Quantitative Detection Method of Second Phase Electrolytic Metallography in Nickel-Based Superalloys
By optimizing the electrolyte and process parameters, and combining them with Image processing software, quantitative detection of the δ/η phases in GH4169/GH4169D alloys was achieved. This solves the problems of low detection accuracy and high cost in existing technologies and is applicable to the detection of nickel-based high-temperature alloys with various microstructures.
Patent Information
- Application Number
- CN202611313206.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies cannot quickly, quantitatively, and cost-effectively detect the δ and η phase contents in GH4169 and GH4169D alloys. Furthermore, traditional methods suffer from high error rates, high equipment costs, and long detection cycles.
By optimizing the electrolyte system and process parameters, using a 10% phosphoric acid aqueous solution as the electrolyte, and combining manual constant potential electrolysis with Image processing software, clear identification and quantitative statistics of the δ/η phase are achieved, solving the tip effect and Newton's rings interference of non-standard large-size samples.
The quantitative detection accuracy of the δ/η phase of GH4169/GH4169D alloy reaches ±1%, improving detection efficiency, reducing costs, and making it suitable for engineering production, covering a variety of microstructure types.
Smart Images

Figure CN123066072A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallographic testing technology for metallic materials, and particularly relates to a quantitative method for electrolytic metallographic testing of the second phase of nickel-based high-temperature alloys. Background Technology
[0002] GH4169 alloy is the main material currently used in core rotating components such as compressor disks and turbine disks of aero-engines, accounting for approximately 70% of the applications of high-temperature alloys. Modified GH4169D alloy, with its superior heat resistance, is gradually being promoted, reaching an application share of 22%. Both alloys are δ- and η-phase precipitation-strengthened nickel-based high-temperature alloys. The precipitation content and microstructure of the δ and η phases directly control the alloy's strength, plasticity, creep rupture, and fatigue properties. The optimal range for δ phase volume fraction is 2%–5%. The dispersed short rod-shaped and granular δ phases are discontinuously distributed along grain boundaries, effectively pinning grain boundaries and inhibiting grain growth. When excessive δ phase precipitation occurs (volume fraction > 6%) and forms continuous acicular or lath Widmanstätten structures, it disrupts the matrix continuity, significantly reducing plasticity, fatigue, and creep rupture life. The optimal volume fraction of the η phase is between 1% and 2%, where it disperses at grain boundaries in the form of fine particles and short rods. When the volume fraction of the η phase exceeds 4% and forms coarse needle-like or lamellar Widmanstätten structures, the continuous network of η phase will completely rupture the grain boundaries, inducing intergranular cracks and leading to a sharp decrease in high-temperature plasticity, fatigue resistance, and creep rupture performance. However, the national standard lacks comparative analysis of spectral data. Currently, the detection methods for the δ / η phase in GH4169 / GH4169D alloys have the following shortcomings:
[0003] (1) Image comparison method: The current standard adopts the standard image comparison method (GH4169 adopts the internal model standard XX-0102, and GH4169D is implemented with reference to it). The grade is divided according to the content and morphology of the precipitated phase, and it is judged to be qualified if it does not exceed the specified grade. This method only specifies the upper limit of the content and does not restrict the lower limit, which has the risk of misjudgment of "insufficient precipitation but qualified"; the image grade is a discrete typical sample, and the actual microstructure of the alloy is mostly in the intermediate state of transition. The rating is highly dependent on subjective judgment, and the microstructure and properties of products of the same grade fluctuate significantly.
[0004] (2) X-ray diffraction (XRD): The sample preparation requirements are high, the equipment cost is high, the efficiency is low, the signal is submerged and cannot be detected when the content is low, and only semi-quantitative information can be obtained when the content is high, and morphological information cannot be provided.
[0005] (3) Physicochemical analysis method (electrolytic extraction): It requires the use of electrolytes with complex formulations and poor versatility. The operation is cumbersome, the cycle is long, the cost is high, and the morphological information of the precipitated phase is completely lost during the extraction process.
[0006] (4) Electron backscatter diffraction (EBSD): The field of view is much smaller than the effective statistical lower limit, resulting in large deviations and poor repeatability. Moreover, the equipment investment is as high as 3-5 million yuan, making it difficult to promote in engineering. 2-4 have high equipment costs and long detection cycles.
[0007] (5) Traditional chemical etching metallographic method: After etching with chemical reagents such as FeCl3, the contrast between the second phase and the matrix is insufficient, and the grayscale difference between the phases is small. Automatic segmentation tools based on grayscale thresholds cannot effectively separate the target phase from the matrix, making quantitative analysis impossible and qualitative morphological identification difficult. The misjudgment rate is as high as 21% or more. Although it can be displayed, it cannot be quantified, and qualitative morphological identification is also difficult.
[0008] In summary, existing detection technologies in the industry cannot rapidly and quantitatively characterize the δ and η phase contents of GH4169 and GH4169D alloys, making it difficult to balance accuracy, efficiency, and cost. There is an urgent need to develop a δ / η phase detection method that combines quantitative accuracy, low cost, high throughput, and engineering applicability. Summary of the Invention
[0009] The present invention provides a quantitative detection method for the second phase of nickel-based superalloys via electrolytic metallography. By optimizing the electrolyte system and process parameters, the optical contrast between the δ / η phase and the matrix is enhanced, enabling clear identification of the δ / η phase morphology and accurate quantitative statistics of its content. At the same time, it solves practical engineering problems such as the tip effect and Newton's rings interference during the electrolysis of non-standard large-size samples, thus meeting the daily testing needs of aero-engine forgings for large batches, high precision, and low cost.
[0010] A quantitative electrolytic metallographic method for detecting the second phase of nickel-based superalloys is disclosed, applicable to the quantitative characterization of the microstructure of GH4169 alloy, GH4169D alloy and their modified alloy forgings, bars and parts. The method includes the following steps: S1: The alloy sample is pretreated to remove the plastic deformation layer and micro-unevenness on the sample surface and obtain a mirror-level flat surface. S2: An insulating film is formed on the surface of the alloy sample, which can block the electric field concentration at sharp corners and edges and eliminate preferential over-corrosion and edge collapse defects at the corners. S3: Prepare an aqueous solution of phosphoric acid as an electrolyte. By coloring the matrix while leaving the δ or η phase uncolored, different colors are obtained under light interference, increasing the contrast between the matrix and the δ or η phase. This improves the efficiency and quality of quantitative detection during metallographic optical observation and analysis. S4: Manual constant potential electrolytic coloring, including, The alloy sample in step S2 is used as the anode, and the platinum electrode or stainless steel electrode is used as the cathode, and the phosphoric acid aqueous solution in step S3 is used as the electrolyte. Electrolytic coloring was performed in constant potential mode, wherein different electrolytic process parameters were adjusted according to alloy samples with different supply states and size specifications and carried out at room temperature, and low-speed stirring was used to eliminate local concentration differences in the solution, wherein the voltage was set so that the current density was controlled at 0.01-0.02 A / cm². After electrolysis, the surface of the alloy sample is rinsed with deionized water to remove residual electrolyte and then dried with cold air. S5: Metallographic image acquisition and processing using Image image processing and analysis software; Based on a grayscale thresholding algorithm, the δ-phase or η-phase pixels are separated from the matrix, and the area fraction of the δ-phase or η-phase in the metallographic image is directly measured.
[0011] The beneficial effects of the present invention are as follows: 1) Quantitative detection of the δ / η phases in GH4169 / GH4169D alloys was achieved. Through selective electrolytic coloring with a 10% phosphoric acid aqueous solution, a nano-thickness interference oxide film (pale blue-gray or black) was generated on the γ-matrix surface, while preserving the original morphology of the δ / η phases (light gray or white), creating strong optical contrast. This solved the problem of small grayscale differences between phases and the inability to automatically segment them using traditional chemical etching methods, making automatic segmentation based on grayscale thresholds possible with Image software. The detection accuracy can reach within ±1%.
[0012] (2) The detection efficiency is significantly improved. The time for a single detection (from sample preparation to quantitative result output) is no more than 30 minutes, which is far better than the several days of time required by the traditional electrolytic extraction method and the sample preparation time of more than 2 hours for the EBSD method.
[0013] (3) The detection cost is greatly reduced. The cost of a single detection is only RMB 100-200 (reagent consumption + labor time), which is far lower than that of SEM / TEM (about RMB 2,000 / piece) and chemical extraction (about RMB 5,000 / piece). The equipment investment only requires a conventional metallographic microscope (about RMB 50,000) and electrolysis equipment, without the need to purchase large-scale characterization equipment worth millions of RMB.
[0014] (4) Solved the engineering testing problem of non-standard large-size samples. By using the dual measures of OPU fine polishing and nail polish insulation sealing, the sharp electric field concentration effect and Newton's ring light interference artifact are eliminated from the mechanism, so that non-standard samples can also obtain a uniform electrolytic coloring effect, which meets the actual engineering testing requirements.
[0015] (5) The method has strong universality. It has been verified by four typical microstructure states: bar stock, typical forgings, large deformation blades, and insufficiently deformed parts. It can be fully adapted by only fine-tuning the parameters within the range of 2~5 V and 10~30 s, covering all production microstructure types of GH4169 / GH4169D alloy.
[0016] (6) It can be directly applied to engineering production to establish a quantitative correlation between microstructure and properties. By outputting the quantitative volume fraction of the δ / η phase, it provides a quantitative criterion for the optimization of forging and heat treatment processes and the development of new processes, making up for the shortcomings of the traditional spectrum comparison method which is only qualitative and not quantitative, and improving the consistency of forging quality and mechanical properties. Attached Figure Description
[0017] To more clearly illustrate the technical solutions of the embodiments of this disclosure, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a flowchart of the present invention; Figure 2 The microstructures after electrolysis are shown for four typical microstructure states: (a) bar stock 3~3.8V / 20~30s; (b) typical forging 3~3.5V / 10~20s; (c) blade with large deformation 2~3V / 10~15s; (d) part with uneven deformation 4~5V / 15~25s. Figure 3 The flowchart of quantitative statistics for threshold segmentation in Image software and the comparison of original and segmentation results for typical fields of view are shown. In the top row (a)(b)(c): original images of fields of view 1 / 2 / 3; in the bottom row (d)(e)(f): corresponding segmentation results (red η phase), with area fractions of 4.54%, 5.11%, and 0.24% respectively. Detailed Implementation
[0019] The embodiments of this disclosure will now be described in detail with reference to the accompanying drawings.
[0020] The following specific examples illustrate the implementation of this disclosure. Those skilled in the art can easily understand other advantages and effects of this disclosure from the content disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of this disclosure, and not all of them. This disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of this disclosure. It should be noted that, in the absence of conflict, the following embodiments and features in the embodiments can be combined with each other. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this disclosure.
[0021] It should be noted that various aspects of embodiments within the scope of the appended claims are described below. It will be apparent that the aspects described herein can be embodied in a wide variety of forms, and any particular structure and / or function described herein is merely illustrative. Based on this disclosure, those skilled in the art will understand that one aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number of aspects set forth herein can be used to implement the device and / or practice the method. Additionally, this device and / or method can be implemented using other structures and / or functionalities besides one or more of the aspects set forth herein.
[0022] like Figures 1 to 3 The detection method shown is applicable to the quantitative detection of the δ phase or η phase in GH4169 or GH4169D alloys, and includes the following steps: S1: The alloy sample is pretreated to remove the plastic deformation layer and micro-unevenness on the sample surface and obtain a mirror-level flat surface. For example, the GH4169 or GH4169D alloy sample is cut, inlaid, ground step by step with 120#-2400# water sandpaper, polished with 3 μm diamond suspension, and fine polished with OPU oxide suspension. S2: An insulating film forms on the surface of the alloy sample, which can block the electric field concentration at sharp corners and edges, and eliminate preferential over-corrosion and edge collapse defects at the corners. Specifically, A single layer of commercially available nail polish (main ingredients: nitrocellulose, ethyl acetate, butyl acetate, alkyd resin, camphor, tributyl acetate citrate) is evenly applied to all sharp corners, edges, and irregular edges of the gold sample. Allow it to air dry for approximately 2 minutes until the surface is dry, forming a dense insulating film. The electrolytic corrosion process involves connecting the sample to the anode, where the anode dissolves and corrodes the sample. If sharp corners are present, electric field distortion (point effect) will occur at these edges, leading to corner corrosion and uneven coloring film on the sample surface after electrolysis. This reduces the effective evaluation field of view. Advantages: 1. Commercially available nail polish can be used as an insulating material, resulting in low cost; 2. It solves the problem of electric field concentration at sharp corners and edges during engineering testing of large-sized, non-standard shaped samples (non-standard circular or square samples, samples with sharp corners or irregular parts), eliminating the point electric field concentration effect and Newton's ring interference artifacts from a mechanistic perspective, allowing non-standard samples to achieve a uniform electrolytic coloring effect.
[0023] S3: Prepare an aqueous solution of phosphoric acid as an electrolyte. By coloring the matrix while leaving the δ or η phase uncolored, different colors are obtained under light interference, increasing the contrast between the matrix and the δ or η phase. This improves the efficiency and quality of quantitative detection during metallographic optical observation and analysis. S4: Manual constant potential electrolytic coloring, including, The alloy sample in step S2 is used as the anode, and the platinum electrode or stainless steel electrode is used as the cathode, and the phosphoric acid aqueous solution in step S3 is used as the electrolyte. Electrolytic coloring was performed in constant potential mode, wherein different electrolytic process parameters were adjusted according to alloy samples with different supply states and size specifications and carried out at room temperature, and low-speed stirring was used to eliminate local concentration differences in the solution, wherein the voltage was set so that the current density was controlled at 0.01-0.02 A / cm². After electrolysis, the surface of the alloy sample is rinsed with deionized water to remove residual electrolyte and then dried with cold air. S5: Metallographic image acquisition and processing using Image image processing and analysis software. Image software preprocessing includes median filtering for noise reduction and adaptive histogram equalization to enhance contrast. Threshold segmentation uses the Otsu automatic thresholding algorithm or manual fine-tuning of the threshold. The δ-phase or η-phase pixels are separated from the matrix based on the grayscale threshold segmentation algorithm, and the area fraction of the δ-phase or η-phase in the metallographic image is directly measured.
[0024] In one embodiment, all sharp corners, edges and irregular edges of the alloy sample in S2 are uniformly coated with nail polish to form a dense insulating film. The nail polish includes ethyl acetate, butyl acetate, nitrocellulose and alkyd resin, with a mass ratio of 15-18 parts: 12-15 parts: 19-21 parts: 11-14 parts.
[0025] In one embodiment, step S3 includes preparing a 10% (w / w) aqueous solution of phosphoric acid (H3PO4) as the electrolyte. The electrolyte is prepared by stirring at room temperature to ensure accurate concentration. For example, 100 mL of analytical grade phosphoric acid (analytical grade, ≥85% (w / w)) is slowly added to 750 mL of deionized water, stirred until homogeneous, and then the deionized water is added to a final volume of 1000 mL to prepare a 10% (w / w) aqueous solution of phosphoric acid. This solution is stored at room temperature and protected from light, and used at room temperature. The purpose of using the aqueous solution of phosphoric acid as the electrolyte is: Nail polish does not dissolve or swell in phosphoric acid water; the decomposition potential E of the δ or η phase in solution is... A A higher value means it will not ionize; the oxyacid anion phosphate (PO4) will not ionize. 3- It selectively generates nanoscale thick interference oxide films (pale blue-gray or black) on the surface of γ-matrix, while retaining the original morphology of δ / η phase (light gray or white), forming strong optical contrast and also causing electrolysis to occur in the lower potential region; Secondly, in traditional chemical etching methods, the second phase (δ or η phase) is invisible in the polished state. After chemical etching, grain boundaries, carbides, and the second phase (δ or η phase) are simultaneously revealed, while the uncorroded matrix appears bright white. Metallographic images have low contrast, and the individual phases cannot be distinguished for measurement. This application, however, colors the matrix while leaving the second phase (δ or η phase) uncolored. Under light interference, different colors are obtained, increasing the contrast between the matrix and the second phase (δ or η phase). This allows for direct metallographic optical observation and analysis, improving the efficiency and quality of quantitative detection. In contrast, after electrolysis with nitric acid-alcohol solution, the matrix is not fully colored, and the sample surface has cracks and is uneven, failing to meet evaluation conditions. Furthermore, the passivation film is unstable due to the release of NO2 and CO2 gases during nitric acid-alcohol electrolysis. In contrast, the passivation film with phosphoric acid solution is stable.
[0026] In one embodiment, S4 includes a specific classification of the alloy samples, as follows: If the alloy sample is a rod-shaped sample with moderate grain size and moderate second phase precipitation, the electrolysis process parameters are voltage 3-3.8 V and time 20-30 s; If the alloy sample is a typical forging sample with a deformation of 2.5~3, the electrolysis process parameters are voltage 3-3.5 V and time 10-20 s, in order to preserve the complete morphology of the submicron fine second phase (the second phase refers to the δ phase and η phase) to the greatest extent. If the alloy sample is a large deformation forging sample with a deformation amount ≥3, the electrolysis process parameters are voltage 2-3 V and time 10-15 s, so as to ensure that the fine δ phase or η phase does not dissolve to the maximum extent. If the alloy sample is an insufficiently deformed forging sample with a deformation amount of <2.5, the electrolysis process parameters are voltage 4-5V and time 15-25s, which can fully expose the needle-like δ phase or η phase.
[0027] The purpose of this setup is to enable clear and quantitative detection of rod-shaped samples (microstructure characteristics: medium grain size, moderate second phase) after the curing process.
[0028] 2. Forged specimens with sufficient deformation (deformation amount 2.5-3, microstructure characteristics: fine grains, low amount of second phase ηδ precipitation): the submicron second phase δ phase or η phase is fully manifested.
[0029] 3. Forging samples with large deformation, such as blades (deformation ≥ 3, microstructure characteristics: grains fully recrystallized, high content of second phase ηδ): fine second phase δ phase or η phase without dissolution.
[0030] 4. Forgings with insufficient deformation (deformation amount ≤ 2.5, microstructure characteristics: lamellar or long needle-like second phase δ phase or η phase): needle-like second phase δ phase or η phase is fully exposed.
[0031] In one embodiment, metallographic image acquisition in S5 includes... Metallographic images of the samples after electrolytic staining in step four were acquired using an optical microscope at a magnification of 500x to 1000x. At least five non-overlapping fields of view were randomly selected for each sample. For a dual-scale characteristic sample where coarse lamellar structures at grain boundaries coexist with fine needle-like precipitates within grains, images were acquired at magnifications of 500x and 1000x. The 500x magnification was used for overall precipitation level statistics, while the 1000x magnification was used for resolution and statistics of submicron-level fine precipitates.
[0032] Furthermore, in S5, the δ-phase or η-phase pixels are separated from the matrix based on the grayscale threshold segmentation algorithm, and the δ / η-phase area fraction of each field of view is calculated, including... The acquired metallographic images were imported into Image image processing and analysis software. After preprocessing (including noise reduction and contrast enhancement), the δ phase and η phase pixels were separated from the matrix based on the grayscale threshold segmentation algorithm. The area fractions of the δ and η phases in each field of view were calculated, and the arithmetic mean of no less than 5 fields of view was used as the volume fractions of the δ and η phases of the sample.
[0033] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the content described.
[0034] Example 1: Quantitative Detection of the η Phase in GH4169D Alloy Low-Pressure Turbine Disk Forgings (1) Sample preparation: Metallographic samples were cut from the GH4169D alloy low-pressure turbine disk forging (part number: 419142006101), with a size of about 15 mm × 20 mm × 10 mm (non-standard size), and hot-mounted.
[0035] (2) Grinding and polishing: Grinding was carried out sequentially using 120#, 240#, 400#, 800#, 1200#, 2000#, and 2400# wet sandpaper, rotating 90° in the grinding direction for each pass to eliminate scratches from the previous pass. Then, polishing was performed on a StruersTegramin-30 grinding and polishing system with 3 μm diamond suspension until no visible scratches were visible. Finally, OPU fine polishing fluid was used for fine polishing to remove the surface plastic deformation layer and obtain a mirror-level smooth surface.
[0036] (3) Corner insulation sealing: Apply commercially available colorless transparent nail polish (main components: ethyl acetate, butyl acetate, nitrocellulose, alkyd resin, camphor, tributyl acetyl citrate, fumed silica) evenly to all sharp corners, edges and irregular edges of the sample, and let it air dry for about 2 minutes until it is surface dry to form a dense insulating film.
[0037] (4) Electrolyte preparation: Measure 100 mL of concentrated phosphoric acid (analytical grade, mass fraction ≥85%), slowly add it to 750 mL of deionized water, stir evenly and then make up to 1000 mL to prepare a 10% phosphoric acid aqueous solution, and keep it at room temperature.
[0038] (5) Manual potentiostatic electrolytic coloring: The sample treated in step (3) is used as the anode (working electrode), and a platinum electrode is used as the cathode. It is immersed in the 10% phosphoric acid aqueous solution prepared in step (4). Connect the potentiostat, set the DC voltage to 2.5 V, the electrolysis time to 30 s, and the current density to approximately 0.015 A / cm². Low-speed magnetic stirring is used throughout the process to eliminate local concentration differences. After electrolysis, the sample is immediately removed, rinsed thoroughly with deionized water for 30 s to remove residual electrolyte, and dried with cold air.
[0039] (6) Metallographic image acquisition: Metallographic images of the samples were acquired using an optical microscope at magnifications of 500x and 1000x. Five non-overlapping fields of view were randomly selected at 500x and five non-overlapping fields of view were randomly selected at 1000x, for a total of 10 images.
[0040] (7) Threshold segmentation and quantitative statistics: The acquired images were imported into Image software, and median filtering for noise reduction (radius 2 pixels), adaptive histogram equalization to enhance contrast, and Otsu automatic threshold segmentation were performed sequentially to separate the η-phase pixels (light gray / white areas) from the matrix (black areas). The η-phase area fraction was calculated for each field of view, and the arithmetic mean of 10 fields of view was used as the η-phase volume fraction of the sample.
[0041] The test results in this embodiment show that the volume fraction of the η phase is 2.81%~3.43% (average at each test location), which is consistent with the subsequent engineering conclusion that the notch creep performance is substandard. This verifies that the low η phase content is an important internal factor leading to the failure of the notch creep performance. Each test takes approximately 25 minutes.
[0042] Example 2: Quantitative Detection of the η Phase in a GH4169D Alloy Sixth-Stage Integral Bladed Disk (1) Sample preparation: Metallographic samples were cut from the blade part and the rim part of the GH4169D alloy sixth-stage integral bladed disk forging (part number: 419115000601), with dimensions as shown in Example 1.
[0043] (2) Grinding and polishing: Same as step (2) in Example 1.
[0044] (3) Corner insulation sealing: Same as step (3) in Example 1.
[0045] (4) Electrolyte preparation: Same as step (4) in Example 1.
[0046] (5) Manual constant potential electrolytic coloring: The sample of the blade part was electrolyzed with a DC voltage of 2 V and an electrolysis time of 30 s; the sample of the rim part was electrolyzed with a DC voltage of 2.5 V and an electrolysis time of 30 s, and the current density was controlled at 0.01~0.02 A / cm². The rest of the operation was the same as step (5) in Example 1.
[0047] (6) Metallographic image acquisition: Same as step (6) in Example 1.
[0048] (7) Threshold segmentation and quantitative statistics: Same as step (7) in Example 1.
[0049] The test results of this embodiment show that the volume fraction of the η phase in the blade part is 7.23% (mean) and the volume fraction of the η phase in the rim part is 6.65% (mean), which is significantly higher than the normal suitable range (4%~6%). This is consistent with the engineering conclusion that the actual 704 ℃ / 621 MPa creep strength is unqualified, verifying that the excessive precipitation of the η phase is the core cause of the failure of the high temperature creep strength.
[0050] Example 3: Quantitative Detection of δ Phase in GH4169 Bars and Typical Forgings (1) Sample preparation: Standard metallographic samples with dimensions of 10 mm × 10 mm × 10 mm were cut from GH4169 alloy bars (multi-pass small deformation rolling + standard heat treatment state) and typical forgings (small deformation + standard solution aging state).
[0051] (2) Grinding and polishing: Same as step (2) in Example 1. Since the sample is of standard size, the sharp corner effect is relatively mild, and the corner insulation sealing step can be selectively omitted.
[0052] (3) Electrolyte preparation: Same as step (4) in Example 1.
[0053] (4) Manual constant potential electrolytic coloring: The bar sample was subjected to a DC voltage of 3.5 V and an electrolysis time of 25 s; the forging sample was subjected to a DC voltage of 3 V and an electrolysis time of 15 s, and the current density was controlled at 0.01~0.02 A / cm².
[0054] (5) Metallographic image acquisition: Using an optical microscope, five non-overlapping fields of view were randomly selected to acquire images at a magnification of 500x.
[0055] (6) Threshold segmentation and quantitative statistics: Same as step (7) in Example 1.
[0056] The test results in this embodiment are as follows: the volume fraction of the δ phase in the bar stock is approximately 3.5%~4.8% (within the normal and suitable range), and the volume fraction of the δ phase in the forging is approximately 1.2%~2.0% (too low, which is consistent with the process characteristics of small deformation and strict solid solution control in the forging). The testing time is approximately 20 minutes per piece.
[0057] Example 4: Verification of universality of four tissue states Three samples each of four typical microstructures—GH4169 / GH4169D bar stock, typical forgings, blades with large deformation, and parts with uneven deformation—were selected and tested according to the method of this invention. Due to differences in corrosion resistance among the various microstructures, the electrolysis parameters were fine-tuned as shown in Table 1.
[0058] Table 1 is a detailed classification table. Verification results show that the method of the present invention can cover all production microstructure types of the current GH4169 / GH4169D alloy within the parameter range of 2~5 V and 10~30 s, and the method has good universality.
[0059] Comparison of detection effects with existing traditional chemical corrosion methods The same GH4169D alloy sample was subjected to metallographic microstructure display using the electrolytic coloring method described in Example 1 of this invention and the traditional FeCl3 chemical etching method (5 g FeCl3 + 15 mL HCl + 100 mL H2O, wiping etching for 10 s). The remaining grinding, polishing, image acquisition and quantitative statistical steps were completely consistent.
[0060] Comparison results: (1) Under the traditional chemical etching method, the gray difference between the δ / η phase and the γ matrix is very small. The automatic threshold segmentation of Image software Otsu cannot effectively separate the second phase from the matrix. The manual threshold segmentation results are extremely unstable, and the area fraction obtained by different operators in the same field of view has a deviation of more than ±5%. (2) Under the electrolytic coloring method of the present invention, the η phase is light gray / white and the matrix is black. The contrast between the two phases is strong. The automatic threshold segmentation results of Otsu are stable and reliable. The area fraction obtained by different operators in the same field of view has a deviation of less than ±0.5%. This comparison fully demonstrates the significant advantages of the method of the present invention in terms of contrast enhancement and quantitative accuracy.
[0061] The above are merely specific embodiments of this disclosure, but the scope of protection of this disclosure is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this disclosure should be included within the scope of protection of this disclosure. Therefore, the scope of protection of this disclosure should be determined by the scope of the claims.
Claims
1. A quantitative detection method for the second phase in nickel-based superalloys via electrolytic metallography, applicable to the quantitative detection of the δ and η phases in GH4169 and GH4169D alloys, characterized in that, Includes the following steps, S1: The alloy sample is pretreated to remove the plastic deformation layer and micro-unevenness on the sample surface and obtain a mirror-level flat surface. S2: An insulating film is formed on the surface of the alloy sample, which can block the electric field concentration at sharp corners and edges and eliminate preferential over-corrosion and edge collapse defects at the corners. S3: Prepare an aqueous solution of phosphoric acid as an electrolyte. By coloring the matrix while leaving the δ or η phase uncolored, different colors are obtained under light interference, increasing the contrast between the matrix and the δ or η phase. This can improve the efficiency and quality of quantitative detection during metallographic optical observation and analysis. S4: Manual constant potential electrolytic coloring, including, The alloy sample in step S2 is used as the anode, and the platinum electrode or stainless steel electrode is used as the cathode, and the phosphoric acid aqueous solution in step S3 is used as the electrolyte. Electrolytic coloring was performed in constant potential mode, wherein different electrolytic process parameters were adjusted according to alloy samples with different supply states and size specifications and carried out at room temperature, and low-speed stirring was used to eliminate local concentration differences in the solution, wherein the voltage was set so that the current density was controlled at 0.01-0.02 A / cm². After electrolysis, the surface of the alloy sample is rinsed with deionized water to remove residual electrolyte and then dried with cold air. S5: Metallographic image acquisition and processing using Image image processing and analysis software; The δ-phase or η-phase pixels are separated from the matrix based on the grayscale threshold segmentation algorithm, and the area fraction of the δ-phase or η-phase in the metallographic image is directly measured.
2. The method according to claim 1, characterized in that, Preprocessing in S1 includes, The GH4169 or GH4169D alloy samples were sequentially cut, inlaid, ground with 120#-2400# wet sandpaper, polished with 3 μm diamond suspension, and finely polished with OPU oxide suspension.
3. The method according to claim 1, characterized in that, In S2, all sharp corners, edges, and irregular edges of the alloy sample are uniformly coated with nail polish to form a dense insulating film.
4. The method according to claim 3, characterized in that, The nail polish comprises ethyl acetate, butyl acetate, nitrocellulose, and alkyd resin, in a mass ratio of 15-18 parts: 12-15 parts: 19-21 parts: 11-14 parts.
5. The method according to claim 1, characterized in that, S3 includes, Prepare a 10% (w / w) phosphoric acid aqueous solution as the electrolyte. Stir the electrolyte at room temperature during preparation to ensure accurate concentration.
6. The method according to claim 1, characterized in that, S4 includes, If the alloy sample is a rod-shaped sample with moderate grain size and moderate second phase precipitation, the electrolysis process parameters are voltage 3-3.8 V and time 20-30 s; If the alloy sample is a typical forging sample with a deformation of 2.5-3, the electrolysis process parameters are voltage 3-3.5 V and time 10-20 s, so as to preserve the complete morphology of the submicron fine second phase to the greatest extent. If the alloy sample is a large deformation forging sample with a deformation amount ≥3, the electrolysis process parameters are voltage 2-3 V and time 10-15 s, so as to ensure that the fine δ phase or η phase does not dissolve to the maximum extent. If the alloy sample is an insufficiently deformed forging sample with a deformation amount of <2.5, the electrolysis process parameters are voltage 4-5V and time 15-25s, which can fully expose the needle-like δ phase or η phase.
7. The method according to claim 1, characterized in that, Metallographic image acquisition in S5 includes, Metallographic images of the samples after electrolytic staining in step four were acquired using an optical microscope at a magnification of 500x to 1000x. At least five non-overlapping fields of view were randomly selected for each sample. For a dual-scale characteristic sample where coarse lamellar structures at grain boundaries coexist with fine needle-like precipitates within grains, images were acquired at magnifications of 500x and 1000x. The 500x magnification was used for overall precipitation level statistics, while the 1000x magnification was used for resolution and statistics of submicron-level fine precipitates.
8. The method according to claim 7, characterized in that, In S5, the grayscale threshold segmentation algorithm separates the δ-phase or η-phase pixels from the matrix, and directly measures the area fraction of the δ-phase or η-phase in the metallographic image, including... The acquired metallographic images are imported into Image image processing and analysis software. After preprocessing, the δ phase or η phase pixels are separated from the matrix based on the grayscale threshold segmentation algorithm. The area fraction of the δ phase or η phase in each field of view is directly measured, and the arithmetic mean of no less than 5 fields of view is taken as the volume fraction of the δ phase or η phase of the sample.