High-transparency easy-to-open linear low-density polyethylene and preparation process thereof
By adding silica and erucamide to the composite, combined with silane coupling agents and ultraviolet absorbers, the problems of insufficient transparency and opening properties of polyethylene film are solved, achieving a high transparency and easy opening effect.
Patent Information
- Application Number
- CN202511366425.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-24
- Publication Date
- 2025-12-05
AI Technical Summary
Existing polyethylene films exhibit reduced transparency and a high coefficient of friction after the addition of inorganic opening agents, making it difficult to achieve both excellent opening properties and transparency.
Silica and erucamide were added in a composite form, and silane coupling agents and epoxy groups were used to improve dispersibility. 2-hydroxy-4-n-octyloxybenzophenone was combined to stabilize ultraviolet absorption, and the 1-butene content and extrusion granulation parameters in the ethylene-butene copolymer were adjusted.
It improves the transparency and opening properties of polyethylene film, reduces the coefficient of friction, achieves a light transmittance of over 92%, haze ≤15%, and static friction coefficient ≤0.15.
Smart Images

Figure SMS_1
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of functional polyethylene, more particularly, it relates to a high-transparency easy-opening linear low-density polyethylene and a preparation process thereof. BACKGROUND
[0002] Linear low-density polyethylene is a thermoplastic plastic copolymerized by ethylene and a small amount of alpha-olefin under low pressure, and its molecular structure is linear with short and uniform distribution of branches, and it has the flexibility of low-density polyethylene (LDPE) and the strength of high-density polyethylene (HDPE), and has good tensile property, impact resistance, puncture resistance and chemical corrosion resistance, and is mainly used for producing films, pipes, injection molded products, etc., and is widely used in packaging, agriculture, chemical industry, daily necessities, etc.
[0003] In the production of blown films, inorganic opening agents are usually added to improve the opening property of polyethylene films, however, when excessive inorganic opening agents are dispersed in the polyethylene film, a large number of uneven structures will be generated on the surface of the film, and the structures are easy to scatter incident light, so that the light cannot penetrate the film along the original path, thereby causing the transparency of the film to decrease significantly. Moreover, the film with only inorganic opening agents added still has a relatively large friction coefficient during use, which affects the packaging efficiency. SUMMARY
[0004] In order to improve the defects that polyethylene films cannot have excellent opening property and transparency, the present application provides a high-transparency easy-opening linear low-density polyethylene and a preparation process thereof.
[0005] In a first aspect, the present application provides a high-transparency easy-opening linear low-density polyethylene, which adopts the following technical solution: The high-transparency easy-opening linear low-density polyethylene comprises the following raw materials: linear low-density polyethylene, antioxidant, ultraviolet absorber, acid absorber, antistatic agent, opening agent and slip agent, the opening agent is silicon dioxide, the slip agent is erucic acid amide, the ultraviolet absorber is 2-hydroxy-4-n-octyloxybenzophenone, the opening agent, slip agent and ultraviolet absorber are added in the form of a complex, and a silane coupling agent is added in the complex, and the silane coupling agent contains an epoxy group.
[0006] Compared with the inorganic opening agent silicon dioxide, the organic slip agent erucic acid amide has better compatibility with polyethylene and is more uniformly dispersed, thereby promoting the polyethylene film to have relatively better transparency, but the long-term effect is poor, and when the silicon dioxide and erucic acid amide are added in the form of a complex, the complex has the long-term effect of silicon dioxide and the high transparency of erucic acid amide, thereby promoting the polyethylene film to have better opening property and transparency.
[0007] In addition, the inorganic opening agent, silica, has the defect of easy agglomeration, which further reduces the transparency of the polyethylene film, and the erucamide has a large number of unsaturated double bonds, which is easy to be oxidized in the light environment, thereby generating a chromophore group, which indirectly reduces the transparency of the polyethylene film.
[0008] When the silane coupling agent is added to the composite, and the silane coupling agent contains an epoxy group, the silane coupling agent will effectively improve the dispersibility of the silica through coupling, which indirectly improves the transparency of the polyethylene film. In addition, the ultraviolet absorber is selected as 2-hydroxy-4-n-octyloxybenzophenone, so that the epoxy group connects the ultraviolet absorber to the silica through the epoxy ring-opening mechanism. Compared with the separate addition of the ultraviolet absorber, the way of connecting the ultraviolet absorber to the silica can more stably and accurately act on the erucamide, further reducing the possibility of oxidation of the erucamide, and indirectly improving the transparency of the polyethylene film.
[0009] Preferably, the silane coupling agent further contains a long-chain alkyl group.
[0010] The lubrication mechanism of erucamide is that erucamide can migrate on the surface of the polyethylene film and form a lubricating film, thereby reducing the friction coefficient of the polyethylene film and reducing the interfacial adhesion. However, if too much erucamide migrates out, a blooming phenomenon will occur on the surface of the polyethylene film, which will affect the transparency of the polyethylene film. When the silane coupling agent contains a long-chain alkyl group, the long-chain alkyl group will be compatible with the long carbon chain of erucamide, slightly limiting the migration of erucamide, without affecting the lubrication effect of erucamide, while effectively inhibiting the occurrence of the blooming phenomenon, and indirectly improving the transparency of the polyethylene film.
[0011] Preferably, the silane coupling agent is a mixture of dodecyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane, and the molar ratio of the dodecyltrimethoxysilane to the γ-glycidoxypropyltrimethoxysilane is (1-2):(1-2).
[0012] When the molar ratio of the dodecyltrimethoxysilane to the γ-glycidoxypropyltrimethoxysilane is as described above, the silane coupling agent will limit the movement of the ultraviolet absorber and the erucamide with a suitable locking effect, thereby enabling the ultraviolet absorber to accurately act on the erucamide, and limiting the migration speed of the erucamide, which indirectly improves the transparency of the polyethylene film.
[0013] Preferably, the mass ratio of the γ-glycidoxypropyltrimethoxysilane to the silica is 1:(4-6).
[0014] Preferably, the content of the silica is 1500-2500 ppm, the content of the erucamide is 500-1500 ppm, the content of the 2-hydroxy-4-n-octyloxybenzophenone is 300-700 ppm, the content of the acid absorbent is 400-800 ppm, and the content of the antistatic agent is 500-700 ppm by mass of the linear low density polyethylene.
[0015] Preferably, the low density polyethylene is an ethylene-butene copolymer, and the content of 1-butene in the ethylene-butene copolymer is ≤10%; and / or the particle size of the silica is 3-5 μm; and / or the particle size of the erucamide is 1-3 μm; and / or the antioxidant is a mixture of a primary antioxidant and a secondary antioxidant, the primary antioxidant is AO-3, the secondary antioxidant is PS-2, and the content ratio of the primary antioxidant to the secondary antioxidant is 1: (1-3).
[0016] By adjusting the content of 1-butene in the ethylene-butene copolymer to be ≤10%, a stable resin powder intermediate product is obtained, and the product has good transparency, haze ≤15%, and the nominal strain at break is increased to ≥500%, which exceeds the national standard requirement of ≥200%.
[0017] By optimizing the addition ratio of the additives, selecting an opening agent with a particle size of 4 μm and a content of 2000 ppm, and a slip agent with a particle size of 2 μm and a content of 1000 ppm, the crystallinity of the polyethylene during the film cooling process is reduced, the static friction coefficient of the polyethylene film is ≤0.15, the dynamic friction coefficient is ≤0.12, and the light transmittance is ≥92%.
[0018] Preferably, the preparation method of the composite includes the following steps: S1, first, uniformly mix dodecyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane and silica, add distilled water and ball mill in a ball mill for 1-3 h, and then place in a vacuum environment at 70-90°C for 6-10 h to obtain modified silica; S2, mix the modified silica with 2-hydroxy-4-n-octyloxybenzophenone, then add aluminum chloride, ball mill in a ball mill for 1-2 h, then add erucamide and continue ball milling for 1-2 h, and finally dry to obtain the composite.
[0019] In the second aspect, the application provides a preparation method of high-transparency easy-opening linear low density polyethylene, which adopts the following technical scheme: The application discloses a preparation method of high-transparency easy-opening linear low-density polyethylene, which comprises the following steps: firstly, mixing linear low-density polyethylene, an acid absorbent, an antioxidant, an antistatic agent and a complex, and then adding the mixture into an extrusion granulator to perform extrusion granulation, so as to obtain the high-transparency easy-opening linear low-density polyethylene.
[0020] Preferably, in the extrusion granulation process, the melt temperature is controlled to be 200±5 DEG C, the extruder rotating speed is controlled to be 240±5 rpm, and the cooling water temperature is controlled to be 58 DEG C.
[0021] By adjusting the process parameters of the extrusion granulation unit, the melt temperature is controlled to be 200±5 DEG C, the extruder rotating speed is controlled to be 240±5 rpm, and the cooling water temperature is controlled to be 58 DEG C, so that the granular product is ensured to have the black spot granules less than 5 per kg, the snake skin and tailing granules less than 10 per kg, and the product appearance quality is improved.
[0022] In conclusion, the application has the following beneficial effects: 1. When the complex is added with the silane coupling agent, and the silane coupling agent contains an epoxy group, the silane coupling agent can effectively improve the dispersibility of the silicon dioxide through coupling effect, and indirectly improve the transparency of the polyethylene film. In addition, the ultraviolet absorber is selected as 2-hydroxy-4-n-octyloxybenzophenone, so that the epoxy group connects the ultraviolet absorber to the silicon dioxide through an epoxy ring-opening mechanism. Compared with the ultraviolet absorber added alone, the way of connecting the ultraviolet absorber to the silicon dioxide can more stably and accurately act on the erucamide, further reduces the possibility of oxidation of the erucamide, and indirectly improves the transparency of the polyethylene film.
[0023] 2. When the silane coupling agent contains a long-chain alkyl group, the long-chain alkyl group is compatible with the long carbon chain of the erucamide, slightly limits the migration of the erucamide, does not affect the lubricating effect of the erucamide, effectively inhibits the generation of the blooming phenomenon, and indirectly improves the transparency of the polyethylene film.
[0024] 3. By adjusting the content of 1-butene in the ethylene-butene copolymer to be less than or equal to 10%, a stable resin powder intermediate product is obtained, and the main antioxidant, the auxiliary antioxidant, the acid absorbent, the antistatic agent, the opening agent and the slip agent are mixed and extrusion granulated, so that the product has good transparency, haze less than or equal to 15%, static friction coefficient less than or equal to 0.15, dynamic friction coefficient less than or equal to 0.12, and light transmittance greater than or equal to 92%. DETAILED DESCRIPTION
[0025] The application will be further described in detail in combination with Examples 1-8 and Comparative Examples 1-2.
[0026] Raw materials Low density polyethylene Ethylene-butene copolymer 1-butene content ≤10% Dow Chemical; UV absorber 2-hydroxy-4-n-octyloxybenzophenone CAS: 1843-05-6; acid absorber Zinc stearate CAS: 557-05-1; antistatic agent Octadecyldiethanolamine CAS: 10213-78-2; opening agent Silicon dioxide Particle size 4 μm; slip agent Erucamide Particle size 2 μm; Dodecyltrimethoxysilane CAS: 3069-21-4; Gamma-glycidoxypropyltrimethoxysilane CAS: 2530-83-8; Vinyltrimethoxysilane CAS: 2768-02-7; AO-3 CAS: 2082-79-3; PS-2 CAS: 31570-04-4.
[0027] Example 1 A high-transparency easy-opening linear low density polyethylene, comprising the following raw materials: linear low density polyethylene, antioxidant, UV absorber, acid absorber, antistatic agent, opening agent and slip agent, the UV absorber is 2-hydroxy-4-n-octyloxybenzophenone, the acid absorber is zinc stearate, the opening agent is silicon dioxide, and the slip agent is erucamide.
[0028] The content of silicon dioxide is 2000 ppm, the content of erucamide is 1000 ppm, the content of 2-hydroxy-4-n-octyloxybenzophenone is 500 ppm, the content of acid absorber is 600 ppm, the content of antistatic agent is 600 ppm, and the content of antioxidant is 1000 ppm, based on the mass of linear low density polyethylene.
[0029] The antioxidant is a mixture of primary antioxidant and secondary antioxidant, the primary antioxidant is AO-3, the secondary antioxidant is PS-2, and the content ratio of the primary antioxidant to the secondary antioxidant is 1:2.
[0030] The opening agent, the slip agent and the UV absorber are added in the form of a composite, and a silane coupling agent is added in the composite, the silane coupling agent is a mixture of dodecyltrimethoxysilane and gamma-glycidoxypropyltrimethoxysilane, the molar ratio of the dodecyltrimethoxysilane to the gamma-glycidoxypropyltrimethoxysilane is 1:1, and the mass ratio of the gamma-glycidoxypropyltrimethoxysilane to the silicon dioxide is 1:5.
[0031] The preparation method of the composite comprises the following steps: S1, first, the dodecyltrimethoxysilane, the gamma-glycidoxypropyltrimethoxysilane and the silicon dioxide are uniformly mixed, 1 / 5 of the mass of the silicon dioxide is added with distilled water and ball milled in a ball mill for 2 h, and then placed in a vacuum environment at 80°C for 8 h to obtain modified silicon dioxide; S2, the modified silicon dioxide is mixed with 2-hydroxy-4-n-octyloxybenzophenone, then 1wt% aluminum chloride is added, after ball milling in a ball mill for 2h, erucamide is added and ball milling is continued for 2h, and finally drying to obtain the composite.
[0032] The preparation method of the high-transparency easy-opening linear low-density polyethylene is: first, mixing linear low-density polyethylene, acid absorbent, antistatic agent and composite, then adding to the extrusion granulator for extrusion granulation to obtain high-transparency easy-opening linear low-density polyethylene; wherein, in the extrusion granulation process, the melt temperature is controlled at 200±5℃, the extruder speed is controlled at 240±5rpm, and the cooling water temperature is controlled at 58℃.
[0033] Example 2 The difference from Example 1 is that the silane coupling agent is only γ-glycidoxypropyltrimethoxysilane.
[0034] Example 3 The difference from Example 1 is that the silane coupling agent is only dodecyltrimethoxysilane.
[0035] Example 4 The difference from Example 1 is that the silane coupling agent is vinyltrimethoxysilane.
[0036] Example 5 The difference from Example 1 is that the molar ratio of dodecyltrimethoxysilane to γ-glycidoxypropyltrimethoxysilane is 1:2.
[0037] Example 6 The difference from Example 1 is that the molar ratio of dodecyltrimethoxysilane to γ-glycidoxypropyltrimethoxysilane is 2:1.
[0038] Example 7 The difference from Example 1 is that the content of silicon dioxide is 1500ppm and the content of erucamide is 1500ppm based on the mass of linear low-density polyethylene.
[0039] Example 8 The difference from Example 1 is that the content of silicon dioxide is 2500ppm and the content of erucamide is 500ppm based on the mass of linear low-density polyethylene.
[0040] Comparative Example 1 The difference from Example 1 is that no silane coupling agent is added in the composite.
[0041] Comparative Example 2 The difference between the comparative example 1 is that the preparation method of the high transparent easy opening linear low density polyethylene is that the linear low density polyethylene, antioxidant, ultraviolet absorber, acid absorber, antistatic agent, opening agent and slip agent are first mixed, and then added to the extrusion granulator for extrusion granulation to obtain the high transparent easy opening linear low density polyethylene; wherein in the extrusion granulation process, the melt temperature is controlled at 200±5℃, the extruder speed is controlled at 240±5rpm, and the cooling water temperature is controlled at 58℃.
[0042] Performance test I. Transmittance test Three samples were taken from each of the examples 1-8 and the comparative examples 1-2, placed in a light environment for 10 days, and then blown into a specified specification film according to GB / T 2410-2008 “Determination of Transmittance and Haze of Transparent Plastics” and tested for transmittance, and the test data was averaged.
[0043] II. Dynamic friction coefficient test Three samples were taken from each of the examples 1-8 and the comparative examples 1-2, and then blown into a specified specification film according to GB / T 10006-2021 “Determination of Friction Coefficient of Plastic Film and Sheet” and tested for dynamic friction coefficient, and the test data was averaged.
[0044] The test data is shown in Table 1.
[0045] Table 1 Test data table of examples 1-8 and comparative examples 1-2
[0046] According to the comparative examples 1 and 2 and in combination with Table 1, it can be seen that the transmittance of the comparative example 1 is slightly improved, and the dynamic friction coefficient of the comparative example 1 is slightly decreased, which shows that the addition of the ultraviolet absorber, the opening agent and the slip agent in the form of a complex can further improve the transparency and opening performance of the polyethylene film.
[0047] The reason may be that the organic slip agent erucic acid amide has better compatibility with polyethylene and is more uniformly dispersed compared with the inorganic opening agent silicon dioxide, thereby promoting the polyethylene film to have relatively better transparency, but the long-term performance is poor, and when the silicon dioxide and the erucic acid amide are added in the form of a complex, the complex will have the long-term performance of the silicon dioxide and the high transparency of the erucic acid amide, thereby promoting the polyethylene film to have better opening performance and transparency.
[0048] Referring to Examples 1-4 and Comparative Example 1 and Table 1, it can be seen that the light transmittance of Examples 1-4 is obviously improved and the dynamic friction coefficient of Examples 1-4 is obviously decreased compared with Comparative Example 1, which indicates that the presence of the silane coupling agent can further improve the opening property and transparency of the polyethylene film.
[0049] The reason may be that the inorganic opening agent, silica, has the defect of easy agglomeration, which further reduces the transparency of the polyethylene film, and when the composite is added with the silane coupling agent, The silane coupling agent can effectively improve the dispersibility of silica through coupling, thereby indirectly improving the transparency of the polyethylene film.
[0050] Referring to Examples 1-4 and Table 1, it can be seen that the light transmittance and dynamic friction coefficient of Example 2 are slightly decreased compared with Example 1, which indicates that the use of only γ-glycidoxypropyltrimethoxysilane can effectively improve the opening property of the polyethylene film, but also reduces the light transmittance of the polyethylene film.
[0051] The reason may be that the lubrication mechanism of erucic acid amide is that it can migrate on the surface of the polyethylene film and form a lubricating film, thereby reducing the friction coefficient of the polyethylene film and reducing the interfacial adhesion, but if too much erucic acid amide migrates out, a blooming phenomenon will occur on the surface of the polyethylene film, thereby affecting the transparency of the polyethylene film. The long-chain alkyl group of dodecyltrimethoxysilane can be compatible with the long carbon chain of erucic acid amide, slightly limiting the migration of erucic acid amide, without significantly affecting the lubrication effect of erucic acid amide, while effectively inhibiting the occurrence of the blooming phenomenon, thereby indirectly improving the transparency of the polyethylene film.
[0052] Compared with Example 1, the light transmittance of Example 3 is slightly decreased and the dynamic friction coefficient of Example 3 is obviously increased, which indicates that the use of only dodecyltrimethoxysilane will obviously reduce the light transmittance and opening property of the polyethylene film.
[0053] The reason may be that the long-chain alkyl group of dodecyltrimethoxysilane can be compatible with the long carbon chain of erucic acid amide, and excessive dodecyltrimethoxysilane will obviously limit the migration of erucic acid amide, thereby affecting the opening property of the polyethylene film. In addition, erucic acid amide has a large number of unsaturated double bonds, which can easily be oxidized under light, thereby generating a chromophore group, which indirectly reduces the transparency of the polyethylene film.
[0054] And the epoxy group on the γ-glycidoxypropyltrimethoxysilane can connect the ultraviolet absorber 2-hydroxy-4-n-octyloxybenzophenone to the silica through an epoxy ring-opening mechanism. Compared with adding the ultraviolet absorber alone, connecting the ultraviolet absorber to the silica can more stably and accurately act on the erucamide, further reducing the possibility of oxidation of the erucamide, and indirectly improving the transparency of the polyethylene film.
[0055] Compared with examples 1-3, example 4 has a higher dynamic friction coefficient, but the lowest light transmittance. The reason is that the vinyltrimethoxysilane has no limiting effect on the movement of erucamide, but also has no locking effect on 2-hydroxy-4-n-octyloxybenzophenone.
[0056] Referring to examples 1, 5-6 and combining table 1, it can be seen that compared with example 1, the light transmittance of examples 5-6 is slightly decreased, which indicates that when the molar ratio of dodecyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane is used in example 1, the prepared polyethylene film will have more excellent light transmittance.
[0057] Referring to examples 1, 7-8 and combining table 1, it can be seen that compared with example 1, the light transmittance of examples 7-8 is significantly reduced, and the dynamic friction coefficient of examples 7-8 is significantly improved, which indicates that when the content of silica and erucamide is used in example 1, the prepared polyethylene film will have more excellent transparency and opening performance.
[0058] In addition, in this application, by adjusting the content of 1-butene in the ethylene-butene copolymer to be ≤10%, a stable performance resin powder intermediate product is obtained, and mixed with the main antioxidant, auxiliary antioxidant, acid absorbent, antistatic agent, opening agent and slip agent to extrude and granulate, so that the product has good transparency, haze ≤15%, and the nominal strain at break is increased to ≥500%, which exceeds the national standard requirement of ≥200%.
[0059] By optimizing the addition ratio of the additives, selecting a particle size of 4 μm, and an opening agent content of 2000 ppm; and a particle size of 2 μm, and a slip agent content of 1000 ppm, the crystallinity of polyethylene during film forming and cooling process is reduced, the static friction coefficient of the polyethylene film is ≤0.15, the dynamic friction coefficient is ≤0.12, and the light transmittance is ≥92%.
[0060] By adjusting the process parameters of the extrusion granulation unit: the melt temperature is controlled at 200±5℃, the extruder speed is controlled at 240±5rpm, and the cooling water temperature is controlled at 58℃. Ensure that the output granular product has ≤5 black spot particles / kg, ≤10 snake skin and tail particles / kg, and improve the appearance quality of the product.
[0061] The specific embodiments are only an explanation of the present application, which is not a limitation of the present application, and those skilled in the art can make modifications to the embodiments without creative contribution after reading the specification, but as long as it is within the scope of the claims of the present application, it is protected by the patent law.
Claims
1. A highly transparent, easy-to-open linear low-density polyethylene, characterized in that, The product comprises the following raw materials: linear low-density polyethylene, antioxidant, ultraviolet absorber, acid absorber, antistatic agent, opening agent, and slip agent. The opening agent is silica, the slip agent is erucamide, and the ultraviolet absorber is 2-hydroxy-4-n-octyloxybenzophenone. The opening agent, slip agent, and ultraviolet absorber are added in the form of a composite, and a silane coupling agent is added to the composite. The silane coupling agent contains epoxy groups.
2. The high-transparency, easy-opening linear low-density polyethylene according to claim 1, characterized in that: The silane coupling agent also contains long-chain alkyl groups.
3. The high-transparency, easy-opening linear low-density polyethylene according to claim 2, characterized in that: The silane coupling agent is a mixture of dodecyltrimethoxysilane and γ-glycidyl etherpropyltrimethoxysilane, wherein the molar ratio of dodecyltrimethoxysilane to γ-glycidyl etherpropyltrimethoxysilane is (1-2):(1-2).
4. The high-transparency, easy-opening linear low-density polyethylene according to claim 3, characterized in that: The mass ratio of γ-glycidyl ether propyltrimethoxysilane to silicon dioxide is 1:(4-6).
5. The high-transparency, easy-opening linear low-density polyethylene according to claim 1, characterized in that: Based on the mass of the linear low-density polyethylene, the content of silica is 1500-2500 ppm, the content of erucamide is 500-1500 ppm, the content of 2-hydroxy-4-n-octyloxybenzophenone is 300-700 ppm, the content of antioxidant is 500-1500 ppm, the content of acid absorber is 400-800 ppm, and the content of antistatic agent is 500-700 ppm.
6. The high-transparency, easy-opening linear low-density polyethylene according to claim 1, characterized in that: The low-density polyethylene is an ethylene-butene copolymer, and the 1-butene content in the ethylene-butene copolymer is ≤10%; And / or the particle size of the silica is 3-5 μm; And / or the particle size of the erucamide is 1-3 μm; And / or the antioxidant is a mixture of a primary antioxidant and a secondary antioxidant, wherein the primary antioxidant is AO-3, the secondary antioxidant is PS-2, and the content ratio of the primary antioxidant to the secondary antioxidant is 1:(1-3).
7. The high-transparency, easy-opening linear low-density polyethylene according to claim 3, characterized in that, The method for preparing the composite includes the following steps: S1. First, dodecyltrimethoxysilane, γ-glycidyl ether propyltrimethoxysilane and silica are uniformly mixed, then distilled water is added and the mixture is ball-milled in a ball mill for 1-3 hours. Then, it is placed in a vacuum environment of 70-90℃ for 6-10 hours to obtain modified silica. S2. Modified silica is mixed with 2-hydroxy-4-n-octyloxybenzophenone, followed by the addition of aluminum chloride. The mixture is ball-milled for 1-2 hours, then erucamide is added and the mixture is ball-milled for another 1-2 hours. Finally, the mixture is dried to obtain the composite.
8. A preparation process for high-transparency, easy-opening linear low-density polyethylene according to any one of claims 1-7, characterized in that, The steps are as follows: First, linear low-density polyethylene, acid absorber, antioxidant, antistatic agent and composite are mixed, and then added to an extrusion granulator for extrusion granulation to obtain high-transparency, easy-opening linear low-density polyethylene.
9. The preparation process of high-transparency, easy-opening linear low-density polyethylene according to claim 8, characterized in that: In the extrusion granulation process, the melt temperature is controlled at 200±5℃, the extruder speed is controlled at 240±5rpm, and the cooling water temperature is controlled at 58℃.
Citation Information
Patent Citations
Modified linear polyethylene resin and preparation method thereof
CN102952326A
Preparation method of aerogel film lubricant
CN109705402A
Opening-smoothing composite polyethylene resin
CN109851887A
Open extrusion-assisting master batch for heavy packaging film and preparation method of open extrusion-assisting master batch
CN117659555A