Preparation method and application of carbon fiber / polypropylene composite material with self-reinforced interface

By stretching carbon fibers at different rates during the preforming stage, the transcrystalline structure of the carbon fiber/polypropylene composite interface is controlled, solving the problems of high cost and damage to the carbon fiber surface in the prior art, and achieving efficient control of interface properties and improvement of overall performance.

CN121405981APending Publication Date: 2026-01-27ZHONGBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511855272.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-10
Publication Date
2026-01-27

AI Technical Summary

Technical Problem

Existing methods for reinforcing carbon fiber/polypropylene composite interfaces are costly, technically challenging, and damage the carbon fiber surface, making it difficult to effectively control the transcrystalline structure at the interface to improve overall performance.

Method used

By stretching carbon fibers at different rates during the preforming stage, the content of α and β crystal forms in the interfacial transverse crystals can be controlled by the matrix shear force, thereby improving the interfacial bonding performance.

Benefits of technology

It enables low-cost and convenient control of the interfacial properties of carbon fiber/polypropylene composites, improving interfacial shear strength and overall performance, and meeting the diverse needs of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121405981A_ABST
    Figure CN121405981A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a carbon fiber / polypropylene composite material with a self-reinforced interface, and belongs to the technical field of composite materials. The preparation method of the carbon fiber / polypropylene composite material with the self-reinforced interface comprises the following steps: impregnating carbon fibers in molten polypropylene; cooling to a pre-forming temperature, and stretching the carbon fibers at a rate of 40-300 [mu] m / s; continuously cooling to a forming temperature, and carrying out isothermal crystallization; and cooling to room temperature to obtain the carbon fiber / polypropylene composite material with the self-reinforced interface. The contents of alpha and beta crystal forms in an interface transverse crystal are regulated and controlled in a manner of stretching the carbon fiber at different rates and giving a shear force to a matrix in a pre-forming stage, so that the interface bonding performance of the carbon fiber / polypropylene composite material is improved, the designability and the regulation and control of the comprehensive performance of the carbon fiber / polypropylene composite material are improved, and the industrial application diversity is met.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of composite materials, and more particularly relates to a preparation method and application of carbon fiber / polypropylene composite material with self-reinforced interface. BACKGROUND

[0002] The carbon fiber / polypropylene composite material has the advantages of high specific strength, short forming cycle, environmental friendliness, and the like, and is widely used in the fields of aerospace, automobiles, daily chemicals, and the like. The interface plays a key role in load transmission and has an important influence on the mechanical properties of the carbon fiber / polypropylene composite material.

[0003] When the carbon fiber / polypropylene composite material is formed, a Transcrystallinity or HSC (Hybrid shish-calabash) crystal structure composed of different crystal forms of alpha and beta is formed at the interface, and the different crystal structures at the interface will affect the interface bonding performance of the composite material. The alpha crystal form of monoclinic system is in the most stable state of thermodynamics, has high bending strength, bending modulus, hardness, and the like, but has poor fracture toughness. The beta crystal form of hexagonal system is in the metastable state of thermodynamics, has excellent heat distortion temperature, fracture toughness, impact strength, and the like.

[0004] In order to improve the interface bonding performance of the composite material, surface modification of the carbon fiber is a common and effective method, such as adding nanoparticles, plasma irradiation, surface grafting, chemical etching, and the like. The alpha and beta crystal form contents in the interface Transcrystallinity of the carbon fiber / polypropylene composite material can be controlled so as to obtain a carbon fiber / polypropylene composite material product with excellent comprehensive performance. These methods need to add substances or treat the surface of the carbon fiber, which increases the material cost and process cost and damages the surface of the carbon fiber.

[0005] Based on this, the application is proposed. SUMMARY

[0006] The application aims to provide a preparation method and application of carbon fiber / polypropylene composite material with self-reinforced interface, so as to improve the problems of high cost, great technical difficulty, damage to the surface of the carbon fiber, and the like of the interface reinforcing method in the prior art. The alpha and beta crystal form contents in the interface Transcrystallinity are controlled in the form of shear force of the matrix by stretching the carbon fiber at different rates in the preforming stage, the interface bonding performance is improved, the designability and controllability of the comprehensive performance of the carbon fiber / polypropylene composite material are improved, and the industrial application diversity is met.

[0007] To achieve the above-mentioned purpose, the application provides the following scheme.

[0008] One of the technical schemes of the application: a preparation method of carbon fiber / polypropylene composite material with self-reinforced interface is provided, comprising the following steps:

[0009] The carbon fiber is immersed in molten polypropylene; the temperature is decreased to a preforming temperature, the carbon fiber is stretched at a rate of 40-300 μm / s; the temperature is continuously decreased to a forming temperature for isothermal crystallization; and the temperature is cooled to room temperature, thereby obtaining the self-reinforced interface carbon fiber / polypropylene composite material.

[0010] Preferably, the melting of the polypropylene comprises: increasing the temperature to 200 ℃ at a temperature increasing rate of 20 ℃ / min, and maintaining the temperature for 5-10 min.

[0011] Preferably, the temperature of the preforming is 140-160 ℃.

[0012] Preferably, the temperature of the isothermal crystallization is 110-140 ℃, and the time is 30-180 min.

[0013] Further, the temperature of the isothermal crystallization is 130.8 ℃, and the time is 30 min.

[0014] Preferably, the rate of the temperature decreasing is 10-30 ℃ / min.

[0015] The present application controls the content of α and β crystal forms in the interface transcrystalline by stretching the carbon fiber at different rates in the preforming stage, and improves the transcrystalline structure and the bonding performance of the carbon fiber / polypropylene composite material interface.

[0016] Under the stretching action of the carbon fiber, the polypropylene is sheared, the molecular chains are arranged and oriented according to the force direction, the order is increased, the crystal nucleus is more easily formed, and the molecular crystallization is more easily. The crystallization speed is accelerated, the forming time is shortened, and the impact strength and the heat resistance of the material are effectively improved.

[0017] Under the action of different stretching rates, the transcrystalline structures formed at the interface of the carbon fiber / polypropylene composite material are different, mainly the content of α and β crystal forms is different, which is related to the orientation degree of the molecular chains caused by the shearing. For example, under the action of the stretching rate of 50 μm / s, the interface is composed of α and β crystal forms, and the α crystal form accounts for the majority; under the action of the stretching rate of 120 μm / s, the interface is almost composed of β crystal form; under the action of the stretching rate of 150 μm / s or 200 μm / s, the interface is composed of α and β crystal forms, and the β crystal form accounts for the majority; and under the action of the stretching rate of 300 μm / s, the interface is almost composed of α crystal form.

[0018] The appropriate stretching rate depends on the transcrystalline structure of the carbon fiber / polypropylene composite material interface that is desired, i.e. the interface shear strength of the carbon fiber / polypropylene composite material that is desired. For example, under the action of the stretching rate of 120 μm / s, the content of β crystal form in the transcrystalline structure of the carbon fiber / polypropylene composite material interface is the most, and the interface shear strength of the carbon fiber / polypropylene composite material is the highest.

[0019] That is, the method of the present application can regulate the content of alpha and beta crystal forms in the interface transcrystalline of carbon fiber / polypropylene composite material, so as to obtain carbon fiber / polypropylene composite material products with excellent comprehensive performance.

[0020] The second technical scheme of the present application provides the carbon fiber / polypropylene composite material with self-reinforced interface prepared by the above preparation method.

[0021] The third technical scheme of the present application provides the application of the carbon fiber / polypropylene composite material with self-reinforced interface in the fields of aerospace, ship, automobile and sports equipment.

[0022] The fourth technical scheme of the present application provides a method for regulating the content of alpha and beta crystal forms in the interface transcrystalline of carbon fiber / polypropylene composite material, and the carbon fiber / polypropylene composite material with self-reinforced interface is prepared by the above preparation method.

[0023] The present application regulates the content of alpha and beta crystal forms in the interface transcrystalline by stretching the carbon fiber at different speeds in the preforming stage, and the shear force is applied to the matrix, so as to self-reinforce the interface bonding performance of the carbon fiber / polypropylene composite material. The surface of the carbon fiber does not need to be treated by adding substances or technical treatment. The cost is low, the technology is simple, and the industrial application requirements can be better met.

[0024] The present application discloses the following technical effects:

[0025] The current reported interface regulation and research of carbon fiber / polypropylene composite material are mainly through carbon fiber surface treatment (such as plasma treatment) or carbon fiber sizing agent to regulate the performance of the composite material, such as adding nanoparticles, plasma radiation, surface grafting, chemical etching, etc. The interface shear strength can be improved; these methods need to add substances or treat the surface of the carbon fiber, which increases the material cost, process cost and damages the surface of the carbon fiber.

[0026] The present application starts from the alpha and beta crystal forms of the microstructure constituting the interface transcrystalline, provides a preparation method and application technology of the carbon fiber / polypropylene composite material with self-reinforced interface, changes the content of alpha and beta crystal forms in the interface transcrystalline of the carbon fiber / polypropylene composite material by stretching the carbon fiber at a proper stretching speed in the preforming process, so as to regulate the interface bonding performance, impact resistance and heat resistance of the composite material, and the interface shear strength can be improved by 100%. The interface bonding performance is improved, the designability and controllability of the comprehensive performance of the carbon fiber / polypropylene composite material are improved, the industrial application diversity is met, and the problems of high cost, great technical difficulty and damage to the surface of the carbon fiber in the interface reinforcement method in the prior art are improved. BRIEF DESCRIPTION OF DRAWINGS

[0027] Figure 1 The sample schematic diagram for the interface shear experiment;

[0028] Figure 2 are polarizing microscope images of carbon fiber / polypropylene composite materials in which carbon fibers were stretched at different stretching rates, wherein a is a stretching rate of 0 μm / s, b is a stretching rate of 50 μm / s, c is a stretching rate of 120 μm / s, and d is a stretching rate of 200 μm / s;

[0029] Figure 3 are X-ray diffraction patterns of carbon fiber / polypropylene composite materials in which carbon fibers were stretched at different stretching rates;

[0030] Figure 4 are interfacial shear strengths of carbon fiber / polypropylene composite materials in which carbon fibers were stretched at different stretching rates. DETAILED DESCRIPTION

[0031] Various illustrative embodiments of the present application are described in detail herein below with reference to the attached drawings. The present application should not be considered limited to the embodiments described herein, but rather those described herein are presented as being illustrative of the present application. Various modifications and changes can be made to the present application by those skilled in the art which will be apparent from this description without departing from the spirit of the application. It is intended that the description be considered as exemplary only and not in limitation of the scope of the application. It is to be understood that the drawings are not to scale and that, unless otherwise specifically indicated herein, the drawings are meant to be only illustrative of the present application.

[0032] It is to be understood that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the present application. In addition, any numerical range recited herein is intended to include all sub-ranges of the same numerical precision subsumed therein. In addition, all ranges are inclusive of the endpoints. In addition, any numerical value recited herein is intended to include all values reasonably falling within the range, unless the context clearly indicates otherwise. These and other modifications can be made to the application in light of the foregoing description.

[0033] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. Although preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein can be used in the practice of the present application. All documents mentioned herein are incorporated by reference to disclose and describe the methods and / or materials in connection with which the documents are cited. In the case of conflict between the present specification and any document incorporated by reference, the present specification will control.

[0034] Various modifications and changes can be made to the present application in light of the foregoing description, without departing from the scope or spirit of the present application. Other embodiments of the present application will be apparent to those skilled in the art from the foregoing description. The scope of the present application is to be limited only by the claims.

[0035] With respect to the use of "comprising", "including", "containing", "having" and "ensing" and the like, these terms are used in the sense of "open" terms (i.e., in the sense of "including, but not limited to").

[0036] It should be noted that the present application does not describe in detail the conventional operation means in the art, and is not the focus of the present application.

[0037] The polypropylene used in the following examples and comparative examples of the present application is a commercial product Sanren Y600 (Premium-grade) of Shanghai Petrochemical, the melt mass flow rate thereof at 230℃ is 4.5-7.5 g / 10 min, the yield strength is 38.2 MPa, the flexural modulus is 1350 MPa, and the unnotched Izod impact strength is 29 J / m. The carbon fiber used is continuous carbon fiber AS4C-3K of Hexcel Corporation, USA, the diameter thereof is 6.9 μm, the tensile modulus is 231 GPa, the tensile strength is 4723 MPa, and the elongation at break is 1.8%. Other raw materials used are commercially available products, and the source of the commercially available products does not affect the technical effects of the present application.

[0038] Comparative Example 1

[0039] The polypropylene was heated from room temperature to 200℃ at a heating rate of 20℃ / min and kept for 5 min to obtain a polypropylene melt; the carbon fiber was completely immersed in the polypropylene melt; preforming was performed by cooling to 140℃ at a rate of 20℃ / min; the carbon fiber was stretched at a stretching rate of 50 μm / s; isothermal crystallization was performed by cooling to 130.8℃ at a rate of 20℃ / min for 30 min; and the sample to be tested was obtained by cooling to room temperature at a rate of 20℃ / min.

[0040] Example 1

[0041] The polypropylene was heated from room temperature to 200℃ at a heating rate of 20℃ / min and kept for 5 min to obtain a polypropylene melt; the carbon fiber was completely immersed in the polypropylene melt; preforming was performed by cooling to 140℃ at a rate of 20℃ / min; the carbon fiber was stretched at a stretching rate of 50 μm / s; isothermal crystallization was performed by cooling to 130.8℃ at a rate of 20℃ / min for 30 min; and the sample to be tested was obtained by cooling to room temperature at a rate of 20℃ / min.

[0042] Example 2

[0043] The polypropylene was heated from room temperature to 200℃ at a heating rate of 20℃ / min and kept for 5 min to obtain a polypropylene melt; the carbon fiber was completely immersed in the polypropylene melt; preforming was performed by cooling to 140℃ at a rate of 20℃ / min; the carbon fiber was stretched at a stretching rate of 70 μm / s; isothermal crystallization was performed by cooling to 130.8℃ at a rate of 20℃ / min for 30 min; and the sample to be tested was obtained by cooling to room temperature at a rate of 20℃ / min.

[0044] Example 3

[0045] The polypropylene was heated from room temperature to 200℃ at a heating rate of 20℃ / min and kept for 5min to obtain polypropylene melt; the carbon fiber was immersed in the polypropylene melt and completely immersed; preforming was performed at a cooling rate of 20℃ / min to 140℃; the carbon fiber was stretched at a stretching rate of 100μm / s; isothermal crystallization was performed at a cooling rate of 20℃ / min to 130.8℃ for 30min; cooling was performed at a cooling rate of 20℃ / min to room temperature to obtain the sample to be tested.

[0046] Example 4

[0047] The polypropylene was heated from room temperature to 200℃ at a heating rate of 20℃ / min and kept for 5min to obtain polypropylene melt; the carbon fiber was immersed in the polypropylene melt and completely immersed; preforming was performed at a cooling rate of 20℃ / min to 140℃; the carbon fiber was stretched at a stretching rate of 120μm / s; isothermal crystallization was performed at a cooling rate of 20℃ / min to 130.8℃ for 30min; cooling was performed at a cooling rate of 20℃ / min to room temperature to obtain the sample to be tested.

[0048] Example 5

[0049] The polypropylene was heated from room temperature to 200℃ at a heating rate of 20℃ / min and kept for 5min to obtain polypropylene melt; the carbon fiber was immersed in the polypropylene melt and completely immersed; preforming was performed at a cooling rate of 20℃ / min to 140℃; the carbon fiber was stretched at a stretching rate of 200μm / s; isothermal crystallization was performed at a cooling rate of 20℃ / min to 130.8℃ for 30min; cooling was performed at a cooling rate of 20℃ / min to room temperature to obtain the sample to be tested.

[0050] Example 6

[0051] The polypropylene was heated from room temperature to 200℃ at a heating rate of 20℃ / min and kept for 5min to obtain polypropylene melt; the carbon fiber was immersed in the polypropylene melt and completely immersed; preforming was performed at a cooling rate of 20℃ / min to 140℃; the carbon fiber was stretched at a stretching rate of 300μm / s; isothermal crystallization was performed at a cooling rate of 20℃ / min to 130.8℃ for 30min; cooling was performed at a cooling rate of 20℃ / min to room temperature to obtain the sample to be tested.

[0052] Performance test:

[0053] The interface crystallization process of the carbon fiber / polypropylene composite material obtained in each example and the comparative example was observed and characterized by a cold-hot stage polarizing microscope. The interface nanomechanical property thereof was determined by a peak force quantitative nanomechanical property test module of an atomic force microscope. The interface shear strength thereof was determined according to the standard ISO 527-2: 2012 Determination of tensile properties of plastics - Part 2: test conditions for moulded and extruded plastics.

[0054] The crystallization process of the carbon fiber / polypropylene composite was observed in real time by polarizing microscope, the structure and content of the alpha and beta crystal forms in the interface transcrystalline were determined by X-ray diffractometer, and the interface shear performance was determined by a universal mechanical testing machine Figure 1 )。

[0055] According to the polarizing microscope test result, when the carbon fiber is stretched at a stretching rate of 120 μm / s, the carbon fiber / polypropylene composite interface transcrystalline has the least blue-red cross extinction area and the most bright yellow area, and the content of the beta crystal form is the most Figure 2 )。

[0056] In the X-ray diffraction pattern, the carbon fiber / polypropylene composite without stretching the carbon fiber has only the alpha (1 1 0) peak representing the alpha crystal form, and the beta (3 0 0) peak representing the beta crystal form does not exist; after the carbon fiber is stretched, the beta (3 0 0) peak representing the beta crystal form begins to appear; when the carbon fiber is stretched at a stretching rate of 120 μm / s, the beta (3 0 0) peak of the beta crystal form is the highest, and the alpha (1 1 0) peak is the lowest, which indicates that the content of the alpha crystal form in the carbon fiber / polypropylene composite interface transcrystalline is the least, and the content of the beta crystal form is the most Figure 3 )。

[0057] When the carbon fiber is stretched at a stretching rate of 120 μm / s, the carbon fiber / polypropylene composite interface shear strength is the strongest, which is improved by 100% compared with the interface shear strength of the carbon fiber / polypropylene composite without stretching the carbon fiber Figure 4 )。

[0058] The various embodiments in the specification are described in a progressive manner, and each embodiment focuses on the difference from other embodiments. The same or similar parts between the various embodiments can be referred to each other.

[0059] The above description of disclosed embodiments enables a person skilled in the art to implement or use the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a self-reinforcing carbon fiber / polypropylene composite material, characterized in that, Includes the following steps: Carbon fibers are impregnated in molten polypropylene; the temperature is lowered to the pre-forming temperature, and the carbon fibers are stretched at a rate of 40~300μm / s; the temperature is further lowered to the forming temperature for isothermal crystallization; and the carbon fiber / polypropylene composite material with the self-reinforced interface is obtained.

2. The preparation method according to claim 1, characterized in that, The melting of polypropylene includes heating to 200°C at a heating rate of 20°C / min and holding at that temperature for 5-10 minutes.

3. The preparation method according to claim 1, characterized in that, The preforming temperature is 140~160℃.

4. The preparation method according to claim 1, characterized in that, The isothermal crystallization temperature is 110~140℃, and the time is 30~180min.

5. The preparation method according to claim 4, characterized in that, The isothermal crystallization was performed at a temperature of 130.8°C for 30 minutes.

6. The preparation method according to claim 1, characterized in that, The cooling rate is 10~30℃ / min.

7. The carbon fiber / polypropylene composite material with a self-reinforced interface prepared by the preparation method according to any one of claims 1 to 6.

8. The application of the self-reinforcing interface carbon fiber / polypropylene composite material of claim 7 in the fields of aerospace, shipbuilding, automobile and sporting goods.

9. A method for controlling the content of α and β crystal forms in the transverse crystals at the interface of carbon fiber / polypropylene composite materials, characterized in that, Self-reinforced carbon fiber / polypropylene composite materials are prepared by the preparation method according to any one of claims 1 to 6.