Method for improving strength of silicate clinker based on mineral and crystal form composition analysis

By analyzing the mineral and crystal composition of silicate clinker and optimizing it using multiple linear regression, the problem of simultaneously achieving high 3d and 28d strength of silicate clinker was solved, resulting in an overall improvement in clinker strength and grindability.

CN122130481APending Publication Date: 2026-06-02GEZHOUBA SONGZI CEMENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610137127.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-30
Publication Date
2026-06-02

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously achieve both 3d and 28d strength of silicate clinker in industrial production, resulting in low 3d strength or low 28d strength, as well as poor grindability, making it difficult to achieve a balanced improvement in both in actual production.

Method used

By analyzing the mineral and crystal composition of clinker produced in industrial production, combined with XRD quantitative analysis and multiple linear regression, the appropriate relative contents of C3S and C2S were determined. Furthermore, by adjusting the clinker's liter weight, f-CaO, and chemical composition, the saturation ratio of the clinker was optimized, thereby improving the strength of silicate clinker.

Benefits of technology

The overall 3d and 28d compressive strength of silicate clinker was improved, ensuring that the clinker was at a high level while improving its grindability, thus meeting the needs of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122130481A_ABST
    Figure CN122130481A_ABST
Patent Text Reader

Abstract

This invention relates to the field of cement building materials technology, specifically disclosing a method for improving the strength of silicate clinker based on mineral and crystal composition analysis. The method involves collecting 3-day and 28-day compressive strength test data of silicate clinker and quantitatively analyzing the mineral and crystal composition data using XRD. A mineral composition and strength zoning statistical method is employed to obtain appropriate C3S or C2S content to maintain a relatively good overall level of 3-day and 28-day compressive strength of the clinker. Then, a stepwise multiple linear regression analysis is used to establish the relationship between the 3-day and 28-day compressive strength of the clinker, clinker liter weight, f-CaO, the content of other chemical components, and the mineral composition and crystal content of the clinker. Specific analytical methods are used to determine optimization measures, further optimizing and improving the clinker strength. Using the above method, the 3-day and 28-day compressive strength of silicate clinker can be improved simultaneously.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cement building materials technology, specifically to a method for improving the strength of silicate clinker based on mineral and crystal composition analysis. Background Technology

[0002] Silicate cement clinker is prepared by calcination of four elements: calcium, silicon, aluminum, and iron. The main minerals are Al (C3S), Be (C2S), aluminum (C3A), and iron (C4AF). In actual industrial production, C3S mainly includes two crystal forms: M1-C3S and M3-C3S; C3A mainly includes two crystal forms: cubic C3A and orthorhombic C3A; and C2S includes α-C2S and α... H There are four crystal forms: -C2S, β-C2S, and γ-C2S. In reality, γ-C2S rarely appears under normal cooling of clinker, and its formation is almost negligible; it generally only appears under slow cooling conditions. Furthermore, in actual industrial production, although the process equipment and parameters can remain relatively stable for a certain period, raw materials inevitably introduce other elements such as magnesium, sulfur, potassium, and sodium. The solid solution effect of these elements in the clinker minerals has a significant impact on the final clinker minerals and crystal forms, thereby affecting properties such as clinker strength.

[0003] Numerous studies have investigated the effects of magnesium oxide (MgO) and sulfur trioxide (STO) on clinker mineral composition, with most focusing on laboratory-scale clinker production using pelleting. Most results indicate that increased MgO content leads to a decrease in M1-type C3S (A-ore) content and an increase in M3-type C3S (A-ore) content, resulting in decreased clinker strength. Increasing SO3 content can improve M1-type C3S content and thus enhance clinker strength. Introducing gypsum (SO3) can improve burnability and promote C3S formation to some extent, although some studies suggest that SO3 can hinder C3S formation, leading to an increase in C2S. Regarding the effect of MgO on clinker mineral composition, most researchers believe it increases C4AF content. Therefore, iron content should be reduced and the aluminum ratio (IM) increased in clinker formulation. However, these studies are relatively isolated, often focusing only on the effects of certain non-calcium, silicon, aluminum, iron, and heterogeneous elements on single clinker or clinker minerals. There are few studies that simultaneously analyze the chemical composition, mineral and crystal content, and strength of industrial clinker.

[0004] In actual production statistical studies, it was found that when the MgO content of clinker is at a low level (<2.0%), as the MgO content increases, both M1-type C3S and M3-type C3S increase simultaneously. However, the ratio of M1-type C3S to M3-type C3S does not increase significantly. In addition, the C4AF content of clinker increases while the C3A content decreases. However, as the MgO content increases to a certain level (≥2.0%), its impact on the mineral composition of clinker becomes negligible. Furthermore, while many researchers now propose introducing gypsum (SO3) to increase the proportion of M1-type C3S in clinker and improve clinker strength, they overlook the fact that SO3 introduction alters the C3S content in clinker. When the sulfur-alkali ratio of clinker does not exceed 0.6, SO3 introduction leads to an increase in C3S content. However, when SO3 levels are high (sulfur-alkali ratio exceeding 0.8), the C3S content decreases significantly. Although the proportion of M1-type C3S increases in this case, the significant reduction in C3S content negatively impacts clinker performance, such as a marked decrease in 3-day strength and even hindering 28-day strength development. Some cement companies maintain a high clinker saturation ratio (KH) to achieve higher 3-day strength, but the 28-day strength remains low. Other companies, due to high clinker alkali content and a focus solely on achieving high 28-day strength, control the KH to a lower level to improve 28-day strength, but this results in low 3-day strength and poor grindability. Therefore, in actual industrial production, the factors affecting the 3d and 28d strength of clinker may be mutually restrictive. How to balance and control them so that the 3d and 28d strengths of silicate clinker are maintained at a high level, such as not less than 34MPa and 60MPa respectively, is of great significance to cement kiln line enterprises.

[0005] Therefore, to address the issue of simultaneously improving the 3-day and 28-day strength of silicate clinker, we should start from the fundamental point that silicate clinker is mainly composed of silicate minerals (C3S and C2S). First, we should find the appropriate relative content of C3S and C2S for different plants based on their current actual conditions. Then, we should conduct a correlation analysis on the clinker's strength, mineral composition and crystal content, chemical composition, etc., to find the direction and space for further optimization. Summary of the Invention

[0006] To address the aforementioned problems, this invention discloses a method for improving the strength of silicate clinker based on mineral and crystal composition analysis. After collecting data on the chemical composition, mineral composition and crystal content, 3-day compressive strength, and 28-day compressive strength of the clinker over a period of time, the method first analyzes the most important silicate minerals in the clinker. Typically, the kiln line saturation ratio is controlled within a certain range; that is, if C3S is high (or low), then C2S is low (or high). C3S or C2S is statistically analyzed in relation to the 3-day and 28-day compressive strength of the clinker to obtain suitable relative contents of the silicate phases C3S and C2S in the clinker, maintaining the overall 3-day and 28-day strength of the clinker at a good level. Then, the mineral and crystal structure factors that influence the 3-day and 28-day compressive strength of the clinker in the same direction are identified. These mineral and crystal structure factors are then correlated with the clinker's liter weight, f-CaO, and chemical composition to identify influencing factors and determine further optimization directions.

[0007] The technical solution of this invention is a method for improving the strength of silicate clinker based on mineral and crystal composition analysis, comprising the following steps: S1. The clinker produced in industrial production is ground with dihydrate gypsum. A portion of the resulting sample is tested for 3-day and 28-day compressive strength, and the other portion is subjected to XRD quantitative analysis of mineral and crystal composition. Data on the 3-day and 28-day compressive strength of the clinker, as well as the content of C3S, C2S, C3A and C4AF minerals and their related crystal forms in the clinker are obtained respectively. S2. Collect data from S1 over a period of time and perform statistical analysis on the obtained data. Specifically, based on XRD analysis, determine the appropriate relative contents of C3S and C2S in clinker by using a mineral composition and strength zoning statistical method with the 3-day and 28-day compressive strength of clinker. Then, establish the correlation between the C3S or C2S content in clinker and the clinker weight per liter, f-CaO, and other chemical components using stepwise multiple linear regression analysis. Based on the obtained appropriate relative contents of C3S and C2S and the correlation between the C3S or C2S content and the clinker weight per liter, f-CaO, and other chemical components, calculate the appropriate control saturation ratio of clinker. Control the production of clinker according to this saturation ratio to maintain the relative contents of C3S and C2S in clinker at an appropriate level, thereby maintaining the overall improvement of the 3-day and 28-day compressive strength of silicate clinker.

[0008] Optionally, 4 wt% gypsum is added to the clinker produced industrially in S1; C3S includes two crystal forms, M1-C3S and M3-C3S, C3A includes two crystal forms, cubic C3A and orthorhombic C3A, and C2S includes α-C2S and α-C2S. H There are four crystal forms: -C2S, β-C2S, and γ-C2S.

[0009] Optionally, each test in S1 is recorded as one sample size, and in S2, data on compressive strength and mineral and related crystal content are collected over a period of time, with a sample size ≥ 90.

[0010] Optionally, the mineral composition and strength zoning statistical method in S2 refers to dividing the C3S or C2S content in clinker into multiple different intervals, and then statistically analyzing the number, proportion, and average strength of the 3d compressive strength of clinker in different strength intervals within these intervals. A graph showing the distribution ratio and average trend of different 3d compressive strengths under different C3S or C2S content intervals is then plotted. Similarly, a graph showing the distribution ratio and average trend of different 28d compressive strengths under different intervals is plotted. A suitable relative content of C3S and C2S refers to the value of C3S and C2S content or a range within which the overall 3d and 28d compressive strength of silicate clinker can be improved.

[0011] Optionally, in addition to the conventional CaO, SiO2, Al2O3 and Fe2O3, other chemical components in S2 may also include one or more of the heteroelement K2O, Na2O, MgO and SO3.

[0012] Optionally, in S2, stepwise multiple linear regression analysis is further used to establish the correlation between the 3-day and 28-day compressive strength of clinker and the clinker liter weight, f-CaO, impurity element content, and clinker mineral composition and crystal form content, respectively. Specifically, the impurity element influencing factor selection method is first used to identify the factors that have a significant impact on the 3-day and 28-day compressive strength from the significant influencing factors and directly use them as the direction for optimization and improvement. Then, from the significant influencing factors, the mineral composition and crystal form influencing factors that have the same effect on the 3-day and 28-day compressive strength of clinker are selected. Stepwise multiple linear regression analysis is used again to establish the correlation between these mineral composition and crystal form content and the clinker liter weight, f-CaO, and other chemical components. From the significant influencing factors, the chemical component influencing factors that affect these mineral composition and crystal form content and thus have a positive or negative impact on the 3-day and 28-day compressive strength are identified as the direction for further optimization and adjustment.

[0013] Optionally, the method for selecting the influencing factors of impurity elements is to select factors that have a significant impact on the dependent variables 3d and 28d compressive strength. Specifically, if the impurity element content has the same effect on the dependent variables 3d and 28d compressive strength, and in the process of establishing the correlation between the clinker 3d compressive strength and 28d compressive strength and the clinker liter weight, f-CaO, impurity element content, and clinker mineral composition and crystal form content, respectively, using stepwise multiple linear regression analysis, the proportion of the change in the root mean square error corresponding to the impurity element content to the total change in the F value reaches 50% or more, then it is directly identified as an important influencing factor.

[0014] Optionally, if a direction for optimization and improvement is found, after fine-tuning the component parameters, the appropriate control saturation ratio of the clinker is recalculated based on the suitable relative content of C3S and C2S in S2 and the correlation between the C3S or C2S content in the clinker and the clinker liter weight, f-CaO and other chemical components, so as to further optimize and improve the clinker strength.

[0015] Optionally, if no factor can be found that significantly affects the 3d and 28d compressive strength of clinker, or if a chemical component that significantly affects the 3d and 28d compressive strength of clinker but does not have a synergistic effect, then it indicates that mineral composition and crystal form regulation is not required at this time.

[0016] Optionally, the mineral composition and crystal form influencing factors that have a synergistic effect on the 3d and 28d compressive strength of clinker refer to the adjustments of mineral composition and crystal form influencing factors that are simultaneously beneficial to the 3d and 28d compressive strength of clinker or simultaneously detrimental to the 3d and 28d compressive strength of clinker; or improve at least one of the age-specific strength indices of the 3d and 28d compressive strength of clinker without adversely affecting the other age-specific strength index.

[0017] The present invention has the following beneficial effects: This invention obtains suitable component control and optimization parameters for clinker calcination by testing the 3-day and 28-day compressive strength of clinker samples and analyzing the accumulated data. The invention includes two control methods: Control method 1: Using a mineral composition and strength zoning statistical method to obtain suitable A-ore (C3S) or B-ore (C2S) content to maintain the overall 3-day and 28-day compressive strength of clinker at a good level. Control method 2: Using stepwise multiple linear regression analysis to establish the relationship between the 3-day and 28-day compressive strength of clinker, clinker liter weight, f-CaO, chemical component content, and clinker mineral composition and crystal form content, specific analytical methods are used to determine optimization measures and further optimize and improve clinker strength. The method for improving silicate clinker strength based on mineral and crystal form composition analysis provided by this invention can simultaneously improve the 3-day and 28-day strength of silicate clinker, maintaining both at a good level. Attached Figure Description

[0018] Figure 1 The distribution of 3-day compressive strength of clinker with different C2S contents in Example 1; Figure 2 The distribution of 28-day compressive strength of clinker with different C2S contents in Example 1; Figure 3 To plot the relationship between C2S content and 3d compressive strength of clinker using probability density function; Figure 4To plot the relationship between C2S content and 28-day compressive strength of clinker using probability density function; Detailed Implementation Unless otherwise specified, the experimental methods used in the following examples are conventional methods. Unless otherwise specified, all raw materials and reagents used are commercially available.

[0019] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are only for illustrating the present invention and should not be regarded as limiting the scope of the present invention.

[0020] Example 1 A cement plant controls the clinker saturation ratio (KH) at 0.895±0.15. The 28-day compressive strength is relatively good, around 61 MPa, but the 3-day compressive strength is low, around 32 MPa. To stabilize the 28-day compressive strength at a good level and further improve the 3-day compressive strength, the following methods are adopted for control and optimization. The specific steps are as follows: 1) Take a comprehensive clinker sample retained daily for each hour, add 4% refined gypsum (grade not less than 95%, to avoid impurities introduced by grade fluctuations, thus affecting the stability of XRD analysis results). Prepare clinker samples using a standard test mill according to GB / T 21372 "Silicate Cement Clinker". Then, perform 3-day and 28-day compressive strength tests on the clinker, and simultaneously perform quantitative X-ray diffraction (XRD) analysis to obtain the contents of four main minerals in silicate clinker: mineral A (C3S), mineral B (C2S), aluminum phase (C3A), and iron phase (C4AF) and their related crystal forms. Among them, C3S includes two crystal forms, M1-C3S and M3-C3S; C3A includes two crystal forms, cubic C3A and orthorhombic C3A; and C2S includes α-C2S, α... H -C2S, β-C2S, and γ-C2S.

[0021] 2) Collect sample data on the XRD mineral composition and crystal content of clinker and the 3-day and 28-day compressive strength of clinker over a period of time.

[0022] 3) The C2S content of B ore (all crystal forms) in the routine clinker XRD analysis was statistically analyzed by mineral composition and strength zoning, with the 3-day and 28-day compressive strength of the clinker as the basis. The C2S content (%) was divided into 9 different intervals: <6, [6,8), [8,10), [10,12), [12,14), [14,16), [16,18), [18,20), and ≥20. Then, the number, proportion, and mean strength of the 3-day compressive strength (MPa) of the clinker in these 9 different intervals were counted. The distribution ratio and mean trend of the 3-day compressive strength under different C2S content (%) intervals were plotted. Similarly, the distribution ratio and mean trend of the 28-day compressive strength under different C2S content (%) intervals were plotted. The results are shown in the figure below. Figure 1 and Figure 2 As shown, the early 3-day compressive strength of clinker decreases with increasing C2S content, especially the proportion of clinker with ≥36 MPa decreases significantly, while the 28-day compressive strength first increases and then decreases. Therefore, while ensuring the 28-day compressive strength of clinker remains around 61 MPa, the 3-day strength of clinker should be increased as much as possible. The C2S content of clinker samples from small grinding mills should be controlled between 8% and 12%. When it is around 10%, the average 3-day and 28-day strengths are above 35 MPa and 60 MPa, respectively, and the proportions with values ​​below 34 MPa and 60 MPa are relatively small. Using this mineral composition and strength zoning statistical method, compared with other software that uses the probability density function method (based on the jointplot function in the Seaborn library of Python) to draw the strength and mineral composition distribution map, this method is superior. Figures 3-4 This allows for a clearer and more intuitive understanding of the appropriate mineral content.

[0023] 4) A stepwise multiple linear regression analysis was used to establish the correlation between C2S content in clinker and clinker weight per liter, f-CaO, and chemical composition (including non-calcium, silicon, aluminum, iron, and other heterogeneous elements such as MgO and SO3). After significance testing and elimination of collinearly correlated variables (the variance expansion factor (VIF) of the independent variables generally does not exceed 10), the factors that significantly affected clinker C2S content were found to be magnesium oxide content (MgO, %), clinker saturation ratio (KH), sulfur trioxide content (SO3, %), potassium oxide content (K2O, %), and weight per liter (g / L). The summary results of the stepwise regression analysis of clinker C2S content are shown in Table 1, including the correlation coefficient (R) and determination coefficient (R²) after stepwise inclusion of independent variables. 2 ), and the coefficient of determination of the corrected degrees of freedom (adjusted R) 2The regression coefficients and statistical analysis results of the clinker C2S content are shown in Table 2, including the regression coefficients of each independent variable and their t-test results, as well as the collinearity judgment between independent variables (tolerance and variance inflation factor VIF).

[0024] Table 1. Summary results of stepwise regression analysis of C2S content in clinker

[0025] Table 2. Regression coefficients and statistical analysis results of C2S content in clinker

[0026] From Table 2, the multivariate linear regression equation is: C2S content (%) = 234.015 - 7.391 MgO (%) -247.406 KH - 16.142 K2O (%) + 0.017 Weight per liter (g / L) - 7.541 SO3 (%) + 22.119 Na2O (%). Currently, the approximate clinker content levels are: MgO (%) = 1.50, K2O (%) = 0.75, mass per liter (g / L) = 1300, SO3 (%) = 0.38, and Na2O (%) = 0.19. The suitable C2S content (%) obtained from step 3) is 10. Substituting this into the above multiple linear regression equation, the suitable saturation ratio KH for clinker can be calculated as 0.906. Therefore, the actual clinker saturation ratio is adjusted to KH = 0.905 ± 0.15. Table 3 shows the three ratios (saturation ratio KH, silicon ratio SM, aluminum ratio IM) and 3-day and 28-day compressive strengths of the clinker before and after adjustment (Comparative Example 1 and Comparative Example 2). It can be seen that the 3-day compressive strength of the clinker increased from 32.4 MPa to 34.8 MPa, while the 28-day compressive strength remained unaffected.

[0027] Table 3. Clinker parameters before and after adjusting the saturation ratio

[0028] 5) Stepwise multiple linear regression analysis was used to establish the correlation between the 3d and 28d compressive strength of clinker and the clinker liter weight, f-CaO, content of impurities (MgO, SO3 and other non-calcium, silicon, aluminum and iron elements), and mineral composition and crystal form content of clinker. After significance testing and elimination of collinearly correlated variables (the variance expansion factor (VIF) of the independent variable generally does not exceed 10), the factors that have a significant impact on the 3d and 28d compressive strength of clinker were finally obtained (the specific results are shown in Tables 4-7).

[0029] Table 4. Summary of Stepwise Regression Analysis Results for 3d Compressive Strength of Clinker

[0030] Table 5 Regression coefficients and statistical analysis results of 3d compressive strength of clinker

[0031] Table 6. Summary of Stepwise Regression Analysis Results for 28-Day Clinker Compressive Strength

[0032] Table 7 Regression coefficients and statistical analysis results of clinker compressive strength at 28 days

[0033] It can be seen that SO3, β-C2S, M1-C3S, and MgO have a significant impact on 3d compressive strength. Among the impurity elements, only SO3 accounts for 50% or more of the total F change value, i.e., 125.702 / (125.702+24.633+10.74+11.847)=72.69%. Furthermore, SO3 has a synergistic effect on both 3d and 28d compressive strength of clinker (SO3 only has a significant effect on 3d compressive strength). Therefore, SO3 can be directly identified as an important influencing factor and used as a direction for optimization and improvement; that is, increasing SO3 content can improve the 3d compressive strength of clinker. Regarding the influence of mineral composition and crystal form on clinker strength, M1-C3S, M3-C3S, β-C2S, and C3A have a synergistic effect. Stepwise multiple linear regression analysis was performed on them, and the results are shown in Tables 8-15.

[0034] Table 8 Summary of Stepwise Regression Analysis Results for M1-C3S Content in Clinker

[0035] Table 9 Regression coefficients and statistical analysis results of M1-C3S content in clinker

[0036] Table 10 Summary of Stepwise Regression Analysis Results for M3-C3S Content in Clinker

[0037] Table 11 Regression coefficients and statistical analysis results of M3-C3S content in clinker

[0038] Table 12 Summary of Stepwise Regression Analysis Results for Clinker β-C2S Content

[0039] Table 13 Regression coefficients and statistical analysis results of clinker β-C2S content

[0040] Table 14 Summary of Stepwise Regression Analysis Results for C3A Content in Clinker

[0041] Table 15 Regression coefficients and statistical analysis results of C3A content in clinker

[0042] Among the significant influencing factors, the chemical components that affect the mineral composition and crystal content, and thus have a positive or negative impact on both 3d and 28d compressive strength (including chemical components that only affect the strength at one of the 3d and 28d ages) are identified as Al2O3 (aluminum ratio IM or Fe2O3) and Na2O. For example, increasing the Al2O3 content (increasing the aluminum ratio IM and decreasing the Fe2O3 content) can increase the M1-C3S and C3A content and decrease the M3-C3S content, while having no significant effect on the β-C2S content, thereby improving the 3d and 28d compressive strength of the clinker. On the other hand, decreasing Na2O can increase the M1-C3S content and decrease the β-C2S content, while having no significant effect on the M3-C3S and C3A content, thereby improving the 3d and 28d compressive strength of the clinker. Other chemical components cannot simultaneously benefit the 3-day or 28-day compressive strength of clinker. For example, increasing the MgO content can increase the M1-C3S content and decrease the β-C2S content (which is beneficial to clinker strength), but it also increases the M3-C3S and C3A content (which is detrimental to clinker strength).

[0043] 6) In step 5), the directions for optimizing and improving clinker strength were identified, mainly including increasing the SO3 and Al2O3 content (increasing the aluminum ratio IM and decreasing the Fe2O3 content) and decreasing the Na2O content. Based on the current factory conditions, increasing the SO3 and Al2O3 content (increasing the aluminum ratio IM and decreasing the Fe2O3 content) is relatively easy to achieve, which can be done by introducing low-cost sulfur-containing materials (such as phosphogypsum, titanium gypsum, and other industrial by-product gypsum) and increasing the amount of aluminum materials (reducing the amount of iron materials). However, the Na2O content is affected by various silicon-aluminum materials and is more difficult to change. Therefore, the SO3 content (%) of the clinker was increased from 0.38 to 0.60, and the sulfur-alkali ratio was increased from 0.38 / 80 / [(0.19+0.75)]. [0.658) / 62]=0.43 increased to 0.60 / 80 / [(0.19+0.75] [0.658) / 62]=0.68. The Al2O3 content (%) of the clinker increased from about 5.10 to about 5.20, the Fe2O3 content (%) decreased from about 3.30 to about 3.15, and the aluminum ratio IM increased from about 1.55 to about 1.65.

[0044] 7) Based on the modified and optimized parameters, and according to the suitable C2S content (%) = 10, it is substituted into the multiple linear regression equation in step 4) to calculate the suitable saturation ratio KH = 0.900 for clinker. Combining the parameters adjusted in step 6), the optimized clinker production was carried out, and the results of the clinker's 3d and 28d compressive strength and other indicators are shown in Table 3, Example 1. It can be seen that the 3d compressive strength of the clinker has been further improved, and the 28d compressive strength has also been slightly improved.

[0045] The above embodiments describe preferred embodiments of the present invention, but the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other way. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.

Claims

1. A method for improving the strength of silicate clinker based on mineral and crystal composition analysis, characterized in that, Includes the following steps: S1. The clinker produced in industrial production is ground with dihydrate gypsum. A portion of the resulting sample is tested for 3-day and 28-day compressive strength, and the other portion is subjected to XRD quantitative analysis of mineral and crystal composition. Data on the 3-day and 28-day compressive strength of the clinker, as well as the content of C3S, C2S, C3A and C4AF minerals and their related crystal forms in the clinker are obtained respectively. S2. Collect data from S1 over a period of time and perform statistical analysis on the obtained data. Specifically, based on XRD analysis, determine the appropriate relative contents of C3S and C2S in clinker by using a mineral composition and strength zoning statistical method with the 3-day and 28-day compressive strength of clinker. Then, establish the correlation between the C3S or C2S content in clinker and the clinker weight per liter, f-CaO, and other chemical components using stepwise multiple linear regression analysis. Based on the obtained appropriate relative contents of C3S and C2S and the correlation between the C3S or C2S content and the clinker weight per liter, f-CaO, and other chemical components, calculate the appropriate control saturation ratio of clinker. Control the production of clinker according to this saturation ratio to maintain the relative contents of C3S and C2S in clinker at an appropriate level, thereby maintaining the overall improvement of the 3-day and 28-day compressive strength of silicate clinker.

2. The method according to claim 1, characterized in that: S1 contains 4 wt% gypsum added to clinker produced industrially; C3S includes two crystal forms, M1-C3S and M3-C3S; C3A includes two crystal forms, cubic C3A and orthorhombic C3A; C2S includes α-C2S and α-C3A. H There are four crystal forms: -C2S, β-C2S, and γ-C2S.

3. The method according to claim 1, characterized in that: Each test in S1 is recorded as one sample size. In S2, data on compressive strength and mineral and related crystal content are collected over a period of time, with a sample size ≥ 90.

4. The method according to claim 1, characterized in that: The S2 method for mineral composition and strength zoning statistical analysis involves dividing the C3S or C2S content in clinker into multiple different intervals, then statistically analyzing the number, proportion, and average strength of the 3-day compressive strength of clinker in different strength intervals, and plotting the distribution ratio and average trend of different 3-day compressive strengths under different C3S or C2S content intervals. Similarly, plotting the distribution ratio and average trend of different 28-day compressive strengths under different intervals is also performed. The appropriate relative content of C3S and C2S refers to the value of C3S and C2S content or a certain range within which the overall 3-day and 28-day compressive strength of silicate clinker can be improved.

5. The method according to claim 1, characterized in that: In addition to the conventional CaO, SiO2, Al2O3 and Fe2O3, other chemical components in S2 also include one or more of the heteroelement K2O, Na2O, MgO and SO3.

6. The method according to any one of claims 1 to 5, characterized in that: In S2, a stepwise multiple linear regression analysis was further used to establish the correlation between the 3-day and 28-day compressive strength of clinker and the clinker liter weight, f-CaO, impurity element content, and clinker mineral composition and crystal form content. Specifically, the impurity element influencing factor selection method was first used to identify the factors that have a significant impact on the 3-day and 28-day compressive strength from the significant influencing factors, which were directly used as the direction for optimization and improvement. Then, the mineral composition and crystal form influencing factors that have the same effect on the 3-day and 28-day compressive strength of clinker were selected from the significant influencing factors. The stepwise multiple linear regression analysis was used to establish the correlation between these mineral composition and crystal form contents and the clinker liter weight, f-CaO, and other chemical components. The chemical component influencing factors that affect these mineral composition and crystal form contents and thus have a positive or negative impact on the 3-day and 28-day compressive strength were identified from the significant influencing factors as the direction for further optimization and adjustment.

7. The method according to claim 6, characterized in that: The method for selecting factors influencing impurity elements is to select factors that have a significant impact on the dependent variables 3d and 28d compressive strength. Specifically, if the content of impurity elements has the same effect on the dependent variables 3d and 28d compressive strength, and in the process of establishing the correlation between the 3d and 28d compressive strength of clinker and clinker liter weight, f-CaO, impurity element content, and clinker mineral composition and crystal form content, respectively, using stepwise multiple linear regression analysis, the proportion of the change in the root mean square error (F value) corresponding to the impurity element content to the total change in F value reaches 50% or more, then it is directly identified as an important influencing factor.

8. The method according to claim 6, characterized in that: If a direction for optimization and improvement is found, after fine-tuning the component parameters, the appropriate control saturation ratio of the clinker is recalculated based on the suitable relative content of C3S and C2S in S2 and the correlation between the C3S or C2S content in the clinker and the clinker liter weight, f-CaO and other chemical components, so as to further optimize and improve the clinker strength.

9. The method according to claim 6, characterized in that: If no factor can be found that significantly affects the 3d and 28d compressive strength of clinker, or if a chemical component that significantly affects the 3d and 28d compressive strength of clinker but does not have a synergistic effect, then it indicates that mineral composition and crystal form regulation is not necessary at this time.

10. The method according to claim 6, characterized in that: Mineral composition and crystal form influencing factors that have a unidirectional effect on the 3-day and 28-day compressive strength of clinker refer to adjustments in mineral composition and crystal form that are simultaneously beneficial to the 3-day and 28-day compressive strength of clinker or simultaneously detrimental to the 3-day and 28-day compressive strength of clinker; or improve at least one of the strength indicators of 3-day and 28-day compressive strength of clinker without adversely affecting the other strength indicator.