Electrolyte additive, electrolyte, preparation method of electrolyte and aluminum air battery

By using peroxides, persulfates, or iodates as electrolyte additives in aluminum-air batteries, the oxygen reduction reaction is promoted, solving the problem of slow cathode reaction rate and achieving improved power density and discharge performance of aluminum-air batteries.

CN121076345APending Publication Date: 2025-12-05SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511243813.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-09-02
Publication Date
2025-12-05

AI Technical Summary

Technical Problem

The slow kinetics of the oxygen reduction reaction at the cathode in aluminum-air batteries result in low power density, and the existing catalysts have complex synthesis steps that make mass production difficult.

Method used

Peroxides, persulfates, or iodates are used as electrolyte additives to prepare alkaline or neutral electrolytes, which promote oxygen reduction reaction kinetics and increase the cathode reaction rate.

Benefits of technology

It significantly improves the power density of aluminum-air batteries, the catalyst is simple and easy to prepare, and the discharge performance and stability of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121076345A_ABST
    Figure CN121076345A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, in particular to an electrolyte additive, an electrolyte, a preparation method of the electrolyte and an aluminum air battery, and the electrolyte additive comprises peroxide, persulfate or iodate. The concentration of the peroxide ranges from 0.01 mol / L to 0.6 mol / L, the concentration of the persulfate ranges from 0.01 mol / L to 1 mol / L, and the concentration of the iodate ranges from 0.01 mol / L to 1 mol / L; the electrolyte additive peroxide, persulfate and iodate provided by the invention have relatively strong oxidability, and after the electrolyte additive peroxide, persulfate and iodate are added into an alkaline electrolyte or a neutral electrolyte, the peroxide, persulfate and iodate are simultaneously reduced besides oxygen is reduced at an air cathode in a discharge process, so that a cathode depolarization process is accelerated, and the discharge efficiency is improved. And the dynamic reaction speed of the cathode is increased, so that the power density of the aluminum-air battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of battery materials, and particularly relates to an electrolyte additive, an electrolyte, a preparation method thereof and an aluminum-air battery. BACKGROUND

[0002] The aluminum-air battery is a new energy technology, which generates electricity by the reaction of aluminum and oxygen in the air. This battery has the advantages of high energy density and low cost, and is considered as a potential alternative for renewable energy in the future.

[0003] However, the aluminum-air battery generally has relatively low power density, which limits its commercial application field to some extent. The main reason for the low power density of the aluminum-air battery is the slow kinetics of the cathode oxygen reduction reaction. The conventional method to enhance the power of the aluminum-air battery is to develop a high-activity oxygen reduction catalyst to promote the kinetics of the oxygen reduction reaction. This can improve the power density to a certain extent, but the improvement is very limited, and the synthesis steps of the catalyst are complex and difficult to mass-produce. Exploring new ways to improve the power density of the aluminum-air battery is currently a research bottleneck that needs to be overcome. SUMMARY

[0004] To solve the above technical problems, embodiments of the present application provide an electrolyte additive, an electrolyte, a preparation method thereof and an aluminum-air battery.

[0005] To achieve the above-mentioned purposes, embodiments of the present application adopt the following technical solutions: In one aspect, the present application provides an electrolyte additive, which comprises a peroxide, a persulfate or an iodate.

[0006] In some embodiments, the concentration of the peroxide is 0.01-0.6 mol / L, the concentration of the persulfate is 0.01-1 mol / L, and the concentration of the iodate is 0.01-1 mol / L.

[0007] In some embodiments, the peroxide comprises at least one of hydrogen peroxide, sodium peroxide and potassium peroxide, the persulfate comprises potassium persulfate and / or sodium persulfate, and the iodate comprises at least one of potassium iodate, sodium iodate and calcium iodate.

[0008] In another aspect, the present application provides an electrolyte, which comprises a basic electrolyte or a neutral electrolyte and the above-mentioned electrolyte additive.

[0009] In some embodiments, the basic electrolyte is a 4-8 mol / L KOH solution or a 3-5 mol / L NaOH solution, and the neutral electrolyte is a 1-4 mol / L sodium chloride solution or a 1-4 mol / L sodium sulfate solution.

[0010] In another aspect, the present application provides a preparation method of an electrolyte, comprising the following steps: dissolving an alkaline electrolyte and an electrolyte additive in a solvent to prepare an electrolyte or dissolving a neutral electrolyte and an electrolyte additive in a solvent to prepare an electrolyte.

[0011] In another aspect, the present application provides an aluminum-air battery, comprising an air cathode, an aluminum anode and an electrolyte, wherein the electrolyte is an electrolyte prepared by the above method.

[0012] In some embodiments, the air cathode is prepared by mixing manganese dioxide, conductive carbon material and binder and rolling on a conductive current collector to form an air cathode.

[0013] In some embodiments, the mass ratio of the manganese dioxide to the conductive carbon material is 1:3-1:1, the mass ratio of the manganese dioxide to the binder is 1:0.9-1:1.1, the manganese dioxide comprises at least one of α-MnO2, β-MnO2, γ-MnO2 and δ-MnO2, the conductive carbon material comprises at least one of carbon nanotubes, graphyne, conductive carbon black, graphene and porous carbon, the binder comprises polytetrafluoroethylene and / or polyvinylidene fluoride, the conductive current collector is a nickel mesh, a copper mesh, an iron mesh or an iron-nickel-copper alloy mesh, the aluminum anode is a pure aluminum plate or an aluminum alloy, and the aluminum alloy is Al-Mg, Al-Mg-Sn-Ga, Al-Bi-Sn-In or Al-Sn-Sb-In.

[0014] Compared with the prior art, the present application has at least the following beneficial effects: The electrolyte additive provided by the present application has strong oxidizing property, and after being added into an alkaline electrolyte or a neutral electrolyte, peroxide, persulfate and iodate are simultaneously reduced in addition to oxygen being reduced in the air cathode during the discharge process, so as to accelerate the cathode depolarization process, improve the cathode kinetic reaction speed, and improve the power density of the aluminum-air battery. BRIEF DESCRIPTION OF DRAWINGS

[0015] Figure 1 The figure is a step current-voltage and power density test curve of the aluminum-air battery in Example 1 and Comparative Example 1; Figure 2 The figure is a constant current discharge test of the aluminum-air battery in Example 2 and Comparative Example 2; Figure 3 The figure is a relationship curve of the peak power density and the added hydrogen peroxide concentration of the aluminum-air battery in Example 3 to Example 8 and Comparative Example 3; Figure 4 The figure is a step current-voltage and power density test curve of the aluminum-air battery in Example 9 and Comparative Example 4; Figure 5 Figure 6 is a graph of the step current-voltage and power density test of the aluminum-air battery in Example 10 and Comparative Example 5; Figure 6 Figure 7 is a Tafel polarization curve of the aluminum anode in 4 M KOH containing different concentrations of hydrogen peroxide; Figure 7 Figure 8 is a voltage curve of Example 17 at 80 mA cm -2 under constant current discharge. DETAILED DESCRIPTION

[0016] The technical solutions in some embodiments of the present disclosure will be clearly and completely described below with reference to the drawings. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments provided in the present disclosure, all other embodiments obtained by those of ordinary skill in the art belong to the scope of protection of the present disclosure.

[0017] The current conventional method to enhance the power of aluminum-air batteries is to develop high-activity oxygen reduction catalysts to promote the kinetics of oxygen reduction reactions. This can improve the power density to a certain extent, but the improvement is very limited.

[0018] To solve the above technical problems, in one aspect, the present disclosure provides an electrolyte additive, which includes a peroxide, a persulfate or an iodate.

[0019] In some embodiments, the concentration of the peroxide is 0.01-0.6 mol / L, the concentration of the persulfate is 0.01-1 mol / L, and the concentration of the iodate is 0.01-1 mol / L.

[0020] Exemplarily, the concentration of the peroxide can be any one of 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, 0.55 mol / L, 0.6 mol / L, or a range value between any two of them, for which the embodiments of the present disclosure are not limited.

[0021] Exemplarily, the concentration of the persulfate salt can be a point value of any one of 0.01 mol / L, 0.02 mol / L, 0.05 mol / L, 0.06 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, 0.55 mol / L, 0.6 mol / L, 0.65 mol / L, 0.7 mol / L, 0.75 mol / L, 0.8 mol / L, 0.85 mol / L, 0.9 mol / L, 0.95 mol / L, 1 mol / L or a range value between any two of them, for which the embodiments of the present application are not specifically limited.

[0022] Exemplarily, the concentration of the iodate salt can be a point value of any one of 0.01 mol / L, 0.02 mol / L, 0.05 mol / L, 0.06 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, 0.55 mol / L, 0.6 mol / L, 0.65 mol / L, 0.7 mol / L, 0.75 mol / L, 0.8 mol / L, 0.85 mol / L, 0.9 mol / L, 0.95 mol / L, 1 mol / L or a range value between any two of them, for which the embodiments of the present application are not specifically limited.

[0023] In some embodiments, the peroxide includes at least one of hydrogen peroxide, sodium peroxide and potassium peroxide, the persulfate salt includes potassium persulfate and / or sodium persulfate, and the iodate salt includes at least one of potassium iodate, sodium iodate and calcium iodate.

[0024] In another aspect, the present application provides an electrolyte including a basic electrolyte or a neutral electrolyte and one of the electrolyte additives described above.

[0025] In some embodiments, the basic electrolyte is a 4-8 mol / L KOH solution or a 3-5 mol / L NaOH solution, and the neutral electrolyte is a 1-4 mol / L sodium chloride solution or a 1-4 mol / L sodium sulfate solution.

[0026] Exemplarily, the concentration of the KOH solution can be a point value of any one of 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L or a range value between any two of them, for which the embodiments of the present application are not specifically limited.

[0027] Exemplarily, the concentration of the NaOH solution can be a point value of any one of 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L or a range value between any two of them, for which the embodiments of the present application are not specifically limited.

[0028] Exemplarily, the concentration of the NaOH solution can be a point value of any one of 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L or a range value between any two of them, for which the embodiments of the present application are not specifically limited.

[0029] Exemplarily, the concentration of the NaOH solution can be a point value of any one of 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L or a range value between any two of them, for which the embodiments of the present application are not specifically limited.

[0030] In another aspect, the present application provides a preparation method of an electrolyte, comprising the following steps: dissolving an alkaline electrolyte and an electrolyte additive in a solvent to obtain an electrolyte or dissolving a neutral electrolyte and an electrolyte additive in a solvent to obtain an electrolyte, wherein the solvent can be deionized water or an organic solvent.

[0031] In another aspect, the present application provides an aluminum-air battery, comprising an air cathode, an aluminum anode and an electrolyte, wherein the electrolyte is one of the above electrolytes or is prepared by the above preparation method.

[0032] In some embodiments, the air cathode is prepared by mixing manganese dioxide, conductive carbon material and a binder and rolling them onto a conductive current collector to form the air cathode.

[0033] In some embodiments, the mass ratio of the manganese dioxide to the conductive carbon material is 1:3 to 1:1, the mass ratio of the manganese dioxide to the binder is 1:0.9 to 1:1.1, the mass ratio of the manganese dioxide to the conductive carbon material can be 1:3, 1:2 or 1:1, the mass ratio of the manganese dioxide to the binder can be 1:0.9, 1:1 or 1:1.1, the manganese dioxide comprises at least one of a-MnO2, b-MnO2, g-MnO2 and d-MnO2, the conductive carbon material comprises at least one of carbon nanotubes, graphyne, conductive carbon black, graphene and porous carbon, the binder comprises at least one of polytetrafluoroethylene, perfluorinated resin and polyvinylidene fluoride, the conductive current collector is a nickel mesh, a copper mesh, an iron mesh or an iron-nickel-copper alloy mesh, the aluminum anode is a pure aluminum plate or an aluminum alloy, and the aluminum alloy is Al-Mg, Al-Mg-Sn-Ga, Al-Bi-Sn-In or Al-Sn-Sb-In.

[0034] In order to objectively evaluate the technical effects of the embodiments of the present disclosure, the technical solutions provided by the present disclosure will be described in detail by experimental examples.

[0035] In order to make the present application easier to understand, the present application will be described in detail below in conjunction with embodiments, which are only illustrative and do not limit the scope of application of the present application.

[0036] Unless otherwise specified, the operation and processing method involved in the present application belongs to the conventional method in the art.

[0037] Unless otherwise specified, the instruments used in the present application are conventional instruments in the art.

[0038] Example 1 (1) Mix a-MnO2 and conductive carbon black at a mass ratio of 1:3, then add PTFE binder with the same mass as a-MnO2, add ethanol, stir thoroughly and volatilize ethanol in a 70°C water bath until black mixture is precipitated, then roll the black mixture onto a nickel mesh to form an air cathode.

[0039] (2) Prepare an electrolyte, wherein the concentration of sodium hydroxide in the electrolyte is 4 mol / L, and the concentration of potassium iodate is 0.5 mol / L.

[0040] (3) Place the air cathode and aluminum plate on both sides of the battery mold, then add the electrolyte in (2), and after standing for 20 min, start the step current-voltage and power density test.

[0041] Comparative Example 1 The same as Example 1, except that it does not contain potassium iodate.

[0042] ByFigure 1 It can be seen that after adding potassium iodate in Example 1, the peak power density increased from 104 mW / cm². -2 Increased to 128mW cm -2 This indicates that the power-enhancing electrolyte prepared with potassium iodate effectively improves the power density of aluminum-air batteries.

[0043] Example 2 (1) Mix β-MnO2 and conductive carbon black at a mass ratio of 1:2, then add polytetrafluoroethylene binder of the same mass as β-MnO2, add ethanol and stir thoroughly, and let the ethanol evaporate in a 70°C water bath until a black mixture is precipitated. Then roll the black mixture onto a nickel grid to form an air cathode.

[0044] (2) Prepare an electrolyte solution, wherein the concentration of potassium hydroxide in the electrolyte solution is 4 mol / L and the concentration of sodium iodate is 0.3 mol / L.

[0045] (3) Place the air cathode and the aluminum-magnesium-tin-gallium alloy plate from step (1) on both sides of the battery mold, and then add the electrolyte from step (2) to each side. After standing for 5 minutes, start a 1-hour constant current discharge test (current density of 160 mA cm⁻¹). -2 ).

[0046] Comparative Example 2 Same as Example 2, except that it does not contain sodium iodate.

[0047] pass Figure 2 It can be seen that the discharge voltage was significantly increased after adding sodium iodate in Example 2, indicating that the power-enhancing electrolyte prepared with potassium iodate effectively improved the discharge performance of the aluminum-air battery.

[0048] Example 3 (1) Mix γ-MnO2 and conductive carbon black at a mass ratio of 1:3, add polytetrafluoroethylene binder of the same mass as γ-MnO2, add ethanol and stir thoroughly, and let the ethanol evaporate in a 70°C water bath until a black mixture is precipitated. Then roll the black mixture onto an iron mesh to form an air cathode.

[0049] (2) Prepare an electrolyte solution, wherein the concentration of potassium hydroxide in the electrolyte solution is 6 mol / L and the concentration of hydrogen peroxide is 0.01 mol / L.

[0050] (3) Place the air cathode and aluminum-magnesium alloy plate from step (1) on both sides of the battery mold, then add the electrolyte from step (2), let stand for 7 minutes, and then start the step current-voltage and power density test.

[0051] Example 4 The same as example 3, except that the concentration of the hydrogen peroxide solution is 0.05 mol / L.

[0052] Example 5 The same as example 3, except that the concentration of the hydrogen peroxide solution is 0.1 mol / L.

[0053] Example 6 The same as example 3, except that the concentration of the hydrogen peroxide solution is 0.3 mol / L.

[0054] Example 7 The same as example 3, except that the concentration of the hydrogen peroxide solution is 0.5 mol / L.

[0055] Example 8 The same as example 3, except that the concentration of the hydrogen peroxide solution is 0.6 mol / L.

[0056] Comparative Example 3 The same as example 3, except that the hydrogen peroxide solution is not included.

[0057] By Figure 3 It can be seen that the peak power density of the aluminum-air battery is improved after adding different concentrations of hydrogen peroxide.

[0058] Example 9 (1) Mix δ-MnO2 and porous carbon at a mass ratio of 1:2, then add the same mass of polytetrafluoroethylene binder as δ-MnO2, add ethanol, stir well, and evaporate the ethanol in a 70°C water bath until the black mixture is precipitated. Then roll the black mixture onto a copper mesh to form an air cathode.

[0059] (2) Prepare an electrolyte, wherein the concentration of sodium hydroxide in the electrolyte is 4 mol / L, and the concentration of sodium peroxide is 0.3 mol / L.

[0060] (3) Place the air cathode in step (1) and the Al-Bi-Sn-In alloy plate on both sides of the battery mold, then add the electrolyte in step (2), and after standing for 2 min, start the step current-voltage and power density test.

[0061] Comparative Example 4 The same as example 9, except that the sodium peroxide solution is not included.

[0062] By Figure 4 It can be seen that by adding sodium peroxide, the peak power density is increased from 117 mW cm -2 to 138 mW cm -2, which shows that the power enhanced electrolyte prepared by using sodium peroxide effectively improves the power density of the aluminum-air battery.

[0063] Example 10 (1) α-MnO2 was mixed with conductive carbon black at a mass ratio of 1:3, and then PTFE binder was added in an amount equal to the mass of α-MnO2. Ethanol was added and stirred, and the ethanol was volatilized in a water bath at 70°C until the black mixture was precipitated. Then the black mixture was rolled onto a copper mesh to form an air cathode. (2) The electrolyte was prepared, in which the concentration of potassium hydroxide in the electrolyte was 4 mol / L, and the concentration of sodium persulfate was 0.1 mol / L.

[0064] (3) The air cathode in step (1) and a pure aluminum plate were placed on both sides of the battery mold, and then the electrolyte in step (2) was added. After standing for 2 min, the step current-voltage and power density test was started.

[0065] Comparative Example 5 The same as Example 10, except that it does not contain sodium persulfate.

[0066] By Figure 5 It can be seen that by adding sodium persulfate, the peak power density is increased from 90 mW cm -2 to 112 mW cm -2 , which shows that the power enhanced electrolyte prepared by using sodium peroxide effectively improves the power density of the aluminum-air battery.

[0067] Example 11 The same as Example 10, except that the concentration of potassium hydroxide is 4 mol / L, and the concentration of sodium chloride is 4 mol / L instead.

[0068] Example 12 The same as Example 10, except that the concentration of potassium hydroxide in the electrolyte is 4 mol / L, and the concentration of sodium chloride is 1 mol / L instead.

[0069] Example 13 The same as Example 10, except that the concentration of potassium hydroxide in the electrolyte is 4 mol / L, and the concentration of sodium chloride is 3 mol / L instead.

[0070] Example 14 The same as Example 10, except that the concentration of potassium hydroxide in the electrolyte is 4 mol / L, and the concentration of sodium sulfate is 4 mol / L instead.

[0071] Example 15 The same as example 10, except that the concentration of potassium hydroxide in the electrolyte is 4 mol / L, and the concentration of sodium sulfate is 3 mol / L.

[0072] Example 16 The same as example 10, except that the concentration of potassium hydroxide in the electrolyte is 4 mol / L, and the concentration of sodium sulfate is 1 mol / L.

[0073] Example 17 The same as example 10, except that the electrolyte is 4 M KOH + 0.1 M H2O2.

[0074] Test Example 1. Anodic accelerated dissolution The test uses the electrolyte of comparative example 3, example 4 and example 5, in addition, pure aluminum is used as anode, and discharged at a constant current of 10 mA cm -2 for one hour, and the anode discharge specific capacity is listed in table 1. The addition of hydrogen peroxide additive does not accelerate the anode dissolution.

[0075] Table 1 Discharge specific capacity under different concentrations of hydrogen peroxide Hydrogen peroxide concentration (M) Discharge specific capacity (mA cm"2) 0 1133 0.05 1137 0.1 1143 2. Anodic passivation A three-electrode system is used, the reference electrode is Hg / HgO electrode, the counter electrode is graphite sheet or platinum sheet, and pure aluminum is used as the working electrode, and the electrolyte contains different concentrations of hydrogen peroxide and 4 M KOH, and the Tafel polarization curve test is carried out. As shown in Figure 6 , no anodic passivation occurs in the Tafel curve.

[0076] 3. Accelerated battery degradation Example 17 is used to discharge at a constant current of 80 mA cm -2 , and mechanical charging is carried out every 3 hours. The voltage curve is shown in Figure 7 , and no obvious degradation occurs.

[0077] In the description of the present specification, specific features, structures, materials or characteristics can be combined in any one or more embodiments or examples in a suitable manner.

[0078] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto, and any person skilled in the art can easily think of changes or replacements within the technical range disclosed by the present application, which should be covered within the protection scope of the present application. Therefore, the protection scope of the present application should be subject to the protection scope of the claims.

Claims

1. An electrolyte additive characterized in that, The peroxide, the persulfate or the iodate.

2. An electrolyte additive according to claim 1, characterized in that The concentration of the peroxide is 0.01-0.6 mol / L, the concentration of the persulfate is 0.01-1 mol / L, and the concentration of the iodate is 0.01-1 mol / L.

3. The electrolyte additive according to claim 1, characterized in that, The peroxide includes at least one of hydrogen peroxide, sodium peroxide and potassium peroxide, the persulfate includes potassium persulfate and / or sodium persulfate, and the iodate includes at least one of potassium iodate, sodium iodate and calcium iodate.

4. An electrolyte, characterized by The basic electrolyte is a 4-8 mol / L KOH solution or a 3-5 mol / L NaOH solution, and the neutral electrolyte is a 1-4 mol / L sodium chloride solution or a 1-4 mol / L sodium sulfate solution.

5. An electrolyte according to claim 4, wherein The method comprises the following steps:

6. A method of preparing an electrolyte as claimed in any one of claims 4-5, characterized in that, The basic electrolyte and the electrolyte additive are dissolved in a solvent to prepare the electrolyte, or the neutral electrolyte and the electrolyte additive are dissolved in a solvent to prepare the electrolyte. The air cathode, the aluminum anode and the electrolyte, wherein the electrolyte is the electrolyte of claim 4 or 5 or the electrolyte prepared by the method of claim 6.

7. An aluminum-air battery characterized by The air cathode is prepared by mixing manganese dioxide, conductive carbon material and binder and rolling them onto a conductive current collector to form the air cathode.

8. The aluminum-air cell of claim 7, wherein, The mass ratio of the manganese dioxide to the conductive carbon material is 1:3-1:1, the mass ratio of the manganese dioxide to the binder is 1:0.9-1:1.1, the manganese dioxide includes at least one of α-MnO2, β-MnO2, γ-MnO2 and δ-MnO2, the conductive carbon material includes at least one of carbon nanotube, graphyne, conductive carbon black, graphene and porous carbon, the binder includes polytetrafluoroethylene and / or polyvinylidene fluoride, the conductive current collector is a nickel mesh, a copper mesh, an iron mesh or an iron-nickel-copper alloy mesh, the aluminum anode is a pure aluminum plate or an aluminum alloy, and the aluminum alloy is Al-Mg, Al-Mg-Sn-Ga, Al-Bi-Sn-In or Al-Sn-Sb-In.

9. The aluminum-air cell of claim 8, wherein, ​