon-based electrode materials, improves the electrochemical performance and space utilization of supercapacitors, and achieves high energy density and excellent electrochemical stability.
Patent Information
- Application Number
- CN202510961164.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-13
- Publication Date
- 2025-09-26
AI Technical Summary
The conductive agents and binders introduced into traditional powdered carbon-based electrode materials during the preparation of supercapacitor electrodes lead to pore blockage, affecting the improvement of electrochemical performance. In addition, the space utilization rate of wood pores is low, making it difficult to further improve the area-specific capacitance of the integral composite porous carbon.
A preparation method for biomass integral composite porous carbon modified with nano-carbon balls is adopted. Through hydrothermal carbonization coupled with thermochemical conversion technology, a self-supporting porous capacitor carbon modified with nano-carbon balls is constructed to form a hierarchical pore structure with micropores, mesopores and macropores. The natural tracheid structure of pine wood is utilized to avoid the use of conductive agents and adhesives.
The space utilization and electrochemical performance of self-supporting capacitive carbon are significantly improved, and a high specific surface area and excellent electrolyte transfer efficiency are achieved. It can be directly used as a supercapacitor electrode without the need for conductive agents and binders, and has high energy density, excellent rate performance and cycle stability.
Smart Images

Figure CN120698440A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of energy and chemical technology, and specifically refers to a preparation method and application of a nano-carbon ball modified biomass integral composite porous carbon. Background Art
[0002] As a new generation of energy storage devices, supercapacitors have attracted much attention due to their excellent electrochemical stability, ultra-long cycle life, and rapid charge and discharge characteristics. The conductive agents and binders introduced into traditional powdered carbon-based electrode materials during the preparation of supercapacitor electrodes may cause pore blockage and induce uncontrollable side reactions, thereby restricting the improvement of the electrochemical performance of carbon-based electrode materials. Therefore, constructing an integral composite porous carbon that does not require conductive agents, binders, and current collectors to achieve rapid charge migration and efficient transmission of electrolyte ions is an important research direction for improving the electrochemical performance of supercapacitors.
[0003] Wood has a tracheid structure for the transport of water and nutrients. After carbonization, the tracheid structure can be transformed into a regularly arranged micron-scale low-curvature pore structure. The pore structure formed after the wood is carbonized has a diameter of about 20-30μm and a wall thickness of about 1-2μm. The regularly arranged pore structure provides space for storing electrolyte solutions, significantly reducing the resistance to ion transport, while providing sufficient mechanical strength for the monolithic composite porous carbon. However, the cavity of the wood pores accounts for about 80% of the total volume of the monolithic composite porous carbon. Current research has not fully utilized the structural space of the pores, making it difficult to further improve the area-specific capacitance of the monolithic composite porous carbon. Summary of the Invention
[0004] In order to overcome some of the problems mentioned in the above background, the present invention provides a method for preparing a nano-carbon sphere-modified biomass monolithic composite porous carbon and its application, so as to at least partially solve the above problems.
[0005] According to the technical solution of the present invention, a method for preparing a nanocarbon sphere-modified biomass monolithic composite porous carbon is provided, comprising the following steps:
[0006] S1. The pine wood is cut into pine chips along the growth direction and then placed in a blast drying oven for drying. The dried pine chips are placed in a nitrogen atmosphere tube furnace for high-temperature carbonization to obtain a carbonized product.
[0007] S2. The carbonized product was immersed in a hydrochloric acid solution to remove inorganic salt impurities, and then rinsed with deionized water to a neutral pH value. The rinsed carbonized product was transferred to a drying oven for dehydration and then polished to a thickness of 0.6-1.2 mm to obtain CW-1 composite porous carbon;
[0008] S3. The CW-1 composite porous carbon was placed in a glucose solution for vacuum-assisted impregnation and then transferred to a hydrothermal reactor for hydrothermal carbonization to obtain a hydrothermal carbonized product. The hydrothermal carbonized product was dried in an oven and placed in a tubular furnace in a nitrogen atmosphere for constant temperature chemical conversion to obtain CW-H composite porous carbon;
[0009] S4. The CW-H composite porous carbon is placed in a potassium bicarbonate solution for vacuum impregnation and then transferred to a drying oven for dehydration. The carbonized product is then placed in a tubular furnace in a nitrogen atmosphere for constant-temperature chemical conversion to obtain a converted carbonized product. The converted carbonized product is immersed in hydrochloric acid to remove inorganic salt impurities, then rinsed with deionized water to a neutral pH value, and then dried in a drying oven to obtain CW-H-6 composite porous carbon.
[0010] Preferably, during the drying process of the pine wood chips in the blast drying oven in step S1, a briquette is placed on top of the pine wood chips, the temperature of the blast drying oven during the drying process is 60° C., and the drying time is 12 hours;
[0011] The gas flow rate in the nitrogen atmosphere tube furnace in step S1 is 200-400 mL / min, and the temperature in the tube furnace is increased to 600-1000° C. at a heating rate of 5-20° C. / min after starting operation and then maintained at high temperature for 60-180 minutes.
[0012] Preferably, the concentration of the hydrochloric acid solution in step S2 is 1 mol / L;
[0013] The temperature of the carbonized product in step S2 in the drying oven is 105° C., and the dehydration treatment time is 12 hours.
[0014] Preferably, the concentration of the glucose solution in step S3 is 10 g / 100 mL, the vacuum impregnation time of the CW-1 composite porous carbon in the glucose solution is 30 min, the reaction temperature of the hydrothermal reactor is 180° C., and the hydrothermal reaction time is 8 h;
[0015] The temperature of the hydrothermal carbide in the oven is 105°C, the drying time is 12 hours, the gas flow rate in the nitrogen atmosphere tube furnace in step S3 is 200-600 mL / min, and the temperature in the tube furnace is heated to 600-900°C at a heating rate of 5-20°C / min after starting work and then maintained at high temperature for carbonization for 60-180 minutes.
[0016] Preferably, the concentration of the potassium bicarbonate solution in step S4 is 6 g / 100 mL, the vacuum impregnation time of the CW-H composite porous carbon in the potassium bicarbonate solution is 30 min, the drying temperature in the drying oven is 105° C., and the drying time is 12 h;
[0017] The gas flow rate in the nitrogen atmosphere tube furnace in step S4 is 200-600 mL / min, and the temperature in the tube furnace is increased to 600-900° C. at a heating rate of 5-20° C. / min after starting operation and then maintained at high temperature for 60-180 minutes.
[0018] Preferably, the concentration of the hydrochloric acid solution in step S4 is 0.1-3 mol / L, the converted carbonized product is immersed in the hydrochloric acid solution for 12 hours, then rinsed with deionized water to a neutral pH value, and then dried in a drying oven at 105° C. for 12 hours.
[0019] Preferably, the temperature in the nitrogen atmosphere tube furnace in step S1 is raised to 900° C. at a heating rate of 10° C. / min after starting operation and then maintained at the temperature for high-temperature carbonization for 120 minutes, and the polishing thickness is 1 mm.
[0020] Preferably, the temperature in the nitrogen atmosphere tube furnace in step S3 is raised to 800° C. at a heating rate of 10° C. / min after starting operation and then maintained at the high temperature for carbonization for 120 minutes;
[0021] In step S4, the temperature in the nitrogen atmosphere tube furnace is raised to 800° C. at a heating rate of 10° C. / min after starting operation and then maintained at the high temperature for 120 minutes of carbonization. The concentration of the hydrochloric acid solution is 1 mol / L.
[0022] On the other hand, the present invention also provides a nano-carbon ball modified biomass integral composite porous carbon, the composite porous carbon obtained according to the above preparation method has a specific surface area of 277.2m 2 / g, the diameter of the nano-carbon balls is 200-300nm, and the nano-carbon balls are evenly distributed on the surface and inner wall of the pores of the monolithic composite porous carbon.
[0023] On the other hand, the present invention also provides an application of a method for preparing a nano-carbon ball-modified biomass integral composite porous carbon. The composite porous carbon obtained according to the above preparation method is applied in the field of capacitors. The composite porous carbon does not require a conductive agent, a binder, and a current collector, and can be directly used as an electrode of a supercapacitor.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention uses pine wood with a naturally porous structure as a precursor and develops a carbon source secondary deposition technology that couples hydrothermal carbonization with thermochemical conversion to successfully construct a self-supporting porous capacitor carbon modified with carbon nanospheres. The carbon nanospheres exhibit excellent self-support and electrochemical properties, and the electrodes can be directly used as electrodes for symmetrical supercapacitors without the need for conductive agents or binders.
[0026] The present invention uses economical pine wood as raw material to achieve the controllable preparation of nano-carbon sphere-modified monolithic composite porous carbon. The nano-carbon sphere-modified biomass monolithic composite porous carbon prepared by hydrothermal carbonization and high-temperature thermochemical conversion processes is uniformly loaded with nano-carbon spheres with a diameter of about 200-300 nm on the surface and inner wall of the pore structure, forming a hierarchical pore structure with micropores, mesopores and macropores, which significantly improves the space utilization and energy storage capacity of the self-supporting capacitive carbon.
[0027] This invention preserves the natural tracheid structure of pine wood after high-temperature carbonization, forming a uniformly arranged pore network that provides excellent mechanical properties for self-supporting capacitor carbon. Furthermore, the wood's characteristic pits are converted into circular pores with a diameter of approximately 2-3 μm after high-temperature carbonization, facilitating the transfer of electrolyte between adjacent pores and improving the efficiency of lateral electrolyte ion transport. The nanocarbon spheres effectively deposit on the inner walls of the pores, with the diameter of the nanocarbon spheres deposited on the inner walls of the CW-H-6 pores being 200-300 nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is a process flow chart of an embodiment of the present invention;
[0029] Figure 2 The SEM images of Examples 1 and 3 of the present invention are shown;
[0030] Figure 3 This is the HR-TEM image of Example 3 of the present invention;
[0031] Figure 4 1 is a nitrogen adsorption and desorption isotherm diagram of Examples 1 to 3 of the present invention;
[0032] Figure 5 The pore size distribution diagrams of Examples 1 to 3 of the present invention are shown;
[0033] Figure 6 CV curves of Examples 1 to 3 of the present invention at a scan rate of 5 mV / s;
[0034] Figure 7 For example 1 to example 3 of the present invention, the current density is 5 mA / cm 2 GCD curve diagram when ;
[0035] Figure 8The area specific capacitance diagrams of Examples 1 to 3 of the present invention at different current densities are shown;
[0036] Figure 9 CV curves of Example 3 of the present invention at different scanning speeds;
[0037] Figure 10 This is a GCD curve diagram of Example 3 of the present invention at different current densities;
[0038] Figure 11 CV curves of the symmetrical supercapacitor constructed in Example 3 of the present invention at different scan rates;
[0039] Figure 12 This is a GCD curve diagram of the symmetrical supercapacitor constructed in Example 3 of the present invention at different current densities;
[0040] Figure 13 This is a graph of the area-to-capacitance ratio of the symmetrical supercapacitor constructed in Example 3 of the present invention at different current densities;
[0041] Figure 14 This is the Ragone diagram of the symmetrical supercapacitor constructed in Example 3 of the present invention;
[0042] Figure 15 This is a graph showing the charge-discharge cycle stability of the symmetrical supercapacitor constructed in Example 3 of the present invention. DETAILED DESCRIPTION
[0043] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection.
[0044] In response to the shortcomings of the existing technology, this application solves the problem that the natural pore structure of the biomass precursor is destroyed after being crushed in the traditional preparation process of supercapacitor electrodes, the introduction of the binder increases the electrode interface impedance and causes pore structure blockage, hindering the flow and diffusion of the electrolyte, and in the long-term charge and discharge process, irreversible side reactions may occur between the current collector and the binder, causing the energy storage performance of the electrode material to decline. In addition, the problem of low pore space utilization of the monolithic carbon material after wood carbonization is solved by loading with nano-carbon balls, and the area specific capacitance of the monolithic carbon material is further improved by combining the pore structure construction; this application constructs a nano-carbon ball-modified biomass monolithic composite porous carbon through the carbon source secondary deposition technology of hydrothermal carbonization coupled with thermochemical conversion, which significantly improves the space utilization of self-supporting capacitive carbon. The symmetrical supercapacitor constructed with this electrode has a high energy density, excellent rate performance and cycle stability.
[0045] The present invention provides a method for preparing a nanocarbon sphere-modified biomass monolithic composite porous carbon, comprising the following steps:
[0046] S1. The pine wood is cut into pine chips along the growth direction and then placed in a blast drying oven for drying. The dried pine chips are placed in a nitrogen atmosphere tube furnace for high-temperature carbonization to obtain a carbonized product.
[0047] S2. The carbonized product was immersed in a hydrochloric acid solution to remove inorganic salt impurities, and then rinsed with deionized water to a neutral pH value. The rinsed carbonized product was transferred to a drying oven for dehydration and then polished to a thickness of 0.6-1.2 mm to obtain CW-1 composite porous carbon;
[0048] S3. The CW-1 composite porous carbon was placed in a glucose solution for vacuum-assisted impregnation and then transferred to a hydrothermal reactor for hydrothermal carbonization to obtain a hydrothermal carbonized product. The hydrothermal carbonized product was dried in an oven and placed in a tubular furnace in a nitrogen atmosphere for constant temperature chemical conversion to obtain CW-H composite porous carbon;
[0049] S4. The CW-H composite porous carbon is placed in a potassium bicarbonate solution for vacuum impregnation and then transferred to a drying oven for dehydration. The carbonized product is then placed in a tubular furnace in a nitrogen atmosphere for constant-temperature chemical conversion to obtain a converted carbonized product. The converted carbonized product is immersed in hydrochloric acid to remove inorganic salt impurities, then rinsed with deionized water to a neutral pH value, and then dried in a drying oven to obtain CW-H-6 composite porous carbon.
[0050] In a further embodiment of this embodiment, during the drying process of the pine wood chips in step S1 in a blast drying oven, a briquette is placed on top of the pine wood chips, and the temperature of the blast drying oven during the drying process is 60° C., and the drying time is 12 hours;
[0051] The gas flow rate in the nitrogen atmosphere tube furnace in step S1 is 200-400 mL / min, and the temperature in the tube furnace is increased to 600-1000° C. at a heating rate of 5-20° C. / min after starting operation and then maintained at high temperature for 60-180 minutes.
[0052] In a further embodiment of this example, the concentration of the hydrochloric acid solution in step S2 is 1 mol / L;
[0053] The temperature of the carbonized product in step S2 in the drying oven is 105° C., and the dehydration treatment time is 12 hours.
[0054] In a further embodiment of this embodiment, the concentration of the glucose solution in step S3 is 10 g / 100 mL, the vacuum impregnation time of the CW-1 composite porous carbon in the glucose solution is 30 min, the reaction temperature of the hydrothermal reactor is 180° C., and the hydrothermal reaction time is 8 h;
[0055] The temperature of the hydrothermal carbide in the oven is 105°C, the drying time is 12 hours, the gas flow rate in the nitrogen atmosphere tube furnace in step S3 is 200-600 mL / min, and the temperature in the tube furnace is heated to 600-900°C at a heating rate of 5-20°C / min after starting work and then maintained at high temperature for carbonization for 60-180 minutes.
[0056] In a further embodiment of this embodiment, the concentration of the potassium bicarbonate solution in step S4 is 6 g / 100 mL, the vacuum impregnation time of the CW-H composite porous carbon in the potassium bicarbonate solution is 30 min, the drying temperature in the drying oven is 105° C., and the drying time is 12 h;
[0057] The gas flow rate in the nitrogen atmosphere tube furnace in step S4 is 200-600 mL / min, and the temperature in the tube furnace is increased to 600-900° C. at a heating rate of 5-20° C. / min after starting operation and then maintained at high temperature for 60-180 minutes.
[0058] In a further embodiment of this embodiment, the concentration of the hydrochloric acid solution in step S4 is 0.1-3 mol / L, the converted carbonized product is immersed in the hydrochloric acid solution for 12 hours, then rinsed with deionized water to a neutral pH value, and then dried in a drying oven at 105°C for 12 hours.
[0059] In a further implementation of this embodiment, the temperature in the nitrogen atmosphere tube furnace in step S1 is raised to 900°C at a heating rate of 10°C / min after starting operation and then maintained at high temperature for 120 minutes, and the polishing thickness is 1 mm.
[0060] In a further embodiment of this embodiment, the temperature in the nitrogen atmosphere tube furnace in step S3 is raised to 800° C. at a heating rate of 10° C. / min after starting operation and then maintained at the high temperature for carbonization for 120 min;
[0061] In step S4, the temperature in the nitrogen atmosphere tube furnace is raised to 800° C. at a heating rate of 10° C. / min after starting operation and then maintained at the high temperature for 120 minutes of carbonization. The concentration of the hydrochloric acid solution is 1 mol / L.
[0062] It should be noted that the nitrogen flow rate significantly affects the preparation of monolithic porous carbon. Volatiles such as small molecules produced during wood pyrolysis accumulate in the tubular furnace. A suitable nitrogen flow rate not only provides an inert atmosphere but also carries the volatiles away from the furnace, preventing them from reattaching to the surface of the monolithic porous carbon or entering the pores to deposit amorphous carbon, thereby preventing pore blockage and a decrease in hydrophilicity.
[0063] A heating rate that is too high can easily cause deformation of the wood during pyrolysis, making it difficult for the macrostructure of the monolithic porous carbon to remain flat; while a heating rate that is too low can significantly prolong the thermochemical conversion time and increase the energy consumption of carbonization.
[0064] Thermochemical conversion temperature and time also have a significant impact on the preparation of monolithic porous carbon. Too low a temperature or too short a time can easily lead to insufficient pyrolysis or incomplete pore structure construction; while too high a temperature or too long a time may cause the microscopic pore structure to transform from micropores to macropores, thereby reducing the specific surface area and electrochemical performance of the monolithic porous carbon. In addition, too high a temperature or too long a time can also cause its macroscopic structure to collapse and mechanical properties to deteriorate, limiting its application potential as a supercapacitor electrode.
[0065] Tracheids, as the main conducting tissue of the xylem of vascular plants, have the functions of water transport, nutrient conduction, and mechanical support. Their morphological characteristics are characterized by a spindle shape with sharp ends. The minimum length of pine tracheids is about 1.2 mm. As the thickness of the monolithic porous carbon increases, the frequency of the closed structure at the ends of the tracheids increases significantly, and a pore structure with closed ends appears after the complete tracheids are carbonized. It is difficult for the electrolyte to flow into the pore structure with closed ends, resulting in a hysteresis zone for the electrolyte flow, which leads to a further decrease in the effective specific surface area of the self-supporting capacitor carbon, thereby reducing its energy storage capacity. Therefore, the thickness of the monolithic porous carbon should not exceed 1.2 mm.
[0066] A carbon source secondary deposition technique, combining hydrothermal carbonization with thermochemical conversion, has been developed, resulting in the successful construction of self-supporting porous capacitor carbon modified with carbon nanospheres. This research reveals the synergistic regulatory mechanism of carbon source secondary deposition on the microstructure and electrochemical properties of self-supporting capacitor carbon. Carbon nanospheres with diameters of approximately 200-300 nm are uniformly loaded on the surface and inner walls of the pore structure of CW-H-6, forming a hierarchical microporous-mesoporous-macroporous pore structure, significantly improving the spatial utilization and energy storage capacity of the self-supporting capacitor carbon.
[0067] On the other hand, the embodiment of the present invention also provides a nano-carbon ball modified biomass monolithic composite porous carbon. The composite porous carbon obtained by the above preparation method has a specific surface area of 277.2 m 2 / g, the diameter of the nano-carbon balls is 200-300nm, and the nano-carbon balls are evenly distributed on the surface and inner wall of the pores of the monolithic composite porous carbon.
[0068] On the other hand, an embodiment of the present invention also provides an application of a method for preparing a nano-carbon ball-modified biomass integral composite porous carbon. The composite porous carbon obtained according to the above preparation method is applied in the field of capacitors. The composite porous carbon does not require a conductive agent, a binder, and a current collector, and can be directly used as an electrode of a supercapacitor.
[0069] Example 1
[0070] Step 1: Cut the pine wood into 15mm long, 15mm wide, and 2.0mm thick chips along its growth direction. Dry the chips in a 60°C forced air drying oven for 12 hours. Place a 2kg weight on top of the chips during the drying process to prevent deformation.
[0071] Step 2: The dried pine wood chips were placed in a nitrogen atmosphere with a gas flow rate of 400 mL / min. 2 In an atmosphere tube furnace, the temperature was programmed to 900°C (10°C / min) and thermochemically converted at this temperature for 120 minutes. The resulting carbonized product was immersed in a 1 mol / L hydrochloric acid solution for 12 hours to remove impurities such as inorganic salts. It was then repeatedly rinsed with deionized water to a neutral pH value. The carbonized product was transferred to a drying oven at 105°C for dehydration for 12 hours and then polished with sandpaper to a thickness of 1 mm. The self-supporting capacitor carbon prepared by this process was named CW-1.
[0072] Step 3: The nano-carbon sphere-modified biomass monolithic composite porous carbon prepared by the above preparation method is characterized and electrochemical performance tested, wherein the three-electrode system and the assembled symmetrical super-class container are subjected to cyclic voltammetry test, constant current charge-discharge test and electrochemical impedance spectroscopy test by an electrochemical workstation (CHI660e). In the three-electrode system, Hg / HgO electrode is selected as the reference electrode, platinum electrode is used as the counter electrode, and KOH solution with a concentration of 6 mol / L is used as the electrolyte. Parameters such as scan rate and current density are adjusted to obtain the electrochemical properties of the electrode material under different parameters, and the area specific capacitance, energy density / power density, cycle stability and AC impedance parameters of the monolithic composite porous carbon are further calculated. The calculation formulas for each parameter are as follows:
[0073] In a three-electrode system:
[0074]
[0075] In the above formula, C a Indicates the area specific capacitance of self-supporting capacitor carbon, in farads per square centimeter (F / cm 2 );I d1 is the discharge current in amperes (A); Δt1 represents the discharge time in seconds (s); a1 is the area of the self-supporting capacitor carbon in square centimeters (cm 2 ); ΔV1 is the potential window, in volts (V).
[0076] The specific capacitance, energy density, and power density of the symmetric supercapacitor based on the self-supporting capacitive carbon were calculated by the following formula:
[0077]
[0078] Among them, C h Represents the area specific capacitance of symmetric / asymmetric supercapacitors based on self-supporting capacitive carbon, in farads per square centimeter (F / cm 2 ). I d2 is the discharge current in amperes (A). Δt2 is the discharge time in seconds (s). a2 is the average area of the positive and negative electrodes in square centimeters (cm 2 ). ΔV2 represents the voltage window, in volts (V). E is the energy density of the supercapacitor based on area, in milliwatt hours per square centimeter (mWh / cm 2 ), P is the power density of the supercapacitor based on area, in milliwatts per square centimeter (mW / cm 2 ).
[0079] Example 2
[0080] Step 1: Same as step 1 of Example 1;
[0081] Step 2: Same as step 2 of Example 1;
[0082] Step 3: Prepare 100 mL of 10 g / 100 mL glucose solution, place CW-1 in the glucose solution for vacuum-assisted impregnation for 30 minutes, and then transfer it to a 150 mL polytetrafluoroethylene reactor for hydrothermal carbonization at 180 ° C for 8 hours. The carbonized product was dried in an oven at 105 ° C for 12 hours and then placed in a N2 atmosphere tube furnace with a gas flow rate of 400 mL / min. The temperature was programmed (10 ° C / min) to 800 ° C and thermochemically converted at constant temperature for 120 minutes. The nano-carbon sphere-modified self-supporting porous capacitor carbon prepared by this process was named CW-H;
[0083] Step 4 is the same as step 3 in Example 1.
[0084] Example 3
[0085] Step 1: Same as step 1 of Example 1;
[0086] Step 2: Same as step 2 of Example 1;
[0087] Step 3: Same as step 3 of Example 2;
[0088] Step 4: Prepare 100mL of potassium bicarbonate solution with a concentration of 6g / 100mL, place CW-H in potassium bicarbonate solution, vacuum-assisted impregnation for 30min, transfer to a drying oven at 105°C for dehydration for 12 hours, place in a N2 atmosphere tube furnace with a gas flow rate of 400mL / min, program temperature rise (10°C / min) to 800°C, and perform constant temperature thermochemical conversion for 120 minutes. The obtained carbonized product is immersed in a 1mol / L hydrochloric acid solution for 12 hours to remove inorganic salts and other substances, and then repeatedly rinsed with deionized water to a neutral pH value. The carbonized product is transferred to a drying oven at 105°C for dehydration for 12 hours. The nano-carbon sphere-modified self-supporting porous capacitor carbon prepared by this process is named CW-H-6.
[0089] Step 5: Electrochemical testing in a three-electrode system is the same as step 3 in Example 1.
[0090] The results obtained are as follows: Morphology and characterization analysis:
[0091] The SEM images of Example 1 (CW-1) and Example 3 (CW-H-6) are as follows: Figure 2 During the cutting process, the sawdust residue on the surface of the pine wood forms a flaky carbon structure after high-temperature carbonization. Although this enriches the surface characteristics of the self-supporting capacitor carbon, it affects the uniform loading of the micron carbon spheres during the hydrothermal process. Therefore, this application removes the carbon structure on the surface of the self-supporting capacitor carbon by polishing.
[0092] like Figure 2 As shown in (ac), the surface pore structure of Example 1 (CW-1) is evenly distributed.
[0093] Figure 2 (df) shows the scanning electron microscope images of Example 3 (CW-H-6), where the carbon nanospheres grow evenly on the surface of the self-supporting capacitor carbon and are clustered in some areas. Figure 2 As shown in (f), the diameter of the nanocarbon spheres is about 200-300 nm, which helps them to fully contact with the electrolyte and effectively promote the redox reaction during the charge and discharge process.
[0094] Figure 2 (gi) shows an SEM image of a longitudinal cross-section of Example 1 (CW-1). After high-temperature carbonization, Example 1 (CW-1) maintains the natural tracheid structure of pine wood, forming a uniformly arranged pore network. The pores have a diameter of approximately 20-30 μm and a wall thickness of approximately 1-2 μm, providing excellent mechanical properties for the self-supporting capacitive carbon. Furthermore, after high-temperature carbonization, the wood's characteristic pits are converted into circular pores with a diameter of approximately 2-3 μm, facilitating the transport of electrolyte between adjacent pores and improving the lateral transport efficiency of electrolyte ions. Figure 2 (jl) shows the longitudinal cross-sectional SEM image of Example 3 (CW-H-6), in which the carbon nanospheres are effectively deposited on the inner wall of the pores.
[0095] In addition, if Figure 2 As shown in (i), the diameter of the carbon nanospheres deposited on the inner wall of the pores of Example 3 (CW-H-6) is 200-300 nm, which is the same as the diameter of the carbon nanospheres deposited on the surface of the self-supporting composite electrode. Figure 3 HRTEM of (ac) reveals the microstructural regulation mechanism of carbon nanosphere loading on self-supporting capacitor carbon. Figure 3 As shown in (a, b), catalysis induces the formation of graphene sheets with typical layered stacking characteristics.
[0096] The N2 adsorption-desorption isotherms of Example 1 (CW-1), Example 2 (CW-H) and Example 3 (CW-H-6) are as follows: Figure 4 As shown in Figure 2, the isotherm of Example 1 (CW-1) exhibits a typical type IV curve and an H4 hysteresis loop, indicating the presence of a rich mesoporous structure within Example 1 (CW-1). The hysteresis loops of Example 2 (CW-H) loaded with carbon nanospheres and Example 3 (CW-H-6) after the pore structure is constructed are significantly weakened. Figure 5The pore size distribution of Example 1 (CW-1), Example 2 (CW-H) and Example 3 (CW-H-6) is shown. The activation treatment changes the pore structure of the self-supporting capacitive carbon from the mesopore-dominated pore structure of Example 1 (CW-1) to the micropore-mesopore coordinated distribution of Example 3 (CW-H-6).
[0097] Table 1 Pore structure parameters of Example 1 (CW-1), Example 2 (CW-H) and Example 3 (CW-H-6)
[0098]
[0099] As shown in Table 1, the specific surface area of Example 2 (CW-H) was reduced to 46.2 m 2 / g, the loading of nanocarbon balls without pore structure construction leads to a significant decrease in the specific surface area of the self-supporting capacitor carbon. After activation with potassium bicarbonate, the specific surface area of Example 3 (CW-H-6) is increased to 277.2m 2 / g, which is 2.7 times higher than that of Example 1 (CW-1), indicating that the etching effect of the activator forms a developed hierarchical porous structure in the nanocarbon spheres and self-supporting capacitor carbon during the one-step thermochemical conversion process.
[0100] The electrochemical performance of the self-supporting porous capacitive carbon modified with nanocarbon spheres was evaluated in a three-electrode system. Figure 6 As shown, there are obvious differences in the CV curves of Example 1 (CW-1), Example 2 (CW-H) and Example 3 (CW-H-6) at a scan rate of 5mV / s. CW-H modified with nanocarbon spheres exhibits a typical quasi-triangular CV curve, while Example 1 (CW-1) and Example 3 (CW-H-6) present characteristic curves that are closer to an ideal rectangle. This morphological difference indicates that the introduction of nanocarbon spheres effectively improves the surface properties of the self-supporting capacitor carbon, but leads to the loss of the microporous structure. It is worth noting that Example 3 (CW-H-6) that has undergone activation treatment exhibits the largest closed area of the CV curve, which indicates that its area specific capacitance reaches the highest value at a scan rate of 5mV / s, showing excellent charge storage capacity.
[0101] Figure 7 The results of the constant current charge and discharge test (GCD) further verified this conclusion. 2 At a current density of 1.5 GHz, Example 3 (CW-H-6) exhibited highly symmetrical charge-discharge curves, with a linear voltage-time response indicating a typical double-layer energy storage mechanism and efficient charge transfer kinetics. In contrast, the GCD curves of Example 2 (CW-H) and Example 1 (CW-1) exhibited varying degrees of polarization, demonstrating lower area-specific capacitance.
[0102] Figure 8 The following table shows the variation trend of area specific capacitance of Example 1 (CW-1), Example 2 (CW-H) and Example 3 (CW-H-6) with current density. 2 , 5mA / cm 2 , 10mA / cm 2 , 20mA / cm 2 、30mA / cm 2 and 50mA / cm 2 When the area specific capacitance of Example 1 (CW-1) is 3.7F / cm 2 、3.51F / cm 2 , 3.27F / cm 2 , 2.99F / cm 2 , 2.85F / cm 2 and 2.65F / cm 2 , the area specific capacitance of Example 2 (CW-H) is 3.2F / cm 2 , 2.86F / cm 2 , 2.52F / cm 2 , 2.06F / cm 2 , 1.78F / cm 2 and 1.48F / cm 2 The area specific capacitance of Example 3 (CW-H-6) is 6.36F / cm 2 , 5.84F / cm 2 , 5.56F / cm 2 , 5.09F / cm 2 , 4.79F / cm 2 and 4.49F / cm 2 Example 1 (CW-1), Example 2 (CW-H) and Example 3 (CW-H-6) were tested at a current density of 2 mA / cm 2 Up to 50mA / cm 2 The rate performances are 71.6%, 46.3% and 70.6% respectively, and Example 3 (CW-H-6) exhibits the highest area specific capacitance.
[0103] Based on the hierarchical porous structure, good self-supporting performance and uniform loading of nano-carbon spheres, Example 3 (CW-H-6) exhibits excellent electrochemical performance. Its unique three-dimensional hierarchical porous structure realizes the gradient matching of micropore-mesopore-macroporous structure, which not only optimizes the transport kinetics of electrolyte ions, but also significantly expands the electrode / electrolyte interface reaction space through the coupling of multi-scale pores. The regularly arranged micron-scale pore structure in Example 3 (CW-H-6) forms a three-dimensional continuous electron conduction network. The uniformly loaded nano-carbon spheres promote the efficient transfer of electrolyte ions by enhancing the contact area between the electrode and the electrolyte on the one hand, and on the other hand, improve the space utilization of self-supporting capacitor carbon, so that Example 3 (CW-H-6) exhibits a higher area specific capacitance at different current densities.
[0104] like Figure 9 As shown, the CV curve of Example 3 (CW-H-6) always shows a typical quasi-rectangular profile of double-layer capacitance characteristics in different scan rate ranges. Its highly symmetrical geometry indicates that the electrode has ideal charge storage kinetics. Figure 10 As shown, at different current densities, the GCD curves of Example 3 (CW-H-6) all show a highly symmetrical isosceles triangle, and with the increase of current density, the IR drop only increases slightly. It is worth noting that even under high current density conditions, Example 3 (CW-H-6) still has a relatively high area specific capacitance. In addition, the rate performance of Example 3 (CW-H-6) is significantly better than that of the self-supporting capacitor carbon prepared by the traditional carbonization / activation process. The synergistic regulation strategy of potassium bicarbonate activation and secondary deposition of carbon source effectively enhances the charge transfer efficiency of the electrode / electrolyte interface by precisely constructing a three-dimensional pore structure and a hierarchical pore structure modified by nano-carbon balls, significantly improves the space utilization of the self-supporting capacitor carbon, and thus achieves a comprehensive improvement in the electrochemical performance of the self-supporting capacitor carbon.
[0105] In order to systematically evaluate the practical application potential of self-supporting composite capacitor carbon modified with nano-carbon balls, this application uses Example 3 (CW-H-6) as the electrode, cellulose membrane as the diaphragm, and KOH solution with a concentration of 6 mol / L as the electrolyte to construct a symmetrical supercapacitor (CW-H-6 / / CW-H-6).
[0106] like Figure 11 As shown in the figure, CW-H-6 / / CW-H-6 exhibits a rectangular CV curve morphology within different scan rate ranges, which is consistent with the electrochemical response characteristics of Example 3 (CW-H-6) in the three-electrode system, fully confirming the effective continuation of the double-layer energy storage mechanism at the device level.
[0107] like Figure 12As shown, constant-current charge-discharge tests further reveal the excellent electrochemical performance of CW-H-6 / / CW-H-6. The electrodes exhibit highly symmetrical isosceles triangles at various current densities, and their Coulombic efficiency remains near 100% as current density increases. The nano-carbon sphere modification layer, constructed by potassium bicarbonate activation and secondary carbon source deposition, optimizes the charge transfer pathway at the electrode / electrolyte interface. The synergistic effect of the hierarchical porous structure effectively suppresses polarization at high current densities, promoting the enhanced electrochemical performance of CW-H-6 / / CW-H-6.
[0108] Thanks to the synergistic construction of the three-dimensional conductive network modified with nanocarbon balls and the hierarchical porous structure in Example 3 (CW-H-6), the symmetrical supercapacitor assembled based on Example 3 (CW-H-6) exhibits excellent area-specific capacitance.
[0109] like Figure 13 As shown, CW-H-6 / / CW-H-6 at current density of 2mA / cm 2 , 5mA / cm 2 , 10mA / cm 2 , 20mA / cm 2 、30mA / cm 2 , 50mA / cm 2 and 100mA / cm 2 The area specific capacitance is 1.70F / cm 2 , 1.59F / cm 2 , 1.47F / cm 2 , 1.33F / cm 2 , 1.21F / cm 2 , 1.02F / cm 2 and 0.78F / cm 2 It exhibits good rate characteristics in a wide current density range.
[0110] Figure 14 The Ragone plot further reveals the excellent energy storage properties of CW-H-6 / / CW-H-6. 2 At the power density of CW-H-6 / / CW-H-6, the energy density can reach 148.61μWh / cm 2 Even if the power density is increased to 25mW / cm 2 , CW-H-6 / / CW-H-6 can still maintain 76.39μWh / cm 2 energy density, showing comprehensive advantages in energy density, power density and rate performance.
[0111] The charge-discharge cycle stability of CW-H-6 / / CW-H-6 is as follows Figure 15As shown in the figure, after 8,000 charge and discharge cycles, the capacity retention rate of CW-H-6 / / CW-H-6 is as high as 107.3%. Example 3 (CW-H-6) loaded with nanocarbon balls has a complex hierarchical porous structure. At the beginning of the charge and discharge cycle, the electrolyte fails to fully flow into the three-dimensional pore structure of the self-supporting capacitor carbon. As the charge and discharge cycle proceeds, the partially closed pores gradually open, which increases the effective specific surface area of Example 3 (CW-H-6), causing the capacity of CW-H-6 / / CW-H-6 to show an upward trend at the beginning of the cycle. As the number of cycles increases, the capacity retention rate of CW-H-6 / / CW-H-6 gradually remains stable.
[0112] In summary, Example 3 (CW-H-6) developed a carbon source secondary deposition technology of hydrothermal carbonization coupled with thermochemical conversion, constructed a nano-carbon sphere-modified biomass monolithic composite porous carbon, and significantly improved the space utilization of the biomass monolithic carbon electrode. The electrode has excellent electrochemical properties, and the symmetrical supercapacitor constructed by the electrode has excellent energy density, rate performance and cycle stability. The nano-carbon sphere-modified biomass monolithic composite porous carbon proposed in the present invention is of great value in promoting the application of high-performance supercapacitors.
[0113] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention are intended to be within the scope of protection of the present invention.
Claims
1. A method for preparing a biomass monolithic composite porous carbon modified with nanocarbon balls, characterized in that: The following steps are involved: S1. The pine wood is cut into pine chips along the growth direction and then placed in a blast drying oven for drying. The dried pine chips are placed in a nitrogen atmosphere tube furnace for high-temperature carbonization to obtain a carbonized product. S2. The carbonized product was immersed in a hydrochloric acid solution to remove inorganic salt impurities, and then rinsed with deionized water to a neutral pH value. The rinsed carbonized product was transferred to a drying oven for dehydration and then polished to a thickness of 0.6-1.2 mm to obtain CW-1 composite porous carbon; S3. The CW-1 composite porous carbon was placed in a glucose solution for vacuum-assisted impregnation and then transferred to a hydrothermal reactor for hydrothermal carbonization to obtain a hydrothermal carbonized product. The hydrothermal carbonized product was dried in an oven and placed in a tubular furnace in a nitrogen atmosphere for constant temperature chemical conversion to obtain CW-H composite porous carbon; S4. The CW-H composite porous carbon is placed in a potassium bicarbonate solution for vacuum impregnation and then transferred to a drying oven for dehydration. The carbonized product is then placed in a tubular furnace in a nitrogen atmosphere for constant-temperature chemical conversion to obtain a converted carbonized product. The converted carbonized product is immersed in hydrochloric acid to remove inorganic salt impurities, then rinsed with deionized water to a neutral pH value, and then dried in a drying oven to obtain CW-H-6 composite porous carbon.
2. The method for preparing nanocarbon ball-modified biomass monolithic composite porous carbon according to claim 1, characterized in that: During the drying process of the pine wood chips in step S1, a briquette is placed on top of the pine wood chips. The temperature of the blast drying oven during the drying process is 60° C. and the drying time is 12 hours. The gas flow rate in the nitrogen atmosphere tube furnace in step S1 is 200-400 mL / min, and the temperature in the tube furnace is increased to 600-1000° C. at a heating rate of 5-20° C. / min after starting operation and then maintained at high temperature for 60-180 minutes.
3. The method for preparing nanocarbon ball-modified biomass monolithic composite porous carbon according to claim 1, characterized in that: The concentration of the hydrochloric acid solution in step S2 is 1 mol / L; The temperature of the carbonized product in step S2 in the drying oven is 105° C., and the dehydration treatment time is 12 hours.
4. The method for preparing nanocarbon ball-modified biomass monolithic composite porous carbon according to claim 1, characterized in that: The concentration of the glucose solution in step S3 is 10 g / 100 mL, the vacuum impregnation time of the CW-1 composite porous carbon in the glucose solution is 30 min, the reaction temperature of the hydrothermal reactor is 180° C., and the hydrothermal reaction time is 8 h; The temperature of the hydrothermal carbide in the oven is 105°C, the drying time is 12 hours, the gas flow rate in the nitrogen atmosphere tube furnace in step S3 is 200-600 mL / min, and the temperature in the tube furnace is heated to 600-900°C at a heating rate of 5-20°C / min after starting work and then maintained at high temperature for carbonization for 60-180 minutes.
5. The method for preparing nanocarbon ball-modified biomass monolithic composite porous carbon according to claim 1, characterized in that: The concentration of the potassium bicarbonate solution in step S4 is 6 g / 100 mL, the vacuum impregnation time of the CW-H composite porous carbon in the potassium bicarbonate solution is 30 min, the drying temperature in the drying oven is 105° C., and the drying time is 12 h; The gas flow rate in the nitrogen atmosphere tube furnace in step S4 is 200-600 mL / min, and the temperature in the tube furnace is increased to 600-900° C. at a heating rate of 5-20° C. / min after starting operation and then maintained at high temperature for 60-180 minutes.
6. The method for preparing a nanocarbon ball-modified biomass monolithic composite porous carbon according to claim 1, characterized in that: The concentration of the hydrochloric acid solution in step S4 is 0.1-3 mol / L, and the converted carbonized product is immersed in the hydrochloric acid solution for 12 hours, then rinsed with deionized water to a neutral pH value, and then dried in a drying oven at 105° C. for 12 hours.
7. The method for preparing nanocarbon ball-modified biomass monolithic composite porous carbon according to claim 2, characterized in that: In the step S1, the temperature in the nitrogen atmosphere tube furnace is raised to 900° C. at a heating rate of 10° C. / min after starting operation, and then the temperature is maintained for high-temperature carbonization for 120 minutes, and the polishing thickness is 1 mm.
8. The method for preparing the nano-carbon sphere-modified biomass monolithic composite porous carbon according to claim 4, characterized in that: In step S3, the temperature in the nitrogen atmosphere tube furnace is raised to 800° C. at a heating rate of 10° C. / min after starting operation, and then the temperature is maintained for high-temperature carbonization for 120 minutes; In step S4, the temperature in the nitrogen atmosphere tube furnace is raised to 800° C. at a heating rate of 10° C. / min after starting operation and then maintained at the high temperature for carbonization for 120 minutes. The concentration of the hydrochloric acid solution is 1 mol / L.
9. A nanocarbon ball modified biomass monolithic composite porous carbon, characterized in that: The composite porous carbon obtained by the preparation method according to any one of claims 1 to 8 has a specific surface area of 277.2 m 2 / g, the diameter of the nano-carbon balls is 200-300nm, and the nano-carbon balls are evenly distributed on the surface and inner wall of the pores of the monolithic composite porous carbon.
10. Application of a method for preparing a biomass monolithic composite porous carbon modified with nanocarbon balls, characterized in that: According to the application of the composite porous carbon obtained by the preparation method according to any one of claims 1 to 8 in the field of capacitors, the composite porous carbon does not require a conductive agent, a binder and a current collector, and can be directly used as an electrode of a supercapacitor.
Citation Information
Cited By
Resin carbon microsphere aperture regulation and control method and microporous resin carbon microsphere
CN122166762A