A waterborne epoxy-isocyanate hybrid nanoreinforced coating and method of application thereof

By employing the time-sequence reaction control technology of waterborne epoxy-isocyanate hybrid nano-heavyweight anti-corrosion coatings, an organic-inorganic hybrid copolymer interpenetrating network was constructed. This solved the performance deficiencies of existing waterborne coatings in harsh environments, achieving a balance of high mechanical strength, chemical resistance, corrosion protection, and room temperature curing, making it suitable for various construction scenarios.

CN122356970APending Publication Date: 2026-07-10BEIJING HAIYAN TECHNOLOGY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610722948.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-25
Publication Date
2026-07-10

AI Technical Summary

Technical Problem

Existing water-based heavy-duty anti-corrosion coatings cannot achieve both ultra-high mechanical strength and ultra-strong chemical resistance and corrosion resistance in harsh environments, and cannot meet the requirements of room temperature curing and low VOC, which limits their applicability in various construction scenarios.

Method used

A waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating is used. The sequential reaction between isocyanate and epoxy groups is precisely controlled by a silane-modified alkali metal silicate aqueous solution catalyst to generate polyurea chains, oxazolidinone five-membered rings, isocyanurate six-membered rings and amorphous nano-silica particles in situ, thus constructing a highly homogeneous organic-inorganic hybrid copolymer interpenetrating network.

Benefits of technology

It achieves improved coating density, weather resistance, and mechanical properties, exhibits excellent resistance to neutral salt spray and good resistance to chemical media, is suitable for long-term protection in harsh environments, and meets the requirements of room temperature curing and low VOC.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention provides a waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating and its application method, relating to the field of heavy-duty anti-corrosion coating technology. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating provided by this invention includes a primer, which is composed of component A containing epoxy, component B containing isocyanate, and component C containing an aqueous catalyst in a specific ratio. The heavy-duty anti-corrosion coating provided by this invention achieves precise control of the sequential reaction between isocyanate and epoxy groups through the aqueous catalyst, generating in-situ polyurea chains, oxazolidinone five-membered rings, isocyanurate six-membered rings, and amorphous nano-silica particles, forming a highly homogeneous organic-inorganic hybrid copolymer interpenetrating network. The resulting coating possesses both ultra-high mechanical strength and superior chemical resistance and corrosion resistance, is safe and environmentally friendly, and can be widely used for long-term heavy-duty anti-corrosion protection in harsh corrosive environments in fields such as petrochemicals, energy, shipbuilding, marine engineering, infrastructure, and military equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heavy-duty anti-corrosion coatings, and in particular to a water-based epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating and its application method. Background Technology

[0002] Heavy-duty anti-corrosion coatings are core materials for ensuring the long-term service life of steel structures, concrete, and other substrates in harsh corrosive environments. They are widely used in critical fields such as petrochemicals, energy, shipbuilding, marine engineering, and infrastructure. Traditional solvent-based epoxy, polyurethane, and polyurea heavy-duty anti-corrosion coatings are limited due to their high VOC content, which is detrimental to environmental protection, and poses safety and occupational health risks during construction. Water-based heavy-duty anti-corrosion coatings are being increasingly widely adopted.

[0003] Water-based heavy-duty anti-corrosion coatings mainly include water-based epoxy coatings and water-based polyurea coatings. However, existing water-based heavy-duty anti-corrosion coatings struggle to achieve a balance between ultra-high mechanical strength and superior chemical resistance. Their salt spray resistance is mostly below 3000 hours, and under harsh environments such as strong acids and alkalis, high salt spray, and strong UV aging, they are prone to coating loss of gloss, chalking, cracking, and corrosion, failing to provide long-term protection of more than 10 years. Furthermore, existing water-based heavy-duty anti-corrosion coatings typically require high-temperature baking for curing, which cannot meet the room-temperature curing requirements for on-site application, limiting their applicability. Summary of the Invention

[0004] In view of this, the purpose of this invention is to provide a waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating and its application method. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating provided by this invention is a heavy-duty anti-corrosion coating system that cures at room temperature and possesses both ultra-high mechanical strength and ultra-strong chemical and weather resistance.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides an aqueous epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating, comprising a primer; the primer comprises separately packaged components A1, B1, and C1; The A1 component comprises the following components by mass percentage: 86-90% liquid epoxide, 8-12% pigments and fillers, and 1-3% additives; the B1 component comprises aromatic isocyanate and alicyclic isocyanate, wherein the mass ratio of aromatic isocyanate to alicyclic isocyanate is (80-100):(0-20); the C1 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, wherein the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A1 component, the B1 component and the C1 component is (40-50):(50-60):(17-27).

[0006] Preferably, the liquid epoxide in component A1 includes one or more of bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and epoxy reactive diluent; the pigments and fillers include one or more of titanium dioxide, carbon black, and barium sulfate; and the additives include rheology modifiers and / or defoamers.

[0007] Preferably, the aromatic isocyanate in component B1 includes polymeric MDI and / or polymeric MDI derivatives, and the alicyclic isocyanate includes 4,4'-dicyclohexylmethane diisocyanate and / or 4,4'-dicyclohexylmethane diisocyanate derivatives.

[0008] Preferably, the aqueous catalyst of component C1 is C30 aqueous curing agent provided by Beijing Haiyan Technology Co., Ltd.

[0009] Preferably, the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating further includes a topcoat; the topcoat includes separately packaged components A2, B2, and C2. The A2 component comprises the following components by mass percentage: 62-70% liquid epoxide, 28-36% pigments and fillers, and 1-3% additives; the B2 component comprises aliphatic isocyanate and alicyclic isocyanate, wherein the mass ratio of the aliphatic isocyanate to the alicyclic isocyanate is (40-60):(40-60); the C2 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, and the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A2 component, the B2 component and the C2 component is (40-50):(50-60):(17-27).

[0010] Preferably, the liquid epoxide in component A2 includes one or more of bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and epoxy reactive diluent; the pigments and fillers include one or more of titanium dioxide, carbon black, and barium sulfate; and the additives include one or more of rheology modifiers, defoamers, and organometallic salt catalysts.

[0011] Preferably, the aliphatic isocyanate in component B2 includes one or more of hexamethylene diisocyanate, hexamethylene diisocyanate dimer, hexamethylene diisocyanate trimer, hexamethylene diisocyanate derivative, hexamethylene diisocyanate dimer derivative, and hexamethylene diisocyanate trimer derivative, and the alicyclic isocyanate includes 4,4'-dicyclohexylmethane diisocyanate and / or 4,4'-dicyclohexylmethane diisocyanate derivative.

[0012] This invention provides a waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion topcoat, comprising separately packaged components A2, B2, and C2; The A2 component comprises the following components by mass percentage: 62-70% liquid epoxide, 28-36% pigments and fillers, and 1-3% additives; the B2 component comprises aliphatic isocyanate and alicyclic isocyanate, wherein the mass ratio of the aliphatic isocyanate to the alicyclic isocyanate is (40-60):(40-60); the C2 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, and the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A2 component, the B2 component and the C2 component is (40-50):(50-60):(17-27).

[0013] This invention provides a method for applying the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating described above, wherein the application of the primer includes the following steps: Mix components A1, B1, and C1 to obtain the primer; The primer is applied to the surface of the workpiece and cured for the first time to form a primer coating; the first curing is at room temperature.

[0014] Preferably, when the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating further includes a topcoat, the application of the topcoat includes the following steps: mixing components A2, B2 and C2 to obtain the topcoat, applying the topcoat to the surface of the primer coating, and subjecting it to a second curing process to form a topcoat coating; the second curing process is room temperature curing.

[0015] This invention provides a waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating, comprising a primer, wherein the primer is composed of component A containing epoxy, component B containing isocyanate, and component C containing an aqueous catalyst in a specific ratio. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating provided by this invention precisely controls the sequential reaction between isocyanate and epoxy groups through the aqueous catalyst, generating in situ polyurea chains, oxazolidinone five-membered rings, isocyanurate six-membered rings, and amorphous nano-silica particles, forming a highly homogeneous organic-inorganic hybrid copolymer interpenetrating network. Compared with the prior art, this invention has the following beneficial effects: Superior chemical resistance, corrosion resistance, and weather resistance: The coating is highly dense, with no blistering, rust, or significant decrease in adhesion after ≥6000h of neutral salt spray resistance; it withstands immersion in 50% sulfuric acid, 50% sodium hydroxide, and 37% sodium chloride solutions for ≥6000h without any abnormalities; after ≥3000h of QUV ultraviolet aging, the gloss loss rate is ≤10%, with no chalking or cracking, achieving long-term protection for more than 15 years in harsh environments; Breakthrough in mechanical properties: The constructed interpenetrating network takes into account both rigidity and toughness, with coating pull-out adhesion ≥20MPa (carbon steel substrate), impact resistance ≥50cm, pencil hardness ≥3H, and abrasion resistance (1000g / 1000r) ≤30mg, far exceeding the level of conventional heavy-duty anti-corrosion coatings. Cures at room temperature and has wide applicability: No high-temperature baking is required; it can be cured normally at temperatures above 10°C. It is suitable for various construction scenarios, such as factory prefabrication and on-site repair, and can be used on a variety of substrates, including carbon steel, stainless steel, concrete, and galvanized sheet. Excellent environmental performance: The coating system of this invention is a water-based hybrid system with VOC content approaching zero, far below the national environmental protection standard GB38507-2020. It has no irritating odor and is safe and environmentally friendly during construction. Highly controllable reaction and wide application window: The time-series reaction is precisely controlled through the interface effect of the aqueous catalyst, and the working period after mixing is ≥60 minutes, making it suitable for various on-site construction scenarios; Good storage stability: Components A, B, and C are stored separately, with a shelf life of ≥12 months.

[0016] The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating provided by this invention has both ultra-high mechanical strength and ultra-strong chemical resistance and weather resistance, and can be widely used in the field of petrochemical, energy, shipbuilding, marine engineering, infrastructure, military equipment and other fields for long-term heavy-duty anti-corrosion protection in harsh corrosive environments. Detailed Implementation

[0017] This invention provides an aqueous epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating, comprising a primer; the primer comprises separately packaged components A1, B1, and C1; The A1 component comprises the following components by mass percentage: 86-90% liquid epoxide, 8-12% pigments and fillers, and 1-3% additives; the B1 component comprises aromatic isocyanate and alicyclic isocyanate, wherein the mass ratio of aromatic isocyanate to alicyclic isocyanate is (80-100):(0-20); the C1 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, wherein the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A1 component, the B1 component and the C1 component is (40-50):(50-60):(17-27).

[0018] Unless otherwise specified, all components involved in this invention are commercially available products in the field.

[0019] In this invention, the mass percentage of liquid epoxide in component A1 can be 87%, 88%, 89%, or 90%, the mass percentage of pigments and fillers can be 8%, 9%, 10%, 11%, or 12%, and the mass percentage of additives can be 1%, 2%, or 3%. In this invention, the liquid epoxide preferably comprises one or more of bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and epoxy reactive diluent, more preferably bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and epoxy reactive diluent. The mass ratio of the bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and epoxy reactive diluent is preferably 33:23:31. The bisphenol A epoxy resin provides basic mechanical strength and chemical resistance, the hydrogenated bisphenol A epoxy resin improves weather resistance and flexibility, and the epoxy reactive diluent reduces viscosity. In embodiments of the present invention, the bisphenol A epoxy resin preferably includes one or more of Epon Resin 828 (Hexion), DER 331 (Dow), Araldite 250 (Huntsman), and NPEL-128 (Nan Ya); the hydrogenated bisphenol A epoxy resin preferably includes one or more of Eponex Resin 1510 (Hexion), EP-4080E (Adeka), ST-3000 (Kukdo), Epalloy 5000 (CVC), and XY518 (Anhui Xinyuan Technology Co., Ltd.); and the epoxy reactive diluent preferably includes one or more of Ultra LITE 513 (Cardolite), HeloxyModifier HD (Hexion), Araldite DY-H (Huntsman), Erisys GE 25 (CVC), and XY632 (Anhui Xinyuan Technology Co., Ltd.). In this invention, the pigments and fillers preferably include one or more of titanium dioxide (such as titanium dioxide), carbon black, and barium sulfate. In this invention, the additives preferably include rheology modifiers and / or defoamers, more preferably rheology modifiers and defoamers, with a preferred mass ratio of 2.2:0.8; in an embodiment of this invention, the rheology modifier is specifically Crayvallac Optima (Arkema), and the defoamer is specifically BYK-1794 (BYK).

[0020] In this invention, component B1 comprises aromatic isocyanate and alicyclic isocyanate, wherein the mass ratio of aromatic isocyanate to alicyclic isocyanate is (80~100):(0~20), which can be 100:0, 90:10, or 80:20. In this invention, the aromatic isocyanate preferably comprises polymeric MDI (a mixture of 4,4'-diphenylmethane diisocyanate with highly functional isomers and homologues) and / or polymeric MDI derivatives; the alicyclic isocyanate preferably comprises 4,4'-dicyclohexylmethane diisocyanate (HMDI) and / or 4,4'-dicyclohexylmethane diisocyanate derivatives. In embodiments of the present invention, the aromatic isocyanate is specifically one or more of Suprasec 5005 (Huntsman), Desmodur 44V20L (Covestro), Lupranate M20 (BASF), and Wannate PM-200 (Wanhua), and the alicyclic isocyanate is specifically Vestanat H. 12 One or more of MDI (Evonik), Desmodur W (Covestro), and Wannate HMDI (Wanhua). In this invention, the primer is selected from aromatic isocyanates or combinations of aromatic isocyanates / alicyclic isocyanates, whose high functionality is beneficial for forming a high crosslinking density.

[0021] In this invention, the C1 component is an aqueous catalyst, which is a silane-modified alkali metal silicate aqueous solution. The solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%, which can be 35-55 wt%, and the content of the alkali metal oxide is 10-18 wt%, which can be 12-16 wt%. In this invention, the aqueous catalyst is preferably a C30 aqueous curing agent provided by Beijing Haiyan Technology Co., Ltd. In this invention, the functions of the aqueous catalyst include: time-series regulation, emulsion stabilization, in-situ production of nano-silica gel, and silane coupling bonding.

[0022] In this invention, the mass ratio of component A1, component B1, and component C1 is (40~50):(50~60):(17~27), ​​preferably 45:55:(17~27, but can be 45:55:17, 45:55:22, or 45:55:27. By controlling the mass ratio of component A1, component B1, and component C1, this invention ensures that each reaction step proceeds in equilibrium, forming a homogeneous and dense interpenetrating network.

[0023] In this invention, the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating preferably includes a topcoat; the topcoat includes separately packaged components A2, B2, and C2. The A2 component comprises the following components by mass percentage: 62-70% liquid epoxide, 28-36% pigments and fillers, and 1-3% additives; the B2 component comprises aliphatic isocyanate and alicyclic isocyanate, wherein the mass ratio of the aliphatic isocyanate to the alicyclic isocyanate is (40-60):(40-60); the C2 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, and the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A2 component, the B2 component and the C2 component is (40-50):(50-60):(17-27).

[0024] In this invention, the mass percentage of liquid epoxide in component A2 can be 64%, 65%, 66%, 67%, or 68%, the mass percentage of pigments and fillers can be 30%, 31%, 32%, 33%, 34%, or 35%, and the mass percentage of additives can be 1%, 2%, or 3%. In this invention, the liquid epoxide preferably includes one or more of bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and epoxy reactive diluent, more preferably hydrogenated bisphenol A epoxy resin and epoxy reactive diluent, and the mass ratio of hydrogenated bisphenol A epoxy resin to epoxy reactive diluent is preferably 36:30. In this embodiment of the invention, the bisphenol A epoxy resin is specifically one or more of Epon Resin 828 (Hexion), DER 331 (Dow), Araldite 250 (Huntsman), and NPEL-128 (Nan Ya); the hydrogenated bisphenol A epoxy resin is specifically one or more of EponexResin 1510 (Hexion), EP-4080E (Adeka), ST-3000 (Kukdo), Epalloy 5000 (CVC), and XY518 (Anhui Xinyuan Technology Co., Ltd.); and the epoxy reactive diluent is specifically one or more of Ultra LITE 513 (Cardolite), Heloxy Modifier HD (Hexion), Araldite DY-H (Huntsman), Erisys GE 25 (CVC), and XY632 (Anhui Xinyuan Technology Co., Ltd.). In this invention, the pigments and fillers preferably include one or more of titanium dioxide (such as titanium dioxide), carbon black, and barium sulfate. In this invention, the additives preferably include one or more of a rheology modifier, a defoamer, and an organometallic salt catalyst, more preferably a rheology modifier, a defoamer, and an organometallic salt catalyst, with a preferred mass ratio of 1.2:0.7:0.1. In an embodiment of this invention, the rheology modifier is specifically Crayvallac Optima (Arkema), the defoamer is specifically BYK-1794 (BYK), and the organometallic salt catalyst is specifically TCAT-S029 (Guangzhou Yourun Synthetic Materials Co., Ltd.). The organometallic salt catalyst can accelerate the reaction rate of aliphatic isocyanates.

[0025] In this invention, component B2 comprises aliphatic isocyanates and alicyclic isocyanates, wherein the mass ratio of the aliphatic isocyanate to the alicyclic isocyanate is (40~60):(40~60), which can be 40:60, 50:50, or 60:40. Preferably, the aliphatic isocyanate comprises one or more of hexamethylene diisocyanate (HDI), hexamethylene diisocyanate dimer (HDI ureadione), hexamethylene diisocyanate trimer (HDI trimer), hexamethylene diisocyanate derivatives, hexamethylene diisocyanate dimer derivatives, and hexamethylene diisocyanate trimer derivatives; the alicyclic isocyanate preferably comprises 4,4'-dicyclohexylmethane diisocyanate (HMDI) and / or 4,4'-dicyclohexylmethane diisocyanate derivatives. In embodiments of the present invention, the aliphatic isocyanate is specifically one or more of Desmodur N 3600 (Covestro), Desmodur N 3900 (Covestro), Tolonate HDT-LV2 (Vencorex), Coronate HXLV (Tosoh), Wannate HT-500 (Wanhua), Wannate HT-600 (Wanhua), and Desmodur 3400 (Covestro), and the alicyclic isocyanate is specifically Vestanat H 12 One or more of MDI (Evonik), Desmodur W (Covestro), and Wannate HMDI (Wanhua). In this invention, the topcoat uses a combination of aliphatic / alicyclic isocyanates to ensure both weather resistance and reactivity.

[0026] In this invention, the C2 component is an aqueous catalyst, which is a silane-modified alkali metal silicate aqueous solution. The solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%, which can be 35-55 wt%, and the alkali metal oxide content is 10-18 wt%, which can be 12-16 wt%. In this invention, the aqueous catalyst is preferably a C30 aqueous curing agent provided by Beijing Haiyan Technology Co., Ltd.

[0027] In this invention, the mass ratio of component A2, component B2, and component C2 is (40~50):(50~60):(17~27), ​​preferably 45:55:(17~27, but can be 45:55:17, 45:55:22, or 45:55:27. By controlling the mass ratio of component A2, component B2, and component C2, this invention ensures that each reaction step proceeds in equilibrium, forming a homogeneous and dense interpenetrating network.

[0028] In this invention, the preferred method for preparing component A1 is to mix all components in component A1 evenly, disperse or grind them at high speed to a fineness ≤30µm, and then filter and package them to obtain component A1. In this invention, the preferred method for preparing component B1 is to mix all components in component B1 evenly, filter and package them to obtain component B1. In this invention, the preparation methods for components A2 and B2 are the same as those for components A1 and B1, respectively. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating of this invention can be produced using production equipment and processes commonly used in the coating industry.

[0029] In this invention, both the primer and topcoat are three-component systems that cure at room temperature, determining the coating's adhesion, mechanical strength, chemical and corrosion resistance, weather resistance, and workability. The primer emphasizes high adhesion and chemical and corrosion resistance, while the topcoat emphasizes weather resistance. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating provided by this invention achieves a balance between ultra-high mechanical properties and ultra-strong chemical and corrosion resistance, while also meeting the requirements of room temperature curing, low VOC environmental protection, and a wide application window.

[0030] This invention precisely controls the sequential reaction between isocyanate and epoxy groups using the aforementioned aqueous catalyst. During the curing process, polyurea chains, oxazolidinone five-membered rings, isocyanurate six-membered rings, and amorphous nano-silica particles are generated in situ. A highly homogeneous organic-inorganic hybrid copolymer interpenetrating network is constructed through chemical bonding and physical interpenetration, addressing the performance shortcomings of existing systems at the molecular structure level and achieving long-lasting heavy-duty corrosion protection. The specific reaction principle and network construction mechanism are as follows (through the water-in-oil emulsion interface effect of the aqueous catalyst, the five-step reaction is carried out in an orderly and controllable manner, ultimately forming the target cross-linked network): Step 1 (Isocyanate Interfacial Hydrolysis): The aqueous catalyst is dispersed in isocyanate and epoxide to form a water-in-oil emulsion. At the emulsion interface, isocyanate hydrolysis occurs preferentially to generate carbamic acid intermediate, which further decomposes into primary amine and releases carbon dioxide. Step 2 (In-situ generation of polyurea chains): The primary amine generated in situ undergoes a rapid nucleophilic addition reaction with the isocyanate to form flexible polyurea segments with high toughness and high strength, providing basic adhesion and impact resistance for the coating. The third step (in-situ sol-gel reaction of inorganic phase): The carbon dioxide released by hydrolysis reacts in-situ with the alkali metal silicate in the aqueous catalyst to generate amorphous nano silica particles and carbonate crystals, realizing molecular-level dispersion of the inorganic phase and avoiding the problems of nanoparticle agglomeration and severe phase separation in physical blending. Step 4 (formation of the five-membered ring of oxazolidinone): The epoxy group undergoes a cycloaddition reaction with the isocyanate group to form a rigid five-membered ring structure of oxazolidinone with excellent resistance to chemical media and heat, thereby improving the corrosion resistance and heat resistance of the coating. Step 5 (formation of six-membered isocyanurate ring): Under catalysis, the remaining isocyanate undergoes trimerization to form a six-membered isocyanurate ring structure with high cross-linking density and high chemical stability, further improving the coating's weather resistance and resistance to media penetration. Through the above sequential reaction, a highly homogeneous organic-inorganic hybrid copolymer interpenetrating network is finally formed, consisting of polyurea flexible chains, oxazolidinone / isocyanurate rigid rings, and in-situ nano-silica particles through chemical bonding and physical interpenetration. This achieves high strength, high toughness, high density, and super chemical resistance and corrosion resistance of the coating.

[0031] The innovative aspects of this invention include the following: The pioneering time-sequence reaction precision control technology uses silane-modified alkali metal silicate aqueous solution as an aqueous catalyst. Through the water-in-oil emulsion interface effect, it realizes the orderly and controllable five-step reaction of isocyanate hydrolysis, polyurea generation, in-situ inorganic phase nucleation, and oxazolidinone / isocyanurate cyclization, which solves the core pain points of uncontrollable reaction and short pot life of traditional epoxy-isocyanate system. In-situ construction of organic-inorganic hybrid interpenetrating networks: Polyurea chains, rigid heterocycles and nano-silica particles are generated through in-situ reactions to achieve molecular-level dispersion of the inorganic phase, avoiding the problems of agglomeration and phase separation in physical blending, and constructing a highly homogeneous chemically bonded interpenetrating network, achieving a balance between ultra-high mechanical strength and ultra-strong chemical resistance and corrosion resistance at the molecular structure level. Breakthrough in overall performance: A complete primer + topcoat system has been developed. The primer has excellent adhesion and outstanding anti-corrosion performance, while the topcoat has good weather resistance. It also achieves the comprehensive advantages of room temperature curing, low VOC environmental protection, and a wide application window, making it suitable for various on-site construction scenarios and enabling long-term protection for more than 15 years in harsh environments. Dual-function catalyst design: The aqueous catalyst simultaneously undertakes the dual functions of "reaction timing regulation" and "inorganic phase precursor", which not only realizes the precise control of multi-step reaction, but also participates in the construction of inorganic phase in situ, simplifies the formulation system, improves the homogeneity and stability of the network, and provides a new approach for the development of organic-inorganic hybrid coatings.

[0032] The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating provided by this invention can be used for corrosion protection of metal components, concrete components, and steel structures. In this invention, the metal components can specifically be steel structures, galvanized sheets, etc. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating provided by this invention can be widely used for long-term heavy-duty corrosion protection in harsh corrosive environments in fields such as petrochemicals, energy, shipbuilding, marine engineering, infrastructure, and military equipment.

[0033] This invention provides a waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion topcoat, comprising separately packaged components A2, B2, and C2; The A2 component comprises the following components by mass percentage: 62-70% liquid epoxide, 28-36% pigments and fillers, and 1-3% additives; the B2 component comprises aliphatic isocyanate and alicyclic isocyanate, wherein the mass ratio of the aliphatic isocyanate to the alicyclic isocyanate is (40-60):(40-60); the C2 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, and the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A2 component, the B2 component and the C2 component is (40-50):(50-60):(17-27).

[0034] In this invention, the specific compositions of components A2, B2 and C2 are the same as those in the above technical solution, and will not be repeated here.

[0035] This invention provides a method for applying the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating described above, wherein the application of the primer includes the following steps: Mix components A1, B1, and C1 to obtain the primer; The primer is applied to the surface of the workpiece and cured for the first time to form a primer coating.

[0036] In this invention, the preferred method for mixing components A1, B1 and C1 is as follows: components A1 and B1 are mixed evenly according to the ratio, component C1 is added to them under stirring conditions, and then dispersed at a medium speed (300~1000 rpm, or 500 rpm) for 3~5 minutes.

[0037] Before coating, the present invention preferably performs sandblasting on the surface of the workpiece, and the sandblasting preferably achieves a surface roughness of 25~50µm.

[0038] In this invention, when the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating further includes a topcoat, the application of the primer preferably includes the following steps: mixing components A2, B2 and C2 to obtain the topcoat, applying the topcoat to the surface of the primer coating, and curing it a second time to form a topcoat coating.

[0039] In this invention, the method of mixing components A2, B2 and C2 is the same as the method of mixing components A1, B1 and C1.

[0040] In this invention, the mixing of components A1, B1, and C1, as well as the mixing of components A2, B2, and C2, preferably includes a curing process, the curing time of which is 5-15 minutes (10 minutes is acceptable). In this invention, the curing process serves to: allow the coating system to undergo initial reaction, stabilize, degas, optimize rheology, and ensure the quality of the paint film.

[0041] This invention does not impose any special requirements on the application methods of the primer and topcoat; any application method well-known to those skilled in the art, such as spraying, brushing, or roller coating, can be used. The preferred application conditions are: air and substrate temperature of 10-40°C, relative humidity of 10-80%, and paint temperature of 15-25°C. In this embodiment, the application is carried out at room temperature and under natural ambient humidity.

[0042] In this invention, both the first curing and the second curing are performed at room temperature, and the preferred curing times for the first curing and the second curing are 1 to 7 days.

[0043] In this invention, when the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating is used as an internal coating, only a primer needs to be applied. The thickness of the primer coating is preferably 250-350 micrometers, and can be 300 micrometers. When the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating is used as an external coating, a topcoat is applied after the primer coating. The thickness of the primer coating is preferably 100-200 micrometers, and can be 150 micrometers. The thickness of the topcoat coating is preferably 75-125 micrometers, and can be 100 micrometers.

[0044] To further illustrate the present invention, the following detailed description, in conjunction with examples, of the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating and its application method provided by the present invention, shall not be construed as limiting the scope of protection of the present invention.

[0045] Example 1: Primer preparation, coating and performance testing Component A1 (by mass percentage) has the following composition: Bisphenol A epoxy resin (NPEL-128): 33%; Hydrogenated bisphenol A epoxy resin (Eponex Resin 1510): 23%; Epoxy Reactive Diluent (Araldite DY-H): 31%; Rheology modifier (Crayvallac Optima): 2.2%; Pigment (titanium dioxide): 10%; Defoamer (BYK-1794): 0.8%.

[0046] Component B1 (by mass percentage) has the following composition: Aromatic isocyanate (Wannate PM-200): 100%.

[0047] The composition of component C1 (by mass percentage) is as follows: Water-based catalyst (C30 water-based curing agent, Beijing Haiyan Technology Co., Ltd.): 100%.

[0048] Preparation of component A1: Mix all components in component A1 evenly, grind to a fineness ≤30µm, then filter and package to obtain component A1; Preparation of component B1: The isocyanate was mixed evenly, filtered and packaged to obtain component B1; Preparation of C1 component: The aqueous catalyst was mixed evenly, filtered and packaged to obtain C1 component.

[0049] Before application, mix the components evenly according to the mass ratio (mass ratio: component A1: component B1: component C1 = 45:55:17). Specifically, mix component A1 and component B1 evenly according to the ratio, add component C1 while stirring, then disperse at medium speed (500 rpm) for 5 minutes, and cure for 10 minutes. After that, apply the resulting primer to a sandblasted steel plate (Sa 2.5 grade, roughness 25~50µm) using high pressure airless spraying, control the dry film thickness to be 300±50µm, and then place the sample at room temperature to cure for 7 days.

[0050] The performance of the cured test panels was tested, and the results are shown in Table 1.

[0051] Example 2: Primer preparation, coating and performance testing Component A1 (by mass percentage) has the following composition: Bisphenol A epoxy resin (NPEL-128): 33%; Hydrogenated bisphenol A epoxy resin (Eponex Resin 1510): 23%; Epoxy Reactive Diluent (Araldite DY-H): 31%; Rheology modifier (Crayvallac Optima): 2.2%; Pigment (titanium dioxide): 10%; Defoamer (BYK-1794): 0.8%.

[0052] Component B1 (by mass percentage) has the following composition: Aromatic isocyanate (Wannate PM-200): 100%.

[0053] The composition of component C1 (by mass percentage) is as follows: Water-based catalyst (C30 water-based curing agent, Beijing Haiyan Technology Co., Ltd.): 100%.

[0054] The preparation of components A1, B1, and C1 is the same as in Example 1.

[0055] Before application, mix the components evenly according to the mass ratio (mass ratio: component A1: component B1: component C1 = 45:55:22). Specifically, mix component A1 and component B1 evenly according to the ratio, add component C1 while stirring, then disperse at medium speed (500 rpm) for 5 minutes, and cure for 10 minutes. After that, apply the resulting primer to a sandblasted steel plate (Sa 2.5 grade, roughness 25~50µm) using high pressure airless spraying, control the dry film thickness to be 300±50µm, and then place the sample at room temperature to cure for 7 days.

[0056] The performance of the cured test panels was tested, and the results are shown in Table 1.

[0057] Example 3: Primer preparation, coating and performance testing Component A1 (by mass percentage) has the following composition: Bisphenol A epoxy resin (NPEL-128): 33%; Hydrogenated bisphenol A epoxy resin (Eponex Resin 1510): 23%; Epoxy Reactive Diluent (Araldite DY-H): 31%; Rheology modifier (Crayvallac Optima): 2.2%; Pigment (titanium dioxide): 10%; Defoamer (BYK-1794): 0.8%.

[0058] Component B1 (by mass percentage) has the following composition: Aromatic isocyanate (Wannate PM-200): 100%.

[0059] The composition of component C1 (by mass percentage) is as follows: Water-based catalyst (C30 water-based curing agent, Beijing Haiyan Technology Co., Ltd.): 100%.

[0060] The preparation of components A1, B1, and C1 is the same as in Example 1.

[0061] Before application, mix the components evenly according to the mass ratio (mass ratio: component A1: component B1: component C1 = 45:55:27). Specifically, mix component A1 and component B1 evenly according to the ratio, add component C1 while stirring, then disperse at medium speed (500 rpm) for 5 minutes, and cure for 10 minutes. After that, apply the resulting primer to a sandblasted steel plate (Sa 2.5 grade, roughness 25~50µm) using high pressure airless spraying, control the dry film thickness to be 300±50µm, and then place the sample at room temperature to cure for 7 days.

[0062] The performance of the cured test panels was tested, and the results are shown in Table 1.

[0063] Example 4: Topcoat preparation, application and performance testing Component A2 (by mass percentage) has the following composition: Hydrogenated bisphenol A epoxy resin (Eponex Resin 1510): 36%; Epoxy reactive diluent (Araldite DY-H): 30%; Rheology modifier (Crayvallac Optima): 1.2%; Pigment (titanium dioxide): 32%; Defoamer (BYK-1794): 0.7%; Catalyst (TCAT-S029): 0.1%.

[0064] Component B2 (by mass percentage) has the following composition: Aliphatic isocyanate (Wannate HT-600): 50%; Alicyclic isocyanate (Wannate HMDI): 50%.

[0065] The composition of component C2 (by mass percentage) is as follows: Water-based catalyst (C30 water-based curing agent, Beijing Haiyan Technology Co., Ltd.): 100%.

[0066] Preparation of component A2: Mix all components in component A2 evenly, grind to a fineness ≤30µm, then filter and package to obtain component A2; Preparation of component B2: The isocyanate was mixed evenly, filtered and packaged to obtain component B2; Preparation of C2 component: The aqueous catalyst was mixed evenly, filtered and packaged to obtain C2 component.

[0067] Before construction, mix the components evenly according to the mass ratio (mass ratio: component A2: component B2: component C2 = 45:55:17). Specifically, mix component A2 and component B2 evenly according to the ratio, add component C2 while stirring, then disperse at medium speed (500 rpm) for 5 minutes and cure for 10 minutes. After that, use high pressure airless spraying to apply the obtained topcoat to the steel plate with the primer (where the primer is prepared according to the method of Example 1, the difference being that the dry film thickness of the primer is 150±50µm). Control the dry film thickness of the topcoat to be 100±25µm, and then place the sample at room temperature to cure for 7 days.

[0068] The performance of the cured test panels was tested, and the results are shown in Table 2.

[0069] Example 5: Topcoat preparation, application and performance testing Component A2 (by mass percentage) has the following composition: Hydrogenated bisphenol A epoxy resin (Eponex Resin 1510): 36%; Epoxy reactive diluent (Araldite DY-H): 30%; Rheology modifier (Crayvallac Optima): 1.2%; Pigment (titanium dioxide): 32%; Defoamer (BYK-1794): 0.7%; Catalyst (TCAT-S029): 0.1%.

[0070] Component B2 (by mass percentage) has the following composition: Aliphatic isocyanate (Wannate HT-600): 50%; Alicyclic isocyanate (Wannate HMDI): 50%.

[0071] The composition of component C2 (by mass percentage) is as follows: Water-based catalyst (C30 water-based curing agent, Beijing Haiyan Technology Co., Ltd.): 100%.

[0072] The preparation of components A2, B2, and C2 is the same as in Example 4.

[0073] Before construction, mix the components evenly according to the mass ratio (mass ratio: component A2: component B2: component C2 = 45:55:22). Specifically, mix component A2 and component B2 evenly according to the ratio, add component C2 while stirring, then disperse at medium speed (500 rpm) for 5 minutes, and cure for 10 minutes. After that, apply the topcoat to the steel plate with the primer using high pressure airless spraying (the primer is prepared according to the method of Example 2, except that the dry film thickness of the primer is 150±50µm). Control the dry film thickness of the topcoat to be 100±25µm, and then place the sample at room temperature to cure for 7 days.

[0074] The performance of the cured test panels was tested, and the results are shown in Table 2.

[0075] Example 6: Topcoat preparation, application and performance testing Component A2 (by mass percentage) has the following composition: Hydrogenated bisphenol A epoxy resin (Eponex Resin 1510): 36%; Epoxy reactive diluent (Araldite DY-H): 30%; Rheology modifier (Crayvallac Optima): 1.2%; Pigment (titanium dioxide): 32%; Defoamer (BYK-1794): 0.7%; Catalyst (TCAT-S029): 0.1%.

[0076] Component B2 (by mass percentage) has the following composition: Aliphatic isocyanate (Wannate HT-600): 50%; Alicyclic isocyanate (Wannate HMDI): 50%.

[0077] The composition of component C2 (by mass percentage) is as follows: Water-based catalyst (C30 water-based curing agent, Beijing Haiyan Technology Co., Ltd.): 100%.

[0078] The preparation of components A2, B2, and C2 is the same as in Example 4.

[0079] Before construction, the components were mixed evenly according to the mass ratio (mass ratio: component A2: component B2: component C2 = 45:55:27). Specifically, component A2 and component B2 were mixed evenly according to the ratio, component C2 was added during stirring, and then dispersed at medium speed (500 rpm) for 5 minutes and cured for 10 minutes. The resulting topcoat was then sprayed onto the steel plate with the primer applied in Example 3 using high pressure airless spraying (the primer was prepared according to the method in Example 3, except that the dry film thickness of the primer was 150±50µm). The dry film thickness of the topcoat was controlled to be 100±25µm, and then the sample was placed at room temperature for curing for 7 days.

[0080] The performance of the cured test panels was tested, and the results are shown in Table 2.

[0081] Comparative Example Without the addition of component C, the aqueous catalyst was omitted, and the other components and preparation method were the same as in Example 1. As a result, the coating failed to fully cure within 7 days, the surface became sticky, and subsequent testing was impossible.

[0082] Table 1. Composition and properties of waterborne epoxy-isocyanate hybrid primers

[0083] Table 2 Composition and Properties of Waterborne Epoxy-Isocyanate Hybrid Topcoats

[0084] The test results above show that the waterborne epoxy-isocyanate hybrid heavy-duty anti-corrosion coating provided by the present invention has excellent adhesion, mechanical strength and chemical resistance.

[0085] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A water-based epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating, characterized in that, Includes a primer; the primer comprises separately packaged components A1, B1, and C1; The A1 component comprises the following components by mass percentage: 86-90% liquid epoxide, 8-12% pigments and fillers, and 1-3% additives; the B1 component comprises aromatic isocyanate and alicyclic isocyanate, wherein the mass ratio of aromatic isocyanate to alicyclic isocyanate is (80-100):(0-20); the C1 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, wherein the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A1 component, the B1 component and the C1 component is (40-50):(50-60):(17-27).

2. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating according to claim 1, characterized in that, The liquid epoxide in component A1 includes one or more of bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and epoxy reactive diluent; the pigments and fillers include one or more of titanium dioxide, carbon black, and barium sulfate; and the additives include rheology modifiers and / or defoamers.

3. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating according to claim 1, characterized in that, The aromatic isocyanates in component B1 include polymeric MDI and / or polymeric MDI derivatives, and the alicyclic isocyanates include 4,4'-dicyclohexylmethane diisocyanate and / or 4,4'-dicyclohexylmethane diisocyanate derivatives.

4. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating according to claim 1, characterized in that, The aqueous catalyst of component C1 is C30 aqueous curing agent provided by Beijing Haiyan Technology Co., Ltd.

5. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating according to any one of claims 1 to 4, characterized in that, It also includes a topcoat; the topcoat comprises separately packaged components A2, B2, and C2. The A2 component comprises the following components by mass percentage: 62-70% liquid epoxide, 28-36% pigments and fillers, and 1-3% additives; the B2 component comprises aliphatic isocyanate and alicyclic isocyanate, wherein the mass ratio of the aliphatic isocyanate to the alicyclic isocyanate is (40-60):(40-60); the C2 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, and the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A2 component, the B2 component and the C2 component is (40-50):(50-60):(17-27).

6. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating according to claim 5, characterized in that, The liquid epoxide in component A2 includes one or more of bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, and epoxy reactive diluent; the pigments and fillers include one or more of titanium dioxide, carbon black, and barium sulfate; and the additives include one or more of rheology modifiers, defoamers, and organometallic salt catalysts.

7. The waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating according to claim 5, characterized in that, The aliphatic isocyanates in component B2 include one or more of hexamethylene diisocyanate, hexamethylene diisocyanate dimer, hexamethylene diisocyanate trimer, hexamethylene diisocyanate derivative, hexamethylene diisocyanate dimer derivative, and hexamethylene diisocyanate trimer derivative, and the alicyclic isocyanates include 4,4'-dicyclohexylmethane diisocyanate and / or 4,4'-dicyclohexylmethane diisocyanate derivatives.

8. A water-based epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion topcoat, characterized in that, Includes separately packaged components A2, B2, and C2; The A2 component comprises the following components by mass percentage: 62-70% liquid epoxide, 28-36% pigments and fillers, and 1-3% additives; the B2 component comprises aliphatic isocyanate and alicyclic isocyanate, wherein the mass ratio of the aliphatic isocyanate to the alicyclic isocyanate is (40-60):(40-60); the C2 component is an aqueous catalyst, wherein the aqueous catalyst is a silane-modified alkali metal silicate aqueous solution, and the solid content of the silane-modified alkali metal silicate aqueous solution is 30-60 wt%; the mass ratio of the A2 component, the B2 component and the C2 component is (40-50):(50-60):(17-27).

9. The method of applying the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating according to any one of claims 1 to 7, characterized in that, The application of the primer includes the following steps: Mix components A1, B1, and C1 to obtain the primer; The primer is applied to the surface of the workpiece and cured for the first time to form a primer coating; the first curing is at room temperature.

10. The application method according to claim 9, characterized in that, When the waterborne epoxy-isocyanate hybrid nano-heavy-duty anti-corrosion coating further includes a topcoat, the application of the topcoat includes the following steps: mixing components A2, B2 and C2 to obtain the topcoat; applying the topcoat to the surface of the primer coating, and subjecting it to a second curing process to form a topcoat coating; the second curing process is room temperature curing.