Coloring composition, film, color filter, solid-state imaging device, and image display device

A coloring composition with a protected phenolic antioxidant compound addresses spectral fluctuations and color unevenness in color filters by using a high content of organic pigments and controlled antioxidant release, ensuring stable color performance under heat.

JP7574295B2Active Publication Date: 2024-10-28FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022534012
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-02
Filing Date
2021-06-29
Publication Date
2024-10-28
Estimated Expiration
2041-06-29

AI Technical Summary

Technical Problem

Existing colored compositions using organic pigments in color filters exhibit significant spectral fluctuations and color unevenness after long-term heat treatment, particularly with increased content of coloring materials.

Method used

A coloring composition containing an organic pigment, resin, and a compound with a protected phenolic hydroxy group that is removable by heating, with a specific compound represented by formula (AO-1), ensuring a high content of coloring material and controlled release of phenolic hydroxyl groups as antioxidants during film formation.

Benefits of technology

The composition achieves films with reduced spectral fluctuations and suppressed color unevenness even after long-term heat treatment, maintaining color stability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574295000001
    Figure 0007574295000001
  • Figure 0007574295000002
    Figure 0007574295000002
  • Figure 0007574295000003
    Figure 0007574295000003
Patent Text Reader

Abstract

This coloring composition contains: a coloring material including an organic pigment; a resin; and a compound A protected with a protecting group that is capable of detaching, through application of heat, a phenolic hydroxy group of a phenol-based antioxidant. In the total solid content of the coloring composition, the coloring material is contained in an amount of 40 mass% or more. This film is obtained by using said coloring composition. This color filter, this solid-state imaging element, and this image display device include said film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coloring composition containing an organic pigment. The present invention also relates to a film, a color filter, a solid-state imaging device, and an image display device using the coloring composition. [Background technology]

[0002] In recent years, the demand for solid-state imaging elements such as charge-coupled device (CCD) image sensors has increased significantly due to the popularity of digital cameras and mobile phones with cameras. Color filters are used as key devices in displays and optical elements. Color filters usually have pixels of the three primary colors, red, green, and blue, and play the role of separating transmitted light into the three primary colors.

[0003] The colored pixels of each color of the color filter are produced using a coloring composition containing a coloring material such as a pigment.

[0004] Furthermore, Patent Document 1 describes an invention relating to a colored composition containing a latent antioxidant (A) and a colorant (B). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2015-131937 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present inventors have conducted extensive research into films obtained using coloring compositions containing organic pigments, and have found that there is room for further improvement in the spectral variation and color unevenness of the film after long-term heat treatment (e.g., heat treatment at 130° C. for 1000 hours). In particular, the greater the content of the coloring material in the film, the greater the tendency for the spectral variation and color unevenness of the film after long-term heat resistance testing to become.

[0007] Therefore, an object of the present invention is to provide a coloring composition, a film, a color filter, a solid-state imaging element, and an image display device that can provide a film that exhibits small spectral fluctuations and suppresses the occurrence of color unevenness even after long-term heat treatment. [Means for solving the problem]

[0008] According to the present inventors' investigations, it was found that the above object can be achieved by a coloring composition described below, and thus the present invention has been completed. <1> A coloring composition comprising a coloring material containing an organic pigment, a resin, and a compound A in which a phenolic hydroxy group of a phenolic antioxidant is protected with a protecting group that can be removed by heating, A coloring composition comprising the coloring material in an amount of 40% by mass or more based on the total solid content of the coloring composition. <2> The coloring composition contains the compound A in an amount of 1 to 10% by mass based on the total solid content of the coloring composition. <1> The coloring composition according to claim 1. <3> The compound A is contained in an amount of 2 to 25 parts by mass relative to 100 parts by mass of the organic pigment. <1> or <2> The coloring composition according to claim 1. <4> A coloring composition comprising a colorant containing an organic pigment, a resin, and a compound represented by formula (AO-1), a coloring composition comprising the coloring material in an amount of 40 mass% or more based on the total solid content of the coloring composition; [ka] In the formula, R 1 represents a substituent, R 2 -COOR 11 , -CH2-CH=CR 12 R 13 , -CH2(-OL R1 ) q -OR 14 or SiR 15 R 16 R 17 represents R 11 , R 14 , R 15 , R 16 and R 17each independently represents an alkyl group, R 12 and R 13 each independently represents a hydrogen atom or an alkyl group, L R1 represents an alkylene group, q represents 0 or 1, If q is 1, L R1 and R 14 may be bonded to form a ring, m represents an integer of 0 to 4; n represents an integer from 1 to 10; X 1 represents a group having a valence of n. <5> The coloring composition contains the compound represented by formula (AO-1) in an amount of 1 to 10% by mass based on the total solid content of the coloring composition. <4> The coloring composition according to claim 1. <6> The composition contains 2 to 25 parts by mass of the compound represented by the formula (AO-1) relative to 100 parts by mass of the organic pigment. <4> or <5> The coloring composition according to claim 1. <7> The organic pigment includes at least one selected from a green pigment, a yellow pigment, and a red pigment. <1> ~ <6> 13. The coloring composition according to claim 12, <8> The organic pigment comprises a green pigment, and the green pigment comprises a phthalocyanine compound. <1> ~ <6> 13. The coloring composition according to claim 12, <9> The resin includes a graft resin having an acid group. <1> ~ <8> 13. The coloring composition according to claim 12, <10> The acid value of the graft resin is 20 to 150 mgKOH / g. <9> The coloring composition according to claim 1. <11> The weight average molecular weight of the graft resin is 3,000 to 35,000. <9> or <10> The coloring composition according to claim 1. <12> Further, the composition contains a photopolymerization initiator and a polymerizable compound. <1> ~ <11> 13. The coloring composition according to claim 12, <13> The photopolymerization initiator includes an oxime compound having an aromatic ring group in which an electron-withdrawing group is introduced into the aromatic ring. <12> The coloring composition according to claim 1. <14> Further containing a phenolic antioxidant, <1> ~ <13> 13. The coloring composition according to claim 12, <15> <1> ~ <14> A film obtained by using the coloring composition according to any one of the above items. <16> <15> A color filter comprising the film according to claim 1. <17> <15> A solid-state imaging device comprising the film according to claim 1. <18> <15> An image display device comprising the film according to claim 1. Effect of the Invention

[0009] According to the present invention, it is possible to provide a coloring composition, a film, a color filter, a solid-state imaging device, and an image display device which are capable of obtaining a film in which spectral fluctuation is small even after a long-term heat treatment and the occurrence of color unevenness is suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. In this specification, the symbol "to" is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit. In the description of groups (atomic groups) in this specification, when there is no indication of substitution or non-substitution, the notation includes both groups (atomic groups) that have no substituents and groups (atomic groups) that have a substituent. For example, an "alkyl group" includes not only an alkyl group that has no substituents (unsubstituted alkyl group) but also an alkyl group that has a substituent (substituted alkyl group). In this specification, unless otherwise specified, "exposure" includes not only exposure using light but also drawing using particle beams such as electron beams and ion beams. Examples of light used for exposure include the bright line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light (EUV light), X-rays, active rays or radiation such as electron beams. In this specification, "(meth)acrylate" refers to both or either of acrylate and methacrylate, "(meth)acryl" refers to both or either of acryl and methacryl, and "(meth)acryloyl" refers to both or either of acryloyl and methacryloyl. In this specification, Me in the structural formulae represents a methyl group, Et represents an ethyl group, Bu represents a butyl group, and Ph represents a phenyl group. In this specification, the weight average molecular weight and number average molecular weight are values ​​calculated as polystyrene standards measured by GPC (gel permeation chromatography). In this specification, the total solids content refers to the total mass of all components of the composition excluding the solvent. In this specification, the term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes, as long as the intended effect of the process is achieved.

[0011] <Coloring composition> A first aspect of the coloring composition of the present invention is a coloring composition comprising a coloring material containing an organic pigment, a resin, and a compound A in which a phenolic hydroxy group of a phenolic antioxidant is protected with a protecting group that can be removed by heating, and is characterized in that the coloring material is contained in an amount of 40 mass% or more of the total solid content of the coloring composition. A second aspect of the coloring composition of the present invention is a coloring composition comprising a coloring material containing an organic pigment, a resin, and a compound represented by formula (AO-1), and is characterized in that the coloring material is contained in an amount of 40 mass% or more of the total solid content of the coloring composition. Hereinafter, the above-mentioned compound A and the compound represented by formula (AO-1) will be collectively referred to as a specific compound.

[0012] Although the coloring composition of the present invention contains 40% by mass or more of a coloring material containing an organic pigment in the total solid content of the coloring composition, by containing the above-mentioned specific compound, it is possible to form a film with small spectral fluctuation and suppressed color unevenness even after a long-term heat treatment. Although the detailed reason why such an effect is obtained is unknown, it is presumed to be due to the following.

[0013] It is speculated that the specific compound contained in the coloring composition of the present invention has a protective group removed during film formation (e.g., during post-baking) to generate a phenolic hydroxyl group, thereby exerting a function as an antioxidant. It is speculated that the action of the component functioning as an antioxidant generated from the specific compound can suppress the deterioration and aggregation of organic pigments at high temperatures. Therefore, it is speculated that the coloring composition of the present invention can form a film with small spectral fluctuation and suppressed color unevenness even after long-term heat treatment.

[0014] In addition, when forming a film using a coloring composition containing an antioxidant, the antioxidant may decompose or denature due to heating or exposure during film formation, and a sufficient amount of antioxidant may not remain in the film.In contrast, the above-mentioned specific compound is a compound that exhibits its function as an antioxidant by eliminating a protective group during film formation to generate a phenolic hydroxyl group, so that even if the content of the specific compound is small, a sufficient amount of components that function as an antioxidant can be contained in the film.Therefore, the coloring composition of the present invention can also increase the degree of freedom in formulation design.

[0015] The coloring composition of the present invention is preferably used as a coloring composition for color filters. Specifically, it can be preferably used as a coloring composition for forming color pixels of a color filter. Examples of the color pixels include red pixels, green pixels, blue pixels, magenta pixels, cyan pixels, and yellow pixels, and green pixels or cyan pixels are preferable. In addition, the coloring composition of the present invention can be preferably used as a coloring composition for a solid-state imaging device, and more preferably used as a coloring composition for forming color pixels of a color filter used in a solid-state imaging device.

[0016] Hereinafter, each component used in the colored composition of the present invention will be described.

[0017] <<Coloring materials>> The coloring composition of the present invention contains a coloring material. The coloring material contained in the coloring composition of the present invention contains an organic pigment. In this specification, the organic pigment means a pigment composed of an organic compound. In this specification, the pigment means a coloring material that is difficult to dissolve in a solvent. The solubility of the pigment in both 100 g of water at 23° C. and 100 g of propylene glycol monomethyl ether acetate at 23° C. is preferably 0.1 g or less, more preferably 0.01 g or less.

[0018] The average primary particle diameter of the organic pigment is preferably 1 to 200 nm. The lower limit is preferably 5 nm or more, more preferably 10 nm or more. The upper limit is preferably 180 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less. If the average primary particle diameter of the organic pigment is within the above range, the dispersion stability of the organic pigment in the coloring composition is good. In the present invention, the primary particle diameter of the organic pigment can be obtained by observing the primary particles of the organic pigment with a transmission electron microscope and obtaining an image photograph. Specifically, the projected area of ​​the primary particles of the pigment is obtained, and the corresponding circle equivalent diameter is calculated as the primary particle diameter of the pigment. In addition, the average primary particle diameter in the present invention is the arithmetic average value of the primary particle diameters of 400 primary particles of the pigment. In addition, the primary particles of the pigment refer to independent particles without aggregation.

[0019] The organic pigment is preferably a chromatic organic pigment. Examples of the chromatic organic pigment include a yellow pigment, an orange pigment, a red pigment, a green pigment, a purple pigment, and a blue pigment. The organic pigment used in the present invention preferably contains at least one selected from a green pigment, a yellow pigment, and a red pigment, and more preferably contains a green pigment.

[0020] Examples of green pigments include phthalocyanine compounds and squarylium compounds. Here, phthalocyanine compounds (also called phthalocyanine green pigments) as green pigments tend to be easily thermally diffused in a film, and the phthalocyanine green pigments tend to aggregate in the film after heating, causing the spectral characteristics of the film after heating to fluctuate and color unevenness to occur. However, according to the coloring composition of the present invention, even when a phthalocyanine green pigment is used, the fluctuation of spectral characteristics and the occurrence of color unevenness can be effectively suppressed. Therefore, when a phthalocyanine compound (phthalocyanine green pigment) is used as a green pigment, a particularly remarkable effect can be obtained.

[0021] The phthalocyanine green pigment may be a phthalocyanine compound having Cu, Al, Co, Ni, Ti or Zn as a central metal. Since the effect of the present invention is more pronounced, the phthalocyanine green pigment is more preferably a phthalocyanine compound having Cu, Zn or Al as a central metal, and even more preferably a phthalocyanine compound having Cu or Zn as a central metal. The central metal may further be coordinated with a ligand. The phthalocyanine compound is preferably a halogenated phthalocyanine compound. Here, the halogenated phthalocyanine compound refers to a phthalocyanine compound having a halogen atom as a substituent.

[0022] Specific examples of green pigments include Color Index (CI) Pigment Green 7, 10, 36, 37, 58, 59, 62, 63, 64, 65, and 66. In addition, as a green pigment, a halogenated zinc phthalocyanine pigment having an average number of halogen atoms in one molecule of 10 to 14, an average number of bromine atoms of 8 to 12, and an average number of chlorine atoms of 2 to 5 can also be used. Specific examples include the phthalocyanine pigments described in International Publication No. 2015 / 118720. In addition, as green pigments, compounds described in Chinese Patent Application No. 106909027, phthalocyanine compounds having a phosphate ester as a ligand described in International Publication No. 2012 / 102395, phthalocyanine compounds described in JP-A-2019-008014, phthalocyanine compounds described in JP-A-2018-180023, compounds described in JP-A-2019-038958, and the like can also be used.

[0023] As green pigments, CI Pigment Green 7, 36, 58, 59, 62, and 63 are preferred.

[0024] Examples of yellow pigments include azo compounds, azomethine compounds, quinophthalone compounds, isoindolinone compounds, isoindoline compounds, pteridine compounds, and anthraquinone compounds.

[0025] Specific examples of yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 11, 12, 13, 14, 15, 16, 17, 18, 20, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 86, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 1 20, 123, 125, 126, 127, 128, 129, 137, 138, 139, 147, 148, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 193, 194, 199, 213, 214, 215, 228, 231, 232, 233, 234, 235, 236, etc.

[0026] Furthermore, as the yellow pigment, an azobarbituric acid nickel complex having the following structure can also be used. [ka]

[0027] In addition, as yellow pigments, quinophthalone compounds described in paragraphs 0011 to 0034 of JP 2013-054339 A, quinophthalone compounds described in paragraphs 0013 to 0058 of JP 2014-026228 A, isoindoline compounds described in JP 2018-062644 A, quinophthalone compounds described in JP 2018-203798 A, quinophthalone compounds described in JP 2018-062578 A, quinophthalone compounds described in Japanese Patent No. 6432076, quinophthalone compounds described in JP 2018-155881 A, Quinophthalone compounds described in JP 2018-111757 A, JP 2018-040835 A, JP 2017-197640 A, JP 2016-145282 A, JP 2014-085565 A, JP 2014-021139 A, JP 2013-209614 A, JP 2013-209435 A, JP 2013-18 1015, quinophthalone compounds described in JP 2013-061622 A, quinophthalone compounds described in JP 2013-032486 A, quinophthalone compounds described in JP 2012-226110 A, quinophthalone compounds described in JP 2008-074987 A, quinophthalone compounds described in JP 2008-081565 A, quinophthalone compounds described in JP 2008-074986 A, quinophthalone compounds described in JP 2008-074985 A, quinophthalone compounds described in JP 2008-050420 A Quinophthalone compounds described in JP-A-2008-031281, JP-B-48-032765, JP-A-2019-008014, JP-A-6607427, JP-A-2020-033525, JP-A-2020-033524, JP-A-2020-033523, JP-A-2020-033522, JP-A-2020-033521,Compounds described in WO 2020 / 045200, WO 2020 / 045199, and WO 2020 / 045197 can also be used. Polymerized versions of these compounds are also preferably used from the viewpoint of improving color value.

[0028] Furthermore, as the yellow pigment, a compound represented by the following formula (QP1) and a compound represented by the following formula (QP2) can also be used. [ka]

[0029] In formula (QP1), X 1 ~X 16 each independently represents a hydrogen atom or a halogen atom; Z 1 represents an alkylene group having 1 to 3 carbon atoms. Specific examples of the compound represented by formula (QP1) include the compounds described in paragraph 0016 of Japanese Patent No. 6443711. [ka]

[0030] In formula (QP2), Y 1 ~Y 3 each independently represents a halogen atom. n and m represent integers of 0 to 6, and p represents an integer of 0 to 5. (n+m) is 1 or more. Specific examples of the compound represented by formula (QP2) include the compounds described in paragraphs 0047 to 0048 of Japanese Patent No. 6432077.

[0031] As the yellow pigment, CI Pigment Yellow 129, 138, 139, 150, 185, and 215 are preferable, and CI Pigment Yellow 139, 150, and 185 are more preferable.

[0032] Examples of red pigments include diketopyrrolopyrrole compounds, anthraquinone compounds, azo compounds, naphthol compounds, azomethine compounds, xanthene compounds, quinacridone compounds, perylene compounds, and thioindigo compounds.

[0033] Examples of red pigments include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 9, 10, 14, 17, 22, 23, 31, 38, 41, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 52:1, 52:2, 53:1, 57:1, 60:1, 63:1, 66, 67, 81:1, 81:2, 81:3, 83, 88, 90, 105, 112, 119, 122, 123, 144, and 146. , 149, 150, 155, 166, 168, 169, 170, 171, 172, 175, 176, 177, 178, 179, 184, 185, 187, 188, 190, 200, 202, 206, 207, 208, 209, 210, 216, 220, 224, 226, 242, 246, 254, 255, 264, 269, 270, 272, 279, 291, 294, 295, 296, 297, etc. In addition, as the red pigment, a diketopyrrolopyrrole compound in which at least one bromine atom is substituted in the structure described in JP 2017-201384 A, a diketopyrrolopyrrole compound described in paragraphs 0016 to 0022 of Japanese Patent No. 6248838 A, a diketopyrrolopyrrole compound described in WO 2012 / 102399 A, a diketopyrrolopyrrole compound described in WO 2012 / 117965 A, a naphthol azo compound described in JP 2012-229344 A, a red pigment described in Japanese Patent No. 6516119 A, a red pigment described in Japanese Patent No. 6525101 A, etc. can also be used. In addition, as the red pigment, a compound having a structure in which an aromatic ring group in which a group in which an oxygen atom, a sulfur atom or a nitrogen atom is bonded to an aromatic ring is introduced and bonded to a diketopyrrolopyrrole skeleton can also be used.

[0034] Examples of orange pigments include CI Pigment Orange 2, 5, 13, 16, 17:1, 31, 34, 36, 38, 43, 46, 48, 49, 51, 52, 55, 59, 60, 61, 62, 64, 71, and 73.

[0035] Examples of purple pigments include CI Pigment Violet 1, 19, 23, 27, 32, 37, 42, 60, and 61.

[0036] Examples of blue pigments include CI Pigment Blue 1, 2, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 29, 60, 64, 66, 79, 80, 87, and 88.

[0037] For the diffraction angles that various pigments preferably have, the descriptions in Japanese Patent No. 6561862, Japanese Patent No. 6413872, Japanese Patent No. 6281345, Japanese Patent Publication No. 2020-026503, and Japanese Patent Publication No. 2020-033526 can be referred to, the contents of which are incorporated herein by reference.

[0038] Two or more kinds of chromatic organic pigments may be used in combination. For example, when the coloring composition of the present invention is used for forming green pixels of a color filter, it is preferable to use a green pigment and a yellow pigment in combination. The ratio of the green pigment to the yellow pigment is preferably 10 to 120 parts by mass, more preferably 20 to 100 parts by mass, and even more preferably 25 to 75 parts by mass, per 100 parts by mass of the green pigment.

[0039] In addition to the organic pigment, a dye may also be used as the coloring material used in the coloring composition of the present invention. There is no particular limitation on the dye, and a known dye may be used. For example, pyrazole azo compounds, anilino azo compounds, triarylmethane compounds, anthraquinone compounds, anthrapyridone compounds, benzylidene compounds, oxonol compounds, pyrazolotriazole azo compounds, pyridone azo compounds, cyanine compounds, phenothiazine compounds, pyrrolopyrazole azomethine compounds, xanthene compounds, phthalocyanine compounds, benzopyran compounds, indigo compounds, and pyrromethene compounds may be used. In addition, thiazole compounds described in JP-A-2012-158649, azo compounds described in JP-A-2011-184493, and azo compounds described in JP-A-2011-145540 may also be used. In addition, a dye multimer may also be used as the dye. The dye multimer has two or more dye structures in one molecule, and preferably has three or more dye structures. The upper limit is not particularly limited, but may be 100 or less. The multiple dye structures in one molecule may be the same dye structure or different dye structures. The weight average molecular weight (Mw) of the dye multimer is preferably 2000 to 50000. The lower limit is more preferably 3000 or more, and even more preferably 6000 or more. The upper limit is more preferably 30000 or less, and even more preferably 20000 or less. As the dye multimer, compounds described in JP2011-213925A, JP2013-041097A, JP2015-028144A, JP2015-030742A, JP2016-102191A, WO2016 / 031442, etc. may also be used.

[0040] The content of the coloring material in the total solid content of the coloring composition is 40% by mass or more, preferably 45% by mass or more, and more preferably 50% by mass or more. The upper limit of the content of the coloring material in the total solid content of the coloring composition is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. The content of the organic pigment in the total solid content of the coloring composition is preferably 20% by mass or more, more preferably 40% by mass or more, even more preferably 45% by mass or more, and particularly preferably 45% by mass or more. The upper limit of the content of the organic pigment in the total solid content of the coloring composition is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. The content of the organic pigment in the coloring material is preferably 50% by mass or more, more preferably 75% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more. The upper limit may be 100% by mass or less.

[0041] <<Resin>> The coloring composition of the present invention contains a resin. The resin is blended, for example, for dispersing a pigment in the coloring composition or for use as a binder. A resin used mainly for dispersing a pigment is also called a dispersant. However, such uses of the resin are merely examples, and the resin can also be used for purposes other than these uses.

[0042] The weight average molecular weight (Mw) of the resin is preferably 3,000 to 2,000,000. The upper limit is preferably 1,000,000 or less, and more preferably 500,000 or less. The lower limit is preferably 4,000 or more, and more preferably 5,000 or more.

[0043] Examples of the resin include (meth)acrylic resin, enethiol resin, polycarbonate resin, polyether resin, polyarylate resin, polysulfone resin, polyethersulfone resin, polyphenylene resin, polyarylene ether phosphine oxide resin, polyimide resin, polyamideimide resin, polyimine resin, polyolefin resin, cyclic olefin resin, polyester resin, and styrene resin. One of these resins may be used alone, or two or more may be mixed and used. In addition, the resins described in paragraphs 0041 to 0060 of JP-A-2017-206689 and the resins described in paragraphs 0022 to 0071 of JP-A-2018-010856 may also be used.

[0044] In the present invention, it is preferable to use a resin having an acid group as the resin. Examples of the acid group include a carboxyl group, a phosphoric acid group, a sulfo group, and a phenolic hydroxyl group, and the carboxyl group is preferable. The resin having an acid group can be used as, for example, an alkali-soluble resin.

[0045] The resin having an acid group preferably contains a repeating unit having an acid group on a side chain, and more preferably contains 5 to 70 mol % of the repeating units having an acid group on a side chain in all repeating units of the resin. The upper limit of the content of the repeating units having an acid group on a side chain is preferably 50 mol % or less, and more preferably 30 mol % or less. The lower limit of the content of the repeating units having an acid group on a side chain is preferably 10 mol % or more, and more preferably 20 mol % or more.

[0046] It is also preferable that the resin having an acid group contains a repeating unit derived from a monomer component including a compound represented by the following formula (ED1) and / or a compound represented by the following formula (ED2) (hereinafter, these compounds may be referred to as "ether dimers").

[0047] [ka]

[0048] In formula (ED1), R 1 and R 2 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 25 carbon atoms which may have a substituent. [ka] In formula (ED2), R represents a hydrogen atom or an organic group having a carbon number of 1 to 30. For details of formula (ED2), the disclosure of JP-A-2010-168539 can be referred to, the contents of which are incorporated herein by reference.

[0049] Specific examples of ether dimers can be found in, for example, paragraph 0317 of JP2013-029760A, the contents of which are incorporated herein by reference.

[0050] It is also preferable that the resin used in the present invention contains a repeating unit derived from a compound represented by the following formula (X). [ka] In formula (X), R1 represents a hydrogen atom or a methyl group, R2 represents an alkylene group having 2 to 10 carbon atoms, R3 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms which may contain a benzene ring, and n represents an integer of 1 to 15.

[0051] For the resin having an acid group, the description in paragraphs 0558 to 0571 of JP 2012-208494 A (corresponding to paragraphs 0685 to 0700 of U.S. Patent Application Publication No. 2012 / 0235099 A) and the description in paragraphs 0076 to 0099 of JP 2012-198408 A can be referred to, the contents of which are incorporated herein by reference. In addition, a commercially available product can be used as the resin having an acid group.

[0052] The acid value of the resin having an acid group is preferably 5 to 200 mgKOH / g. The upper limit is preferably 150 mgKOH / g or less, more preferably 100 mgKOH / g or less, and even more preferably 80 mgKOH / g or less. The lower limit is preferably 10 mgKOH / g or more, more preferably 15 mgKOH / g or more, and even more preferably 20 mgKOH / g or more. The weight average molecular weight (Mw) of the resin having an acid group is preferably 3000 to 35000. The upper limit is preferably 25000 or less, more preferably 20000 or less, and even more preferably 15000 or less. The lower limit is preferably 4000 or more, more preferably 6000 or more, and even more preferably 7000 or more.

[0053] The coloring composition of the present invention may also use a resin having a basic group. The resin having a basic group is preferably a resin containing a repeating unit having a basic group in a side chain, more preferably a copolymer having a repeating unit having a basic group in a side chain and a repeating unit not having a basic group, and further preferably a block copolymer having a repeating unit having a basic group in a side chain and a repeating unit not having a basic group. The resin having a basic group may also be used as a dispersant. The amine value of the resin having a basic group is preferably 5 to 300 mgKOH / g. The lower limit is preferably 10 mgKOH / g or more, more preferably 20 mgKOH / g or more. The upper limit is preferably 200 mgKOH / g or less, more preferably 100 mgKOH / g or less. Examples of the resin having a basic group include the block copolymer (B) described in paragraphs 0063 to 0112 of JP-A-2014-219665 and the block copolymer A1 described in paragraphs 0046 to 0076 of JP-A-2018-156021.

[0054] The coloring composition of the present invention preferably contains a graft resin having an acid group (hereinafter, also referred to as an acidic graft resin). According to this embodiment, it is possible to more effectively suppress the occurrence of spectral fluctuations and color unevenness of the film after a long-term heat treatment. Although the detailed reason why such an effect is obtained is unclear, it is presumed to be due to the following. That is, it is presumed that the action of the acid group of the acidic graft resin during film formation promotes the elimination reaction of the protective group from the above-mentioned specific compound, and the content of the component functioning as an antioxidant generated from the specific compound in the film can be increased. And, it is presumed that the graft chain of the acidic graft resin can suppress the aggregation of the organic pigment, and further, the action of the component functioning as an antioxidant generated from the specific compound can suppress the deterioration and aggregation of the organic pigment at high temperatures. For these reasons, it is presumed that the occurrence of spectral fluctuations and color unevenness of the film after a long-term heat treatment can be more effectively suppressed.

[0055] The acidic graft resin can be preferably used as a dispersant. Here, the graft resin means a resin containing a repeating unit having a graft chain. Also, the graft chain means a polymer chain that branches out from the main chain of the repeating unit.

[0056] The graft chain is preferably a polymer chain containing at least one structure selected from a polyester structure, a polyether structure, a poly(meth)acrylic structure, a polystyrene structure, a polyurethane structure, a polyurea structure, and a polyamide structure, and more preferably a polymer chain containing at least one structure selected from a polyester structure, a polyether structure, and a poly(meth)acrylic structure.

[0057] The terminal structure of the graft chain is not particularly limited. It may be a hydrogen atom or a substituent. Examples of the substituent include an alkyl group, an aryl group, a heteroaryl group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an alkylthioether group, an arylthioether group, a heteroarylthioether group, a hydroxy group, and an amino group. Among them, from the viewpoint of improving the dispersibility of pigments and the like, a group having a steric repulsion effect is preferred, and an alkyl group or an alkoxy group having 5 to 24 carbon atoms is preferred. The alkyl group and the alkoxy group may be any of linear, branched, and cyclic, and linear or branched is preferred.

[0058] The weight average molecular weight of the graft chain is preferably 500 to 10,000. The upper limit is preferably 5,000 or less, more preferably 3,000 or less. The lower limit is preferably 800 or more, more preferably 1,000 or more. In this specification, the weight average molecular weight of the graft chain is a value calculated from the weight average molecular weight of the raw material monomer used in the polymerization of the repeating unit having the graft chain. For example, the repeating unit having the graft chain can be formed by polymerizing a macromonomer. Here, the macromonomer means a polymeric compound having a polymerizable group introduced at the polymer end. The weight average molecular weight of the raw material monomer is a polystyrene-equivalent value measured by GPC (gel permeation chromatography).

[0059] Examples of the acid group contained in the acidic graft resin include a carboxyl group, a sulfo group, and a phosphate group, and the carboxyl group is preferred. The acid value of the acidic graft resin is preferably 20 to 150 mgKOH / g. The upper limit is preferably 120 mgKOH / g or less, more preferably 100 mgKOH / g or less, and even more preferably 80 mgKOH / g or less. The lower limit is preferably 25 mgKOH / g or more, more preferably 30 mgKOH / g or more, and even more preferably 35 mgKOH / g or more.

[0060] The weight average molecular weight of the acidic graft resin is preferably 3000 to 35000. The upper limit is preferably 25000 or less, more preferably 20000 or less, and even more preferably 15000 or less. The lower limit is preferably 4000 or more, more preferably 6000 or more, and even more preferably 7000 or more.

[0061] Examples of the acidic graft resin include a resin containing a repeating unit having a graft chain and a repeating unit having an acid group, and a resin having a repeating unit represented by the following formula (Ac-2). The acidic graft resin may further contain other repeating units such as a repeating unit having a polymerizable group. Examples of the polymerizable group include an ethylenically unsaturated bond-containing group such as a vinyl group, a (meth)allyl group, or a (meth)acryloyl group.

[0062] When the acidic graft resin is a resin containing a repeating unit having a graft chain and a repeating unit having an acid group, the acidic graft resin preferably contains 1 mol% or more of the repeating unit having a graft chain in the total repeating units of the acidic graft resin, more preferably 2 mol% or more, and even more preferably 3 mol% or more. The upper limit can be 90 mol%, 80 mol% or less, 70 mol% or less, 60 mol% or less, or 50 mol% or less. In addition, the acidic graft resin preferably contains 1 mol% or more of the repeating unit having an acid group in the total repeating units of the acidic graft resin, more preferably 2 mol% or more, and even more preferably 3 mol% or more. The upper limit can be 90 mol%, 80 mol% or less, 70 mol% or less, 60 mol% or less, or 50 mol% or less.

[0063] Next, the repeating unit represented by formula (Ac-2) will be described. [ka] In formula (Ac-2), Ar 10represents a group containing an aromatic carboxyl group, L 11 represents -COO- or -CONH-, and L 12 represents a trivalent linking group, P 10 represents a polymer chain.

[0064] In formula (Ac-2), Ar 10 Examples of the group containing an aromatic carboxyl group represented by the formula (1) include a structure derived from an aromatic tricarboxylic acid anhydride, a structure derived from an aromatic tetracarboxylic acid anhydride, etc. Examples of the aromatic tricarboxylic acid anhydride and the aromatic tetracarboxylic acid anhydride include compounds having the following structures. [ka]

[0065] In the above formula, Q 1 represents a single bond, -O-, -CO-, -COOCH2CH2OCO-, -SO2-, -C(CF3)2-, a group represented by the following formula (Q-1) or a group represented by the following formula (Q-2). [ka]

[0066] Ar 10 The aromatic carboxyl group-containing group represented by may have a polymerizable group. The polymerizable group is preferably an ethylenically unsaturated bond-containing group or a cyclic ether group, and more preferably an ethylenically unsaturated bond-containing group. 10 Specific examples of the group containing an aromatic carboxyl group represented by formula (Ar-11), (Ar-12), (Ar-13), and the like can be mentioned. [ka]

[0067] In formula (Ar-11), n1 represents an integer of 1 to 4, preferably 1 or 2, and more preferably 2. In formula (Ar-12), n2 represents an integer of 1 to 8, preferably an integer of 1 to 4, more preferably 1 or 2, and further preferably 2. In formula (Ar-13), n3 and n4 each independently represent an integer of 0 to 4, and are preferably an integer of 0 to 2, more preferably 1 or 2, and further preferably 1. However, at least one of n3 and n4 is an integer of 1 or more. In formula (Ar-13), Q 1 represents a single bond, -O-, -CO-, -COOCH2CH2OCO-, -SO2-, -C(CF3)2-, a group represented by the above formula (Q-1) or a group represented by the above formula (Q-2). In formulas (Ar-11) to (Ar-13), *1 represents L 11 represents the bonding position with

[0068] In formula (Ac-2), L 11 is preferably -COO-.

[0069] In formula (Ac-2), L 12 Examples of the trivalent linking group represented by include a hydrocarbon group, -O-, -CO-, -COO-, -OCO-, -NH-, -S-, and a group combining two or more of these. Examples of the hydrocarbon group include an aliphatic hydrocarbon group and an aromatic hydrocarbon group. The number of carbon atoms in the aliphatic hydrocarbon group is preferably 1 to 30, more preferably 1 to 20, and even more preferably 1 to 15. The aliphatic hydrocarbon group may be linear, branched, or cyclic. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 30, more preferably 6 to 20, and even more preferably 6 to 10. The hydrocarbon group may have a substituent. Examples of the substituent include a hydroxy group. L 12 The trivalent linking group represented by formula (L12-1) is preferable, and a group represented by formula (L12-2) is more preferable. [ka]

[0070] In formula (L12-1), L 12brepresents a trivalent linking group, X 1 represents S, and *1 represents L in formula (Ac-2). 11 *2 represents the bond position of P in formula (Ac-2). 10 It represents the bond position with L 12b Examples of the trivalent linking group represented by include a hydrocarbon group; a group in which a hydrocarbon group is combined with at least one selected from -O-, -CO-, -COO-, -OCO-, -NH-, and -S-; and the like. A hydrocarbon group or a group in which a hydrocarbon group is combined with -O- is preferred.

[0071] In formula (L12-2), L 12c represents a trivalent linking group, X 1 represents S, and *1 represents L in formula (Ac-2). 11 *2 represents the bond position of P in formula (Ac-2). 10 It represents the bond position with L 12c Examples of the trivalent linking group represented by include a hydrocarbon group; a group formed by combining a hydrocarbon group with at least one selected from -O-, -CO-, -COO-, -OCO-, -NH-, and -S-, and a hydrocarbon group is preferred.

[0072] P in formula (Ac-2) 10 The polymer chain represented by P includes at least one structure selected from a polyester structure, a polyether structure, a poly(meth)acrylic structure, a polystyrene structure, a polyurethane structure, a polyurea structure, and a polyamide structure, and is preferably a polymer chain containing at least one structure selected from a polyester structure, a polyether structure, and a poly(meth)acrylic structure. 10 The weight average molecular weight of the polymer chain represented by is preferably 500 to 10000. The upper limit is preferably 5000 or less, more preferably 3000 or less. The lower limit is preferably 800 or more, more preferably 1000 or more.

[0073] P 10 It is also preferable that the polymer chain represented by P contains a repeating unit having an ethylenically unsaturated bond-containing group in the side chain. 10The proportion of repeating units containing an ethylenically unsaturated bond-containing group in a side chain in all repeating units constituting the polymer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more. The upper limit can be set to 100% by mass, and is preferably 90% by mass or less, and even more preferably 60% by mass or less.

[0074] P 10 It is also preferable that the polymer chain represented by P contains a repeating unit containing an acid group. Examples of the acid group include a carboxyl group, a phosphoric acid group, a sulfo group, and a phenolic hydroxy group. 10 The proportion of the repeating units containing an acid group in all repeating units constituting the copolymer is preferably from 1 to 30 mass %, more preferably from 2 to 20 mass %, and even more preferably from 3 to 10 mass %.

[0075] Specific examples of the acidic graft resin include resins B-1 to B-7 described in the Examples described later. In addition, the acidic graft resin may be the resins described in paragraphs 0025 to 0094 of JP-A-2012-255128 and the polyimine resins described in paragraphs 0102 to 0166 of JP-A-2012-255128.

[0076] The coloring composition of the present invention preferably contains a resin as a dispersant. Examples of dispersants include acidic dispersants (acidic resins) and basic dispersants (basic resins). Here, the acidic dispersant (acidic resin) refers to a resin in which the amount of acid groups is greater than the amount of basic groups. The acidic dispersant (acidic resin) is preferably a resin in which the amount of acid groups is 70 mol% or more when the total amount of the amount of acid groups and the amount of basic groups is 100 mol%, and more preferably a resin substantially composed of only acid groups. The acid group possessed by the acidic dispersant (acidic resin) is preferably a carboxyl group. The acid value of the acidic dispersant (acidic resin) is preferably 40 to 105 mgKOH / g, more preferably 50 to 105 mgKOH / g, and even more preferably 60 to 105 mgKOH / g. The basic dispersant (basic resin) refers to a resin in which the amount of basic groups is greater than the amount of acid groups. The basic dispersant (basic resin) is preferably a resin having a basic group content of more than 50 mol % when the total amount of the acid group and the basic group is taken as 100 mol %. The basic group possessed by the basic dispersant is preferably an amino group.

[0077] The resin used as the dispersant is preferably a resin having a structure in which a plurality of polymer chains are bonded to a core portion. Examples of such resins include dendrimers (including star-shaped polymers). Specific examples of dendrimers include polymer compounds C-1 to C-31 described in paragraphs 0196 to 0209 of JP2013-043962A.

[0078] Furthermore, resins such as the above-mentioned acidic graft resins can also be used as dispersants.

[0079] The resin used as the dispersant is also preferably a resin containing a repeating unit having an ethylenically unsaturated bond-containing group in a side chain. The content of the repeating unit having an ethylenically unsaturated bond-containing group in a side chain is preferably 10 mol % or more, more preferably 10 to 80 mol %, and even more preferably 20 to 70 mol %, of all repeating units of the resin.

[0080] Dispersants are also available as commercially available products, and specific examples thereof include the DISPERBYK series (e.g., DISPERBYK-111, 161, etc.) manufactured by BYKChemie and the Solsperse series (e.g., Solsperse 76500, etc.) manufactured by Lubrizol Japan Co., Ltd. In addition, pigment dispersants described in paragraphs 0041 to 0130 of JP-A-2014-130338 can also be used, the contents of which are incorporated herein. The resins described as dispersants above can also be used for purposes other than dispersants. For example, they can also be used as binders.

[0081] The resin content in the total solid content of the coloring composition is preferably 1 to 45% by mass. The lower limit is preferably 5% by mass or more, more preferably 10% by mass or more. The upper limit is preferably 40% by mass or less, more preferably 30% by mass or less. The content of the acidic graft resin in the total solid content of the colored composition is preferably 1 to 45% by mass. The lower limit is preferably 5% by mass or more, and more preferably 10% by mass or more. The upper limit is preferably 40% by mass or less, and more preferably 30% by mass or less. The content of the acidic graft resin is preferably 100 to 3000 parts by mass relative to 100 parts by mass of the specific compound. The lower limit is preferably 200 parts by mass or more, more preferably 300 parts by mass or more. The upper limit is preferably 2500 parts by mass or less, more preferably 2000 parts by mass or less.

[0082] <<Specific compounds>> The coloring composition of the present invention contains a compound A in which a phenolic hydroxy group of a phenolic antioxidant is protected with a protecting group that can be removed by heating, or a compound represented by formula (AO-1). Hereinafter, the above-mentioned compound A and the compound represented by formula (AO-1) are collectively referred to as specific compounds.

[0083] Compound A is preferably a compound that, when heated to 180° C. or higher, the protective group is eliminated to generate a phenolic hydroxy group. Examples of the protective group in compound A include reaction residues of acid anhydrides, acid chlorides, tert-butoxycarbonylating agents, alkyl halide compounds, silyl chloride compounds, allyl ether compounds, and methallyl ether compounds. Specific examples of the protective group include R in formula (AO-1): 2 The formula weight of the protecting group is preferably 30 to 200, more preferably 35 to 100, and further preferably 40 to 70, because it is preferable that the protecting group volatilizes and does not remain during baking.

[0084] Compound A is preferably a compound containing 1 to 10 phenolic hydroxy groups protected by the above-mentioned protecting groups (hereinafter also referred to as protected hydroxy groups) in one molecule. The lower limit is preferably 2 or more, more preferably 3 or more. The upper limit is preferably 6 or less, more preferably 4 or less.

[0085] Compound A is preferably a compound represented by formula (AO-1).

[0086] [ka] In the formula, R 1 represents a substituent, R 2 -COOR 11 , -CH2-CH=CR 12 R 13 , -CH2(-OL R1 ) q -OR 14 or SiR 15 R 16 R 17 represents R 11 , R 12 , R 14 , R 15 , R 16 and R 17 each independently represents an alkyl group, R 13 represents a hydrogen atom or an alkyl group, L R1 represents an alkylene group, q represents 0 or 1, If q is 1, L R1 and R 14 may be bonded to form a ring, m represents an integer of 0 to 4; n represents an integer from 1 to 10; X 1 represents a group having a valence of n.

[0087] R in formula (AO-1) 1 Examples of the substituent represented by include the substituent T described below, and it is preferably an alkyl group, an aryl group, or a heterocyclic group, and more preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 1 to 30, more preferably 1 to 15, and even more preferably 1 to 8. The alkyl group may be linear, branched, or cyclic, but is preferably branched or cyclic, and more preferably branched, because it provides good functionality as a phenolic antioxidant after elimination.

[0088] R in formula (AO-1) 2 -COOR 11 , -CH2-CH=CR 12 R 13 , -CH2(-OL R1 ) q -OR 14 or SiR 15 R 16 R 17 Represents R 11 , R 14 , R 15 , R 16 and R 17 each independently represents an alkyl group, R 12 and R 13 each independently represents a hydrogen atom or an alkyl group; L R1 represents an alkylene group, q represents 0 or 1, and when q is 1, L R1 and R 14 may be bonded to form a ring.

[0089] R 11 The number of carbon atoms in the alkyl group represented by R is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5. The alkyl group may be linear, branched, or cyclic, but is preferably a branched alkyl group because the temperature at which it is eliminated is appropriate. 11 The alkyl group represented by R may have a substituent. Examples of the substituent include the substituent T described below, and R is preferably an aryl group. 11 Specific examples include a tert-butyl group and a benzyl group.

[0090] R 12 and R 13 The alkyl group represented by R preferably has 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and further preferably 1 to 5 carbon atoms. 11 and R 12 The alkyl group represented by R may be any of linear, branched, and cyclic, but is preferably a linear or branched alkyl group because it can be produced at a lower cost, and is more preferably a linear alkyl group. 12 and R 13 is preferably each independently an alkyl group, more preferably a methyl group.

[0091] R 14 The number of carbon atoms in the alkyl group represented by is preferably 1 to 20, more preferably 1 to 10, further preferably 1 to 5, and particularly preferably 1 to 3. The alkyl group may be linear, branched, or cyclic, but is preferably a linear alkyl group because it can be produced at lower cost.

[0092] R 15 ~R 17 The number of carbon atoms in the alkyl group represented by is preferably 1 to 20, more preferably 1 to 10, further preferably 1 to 5, and particularly preferably 1 to 3. The alkyl group may be linear, branched, or cyclic, but is preferably a linear alkyl group because it can be produced at lower cost.

[0093] LR1 The number of carbon atoms in the alkylene group represented by is preferably 1 to 20, more preferably 1 to 10, further preferably 1 to 5, and particularly preferably 1 to 3. The alkylene group may be linear, branched, or cyclic, but is preferably a linear or branched alkylene group because it can be produced at a lower cost. R1 and R 14 may be bonded to form a ring. R1 ) q -OR 14 ", when q is 0, -CH2-OR 14 It is a group having a structure represented by the following formula:

[0094] R 2 Specific examples of the group represented by include a tert-butoxycarbonyl group, a benzyloxycarbonyl group, a tetrahydropyranyl group, a methoxymethyl group, a 2-methoxyethoxymethyl group, a trimethylsilyl group, -CH2-CH=C(CH3)2, and -CH2-CH=CH2, and of these, a tert-butoxycarbonyl group and -CH2-CH=C(CH3)2 are preferred.

[0095] X in formula (AO-1) 1 The n-valent group represented by is an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a heterocyclic group, -O-, -S-, -CO-, -COO-, -OCO-, -SO2-, -NR X -, -NR X CO-, -CONR X -, -NR X SO2-, -SO2NR X - and combinations thereof; R Xrepresents a hydrogen atom, an alkyl group, or an aryl group. The number of carbon atoms in the aliphatic hydrocarbon group is preferably 1 to 20, more preferably 2 to 20, further preferably 2 to 10, and particularly preferably 2 to 5. The aliphatic hydrocarbon group may be linear, branched, or cyclic. The cyclic aliphatic hydrocarbon group may be monocyclic or polycyclic. The number of carbon atoms in the aromatic hydrocarbon group is preferably 6 to 18, more preferably 6 to 14, and further preferably 6 to 10. The aromatic hydrocarbon group is preferably a monocyclic or condensed ring aromatic hydrocarbon group having 2 to 4 condensed rings. The aromatic hydrocarbon group is preferably a benzene ring group. The heterocyclic group is preferably a monocyclic or condensed ring having 2 to 4 condensed rings. The number of heteroatoms constituting the ring of the heterocyclic group is preferably 1 to 3. The heteroatom constituting the ring of the heterocyclic group is preferably a nitrogen atom, an oxygen atom, or a sulfur atom. The number of carbon atoms constituting the ring of the heterocyclic group is preferably 3 to 30, more preferably 3 to 18, and more preferably 3 to 12. The aliphatic hydrocarbon group, aromatic hydrocarbon group and heterocyclic group may have a substituent. Examples of the substituent include the groups listed as the substituent T described later. X The number of carbon atoms in the alkyl group represented by R is preferably 1 to 20, more preferably 1 to 15, and further preferably 1 to 8. The alkyl group may be linear, branched, or cyclic, preferably linear or branched, and more preferably linear. X The alkyl group represented by may further have a substituent. Examples of the substituent include the substituent T described below. X The number of carbon atoms in the aryl group represented by R is preferably 6 to 30, more preferably 6 to 20, and further preferably 6 to 12. X The aryl group represented by may further have a substituent. Examples of the substituent include the substituent T described below.

[0096] X 1 The n-valent group represented by is preferably a group represented by any one of formulas (X-1) to (X-4). [ka] In formula (X-1), L 3 represents a trivalent group, T 3represents a single bond or a divalent linking group, and there are three T 3 may be the same or different from each other. In formula (X-2), L 4 represents a tetravalent group, T 4 represents a single bond or a divalent linking group, and there are four T 4 may be the same or different from each other. In formula (X-3), L 5 represents a pentavalent group, T 5 represents a single bond or a divalent linking group, and there are five T 5 may be the same or different from each other. In formula (X-4), L 6 represents a hexavalent group, T 6 represents a single bond or a divalent linking group, and there are six T 6 may be the same or different from each other. In the above formula, * represents a bond.

[0097] T 3 ~T 6 Examples of the divalent linking group represented by include an alkylene group, an arylene group, a heterocyclic group, -NH-, -SO-, -SO2-, -CO-, -O-, -COO-, -OCO-, -S-, -NHCO-, -CONH-, and groups formed by combining two or more of these. The number of carbon atoms in the alkylene group is preferably 1 to 20, and more preferably 1 to 10. The alkylene group may be linear, branched, or cyclic, and is preferably linear or branched, and more preferably linear. The arylene group preferably has 6 to 20 carbon atoms, and more preferably has 6 to 12 carbon atoms. The alkylene group, arylene group and heterocyclic group may further have a substituent, for example, the substituent T described below.

[0098] L 3 Examples of the trivalent group represented by L include the above divalent linking groups in which one hydrogen atom has been removed. 4 Examples of the tetravalent group represented by L include groups in which two hydrogen atoms have been removed from the divalent linking groups described above. 5Examples of the pentavalent group represented by L include groups in which three hydrogen atoms have been removed from the divalent linking groups described above. 6 Examples of the hexavalent group represented by include groups in which four hydrogen atoms have been removed from the divalent linking groups described above. 3 ~L 6 The trivalent to hexavalent group represented by may further have a substituent. Examples of the substituent include the substituent T described below.

[0099] In formula (AO-1), m represents an integer of 0 to 4, preferably an integer of 0 to 3, more preferably an integer of 0 to 2, and particularly preferably 1 or 2.

[0100] In formula (AO-1), n ​​represents an integer of 1 to 10, and the lower limit of n is preferably 2 or more, and more preferably 3 or more. The upper limit of n is preferably 6 or less, and more preferably 4 or less.

[0101] (substituent T) The substituent T is a halogen atom, a cyano group, a nitro group, an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, -ORt 1 , -CORt 1 , -COORt 1 , -OCORt 1 , -NRt 1 Rt 2 , -NRt 3 CORt 1 , -CONRt 1 Rt 2 , -NRt 3 CONRt 1 Rt 2 , -NRt 3 COORt 1 , -SRt 1 , -SO2Rt 1 , -SO2ORt 1 , -NRt 3 SO2Rt 1 or -SO2NRt 1 Rt 2 Examples include: Rt 1 ~Rt 3Rt each independently represents a hydrogen atom, an alkyl group, an aryl group, or a heterocyclic group. 1 and Rt 2 may be bonded to form a ring.

[0102] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. The number of carbon atoms in the alkyl group is preferably from 1 to 30, more preferably from 1 to 15, and further preferably from 1 to 8. The alkyl group may be linear, branched, or cyclic. The alkenyl group preferably has 2 to 30 carbon atoms, more preferably 2 to 15 carbon atoms, and even more preferably 2 to 8 carbon atoms. The aryl group preferably has 6 to 30 carbon atoms, more preferably 6 to 20 carbon atoms, and further preferably 6 to 12 carbon atoms. The heterocyclic group may be a monocyclic ring or a condensed ring. The heterocyclic group is preferably a monocyclic ring or a condensed ring having 2 to 4 condensed rings. The number of heteroatoms constituting the ring of the heterocyclic group is preferably 1 to 3. The heteroatoms constituting the ring of the heterocyclic group are preferably nitrogen atoms, oxygen atoms, or sulfur atoms. The number of carbon atoms constituting the ring of the heterocyclic group is preferably 3 to 30, more preferably 3 to 18, and more preferably 3 to 12. The alkyl group, aryl group and heterocyclic group may have a substituent or may be unsubstituted. Examples of the substituent include groups selected from the group of the substituent T described above.

[0103] The specific compound can be obtained by reacting a phenol compound produced by the method described in, for example, JP-A-57-111375, JP-A-03-173843, JP-A-06-128195, JP-A-07-206771, JP-A-07-252191, or JP-T-2004-501128 with an acid anhydride, an acid chloride, a tert-butoxycarbonylating reagent, an alkyl halide compound, a silyl chloride compound, an allyl ether compound, 1-chloro-3-methyl-2-butene, or the like. Specific examples of the specific compound include compounds 1 to 6 described in the Examples described later, compounds described in paragraphs 0106 to 0109 of JP2015-131937A, compounds described in paragraphs 0028 to 0049 of JP2015-132791A, and compounds described in paragraphs 0043 to 0044 of WO2017 / 170183.

[0104] The content of the above-mentioned compound A in the total solid content of the coloring composition is preferably 1 to 10 mass%. The lower limit is preferably 2.5 mass% or more, more preferably 3 mass% or more. The upper limit is preferably 8 mass% or less, more preferably 6 mass% or less. In addition, it is preferable that the compound A is contained in an amount of 2 to 25 parts by mass per 100 parts by mass of the organic pigment. The lower limit is preferably 5.5 mass parts or more, more preferably 7 mass parts or more. The upper limit is preferably 18 mass parts or less, more preferably 13 mass parts or less. In the coloring composition of the present invention, only one type of compound A may be used, or two or more types may be used. When two or more types are used, it is preferable that the total amount thereof is within the above range.

[0105] The content of the compound represented by formula (AO-1) in the total solid content of the coloring composition is preferably 1 to 10% by mass. The lower limit is preferably 2.5% by mass or more, and more preferably 3% by mass or more. The upper limit is preferably 8% by mass or less, and more preferably 6% by mass or less. The compound represented by formula (AO-1) is preferably contained in an amount of 2 to 25 parts by mass per 100 parts by mass of the organic pigment. The lower limit is preferably 5.5 parts by mass or more, and more preferably 7 parts by mass or more. The upper limit is preferably 18 parts by mass or less, and more preferably 13 parts by mass or less. In the coloring composition of the present invention, only one specific compound may be used, or two or more specific compounds may be used. When two or more specific compounds are used, the total amount thereof is preferably within the above range.

[0106] <<Antioxidants>> The coloring composition of the present invention may contain an antioxidant. Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, amine-based antioxidants, and thioether-based antioxidants, and the like, with phenol-based antioxidants being preferred. By using the above-mentioned specific compound in combination with a phenol-based antioxidant, it is expected that the storage stability of the coloring composition will be improved. Examples of the phenol-based antioxidant include hindered phenol compounds. The phenol-based antioxidant is preferably a compound having a substituent at the site (ortho position) adjacent to the phenolic hydroxy group. The aforementioned substituent is preferably a substituted or unsubstituted alkyl group having 1 to 22 carbon atoms. Examples of commercially available phenol-based antioxidants include ADK STAB AO-20, ADK STAB AO-30, ADK STAB AO-40, ADK STAB AO-50, ADK STAB AO-50F, ADK STAB AO-60, ADK STAB AO-60G, ADK STAB AO-80, and ADK STAB AO-330 (all manufactured by ADEKA CORPORATION). In addition, the compounds described in paragraphs 0023 to 0048 of Japanese Patent No. 6268967 can also be used as the antioxidant.

[0107] The content of the antioxidant in the total solid content of the coloring composition is preferably 0.001 to 3 mass%. The lower limit is preferably 0.005 mass% or more, and more preferably 0.01 mass% or more. The upper limit is preferably 1.5 mass% or less, and more preferably 1 mass% or less. The content of the phenol-based antioxidant in the total solid content of the coloring composition is preferably 0.001 to 2 mass%. The lower limit is preferably 0.005 mass% or more, and more preferably 0.01 mass% or more. The upper limit is preferably 1.5 mass% or less, and more preferably 1 mass% or less.

[0108] In addition, the total content of the specific compound and the antioxidant in the total solid content of the coloring composition is preferably 1 to 10% by mass. The lower limit is preferably 2.5% by mass or more, and more preferably 3% by mass or more. The upper limit is preferably 8% by mass or less, and more preferably 6% by mass or less. In addition, the total content of the specific compound and the phenol-based antioxidant in the total solid content of the coloring composition is preferably 1 to 10% by mass. The lower limit is preferably 2.5% by mass or more, and more preferably 3% by mass or more. The upper limit is preferably 8% by mass or less, and more preferably 6% by mass or less.

[0109] The content of the antioxidant is preferably 0.1 to 200 parts by mass, more preferably 1 to 100 parts by mass, and even more preferably 2 to 50 parts by mass, relative to 100 parts by mass of the specific compound. The content of the phenol-based antioxidant is preferably 0.1 to 200 parts by mass, more preferably 1 to 100 parts by mass, and even more preferably 2 to 50 parts by mass, relative to 100 parts by mass of the specific compound. When the ratio of the specific compound to the phenol-based antioxidant is within the above range, the effect of improving the storage stability of the coloring composition can be expected. The antioxidant may be used alone or in combination with two or more kinds. When two or more kinds are used, the total amount is preferably within the above range.

[0110] <<Polymerizable compounds>> The coloring composition of the present invention may contain a polymerizable compound. As the polymerizable compound, a known compound capable of being crosslinked by a radical, an acid, or heat can be used. The polymerizable compound used in the present invention is preferably a compound having an ethylenically unsaturated bond-containing group. Examples of the ethylenically unsaturated bond-containing group include a vinyl group, a (meth)allyl group, and a (meth)acryloyl group. The polymerizable compound used in the present invention is preferably a radical polymerizable compound.

[0111] The polymerizable compound may be in any chemical form such as a monomer, a prepolymer, or an oligomer, but is preferably a monomer. The molecular weight of the polymerizable compound is preferably 100 to 3000. The upper limit is more preferably 2000 or less, and even more preferably 1500 or less. The lower limit is more preferably 150 or more, and even more preferably 250 or more.

[0112] The polymerizable compound is preferably a compound containing 3 or more ethylenically unsaturated bond-containing groups, more preferably a compound containing 3 to 15 ethylenically unsaturated bond-containing groups, and even more preferably a compound containing 3 to 6 ethylenically unsaturated bond-containing groups. The polymerizable compound is preferably a 3-15 functional (meth)acrylate compound, and more preferably a 3-6 functional (meth)acrylate compound. Specific examples of the polymerizable compound include compounds described in paragraphs 0095 to 0108 of JP 2009-288705 A, paragraph 0227 of JP 2013-029760 A, paragraph 0254 to 0257 of JP 2008-292970 A, paragraphs 0034 to 0038 of JP 2013-253224 A, paragraph 0477 of JP 2012-208494 A, JP 2017-048367 A, Japanese Patent No. 6057891, and Japanese Patent No. 6031807, the contents of which are incorporated herein by reference.

[0113] As the polymerizable compound, dipentaerythritol tri(meth)acrylate (commercially available product is KAYARAD D-330; manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol tetra(meth)acrylate (commercially available product is KAYARAD D-320; manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol penta(meth)acrylate (commercially available product is KAYARAD D-310; manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol hexa(meth)acrylate (commercially available products are KAYARAD DPHA; manufactured by Nippon Kayaku Co., Ltd., and NK Ester A-DPH-12E; manufactured by Shin-Nakamura Chemical Co., Ltd.), and compounds having a structure in which these (meth)acryloyl groups are bonded via ethylene glycol and / or propylene glycol residues (e.g., SR454, SR499, commercially available from Sartomer Co., Ltd.) are preferred. In addition, examples of the polymerizable compound that can be used include diglycerol EO (ethylene oxide) modified (meth)acrylate (commercially available product is M-460; manufactured by Toagosei Co., Ltd.), pentaerythritol tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., NK Ester A-TMMT), 1,6-hexanediol diacrylate (manufactured by Nippon Kayaku Co., Ltd., KAYARAD HDDA), RP-1040 (manufactured by Nippon Kayaku Co., Ltd.), Aronix TO-2349 (manufactured by Toagosei Co., Ltd.), NK Oligo UA-7200 (manufactured by Shin-Nakamura Chemical Co., Ltd.), 8UH-1006, 8UH-1012 (manufactured by Taisei Fine Chemical Co., Ltd.), and light acrylate POB-A0 (manufactured by Kyoeisha Chemical Co., Ltd.).

[0114] As the polymerizable compound, it is also preferable to use a trifunctional (meth)acrylate compound such as trimethylolpropane tri(meth)acrylate, trimethylolpropane propylene oxide modified tri(meth)acrylate, trimethylolpropane ethylene oxide modified tri(meth)acrylate, isocyanuric acid ethylene oxide modified tri(meth)acrylate, or pentaerythritol tri(meth)acrylate. Commercially available trifunctional (meth)acrylate compounds include ARONIX M-309, M-310, M-321, M-350, M-360, M-313, M-315, M-306, M-305, M-303, M-452, and M-450 (manufactured by Toagosei Co., Ltd.), NK Ester A9300, A-GLY-9E, A-GLY-20E, A-TMM-3, A-TMM-3L, A-TMM-3LM-N, A-TMPT, and TMPT (manufactured by Shin-Nakamura Chemical Co., Ltd.), KAYARAD GPO-303, TMPTA, THE-330, TPA-330, and PET-30 (manufactured by Nippon Kayaku Co., Ltd.).

[0115] As the polymerizable compound, a polymerizable compound having an acid group can also be used. Examples of the acid group include a carboxyl group, a sulfo group, and a phosphate group, and the carboxyl group is preferred. Examples of commercially available polymerizable compounds having an acid group include ARONIX M-510, M-520, and ARONIX TO-2349 (manufactured by Toagosei Co., Ltd.). The preferred acid value of the polymerizable compound having an acid group is 0.1 to 40 mgKOH / g, and more preferably 5 to 30 mgKOH / g. If the acid value of the polymerizable compound is 0.1 mgKOH / g or more, the solubility in the developer is good, and if it is 40 mgKOH / g or less, it is advantageous in terms of production and handling.

[0116] As the polymerizable compound, a polymerizable compound having a caprolactone structure can also be used. Polymerizable compounds having a caprolactone structure are commercially available as the KAYARAD DPCA series from Nippon Kayaku Co., Ltd., and examples thereof include DPCA-20, DPCA-30, DPCA-60, and DPCA-120.

[0117] As the polymerizable compound, a polymerizable compound having an alkyleneoxy group can also be used. The polymerizable compound having an alkyleneoxy group is preferably a polymerizable compound having an ethyleneoxy group and / or a propyleneoxy group, more preferably a polymerizable compound having an ethyleneoxy group, and even more preferably a trifunctional to hexafunctional (meth)acrylate compound having 4 to 20 ethyleneoxy groups. Commercially available polymerizable compounds having an alkyleneoxy group include, for example, SR-494, a tetrafunctional (meth)acrylate having four ethyleneoxy groups manufactured by Sartomer, and KAYARAD TPA-330, a trifunctional (meth)acrylate having three isobutyleneoxy groups.

[0118] As the polymerizable compound, a polymerizable compound having a fluorene skeleton can also be used. Commercially available polymerizable compounds having a fluorene skeleton include OGSOL EA-0200 and EA-0300 (manufactured by Osaka Gas Chemicals Co., Ltd., (meth)acrylate monomers having a fluorene skeleton).

[0119] It is also preferable to use a polymerizable compound that does not substantially contain environmentally regulated substances such as toluene. Examples of commercially available products of such compounds include KAYARAD DPHA LT and KAYARAD DPEA-12 LT (manufactured by Nippon Kayaku Co., Ltd.).

[0120] As the polymerizable compound, it is also preferable to use urethane acrylates described in JP-B-48-041708, JP-A-51-037193, JP-B-02-032293, and JP-B-02-016765, urethane compounds having an ethylene oxide skeleton described in JP-B-58-049860, JP-B-56-017654, JP-B-62-039417, and JP-B-62-039418, and polymerizable compounds having an amino structure or a sulfide structure in the molecule described in JP-A-63-277653, JP-A-63-260909, and JP-A-01-105238. In addition, commercially available products such as UA-7200 (manufactured by Shin-Nakamura Chemical Co., Ltd.), DPHA-40H (manufactured by Nippon Kayaku Co., Ltd.), UA-306H, UA-306T, UA-306I, AH-600, T-600, AI-600, and LINC-202UA (manufactured by Kyoeisha Chemical Co., Ltd.) can also be used as the polymerizable compound.

[0121] The content of the polymerizable compound in the total solid content of the coloring composition is preferably 0.1 to 50% by mass. The lower limit is more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. The upper limit is more preferably 40% by mass or less, and even more preferably 30% by mass or less. In the coloring composition of the present invention, only one type of polymerizable compound may be used, or two or more types may be used. When two or more types are used, the total amount thereof is preferably within the above range.

[0122] <<Photopolymerization initiator>> The coloring composition of the present invention may contain a photopolymerization initiator. The photopolymerization initiator is not particularly limited and may be appropriately selected from known photopolymerization initiators. For example, a compound having photosensitivity to light rays in the ultraviolet to visible light range is preferred. The photopolymerization initiator is preferably a photoradical polymerization initiator.

[0123] Examples of the photopolymerization initiator include halogenated hydrocarbon derivatives (e.g., compounds having a triazine skeleton, compounds having an oxadiazole skeleton, etc.), acylphosphine compounds, hexaarylbiimidazole, oxime compounds, organic peroxides, thio compounds, ketone compounds, aromatic onium salts, α-hydroxyketone compounds, α-aminoketone compounds, etc. From the viewpoint of exposure sensitivity, the photopolymerization initiator is preferably a trihalomethyltriazine compound, a benzyldimethylketal compound, an α-hydroxyketone compound, an α-aminoketone compound, an acylphosphine compound, a phosphine oxide compound, a metallocene compound, an oxime compound, a triarylimidazole dimer, an onium compound, a benzothiazole compound, a benzophenone compound, an acetophenone compound, a cyclopentadiene-benzene-iron complex, a halomethyloxadiazole compound, and a 3-aryl-substituted coumarin compound, more preferably a compound selected from an oxime compound, an α-hydroxyketone compound, an α-aminoketone compound, and an acylphosphine compound, and even more preferably an oxime compound. Further, as the photopolymerization initiator, the compounds described in paragraphs 0065 to 0111 of JP 2014-130173 A and JP Patent No. 6301489 A, the peroxide-based photopolymerization initiator described in MATERIAL STAGE 37 to 60p, vol. 19, No. 3, 2019, the photopolymerization initiator described in WO 2018 / 221177 A, the photopolymerization initiator described in WO 2018 / 110179 A, ​​the photopolymerization initiator described in JP 2019-043864 A, the photopolymerization initiator described in JP 2019-044030 A, and the peroxide-based initiator described in JP 2019-167313 A can be mentioned, the contents of which are incorporated herein by reference.

[0124] Commercially available α-hydroxyketone compounds include Omnirad 184, Omnirad 1173, Omnirad 2959, Omnirad 127 (manufactured by IGM Resins BV), Irgacure 184, Irgacure 1173, Irgacure 2959, Irgacure 127 (manufactured by BASF), etc. Commercially available α-aminoketone compounds include Omnirad 907, Omnirad 369, Omnirad 369E, Omnirad 379EG (manufactured by IGM Resins BV), Irgacure 907, Irgacure 369, Irgacure 369E, Irgacure 379EG (manufactured by BASF), etc. Commercially available acylphosphine compounds include Omnirad 819, Omnirad TPO (both manufactured by IGM Resins BV), Irgacure 819, Irgacure TPO (both manufactured by BASF), and the like.

[0125] Examples of the oxime compound include compounds described in JP-A-2001-233842, compounds described in JP-A-2000-080068, compounds described in JP-A-2006-342166, compounds described in J.C.S. Perkin II (1979, pp. 1653-1660), compounds described in J.C.S. Perkin II (1979, pp. 156-162), compounds described in Journal of Photopolymer Science and Technology (1995, pp. 202-232), compounds described in JP 2000-066385 A, compounds described in JP-T-2004-534797 A, compounds described in JP-A-2006-342166 A, compounds described in JP-A-2017-019766 A, compounds described in Japanese Patent No. 6065596 A, compounds described in WO 2015 / 152153 A, compounds described in WO 2017 / 051680 A, compounds described in JP 2017-198865 A, compounds described in paragraphs 0025 to 0038 of WO 2017 / 164127 A, compounds described in WO 2013 / 167515 A, and the like. Specific examples of the oxime compound include 3-benzoyloxyiminobutan-2-one, 3-acetoxyiminobutan-2-one, 3-propionyloxyiminobutan-2-one, 2-acetoxyiminopentan-3-one, 2-acetoxyimino-1-phenylpropan-1-one, 2-benzoyloxyimino-1-phenylpropan-1-one, 3-(4-toluenesulfonyloxy)iminobutan-2-one, and 2-ethoxycarbonyloxyimino-1-phenylpropan-1-one. Examples of commercially available products include Irgacure OXE01, Irgacure OXE02, Irgacure OXE03, and Irgacure OXE04 (all manufactured by BASF), TR-PBG-304 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), and Adeka Optomer N-1919 (manufactured by ADEKA Corporation, photopolymerization initiator 2 described in JP 2012-014052 A). In addition, it is also preferable to use, as the oxime compound, a compound that is not colorable or a compound that is highly transparent and does not easily discolor.Commercially available products include ADEKA Arcles NCI-730, NCI-831, and NCI-930 (all manufactured by ADEKA Corporation).

[0126] As the photopolymerization initiator, an oxime compound having a fluorene ring can also be used. Specific examples of the oxime compound having a fluorene ring include the compounds described in JP-A-2014-137466 and the compounds described in JP-A-06636081.

[0127] As the photopolymerization initiator, an oxime compound having a skeleton in which at least one benzene ring of a carbazole ring is replaced with a naphthalene ring can also be used. Specific examples of such oxime compounds include the compounds described in WO 2013 / 083505.

[0128] As the photopolymerization initiator, an oxime compound having a fluorine atom can also be used. Specific examples of the oxime compound having a fluorine atom include the compounds described in JP-A-2010-262028, compounds 24, 36 to 40 described in JP-A-2014-500852, and compound (C-3) described in JP-A-2013-164471.

[0129] As the photopolymerization initiator, an oxime compound having a nitro group can be used. It is also preferable that the oxime compound having a nitro group is a dimer. Specific examples of the oxime compound having a nitro group include the compounds described in paragraphs 0031 to 0047 of JP 2013-114249 A, paragraphs 0008 to 0012, and 0070 to 0079 of JP 2014-137466 A, the compounds described in paragraphs 0007 to 0025 of Japanese Patent No. 4223071 A, and Adeka Arcles NCI-831 (manufactured by ADEKA Corporation).

[0130] As the photopolymerization initiator, an oxime compound having a benzofuran skeleton can also be used. Specific examples include OE-01 to OE-75 described in WO 2015 / 036910.

[0131] As the photopolymerization initiator, an oxime compound in which a substituent having a hydroxyl group is bonded to a carbazole skeleton can also be used. Examples of such photopolymerization initiators include the compounds described in WO 2019 / 088055.

[0132] As a photopolymerization initiator, an aromatic ring group Ar in which an electron-withdrawing group is introduced into the aromatic ring is used. OX1 It is also possible to use an oxime compound having the aromatic ring group Ar OX1 Examples of the electron-withdrawing group of include an acyl group, a nitro group, a trifluoromethyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, and a cyano group. An acyl group and a nitro group are preferred, and an acyl group is more preferred because it is easy to form a film with excellent light resistance, and a benzoyl group is even more preferred. The benzoyl group may have a substituent. The substituent is preferably a halogen atom, a cyano group, a nitro group, a hydroxy group, an alkyl group, an alkoxy group, an aryl group, an aryloxy group, a heterocyclic group, a heterocyclic oxy group, an alkenyl group, an alkylsulfanyl group, an arylsulfanyl group, an acyl group, or an amino group, more preferably an alkyl group, an alkoxy group, an aryl group, an aryloxy group, a heterocyclic oxy group, an alkylsulfanyl group, an arylsulfanyl group, or an amino group, and even more preferably an alkoxy group, an alkylsulfanyl group, an aryl group, an aryloxy group, a heterocyclic oxy group, an alkylsulfanyl group, an arylsulfanyl group, or an amino group.

[0133] The oxime compound OX is preferably at least one selected from the compounds represented by the formula (OX1) and the compounds represented by the formula (OX2), and is more preferably the compound represented by the formula (OX2). [ka] In the formula, R X1represents an alkyl group, an alkenyl group, an alkoxy group, an aryl group, an aryloxy group, a heterocyclic group, a heterocyclic oxy group, an alkylsulfanyl group, an arylsulfanyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, an acyl group, an acyloxy group, an amino group, a phosphinoyl group, a carbamoyl group, or a sulfamoyl group, R X2 represents an alkyl group, an alkenyl group, an alkoxy group, an aryl group, an aryloxy group, a heterocyclic group, a heterocyclic oxy group, an alkylsulfanyl group, an arylsulfanyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, an acyloxy group, or an amino group, R X3 ~R X14 each independently represents a hydrogen atom or a substituent; However, R X10 ~R X14 At least one of the groups is an electron-withdrawing group.

[0134] In the above formula, R X12 is an electron-withdrawing group, and R X10 , R X11 , R X13 , R X14 is preferably a hydrogen atom.

[0135] Specific examples of the oxime compound OX include the compounds described in paragraphs 0083 to 0105 of Japanese Patent No. 4600600.

[0136] Specific examples of oxime compounds that can be preferably used in the present invention are shown below, but the present invention is not limited to these.

[0137] [ka] [ka]

[0138] The oxime compound is preferably a compound having a maximum absorption wavelength in the wavelength range of 350 to 500 nm, more preferably a compound having a maximum absorption wavelength in the wavelength range of 360 to 480 nm. In addition, the molar absorption coefficient of the oxime compound at a wavelength of 365 nm or 405 nm is preferably high from the viewpoint of sensitivity, more preferably 1000 to 300000, even more preferably 2000 to 300000, and particularly preferably 5000 to 200000. The molar absorption coefficient of the compound can be measured using a known method. For example, it is preferable to measure using a spectrophotometer (Varian Cary-5 spectrophotometer) using ethyl acetate as a solvent at a concentration of 0.01 g / L.

[0139] As the photopolymerization initiator, a bifunctional or trifunctional or higher functional photoradical polymerization initiator may be used. By using such a photoradical polymerization initiator, two or more radicals are generated from one molecule of the photoradical polymerization initiator, so that good sensitivity can be obtained. In addition, when a compound with an asymmetric structure is used, the crystallinity is reduced and the solubility in a solvent or the like is improved, so that precipitation is less likely to occur over time, and the stability over time of the coloring composition can be improved. Specific examples of bifunctional or trifunctional or higher functional photoradical polymerization initiators include dimers of oxime compounds described in JP-T-2010-527339, JP-T-2011-524436, WO-2015 / 004565, WO-2016-532675, paragraphs 0407 to 0412, and WO-2017 / 033680, paragraphs 0039 to 0055; compounds (E) and (G) described in WO-T-2013-522445; Examples of the photoinitiator include Cmpd1 to 7 described in JP 2016 / 034963 A, the oxime ester photoinitiator described in paragraph 0007 of JP 2017-523465 A, the photoinitiator described in paragraphs 0020 to 0033 of JP 2017-167399 A, the photopolymerization initiator (A) described in paragraphs 0017 to 0026 of JP 2017-151342 A, and the oxime ester photoinitiator described in Japanese Patent No. 6,469,669 A.

[0140] The content of the photopolymerization initiator in the total solid content of the coloring composition is preferably 0.1 to 30% by mass. The lower limit is preferably 0.5% by mass or more, and more preferably 1% by mass or more. The upper limit is preferably 20% by mass or less, and more preferably 15% by mass or less. In the coloring composition of the present invention, only one type of photopolymerization initiator may be used, or two or more types may be used. When two or more types are used, the total amount thereof is preferably within the above range.

[0141] <<Compounds containing cyclic ether groups>> The coloring composition of the present invention may contain a compound having a cyclic ether group. Examples of the cyclic ether group include an epoxy group and an oxetanyl group. The compound having a cyclic ether group is preferably a compound having an epoxy group (hereinafter also referred to as an epoxy compound). As the epoxy compound, the compounds described in paragraphs 0034 to 0036 of JP-A-2013-011869, paragraphs 0147 to 0156 of JP-A-2014-043556, paragraphs 0085 to 0092 of JP-A-2014-089408, and the compounds described in JP-A-2017-179172 may also be used. The contents of these are incorporated herein by reference.

[0142] The epoxy compound may be a low molecular weight compound (e.g., a molecular weight less than 2000, or even less than 1000) or a high molecular weight compound (macromolecule) (e.g., a molecular weight of 1000 or more, and in the case of a polymer, a weight average molecular weight of 1000 or more). The weight average molecular weight of the epoxy compound is preferably 200 to 100,000, and more preferably 500 to 50,000. The upper limit of the weight average molecular weight is preferably 10,000 or less, more preferably 5,000 or less, and even more preferably 3,000 or less.

[0143] As the epoxy compound, an epoxy resin can be preferably used. Examples of the epoxy resin include an epoxy resin which is a glycidyl ether of a phenolic compound, an epoxy resin which is a glycidyl ether of various novolac resins, an alicyclic epoxy resin, an aliphatic epoxy resin, a heterocyclic epoxy resin, a glycidyl ester epoxy resin, a glycidyl amine epoxy resin, an epoxy resin obtained by glycidylating halogenated phenols, a condensate of a silicon compound having an epoxy group and another silicon compound, a copolymer of a polymerizable unsaturated compound having an epoxy group and another polymerizable unsaturated compound, and the like. The epoxy equivalent of the epoxy resin is preferably 310 to 3300 g / eq, more preferably 310 to 1700 g / eq, and even more preferably 310 to 1000 g / eq.

[0144] Examples of commercially available compounds having a cyclic ether group include EHPE3150 (manufactured by Daicel Corporation), EPICLON N-695 (manufactured by DIC Corporation), Marproof G-0150M, G-0105SA, G-0130SP, G-0250SP, G-1005S, G-1005SA, G-1010S, G-2050M, G-01100, and G-01758 (all manufactured by NOF Corporation, epoxy group-containing polymers).

[0145] The content of the compound having a cyclic ether group in the total solid content of the coloring composition is preferably 0.1 to 20% by mass. The lower limit is, for example, preferably 0.5% by mass or more, and more preferably 1% by mass or more. The upper limit is, for example, preferably 15% by mass or less, and even more preferably 10% by mass or less. The compound having a cyclic ether group may be one type or two or more types. In the case of two or more types, the total amount thereof is preferably within the above range.

[0146] <<Pigment derivatives>> The coloring composition of the present invention preferably contains a pigment derivative. Examples of the pigment derivative include a compound having a structure in which an acid group or a basic group is bonded to a pigment skeleton. Examples of the pigment skeleton constituting the pigment derivative include a quinoline pigment skeleton, a benzimidazolone pigment skeleton, a benzisoindole pigment skeleton, a benzothiazole pigment skeleton, an iminium pigment skeleton, a squarylium pigment skeleton, a croconium pigment skeleton, an oxonol pigment skeleton, a pyrrolopyrrole pigment skeleton, a diketopyrrolopyrrole pigment skeleton, an azo pigment skeleton, an azomethine pigment skeleton, a phthalocyanine pigment skeleton, a naphthalocyanine pigment skeleton, an anthraquinone pigment skeleton, a dianthraquinone pigment skeleton, a quinacridone pigment skeleton, a dioxazine pigment skeleton, a perinone pigment skeleton, a perylene pigment skeleton, and a thiazine indigo pigment skeleton. , thioindigo dye skeleton, isoindoline dye skeleton, isoindolinone dye skeleton, quinophthalone dye skeleton, iminium dye skeleton, dithiol dye skeleton, triarylmethane dye skeleton, pyrromethene dye skeleton, etc., preferably a phthalocyanine dye skeleton, diketopyrrolopyrrole dye skeleton, benzoisoindole dye skeleton, anthraquinone dye skeleton, dianthraquinone dye skeleton, thiazineindigo dye skeleton, azo dye skeleton, quinophthalone dye skeleton or quinacridone dye skeleton, more preferably a phthalocyanine dye skeleton or diketopyrrolopyrrole dye skeleton. That is, the pigment derivative is preferably a phthalocyanine compound or a diketopyrrolopyrrole compound. Examples of the acid group include a sulfo group, a carboxyl group, a phosphoric acid group and salts thereof. Examples of the atom or atomic group constituting the salt include an alkali metal ion (Li + , Na + , K + etc.), alkaline earth metal ions (Ca 2+ , Mg 2+ Examples of the basic group include an amino group, a pyridinyl group and its salt, an ammonium group salt, and a phthalimidomethyl group. Examples of the atom or atomic group constituting the salt include a hydroxide ion, a halogen ion, a carboxylate ion, a sulfonate ion, and a phenoxide ion.

[0147] The pigment derivative may contain a pigment derivative with excellent visible transparency (hereinafter also referred to as a transparent pigment derivative). The maximum molar absorption coefficient (εmax) of the transparent pigment derivative in the wavelength range of 400 to 700 nm is 3000 L·mol -1 ·cm -1 It is preferable that the concentration is less than 1000 L·mol -1 ·cm -1 It is more preferable that it is less than 100 L·mol -1 ·cm -1 The lower limit of εmax is, for example, 1 L mol -1 ·cm -1 is greater than or equal to 10 L mol -1 ·cm -1 More than that is fine.

[0148] Specific examples of the pigment derivative include the compounds described in the examples described later, JP-A-56-118462, JP-A-63-264674, JP-A-01-217077, JP-A-03-009961, JP-A-03-026767, JP-A-03-153780, JP-A-03-045662, JP-A-04-285669, JP-A-06-145546, JP-A-06-212088, JP-A-06-240158, JP-A-10-030063, JP-A-10-195326, and paragraphs of International Publication No. 2011 / 024896. Nos. 0086 to 0098, paragraphs 0063 to 0094 of International Publication No. 2012 / 102399, paragraph 0082 of International Publication No. 2017 / 038252, paragraph 0171 of JP-A-2015-151530, paragraphs 0162 to 0183 of JP-A-2011-252065, JP-A-2003-081972, Japanese Patent No. 5299151, JP-A-2015-172732, JP-A-2014-199308, JP-A-2014-085562, JP-A-2014-035351, and compounds described in JP-A-2008-081565 are included.

[0149] The content of the pigment derivative in the total solid content of the coloring composition is preferably 0.3 to 20 mass%. The lower limit is preferably 0.6 mass% or more, more preferably 0.9 mass% or more. The upper limit is preferably 15 mass% or less, more preferably 12.5 mass% or less, and even more preferably 10 mass% or less. The content of the pigment derivative is preferably 1 to 30 mass parts relative to 100 mass parts of the organic pigment. The lower limit is preferably 2 mass parts or more, more preferably 3 mass parts or more. The upper limit is preferably 25 mass parts or less, more preferably 20 mass parts or less, and even more preferably 15 mass% or less. In the coloring composition of the present invention, only one type of pigment derivative may be used, or two or more types may be used in combination. When two or more types are used in combination, the total amount thereof is preferably within the above range.

[0150] <<Specific amine compounds>> The coloring composition of the present invention may also contain a compound (hereinafter also referred to as a specific amine compound) that contains three or more basic groups in one molecule, has an amine value of 2.7 mmol / g or more, and has a molecular weight of 100 or more.

[0151] The molecular weight of the specific amine compound is preferably 200 or more, more preferably 250 or more. The upper limit is preferably 100,000 or less, more preferably 50,000 or less, even more preferably 10,000 or less, and particularly preferably 2,000 or less. In addition, when the molecular weight value of the specific amine compound can be calculated from the structural formula, the molecular weight of the specific amine compound is the value calculated from the structural formula. On the other hand, when the molecular weight of the specific amine compound cannot be calculated from the structural formula or is difficult to calculate, the value of the number average molecular weight measured by the boiling point elevation method is used. In addition, when the molecular weight cannot be measured by the boiling point elevation method or is difficult to measure, the value of the number average molecular weight measured by the viscosity method is used. In addition, when the molecular weight cannot be measured by the viscosity method or is difficult to measure by the viscosity method, the value of the number average molecular weight in terms of polystyrene measured by the GPC (gel permeation chromatography) method is used.

[0152] The amine value of the specific amine compound is preferably 5 mmol / g or more, more preferably 10 mmol / g or more, and even more preferably 15 mmol / g or more.

[0153] The number of basic groups contained in the specific amine compound is preferably 4 or more, more preferably 6 or more, and further preferably 10 or more.

[0154] The basic group of the specific amine compound is preferably an amino group. The specific amine compound is preferably a compound having a primary amino group, more preferably a compound containing a primary amino group and a tertiary amino group, and further preferably a compound containing a primary amino group, a secondary amino group, and a tertiary amino group.

[0155] The amino group of the specific amine compound may be a cyclic amino group. The cyclic amino group may be an aliphatic cyclic amino group such as a piperidino group, or an aromatic cyclic amino group such as a pyridyl group. The cyclic amino group is preferably a cyclic amino group having a 5-membered or 6-membered ring structure, more preferably a cyclic amino group having a 6-membered ring structure, and even more preferably an aliphatic cyclic amino group having a 6-membered ring structure. The cyclic amino group preferably has a hindered amine structure, and particularly preferably has a 6-membered hindered amine structure. As the hindered amine structure, it is preferable that the two carbon atoms in the ring structure adjacent to the nitrogen atom of the cyclic amino group have a substituent such as an alkyl group. Examples of cyclic amino groups having a hindered amine structure include 1,2,2,6,6-pentamethylpiperidyl group, 2,2,6,6-tetramethylpiperidyl group, 1,2,6,6-trimethylpiperidyl group, 2,6-dimethylpiperidyl group, 1-methyl-2,6-di(t-butyl)piperidyl group, 2,6-di(t-butyl)piperidyl group, 1,2,2,5,5-pentamethylpyrrolidyl group, 2,2,5,5-tetramethylpyrrolidyl group, etc. Among them, 1,2,2,6,6-pentamethylpiperidyl group or 2,2,6,6-tetramethylpiperidyl group is preferable, and 1,2,2,6,6-pentamethylpiperidyl group is more preferable.

[0156] The specific amine compound is preferably a polyalkyleneimine because it can further improve the storage stability of the coloring composition. The polyalkyleneimine is a polymer obtained by ring-opening polymerization of an alkyleneimine, and has a branched structure containing a primary amino group, a secondary amino group, and a tertiary amino group. The number of carbon atoms in the alkyleneimine is preferably 2 to 6, more preferably 2 to 4, even more preferably 2 or 3, and particularly preferably 2. Specific examples of the alkyleneimine include ethyleneimine, propyleneimine, 1,2-butyleneimine, and 2,3-butyleneimine, and are preferably ethyleneimine or propyleneimine, and more preferably ethyleneimine. The polyalkyleneimine is particularly preferably polyethyleneimine. In addition, the polyethyleneimine preferably contains 10 mol % or more of primary amino groups, more preferably 20 mol % or more, and even more preferably 30 mol % or more of primary amino groups based on the total of the primary amino groups, secondary amino groups, and tertiary amino groups. Commercially available polyethyleneimines include Epomin SP-003, SP-006, SP-012, SP-018, SP-200, and P-1000 (all manufactured by Nippon Shokubai Co., Ltd.).

[0157] The content of the specific amine compound in the total solid content of the coloring composition is preferably 0.1 to 5% by mass. The lower limit is preferably 0.2% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. The upper limit is preferably 4.5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less.

[0158] The content of the specific amine compound is preferably 0.5 to 10 parts by mass relative to 100 parts by mass of the pigment. The lower limit is preferably 0.6 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more. The upper limit is preferably 8 parts by mass or less, more preferably 7% by mass or less, and even more preferably 5 parts by mass or less.

[0159] The content of the specific amine compound is preferably 0.5 to 50 parts by mass relative to 100 parts by mass of the graft resin having an acid group. The lower limit is preferably 0.6 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 3 parts by mass or more. The upper limit is preferably 45 parts by mass or less, more preferably 40% by mass or less, and even more preferably 30 parts by mass or less.

[0160] <<Solvent>> The coloring composition of the present invention preferably contains a solvent. The solvent is preferably an organic solvent. Examples of organic solvents include ester-based solvents, ketone-based solvents, alcohol-based solvents, amide-based solvents, ether-based solvents, and hydrocarbon-based solvents. For details, refer to paragraph 0223 of International Publication No. 2015 / 166779, the contents of which are incorporated herein by reference. In addition, ester-based solvents substituted with a cyclic alkyl group and ketone-based solvents substituted with a cyclic alkyl group can also be preferably used. Specific examples of organic solvents include polyethylene glycol monomethyl ether, dichloromethane, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl cellosolve acetate, ethyl lactate, diethylene glycol dimethyl ether, butyl acetate, methyl 3-methoxypropionate, 2-heptanone, 3-pentanone, 4-heptanone, cyclohexanone, 2-methylcyclohexanone, 3-methylcyclohexanone, 4-methylcyclohexanone, cycloheptanone, cyclooctanone, cyclohexyl acetate, cyclopentanone, ethyl carbitol acetate, and butyl ether. Examples of suitable organic solvents include ethyl carbitol acetate, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, propylene glycol diacetate, 3-methoxybutanol, methyl ethyl ketone, gamma butyrolactone, sulfolane, anisole, 1,4-diacetoxybutane, diethylene glycol monoethyl ether acetate, butane-1,3-diyl diacetate, dipropylene glycol methyl ether acetate, and diacetone alcohol. However, aromatic hydrocarbons (benzene, toluene, xylene, ethylbenzene, etc.) as organic solvents may be reduced for environmental reasons (for example, the amount of the organic solvent may be reduced to 50 ppm (parts per million) or less, 10 ppm or less, or 1 ppm or less).

[0161] In the present invention, it is preferable to use an organic solvent with a low metal content, and the metal content of the organic solvent is preferably 10 mass ppb (parts per billion) or less. If necessary, an organic solvent with a mass ppt (parts per trillion) level may be used, and such an organic solvent is provided, for example, by Toyo Gosei Co., Ltd. (The Chemical Daily, November 13, 2015).

[0162] Methods for removing impurities such as metals from organic solvents include, for example, distillation (molecular distillation, thin film distillation, etc.) and filtration using a filter. The filter used for filtration has a filter pore size of preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less. The filter material is preferably polytetrafluoroethylene, polyethylene, or nylon.

[0163] The organic solvent may contain isomers (compounds having the same number of atoms but different structures). In addition, the organic solvent may contain only one type of isomer or multiple types of isomers.

[0164] The content of peroxide in the organic solvent is preferably 0.8 mmol / L or less, and more preferably contains substantially no peroxide.

[0165] The content of the solvent in the coloring composition is preferably from 10 to 95% by mass, more preferably from 20 to 90% by mass, and further preferably from 30 to 90% by mass.

[0166] In addition, the coloring composition of the present invention preferably does not substantially contain environmentally regulated substances from the viewpoint of environmental regulations. In the present invention, substantially not containing environmentally regulated substances means that the content of the environmentally regulated substances in the coloring composition is 50 mass ppm or less, preferably 30 mass ppm or less, more preferably 10 mass ppm or less, and particularly preferably 1 mass ppm or less. Examples of environmentally regulated substances include benzene; alkylbenzenes such as toluene and xylene; and halogenated benzenes such as chlorobenzene. These are registered as environmentally regulated substances under the REACH (Registration Evaluation Authorization and Restriction of CHemicals) regulations, the PRTR (Pollutant Release and Transfer Register) Act, and the VOC (Volatile Organic Compounds) regulations, and the amount of use and the handling method are strictly regulated. These compounds may be used as solvents when producing each component used in the coloring composition, and may be mixed into the coloring composition as a residual solvent. From the viewpoint of human safety and environmental consideration, it is preferable to reduce these substances as much as possible. A method for reducing the environmentally regulated substances includes a method of heating or reducing the pressure in the system to a temperature equal to or higher than the boiling point of the environmentally regulated substances, and distilling off the environmentally regulated substances from the system. In addition, when a small amount of the environmentally regulated substances is distilled off, it is also useful to perform azeotropy with a solvent having a boiling point equivalent to that of the corresponding solvent in order to increase efficiency. In addition, when a compound having radical polymerizability is contained, a polymerization inhibitor or the like may be added and distilled off under reduced pressure in order to suppress crosslinking between molecules caused by the progress of radical polymerization reaction during distillation under reduced pressure. These distillation methods are possible at any stage, such as the stage of the raw materials, the stage of the product obtained by reacting the raw materials (for example, a resin solution or a polyfunctional monomer solution after polymerization), or the stage of a colored composition prepared by mixing these compounds.

[0167] <<Curing accelerator>> The coloring composition of the present invention may contain a curing accelerator. Examples of the curing accelerator include a thiol compound, a methylol compound, an amine compound, a phosphonium salt compound, an amidine salt compound, an amide compound, a base generator, an isocyanate compound, an alkoxysilane compound, and an onium salt compound. Specific examples of the curing accelerator include compounds described in paragraphs 0094 to 0097 of International Publication No. 2018 / 056189, compounds described in paragraphs 0246 to 0253 of JP-A-2015-034963, compounds described in paragraphs 0186 to 0251 of JP-A-2013-041165, ionic compounds described in JP-A-2014-055114, compounds described in paragraphs 0071 to 0080 of JP-A-2012-150180, alkoxysilane compounds having epoxy groups described in JP-A-2011-253054, compounds described in paragraphs 0085 to 0092 of Japanese Patent No. 5765059, and carboxyl group-containing epoxy curing agents described in JP-A-2017-036379. When the colored composition contains a curing accelerator, the content of the curing accelerator in the total solid content of the colored composition is preferably from 0.3 to 8.9 mass %, and more preferably from 0.8 to 6.4 mass %.

[0168] <<Ultraviolet absorber>> The coloring composition of the present invention may contain an ultraviolet absorber. Examples of ultraviolet absorbers include conjugated diene compounds, aminodiene compounds, salicylate compounds, benzophenone compounds, benzotriazole compounds, acrylonitrile compounds, hydroxyphenyltriazine compounds, indole compounds, and triazine compounds. For details, compounds described in paragraphs 0052-0072 of JP-A-2012-208374, paragraphs 0317-0334 of JP-A-2013-068814, and paragraphs 0061-0080 of JP-A-2016-162946 are included, the contents of which are incorporated herein by reference. Examples of commercially available ultraviolet absorbers include UV-503 (manufactured by Daito Chemical Co., Ltd.). Examples of benzotriazole compounds include the MYUA series (The Chemical Daily, February 1, 2016) manufactured by Miyoshi Oil and Fat. In addition, the ultraviolet absorbent may be a compound described in paragraphs 0049 to 0059 of Japanese Patent No. 6268967. The content of the ultraviolet absorbent in the total solid content of the coloring composition is preferably 0.01 to 10 mass%, more preferably 0.01 to 5 mass%. In the coloring composition of the present invention, only one type of ultraviolet absorbent may be used, or two or more types may be used. When two or more types are used, the total amount thereof is preferably within the above range.

[0169] <<Polymerization inhibitor>> The coloring composition of the present invention may contain a polymerization inhibitor. Examples of the polymerization inhibitor include hydroquinone, p-methoxyphenol, di-tert-butyl-p-cresol, pyrogallol, tert-butylcatechol, benzoquinone, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), and N-nitrosophenylhydroxyamine salts (ammonium salts, cerous salts, etc.). Among these, p-methoxyphenol is preferred. When a polymerization inhibitor is contained, the content of the polymerization inhibitor in the total solid content of the coloring composition is preferably 0.0001 to 5 mass%. The polymerization inhibitor may be one type or two or more types. When two or more types are used, the total amount is preferably within the above range.

[0170] <<Silane coupling agent>> The coloring composition of the present invention may contain a silane coupling agent. In the present invention, the silane coupling agent means a silane compound having a hydrolyzable group and other functional groups. The hydrolyzable group refers to a substituent that is directly bonded to a silicon atom and can generate a siloxane bond by at least one of a hydrolysis reaction and a condensation reaction. Examples of the hydrolyzable group include a halogen atom, an alkoxy group, and an acyloxy group, and an alkoxy group is preferred. That is, the silane coupling agent is preferably a compound having an alkoxysilyl group. Examples of functional groups other than the hydrolyzable group include a vinyl group, a (meth)allyl group, a (meth)acryloyl group, a mercapto group, an epoxy group, an oxetanyl group, an amino group, a ureido group, a sulfide group, an isocyanate group, and a phenyl group, and an amino group, a (meth)acryloyl group, and an epoxy group are preferred. Specific examples of the silane coupling agent include N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane (Shin-Etsu Chemical Co., Ltd., trade name KBM-602), N-β-aminoethyl-γ-aminopropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., trade name KBM-603), N-β-aminoethyl-γ-aminopropyltriethoxysilane (Shin-Etsu Chemical Co., Ltd., trade name KBE-602), γ-aminopropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., trade name KBM-903), γ-aminopropyltriethoxysilane (Shin-Etsu Chemical Co., Ltd., trade name KBE-903), 3-methacryloxypropylmethyldimethoxysilane (Shin-Etsu Chemical Co., Ltd., trade name KBM-502), and 3-methacryloxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., trade name KBM-503). Specific examples of the silane coupling agent include compounds described in paragraphs 0018-0036 of JP-A-2009-288703 and compounds described in paragraphs 0056-0066 of JP-A-2009-242604, the contents of which are incorporated herein by reference. When the silane coupling agent is contained, the content of the silane coupling agent in the total solid content of the coloring composition is preferably 0.01-15.0 mass%, more preferably 0.05-10.0 mass%. The silane coupling agent may be one type or two or more types.When two or more types are used, the total amount is preferably within the above range.

[0171] <<Surfactants>> The coloring composition of the present invention may contain a surfactant. As the surfactant, various surfactants such as fluorine-based surfactants, nonionic surfactants, cationic surfactants, anionic surfactants, and silicon-based surfactants may be used. As the surfactant, the surfactants described in paragraphs 0238 to 0245 of WO 2015 / 166779 may be mentioned, the contents of which are incorporated herein by reference.

[0172] In the present invention, the surfactant is preferably a fluorosurfactant. By including a fluorosurfactant in the coloring composition, the liquid properties (particularly, fluidity) can be improved and the liquid saving can be improved. In addition, a film with less unevenness in thickness can be formed.

[0173] The fluorine content in the fluorine-based surfactant is preferably 3 to 40% by mass, more preferably 5 to 30% by mass, and particularly preferably 7 to 25% by mass. A fluorine-based surfactant having a fluorine content within this range is effective in terms of uniformity of the thickness of the coating film and liquid saving properties, and also has good solubility in a coloring composition.

[0174] Examples of fluorine-based surfactants include those described in paragraphs 0060 to 0064 of JP 2014-041318 A (corresponding paragraphs 0060 to 0064 of WO 2014 / 017669 A), those described in paragraphs 0117 to 0132 of JP 2011-132503 A, and those described in JP 2020-008634 A, the contents of which are incorporated herein by reference. Commercially available fluorine-based surfactants include, for example, Megafac F-171, F-172, F-173, F-176, F-177, F-141, F-142, F-143, F-144, F-437, F-475, F-477, F-479, F-482, F-554, F-555-A, F-556, F-557, F-558, F-559, F-560, F-561, F-565, F-563, F-568, F-575, F-780, EXP, MFS-330, and R-41. , R-41-LM, R-01, R-40, R-40-LM, RS-43, TF-1956, RS-90, R-94, RS-72-K, DS-21 (all manufactured by DIC Corporation), Fluorard FC430, FC431, FC171 (all manufactured by Sumitomo 3M Limited), Surflon S-382, SC-101, SC-103, SC-104, SC-105, SC-1068, SC-381, SC-383, S-393, KH-40 (all manufactured by AGC Corporation), PolyFox Examples of such agents include PF636, PF656, PF6320, PF6520, and PF7002 (all manufactured by OMNOVA), and Ftergent 710FM, 610FM, 601AD, 601ADH2, 602A, 215M, and 245F (all manufactured by NEOS Corporation).

[0175] In addition, the fluorosurfactant may be an acrylic compound that has a molecular structure with a functional group containing a fluorine atom, and when heat is applied, the functional group containing the fluorine atom is broken and the fluorine atom volatilizes. Examples of such fluorosurfactants include the Megafac DS series manufactured by DIC Corporation (The Chemical Daily (February 22, 2016), Nikkei Business Daily (February 23, 2016)), such as Megafac DS-21.

[0176] In addition, it is also preferable to use a polymer of a fluorine atom-containing vinyl ether compound having a fluorinated alkyl group or a fluorinated alkylene ether group and a hydrophilic vinyl ether compound as the fluorine-based surfactant. For such a fluorine-based surfactant, the description in JP 2016-216602 A can be referred to, and the contents of this specification are incorporated herein.

[0177] The fluorosurfactant may be a block polymer. For example, the compounds described in JP-A-2011-089090 may be mentioned. The fluorosurfactant may be a fluorine-containing polymer compound containing a repeating unit derived from a (meth)acrylate compound having a fluorine atom and a repeating unit derived from a (meth)acrylate compound having two or more (preferably five or more) alkyleneoxy groups (preferably ethyleneoxy groups, propyleneoxy groups). In addition, the fluorine-containing surfactants described in paragraphs 0016 to 0037 of JP-A-2010-032698 and the following compounds are also exemplified as the fluorosurfactant used in the present invention. [ka] The weight average molecular weight of the above compound is preferably 3,000 to 50,000, for example, 14,000. In the above compound, % indicating the proportion of repeating units is mol %.

[0178] In addition, the fluorine-based surfactant may be a fluorine-containing polymer having an ethylenically unsaturated bond-containing group in a side chain.Specific examples include compounds described in paragraphs 0050 to 0090 and 0289 to 0295 of JP 2010-164965 A, such as Megafac RS-101, RS-102, RS-718K, and RS-72-K manufactured by DIC Corporation.In addition, the fluorine-based surfactant may be compounds described in paragraphs 0015 to 0158 of JP 2015-117327 A.

[0179] Nonionic surfactants include glycerol, trimethylolpropane, trimethylolethane, and their ethoxylates and propoxylates (e.g., glycerol propoxylate, glycerol ethoxylate, etc.), polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyethylene glycol dilaurate, polyethylene glycol distearate, and sorbitan fat. Acid esters, Pluronic L10, L31, L61, L62, 10R5, 17R2, 25R2 (manufactured by BASF), Tetronic 304, 701, 704, 901, 904, 150R1 (manufactured by BASF), Solsperse 20000 (manufactured by Lubrizol Japan Co., Ltd.), NCW-101, NCW-1001, NCW-1002 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), Paionin D-6112, D-6112-W, D-6315 (manufactured by Takemoto Oil Co., Ltd.), Olfine E1010, Surfynol 104, 400, 440 (manufactured by Nissin Chemical Industry Co., Ltd.), and the like.

[0180] Examples of silicone surfactants include Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, Toray Silicone SH8400 (all manufactured by Toray Dow Corning Co., Ltd.), TSF-4440, TSF-4300, TSF-4445, TSF-4460, TSF-4452 (all manufactured by Momentive Performance Materials, Inc.), KP-341, KF-6001, KF-6002 (all manufactured by Shin-Etsu Silicone Co., Ltd.), BYK307, BYK323, BYK330 (all manufactured by BYK-Chemie).

[0181] The content of the surfactant in the total solid content of the coloring composition is preferably 0.001% by mass to 5.0% by mass, more preferably 0.005% by mass to 3.0% by mass. In the coloring composition of the present invention, only one type of surfactant may be used, or two or more types may be used. When two or more types are used, the total amount thereof is preferably within the above range.

[0182] <<Other ingredients>> The coloring composition of the present invention may contain, as necessary, a sensitizer, a curing accelerator, a filler, a heat curing accelerator, a plasticizer, and other auxiliaries (for example, conductive particles, fillers, defoamers, flame retardants, leveling agents, peeling accelerators, fragrances, surface tension regulators, chain transfer agents, etc.). By appropriately incorporating these components, it is possible to adjust the properties such as film properties. For these components, for example, the description in paragraphs 0183 and after of JP-A-2012-003225 (corresponding to paragraph 0237 of US Patent Application Publication No. 2013 / 0034812) and the description in paragraphs 0101-0104, 0107-0109, etc. of JP-A-2008-250074 can be referred to, and the contents of these are incorporated herein.

[0183] The colouring composition of the present invention may contain a light fastness improver. Examples of the light resistance improver include the compounds described in paragraphs 0036 to 0037 of JP-A-2017-198787, the compounds described in paragraphs 0029 to 0034 of JP-A-2017-146350, the compounds described in paragraphs 0036 to 0037 and 0049 to 0052 of JP-A-2017-129774, the compounds described in paragraphs 0031 to 0034 and 0058 to 0059 of JP-A-2017-129674, the compounds described in paragraphs 0036 to 0037 and 0051 to 0054 of JP-A-2017-122803, the compounds described in paragraphs 0025 to 0039 of WO 2017 / 164127, and the compounds described in paragraphs 0025 to 0039 of JP-A-2017-186546. JP-A-2015-025116, JP-A-2012-145604, JP-A-2012-103475, JP-A-2012-103475, JP-A-2012-103475, JP-A-2011-257591, JP-A-2011-257591, JP-A-2011-191483, JP-A-2011-145668, JP-A-2011-145668, JP-A-2011-253174 ...7591, JP-A-2011-257591, JP-A-2011-253174, JP-A-2011-253174, JP-A-2011-253174, JP-A-2011-253174, JP-A-2011-253174,

[0184] The coloring composition of the present invention preferably contains 100 ppm or less, more preferably 50 ppm or less, even more preferably 10 ppm or less, and particularly preferably substantially no free metal that is not bonded or coordinated to a pigment, etc. According to this embodiment, it is possible to expect effects such as stabilization of pigment dispersibility (prevention of aggregation), improvement of spectral characteristics due to improved dispersibility, stabilization of curable components, prevention of conductivity fluctuation due to elution of metal atoms and metal ions, and improvement of display characteristics. In addition, the effects described in JP 2012-153796 A, JP 2000-345085 A, JP 2005-200560 A, JP 08-043620 A, JP 2004-145078 A, JP 2014-119487 A, JP 2010-083997 A, JP 2017-090930 A, JP 2018-025612 A, JP 2018-025797 A, JP 2017-155228 A, JP 2018-036521 A, and the like can also be obtained. The above-mentioned free metals include Na, K, Ca, Sc, Ti, Mn, Cu, Zn, Fe, Cr, Co, Mg, Al, Sn, Zr, Ga, Ge, Ag, Au, Pt, Cs, Ni, Cd, Pb, Bi, etc. In addition, the coloring composition of the present invention preferably has a content of free halogens not bonded or coordinated with pigments, etc. of 100 ppm or less, more preferably 50 ppm or less, even more preferably 10 ppm or less, and particularly preferably substantially free. Examples of halogens include F, Cl, Br, I, and anions thereof. Methods for reducing free metals and halogens in the coloring composition include washing with ion-exchanged water, filtration, ultrafiltration, purification with ion-exchange resin, etc.

[0185] It is also preferable that the coloring composition of the present invention is substantially free of terephthalic acid ester. Here, "substantially free" means that the content of terephthalic acid ester in the total amount of the coloring composition is 1000 mass ppb or less, more preferably 100 mass ppb or less, and particularly preferably zero.

[0186] From the viewpoint of environmental regulations, the use of perfluoroalkylsulfonic acid and its salt, and perfluoroalkylcarboxylic acid and its salt may be restricted. In the coloring composition of the present invention, when the content of the above-mentioned compounds is reduced, the content of perfluoroalkylsulfonic acid (particularly perfluoroalkylsulfonic acid having 6 to 8 carbon atoms in the perfluoroalkyl group) and its salt, and perfluoroalkylcarboxylic acid (particularly perfluoroalkylcarboxylic acid having 6 to 8 carbon atoms in the perfluoroalkyl group) and its salt is preferably in the range of 0.01 ppb to 1,000 ppb, more preferably in the range of 0.05 ppb to 500 ppb, and even more preferably in the range of 0.1 ppb to 300 ppb, based on the total solid content of the coloring composition. The coloring composition of the present invention may be substantially free of perfluoroalkylsulfonic acid and its salt, and perfluoroalkylcarboxylic acid and its salt. For example, a coloring composition that is substantially free of perfluoroalkylsulfonic acid and its salt, and perfluoroalkylcarboxylic acid and its salt may be selected by using a compound that can be a substitute for perfluoroalkylsulfonic acid and its salt, and a compound that can be a substitute for perfluoroalkylcarboxylic acid and its salt. Examples of compounds that can be a substitute for regulated compounds include compounds that are excluded from the scope of regulation due to the difference in the number of carbon atoms in the perfluoroalkyl group. However, the above content does not prevent the use of perfluoroalkylsulfonic acid and its salt, and perfluoroalkylcarboxylic acid and its salt. The coloring composition of the present invention may contain perfluoroalkylsulfonic acid and its salt, and perfluoroalkylcarboxylic acid and its salt within the maximum allowable range.

[0187] <<Containment Container>> The container for storing the coloring composition is not particularly limited, and a known container can be used. In addition, it is also preferable to use a multi-layer bottle whose inner wall is made of six types of six-layer resin or a bottle with a seven-layer structure made of six types of resin as the container, in order to suppress the incorporation of impurities into the raw materials or the coloring composition. Examples of such containers include the containers described in JP-A-2015-123351. In addition, it is also preferable to make the inner wall of the container out of glass or stainless steel in order to prevent metal elution from the inner wall of the container, increase the storage stability of the coloring composition, and suppress the deterioration of the components.

[0188] <Method of preparing coloring composition> The coloring composition of the present invention can be prepared by mixing the above-mentioned components. When preparing the coloring composition, all components may be dissolved and / or dispersed in a solvent at the same time to prepare the coloring composition, or, if necessary, each component may be appropriately prepared as two or more solutions or dispersions, and these may be mixed at the time of use (at the time of application) to prepare the coloring composition.

[0189] In addition, the preparation of the coloring composition preferably includes a process for dispersing the organic pigment. In the process for dispersing the organic pigment, examples of the mechanical force used for dispersing the organic pigment include compression, squeezing, impact, shear, and cavitation. Specific examples of these processes include a bead mill, a sand mill, a roll mill, a ball mill, a paint shaker, a microfluidizer, a high-speed impeller, a sand grinder, a flow jet mixer, high-pressure wet atomization, and ultrasonic dispersion. In addition, in the grinding of the organic pigment in a sand mill (bead mill), it is preferable to use beads with a small diameter, increase the packing rate of the beads, and perform the treatment under conditions that increase the grinding efficiency. In addition, it is preferable to remove coarse particles by filtration, centrifugation, or the like after the grinding treatment. In addition, the process and dispersing machine for dispersing organic pigments may be suitably used as described in "Dispersion Technology Encyclopedia, published by Joho Kika Co., Ltd., July 15, 2005" or "Dispersion Technology and Industrial Application Practices Focusing on Suspension (Solid / Liquid Dispersion System) Comprehensive Data Collection, published by Management Development Center Publishing Department, October 10, 1978" and JP2015-157893A, paragraph number 0022. In addition, in the process for dispersing organic pigments, a salt milling process may be used to perform a particle refinement process. For the materials, equipment, processing conditions, etc. used in the salt milling process, the descriptions in, for example, JP2015-194521A and JP2012-046629A may be referred to.

[0190] In preparing the coloring composition, it is preferable to filter the coloring composition with a filter for the purpose of removing foreign matter and reducing defects. As the filter, any filter that has been used for filtering purposes can be used without any particular limitation. For example, filters using materials such as fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyamide resins such as nylon (e.g., nylon-6, nylon-6,6), and polyolefin resins (including high-density and ultra-high-molecular-weight polyolefin resins) such as polyethylene and polypropylene (PP) are exemplified. Among these materials, polypropylene (including high-density polypropylene) and nylon are preferred.

[0191] The pore size of the filter is preferably 0.01 to 7.0 μm, more preferably 0.01 to 3.0 μm, and even more preferably 0.05 to 0.5 μm. If the pore size of the filter is within the above range, fine foreign matter can be removed more reliably. The nominal value of the filter manufacturer can be referred to for the pore size value of the filter. Various filters provided by Nippon Pall Corporation (DFA4201NXEY, DFA4201NAEY, DFA4201J006P, etc.), Advantech Toyo Co., Ltd., Nippon Integris Co., Ltd. (formerly Nippon Microlith Co., Ltd.), Kitz Microfilter Co., Ltd., etc. can be used.

[0192] It is also preferable to use a fibrous filter medium as the filter. Examples of fibrous filter medium include polypropylene fiber, nylon fiber, glass fiber, etc. Commercially available products include SBP type series (SBP008, etc.), TPR type series (TPR002, TPR005, etc.), and SHPX type series (SHPX003, etc.) manufactured by ROKI TECHNO CO., LTD.

[0193] When using a filter, different filters (for example, a first filter and a second filter, etc.) may be combined. In this case, filtration with each filter may be performed only once or two or more times. Filters having different pore sizes within the above-mentioned range may be combined. Filtration with the first filter may be performed only on the dispersion liquid, and filtration with the second filter may be performed after mixing with other components.

[0194] <Membrane> The film of the present invention is a film obtained from the colored composition of the present invention described above. The film of the present invention can be used for color filters and the like. Specifically, it can be preferably used as a colored layer (pixel) of a color filter. Examples of colored pixels include red pixels, green pixels, blue pixels, magenta pixels, cyan pixels, and yellow pixels. The film thickness of the film of the present invention can be appropriately adjusted depending on the purpose. For example, the film thickness is preferably 5 μm or less, more preferably 1 μm or less, and even more preferably 0.6 μm or less. The lower limit of the film thickness is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more.

[0195] <Membrane manufacturing method> Next, a method for producing the film of the present invention will be described. The film of the present invention can be produced through a step of applying the coloring composition of the present invention. The film production method preferably further includes a step of forming a pattern (pixel). Examples of the method for forming the pattern (pixel) include a photolithography method and a dry etching method, and the photolithography method is preferred.

[0196] The pattern formation by the photolithography method preferably includes a step of forming a coloring composition layer on a support using the coloring composition of the present invention, a step of exposing the coloring composition layer in a pattern, and a step of developing and removing the unexposed part of the coloring composition layer to form a pattern (pixel). If necessary, a step of baking the coloring composition layer (pre-baking step) and a step of baking the developed pattern (pixel) (post-baking step) may be provided.

[0197] In the step of forming a coloring composition layer, a coloring composition layer is formed on a support using the coloring composition of the present invention. The support is not particularly limited and can be appropriately selected depending on the application. For example, a glass substrate, a silicon substrate, etc. can be mentioned, and a silicon substrate is preferable. In addition, a charge-coupled device (CCD), a complementary metal oxide semiconductor (CMOS), a transparent conductive film, etc. may be formed on the silicon substrate. In addition, a black matrix for isolating each pixel may be formed on the silicon substrate. In addition, a base layer may be provided on the silicon substrate to improve adhesion with the upper layer, prevent diffusion of a substance, or flatten the substrate surface. The surface contact angle of the base layer is preferably 20 to 70° when measured with diiodomethane. In addition, it is preferably 30 to 80° when measured with water. If the surface contact angle of the base layer is within the above range, the coloring composition has good wettability. The surface contact angle of the base layer can be adjusted by, for example, a method such as adding a surfactant.

[0198] The coloring composition can be applied by a known method. For example, a dropping method (drop casting), a slit coating method, a spray method, a roll coating method, a spin coating method, a casting coating method, a slit and spin method, a pre-wetting method (for example, a method described in JP-A-2009-145395), various printing methods such as ejection printing such as inkjet (for example, on-demand method, piezo method, thermal method), nozzle jet, flexographic printing, screen printing, gravure printing, reverse offset printing, and metal mask printing method, a transfer method using a mold, and a nanoimprint method can be mentioned. The application method in inkjet is not particularly limited, and examples thereof include the method shown in "Expanding and Usable Inkjet - Infinite Possibilities Seen in Patents -, published in February 2005, Sumibe Techno Research" (particularly pages 115 to 133), and the methods described in JP 2003-262716 A, JP 2003-185831 A, JP 2003-261827 A, JP 2012-126830 A, JP 2006-169325 A, etc. In addition, for the application method of the coloring composition, the descriptions in WO 2017 / 030174 and WO 2017 / 018419 can be referred to, and the contents of these are incorporated herein.

[0199] The colored composition layer formed on the support may be dried (prebaked). When the film is produced by a low-temperature process, prebaking may not be performed. When prebaking is performed, the prebaking temperature is preferably 150° C. or lower, more preferably 120° C. or lower, and even more preferably 110° C. or lower. The lower limit can be, for example, 50° C. or higher, and can also be 80° C. or higher. The prebaking time is preferably 10 to 300 seconds, more preferably 40 to 250 seconds, and even more preferably 80 to 220 seconds. Prebaking can be performed using a hot plate, an oven, or the like.

[0200] Next, the coloring composition layer is exposed to light in a pattern (exposure step). For example, the coloring composition layer can be exposed to light in a pattern by using a stepper exposure machine or a scanner exposure machine through a mask having a predetermined mask pattern. This allows the exposed part to be cured.

[0201] Examples of radiation (light) that can be used for exposure include g-line and i-line. Light with a wavelength of 300 nm or less (preferably light with a wavelength of 180 to 300 nm) can also be used. Examples of light with a wavelength of 300 nm or less include KrF line (wavelength 248 nm) and ArF line (wavelength 193 nm), with KrF line (wavelength 248 nm) being preferred. Long-wave light sources with wavelengths of 300 nm or more can also be used.

[0202] In addition, the exposure may be performed by irradiating the light continuously or by irradiating the light in pulses (pulse exposure). Pulse exposure is an exposure method in which light irradiation and pauses are repeated in a short cycle (for example, on the order of milliseconds or less).

[0203] The irradiation amount (exposure amount) is, for example, 0.03 to 2.5 J / cm 2 is preferable, and 0.05 to 1.0 J / cm 2 is more preferable. The oxygen concentration during exposure can be appropriately selected. In addition to being exposed in air, exposure may be performed in a low-oxygen atmosphere with an oxygen concentration of 19 volume% or less (e.g., 15 volume%, 5 volume%, or substantially oxygen-free), or in a high-oxygen atmosphere with an oxygen concentration of more than 21 volume% (e.g., 22 volume%, 30 volume%, or 50 volume%). The exposure illuminance can be appropriately set, and is usually 1000 W / m 2 ~100000W / m 2 (For example, 5000W / m 2 , 15000W / m 2 , or 35000W / m 2 The oxygen concentration and exposure illuminance may be appropriately combined. For example, the oxygen concentration is 10% by volume and the illuminance is 10,000 W / m 2, oxygen concentration 35% by volume, illuminance 20000W / m 2 etc.

[0204] Next, the unexposed portion of the coloring composition layer is developed and removed to form a pattern (pixel). The unexposed portion of the coloring composition layer can be developed and removed using a developer. As a result, the coloring composition layer in the unexposed portion in the exposure step is dissolved into the developer, and only the photocured portion remains. The temperature of the developer is preferably, for example, 20 to 30°C. The development time is preferably 20 to 180 seconds. In addition, in order to improve the removability of residues, the process of shaking off the developer every 60 seconds and supplying new developer may be repeated several times.

[0205] Examples of the developer include organic solvents and alkaline developers, and alkaline developers are preferably used. As the alkaline developer, an alkaline aqueous solution (alkaline developer) obtained by diluting an alkaline agent with pure water is preferred. Examples of the alkaline agent include organic alkaline compounds such as ammonia, ethylamine, diethylamine, dimethylethanolamine, diglycolamine, diethanolamine, hydroxylamine, ethylenediamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, ethyltrimethylammonium hydroxide, benzyltrimethylammonium hydroxide, dimethylbis(2-hydroxyethyl)ammonium hydroxide, choline, pyrrole, piperidine, and 1,8-diazabicyclo-[5.4.0]-7-undecene, and inorganic alkaline compounds such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium hydrogencarbonate, sodium silicate, and sodium metasilicate. As the alkaline agent, compounds with a large molecular weight are preferred in terms of the environment and safety. The concentration of the alkaline agent in the alkaline aqueous solution is preferably 0.001 to 10% by mass, more preferably 0.01 to 1% by mass. The developer may further contain a surfactant. The developer may be prepared as a concentrated solution from the viewpoint of convenience of transportation and storage, and then diluted to a required concentration when used. The dilution ratio is not particularly limited, but can be set in the range of, for example, 1.5 to 100 times. It is also preferable to wash (rinse) with pure water after development. It is also preferable to perform rinsing by supplying a rinsing liquid to the colored composition layer after development while rotating the support on which the colored composition layer after development has been formed. It is also preferable to perform rinsing by moving the nozzle that ejects the rinsing liquid from the center of the support to the periphery of the support. At this time, when moving the nozzle from the center of the support to the periphery, the nozzle may be moved while gradually decreasing the moving speed. By performing rinsing in this manner, the in-plane variation of the rinse can be suppressed. The same effect can be obtained by gradually decreasing the rotation speed of the support while moving the nozzle from the center of the support to the periphery.

[0206] After development and drying, it is preferable to perform additional exposure treatment or heating treatment (post-baking). Additional exposure treatment and post-baking are curing treatments after development to complete curing. The heating temperature in post-baking is, for example, preferably 100 to 240°C, more preferably 200 to 240°C. Post-baking can be performed continuously or batchwise using a heating means such as a hot plate, a convection oven (hot air circulation dryer), or a high-frequency heater to heat the developed film to the above conditions. When additional exposure treatment is performed, it is preferable that the light used for exposure has a wavelength of 400 nm or less. The additional exposure treatment may be performed by the method described in Korean Patent Publication No. 10-2017-0122130.

[0207] The pattern formation by the dry etching method preferably includes the steps of forming a colored composition layer on a support using the colored composition of the present invention, curing the entire colored composition layer to form a cured layer, forming a photoresist layer on the cured layer, exposing the photoresist layer in a pattern shape and developing it to form a resist pattern, and dry etching the cured layer using an etching gas with the resist pattern as a mask. In the formation of the photoresist layer, it is preferable to further perform a pre-bake treatment. In particular, the process of forming the photoresist layer is preferably a form in which a heat treatment after exposure and a heat treatment after development (post-bake treatment) are performed. For the pattern formation by the dry etching method, the description in paragraphs 0010 to 0067 of JP 2013-064993 A can be referred to, and the contents thereof are incorporated herein.

[0208] <Color filters> Next, the color filter of the present invention will be described. The color filter of the present invention has the above-mentioned film of the present invention. Preferably, the film of the present invention is used as a colored pixel of the color filter, more preferably as a green pixel.

[0209] One embodiment of the color filter includes a color filter having at least red, green, and blue pixels, and at least one of the red, green, and blue color pixels being composed of the film of the present invention. Another embodiment of the color filter includes a color filter having at least cyan, magenta, and yellow pixels, and at least one of the cyan, magenta, and yellow color pixels being composed of the film of the present invention.

[0210] The color filters can be used in solid-state imaging devices such as CCDs (charge-coupled devices) and CMOSs ​​(complementary metal-oxide semiconductors), image display devices, and the like.

[0211] The thickness of the film of the present invention in the color filter can be adjusted appropriately depending on the purpose. The thickness is preferably 5 μm or less, more preferably 1 μm or less, and even more preferably 0.6 μm or less. The lower limit of the thickness is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more.

[0212] The width of the pixels included in the color filter is preferably 0.4 to 10.0 μm. The lower limit is preferably 0.4 μm or more, more preferably 0.5 μm or more, and even more preferably 0.6 μm or more. The upper limit is preferably 5.0 μm or less, more preferably 2.0 μm or less, even more preferably 1.0 μm or less, and even more preferably 0.8 μm or less. The Young's modulus of the pixels is preferably 0.5 to 20 GPa, and more preferably 2.5 to 15 GPa.

[0213] It is preferable that each pixel included in the color filter has high flatness. Specifically, the surface roughness Ra of the pixel is preferably 100 nm or less, more preferably 40 nm or less, and even more preferably 15 nm or less. Although the lower limit is not specified, it is preferable that it is, for example, 0.1 nm or more. The surface roughness of the pixel can be measured, for example, using an AFM (atomic force microscope) Dimension3100 manufactured by Veeco. In addition, the contact angle of water on the pixel can be set to an appropriate preferred value, but is typically in the range of 50 to 110°. The contact angle can be measured, for example, using a contact angle meter CV-DT·A type (manufactured by Kyowa Interface Science Co., Ltd.). In addition, it is preferable that the volume resistance value of the pixel is high. Specifically, the volume resistance value of the pixel is 10 9 It is preferable that the resistance is 10 Ω·cm or more. 11 It is more preferable that the resistivity is Ω·cm or more. There is no upper limit, but for example, 10 14 The volume resistance of the pixel can be measured, for example, by using an ultra-high resistance meter 5410 (manufactured by Advantest Corporation).

[0214] In the color filter, a protective layer may be provided on the surface of the film (pixel) of the present invention. By providing a protective layer, various functions such as oxygen blocking, low reflection, hydrophilicity / hydrophobicity, and blocking of light of a specific wavelength (ultraviolet rays, near infrared rays, etc.) can be imparted. The thickness of the protective layer is preferably 0.01 to 10 μm, more preferably 0.1 to 5 μm. Methods for forming the protective layer include a method of forming the layer by applying a resin composition dissolved in an organic solvent, a chemical vapor deposition method, and a method of attaching a molded resin with an adhesive. The components constituting the protective layer include (meth)acrylic resin, ene-thiol resin, polycarbonate resin, polyether resin, polyarylate resin, polysulfone resin, polyethersulfone resin, polyphenylene resin, polyarylene ether phosphine oxide resin, polyimide resin, polyamideimide resin, polyolefin resin, cyclic olefin resin, polyester resin, styrene resin, polyol resin, polyvinylidene chloride resin, melamine resin, urethane resin, aramid resin, polyamide resin, alkyd resin, epoxy resin, modified silicone resin, fluorine resin, polycarbonate resin, polyacrylonitrile resin, cellulose resin, Si, C, W, Al2O3, Mo, SiO2, Si2N4, etc., and may contain two or more of these components. For example, in the case of a protective layer intended for oxygen blocking, the protective layer preferably contains a polyol resin, SiO2, and Si2N4. In addition, in the case of a protective layer intended for low reflection, the protective layer preferably contains a (meth)acrylic resin and a fluorine resin.

[0215] When the protective layer is formed by applying a resin composition, known methods such as spin coating, casting, screen printing, and inkjet can be used as the method for applying the resin composition. Known organic solvents (e.g., propylene glycol 1-monomethyl ether 2-acetate, cyclopentanone, ethyl lactate, etc.) can be used as the organic solvent contained in the resin composition. When the protective layer is formed by chemical vapor deposition, known chemical vapor deposition methods (thermal chemical vapor deposition, plasma chemical vapor deposition, photochemical vapor deposition) can be used as the chemical vapor deposition.

[0216] The protective layer may contain additives such as organic or inorganic fine particles, absorbents for light of a specific wavelength (e.g., ultraviolet light, near infrared light, etc.), refractive index adjusters, adhesives, and surfactants, as necessary. Examples of organic or inorganic fine particles include polymer fine particles (e.g., silicone resin fine particles, polystyrene fine particles, melamine resin fine particles), titanium oxide, zinc oxide, zirconium oxide, indium oxide, aluminum oxide, titanium nitride, titanium oxynitride, magnesium fluoride, hollow silica, silica, calcium carbonate, and barium sulfate. Known absorbents can be used as absorbents for light of a specific wavelength. The content of these additives can be appropriately adjusted, but is preferably 0.1 to 70% by mass, more preferably 1 to 60% by mass, based on the total mass of the protective layer.

[0217] In addition, as the protective layer, the protective layers described in paragraphs 0073 to 0092 of JP2017-151176A can also be used.

[0218] The color filter may have an underlayer. The surface contact angle of the underlayer is preferably 20 to 70° when measured with diiodomethane. Also, it is preferably 30 to 80° when measured with water. The surface contact angle of the underlayer can be adjusted, for example, by adding a surfactant.

[0219] The color filter may have a structure in which each pixel is embedded in a space partitioned by partitions in, for example, a lattice shape.

[0220] <Solid-state imaging element> The solid-state imaging device of the present invention has the above-mentioned film of the present invention. The configuration of the solid-state imaging device is not particularly limited as long as it has the film of the present invention and functions as a solid-state imaging device, and examples thereof include the following configurations.

[0221] The substrate has a plurality of photodiodes constituting a light receiving area of ​​a solid-state imaging device (such as a CCD (charge-coupled device) image sensor or a CMOS (complementary metal oxide semiconductor) image sensor) and a transfer electrode made of polysilicon or the like, a light shielding film having an opening only for the light receiving portion of the photodiode on the photodiode and the transfer electrode, a device protection film made of silicon nitride or the like formed on the light shielding film so as to cover the entire light shielding film and the light receiving portion of the photodiode, and a color filter on the device protection film. Furthermore, the device protection film may have a light collecting means (e.g., a microlens, etc., the same below) on the device protection film and below the color filter (on the side closer to the substrate), or a light collecting means on the color filter. The color filter may have a structure in which each colored pixel is embedded in a space partitioned by partitions, for example, in a lattice shape. In this case, the partitions preferably have a lower refractive index than each colored pixel. Examples of imaging devices having such a structure include those described in JP 2012-227478 A, JP 2014-179577 A, WO 2018 / 043654 A, and U.S. Patent Application Publication No. 2018 / 0040656 A. An imaging device including the solid-state imaging element of the present invention can be used for digital cameras, electronic devices having an imaging function (such as mobile phones), as well as vehicle-mounted cameras and surveillance cameras.

[0222] <Image display device> The image display device of the present invention has the above-mentioned film of the present invention. Examples of the image display device include liquid crystal display devices and organic electroluminescence display devices. The definition of the image display device and details of each image display device are described, for example, in "Electronic Display Devices" (written by Akio Sasaki, published by Kogyo Chosakai Co., Ltd. in 1990) and "Display Devices" (written by Junsho Ibuki, published by Sangyo Tosho Co., Ltd. in 1989). Liquid crystal display devices are described, for example, in "Next Generation Liquid Crystal Display Technology" (edited by Tatsuo Uchida, published by Kogyo Chosakai Co., Ltd. in 1994). There are no particular limitations on the liquid crystal display device to which the present invention can be applied, and the present invention can be applied to various types of liquid crystal display devices described in the above "Next Generation Liquid Crystal Display Technology." EXAMPLES

[0223] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below.

[0224] <Production of Dispersion> After mixing the raw materials shown in the table below, 230 parts by mass of zirconia beads with a diameter of 0.3 mm were added and dispersed for 5 hours using a paint shaker, and the beads were separated by filtration to produce a dispersion. The numerical values ​​for the amount of each raw material in the table below are parts by mass. The amount of resin (dispersant) is the amount in a resin solution with a solid content of 20% by mass.

[0225] [Table 1] [Table 2] [Table 3] [Table 4] [Table 5]

[0226] The raw materials listed in the above table are abbreviated as follows:

[0227] (Colorant) [Organic pigments] PR122: CI Pigment Red 122 (red pigment) PR177: CI Pigment Red 177 (red pigment) PR254: CI Pigment Red 254 (red pigment) PR264: CI Pigment Red 264 (red pigment) PR269: CI Pigment Red 269 (red pigment) PR272: CI Pigment Red 272 (red pigment) PY129: CI Pigment Yellow 129 (yellow pigment) PY139: CI Pigment Yellow 139 (yellow pigment) PY150: CI Pigment Yellow 150 (yellow pigment) PY185: CI Pigment Yellow 185 (yellow pigment) PY215: CI Pigment Yellow 215 (yellow pigment) Yellow 1: Compound with the following structure [ka] Yellow 2: Compound with the following structure [ka] Yellow 3: Compound with the following structure [ka] PO71: CI Pigment Orange 71 (orange pigment) PG7: CI Pigment Green 7 (green pigment) PG36: CI Pigment Green 36 (green pigment) PG58: CI Pigment Green 58 (green pigment) PG62: CI Pigment Green 62 (green pigment) PG63: CI Pigment Green 63 (green pigment) PB15:6: CI Pigment Blue 15:6 (blue pigment) PB60: CI Pigment Blue 60 (blue pigment) PV23: CI Pigment Violet 23 (purple pigment) PV29: CI Pigment Violet 29 (purple pigment) Al phthalocyanine: a compound with the following structure [ka]

[0228] [dye] AR289: CI Acid Red 289 Dye 1: Compound having the following structure (xanthene dye, in the following structure, iPr is an isopropyl group) [ka] Dye 2: A salt-forming compound of the polymer (weight average molecular weight 7000) with the following structure and CI Acid Red 52 (xanthene dye) [ka] Dye 3: Compound with the following structure (xanthene dye) [ka]

[0229] (Pigment derivatives) Derivative 1: Compound having the following structure [ka] Derivative 2: Compound having the following structure [ka] Derivative 3: Compound having the following structure [ka] Derivative 4: Compound having the following structure [ka] Derivative 5: Compound having the following structure [ka]

[0230] (Dispersion aid) Dispersing agent 1: Polyethyleneimine (Epomin SP-003, manufactured by Nippon Shokubai Co., Ltd., molecular weight 300, resin content 98% or more by mass, viscosity 200 to 500 mPa·s) Dispersing agent 2: Polyethyleneimine (Epomin SP-006, manufactured by Nippon Shokubai Co., Ltd., molecular weight 600, resin content 98% or more by mass, viscosity 500 to 2500 mPa·s) Dispersing agent 3: Polyethyleneimine (Epomin SP-018, manufactured by Nippon Shokubai Co., Ltd., molecular weight 1800, resin content 98% or more by mass, viscosity 8500 to 15000 mPa·s) Dispersing agent 4: Polyethyleneimine (Epomin SP-200, manufactured by Nippon Shokubai Co., Ltd., molecular weight 10,000, resin content 98% or more by mass, viscosity 40,000 to 150,000 mPa·s)

[0231] <Resin> B-1: Resin solution (solids concentration 20% by mass) of Resin B-1 synthesized by the following method. 50 parts by mass of methyl methacrylate, 50 parts by mass of n-butyl methacrylate, and 45.4 parts by mass of PGMEA (propylene glycol monomethyl ether acetate) were charged into a reaction vessel, and the atmospheric gas was replaced with nitrogen gas. The inside of the reaction vessel was heated to 70°C, 6 parts by mass of 3-mercapto-1,2-propanediol were added, and 0.12 parts by mass of AIBN (azobisisobutyronitrile) were further added, and the reaction was carried out for 12 hours. It was confirmed that 95% had reacted by measuring the solid content. Next, 9.7 parts by mass of pyromellitic anhydride, 70.3 parts by mass of PGMEA, and 0.20 parts by mass of DBU (1,8-diazabicyclo-[5.4.0]-7-undecene) as a catalyst were added, and the reaction was carried out for 7 hours at 120°C. It was confirmed that 98% or more of the acid anhydride had been half-esterified by measuring the acid value, and the reaction was terminated. PGMEA was added to adjust the non-volatile content (solid content concentration) to 20% by mass, and a resin solution of Resin B-1 (a graft resin having an acid group) having the following structure and an acid value of 43 mgKOH / g and a weight average molecular weight of 9,000 was obtained. [ka]

[0232] B-2: Resin solution of Resin B-2 (solids concentration: 20% by mass) synthesized by the following method. 50 parts by mass of methyl methacrylate, 30 parts by mass of n-butyl methacrylate, 20 parts by mass of t-butyl methacrylate, and 45.4 parts by mass of PGMEA were charged into a reaction vessel, and the atmospheric gas was replaced with nitrogen gas. The inside of the reaction vessel was heated to 70°C, 6 parts by mass of 3-mercapto-1,2-propanediol was added, and 0.12 parts by mass of AIBN (azobisisobutyronitrile) was further added, and the reaction was carried out for 12 hours. It was confirmed that 95% had reacted by measuring the solid content. Next, 9.7 parts by mass of pyromellitic anhydride, 70.3 parts by mass of PGMEA, and 0.20 parts by mass of DBU (1,8-diazabicyclo-[5.4.0]-7-undecene) as a catalyst were added, and the reaction was carried out at 120°C for 7 hours. It was confirmed that 98% or more of the acid anhydride had been half-esterified by measuring the acid value, and the reaction was terminated. PGMEA was added to adjust the non-volatile content (solid content concentration) to 20 mass %, and a resin solution of Resin B-2 (graft resin having an acid group) having the following structure with an acid value of 43 mgKOH / g and a weight average molecular weight of 9000 was obtained. [ka]

[0233] B-3: Resin solution of Resin B-3 (solids concentration: 20% by mass) synthesized by the following method. In the synthesis of Resin B-2, the same procedure was followed except that 20 parts by mass of t-butyl methacrylate was replaced with 20 parts by mass of (3-ethyloxetan-3-yl)methyl methacrylate, to obtain a resin solution of Resin B-3 (a graft resin having an acid group) having the following structure and an acid value of 43 mgKOH / g and a weight average molecular weight of 9000. [ka]

[0234] B-4: 20% by mass solution of a resin having the following structure (a graft resin having an acid group, the number attached to the main chain is the molar ratio, and the number attached to the side chain is the number of repeating units. Weight average molecular weight: 24,000, acid value: 47 mgKOH / g) in PGMEA [ka]

[0235] B-5: 20% by mass solution of a resin having the following structure (a graft resin having an acid group, the number attached to the main chain is the molar ratio, and the number attached to the side chain is the number of repeating units. Weight average molecular weight 16000, acid value 67 mgKOH / g) in PGMEA [ka]

[0236] B-6: 20% by mass solution of a resin having the following structure (a graft resin having an acid group, the number attached to the main chain is the mass ratio, and the number attached to the side chain is the number of repeating units. Weight average molecular weight 13,000, acid value 65 mgKOH / g) in PGMEA [ka]

[0237] B-7: 20% by mass solution of a resin having the following structure (a graft resin having an acid group, the number attached to the main chain is the molar ratio, and the number attached to the side chain is the number of repeating units. Weight average molecular weight: 10,000) in PGMEA [ka]

[0238] B-8: 20% by mass solution of the resin with the following structure (the numbers attached to the main chain are mass ratios. Weight average molecular weight 13,000, acid value 74 mgKOH / g) in PGMEA [ka]

[0239] B-9: 20% by mass solution of the resin with the following structure (the numbers attached to the main chain are molar ratios; weight average molecular weight 11,000, acid value 69 mgKOH / g) in PGMEA [ka]

[0240] B-10: 20% by mass solution of the resin with the following structure (block copolymer, the values ​​added to the main chain are mass ratios. Weight average molecular weight 74,000, acid value 8 mgKOH / g, amine value 95 mgKOH / g) in PGMEA [ka]

[0241] B-11: 20% by mass solution of the resin with the following structure (block copolymer, the number added to the main chain is the molar ratio. Weight average molecular weight 6000) in PGMEA [ka]

[0242] B-12: 20% by mass solution of a resin having the following structure (a graft resin having an acid group, the number attached to the main chain is the mass ratio, and the number attached to the side chain is the number of repeating units. Weight average molecular weight 13,000, acid value 19 mgKOH / g) in PGMEA [ka]

[0243] (solvent) K-1: Propylene glycol monomethyl ether acetate (PGMEA) K-2: Propylene glycol monomethyl ether (PGME) K-3: Cyclopentanone K-4: Cyclohexanone K-5: Cyclohexyl acetate K-6: 1,4-diacetoxybutane K-7: Diethylene glycol monoethyl ether acetate K-8: Ethyl 3-ethoxypropionate K-9: 3-Pentanone K-10: 3-Methylcyclohexanone K-11: 4-Methylcyclohexanone K-12: 2-Heptanone K-13: Gamma-butyrolactone K-14: butane-1,3-diyl diacetate K-15: Dipropylene glycol methyl ether acetate K-16: Diacetone alcohol

[0244] <Production of Colored Composition> The raw materials shown in the table below were mixed to prepare a coloring composition. The resin content is the content in a resin solution with a solid content of 20% by mass. In the table below, the content of the coloring material in the total solid content of the coloring composition is shown in the "Coloring material content" column. The content of the specific compound in the total solid content of the coloring composition is shown in the "Specific compound content" column. [Table 6] [Table 7] [Table 8] [Table 9] [Table 10] [Table 11]

[0245] Among the raw materials listed by abbreviations in the above table, the raw materials other than the dispersion liquid and resin are as follows.

[0246] (Polymerizable monomer) M-1 to M-3: Compounds having the following structures [ka]

[0247] (Photopolymerization initiator) G-1 and G-2: Compounds having the following structures [ka] G-3: Irgacure OXE01 (BASF, oxime compound) G-4: Irgacure OXE02 (BASF, oxime compound) G-5: Omnirad 379 (IGM Resins BV, α-aminoketone compound)

[0248] (Specific compound) Compounds 1 to 6: Compounds having the following structures (t-Bu in the structural formulas is a tert-butyl group). [ka] [ka]

[0249] (Surfactant) I-1: 1% by mass PGMEA solution of a compound having the following structure (weight average molecular weight: 14000): In the following formula, % indicating the proportion of repeating units is mol %. [ka]

[0250] (Other additives) A-1: EHPE3150 (manufactured by Daicel Corporation, 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2'-bis(hydroxymethyl)-1-butanol) Antioxidant 1: Compound having the following structure (phenolic antioxidant, t-Bu in the structural formula is a tert-butyl group) Antioxidant 2: Compound having the following structure (phenolic antioxidant, t-Bu in the structural formula is a tert-butyl group) Antioxidant 3: Compound having the following structure (phosphorus-based antioxidant) [ka]

[0251] (solvent) K-1: Propylene glycol monomethyl ether acetate (PGMEA) K-2: Propylene glycol monomethyl ether (PGME)

[0252] <Heat resistance> (Spectral fluctuation) Each coloring composition was applied onto a glass wafer by spin coating, then heat-treated (pre-baked) at 100°C for 120 seconds using a hot plate, and then irradiated with i-rays at 1000mJ / cm 2 Then, the film was heated at 200°C for 5 minutes to produce a film having the thickness shown in the table. The glass wafer with the film was stored in a high-temperature chamber set at 120°C for 1000 hours, and a heat resistance test was performed. The transmittance of light with a wavelength of 400 to 700 nm was measured for the film before and after the heat resistance test using MCPD-3000 manufactured by Otsuka Electronics Co., Ltd., and the maximum value of the change in transmittance (ΔTmax) was obtained, and the spectral fluctuation after the heat resistance test was evaluated according to the following criteria. Here, the change in transmittance refers to the difference between the transmittance of the film before and after the heat resistance test (|transmittance of the film before the heat resistance test-transmittance of the film after the heat resistance test|), and the maximum value of the change in transmittance (ΔTmax) refers to the change in transmittance at the wavelength at which the change in transmittance of the film before and after the heat resistance test is the largest. [Evaluation Criteria] A: ΔTmax is less than 1% B: ΔTmax is 1% or more and less than 3% C: ΔTmax is 3% or more and less than 5% D: ΔTmax is 5% or more

[0253] (Color unevenness) A composition for forming an undercoat layer (CT-4000, manufactured by FUJIFILM Electronic Materials Co., Ltd.) was applied onto a glass wafer by spin coating so as to give a film thickness of 0.1 μm, and heated on a hot plate at 220° C. for 1 hour to form an undercoat layer. Each coloring composition was applied onto the glass wafer with the undercoat layer by spin coating so as to give a film thickness after post-baking as shown in the table. Next, a composition layer was formed by heating at 100° C. for 2 minutes using a hot plate. Next, an i-line stepper exposure device (FPA-3000i5+, manufactured by Canon Inc.) was used to expose this composition layer to light having a wavelength of 365 nm at 500 mJ / cm. 2 The film was exposed to an exposure of 100 μm. The composition layer after exposure was paddle-developed for 60 seconds at 23°C using a 0.3% by mass aqueous solution of tetramethylammonium hydroxide. Then, the layer was rinsed with water using a spin shower, and further washed with pure water. Then, the water droplets were blown off with high-pressure air, and the glass wafer was naturally dried, and then post-baked for 300 seconds at 220°C using a hot plate to form a film having the thickness shown in the table. A heat resistance test was carried out on the obtained film by storing it for 1000 hours in a high-temperature cabinet set at 120°C. The luminance distribution was analyzed by the following method using the glass wafer (evaluation substrate) on which the film was formed before and after the heat resistance test, and color unevenness was evaluated based on the number of pixels with a deviation of ±10% or more from the average. The method for measuring the luminance distribution will be described below. The evaluation substrate was placed between the observation lens of an optical microscope and a light source, and light was irradiated toward the observation lens. The transmitted light state was observed using an optical microscope MX-50 (Olympus Corporation) equipped with a digital camera. Five arbitrarily selected areas were photographed on the film surface. The luminance of the photographed images was quantified as a density distribution of 256 gradations from 0 to 255 and saved. The luminance distribution was analyzed from this image, and color unevenness was evaluated based on the number of pixels that deviated from the average by more than ±10%. The evaluation criteria are as follows. If the evaluation is A to C, it is determined that there is no problem in practical use. A: The number of pixels that deviate from the average by more than ±10% is 1000 or less. B: The number of pixels whose deviation from the average exceeds ±10% is more than 1000 but not more than 3000. C: The number of pixels whose deviation from the average exceeds ±10% is more than 3000 but not more than 5000. D: The number of pixels with deviation from the average of ±10% exceeds 5,000.

[0254] <Adhesion> A composition for forming an undercoat layer (CT-4000, manufactured by FUJIFILM Electronic Materials Co., Ltd.) was applied by spin coating onto a silicon wafer having a diameter of 8 inches (=203.2 mm) so as to have a film thickness of 0.1 μm, and heated using a hot plate at 220° C. for 1 hour to form an undercoat layer. Each coloring composition was applied by spin coating onto the silicon wafer with the undercoat layer so that the film thickness after post-baking was the film thickness shown in the table. Then, a composition layer was formed by heating using a hot plate at 100° C. for 2 minutes. Next, an i-line stepper exposure device (FPA-3000i5+, manufactured by Canon Inc.) was used to expose this composition layer to 500 mJ / cm of light having a wavelength of 365 nm through a mask pattern in which square pixels with sides of 1.1 μm were arranged in an area of ​​4 mm×3 mm on the substrate. 2 The composition layer after exposure was paddle-developed at 23°C for 60 seconds using a 0.3% by mass aqueous solution of tetramethylammonium hydroxide. Thereafter, the composition layer was rinsed with water using a spin shower, and then washed with pure water. Thereafter, the water droplets were blown off with high-pressure air, the silicon wafer was naturally dried, and then post-baked at 220°C for 300 seconds using a hot plate to form pixels. The obtained pixels were observed using an optical microscope, and the number of pixels that were in close contact with the silicon wafer among all the pixels was counted to evaluate the adhesion. A to C are ranges that are suitable for use. [Evaluation Criteria] A: All pixels are in close contact with the silicon wafer. B: The percentage of pixels in close contact with the silicon wafer is 98% or more and less than 100% of all pixels. C: The percentage of pixels in close contact with the silicon wafer is 95% or more and less than 98% of all pixels. D: Less than 95% of all pixels are in contact with the silicon wafer.

[0255] <Color mixture> A composition for forming an undercoat layer (CT-4000, manufactured by Fujifilm Electronic Materials Co., Ltd.) was applied by spin coating onto a glass wafer so as to give a film thickness of 0.1 μm, and heated on a hot plate at 220° C. for 1 hour to form an undercoat layer. Each coloring composition was applied by spin coating onto this glass wafer with undercoat layer so as to give a film thickness after post-baking as shown in the table. Next, a composition layer was formed by heating at 100° C. for 2 minutes using a hot plate. Next, an i-line stepper exposure device (FPA-3000i5+, manufactured by Canon Inc.) was used to expose this composition layer to light having a wavelength of 365 nm at 1000 mJ / cm. 2 The exposure was performed with an exposure dose of 10 ... A coloring composition for color mixing evaluation was applied onto the obtained first colored film using a spin coater so that the film thickness after pre-baking would be 0.6 μm, and a heat treatment (pre-baking) was performed for 120 seconds using a hot plate at 100 ° C. to obtain a laminated color filter in which a coloring composition layer (second layer) for color mixing evaluation was formed on the first colored film. The obtained laminated color filter was then developed, rinsed, and spray-dried in the same manner as in the formation of the first colored pixel, and the coloring composition layer for color mixing evaluation was developed and removed. The spectral variation (ΔT%max) of the maximum transmittance of the first colored film immediately after the preparation of the first colored film and after the colored composition layer for color mixing evaluation was developed and removed was measured using MCPD-3000 (manufactured by Otsuka Electronics Co., Ltd.), and the residual color mixing of the second colored composition remaining on the first colored film was evaluated. The maximum transmittance is the amount of change in the transmittance of the first colored film immediately after the preparation of the first colored film and after the colored composition layer for color mixing evaluation was developed and removed, and refers to the amount of change in the transmittance at the wavelength where the amount of change in the transmittance is the largest. The smaller the spectral variation (ΔT%max) of the maximum transmittance, the less likely residual color mixing is to occur, and the more desirable it is. A to C are ranges that are problem-free for use. In addition, for the examples other than B1 to B9, the coloring composition for color mixing evaluation was prepared by mixing 65 parts by mass of dispersion B9, 6 parts by mass of resin B-9, 2.8 parts by mass of polymerizable monomer M-2, 0.8 parts by mass of photopolymerization initiator G-3, 5 parts by mass of surfactant I-1, and 20.4 parts by mass of solvent K-1. In addition, for the examples B1 to B9, the coloring composition for color mixing evaluation was prepared by mixing the coloring composition of the example R1. [Evaluation Criteria] A: ΔT%max is 1.5% or less. B: ΔT%max is greater than 1.5% and less than or equal to 2.0%. C: ΔT%max is greater than 2.0% and less than 2.5%. D: ΔT%max is greater than 2.5%.

[0256] The results are shown in the table below.

[0257] [Table 12] [Table 13] [Table 14]

[0258] As shown in the above table, in the examples, even after the heat resistance test, the spectral variation was small and a film with little color unevenness could be formed.

[0259] In the evaluation of adhesion, the composition for forming the undercoat layer was changed from CT-4000 (manufactured by FUJIFILM Electronic Materials Co., Ltd.) to compositions 1 to 11 for forming the undercoat layer prepared as follows. These compositions for forming the undercoat layer were applied by spin coating to a film thickness of 3 nm, and heated at 220°C for 5 minutes using a hot plate to form an undercoat layer. Even when adhesion was evaluated using the same procedure on the silicon wafer with the obtained undercoat layer using the coloring composition of each example, the same effects as those of each example were obtained.

[0260] [Table 15]

[0261] (resin) Resin C-1: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio; weight average molecular weight: 20,000) in PGMEA Resin C-2: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio; weight-average molecular weight: 25,000) in PGMEA Resin C-3: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio; weight-average molecular weight: 20,000) in PGMEA Resin C-4: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio. Weight average molecular weight: 15,000) in PGMEA Resin C-5: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio; weight-average molecular weight: 20,000) in PGMEA Resin C-6: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio; weight-average molecular weight: 22,000) in PGMEA Resin C-7: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio; weight-average molecular weight: 23,000) in PGMEA Resin C-8: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio; weight-average molecular weight: 22,000) in PGMEA Resin C-9: 30% by mass solution of a resin having the following structure (the number attached to the main chain is the molar ratio. Weight average molecular weight: 13,000) in PGMEA Resin C-10: 30% by mass solution of the resin (weight average molecular weight 15,000) having the following structure in PGMEA [ka] [ka]

[0262] (Surfactant) Surfactant 1: A compound having the following structure (weight average molecular weight: 14,000; % indicating the proportion of repeating units is mol %) [ka] Surfactant 2: KF6001 (Shin-Etsu Chemical Co., Ltd., siloxane surfactant)

[0263] (solvent) Solvent 1: Propylene glycol monomethyl ether acetate (PGMEA)

[0264] (Example 1001) The green colored composition was applied onto a silicon wafer by spin coating so that the film thickness after formation was 1.0 μm. Then, the wafer was heated at 100° C. for 2 minutes using a hot plate. Then, an i-line stepper exposure apparatus FPA-3000i5+ (manufactured by Canon Inc.) was used to apply 1000 mJ / cm 2The green colored composition was patterned by heating at 200°C for 5 minutes using a hot plate to form green pixels. The red colored composition and the blue colored composition were patterned by the same process to sequentially form red and blue pixels, thereby forming a color filter having green, red and blue pixels. In this color filter, the green pixels are formed in a Bayer pattern, and the red and blue pixels are formed in an island pattern in the adjacent area. The obtained color filter was incorporated into a solid-state imaging device according to a known method. This solid-state imaging device had suitable image recognition ability. The green colored composition was the colored composition of Example G1. The red colored composition was the colored composition of Example R1. The blue colored composition was the colored composition of Example B1.

[0265] (Example 1002) A cyan coloring composition was applied onto a silicon wafer by spin coating so that the film thickness after formation was 1.0 μm. Then, the wafer was heated at 100° C. for 2 minutes using a hot plate. Then, an i-line stepper exposure apparatus FPA-3000i5+ (manufactured by Canon Inc.) was used to expose the wafer at 1000 mJ / cm 2The exposure was performed through a mask with a dot pattern of 2 μm square at an exposure dose of 1000 μm. Then, paddle development was performed at 23° C. for 60 seconds using a 0.3% by mass aqueous solution of tetramethylammonium hydroxide (TMAH). After that, rinsing was performed with a spin shower and further washed with pure water. Next, the cyan coloring composition was patterned by heating at 200° C. for 5 minutes using a hot plate to form cyan color pixels. The yellow coloring composition and the magenta coloring composition were also patterned by the same process to sequentially form yellow and magenta color pixels, thereby forming a color filter having cyan, yellow and magenta color pixels. In this color filter, the cyan color pixels are formed in a Bayer pattern, and in the adjacent areas, the yellow and magenta color pixels are formed in an island pattern. The obtained color filter was incorporated into a solid-state imaging device according to a known method. This solid-state imaging device had suitable image recognition ability. The coloring composition of Example C1 was used as the cyan coloring composition. The coloring composition of Example Y1 was used as the yellow coloring composition. As the magenta coloring composition, the coloring composition of Example M1 was used.

Claims

1. A coloring composition comprising a coloring material containing an organic pigment, a resin, and a compound A in which a phenolic hydroxy group of a phenolic antioxidant is protected with a protecting group that can be removed by heating, The coloring composition contains the color material in an amount of 40% by mass or more based on the total solid content of the coloring composition, The coloring composition contains 2.5 to 10 mass% of the compound A in the total solid content, and contains 5.5 to 25 mass parts of the compound A relative to 100 mass parts of the organic pigment, The coloring composition, wherein the resin contains a graft resin having an acid group, and the content of the graft resin is 300 to 2000 parts by mass with respect to 100 parts by mass of the compound A.

2. The coloring composition according to claim 1 , wherein the organic pigment comprises at least one selected from the group consisting of a green pigment, a yellow pigment, and a red pigment.

3. The coloring composition according to claim 1 or 2, wherein the organic pigment comprises a green pigment, and the green pigment comprises a phthalocyanine compound.

4. The colored composition according to any one of claims 1 to 3, wherein the graft resin has an acid value of 20 to 150 mgKOH / g.

5. The colored composition according to any one of claims 1 to 4, wherein the graft resin has a weight average molecular weight of 3,000 to 35,000.

6. The colored composition according to any one of claims 1 to 5, further comprising a photopolymerization initiator and a polymerizable compound.

7. The colored composition according to claim 6 , wherein the photopolymerization initiator comprises an oxime compound having an aromatic ring group in which an electron-withdrawing group is introduced into the aromatic ring.

8. The coloring composition according to any one of claims 1 to 7, further comprising a phenolic antioxidant.

9. A film obtained by using the colored composition according to any one of claims 1 to 8.

10. A color filter comprising the film of claim 9.

11. A solid-state imaging device comprising the film according to claim 9 .

12. An image display device comprising the film according to claim 9.

Citation Information

Patent Citations

  • Pigment dispersion composition, colored curable composition, color filter, liquid crystal display device, and solid-state image sensor

    JP2010211200A

  • Coloring compositions

    JP2015131937A

  • Photosensitive composition

    JP2016038569A

  • Composition

    WO2017030005A1