Surfaces with lubricious or low-friction properties
Patent Information
- Application Number
- JP2023519065
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-09-25
- Filing Date
- 2021-09-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-09-24
AI Technical Summary
Existing methods for creating low-friction surfaces on medical devices, such as catheters, are prone to abrasion, delamination, and toxicity issues, and require costly processes that are not suitable for all device configurations, leading to potential health risks and functional limitations.
The use of oligofluorinated additives, or surface-modifying polymers (SMMs), mixed with base polymers to create low-friction surfaces by melt extrusion or molding, which migrate to the surface during manufacturing, providing stable and lubricious properties.
The SMMs significantly reduce the coefficient of friction by 30-88% in various polymers, enhancing lubricity and durability, while avoiding the drawbacks of traditional coatings, thus improving device functionality and safety.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] This invention relates to the use of oligofluorinated additives (also known as surface-modifying polymers or SMMs) for the purpose of modifying surface properties to produce lubricating or low-friction surfaces. The additives can be mixed with a base polymer to form a mixture used in the manufacture of equipment, components, or coatings where a low coefficient of friction (CoF) is required.
[0002] Background explanation A low coefficient of friction or lubricity of an article's surface is desirable in a variety of applications where it is necessary to allow one surface to move easily on another for proper or optimal function. This is particularly important in medical device applications. For example, in devices such as catheters and guidewires, a lubricated surface allows for the use of lower insertion forces, easier tracking through complex vascular systems, reduced tissue inflammation / damage, and improved patient comfort. Furthermore, lubricity may be desirable to facilitate the drainage of fluids within medical conduits. Lubricity may be required on all parts of a medical device, or only on some parts of the device.
[0003] One common method for creating low-friction surfaces in medical devices is to apply hydrophilic or water-loving coatings. These are typically based on hydrogel polymers such as PVP, which can absorb large amounts of water. However, coatings can be susceptible to abrasion and delamination, which can lead to reduced functionality and potential hazards due to the generation of microparticles in the body. For example, microparticles from coatings on intravascular catheters can cause embolism, potentially leading to fatal consequences for patients. Furthermore, coatings can be difficult to apply to certain substrates, often requiring a base coat, tie coat, and curing method, and may need to be specially formulated to match the substrate to ensure that plasticizers or colorants that cause blooming on the substrate surface do not affect coating adhesion. The use of organic solvents or polymerizable monomers and associated reagents in the coating process can raise toxicity concerns if residual reagents are not completely removed from the final coating. In addition, coating applications require costly capital investment and generate large amounts of reagent waste.
[0004] Another limitation of coatings is that they may be difficult or impossible to apply to all instrument configurations, such as multiple catheter lumens. Furthermore, especially with hydrogel coatings, significant swelling upon water absorption can increase the coating thickness, which can affect instrument function when dimensional tolerances are critical. Additionally, certain hydrogel coatings tend to dry rapidly, potentially losing lubricity after removal from the hydration solution and before use if sufficient hydration cannot be maintained.
[0005] Another way to form a low-friction surface on a thermoplastic catheter tube is by co-extrusion with a very thin PTFE liner, but this process is expensive because it requires a fair amount of technical expertise. Yet another method is to incorporate PTFE powder or a lubricating oil into the thermoplastic resin used for extrusion. However, these surfaces often require "conditioning" in the sense of removing some material from the surface to function properly and are not suitable for all applications. Additionally, PTFE powder can cause bonding problems in post-extrusion processes.
[0006] Polymers used to form medical devices, components, or coatings that require low-friction properties can be selected particularly from the group consisting of polyurethane, silicone, polyamide, polyester, copolyester, polyether, polyether-block-amide copolymer, polypropylene, polyethylene, polyvinyl chloride, polysulfone, polyetherimide, polycarbonate, polyetheretherketone, ethyl vinyl acetate, polyolefin, styrene block copolymer, and vulcanized rubber. The polymer can particularly contain other additives such as a radiopaque filler, a colorant, a processing aid, an antibacterial agent, or a preservative.
[0007] U.S. Patent No. 6,127,507 to Santerre discloses a fluoro-oligomer surface modifier for polymers and articles manufactured therefrom.
[0008] U.S. Patent Nos. 8,071,683, 8,178,620, and 8,338,537 to Mullick et al. report a surface-modifying polymer having a high decomposition temperature and its use.
[0009] Mullick et al.'s U.S. Patent No. 8,318,867, U.S. Patent No. 9,751,972, U.S. Patent Publication No. 2011 / 0207893, and U.S. Patent Publication No. 2018 / 0179327 report on surface-modifying polymers based on thermally stable biuret and isocyanurate, as well as their uses.
[0010] Mullick et al.'s U.S. Patent Application Publication No. 2017 / 0369646 describes ester-bonded surface-modified polymers.
[0011] Santerre et al.'s international publication No. 2019 / 169500 reports on carbonate-bonded surface-modified polymers.
[0012] Steedman et al., in U.S. Patent Application Publication No. 2019 / 0142317, report an embedded glucose sensor having a biostable surface.
[0013] Summary of the Invention In this invention, an oligofluorinated additive (SMM) is mixed with a base polymer or composite material used in the manufacture of articles such as medical devices that require low friction properties, and the low friction surface contains the oligofluorinated additive mixed with the base polymer.
[0014] In a further embodiment, the present invention is characterized by an article having a surface with low friction properties.
[0015] A further aspect of the present invention relates to a medical device having a surface with low friction properties.
[0016] A further aspect of the present invention relates to a medical catheter having a surface with low friction properties.
[0017] A further aspect of the present invention relates to a method for reducing the coefficient of friction of a surface by applying a mixture comprising an oligofluorinated additive and a base polymer to a surface.
[0018] A further aspect of the present invention relates to a method for producing an article by melt extrusion or molding a composition comprising an oligofluorinated additive and a base polymer.
[0019] These and other aspects of the present invention are provided by articles having a surface comprising an oligofluorinated additive mixed with a base polymer.
[0020] The inventors have discovered that a mixture of an oligofluorinated additive and a base polymer provides a surface with low friction properties.
[0021] By considering the attached drawings in conjunction with the following detailed description, a deeper understanding of the present invention and its many associated advantages will be easily achieved. [Brief explanation of the drawing]
[0022] [Figure 1] This shows the coefficient of friction of polyether block amide copolymer rods with and without surface modification additives. [Figure 2] This shows the coefficient of friction of polyurethane rods with and without surface modification additives. [Figure 3] This shows the coefficient of friction of polyurethane rods with and without surface modification additives. [Figure 4] This shows the coefficient of friction of polyurethane catheter tubes with and without surface modification additives. [Figure 5] This shows the coefficient of friction of silicone catheter tubes with and without surface modification additives. [Figure 6] This shows the coefficient of friction of polyurethane films with and without surface modification additives. [Figure 7] This shows the coefficient of friction of polyether block amide copolymer catheter tubes with and without surface modification additives. [Figure 8] This shows the coefficient of friction of polyamide rods with and without surface modification additives. [Figure 9] This shows the coefficient of friction of polyvinyl chloride rods with and without surface modification additives.
[0023] Detailed description of preferred embodiments Fluorooligomer (SMM) In one embodiment, the present invention provides a fluorooligomer (also called a surface-modified polymer or SMM) having a central portion and terminal groups, wherein the central portion comprises segmented oligomeric copolymer units and the terminal groups comprise α-ω-terminated polyfluorooligomer groups.
[0024] Due to their surfactant properties, additives migrate to all surfaces of the material during manufacturing, creating a unique surface chemistry.
[0025] Preferably, the polyfluorooligomer group is a perfluoroalkyl group, and the polar hard segment is selected from the group consisting of urethanes, esters, amides, sulfonamides, and carbonates.
[0026] The SMM according to the present invention is synthesized to include a base polymer-compatible segment and a terminally hydrophobic fluorine component that is incompatible with the base polymer. The compatible segment of the SMM is selected to provide anchors for the SMM within the base polymer substrate during mixing. Although not bound by theory, it is thought that the fluorine tails partially play a role in transporting the SMM to the surface of the mixture, causing the fluorine chain to be exposed from the surface. The latter process is thought to be driven by the thermodynamic incompatibility of the fluorine tails and the polymer base substrate, and the tendency for them to have lower surface energies at the surface of the mixture. When there is a balance between fixation and surface migration, the SMM remains stable on the polymer surface, while simultaneously altering its surface properties. The usefulness of the additive of the present invention compared to other known polymer additives lies in 1) the molecular arrangement of the amphiphilic segment of the SMM chain, i.e., having two ω-fluoro tails, one at each end, and a central portion between them; and 2) the molecular weight of the fluorine tails relative to the molecular weight of the central portion.
[0027] More specifically, the compounds of the present invention include formulations synthesized using hydrophilic or amphiphilic building blocks incorporated into the main chain of an SMM molecule. These building blocks may include hydrophilic reactive monomers or oligomers, or reactive oligomers having both hydrophilic and hydrophobic segments. Examples of building blocks include oligomeric diols containing only polyethylene oxide (PEO) segments, or alternating PEO segments with hydrophobic polyether or siloxane segments.
[0028] A suitable fluorooligomer can also be described by any one of the structures shown below in formulas (I), (II), (III), (IV), (V), and (VI). (1) Equation (I): F T -[BA] n -BF T (I) [In the formula, (i) A is polypropylene oxide, polyethylene oxide, polytetramethylene oxide, hydrogenated polybutadiene (e.g., HLBH), polybutadiene (e.g., LBHP), hydrogenated polyisoprene (e.g., HHTPI), poly(diethylene glycol) adipate, diethylene glycol-orthophthalic anhydride) polyester, (neopentyl glycol-orthophthalic anhydride) polyester, (1,6-hexanediol-orthophthalic anhydride) polyester, poly(hexamethylene carbonate), poly((2,2-dimethyl)-1,3-propylene carbonate Includes polycarbonate polyols, poly(ethylene-co-butylene), polystyrene, polysiloxane, polydimethylsiloxane, polypropylene glycol-polyethylene glycol block copolymer, polysiloxane-polyethylene glycol block copolymer, polysiloxane-polypropylene glycol block copolymer, or other block copolymers containing block segments selected from the group of polypropylene oxide, polyethylene oxide, polytetramethylene oxide, polysiloxane, and polydimethylsiloxane; (ii) B is a segment containing urethane; (iii)F T It is a polyfluoroorgano group; (iv) n is an integer between 1 and 10. (2) Equation (II) or Equation (III): [ka] [In the formula, (i) A is an oligomer segment containing ether bonds, ester bonds, carbonate bonds, and polyalkylene, where A is polypropylene oxide, polyethylene oxide, polytetramethylene oxide, hydrogenated polybutadiene (e.g., HLBH), polybutadiene (e.g., LBHP), hydrogenated polyisoprene (e.g., HHTPI), poly(diethylene glycol) adipate, (diethylene glycol-orthophthalic anhydride) polyester, (neopentyl glycol-orthophthalic anhydride) polyester, (1,6-hexanediol-orthophthalic anhydride) polyester, poly(hexamethylene carbonate), Includes ((2,2-dimethyl)-1,3-propylene carbonate), polycarbonate polyol, poly(ethylene-co-butylene), polystyrene, polysiloxane, polydimethylsiloxane, polypropylene glycol-polyethylene glycol block copolymer, polysiloxane-polyethylene glycol block copolymer, polysiloxane-polypropylene glycol block copolymer, or other block copolymers containing block segments selected from the group of polypropylene oxide, polyethylene oxide, polytetramethylene oxide, polysiloxane, and polydimethylsiloxane; (ii) B is a segment containing an isocyanurate trimer or a biuret trimer, and B' is a segment containing urethane, if present; (iii) Each F T It is a polyfluoroorgano group; (iv) n is an integer between 0 and 10. (3) Formula (IV): [ka] [In the formula, (i)Each F T These are surfactant groups independently selected from polydimethylsiloxanes, hydrocarbons, and polyfluoroorgano groups, and combinations thereof (e.g., each F T It is independently a polyfluoroorgano; (ii) X1 is H, CH3, or CH2CH3; (iii) Each of X2 and X3 is independently H, CH3, CH2CH3, or F T ; (iv) Each of L1 and L2 is independently a bond, an oligomeric linking group, or a linking group having two terminal carbonyls; (v) n is an integer from 5 to 50]. (4) Formula (V): [wherein, (i) Each F is independently a surfactant group (for example, polyfluoroorgano, hydroxyl, or polyethylene glycol); T (ii) Each of X1, X2, and X3 is independently H, CH3, CH2CH3, or F ; T (iii) Each of L1 and L2 is independently a bond, an oligomeric linking group, a linking group having two terminal carbonyls, or is formed from a diisocyanate; (iv) Each of n1 and n2 is independently an integer from 5 to 50].<00002XX>(iv) Each of n1 and n2 is independently an integer from 5 to 50].
[0029] In one embodiment of formula (I), A is polypropylene oxide, polyethylene oxide, or polytetramethylene oxide.<XXXXXX><XXXXXX><XXXXXX>In another embodiment of formula (I), A is polypropylene oxide, polyethylene oxide, or polytetramethylene oxide, or a mixture thereof, and has a theoretical molecular weight of 200 to 3,000 Daltons (for example, 500 to 2,000 Daltons, 1,000 to 2,000 Daltons, or 1,000 to 3,000 Daltons).
[0031] In another embodiment of formula (I), A is a segment selected from the group consisting of hydrogenated polybutadiene (e.g., HLBH), poly(diethylene glycol) adipate, or (diethylene glycol-orthophthalic acid) anhydride polyester, having a theoretical molecular weight of 750 to 3,500 daltons (e.g., 750 to 2,000 daltons, 1,000 to 2,500 daltons, or 1,000 to 3,500 daltons).
[0032] In another embodiment of formula (I), A comprises a polypropylene glycol-polyethylene glycol block copolymer (PLN diol) or a block copolymer having a block segment selected from polypropylene oxide, polyethylene oxide, polytetramethylene oxide, or a mixture thereof, and a block segment selected from polysiloxane or polydimethylsiloxane (C10 diol), wherein A has a theoretical molecular weight of 1,000 to 5,000 daltons (e.g., 1,000 to 3,000 daltons, 2,000 to 5,000 daltons, or 2,500 to 5,000 daltons).
[0033] In another embodiment of formula (II) or (III), A is an oligomeric segment comprising polyethylene oxide, polypropylene oxide, polytetramethylene oxide, or a mixture thereof, and having a theoretical molecular weight of 200 to 3,000 daltons (e.g., 500 to 2,000 daltons, 1,000 to 2,000 daltons, or 1,000 to 3,000 daltons).
[0034] In another embodiment of formula (II) or (III), A comprises a polypropylene glycol-polyethylene glycol block copolymer (PLN diol) or a block copolymer having a block segment selected from polypropylene oxide, polyethylene oxide, polytetramethylene oxide, or a mixture thereof, and a block segment selected from polysiloxane or polydimethylsiloxane (C10 diol), wherein A has a theoretical molecular weight of 1,000 to 5,000 daltons (e.g., 1,000 to 3,000 daltons, 2,000 to 5,000 daltons, or 2,500 to 5,000 daltons).
[0035] In another embodiment of formula (II) or (III), A is hydrogenated polybutadiene (e.g., HLBH), poly(diethylene glycol) adipate, or (diethylene glycol-orthophthalic acid) anhydride polyester, having a theoretical molecular weight of 750 to 3,500 daltons (e.g., 750 to 2,000 daltons, 1,000 to 2,500 daltons, or 1,000 to 3,500 daltons).
[0036] The SMM of formula (I) may include B formed from diisocyanates (e.g., 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate; 4,4'-methylenebis(cyclohexyl isocyanate); 4,4'-methylenebis(phenyl isocyanate); toluene-2,4-diisocyanate; m-tetramethylxylenediisocyanate; or hexamethylenediisocyanate). The variable n may be 1 or 2. The medical device of the present invention may comprise a base polymer and the SMM of formula (I).
[0037] In the SMM of formula (II) or (III), B is formed by reacting a triisocyanate (e.g., hexamethylene diisocyanate (HDI) biuret trimer, isophorone diisocyanate (IPDI) trimer, or hexamethylene diisocyanate (HDI) trimer) with a diol containing oligomeric segment A. The medical device of the present invention may comprise a base polymer and the SMM of formula (II). The medical device of the present invention may comprise a base polymer and the SMM of formula (III).
[0038] In the SMM of formula (I), B may be a segment formed from 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate; 4,4'-methylenebis(cyclohexyl isocyanate); 4,4'-methylenebis(phenyl isocyanate); toluene-2,4-diisocyanate; m-tetramethylxylene diisocyanate; and hexamethylene diisocyanate. In the SMM of formula (I), segment A may be poly(ethylene oxide). The variable n may be an integer from 1 to 3. The medical device of the present invention may comprise a base polymer and the SMM of formula (I).
[0039] In the SMM of formula (II) or (III), B is a segment formed by the reaction of a triisocyanate with the diol of A. The triisocyanate may be a hexamethylene diisocyanate (HDI) biuret trimer, an isophorone diisocyanate (IPDI) trimer, or a hexamethylene diisocyanate (HDI) trimer. In the SMM of formula (II) or (III), segment A may be poly(ethylene oxide). The variable n may be 0, 1, 2, or 3. The medical device of the present invention may comprise a base polymer and an SMM of formula (II) or (III).
[0040] In the SMM of formula (I), B may be a segment formed from 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate; 4,4'-methylenebis(cyclohexyl isocyanate); 4,4'-methylenebis(phenyl isocyanate); toluene-2,4-diisocyanate; m-tetramethylxylene diisocyanate; and hexamethylene diisocyanate. In the SMM of formula (I), segment A may be poly(ethylene oxide)-b-poly(propylene oxide)-b-poly(ethylene oxide). The variable n may be an integer from 1 to 3. The medical device of the present invention may comprise a base polymer and the SMM of formula (I).
[0041] In the SMM of formula (II) or (III), B is a segment formed by the reaction of a triisocyanate with the diol of A. The triisocyanate may be a hexamethylene diisocyanate (HDI) biuret trimer or a hexamethylene diisocyanate (HDI) trimer. In the SMM of formula (II) or (III), segment A may be poly(ethylene oxide)-b-poly(propylene oxide)-b-poly(ethylene oxide). The variable n may be 0, 1, 2, or 3. The medical device of the present invention may comprise a base polymer and the SMM of formula (II) or (III).
[0042] In the SMM of formula (I), B is a segment formed from a diisocyanate. Segment A may include a polysiloxane-polyethylene glycol block copolymer (e.g., PEG-PDMS-PEG). Segment B can be formed from 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate; 4,4'-methylenebis(cyclohexyl isocyanate); 4,4'-methylenebis(phenyl isocyanate); toluene-2,4-diisocyanate; m-tetramethylxylene diisocyanate; and hexamethylene diisocyanate. The variable n may be 1, 2, or 3. The medical device of the present invention may comprise a base polymer and the SMM of formula (I).
[0043] In the SMM of formula (II) or (III), B is a segment formed by reacting a triisocyanate with the diol of A. Segment A may include a polysiloxane-polyethylene glycol block copolymer (e.g., PEG-PDMS-PEG). The triisocyanate may be a hexamethylene diisocyanate (HDI) biuret trimer, an isophorone diisocyanate (IPDI) trimer, or a hexamethylene diisocyanate (HDI) trimer. The variable n may be 0, 1, 2, or 3. The medical device of the present invention may comprise a base polymer and an SMM of formula (II) or (III).
[0044] The SMM of formula (IV) may include segment L1, which is an oligomeric linking group (e.g., less than 50 repeating units (e.g., 2 to 40 units, 2 to 30 units, 3 to 20 units, or 3 to 10 units)). In some embodiments of formula (IV), L2 is an oligomeric linking group (e.g., less than 50 repeating units (e.g., 2 to 40 units, 2 to 30 units, 3 to 20 units, or 3 to 10 units)). In certain embodiments of formula (IV), L1 and L2 are each a bond. In certain embodiments of formula (IV), the SMM comprises an oligomer segment (e.g., in either L1 or L2) selected from the group consisting of polyurethane, polyurea, polyamide, polyalkylene oxide (e.g., polypropylene oxide, polyethylene oxide, or polytetramethylene oxide), polyester, polylactone, polysilicone, polyethersulfone, polyolefin, polyvinyl derivative, polypeptide, polysaccharide, polysiloxane, polydimethylsiloxane, poly(ethylene-co-butylene), polyisobutylene, and polybutadiene. In some embodiments of formula (IV), the SMM comprises formula (IV-A): [ka] [In the formula, m1 and m2 are independently integers between 0 and 50.] It is a compound of the formula (IV-A). In certain embodiments of formula (IV-A), m1 is 5, 6, 7, 8, 9, or 10 (for example, m1 is 6). In some embodiments of formula (IV-A), m2 is 5, 6, 7, 8, 9, or 10 (for example, m2 is 6).
[0045] In certain embodiments of formula (IV) or (IV-A), X2 is F T In another embodiment, X2 is CH3 or CH2CH3. In a particular embodiment of formula (IV) or (IV-A), X3 is F T In another embodiment, each F T These are independently polyfluoroorganos (e.g., -(O) q -C(=O)] r (CH2) o (CF2) p A polyfluoroacyl such as CF3, where q is 0, r is 1, o is 0-2, and p is 0-10. In certain embodiments of formula (IV) or (IV-A), n is an integer from 5 to 40 (e.g., 5-20 such as 5, 6, 7, 8, 9, or 10). In some embodiments of formula (IV) or (IV-A), each F T (CF2)5CF3 is included. The medical device of the present invention may include a base polymer and SMM of formula (IV). The medical device of the present invention may include a base polymer and SMM of formula (IV-A).
[0046] The SMM of formula (V) may include segment L1, which is an oligomeric linking group (e.g., less than 50 repeating units (e.g., 2 to 40 units, 2 to 30 units, 3 to 20 units, or 3 to 10 units)). In some embodiments of formula (V), L2 is an oligomeric linking group (e.g., less than 50 repeating units (e.g., 2 to 40 units, 2 to 30 units, 3 to 20 units, or 3 to 10 units)). In certain embodiments of formula (V), L1 and L2 are each a bond. In certain embodiments of formula (V), the SMM comprises an oligomer segment (e.g., in either L1 or L2) selected from polyurethane, polyurea, polyamide, polyalkylene oxide (e.g., polypropylene oxide, polyethylene oxide, or polytetramethylene oxide), polyester, polylactone, polysilicone, polyethersulfone, polyolefin, polyvinyl derivative, polypeptide, polysaccharide, polysiloxane, polydimethylsiloxane, poly(ethylene-co-butylene), polyisobutylene, and polybutadiene. In some embodiments of formula (V), the SMM comprises an oligomer segment (e.g., in either L1 or L2) of formula (VA): [ka] [In the formula, m1 and m2 are independently integers between 0 and 50.] It is a compound of the formula (VA). In certain embodiments of formula (VA), m1 is 5, 6, 7, 8, 9, or 10 (for example, m1 is 6). In some embodiments of formula (VA), m2 is 5, 6, 7, 8, 9, or 10 (for example, m2 is 6).
[0047] In certain embodiments of formula (V) or (VA), X2 is F T In another embodiment of formula (V) or (VA), X2 is CH3 or CH2CH3. In a particular embodiment of formula (V) or (VA), X3 is F T In another embodiment of formula (V) or (VA), each F T These are independently polyfluoroorganos (e.g., -(O) q -C(=O)] r (CH2)o (CF2) p It is a polyfluoroacyl such as CF3, where q is 0, r is 1, o is 0-2, and p is 0-10. In some embodiments of formula (V) or (VA), each F T (CF2)3CF3 is included. The medical device of the present invention may include a base polymer and SMM of formula (V).
[0048] The medical device of the present invention may comprise a base polymer and an SMM of formula (VA).
[0049] In any of the SMMs of the present invention formed from diisocyanates, the diisocyanate is 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate; 4,4'-methylenebis(cyclohexyl isocyanate) (HMDI); 2,2'-, 2,4'-, and 4,4'-methylenebis(phenyl isocyanate) (MDI); toluene-2,4-diisocyanate; aromatic aliphatic isocyanates such as 1,2-, 1,3-, and 1,4-xylenediisocyanate; and meta-tetramethylxylenediisocyanate (m-T MXDI); p-tetramethylxylene diisocyanate (p-TMXDI); hexamethylene diisocyanate (HDI); ethylene diisocyanate; propylene-1,2-diisocyanate; tetramethylene diisocyanate; tetramethylene-1,4-diisocyanate; octamethylene diisocyanate; decamethylene diisocyanate; 2,2,4-trimethylhexamethylene diisocyanate; 2,4,4-trimethylhexamethylene diisocyanate; dodecane-1,12-diisocyanate; dicyclohexylmethane diisocyanate ;Cyclobutane-1,3-diisocyanate;Cyclohexane-1,2-diisocyanate;Cyclohexane-1,3-diisocyanate;Cyclohexane-1,4-diisocyanate;Methylcyclohexylene diisocyanate (HTDI);2,4-dimethylcyclohexane diisocyanate;2,6-dimethylcyclohexane diisocyanate;4,4'-dicyclohexyl diisocyanate;2,4'-dicyclohexyl diisocyanate;1,3,5-cyclohexanetriisocyanate;Isocyanatemethylcyclohexaneisocyanate;1 -Isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane; isocyanatoethylcyclohexane isocyanate; bis(isocyanatomethyl)-cyclohexane; 4,4'-bis(isocyanatomethyl)dicyclohexane; 2,4'-bis(isocyanatomethyl)dicyclohexane; isophorone diisocyanate (IPDI); 2,4-hexahydrotoluene diisocyanate; 2,6-hexahydrotoluene diisocyanate; 3,3'-dimethyl-4,4'-biphenylenediisocyanate (TODD; polymeric MDI;Carbodiimide-modified liquid 4,4'-diphenylmethane diisocyanate; para-phenylenediisocyanate (PPDI); meta-phenylenediisocyanate (MPDI); naphthylene-1,5-diisocyanate; 2,4'-, 4,4'-, or 2,2'-biphenyl diisocyanate; polyphenylpolymethylene polyisocyanate (PMDI); mixtures of MDI and PMDI; mixtures of PMDI and TDI; dimerized uretdiones of any isocyanates described herein, e.g., uretdione of toluene diisocyanate, uretdione of hexamethylene diisocyanate, or mixtures thereof; or mixtures of substituted or isomerized forms thereof.
[0050] In any of the SMMs of the present invention formed from an isocyanate trimer, the isocyanate trimer may be a hexamethylene diisocyanate (HDI) biuret or trimer, an isophorone diisocyanate (IPDI) trimer, a hexamethylene diisocyanate (HDI) trimer; a 2,2,4-trimethyl-1,6-hexane diisocyanate (TMDI) trimer; a trimer of any isocyanate described herein, such as an isocyanurate of toluene diisocyanate, a trimer of diphenylmethane diisocyanate, a trimer of tetramethylxylene diisocyanate, or a mixture thereof; a trimer of any isocyanate described herein; a modified isocyanate derived from the diisocyanate above; or a mixture of substituted or isomers thereof.
[0051] SMM is a polyfluoroorgano group with a theoretical molecular weight of 100 Da to 1,500 Da. T It can include a base. For example, F T is CF3 (CF2) r (CH2CH2) p -[wherein p is 0 or 1 and r is 2 to 20], and CF3(CF2) s (CH2CH2O) χ [In the formula, χ is between 0 and 10, and s is between 1 and 20] may be used. Alternatively, F T CHm F (3-m) (CF2) r CH2CH2- or CH m F (3-m) (CF2) s (CH2CH2O) χ -[wherein m is 0, 1, 2, or 3, χ is an integer from 0 to 10, r is an integer from 2 to 20, and s is an integer from 1 to 20]. In certain embodiments, F T is 1H,1H,2H,2H-perfluoro-1-decanol; 1H,1H,2H,2H-perfluoro-1-octanol; 1H,1H,5H-perfluoro-1-pentanol; or 1H,1H-perfluoro-1-butanol, or a mixture thereof. In certain embodiments, F T These are (CF3)(CF2)5CH2CH2O-, (CF3)(CF2)7CH2CH2O-, (CF3)(CF2)5CH2CH2O-, CHF2(CF2)3CH2O-, (CF3)(CF2)2CH2O-, or (CF3)(CF2)5-. In yet another embodiment, the polyfluoroalkyl group is (CF3)(CF2)5-, for example, the polyfluoroalkyl group is bonded to the carbonyl group of the ester group. In a particular embodiment, the polyfluoroorgano is -(O) q [C(=O)] r -(CH2) o (CF2) p CF3 [wherein q is 0 and r is 1, or q is 1 and r is 0, o is between 0 and 2, and p is between 0 and 10].
[0052] Equation (VI): F T -OC(O)OB-OC(O)O-[A-OC(O)OB] n -OC(O)OF T (VI) [In the formula, (i) A contains a soft segment which is covalently bonded to B via a carbonate bond; (ii) B is a polyalkylene oxide or formula: [ka] It includes the region represented by and is covalently bonded to A via a carbonate bond; (iii) FT is a surfactant group containing a polyfluoroorgano group, F T It is covalently bonded to B via a carbonate bond; (iv) n is an integer between 1 and 10. The following compounds are also suitable.
[0053] A compound of formula (I), (i) A is [ka] (ii) B is a segment containing urethane formed from 4,4'-methylenebis(cyclohexyl isocyanate); (iii) F T (iv) is a polyfluoroorgano group; (iv) x is an integer from 8 to 12, y is an integer from 6 to 9, and n is an integer from 1 to 10; compounds are also suitable. In certain embodiments, n is 1 or 2.
[0054] The present invention relates to a compound of formula (I), (i) A is, [ka] (ii) B is a segment having 7,000 to 9,000 Da MW, containing 75% to 85% (w / w) polyethylene oxide and 15% to 25% (w / w) polypropylene oxide; (ii) B is a segment containing urethane formed from 4,4'-methylenebis(cyclohexyl isocyanate); (iii) F T The compound is characterized by having a polyfluoroorgano group; (iv)n is an integer from 1 to 10. In certain embodiments, n is 1 or 2. In some embodiments, A has an average MW of about 8,000 Da and contains about 80% (w / w) polyethylene oxide and about 20% (w / w) polypropylene oxide.
[0055] The present invention relates to a compound of formula (II), (i) A is, [ka] (ii) B is a segment having a MW of 7,000 to 9,000 Da, containing 75% to 85% (w / w) polyethylene oxide and 15% to 25% (w / w) polypropylene oxide; (ii) B is a segment containing an isocyanurate trimer or biuret trimer formed from an isophorone diisocyanate (IPDI) trimer; (iii) F T The compound is characterized by having a polyfluoroorgano group; (iv)n is an integer between 0 and 10.
[0056] In any embodiment of the above compound, F T The general formula is CH m F (3-m) (CF2) r CH2 CH2- and CH m F (3-m) (CF2) s (CH2CH2O) χ -Selected from the group consisting of radicals [wherein m is 0, 1, 2, or 3, χ is an integer from 1 to 10, r is an integer from 2 to 20, and s is an integer from 1 to 20]. In certain embodiments, m is 0 or 1.
[0057] Specific examples of SMMs of the present invention include compounds having the following formula: compound 1 [ka] [The PEG content is 50% by weight, the (x+z):y ratio is approximately 1.38, and the Mn content is approximately 1,900 g / mol.] compound 2 [The PEG content is 50% by weight, the (x+z):y ratio is approximately 1.38, and the Mn content is approximately 1,900 g / mol.] compound 3 [The PEG content is 40% by weight, the (x+z):y ratio is approximately 0.88, and the Mn content is approximately 2,900 g / mol.] compound 4 [ka] [n is approximately 46] compound 5 [ka] [n is approximately 9] compound 6 [ka] [n is approximately 20-28] compound 7 [ka]
[0058] Suitable fluorooligomers are described in U.S. Patent Nos. 6,127,507, 8,071,683, 8,178,620, 8,338,537, 8,318,867, 9,751,972, U.S. Patent Publication No. 2011 / 0207893, U.S. Patent Publication No. 2018 / 0179327, U.S. Patent Publication No. 2017 / 0369646, International Publication No. 2019 / 169500, and U.S. Patent Publication No. 2019 / 0142317, which are incorporated herein by reference.
[0059] SMM compounds may have theoretical molecular weights between 500 Da and 20 kDa. Non-limiting examples of SMMs include those with theoretical molecular weights of 500-10,000 Da, 500-9,000 Da, 500-5,000 Da, 1,000-10,000 Da, 1,000-6,000 Da, or 1,500-8,000 Da. Those skilled in the art will recognize that these structural formulas represent idealized theoretical structures. Specifically, the reaction of segments at specific stoichiometric ratios provides oligofluorinated additives as a distribution of molecules having segments in various ratios. Therefore, the variable n in formulas (I), (II), (III), (IV), (V), and (VI) represents the theoretical stoichiometry of the segments.
[0060] Methods for preparing suitable SMM compounds are recognizable to those skilled in the art without excessive experimentation.
[0061] Base polymer Typical base polymers used in combination with the aforementioned SMM according to the present invention include polyurethane (PU), silicone, polyamide (PA), polyester, copolyester, polyether, polyether block amide copolymer (PEBA), polyetherimide, polycarbonate, polyether ether ketone (PEEK), ethyl vinyl acetate (EVA), polypropylene (PP), polyethylene (PE), polyvinyl chloride (PVC), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), and polyacrylamide (PAAM). Examples include polyethylene oxide (PEO), poly(ethylene oxide)-b-poly(propylene oxide)-b-poly(ethylene oxide), poly(hydroxyethyl methacrylate) (polyHEMA), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polymethyl methacrylate (PMMA), polysulfone, styrene-based block copolymers, vulcanized rubber, polyolefins, cyclic olefin polymers (COP), cyclic olefin copolymers (COC), cellulose-based polymers, or copolymers or blends thereof.
[0062] The base polymer has a theoretical molecular weight of 20 kDa or more (for example, 50 kDa or more, 75 kDa or more, 100 kDa or more, 150 kDa or more, or 200 kDa or more).
[0063] In further embodiments, the base polymer is a thermoplastic resin.
[0064] The base polymer may contain suitable additives known to those skilled in the art, such as fillers, colorants, pigments, stabilizers, antioxidants, plasticizers, reinforcing agents, impact modifiers, foaming agents, curing agents, flame retardants, antistatic agents, conductive agents, processing aids, antimicrobial agents, preservatives, antibiotics, or other functional additives. Additives may be organic or inorganic in nature. Examples of fillers include radiopaque fillers such as barium sulfate, bismuth subcarbonate, bismuth trioxide, or tungsten. Examples of plasticizers include bis(2-ethylhexyl) phthalate (DEHP), di(2-ethylhexyl) terephthalate (DEHT), or trioctyl trimellitate (TOTM), which are used to plasticize PVC resins. Examples of antimicrobial agents, preservatives, or antibiotics include triclosan, silver sulfadiazine, chlorohexidine, rifampin, or clindamycin.
[0065] In a preferred embodiment, the present invention provides a composition comprising a mixture of a base polymer and a compatible surface-modifying polymer in an amount that enhances surface modification.
[0066] The amount of fluorooligomer / base polymer is 0.05 to 15% w / w, preferably 0.1 to 12% w / w, more preferably 0.5 to 10% w / w, and even more preferably 1 to 5% w / w of fluorooligomer in the base polymer.
[0067] In one embodiment, the oligofluorinated additive is of formula (I), and the base polymer is selected from the group consisting of polyurethane, silicone, and polyether-block-amide copolymer (PEBA).
[0068] In another embodiment, the oligofluorinated additive is of formula (IV), and the base polymer is polyurethane.
[0069] In another embodiment, the oligofluorinated additive of the present invention is compound 8 having the structure shown below. [ka] [The PEG content is 50% by weight, the (x+z):y ratio is approximately 1.38, and the Mn content is approximately 1,900 g / mol.] The oligofluorinated additive significantly reduces the coefficient of friction of the base polymer compared to when it is added to Carbonhane 85A polyurethane.
[0070] device Medical devices requiring low friction characteristics include, in particular, catheters, shunts, surgical cannulas, guidewires, stents, grafts, stent grafts, internal prostheses, angioplasty balloons, insertion sheaths, introducers, stylets, implantable biosensors, contraceptives, breast implants, scaffolds, tympanotomy tubes, ophthalmic equipment, contact lenses, IOLs, corneal implants, endotracheal tubes, tracheostomy tubes, endoscopes, syringes, medical blood or fluid transfer tubes, 3D printed implants, orthopedic implants, prosthetic implants, implantable pacemakers and defibrillator leads, LVAD drivelines, structural cardiac implants, retractors, endoscopes, vena cava filters, instrument valves and manifolds, vascular occlusion devices, and embolization prevention devices. Specifically, catheters include vascular catheters, drainage catheters, neurovascular catheters, infusion catheters, parenteral nutrition catheters, stroke treatment catheters, urinary catheters, peritoneal dialysis catheters, support catheters, diagnostic catheters, atherosclerotic catheters, electrophysiological catheters, microcatheters, angioplasty catheters, mechanical thrombectomy catheters, aspiration catheters, imaging catheters, and delivery catheters.
[0071] Examples of equipment manufacturing methods related to the present invention include, in particular, melting processes such as extrusion and molding, or solution processes such as film casting, solution spinning, electrospinning, dip coating, spray coating, and 3D printing, as well as techniques that are recognized by those skilled in the art without excessive experimentation.
[0072] The migration of SMM to the instrument surface can be confirmed using standard analytical methods such as X-ray photoelectron spectroscopy, and the fluorine content on the surface may be in the range of 1 to 50 atomic percent. The relative hydrophilicity of the modified surface can be determined by water contact angle analysis.
[0073] The coefficient of friction (CoF) can be measured by many different test methods, including the ASTM D1894-14 test, pinch test, meandering path test, and various customized tribological methods. The pinch test is common, especially for testing the lubricity of medical devices such as catheter tubes. In this test, one end of the test item, such as a catheter tube, is connected to a device capable of measuring tensile force. The sample is submerged in the fluid of interest and clamped with a predetermined force between two pads of a given substrate. The sample is then pulled at a predetermined speed, and the force required to move the sample is recorded. The CoF is calculated by dividing the force required to pull the sample by the force applied to the sample by the clamp. Repeated test cycles can be performed consecutively on the same sample to evaluate the durability of surface modifications.
[0074] In a preferred embodiment, the pinch test is performed using a Harland FTS 6000 tester, in which a 15 cm rod or tube sample is mounted on the device, submerged in water at room temperature, and clamped with a constant force of 200 g between silicone friction pads (60A durometer). The sample is then pulled at a constant speed of 1 cm / s over a distance of 10 cm, and the force required to pull the sample is recorded. The dynamic CoF is calculated using the average tensile force divided by the clamping force.
[0075] In another preferred embodiment, the pinch test is repeated on the same sample (e.g., 5 to 25 times) to evaluate the coefficient of friction and the durability of the surface modification.
[0076] Equipment modified with the SMM additive of the present invention may have a surface with improved lubricity, indicated by a reduced CoF compared to the same unmodified surface under dry or wet conditions. In certain embodiments, a reduction of more than 50% in CoF can be achieved in SMM-modified equipment when tested in a pinch test using water or PBS as the conditioning medium, a clamping force of 100-500 g, a silicone or PTFE pad as the clamping substrate, a tensile speed of 1 cm / min, and a travel distance of 10 cm.
[0077] The SMM additive of the present invention can be used to reduce CoF in various resins used to manufacture devices, components, or coatings, including, but not limited to, the aforementioned resins. The additive can be used to reduce CoF in any conceivable device or application where minimizing surface friction is important, particularly in medical devices that can be inserted into or moved within the body. The SMM additive can function to reduce CoF in disposable applications or in applications where the surface may be repeatedly exposed to frictional forces.
[0078] While the present invention has been described in general terms, it can be further understood by referring to specific examples. These examples are provided herein for illustrative purposes only and are not intended to limit the invention unless otherwise stated.
[0079] Examples Example 1: Reduction of the coefficient of friction in a PEBA rod A prototype model of polyether block amide copolymer (PEBA) containing 2-4% by weight of the compound of the present invention was prepared using a small laboratory mixer. Specifically, Arkema PEBAX2533 was dried in a vacuum oven at 65°C for 6 hours. This resin was blended in batches with various compounds of the present invention using a 15 mL twin-screw mixer with a cycle time of 3 minutes (after adding the resin) and a melting temperature of approximately 160°C. The blend was extruded into a rod with a diameter of approximately 3.5 mm by opening the mixing chamber valve and releasing the molten polymer. The resulting rod was rapidly cooled in a water bath and air-dried.
[0080] The coefficient of friction (CoF) of the extruded prototype was measured by a pinch test using a Harland FTS6000 test machine. A 15 cm rod sample was mounted in the machine, submerged in water at room temperature, and clamped with a constant force of 200 g between silicone friction pads (60A durometer). The sample was then pulled at a constant speed of 1 cm / s over a distance of 10 cm, and the force required to pull the sample was recorded. The dynamic CoF was calculated using the average tensile force divided by the clamping force. Five independent samples were tested: an unmodified PEBAX control and prototypes modified with SMM. The average CoF is shown in Figure 1, with error bars representing the standard deviation. Two of the SMM formulations tested, compound 2 and compound 4, were found to reduce the CoF of the PEBA prototype by more than 30% (specifically, 97% and 83%, respectively).
[0081] Example 2: Reduction of the coefficient of friction in polyurethane rods A prototype polyurethane model containing 2% by weight of the compound of the present invention was prepared using the small laboratory kneader described in Example 1. Lubrizol's Carbonthane 3585A was dried in a vacuum oven at 65°C for 4 hours before processing, and a melting temperature of approximately 230°C was used for blending with the polyurethane resin SMM and for extrusion. The resulting prototype rod had a diameter of approximately 3.3 mm.
[0082] The coefficient of friction (CoF) of the extruded prototype was measured by pinch testing using the Harland FTS6000 testing machine described in Example 1. Five independent samples were tested using a clamping force of 510 g, consisting of an unmodified polyurethane control and prototypes modified with SMM. The pinch test was repeated 15 times for each sample to ensure that the reduction was maintained across the repeated test cycles. The average CoF for the five samples and over 15 cycles is shown in Figure 2, with error bars representing the standard deviation. Compound 7, one of the SMM formulations tested, was found to reduce the CoF of the polyurethane prototype by more than 30% (specifically, 61%).
[0083] Example 3: Reduction of the coefficient of friction in a polyurethane rod A prototype polyurethane model containing 2% by weight of the compound of the present invention was prepared using the small laboratory kneader described in Example 1. Lubrizol's Carbonthane 3585A was dried in a vacuum oven at 65°C for 4 hours before processing, and a melting temperature of 230°C was used for blending with the polyurethane resin SMM and for extrusion. The resulting prototype rod had a diameter of approximately 3.3 mm.
[0084] The coefficient of friction (CoF) of the extruded prototype was measured by pinch testing using the Harland FTS6000 testing machine described in Example 1. Five independent samples were tested using a clamping force of 200g, consisting of an unmodified polyurethane control and prototypes modified with SMM. The pinch test was repeated five times for each sample to ensure that the reduction was maintained across the repeated test cycles. The average CoF for the five samples and over the five cycles is shown in Figure 3, with error bars representing the standard deviation.
[0085] All three SMM formulations tested—compound 2, compound 4, and compound 3—were found to reduce the CoF of the polyurethane prototype model by more than 30% (specifically by 88%, 84%, and 54%, respectively).
[0086] Example 4: Reduction of the coefficient of friction in polyurethane catheter tubes First, a polyurethane catheter tube containing 20% barium sulfate, a radiopaque filler, and 2% by weight of Compound 2 of the present invention was manufactured by compounding SMM with Lubrizol's Carbonethane 3595A-B20 resin using an industrial compounding process. Then, both the virgin polyurethane resin and the compounded resin containing SMM were extruded into 10F tubes using an industrial tube extrusion process.
[0087] The coefficient of friction (CoF) of the extruded tube was measured by a pinch test using the Harland FTS6000 test machine described in Example 1. Three independent samples were tested using a clamping force of 200 g: an unmodified polyurethane control tube and an SMM-modified tube. The pinch test was repeated five times for each sample to confirm that the reduction was maintained over the repeated test cycles. The average CoF for the three samples and over the five cycles is shown in Figure 4, with error bars representing the standard deviation. Compound 2, the SMM formulation tested, was found to reduce the CoF of a polyurethane tube containing 20% barium sulfate by 75%.
[0088] Example 5: Reduction of the coefficient of friction in a silicone catheter tube Silicone catheter tubes containing 4% by weight of compound 6, the compound of the present invention, were manufactured by blending SMM with Dow Corning's SilasticQ7-4750 silicone elastomer using a two-roll mill, followed by cold extrusion into 15.5 Fr tubes according to a standard silicone tube extrusion method and curing. Control silicone tubes were manufactured in the same manner, but without the addition of SMM.
[0089] The coefficient of friction of the extruded prototype was measured by a pinch test using the Harland FTS6000 test machine described in Example 1. Five independent samples of unmodified silicone control tubes and SMM-modified tubes were tested using a clamping force of 200g. The pinch test was repeated 25 times for each sample to confirm that the reduction was maintained across the repeated test cycles. The average CoF for the five samples and over 25 cycles is shown in Figure 5, with error bars representing the standard deviation. Compound 6, the SMM formulation tested, was found to reduce the CoF of the silicone tubes by 88%.
[0090] Example 6: Reduction of the coefficient of friction in polyurethane film A polyurethane film containing 2% by weight of Compound 2, the compound of the present invention, was manufactured using a small laboratory mixer and a heat press. Specifically, Lubrizol's Carbonate 3585A was dried in a vacuum oven at 65°C for 4 hours prior to processing, and a melting temperature of approximately 230°C was used for blending with the polyurethane resin SMM and extruding into rod form, as described in Example 1. Subsequently, the rods were aligned in a mold and compression-molded into a 130 × 90 mm, 1 mm thick film using a Carver press (Type 2627-5) operated at a temperature of 210°C and a pressure of 500 psi for 5 minutes. After compression, the mold was rapidly cooled with cold water and the film was immediately peeled off.
[0091] The coefficient of friction (CoF) of the film was measured according to the ASTM D1894 test method. The substrate selected for testing was a 12-inch × 12-inch, 1 / 32-inch thick 60A silicone sheet. Film samples were conditioned at 23°C ± 2°C and 50% ± 10% RH for 40 hours. After the conditioning period, the samples were cut into 64 × 64 mm square test pieces and attached to a sled of known weight (200 g) using double-sided tape. This sled was pulled across the plane of the silicone substrate at a speed of 150 mm / min using an Instron Series 5565 instrument, and the force that initiated the sled's movement (static force) and the force that maintained the movement (kinetic force) were recorded. The tests were performed at room temperature under both dry and wet conditions (water was sprayed onto the substrate before each wet test). The same side of the film was used for both the dry and wet tests. A new silicone substrate sheet was used in each test group. Static coefficient of friction (μ) s The coefficient of kinetic friction (μ) was calculated by dividing the static force by the weight of the sled. k The force was calculated by dividing the average force reading obtained during the uniform sliding of the warp across the surface of the silicone substrate by the force reading.
[0092] Five independent samples of unmodified polyurethane control film and SMM-modified film were tested. The mean CoF is shown in Figure 6, and the error bars represent the standard deviation. Compound 2, the SMM formulation tested, was found to reduce the static CoF on the polyurethane film by 37% and 68% in the dry and wet conditions, respectively, and the dynamic CoF by 35% and 33% in the dry and wet conditions, respectively.
[0093] Example 7: Reduction of the coefficient of friction in PEBA catheter tubes First, PEBA catheter tubes containing 4% by weight of compounds 2 and 4 of the present invention were manufactured by compounding SMM with Evonik's PEBA (Vestamid® ME40) resin using an industrial compounding process. Then, both the virgin PEBA resin and the compounded resin containing SMM were extruded into 8F tubes using a commercially available tube extrusion process.
[0094] The coefficient of friction (CoF) of the extruded tubes was measured by a pinch test using a Harland FTS6000 tester as described in Example 1. Four independent samples of unmodified PEBA control tubes and SMM-modified tubes were tested using a clamping force of 200 g. The pinch test was repeated 25 times for each sample to ensure that the reduction was maintained across the repeated test cycles. The average CoF for the four samples and over 25 cycles is shown in Figure 7, with error bars representing the standard deviation. Compounds 2 and 4, the SMM formulations tested, were found to reduce the CoF of the PEBA tubes by more than 30% (specifically, by 92% and 88%, respectively).
[0095] Example 8: Reduction of the coefficient of friction in a polyamide rod A polyamide prototype containing 6% by weight of compounds 2, 3, and 4 of the present invention was prepared using the small laboratory kneader described in Example 1. Specifically, Vestamid® ML24 from Evonik was dried in a vacuum oven at 80°C for 4 hours before processing, and a melting temperature of approximately 215°C was used for blending with the polyamide resin SMM and for extrusion. The resulting rod prototype had a diameter of approximately 3.5 mm.
[0096] The coefficient of friction (CoF) of the extruded prototype was measured by pinch testing using the Harland FTS6000 testing machine described in Example 1. Five independent samples were tested using a clamping force of 200 g, with an unmodified polyamide control and SMM-modified prototypes. The pinch test was repeated 25 times for each sample to ensure that the reduction was maintained across the repeated test cycles. The average CoF for the five samples and over 25 cycles is shown in Figure 8, with error bars representing the standard deviation.
[0097] All three SMM formulations tested—compound 2, compound 3, and compound 4—were found to reduce the CoF of the polyamide prototype model by more than 30% (specifically by 83%, 77%, and 87%, respectively).
[0098] Example 9: Reduction of the coefficient of friction in a PVC rod A PVC prototype containing 2% by weight of compounds 2 and 4 of the present invention was prepared using the small laboratory mixer described in Example 1. Specifically, 85APVC from Cary Compounds was dried overnight at room temperature in a vacuum oven before processing, and a melting temperature of approximately 160°C was used for blending with the SMM of the PVC resin and for extrusion. The resulting rod prototype had a diameter of approximately 3.6 mm.
[0099] The coefficient of friction (CoF) of the extruded prototype was measured by a pinch test using the Harland FTS6000 test machine described in Example 1. Four independent samples were tested using a clamping force of 200g, consisting of an unmodified PVC control and prototypes modified with SMM. The pinch test was repeated 25 times for each sample to ensure that the reduction was maintained across the repeated test cycles. The average CoF for the four samples and over 25 cycles is shown in Figure 9, with error bars representing the standard deviation.
[0100] Both Compound 2 and Compound 4, the SMM formulations tested, were found to reduce the CoF of the PVC prototype model by more than 30% (specifically by 62% and 87%, respectively).
[0101] Based on the above teachings, it is obvious that numerous modifications and variations of the present invention are possible. Therefore, it should be understood that the present invention may be carried out in ways other than those specifically described herein, within the scope of the appended claims.
[0102] Item 1: Articles, It includes a low-friction surface containing an oligofluorinated additive mixed with a base polymer, The coefficient of friction of the low-friction surface is reduced by at least 30% compared to the surface of the base polymer that does not contain the oligofluorinated additive. Goods.
[0103] Item 2 The article according to Item 1, wherein the coefficient of friction of the low-friction surface is measured by a pinch test.
[0104] Item 3: The article described in Item 1 or 2, wherein the surface is in a hydrated state.
[0105] Item 4: An item that is a medical device and is listed in any one of items 1 through 3.
[0106] Item 5 The article described in Item 4, wherein the medical device is a catheter selected from the group consisting of vascular catheters, drainage catheters, neurovascular catheters, infusion catheters, parenteral nutrition catheters, and urinary catheters.
[0107] Item 6 An article according to any one of items 1 to 5, wherein the low-friction surface is the outer surface.
[0108] Item 7 An article according to any one of items 1 to 5, wherein the low-friction surface is the inner surface.
[0109] Item 8 An article according to any one of items 1 to 7, wherein the low-friction surface is obtained by applying a coating comprising an oligofluorinated additive and a base polymer.
[0110] Article according to any one of items 1 to 8, wherein the base polymer is selected from the group consisting of polyurethane, silicone, polyamide, polyester, copolyester, polyether, polyether-block-amide copolymer, polypropylene, polyethylene, polyvinyl chloride, polysulfone, polyetherimide, polycarbonate, polyetheretherketone, ethyl vinyl acetate, polyolefin, styrene block copolymer, vulcanized rubber, and mixtures thereof.
[0111] Item 10 An article according to any one of items 1 to 8, wherein the base polymer is selected from the group consisting of polyurethane, silicone, polyether block amide copolymer, polyamide, polyvinyl chloride, and mixtures thereof.
[0112] Article according to item 2, wherein the coefficient of friction, as measured by a pinch test, is reduced by at least 50% compared to the base polymer.
[0113] Item 12 An article according to any one of items 1 to 11, wherein the oligofluorinating additive is present in an amount of 0.05 to 15% by weight relative to the base polymer.
[0114] Item 13 The oligofluorinated additive is of formula (I): F T -[BA] n -BF T (I) [In the formula, (i) A includes polypropylene oxide, polyethylene oxide, polytetramethylene oxide, hydrogenated polybutadiene, polybutadiene, hydrogenated polyisoprene, poly(diethylene glycol) adipate, diethylene glycol-orthophthalic anhydride) polyester, (neopentyl glycol-orthophthalic anhydride) polyester, (1,6-hexanediol-orthophthalic anhydride) polyester, poly(hexamethylene carbonate), poly((2,2-dimethyl)-1,3-propylene carbonate), polycarbonate polyol, poly(ethylene-co-butylene), polystyrene, polysiloxane, polydimethylsiloxane, polypropylene glycol-polyethylene glycol block copolymer, polysiloxane-polyethylene glycol block copolymer, polysiloxane-polypropylene glycol block copolymer, or other block copolymers containing block segments selected from the group of polypropylene oxide, polyethylene oxide, polytetramethylene oxide, polysiloxane, and polydimethylsiloxane; (ii) B is a segment containing urethane; (iii)F T It is a polyfluoroorgano group; (iv) n is an integer between 1 and 10. An item that conforms to any one of the items listed in items 1 through 12.
[0115] Item 14 The article according to Item 13, wherein the base polymer is selected from the group consisting of polyurethane, silicone, polyether block amide copolymer, polyamide, polyvinyl chloride, and mixtures thereof.
[0116] Item 15 The oligofluorinated additive is of formula (II) or formula (III): [ka] [In the formula, (i) A is an oligomer segment containing ether bonds, ester bonds, carbonate bonds, and polyalkylene, and A is polypropylene oxide, polyethylene oxide, polytetramethylene oxide, hydrogenated polybutadiene, polybutadiene, hydrogenated polyisoprene, poly(diethylene glycol) adipate, (diethylene glycol-orthophthalic anhydride) polyester, (neopentyl glycol-orthophthalic anhydride) polyester, (1,6-hexanediol-orthophthalic anhydride) polyester, poly(hexamethylene carbonate), poly((2,2-dimethyl)-1 Includes other block copolymers containing block segments selected from the group consisting of polypropylene oxide, polyethylene oxide, polytetramethylene oxide, polysiloxane, and polydimethylsiloxane; (ii) B is a segment containing an isocyanurate trimer or a biuret trimer, and B' is a segment containing urethane, if present; (iii) Each F T It is a polyfluoroorgano group; (iv) n is an integer between 0 and 10. An item that conforms to any one of the items listed in items 1 through 12.
[0117] Item 16 The oligofluorinated additive is of formula (IV): [ka] [In the formula, (i)Each F T These are, independently, surfactant groups selected from polydimethylsiloxanes, hydrocarbons, and polyfluoroorgano groups; (ii) X1 is H, CH3, or CH2CH3; (iii) Each of X2 and X3 is independently H, CH3, CH2CH3, or F T and; (iv) Each of L1 and L2 is independently a bond, an oligomeric linking group, or a linking group having two terminal carbonyls; (v)n is an integer between 5 and 50. An item that conforms to any one of the items listed in items 1 through 12.
[0118] Item 17 The article according to Item 16, wherein the base polymer is selected from the group consisting of polyurethane, silicone, polyether block amide copolymer, polyamide, polyvinyl chloride, and mixtures thereof.
[0119] Item 18 A method for reducing the coefficient of friction of a surface, A method comprising applying a mixture of an oligofluorinated additive and a base polymer to a surface requiring it.
[0120] Item 19 The method according to Item 18, wherein the mixture contains 0.05 to 15% by weight of the oligofluorinating additive relative to the base polymer.
[0121] Item 20 A method for manufacturing a medical device having a reduced coefficient of friction, comprising extruding, molding, or coating a composition containing an oligofluorinated additive and a base polymer.
[0122] Item 21 Use of an oligofluorinated additive to reduce the coefficient of friction of a polymer article or layer by at least 30% compared to the coefficient of friction of the polymer article or layer without the oligofluorinated additive, wherein the oligofluorinated additive is mixed with the base polymer of the polymer article or layer.
Claims
1. An article, a low friction surface comprising an oligofluorinated additive mixed with a base polymer; The coefficient of friction of the low friction surface is reduced by at least 30% compared to a surface of the base polymer without the oligofluorinated additive. Goods.
2. The article of claim 1 , wherein the coefficient of friction of the low friction surface is measured by a pinch test.
3. The article of claim 1 or 2, wherein the surface is in a hydrated state.
4. 3. The article of claim 1 or 2 which is a medical device.
5. 5. The article of claim 4, wherein the medical device is a catheter selected from the group consisting of a vascular catheter, a drainage catheter, a neurovascular catheter, an infusion catheter, a parenteral nutrition catheter, and a urological catheter.
6. The article of claim 1 or 2, wherein the low friction surface is an exterior surface.
7. The article of claim 1 or 2, wherein the low friction surface is an interior surface.
8. 3. The article of claim 1 or 2, wherein the low friction surface is obtained by applying a coating comprising an oligofluorinated additive and a base polymer.
9. 3. The article of claim 1 or 2, wherein the base polymer is selected from the group consisting of polyurethane, silicone, polyamide, polyester, copolyester, polyether, polyether-block-amide copolymer, polypropylene, polyethylene, polyvinyl chloride, polysulfone, polyetherimide, polycarbonate, polyetheretherketone, ethylvinylacetate, polyolefin, styrene block copolymer, vulcanized rubber, and mixtures thereof.
10. The article of claim 1 or 2, wherein the base polymer is selected from the group consisting of polyurethane, silicone, polyether block amide copolymer, polyamide, polyvinyl chloride, and mixtures thereof.
11. 3. The article of claim 2, wherein the coefficient of friction as measured by a pinch test is reduced by at least 50% of the base polymer.
12. The article of claim 1 or 2, wherein the oligofluorinated additive is present in an amount of 0.05 to 15% by weight relative to the base polymer.
13. The oligofluorinated additive has the formula (I): F T -[B-A] n -B-F T (I) [In the formula, (i) A comprises polypropylene oxide, polyethylene oxide, polytetramethylene oxide, hydrogenated polybutadiene, polybutadiene, hydrogenated polyisoprene, poly(diethylene glycol) adipate, (diethylene glycol-orthophthalic anhydride) polyester, (neopentyl glycol-orthophthalic anhydride) polyester, (1,6-hexanediol-orthophthalic anhydride) polyester, poly(hexamethylene carbonate), poly((2,2-dimethyl)-1,3-propylene carbonate), polycarbonate polyol, poly(ethylene-co-butylene), polystyrene, polysiloxane, polydimethylsiloxane, polypropylene glycol-polyethylene glycol block copolymer, polysiloxane-polyethylene glycol block copolymer, polysiloxane-polypropylene glycol block copolymer, or other block copolymer comprising block segments selected from the group of polypropylene oxide, polyethylene oxide, polytetramethylene oxide, polysiloxane, and polydimethylsiloxane; (ii) B is a urethane-containing segment; (iii) F T is a polyfluoroorgano group; (iv) n is an integer from 1 to 10.
3. The article of claim 1 or 2 according to
14. 14. The article of claim 13, wherein the base polymer is selected from the group consisting of polyurethane, silicone, polyether block amide copolymer, polyamide, polyvinyl chloride, and mixtures thereof.
15. The oligofluorinated additive has formula (II) or formula (III): 【Chemistry 1】 [In the formula, (i) A is an oligomer segment containing an ether bond, an ester bond, a carbonate bond, and a polyalkylene, and A is selected from the group consisting of polypropylene oxide, polyethylene oxide, polytetramethylene oxide, hydrogenated polybutadiene, polybutadiene, hydrogenated polyisoprene, poly(diethylene glycol) adipate, (diethylene glycol-orthophthalic anhydride) polyester, (neopentyl glycol-orthophthalic anhydride) polyester, (1,6-hexanediol-orthophthalic anhydride) polyester, poly(hexamethylene carbonate), poly((2,2-dimethyl)-1 ,3-propylene carbonate), polycarbonate polyols, poly(ethylene-co-butylene), polystyrene, polysiloxane, polydimethylsiloxane, polypropylene glycol-polyethylene glycol block copolymers, polysiloxane-polyethylene glycol block copolymers, polysiloxane-polypropylene glycol block copolymers, or other block copolymers comprising block segments selected from the group of polypropylene oxide, polyethylene oxide, polytetramethylene oxide, polysiloxane, and polydimethylsiloxane; (ii) B is an isocyanurate trimer or biuret trimer containing segment, and B′, when present, is a urethane containing segment; (iii) Each F T is a polyfluoroorgano group; (iv) n is an integer from 0 to 10.
3. The article of claim 1 or 2 according to
16. The oligofluorinated additive has the formula (IV): 【Chemistry 2】 [In the formula, (i) Each F T is independently a surface active group selected from polydimethylsiloxane, hydrocarbon, and polyfluoroorgano groups; (ii) X 1 is H, CH 3 , or C.H. 2 CH 3 and (iii) X 2 and X 3 each independently represents H, CH 3 , C.H. 2 CH 3 , or F T and (iv) L 1 and L 2 each is independently a bond, an oligomeric linking group, or a linking group having two terminal carbonyls; (v) n is an integer from 5 to 50.
3. The article of claim 1 or 2 according to
17. 17. The article of claim 16, wherein the base polymer is selected from the group consisting of polyurethane, silicone, polyether block amide copolymer, polyamide, polyvinyl chloride, and mixtures thereof.
18. 1. A method for reducing the coefficient of friction of a surface, comprising the steps of: A method comprising applying a mixture of an oligofluorinated additive and a base polymer to a surface in need thereof.
19. The method of claim 18, wherein the mixture contains 0.05 to 15 weight percent of the oligofluorinated additive relative to the base polymer.
20. A method of producing a medical device having a reduced coefficient of friction, comprising extruding, molding, or coating a composition containing an oligofluorinated additive and a base polymer.