Foam separation treatment method, aqueous solution, method for using vinyl alcohol-based polymer, and foam generation accelerator

By using vinyl alcohol-based polymers to generate foam for PFAS separation in water, the problem of low separation efficiency in foam separation methods is solved, achieving efficient PFAS separation and water purification.

CN122374260APending Publication Date: 2026-07-10KURARAY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202480078677.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-12-13
Filing Date
2024-12-12
Publication Date
2026-07-10

AI Technical Summary

Technical Problem

Existing foam separation methods suffer from low separation efficiency when treating PFAS in water due to poor foaming.

Method used

Vinyl alcohol-based polymers (such as PVA) are used as high molecular surfactants. They are introduced into the water to be treated to generate foam. The foam is then fed back by gas to separate PFAS. The content and ratio of the high molecular surfactant are controlled to optimize the separation effect.

Benefits of technology

This improved the separation efficiency of PFAS, achieving a highly efficient water purification effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

A foam separation treatment method is provided that separates organofluorine compounds from treated water by introducing gas into the treated water containing organofluorine compounds and recovering the foam generated. A polymeric surfactant is introduced into the treated water. Therefore, a foam separation treatment method capable of efficiently separating organofluorine compounds from treated water containing organofluorine compounds is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to foam separation and treatment methods, aqueous solutions, methods of using vinyl alcohol-based polymers, and foam generation promoters. Background Technology

[0002] In recent years, the environmental pollution problems caused by perfluorooctanoic acid (PFOS) and perfluorooctanoic acid (PFOA), which are classified as organofluorine compounds (PFAS), have become increasingly apparent. Technologies for separating and recovering these chemicals (Patent Document 1) and technologies for decomposing them (Patent Document 2) have been proposed. In particular, among the technologies for separating and recovering chemical substances, a water treatment method known as the foam separation method is known. Patent Document 1 discloses a foam separation treatment device used in this foam separation method.

[0003] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2023-50657 Patent Document 2: Japanese Patent Publication No. 2022-537895. Summary of the Invention

[0004] The problem the invention aims to solve When PFAS are separated and recovered from water to be treated by foam separation treatment, the efficiency of foam separation is sometimes poor when the foaming of the water to be treated is poor.

[0005] One of the objectives of this application is to provide a foam separation treatment method, an aqueous solution, a method of using a vinyl alcohol-based polymer, and a foam generation promoter that can efficiently separate PFAS from treated water containing PFAS.

[0006] Methods for solving problems The above objectives are achieved by providing any of the following solutions.

[0007] [1] A foam separation treatment method that separates organic fluorine compounds from the water to be treated by introducing a high molecular surfactant into the water to be treated. [2] The foam separation treatment method according to claim 1, wherein the aforementioned polymeric surfactant is a vinyl alcohol-based polymer; [3] According to the foam separation treatment method of [2], the viscosity-average polymerization degree of the aforementioned vinyl alcohol polymer is 100 or more and 5,000 or less, and the saponification degree is 30 mol% or more and 99.99 mol% or less; [4] According to any one of [1] to [3], a foam separation treatment method is used, wherein a polymeric surfactant is introduced into the water to be treated in such a way that the content of the polymeric surfactant in the water to be treated is less than 1% by mass; [5] According to any one of [1] to [4], a foam separation treatment method is introduced, wherein a polymeric surfactant is introduced at a mass ratio of more than 1 times the amount of the organic fluorine compound contained in the water to be treated. [6] An aqueous solution containing vinyl alcohol polymers and organofluorine compounds; [7] According to the aqueous solution of [6], wherein the viscosity-average degree of polymerization of the aforementioned vinyl alcohol polymer is 100 or more and 5,000 or less, and the degree of saponification is 30 mol% or more and 99.99 mol% or less; [8] According to the aqueous solution of [6] or [7], wherein the content of the vinyl alcohol polymer in the aqueous solution is less than 1% by mass; [9] According to any one of [6] to [8], the content of the vinyl alcohol polymer is more than 1 times the mass of the content of the organofluorine compound in the aqueous solution;

[10] A foam separation and treatment method, wherein gas is introduced into an aqueous solution of any one of [6] to [9] to generate foam, and the aforementioned foam is recovered;

[11] A method of using vinyl alcohol polymers, wherein the organic fluorine compounds are separated from the treated water by recovering foam generated by introducing gas into the treated water containing the organic fluorine compounds. Foam formation is promoted by mixing vinyl alcohol-based polymers into the water being treated.

[12] A foam generation promoter, which is introduced into the water to be treated during the separation of organofluorine compounds from the water to be treated by foam separation treatment, and contains a vinyl alcohol polymer.

[0008] Invention Effects According to the foam separation treatment method, aqueous solution, method of using vinyl alcohol-based polymers, and foam generation promoter of this application, the separation efficiency of PFAS can be improved. Therefore, it is possible to efficiently separate organofluorine compounds from the treated water, which is useful for the purification of water contaminated with organofluorine compounds. Detailed Implementation

[0009] <Foam Separation Treatment Method> The foam separation treatment method of this application is a foam separation treatment method that separates organic fluorine compounds from the treated water by introducing a high molecular surfactant into the treated water. This method involves recycling the foam generated by introducing gas into the treated water containing organic fluorine compounds.

[0010] In the foam separation and treatment method of this application, a polymeric surfactant can be introduced into the water to be treated containing organofluorine compounds (PFAS), gas is introduced into the water to be treated to generate bubbles, and at the air-water interface of the aforementioned bubbles, the polymeric surfactant and PFAS are concentrated to generate foam, and the aforementioned foam is recovered near the surface of the water to be treated.

[0011] The method of introducing polymeric surfactants into the water to be treated is not particularly limited, as long as it does not impair the scope of the present invention. For example, the polymeric surfactant can be added to the water to be treated before gas is introduced, or it can be added to the water to be treated while gas is being introduced. Alternatively, the water to be treated can be introduced into a treatment tank or the like pre-filled with polymeric surfactants for foam separation treatment.

[0012] There are no particular limitations on the gas introduced into the water being treated; for example, air or nitrogen can be used, but air is preferred.

[0013] As a means of introducing gas into the water being treated, there are no particular limitations as long as foam can be generated. For example, gas can be introduced from an air supply pipe installed in the water being treated.

[0014] After foam separation, the recovered mixture of polymeric surfactants and PFAS can be directly incinerated, or it can be adsorbed onto adsorbents such as activated carbon before incineration.

[0015] In one embodiment of the foam separation treatment method of this application, foam separation treatment can be performed continuously. For example, at least one of the following steps can be performed continuously: feeding water to be treated into the foam separation treatment apparatus, introducing a polymeric surfactant into the water to be treated, feeding gas into the water to be treated, and recovering the generated foam.

[0016] The foam separation treatment method of this application can be a treatment that reduces the concentration of PFAS in the treated water by separating and recovering a portion of the PFAS contained in the treated water, or it can be a treatment that removes PFAS from the treated water by separating and recovering the actual total amount of PFAS contained in the treated water.

[0017] The amount of polymeric surfactant introduced into the treated water is not particularly limited as long as it does not impair the spirit of the invention. The content of polymeric surfactant in the treated water is sometimes preferably 0.1 ppm or more by mass, more preferably 1 ppm or more by mass, further preferably 10 ppm or more by mass, and even more preferably 100 ppm or more by mass. Furthermore, the content of polymeric surfactant in the treated water is preferably 1% by mass or less. That is, in the foam separation treatment method of this application, it is preferable to introduce polymeric surfactant into the treated water such that the content of polymeric surfactant in the treated water is within the above-mentioned range. By keeping the content of polymeric surfactant in the treated water within the above-mentioned range, the foaming properties are more excellent. In one embodiment where foam separation treatment is performed continuously, it is also preferable to adjust the amount of polymeric surfactant introduced into the treated water such that the content of polymeric surfactant in the treated water is within the above-mentioned range.

[0018] Furthermore, the amount of polymeric surfactant relative to the PFAS content in the treated water is preferably at least 1 times by mass, more preferably at least 10 times by mass, even more preferably at least 50 times by mass, and even more preferably at least 100 times by mass. That is, in the foam separation treatment method of this application, it is preferable to introduce a polymeric surfactant at least 1 times by mass relative to the PFAS content in the treated water. By ensuring that the amount of polymeric surfactant relative to the PFAS content in the treated water is within the above-mentioned range, the PFAS recovery efficiency is superior. In one embodiment where foam separation treatment is performed continuously, it is preferable to adjust the amount of treated water introduced into the treatment system and / or the amount of polymeric surfactant introduced into the treated water in such a way that the amount of polymeric surfactant relative to the PFAS content in the treated water is within the above-mentioned range.

[0019] Without prejudice to the spirit of the invention, the water to be treated may contain other impurities and other components in addition to PFAS.

[0020] (Polymer surfactants) The polymeric surfactant used in this application is a polymer and a compound exhibiting surface activity. It should be noted that "polymeric" means a molecular weight of 1000 or higher. In the foam separation and treatment method of this application, one polymeric surfactant or two or more polymeric surfactants may be used.

[0021] The polymeric surfactant has a molecular weight of 1,000 or more, preferably 2,000 or more, more preferably 5,000 or more, and even more preferably 10,000 or more.

[0022] The HLB value of the polymeric surfactant is preferably 3 or higher, more preferably 8 or higher, and even more preferably 13 or higher. The HLB value is an indicator of the surfactant's affinity for water and oil, ranging from 0 to 20. A value closer to 0 indicates higher lipophilicity, and a value closer to 20 indicates higher hydrophilicity. Here, the HLB value is defined using the Griffin method: HLB value = 20 × (total formula weight of the hydrophilic portion) / (molecular weight). For example, when a surfactant is strongly mixed in water, if a portion of the surfactant is dispersed in the water, the surfactant has an HLB value of 3 to 6; if dispersed in a milky state, it corresponds to an HLB value of 6 to 8; if dispersed in a stable milky state, it corresponds to an HLB value of 8 to 10; if dispersed in a semi-transparent or transparent state, it corresponds to an HLB value of 10 to 13; and if dissolved and transparent, it corresponds to an HLB value of 13 or higher.

[0023] Polymer surfactants can be polymers formed by polymerizing monomers, preferably polymers of nonionic and / or anionic monomers. Examples of nonionic monomers include ethylene oxide, propylene oxide, (meth)acrylamide compounds, alkyl (meth)acrylates, styrene, acrylonitrile, and vinyl acetate. Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate. Examples of anionic monomers include (meth)acrylic acid, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, maleic acid, and their salts. It should be noted that in this application, "(meth)acryloyl" refers to the collective term for methacryloyl and acryloyl groups. Furthermore, polymer surfactants can be polymers formed by polymerizing one monomer or polymers copolymerized from two or more monomers. Additionally, polymer surfactants can be polymers obtained by polymerizing monomers, for example, through a process of introducing functional groups. Among polymeric surfactants, vinyl alcohol polymers (PVA) obtained from vinyl acetate and other vinyl ester monomers are preferred due to their superior water solubility, foam-forming properties, and biodegradability. Specifically, a preferred embodiment of the foam separation treatment method of this application involves separating the organic fluorine compounds from the treated water by recovering the foam generated from the water containing organofluorine compounds through the introduction of gas. This foam separation treatment method involves introducing PVA into the treated water. It should be noted that the monomers used as raw materials for PVA, as described below, can be vinyl ester monomers other than vinyl acetate.

[0024] PVA is a polymer containing vinyl alcohol units as monomer units. PVA is obtained by saponifying a vinyl ester polymer synthesized from vinyl ester monomers used as raw materials. In addition to vinyl alcohol units, saponified PVA may also contain vinyl ester units.

[0025] Additionally, PVA can be made as follows: PVA comprising monomer units other than vinyl alcohol units and vinyl ester units, obtained by saponifying copolymers formed by copolymerizing vinyl ester monomers as raw material monomers with other monomers; or PVA in which specific chemical species are reacted to introduce specific functional groups into the side chains and ends during the polymerization, saponification, and / or after saponification processes in the manufacturing of PVA. In this application, such PVA is sometimes referred to as "modified vinyl alcohol polymer (modified PVA)". Furthermore, in this application, the formulation used to modify PVA is sometimes referred to as a "modifying species". For example, in one embodiment, when the modified PVA has a terminal structure derived from a chain transfer agent, the chain transfer agent is sometimes referred to as a modifying species; in another embodiment, when the modified PVA is a substance copolymerized from "other monomers" other than vinyl ester monomers, the "other monomers" are sometimes referred to as modifying species. Furthermore, in this application, the ratio of units derived from modifying species to all monomer units constituting the modified PVA is sometimes referred to as the "modification amount".

[0026] The lower limit of the proportion of vinyl alcohol units in PVA relative to all monomer units is sometimes preferably 35 mol%, more preferably 50 mol%, and even more preferably 65 mol%. On the other hand, the upper limit of the proportion of the above-mentioned vinyl alcohol units is sometimes preferably 99.95 mol%, more preferably 95 mol%, and even more preferably 90 mol%.

[0027] The viscosity-uniform polymerization degree of PVA is preferably 100 or more and 5,000 or less. The lower limit of the viscosity-uniform polymerization degree of PVA is sometimes more preferably 200, and even more preferably 500. Furthermore, the upper limit of the viscosity-uniform polymerization degree of PVA is sometimes more preferably 4,000, even more preferably 3,000, and even more preferably 2,000. By setting the viscosity-uniform polymerization degree within the above range, it tends to be easier to manufacture. The viscosity-uniform polymerization degree is a value obtained by measurement according to JIS K 6726:1994. Specifically, when the degree of saponification of PVA is less than 99.5 mol%, for PVA saponified to a degree of saponification of 99.5 mol% or more, the viscosity-uniform polymerization degree is obtained using the intrinsic viscosity [η] (L / g) measured in water at 30°C, and calculated using the following formula.

[0028] P = ([η] × 10) 4 (8.29) (1 / 0.62) The lower limit of the degree of saponification of PVA is sometimes preferably 30 mol%, more preferably 50 mol%, and even more preferably 65 mol%. On the other hand, the upper limit of the degree of saponification of PVA is sometimes preferably 99.99 mol%, more preferably 99 mol%, even more preferably 90 mol%, and even more preferably 80 mol%. In addition, the degree of saponification of PVA is sometimes preferably 30 mol% or more and 99.99 mol% or less, more preferably 50 mol% or more and 99.99 mol% or less, and even more preferably 65 mol% or more and 90 mol% or less. By making the degree of saponification of PVA within the above range, the foam separation efficiency is improved, and there is a tendency to manufacture PVA more stably in industrial applications.

[0029] The preferred method for manufacturing PVA includes a polymerization step of polymerizing ethylene ester monomers and a saponification step of saponifying the resulting ethylene ester polymer.

[0030] Vinyl ester polymers can be manufactured by polymerizing vinyl ester monomers using existing known methods such as bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, and dispersion polymerization. From the viewpoint of improving the performance of this application, solution polymerization using lower alcohols is preferred. The lower alcohol is not particularly limited, but is preferably an alcohol with 3 or fewer carbon atoms, such as methanol, ethanol, propanol, or isopropanol, and more preferably methanol. The polymerization operation can also employ any polymerization method among batch, semi-batch, and continuous polymerization.

[0031] Examples of vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl pentanoate, vinyl tert-carbonate, vinyl hexanoate, vinyl octanoate, vinyl laurate, vinyl palmitate, vinyl stearate, vinyl oleate, and vinyl benzoate. Vinyl acetate is preferred.

[0032] Furthermore, as mentioned above, for PVA, without prejudice to the purpose of this application, modified PVA can be prepared by copolymerizing ethylene ester monomers with other monomers. Examples of other monomers include, for instance, α-olefins such as ethylene, propylene, n-butene, and isobutene; (meth)acrylic acid and its salts; (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate; and (meth)acrylamide, N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, diacetone (meth)acrylamide, and (meth)acrylamide. Acrylamide compounds, including acrylamide propane sulfonic acid and its salts, (meth)acrylamide propyl dimethylamine and its salts or quaternary salts, N-hydroxymethyl (meth)acrylamide and its derivatives; vinyl ethers, including methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether; nitrile compounds, including acrylonitrile and methacrylonitrile; halogenated vinylides, including vinyl chloride and vinyl fluoride; vinylidene halogenated vinylides, including vinylidene chloride and vinylidene fluoride; allyl acetate, allyl chloride, and other allyl compounds; unsaturated dicarboxylic acids, including maleic acid, itaconic acid, and fumaric acid, and their salts or esters; and isopropyl acetate, etc. These compounds can be used alone or in combination of two or more. Among them, 3-(methacryloylamino)propyltrimethylammonium chloride (MAPTAC) is preferred as an acrylamide compound. The copolymerization amount (modification amount) of other monomers is preferably less than 10 mol%. It should be noted that the copolymerization amount of other monomers refers to the proportion of units derived from other monomers relative to all monomer units constituting the modified PVA.

[0033] The polymerization initiator used in polymerization can be selected from known initiators (e.g., azo initiators, peroxide initiators, redox initiators, etc.). Examples of azo initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylpentanonitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylpentanonitrile). Examples of peroxide initiators include percarbonate compounds such as di-n-propyl peroxide, diisopropyl peroxide, di(2-ethylhexyl) peroxide, and diethoxyethyl peroxide; perester compounds such as tert-butyl peroxydecanoate, α-cumyl peroxydecanoate, and tert-butyl peroxydecanoate; acetylcyclohexylsulfonyl peroxide; and 2,4,4-trimethylpentyl peroxyphenoxyacetic acid. Initiators can be prepared by combining these initiators with potassium persulfate, ammonium persulfate, hydrogen peroxide, etc. Examples of redox initiators include those composed of the aforementioned peroxides combined with reducing agents such as sodium bisulfite, sodium bicarbonate, tartaric acid, L-ascorbic acid, and sodium silicate. When polymerization is carried out at high temperatures, discoloration due to the decomposition of vinyl ester monomers is sometimes observed. In such cases, to prevent discoloration, antioxidants such as tartaric acid can be added to the polymerization system at a concentration of 1 to 100 ppm by mass relative to the vinyl ester monomers.

[0034] During the polymerization of vinyl ester monomers, chain transfer agents can be coexisting to adjust the degree of polymerization of the resulting PVA and to introduce functional groups into the PVA. Examples of chain transfer agents include aldehydes such as acetaldehyde, propionaldehyde, butyraldehyde, and benzaldehyde; ketones such as acetone, methyl ethyl ketone, hexanone, and cyclohexanone; thiols such as 2-hydroxyethanethiol; thiocarboxylic acids such as thioacetic acid; halogenated hydrocarbons such as trichloroethylene and perchloroethylene; and alkyl thiols such as n-dodecyl mercaptan (n-DDM). Aldehydes and alkyl thiols are particularly suitable. The amount of chain transfer agent added is determined based on the chain transfer constant of the added chain transfer agent and the degree of polymerization of the target PVA, and is typically preferably 0.1 to 10% by mass relative to the vinyl ester used. As one embodiment, by using alkyl thiols as chain transfer agents in the PVA polymerization process, modified PVA with alkyl groups derived from alkyl thiols introduced at the ends can be obtained. The amount of modification in this modified PVA, i.e., the ratio of the alkyl unit derived from the alkyl thiol to all the monomer units constituting the modified PVA, is preferably 0.01 mol% or more and 5 mol% or less, more preferably 0.1 mol% or more and 3 mol% or less, and even more preferably 0.3 mol% or more and 1 mol% or less. The alkyl thiol is preferably n-DDM.

[0035] The polymerization temperature is not particularly limited, but is preferably 0~180℃, more preferably 20~160℃, and even more preferably 30~150℃. When polymerization is carried out below the boiling point of the solvent used in the polymerization process, either vacuum boiling polymerization (polymerization under reduced pressure while the solvent boils) or atmospheric pressure non-boiling polymerization (polymerization under normal pressure without the solvent boiling) can be selected. Alternatively, when polymerization is carried out above the boiling point of the solvent used in the polymerization process, either pressurized non-boiling polymerization (polymerization under pressure without the solvent boiling) or pressurized boiling polymerization (polymerization under pressure while the solvent boils) can be selected.

[0036] As described above, PVA can be obtained by saponifying vinyl ester polymers. Examples of saponification reactions include alcoholysis or hydrolysis using alkaline catalysts such as sodium hydroxide, potassium hydroxide, or sodium methoxide, and acidic catalysts such as p-toluenesulfonic acid. Examples of solvents that can be used in this reaction include alcohols such as methanol and ethanol; esters such as methyl acetate and ethyl acetate; ketones such as acetone and methyl ethyl ketone; and aromatic hydrocarbons such as benzene and toluene. These solvents can be used alone or in combination of two or more. Using methanol or a methanol / methyl acetate mixture as the solvent and sodium hydroxide as the catalyst for saponification is simple and therefore preferred.

[0037] (Organofluorine compounds) Organofluorine compounds (PFAS) can be amphiphilic perfluoroalkane derivatives. Examples of amphiphilic perfluoroalkane derivatives include perfluoroalkane carboxylic acids, perfluoroalkyl sulfonic acids, and 1H,1H,2H,2H-perfluoroalkyl alcohols. Examples of perfluoroalkane carboxylic acids include perfluorobutyric acid, perfluorovaleric acid, perfluorohexanoic acid, perfluoroheptanoic acid, perfluorooctanoic acid, perfluorononanoic acid, perfluorodecanoic acid, perfluoroundecanoic acid, and perfluorododecanoic acid. In particular, the foam separation treatment method of this application is suitable for perfluorovaleric acid, perfluorohexanoic acid, perfluoroheptanoic acid, and perfluorooctanoic acid. Examples of perfluoroalkyl sulfonic acids include perfluorobutyric acid, perfluorohexanesulfonic acid, perfluorooctanoic acid, and their salts. Examples of PFAS that can be used for 1H,1H,2H,2H-perfluoroalkyl alcohols include 1H,1H,2H,2H-perfluoro-1-hexanol, 1H,1H,2H,2H-perfluoro-1-octanol, and 1H,1H,2H,2H-perfluoro-1-decanol. One or more PFAS can be used for foam separation treatment.

[0038] <Aqueous solution> One embodiment of the present invention is an aqueous solution containing PVA and PFAS. Based on the composition of this aqueous solution, the PFAS contained in the aqueous solution can be easily separated by a foam separation process.

[0039] The preferred method for including PVA and PFAS in the aqueous solution is the same as that for PVA and PFAS described above.

[0040] The PVA content in the aqueous solution is sometimes preferably 0.1 ppm by mass or more, more preferably 1 ppm by mass or more, even more preferably 10 ppm by mass or more, and even more preferably 100 ppm by mass or more. Furthermore, the PVA content in the aqueous solution is preferably 1% by mass or less. By setting the PVA content in the aqueous solution to the above range, the foaming properties are improved.

[0041] Furthermore, the PVA content in the aqueous solution is preferably at least 1 times the PFAS content, more preferably at least 10 times the PFAS content, even more preferably at least 50 times the PFAS content, and even more preferably at least 100 times the PFAS content. By maintaining the PVA content within the above range, the PFAS recovery efficiency is improved.

[0042] The aqueous solution of this application may contain various additives and impurities without prejudice to the spirit of this invention.

[0043] Another embodiment of the present invention is a foam separation and treatment method, wherein gas is introduced into the above-mentioned aqueous solution to generate foam, and the aforementioned foam is recovered.

[0044] <Instructions for using vinyl alcohol polymers> One embodiment of the present invention is a method of using PVA, wherein, in a process of separating PFAS from the treated water by recovering foam generated by introducing gas into the treated water containing PFAS, foam generation is promoted by mixing PVA into the treated water.

[0045] The preferred method of using PVA in this method is the same as that described above.

[0046] Foaming promoter One embodiment of the present invention is a foam generation promoter, which is introduced into the water to be treated during the separation of organofluorine compounds from the water to be treated by foam separation treatment, and contains a vinyl alcohol polymer.

[0047] The preferred method for PVA in this foam-forming promoter is the same as that for PVA described above. Example

[0048] The present invention will now be described in more detail through examples, but the present invention is not limited to these examples at all. It should be noted that, unless otherwise specified, "%" and "ppm" in the examples and comparative examples refer to "mass %" and "mass ppm" respectively.

[0049] [Viscosity-uniform degree of polymerization] The viscosity-uniform degree of polymerization of the PVA used in the examples was determined according to JIS K 6726:1994. Specifically, for PVA saponified to a degree of saponification of 99.5 mol% or more, the viscosity-uniform degree of polymerization was calculated using the intrinsic viscosity [η] (L / g) measured in water at 30°C, when the degree of saponification was less than 99.5 mol%, using the following formula.

[0050] P = ([η] × 10) 4 (8.29) (1 / 0.62) [Degree of saponification] The degree of saponification of the PVA used in the examples was determined according to JIS K 6726:1994.

[0051] <Manufacturing Example 1> [The manufacture of PVA1] PVA1 was manufactured as a polymeric surfactant using the following method. 640 g of vinyl acetate and 960 g of methanol were added to a 3 L reactor equipped with a stirrer, reflux condenser, nitrogen inlet, and initiator inlet. The system was purged with nitrogen for 30 minutes while bubbling nitrogen. The reactor was then heated, and when the internal temperature reached 60 °C, 0.3 g of 2,2'-azobisisobutyronitrile (AIBN) was added to initiate polymerization. After polymerization at 60 °C for 5 hours, 0.3 g of hydroquinone was added, and the polymerization was stopped by cooling. The solids concentration at the point of polymerization cessation was 20.0%, and the polymerization rate was 50%. Next, unreacted vinyl acetate monomers were removed by continuously adding methanol at 50 °C under reduced pressure to obtain a 35% methanol solution of the vinyl acetate polymer (PVAc). Subsequently, 3.7 g of an alkaline solution (10% methanol solution of sodium hydroxide) was added to 457 g of a methanol solution of an ethylene ester polymer prepared by adding methanol (160.0 g of the ethylene ester polymer in the solution). Saponification was then carried out (the concentration of the ethylene ester polymer in the saponification solution was 30%, and the molar ratio of sodium hydroxide to vinyl acetate units was 0.005). A gel-like substance formed after approximately 15 minutes following the addition of the alkaline solution. This substance was then pulverized and placed at 40°C for 1 hour for saponification. 500 g of methyl acetate was then added to neutralize the remaining alkali. After confirming neutralization was complete using phenolphthalein indicator, the solid was filtered to obtain a white solid. 2,000 g of methanol was added to this solid, and the solid was left to stand at room temperature for 3 hours for washing. This washing process was repeated three times. The solid was then centrifuged to remove the liquid, and the resulting white solid was placed in a dryer at 65°C for 2 days to obtain PVA1. PVA1 had a viscosity-average degree of polymerization of 530 and a degree of saponification of 88.0 mol%.

[0052] <Manufacturing Examples 2-4> [Crafting PVA2~4] PVA2-4 were manufactured as polymeric surfactants using the following method. The polymerization conditions (amount of vinyl acetate, amount of methanol, polymerization rate) and saponification conditions (PVAc concentration, molar ratio of sodium hydroxide to PVAc) were changed as shown in Table 1. Otherwise, the process was the same as that used for manufacturing PVA1 in Manufacturing Example 1 to obtain PVA2-4.

[0053] <Manufacturing Example 5> [The Manufacturing of PVA5] PVA5 was manufactured as a polymeric surfactant using the following method. 960 g of vinyl acetate, 640 g of methanol, and 4.3 g of 3-(methacryloylamino)propyltrimethylammonium chloride (MAPTAC) as a comonomer were added to a 3L reactor equipped with a stirrer, reflux condenser, nitrogen inlet, delayed solution dropper, and initiator addition port. The system was purged with nitrogen for 30 minutes while bubbling nitrogen. Separately, a 20% comonomer solution of MAPTAC dissolved in methanol was prepared as the delayed solution, and nitrogen purged with nitrogen. The reactor was heated until the internal temperature reached 60°C. 0.2 g of 2,2'-azobisisobutyronitrile (AIBN) was added to initiate polymerization. While adding the delayed solution dropwise to maintain a constant monomer composition (vinyl acetate to MAPTAC ratio) in the polymerization solution, polymerization was continued at 60°C for 3 hours. Then, 0.4 g of hydroquinone was added, and the polymerization was stopped by cooling. The total amount of MAPTAC added until polymerization was stopped was 13.4 g. Furthermore, the solids concentration at polymerization stop was 17.0%, and the polymerization rate was 30%. Next, unreacted vinyl acetate monomers were removed by continuously adding methanol at 50°C under reduced pressure, resulting in a methanol solution (concentration 35%) of the MAPTAC-modified vinyl acetate polymer. Then, saponification conditions (PVAc concentration, molar ratio of sodium hydroxide to PVAc) were changed as shown in Table 1, except that saponification was performed under the same conditions as in Manufacturing Example 1 above, yielding PVA5. The modification amount (the proportion of units derived from MAPTAC to all monomer units constituting PVA5) was 2.0 mol%. It should be noted that the modification amount of PVA5 was determined by utilizing… 1 The determination was made by measuring the precursor before saponification, namely the MAPTAC-modified vinyl ester polymer.

[0054] <Manufacturing Example 6> [The manufacture of PVA6] PVA6 was manufactured as a polymeric surfactant using the following method. 960 g of vinyl acetate, 640 g of methanol, and 0.36 g of n-dodecyl mercaptan (n-DDM) were added to a 3L reactor equipped with a stirrer, reflux condenser, nitrogen inlet, delayed solution dropper, and initiator addition port. The system was purged with nitrogen for 30 minutes while bubbling nitrogen. A 10% chain transfer agent solution of n-DDM dissolved in methanol was prepared as the delayed solution, and nitrogen purging was performed by nitrogen bubbling. The reactor was heated until the internal temperature reached 60°C. 1.0 g of 2,2'-azobisisobutyronitrile (AIBN) was added to initiate polymerization. While adding the delayed solution dropwise to maintain a constant ratio of vinyl acetate to n-DDM in the polymerization solution, polymerization was continued at 60°C for 3 hours. Then, 2.0 g of hydroquinone was added, and the polymerization was stopped by cooling. The total amount of n-DDM added until polymerization was stopped was 6.32 g. Furthermore, the solids concentration at polymerization cessation was 28.9%, and the polymerization rate was 50%. Next, unreacted vinyl acetate monomers were removed while methanol was continuously added under reduced pressure at 50°C, yielding a methanol solution (concentration 35%) of the n-DDM-modified vinyl acetate polymer. Then, saponification was performed under the same conditions as in Manufacturing Example 1 above, yielding a modified PVA, namely PVA6, with a structure derived from n-DDM at the ends. The modification amount of PVA6 (the ratio of units with alkyl groups derived from n-DDM to all monomer units constituting PVA6) was 0.5 mol%. It should be noted that the modification amount of PVA6 was determined by using... 1 The determination is made by measuring the precursor before saponification, namely the n-DDM modified vinyl ester polymer.

[0055] [Table 1] .

[0056] <Example 1> [PFAS Foam Separation Treatment Experiment] A cylindrical ceramic air stone (10 mm in diameter, 150 mm in length, #240) was placed at the bottom of a 1 L beaker. 200 ml of an aqueous solution containing 1.0 ppm PFOA (perfluorooctanoic acid) and 100 ppm PVA1 (PFAS) was added as the water to be treated. Air was then introduced into the water by passing it through the air stone at a flow rate of 0.15 ml / min, and the generated foam was continuously collected over 30 minutes. The concentration of PFOA in the residual liquid after the experiment was analyzed using LC / MS (Shimadzu Corporation LC / MS-8030, column: TSKgel ODS-80Ts, detector: MS detector, ionization method: ESI mode, detection charge: negative charge), and the result was 0.08 ppm.

[0057] <Examples 2~10> The types and concentrations of PVA and PFAS were varied as shown in Table 2. Otherwise, the PFAS separation test was performed under the same conditions as in Example 1. The results are shown in Table 2.

[0058] <Example 11> Instead of PVA1, polyoxyethylene lauryl ether (NONION K-230 manufactured by Nippon Oil Co., Ltd., ethylene oxide addition molar number n=30, HLB value 17.5) was used, and PFAS separation tests were performed under the same conditions as in Example 1. The PFOA content in the residual liquid after the test was 0.12 ppm. The results are shown in Table 2.

[0059] <Comparative Example 1> Under the same conditions as in Example 1, the foam separation treatment test of PFAS was carried out without the addition of surfactants, and the PFOA content in the residual solution was 0.82 ppm.

[0060] <Comparative Example 2> Instead of PVA1, lauryl dimethylaminoacetic acid betaine (Nissan Anon BL-SF, molecular weight 271.44) was used, and PFAS separation tests were performed under the same conditions as in Example 1. The residual liquid after the test contained 0.75 ppm of PFOA. The results are shown in Table 2.

[0061] [Table 2]

[0062] The results in Table 2 show that the PFAS residue rate of the examples that used polymeric surfactants for foam separation treatment was lower than that of the comparative examples that did not use polymeric surfactants, and the separation and recovery efficiency of the examples was excellent.

Claims

1. A foam separation treatment method, which separates organic fluorine compounds from water containing organofluorine compounds by recovering the foam generated when gas is introduced into the water to be treated. A high molecular weight surfactant is introduced into the water to be treated.

2. The foam separation and treatment method according to claim 1, wherein, The aforementioned polymeric surfactant is a vinyl alcohol-based polymer.

3. The foam separation and treatment method according to claim 2, wherein, The aforementioned vinyl alcohol polymers have a viscosity-average degree of polymerization of 100 or more and 5,000 or less, and a saponification degree of 30 mol% or more and 99.99 mol% or less.

4. The foam separation and treatment method according to claim 1, wherein, The polymeric surfactant is introduced into the water to be treated in such a way that the content of the polymeric surfactant in the water is less than 1% by mass.

5. The foam separation and treatment method according to any one of claims 1 to 4, wherein, A high molecular weight surfactant is introduced in an amount that is more than one times the mass of the organic fluorine compounds contained in the water being treated.

6. An aqueous solution containing vinyl alcohol polymers and organofluorine compounds.

7. The aqueous solution according to claim 6, wherein, The aforementioned vinyl alcohol polymers have a viscosity-average degree of polymerization of 100 or more and 5,000 or less, and a saponification degree of 30 mol% or more and 99.99 mol% or less.

8. The aqueous solution according to claim 6, wherein, The content of vinyl alcohol polymers in the aqueous solution is less than 1% by mass.

9. The aqueous solution according to claim 6, wherein, The content of vinyl alcohol polymers is more than 1 times the mass of the content of organofluorine compounds in the aqueous solution.

10. Foam separation and treatment method, wherein, Gas is introduced into the aqueous solution according to any one of claims 6 to 9 to generate foam, and the aforementioned foam is recovered.

11. Methods of using vinyl alcohol-based polymers, wherein, In a treatment process that separates organofluorine compounds from water by recovering the foam generated when gas is introduced into the water to be treated, the organofluorine compounds are introduced into the water. Foam formation is promoted by mixing vinyl alcohol-based polymers into the water being treated.

12. A foam generation promoter, which is introduced into the water to be treated during the separation of organofluorine compounds from the water to be treated by foam separation treatment, and which contains a vinyl alcohol polymer.

Citation Information

Patent Citations

  • Equipment suitable for the destruction of PFAS through an oxidation process and for transport to contaminated sites

    JP2022537895A