Zn-al-mg-based hot-dip plated steel member
Patent Information
- Application Number
- MYPI2025004217
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-09
- Filing Date
- 2024-02-09
- Publication Date
- 2024-08-09
AI Technical Summary
Existing Zn-Al-Mg hot-dip galvanized steel members face challenges in achieving a well-balanced improvement in corrosion resistance, adhesion of the chemical conversion treatment layer, weldability, and appearance, particularly in reducing the conspicuousness of scratches and enhancing conductivity during electric resistance welding.
A Zn-Al-Mg hot-dip plated steel member with a hot-dip plating layer composition of 4-22% Al, 1.0-10% Mg, and specific trace elements, where the surface is treated with a cooling device using oxygen-enriched air to promote surface oxidation and binarization using Otsu's method to achieve a satin-like appearance with a controlled ratio of white and glossy areas, enhancing adhesion and corrosion resistance.
The solution results in a steel member with excellent corrosion resistance, improved adhesion of the chemical conversion treatment layer, enhanced conductivity for welding, and a reduced visibility of scratches, achieving a balanced set of properties for industrial applications.
Smart Images

Figure PI2025004217_DRAWING_001 
Figure PI2025004217_DRAWING_002
Abstract
Description
Zn-Al-Mg hot-dip plated steel members
[0001] The present invention relates to a Zn-Al-Mg hot-dip coated steel member. This application claims priority to Japanese Patent Application No. 2023-018261, filed on February 9, 2023, the contents of which are incorporated herein by reference.
[0002] Hot-dip galvanized steel sheets are a type of steel material with excellent corrosion resistance. Hot-dip galvanized steel sheets, a typical example of hot-dip galvanized steel materials, are widely used in various manufacturing industries, including automobiles, home appliances, and building materials.
[0003] For the purpose of further improving the corrosion resistance of hot-dip galvanized steel members, Zn-Al-Mg-based hot-dip galvanized steel members have been proposed in which Al or Mg is contained in the hot-dip galvanized layer. Techniques for improving the appearance of the coated surface of Zn-Al-Mg-based hot-dip galvanized steel members have also been proposed.
[0004] Patent Document 1 describes a hot-dip Zn-based plated steel sheet containing Mg, Al, and Zn and having antiglare properties. Patent Document 2 describes a Zn-Al-Mg hot-dip plated steel sheet having a fine texture and a pear-like finish with many smooth glossy portions. Patent Document 3 describes a hot-dip plated steel sheet containing Mg, Al, and Zn and having excellent appearance quality.
[0005] Japanese Patent Publication No. 2015-193881 International Publication No. 2011 / 001662 Japanese Patent Publication No. 2004-143505
[0006] The hot-dip galvanized steel sheets described in Patent Documents 1 to 3 are technologies related to appearance, but in recent years, in addition to improved appearance, there has been a growing need for further improved corrosion resistance and improved adhesion of chemical conversion coating layers to enhance corrosion resistance. Furthermore, in order to improve weldability in electric resistance welding such as spot welding, improved conductivity when in contact with a welding electrode is also required. Thus, hot-dip galvanized steel members are required to have a balanced improvement in these properties.
[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a Zn-Al-Mg hot-dip coated steel member that has excellent corrosion resistance and adhesion of a chemical conversion coating layer, excellent electrical conductivity with a welding electrode even when a chemical conversion coating layer is formed, and an excellent appearance in which scratches are less noticeable.
[0008] In order to solve the above problems, the present invention employs the following configuration. [1] A Zn-Al-Mg based hot-dip coated steel member according to one aspect of the present invention comprises a steel member and a hot-dip coated layer disposed on a surface of the steel member, wherein the hot-dip coated layer has an average composition, in mass %, of Al: 4-22%, Mg: 1.0-10%, Fe: 0.0001-2%, Si: 0-2%, Ni: 0-2%, Ti: 0-2%, Zr: 0-2%, Sr: 0-2%, Sb: 0-2%, Pb: 0-2%, Sn: 0-2%, Ca: 0-2%, Co: 0-2%, Mn: 0-2%, P: 0-2%, B: 0-2%, Bi: 0-2%, Cr: 0-2%, Sc: 0-2%, Y: 0-2%, REM: 0-2%,
[0014]
[0015]
[0016]
[0017]
[0018]
[0019]
[0020]
[0021]
[0022]
[0023]
[0024]
[0025]
[0026]
[0027]
[0028]
[0029]
[0030]
[0031]
[0032]
[0033]
[0034]
[0035]
[0036]
[0037]
[0038]
[0039]
[0040]
[0041]
[0042]
[0043]
[0044]
[0050]
[0051]
[0052]
[0053]
[0054]
[0055]
[0056]
[0057]
[0058]
[0059]
[0060]
[0061]
[0062]
[0063]
[0064]
[0065]
[0066]
[0070]
[0071]
[0072]
[0073]
[0074]
[0075]
[0076]
[0077]
[0078]
[0079]
[0080]
[0081]
[0082]
[0083]
[0084]
[0085]
[0086]
[0087]
[0088]
[0089]
[0090]
[0091]
[0092]
[0093]
[0094]
[0095]
[0096]
[0097]
[0098]
[0099]
[0099]
[0099]
[0099]
[0099]
[0099]
[0099]
[0099] [ [4] In the Zn-Al-Mg-based hot-dip plated steel member described in [1] above, the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered may be 150 or less, and the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where black pixels are gathered may be 1.5 times or more the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered. [5] In the Zn-Al-Mg-based hot-dip plated steel member described in [2] above, the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered may be 150 or less, and the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where black pixels are gathered may be 1.5 times or more the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered.[6] In the Zn-Al-Mg-based hot-dip plated steel member according to the above item [1], the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered may be 70 or less, and the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where black pixels are gathered may be 1.5 times or more the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered. [7] In the Zn-Al-Mg-based hot-dip plated steel member according to any of the above items [1] to [6], the hot-dip plated layer may contain, in an average composition, one or more elements selected from the following Group A, Group B, and Group C: Group A: Si: 0.0001 to 2 mass% Group B: One or more of Ni, Ti, Zr, and Sr, in a total of 0.0001 to 2 mass% Group C: One or more of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C, in a total of 0.0001 to 2 mass% [8] In the Zn-Al-Mg hot-dip galvanized steel member described in [5] above, the average composition of the hot-dip galvanized layer may contain the Group A element. [9] In the Zn-Al-Mg hot-dip galvanized steel member described in [5] above, the average composition of the hot-dip galvanized layer may contain the Group B element.
[10] In the Zn-Al-Mg hot-dip galvanized steel member described in [5] above, the average composition of the hot-dip galvanized layer may contain the Group C element.
[0009] According to the present invention, it is possible to provide a Zn-Al-Mg hot-dip coated steel member which has excellent corrosion resistance and adhesion of a chemical conversion coating layer, excellent electrical conductivity with a welding electrode even when a chemical conversion coating layer is formed, and further has an excellent appearance in which scratches are less noticeable.
[0010] Fig. 1 is a schematic diagram illustrating a method for producing a Zn—Al—Mg-based hot-dip coated steel member. Fig. 2 shows image data illustrating regions of white and black pixels, which are binary image data obtained by binarizing image data of an image of the surface of a hot-dip coated layer using Otsu's binarization method.
[0011] The hot-dip coating layer of a Zn-Al-Mg-based hot-dip coated steel member has a matte appearance. The matte appearance is caused by the mixture of fine white areas and glossy areas on the surface of the hot-dip coating layer. The white areas have a relatively large surface roughness, which causes incident light to be diffusely reflected, resulting in a white or near-white appearance. On the other hand, the glossy areas have a relatively small surface roughness, which makes it difficult for incident light to be diffusely reflected, resulting in a metallic luster or a form near metallic luster. The increased number of white areas makes scratches less noticeable.
[0012] When a chemical conversion coating layer is formed on a hot-dip coated layer, it is generally formed so that the surface height of the chemical conversion coating layer is approximately uniform throughout the entire hot-dip coated layer. In this case, if the hot-dip coated layer has many white areas, the surface roughness of the hot-dip coated layer increases overall, resulting in an anchor effect that enhances the adhesion of the chemical conversion coating layer. Furthermore, because the surface roughness of the hot-dip coated layer is high, the chemical conversion coating layer tends to be formed relatively thick, which also tends to improve the corrosion resistance of the hot-dip coated layer. On the other hand, if the hot-dip coated layer has many shiny areas, the surface roughness of the entire hot-dip coated layer decreases, allowing the chemical conversion coating layer to be formed relatively thin. As a result, when a welding electrode is pressed against a hot-dip coated steel sheet, the conductivity between the welding electrode and the hot-dip coated layer is improved. Therefore, a hot-dip coated layer with many shiny areas has improved weldability in electric resistance welding, such as spot welding.
[0013] From the above, it is believed that if it were possible to adjust the ratio of white to shiny areas in the hot-dip galvanized layer within an appropriate range, it would be possible to achieve an excellent appearance with less noticeable scratches, corrosion resistance of the hot-dip galvanized layer, adhesion between the hot-dip galvanized layer and the chemical conversion coating layer, and conductivity between the hot-dip galvanized layer and the welding electrode. However, it has been difficult to obtain a hot-dip galvanized layer that satisfies all of these requirements.
[0014] The inventors further investigated the possibility of forming a hot-dip galvanized layer on the surface of a steel member, such as a steel sheet, by spraying an oxygen-added air refrigerant from a cooling device equipped with multiple spray nozzles. The inventors discovered that spraying the refrigerant from a select number of nozzles, rather than simultaneously from all nozzles, while randomly switching the nozzles spraying the refrigerant, simultaneously achieves excellent appearance with less noticeable scratches, corrosion resistance, adhesion to the chemical conversion coating layer, and conductivity with the welding electrode. Furthermore, the inventors discovered that when a digital image of a hot-dip galvanized layer with this characteristic is binarized using a binarization method known as the "Otsu binarization method," a binarized image containing both white and black pixels has a total area ratio of white pixels within a predetermined range. That is, a plated steel sheet in which the total area ratio of white pixels in the binarized image is within a predetermined range can simultaneously satisfy the following: an excellent appearance in which scratches are less noticeable; corrosion resistance; adhesion to the chemical conversion coating layer; and conductivity with the welding electrode.
[0015] The Zn-Al-Mg hot-dip galvanized steel member of this embodiment will be described below. The Zn-Al-Mg hot-dip galvanized steel member of this embodiment (hereinafter referred to as the hot-dip galvanized steel member) comprises a steel member and a hot-dip galvanized layer disposed on the surface of the steel member. The hot-dip galvanized layer has an average composition, in mass %, of 4 to 22% Al, 1.0 to 10% Mg, and 0.0001 to 2% Fe, with the remainder comprising Zn and impurities. In binary image data obtained by capturing an image of the surface of the hot-dip galvanized layer, the total area ratio of white pixels is 30% to 70%. The hot-dip galvanized steel member of this embodiment may further comprise a chemical conversion layer on the surface of the hot-dip galvanized layer. Furthermore, in binary image data obtained by capturing an image of the surface of the hot-dip galvanized layer from above the chemical conversion layer, the total area ratio of white pixels is 30% to 70%. The hot-dip galvanized steel member may have a metallic appearance.
[0016] The steel member that serves as the substrate for the hot-dip coating layer is, for example, a steel plate, a steel material, or a member obtained by processing these, but there is no particular limitation on the material. As will be described in detail later, general steel and the like can be used as the material of the steel member without any particular limitation, and Al-killed steel and some high-alloy steels can also be applied. There is no particular limitation on the shape of the steel member. The hot-dip coating layer according to this embodiment is formed by applying the hot-dip coating method described later to the steel member. The hot-dip coating layer is formed on the surface of the steel member. That is, when the steel member is a steel plate, the hot-dip coating layer is formed on both sides of the steel plate. Note that the steel member includes not only steel plates and steel materials, but also members obtained by processing these. The steel member may be, for example, a steel product used in the fields of automobiles, home appliances, building materials, etc.
[0017] Next, the chemical components of the hot-dip galvanized layer will be described. The hot-dip galvanized layer has an average composition, in mass %, of 4 to 22% Al, 1.0 to 10% Mg, and 0.0001 to 2% Fe, with the balance being Zn and impurities. The hot-dip galvanized layer may also have an average composition, in mass %, of 4 to 22% Al, 1.0 to 10% Mg, and 0.0001 to 2% Fe, with the balance being Zn and impurities.
[0018] The hot-dip galvanized layer may contain, in its average composition, one or more elements selected from the following Group A, Group B, or Group C. In the chemical composition of the hot-dip galvanized layer, the lower limit of each element in Group A, Group B, or Group C may be 0% or may exceed 0%. The hot-dip galvanized layer may contain, in its average composition, 4 to 22% Al, 1.0 to 10% Mg, and 0.0001 to 2% Fe, and may further contain one or more elements selected from the following Group A, Group B, or Group C, with the balance being Zn and impurities.
[0019] Group A: Si: 0.0001 to 2 mass% Group B: Ni, Ti, Zr, Sr, any one or more of which are 0.0001 to 2 mass% in total Group C: Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, C, any one or more of which are 0.0001 to 2 mass% in total
[0020] The composition of the hot-dip coating layer can be measured using the following method. First, a 50 mm x 50 mm rectangular area 50 mm from the edge of the hot-dip coated steel sheet is cut to obtain a sample, free of obvious defects such as corrosion. Next, the surface coating layer and chemical conversion coating layer are removed from the sample using a coating remover that does not corrode the coating layer (e.g., Neo River SP-751 manufactured by Sansai Kako Co., Ltd.). If the surface coating layer and chemical conversion coating layer cannot be sufficiently removed, they can be removed by polishing with an abrasive that is softer than the coating layer. The hot-dip coating layer is then dissolved by immersing the sample in 5% hydrochloric acid containing an inhibitor (e.g., Hibilon manufactured by Sugimura Chemical Industry Co., Ltd.). The composition of the hot-dip coating layer can be determined by inductively coupled plasma (ICP) atomic emission spectroscopy. However, for silicon, which cannot be accurately analyzed using the above method, the resulting solution can be further treated with the acid decomposition / sodium carbonate fusion method based on JIS G1258-3 and then analyzed to determine the Si content.
[0021] The Al content is 4 to 22 mass% in average composition. Al is an element necessary for ensuring corrosion resistance. If the Al content in the hot-dip coating layer is less than 4 mass%, the effect of improving corrosion resistance becomes insufficient, and if it exceeds 22 mass%, the effect of improving corrosion resistance becomes saturated. From the viewpoint of corrosion resistance, the Al content is preferably 5 to 20 mass%, and more preferably 6 to 20 mass%.
[0022] The Mg content is 1.0 to 10 mass% in average composition. Mg is an element necessary for improving corrosion resistance. If the Mg content in the hot-dip coating layer is less than 1.0 mass%, the effect of improving corrosion resistance is insufficient. If the Mg content in the hot-dip coating layer exceeds 10 mass%, significant dross is generated in the coating bath, making it difficult to stably produce hot-dip coated steel members. From the viewpoint of the balance between corrosion resistance and dross generation, the Mg content is preferably 1.5 to 8 mass%. The Mg content is more preferably 2.0 to 7.0 mass%.
[0023] The hot-dip plated layer may contain Si as an element of Group A in the range of 0.0001 to 2 mass%. Si is an element effective for improving the adhesion of the hot-dip plated layer. Since the effect of improving the adhesion of the hot-dip plated layer is achieved by containing 0.0001 mass% or more of Si, it is preferable to contain 0.0001 mass% or more of Si. On the other hand, even if the Si content exceeds 2 mass%, the effect of improving the plating adhesion saturates, so the Si content is 2 mass% or less. From the viewpoint of plating adhesion, the Si content is more preferably 0.0010 to 1 mass%, and even more preferably 0.0100 to 0.8 mass%. The Si content may be 0% or more.
[0024] The hot-dip coating layer may contain, as elements of group B, one or more of Ni, Ti, Zr, and Sr in an average composition in total of 0.0001 to 2 mass%. The average composition is more preferably 0.001 to 1 mass%, and even more preferably 0.002 to 0.10 mass%. By containing these elements of group B, corrosion resistance can be further improved. The contents of Ni, Ti, Zr, and Sr may be 0% or more than 0%.
[0025] The hot-dip coating layer may contain, as an element of group C, one or more of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in an average total amount of 0.0001 to 2 mass%. The average total amount is more preferably 0.001 to 1 mass%, and even more preferably 0.002 to 0.10 mass%. The inclusion of these elements of group C can further improve corrosion resistance. REM refers to one or more rare earth elements having atomic numbers 57 to 71 in the periodic table. The contents of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C may be 0% or greater than 0%.
[0026] The remainder of the chemical components of the hot-dip galvanized layer is zinc and impurities. Furthermore, when the hot-dip galvanized layer is formed, Fe (iron), a main component of the steel member, is mixed into the hot-dip galvanized layer. In the hot-dip galvanized layer of this embodiment, the Fe content is in the range of 0.0001 to 2 mass% in terms of average composition.
[0027] Next, the appearance of the hot-dip plated layer will be described. In the hot-dip plated layer according to this embodiment, when image data of the surface of the hot-dip plated layer is binarized using Otsu's binarization method to produce binary image data, the total area ratio of white pixels contained in the binary image data is 30% to 70%. When the steel member is a plate having an upper surface and a lower surface, such as a steel plate, the binary image data may be obtained by binarizing image data of the surface of the hot-dip plated layer, captured from one or both sides of the steel member (steel plate), using Otsu's binarization method.
[0028] Here, we will provide a supplementary explanation of "image data of the surface of the hot-dip galvanized layer, image data captured from one or both sides of the steel member (steel plate)." When the steel member is a steel plate, the hot-dip galvanized layer according to this embodiment is formed on the surface of the steel plate, i.e., on one side and the other side in the thickness direction of the steel plate. In such a case, the image data used in the binarization process may be data of an image of the surface of either one of the hot-dip galvanized layers arranged on one side and the other side, or may be data of an image of both surfaces of the hot-dip galvanized layers arranged on one side and the other side.
[0029] That is, the hot-dip galvanized steel member according to this embodiment only needs to satisfy the following: a total area ratio of white pixels contained in binarized image data obtained from image data of the surface of the hot-dip galvanized layer captured from one side of the steel member of 30% to 70%; a total area ratio of white pixels contained in binarized image data obtained from image data of the surface of the hot-dip galvanized layer captured from both sides of the steel member of 30% to 70%; and a flat portion of the steel member of 30% to 70%. When the shape of the hot-dip galvanized steel member according to this embodiment is not plate-like (for example, when it is a processed member), the flat portion of the steel member can be imaged to obtain the image data.
[0030] The photographed area for obtaining image data of the surface of the hot-dip coated layer is selected by cutting a rectangular area of 100 mm x 100 mm that is free of obvious defects such as corrosion and is located 50 mm away from the edge. If the hot-dip coated steel member is a processed product, a rectangular flat area of 100 mm x 100 mm located 50 mm away from the edge or processed portion is selected by cutting. If the photographed area is smaller than this, it becomes difficult to properly evaluate the appearance of the hot-dip coated layer. Furthermore, if the photographed area is larger than this, the amount of data increases and the processing time increases, which is not preferable.
[0031] A sample including the selected photographed area and its surroundings is cut out from the hot-dip galvanized steel member, and image data of the photographed area is obtained using this sample.
[0032] Image data is acquired by scanning the surface of the hot-dip coated layer of the sample with a scanner connected to a computer. The image data is extracted as image data with 256 grayscale levels at a resolution of 300 dpi (dots per inch), for example. A flatbed scanner is preferably used. If local brightness variations occur in the image data due to distortion of the steel member, etc., it is preferable to eliminate the local brightness variations by image correction.
[0033] Generally, image data can be extracted by taking a photograph with a camera. However, when taking a photograph with a camera, it is difficult to irradiate the entire hot-dip galvanized layer, which is the subject, with illumination light at the time of photographing completely and evenly, which may result in an inaccurate evaluation of the appearance pattern. Therefore, extraction of image data with a scanner is preferred.
[0034] The image data is assumed to be grayscale image data with 256 gradations. Image data includes color image data in addition to grayscale, but color image data has an excessive amount of information because each pixel carries color information. Since the surface appearance of the hot-dip galvanized layer in this embodiment has low saturation, grayscale image data is sufficient in terms of the amount of information. Therefore, in this embodiment, grayscale image data with 256 gradations, which has an appropriate amount of information and is easy to handle on a computer, is preferred.
[0035] The image data is preferably image data obtained using visible light as a light source, and is preferably not a secondary electron image or a backscattered electron image obtained by an electron microscope. Secondary electron images and backscattered electron images obtained by an electron microscope are convenient for observing minute surface shapes and differences in elemental composition, but provide no information on the color of an object. In contrast, the image data according to this embodiment, although grayscaled, can capture color information on the plating layer surface, reflecting the impression of observing the plating layer with the naked eye under visible light.
[0036] Next, the obtained image data is subjected to binarization processing using Otsu's binarization method to obtain binarized image data. The binarization processing using Otsu's binarization method can be performed by a computer with a pre-installed program.
[0037] Otsu's binarization method is generally known as a method for binarizing a grayscale image and selecting a threshold level to separate the target area from the background. Details of the method are described in the following document. The contents are briefly described below.
[0038] Nobuyuki Otsu, "Automatic Threshold Selection Method Based on Discrimination and Least Squares Criteria," Transactions of the Institute of Electronics and Communication Engineers, Vol. 63, No. 4, pp. 349-356, 1980
[0039] Consider a grayscale image with 256 levels (0 to 255). Let U be the entire set of pixels in the entire image. Using k in the range of 0 to 255 as a threshold, let A be the set of pixels with pixel values 0 to k, and let B be the set of pixels with pixel values k+1 to 255. Let N be the total number of U, A, and B, respectively. A , N B Let the average pixel values of U, A, and B be x and x A , x B Next, Y is defined as follows: In this case, the method of binarizing a grayscale image using k that maximizes Y is equivalent to Otsu's binarization method. The following Y corresponds to equation (16) in the above document.
[0040] Y = (N A / N) (x A -x) 2+ (N B / N) (x B -x) 2
[0041] In this embodiment, in the binarized image data after the binarization process, pixels included in set A of pixels having pixel values of 0 to k become black pixels, and pixels included in set B of pixels having pixel values of k+1 to 255 become white pixels. In the matte appearance, black pixels correspond to glossy parts, and white pixels correspond to white parts.
[0042] In this embodiment, the total area ratio of white pixels in the binary image data of the hot-dip coating layer must be in the range of 30% to 70%. If the total area ratio of white pixels is less than 30%, the area of black pixels becomes excessively large, i.e., the area of glossy parts becomes wider, and defects on the surface of the hot-dip coating layer become more noticeable. Furthermore, although the weldability of electric resistance welding such as spot welding is improved, the adhesion of the chemical conversion coating layer and the corrosion resistance of the hot-dip coating layer are reduced.
[0043] On the other hand, if the total area ratio of white pixels exceeds 70%, the white pixel region becomes excessively large, i.e., the white area becomes wider, and scratches become less noticeable. This improves the adhesion of the chemical conversion coating layer and the corrosion resistance of the hot-dip plating layer, but reduces the weldability of electric resistance welding such as spot welding. Therefore, the total area ratio of white pixels is preferably in the range of 30% to 70%. Such a hot-dip plating layer will have a matte appearance with a mixture of glossy and white areas. Furthermore, the hot-dip plating layer will have a metallic appearance with a metallic texture.
[0044] In the hot-dip plated layer according to this embodiment, the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are concentrated is 150 or less, preferably 70 or less. Furthermore, the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where black pixels are concentrated is preferably 1.5 times or more, more preferably 2.1 times or more, of the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are concentrated. When a chemical conversion coating layer that is transparent to visible light is formed on the hot-dip plated layer and removal of the chemical conversion coating layer is difficult, the gloss may be measured from above the chemical conversion coating.
[0045] A region of white pixels is a pixel region where white pixels are gathered in an area large enough to measure the 60-degree specular gloss Gs (60°) using a gloss meter. Specifically, as shown in FIG. 2 , a region of white pixels is a 3 mm square rectangular region containing 60% or more white pixels. In other words, if the area of white pixels in this 3 mm square rectangular region is 60% or more, this region is considered to be a region of white pixels. Similarly, a region of black pixels is a pixel region where black pixels are gathered, and as shown in FIG. 2 , this region is considered to be a 3 mm square rectangular region containing 60% or more black pixels. In other words, if the area of black pixels in this 3 mm square rectangular region is 60% or more, this region is considered to be a region of black pixels.
[0046] The 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where white pixels are gathered is preferably 150 or less, and more preferably 70 or less. This makes it possible to obtain an appearance with a calm and pleasant impression without excessively emphasizing the metallic luster. The lower limit of the 60-degree specular gloss Gs(60°) measured for the area where white pixels are gathered is not particularly limited, but may be 10 or more. Note that the "60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where white pixels are gathered" here refers to the average value of the 60-degree specular gloss Gs(60°) in each of the 10 areas where white pixels are gathered. The same applies to the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where black pixels are gathered.
[0047] Furthermore, in the hot-dip plated layer, the 60-degree specular gloss Gs (60°) of the surface of the hot-dip plated layer corresponding to a region where black pixels are collected is preferably at least 1.5 times the 60-degree specular gloss Gs (60°) of the surface of the hot-dip plated layer corresponding to a region where white pixels are collected. This makes it possible to clearly contrast the appearance of the white portion corresponding to the region where white pixels are collected and the gloss portion corresponding to the region where black pixels are collected, thereby creating a favorable impression of the surface pattern.
[0048] The 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer is measured using a glossmeter based on the method specified in JIS Z 8741. Specifically, the 60-degree gloss (%) is measured by the method specified in JIS Z 8741, and Gs(60°) is calculated based on the obtained gloss (%). When measuring the 60-degree specular gloss Gs(60°), that is, when identifying the areas where white pixels or black pixels are collected, the individual 3 mm square rectangular areas to be measured are set so that they do not overlap with each other.
[0049] Furthermore, the hot-dip plated steel member of this embodiment may be provided with a chemical conversion treatment layer on the surface of the hot-dip plated layer. The chemical conversion treatment layer does not have to be provided on the entire steel member; for example, in the case of a steel sheet, a chemical conversion treatment layer may be provided on both the hot-dip plated layers arranged on one side and the other side of the steel sheet. The type of chemical conversion treatment is not particularly limited, and any known chemical conversion treatment can be used, but in this case, the chemical conversion treatment layer is preferably a chemical conversion treatment layer that is transparent to visible light.
[0050] The hot-dip coating layer of a hot-dip coated steel member having a chemical conversion coating layer is obtained by binarizing image data of the surface of the hot-dip coating layer photographed from above the chemical conversion coating layer using Otsu's binarization method, and the total area ratio of white pixels contained in the binarized image data is 30% to 70%. In other words, the chemical conversion coating layer provided on the hot-dip coated steel member of this embodiment preferably does not affect the appearance of the surface of the hot-dip coating layer. A hot-dip coated steel member having such a chemical conversion coating layer has a metallic appearance. Furthermore, when a coating layer is formed on the surface of the hot-dip coating layer or the chemical conversion coating layer, a painting process is performed on the hot-dip coating layer or the hot-dip coated steel member after the chemical conversion coating layer is formed. The type of painting process is not particularly limited, and known painting processes can be used. In this case, the painting process is preferably a painting process that is transparent to visible light.
[0051] An example of the chemical conversion treatment layer according to this embodiment is one containing 20% by mass or more of a resin and 1 to 20% by mass of silica particles having a particle size of 5 to 200 nm. This chemical conversion treatment layer is obtained by applying an aqueous composition containing the resin and the silica particles to the hot-dip plated layer and drying it.
[0052] The resin contained in the chemical conversion treatment layer may be any common resin, such as polyolefin resin, fluororesin, acrylic resin, urethane resin, polyester resin, epoxy resin, or phenolic resin. These resins may be water-soluble resins, or may be resins (water-dispersible resins) that are originally water-insoluble but can be finely dispersed in water, such as emulsions or suspensions. In addition to water-soluble resins, this term also includes resins (water-dispersible resins) that are originally water-insoluble but can be finely dispersed in water, such as emulsions or suspensions. In particular, it is preferable to include one or more resins selected from polyolefin resins, fluororesins, acrylic resins, and phenolic resins, as these resins have excellent weather resistance.
[0053] The resin is preferably contained in the chemical conversion coating layer at a ratio of 20% by mass or more. By making the resin content 20% by mass or more, the chemical conversion coating layer itself does not become brittle, and the hot-dip plating layer can be stably coated. Note that the chemical conversion coating layer may contain components other than the resin, such as Nb compounds and phosphate compounds, in addition to the resin, silica particles, and pigment, and the resin content may be the remainder of these components.
[0054] Silica particles are added to improve the corrosion resistance of the chemical conversion coating layer. The silica particles preferably have an average particle size in the range of 5 to 200 nm. The silica particles are contained in the chemical conversion coating layer at a ratio of 1 to 20 mass %. By increasing the silica particle content to 1 mass % or more, improved corrosion resistance can be achieved. Furthermore, by increasing the silica particle content to 20 mass % or less, the chemical conversion coating layer itself does not become brittle, and the Zn-based plating layer can be stably coated. Since silica particles with an average particle size of less than 5 nm are difficult to obtain and chemical conversion coating layers containing silica particles with an average particle size of less than 5 nm are practically difficult to produce, the lower limit of the average particle size of the silica particles is set to 5 nm or more. Furthermore, if the average particle size of the silica particles exceeds 200 nm, the chemical conversion coating layer may become cloudy, impairing the metallic appearance of the hot-dip plating layer.
[0055] Generally, inorganic pigments such as silica particles have small particle sizes, and therefore may exist in the chemical conversion treatment layer in the form of secondary particles that are larger than the primary particle size. The particle size of these secondary particles (particles formed by agglomeration of inorganic pigments) will be referred to as the "secondary particle size" hereinafter. The silica particles in this embodiment may be a mixture of primary particles and secondary particles, and even if primary particles and secondary particles are mixed, the average particle size should be in the range of 5 to 200 nm.
[0056] In order to improve the corrosion resistance of the chemical conversion coating layer, titania particles, alumina particles, zirconia particles, etc. may be contained in addition to silica particles.
[0057] The chemical conversion coating layer may further contain either or both of an Nb compound and a phosphate compound. When an Nb compound or a phosphate compound is contained, the corrosion resistance of the Zn-based plating layer is improved.
[0058] As the Nb compound, a conventionally known niobium-containing compound can be used, for example, niobium oxide, niobic acid and its salts, fluoroniobate, fluorooxoniobate, etc. Among these, niobium oxide is preferred from the viewpoint of improving corrosion resistance.
[0059] Examples of phosphoric acid compounds include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid, and salts thereof; phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid), and salts thereof; and organic phosphoric acids such as phytic acid and salts thereof. The cation species of the salts is not particularly limited, and examples include Cu, Co, Fe, Mn, Sn, V, Mg, Ba, Al, Ca, Sr, Nb, Y, Ni, and Zn. These may be used alone, or two or more may be used in combination.
[0060] The Nb compound and the phosphate compound may be contained in the chemical conversion coating layer in a total amount of 0.5 to 30 mass %. If the amount is 0.5 mass % or more, the corrosion resistance is improved, and if the amount is 30 mass % or less, the chemical conversion coating layer does not become brittle and the Zn-based plating layer can be stably coated.
[0061] The coating weight of the chemical conversion coating layer on one side of the hot-dip plating layer is 0.1 to 15 g / m 2 It is preferable that the coating amount is 0.1 g / m 2 If the coating weight is 15 g / m or more, the coating weight of the chemical conversion coating layer becomes sufficient, the blackened portion on the surface of the hot-dip plating layer can be made less noticeable, and the corrosion resistance of the hot-dip plating layer can be improved. 2 If the coating amount is less than this, the reflection of light on the surface of the chemical conversion coating layer is reduced, and the metallic appearance of the surface of the hot-dip plated layer can be visually recognized. 2 is.
[0062] The chemical conversion coating layer may further contain at least one crosslinking agent selected from the group consisting of a silane coupling agent, a crosslinkable zirconium compound, and a crosslinkable titanium compound. These may be used alone or in combination of two or more.
[0063] The chemical conversion coating layer of the hot-dip plated steel member of this embodiment is not limited to the one described above, and it goes without saying that any known chemical conversion coating layer may be used, for example.
[0064] Next, a method for manufacturing a hot-dip galvanized steel member according to this embodiment will be described. Figure 1 shows a hot-dip galvanizing facility suitable for manufacturing the hot-dip galvanized steel member according to this embodiment. The hot-dip galvanizing facility shown in Figure 1 includes a hot-dip galvanizing bath 2, a sink roll 3 disposed in the hot-dip galvanizing bath 2, a pair of wiping nozzles 4 disposed above the hot-dip galvanizing bath 2, a cooling device 5 disposed above at least one of the pair of wiping nozzles 4, and a top roll 7 disposed above the cooling device 5. The cooling device 5 may be disposed above both of the pair of wiping nozzles 4.
[0065] The hot-dip galvanizing bath 2 contains, by mass%, 4 to 22% Al, 1.0 to 10% Mg, and the remainder Zn and impurities. The hot-dip galvanizing bath may also contain 0.0001 to 2% Si. The hot-dip galvanizing bath may also contain 0.0001 to 2% by mass of one or more of Ni, Ti, Zr, and Sr in total. The hot-dip galvanizing bath may also contain 0.0001 to 2% by mass of one or more of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in total. The temperature of the hot-dip galvanizing bath 2 varies depending on the composition, but is preferably in the range of 400 to 500°C. This is because a desired hot-dip galvanizing layer can be formed if the temperature of the hot-dip galvanizing bath 2 is within this range.
[0066] The cooling device 5 cools the hot-dip coating layer and has a plurality of cooling nozzles that spray a coolant toward the steel member. An example of the coolant is air to which oxygen has been added, such as 26% oxygen-74% nitrogen.
[0067] A method for manufacturing a hot-dip plated steel member using the manufacturing equipment of FIG. 1 will be described below. The hot-dip plated steel member according to this embodiment only needs to have a hot-dip plated layer on the surface of the steel member, and for example, the timing of processing the steel sheet is not important. That is, the hot-dip plated steel member according to this embodiment may be obtained by forming a hot-dip plated layer on the surface of a steel sheet / steel material to obtain a plated steel sheet / steel material, and then processing these. Alternatively, the hot-dip plated steel member according to this embodiment may be obtained by forming a hot-dip plated layer on the surface of a steel member that has been processed in advance. In the following description of the manufacturing method, a case will be described in which the steel member is a plate-shaped steel sheet. First, a hot-rolled steel sheet is manufactured, and if necessary, hot-rolled sheet annealing is performed. After pickling, the steel sheet is cold-rolled to obtain a cold-rolled sheet. The cold-rolled sheet is degreased, washed with water, and then annealed (cold-rolled sheet annealing).
[0068] Next, as shown in Figure 1, the annealed steel sheet 1 is immersed in a hot-dip galvanizing bath 2, and then the direction of travel is changed by a sink roll 3 and the steel sheet is pulled up vertically. Excess hot-dip coating adhering to the surface of the pulled-up steel sheet 1 is removed by spraying high-pressure gas such as air or nitrogen from a wiping nozzle 4 arranged above the hot-dip galvanizing bath 2 onto the surface of the pulled-up steel sheet 1.
[0069] The total coating weight of the hot-dip coating layer on both sides of the steel sheet is 30 to 600 g / m 2 It is preferable to adjust the amount of adhesion so that it is in the range of 30 g / m 2 If the coating weight is less than 600 g / m, the corrosion resistance of the hot-dip galvanized steel sheet will decrease, which is not preferable. 2 If the coating weight exceeds 1000 g / m2, the molten metal adhering to the steel sheet will drip, making it impossible to make the surface of the hot-dip coated layer smooth, which is not preferable. When the steel member is not in the form of a plate, the coating weight of the hot-dip coated layer should be 30 to 600 g / m2 in total for the entire steel member. 2 It is preferable to adjust it so that
[0070] Next, as shown in Fig. 1, the hot-dip plating layer adhered to the surface of the steel sheet 1 is cooled by a cooling device 5 equipped with a plurality of injection nozzles. At this time, the refrigerant is not injected from all the injection nozzles at the same time, but rather the injection nozzles from which the refrigerant is injected are switched randomly while the refrigerant is injected from some of the injection nozzles. An air refrigerant containing added oxygen, such as 26% oxygen-74% nitrogen, is injected from the injection nozzles.
[0071] In areas where the coolant is sprayed, surface oxidation of the hot-dip plated layer is promoted, making it easier for white areas to form. On the other hand, in areas where the coolant is not sprayed, the cooling rate of the hot-dip plated layer is slowed, making it easier for shiny areas to form. In this way, the desired hot-dip plated steel component can be obtained by randomly switching the spray nozzles that spray the coolant. It is preferable that multiple spray nozzles are arranged at 25 mm intervals. The spray nozzles are switched on and off at 0.1 second intervals, and are adjusted to spray coolant from 30 to 60% of all spray nozzles using random numbers. The coolant flow rate is adjusted so that the average cooling rate of the entire steel sheet is 5 to 20°C / s.
[0072] The above-mentioned cooling control for the hot-dip galvanized layer may be performed, for example, only on the hot-dip galvanized layer arranged on one side of the steel sheet, or may be performed on the hot-dip galvanized layers arranged on both one side and the other side of the steel sheet.
[0073] When a steel sheet is cooled after hot-dip galvanization, cooling is usually performed under the same conditions on one side and the other side of the steel sheet, so that the total area ratio of white pixels contained in the binarized image data obtained from image data captured from both sides of the steel sheet satisfies 30% to 70%. On the other hand, if cooling is performed on one side of the steel sheet under the above-mentioned preferred conditions and cooling is performed on the other side under conditions that deviate from the preferred conditions, the total area ratio of white pixels contained in the binarized image data obtained from image data captured from both sides of the steel sheet may satisfy 30% to 70%.
[0074] A chemical conversion treatment layer may be further formed on the cooled hot-dip plated layer. The coating method of the aqueous composition used to form the chemical conversion treatment layer involves applying the aqueous composition to the surface of the hot-dip plated layer to form a film. The coating method is not particularly limited, and commonly used methods such as roll coating, air spraying, airless spraying, and immersion can be appropriately used. The drying method after application of the aqueous composition may be any method such as hot air, induction heating, near infrared, or far infrared, or a combination of these may be used. The heating temperature of the coated object is 50 to 250°C, preferably 70 to 220°C.
[0075] According to the hot-dip galvanized steel member of this embodiment, in the binary image data obtained by binarizing image data of the surface of the hot-dip galvanized layer using Otsu's binarization method, the total area ratio of white pixels contained in the binary image data is 30% or more and 70% or less, so that the corrosion resistance of the hot-dip galvanized steel member and the adhesion of the chemical conversion coating layer are improved, the conductivity with the welding electrode is increased, and furthermore, an excellent appearance can be obtained.
[0076] Next, examples of the present invention will be described. In the following examples, the case where the steel member is a plate-shaped steel plate will be described as an example. After cold rolling, the steel plate was degreased and washed with water. Then, the steel plate was subjected to cold-rolled sheet annealing. After cold-rolled sheet annealing, the steel plate was immersed in a hot-dip galvanizing bath and then pulled out. The coating weight was then adjusted by gas wiping, and the steel plate was further cooled to form a hot-dip galvanized layer on the steel plate. In this manner, samples No. 1 to 110 (hot-dip galvanized steel members) shown in Tables 1A to 3C were produced.
[0077] Furthermore, for some samples, a chemical conversion treatment layer was formed on the surface of the hot-dip plated layer after the formation of the hot-dip plated layer. The method for coating the aqueous composition used to form the chemical conversion treatment layer was to apply the aqueous composition to the surface of the hot-dip plated layer by roll coating. Drying after application was performed by hot air drying. The heating temperature of the coated object was 50 to 250°C. The chemical conversion treatment layer contained 20 mass % or more of resin and 1 to 20 mass % of silica particles with a particle size of 5 to 200 nm. The deposition amount of the chemical conversion treatment layer was 0.1 to 15 g / m 2 The formed chemical conversion coating layers, except for No. 97, were colorless and transparent when observed visually.
[0078] The composition of the hot-dip coating layer was measured using the following method. First, a 50 mm x 50 mm rectangular area was cut from the hot-dip coated steel member, 50 mm from the edge, and free of obvious defects such as corrosion. Next, the surface coating and chemical conversion coating layer were removed from the sample using a coating remover (Neoliver SP-751, manufactured by Sansai Kako Co., Ltd.) that does not corrode the coating. If the surface coating and chemical conversion coating layers could not be sufficiently removed, they were removed by polishing with an abrasive that was softer than the coating layer. The hot-dip coating layer was then dissolved by immersing the sample in 5% hydrochloric acid containing an inhibitor (Hibilon, manufactured by Sugimura Chemical Industry Co., Ltd.). The resulting solution was subjected to inductively coupled plasma (ICP) atomic emission spectroscopy to determine the composition of the hot-dip coating layer. However, for Si, which could not be accurately analyzed using the above method, the resulting solution was further treated with the acid decomposition / sodium carbonate fusion method based on JIS G1258-3 before analysis. The average composition of the hot-dip plated layer was almost the same as the composition of the hot-dip plating bath except for Fe. The Fe content of the hot-dip plated layer was 0.0001 to 2 mass % in all examples.
[0079] Cooling after gas wiping was performed using a cooling device with multiple cooling nozzles that sprayed a coolant toward one side and the other side of the steel sheet. The spray nozzles were arranged at 25 mm intervals. The coolant used was air with oxygen added to it, resulting in a gas with a composition of 26% oxygen and 74% nitrogen. Cooling was performed by spraying the coolant from some of the nozzles simultaneously, rather than from all the nozzles at the same time, while randomly switching the nozzles spraying the coolant. The spray nozzles were switched on and off at 0.1 second intervals, and random numbers were used to randomly switch the nozzles so that the coolant was sprayed from 30 to 60% of the nozzles. The coolant flow rate was adjusted so that the average cooling rate of the entire steel sheet was 5 to 20°C / s.
[0080] However, for Nos. 103 and 109, cooling after gas wiping was performed under conventional conditions. That is, air without additional oxygen was used as the coolant. In addition, the spray nozzle was not randomly turned on and off. The coolant flow rate was adjusted so that the average cooling rate of the entire steel sheet was 5 to 20°C / s.
[0081] For Nos. 104 and 110, cooling was performed using a gas obtained by adding oxygen to air to achieve a composition of 26% oxygen and 74% nitrogen. Cooling was performed by spraying the coolant from some of the spray nozzles at the same time, rather than spraying the coolant from all of the spray nozzles at the same time, while randomly switching the spray nozzles spraying the coolant. The spray nozzles were switched on and off at 0.1 second intervals, and random numbers were used to randomly switch the spraying of the coolant from 80% of the spray nozzles. The coolant flow rate was adjusted so that the average cooling rate of the entire steel sheet was 5 to 20°C / s.
[0082] Furthermore, in No. 97, a white pigment was added to the above-mentioned chemical conversion coating layer to make it opaque. Furthermore, for No. 97, the total area ratio of white pixels and glossiness were evaluated before the formation of the chemical conversion coating layer, and after the formation of the chemical conversion coating layer, the corrosion resistance, adhesion, and conductivity, as described below, were evaluated. Evaluation of appearance and conspicuousness of scratches were omitted.
[0083] A rectangular area with a side length of 100 mm was set as the imaging area for the hot-dip plating layer on one side of the obtained hot-dip plated steel member. A sample including the set imaging area and its surroundings was cut out from the hot-dip plated steel member. Then, image data was obtained by scanning the surface of the hot-dip plating layer of the cut-out sample with a flatbed scanner connected to a computer. For samples having a chemical conversion coating layer, image data was obtained by scanning from above the chemical conversion coating layer. The image data was extracted as image data with a grayscale of 256 gradations at a resolution of 300 dpi. If local brightness variations occurred in the image data, the local brightness variations were eliminated by image correction.
[0084] Next, the obtained image data was subjected to binarization processing using the Otsu binarization method described above to obtain binarized image data. The binarization processing using the Otsu binarization method was performed using a computer with a pre-installed program. The total area ratio of white pixels in the binarized image data was then calculated. The results are shown in Tables 2A to 2C.
[0085] (Metal Appearance) The metal appearance was evaluated by showing the surface of the hot-dip plated layer of the hot-dip plated steel member to five panelists and judging the appearance of the surface. That is, the metal appearance was evaluated based on whether each panelist could visually recognize the metal appearance of the plated layer surface. The evaluation was based on the following scoring system, with a score of 3 or 2 being considered a pass. The results are shown in Tables 3A to 3C.
[0086] 3: Three or more people out of five could see the metallic appearance of the plating. 2: Two people out of five could see the metallic appearance of the plating. 1: One or less people out of five could see the metallic appearance of the plating.
[0087] (60° Specular Gloss Gs (60°)) Using a glossmeter, the 60° gloss (%) was measured for each of the areas corresponding to the aggregated regions of white pixels and the areas corresponding to the aggregated regions of black pixels of the hot-dip plated layer, based on the method specified in JIS Z 8741. The 60° specular gloss Gs (60°) was calculated from the obtained 60° gloss (%) based on the description in JIS Z 8741.
[0088] The white pixel aggregation region was a rectangular region measuring 3 mm square, where the area ratio of white pixels in the binarized image data was 60% or more. The black pixel aggregation region was a rectangular region measuring 3 mm square, where the area ratio of black pixels in the binarized image data was 60% or more.
[0089] (Appearance Evaluation) Furthermore, the inconspicuousness of scratches was evaluated visually. The plating appearance was evaluated visually. Specifically, after scratching the surface of the plating layer, if the scratch was not visible from a distance of 2 m, the inconspicuousness of the scratches was judged to be good and rated as F. On the other hand, if the scratch was visible even from a distance of 2 m, the inconspicuousness of the scratches was deemed insufficient and rated as P. F was considered to be pass.
[0090] (Corrosion Resistance) The corrosion resistance of the hot-dip galvanized steel members was evaluated by corrosion weight loss after a CCT test. The hot-dip galvanized steel members were cut into 150 x 70 mm pieces, and the corrosion weight loss after 30 cycles of CCT was investigated using a CCT in accordance with JASO-M609. Corrosion weight loss of 30 g / m 2 If it is less than F, corrosion weight loss is 30g / m 2 50g / m or more 2 If it is less than G, corrosion weight loss is 50g / m 2 The above cases were rated as P, and F and G were judged as pass. The results are shown in Tables 3A to 3C. When a chemical conversion coating layer was present, it was removed before evaluating corrosion resistance.
[0091] (Adhesion) The adhesion of the chemical conversion coating layer was evaluated as follows. First, the test piece was immersed in boiling water for 30 minutes, and then a grid of cuts was made on the surface of the test piece at 1 mm intervals, and the percentage of cuts where the chemical conversion coating layer remained unpeeled (number of remaining cuts / number of cuts (100)) was investigated. In other words, the adhesion of the chemical conversion coating layer was evaluated based on the percentage of the 100 grid cuts where no peeling of the chemical conversion coating layer was observed. Peeling of the chemical conversion coating layer was observed with a scanning electron microscope. The evaluation criteria for adhesion were as follows, with F and G being judged as passing. <Evaluation criteria> F = 95% or more G = 90% or more but less than 95% P = less than 90%
[0092] (Electrical Conductivity) Electrical conductivity was evaluated as follows: First, a test piece was cut out from a hot-dip plated steel member on which a chemical conversion coating layer was formed, and the interlaminar resistance value (Ω cm ) of the obtained test piece was measured in accordance with the method for measuring surface insulation resistance specified in JIS C 2550:2019. 2 The test voltage was 0.5 V, the measurement current range was 0 to 1 A, and the contact area of the 10 contact electrodes was 1 cm 2 x 10 pieces, test pressure 2N / mm 2 ±5%. The interlayer resistance was 5 Ω cm 2 Less than P, Ω cm 2 7Ω・cm or more 2 Less than G, 7 Ω cm 2 The above was rated F.
[0093] As shown in Tables 1A to 3C, Nos. 1 to 48 are examples in which no chemical conversion coating layer was formed. For Nos. 1 to 48, the chemical components of the hot-dip plating layer satisfied the range of the present invention, and the manufacturing conditions were within the preferred range. As a result, the total area ratio of white pixels was in the range of 30 to 70%, and the samples exhibited a good appearance. They also had excellent corrosion resistance.
[0094] As shown in Tables 1B to 3C, Nos. 49 to 98 were coated with a chemical conversion coating. Because the chemical composition of the hot-dip coating layer for Nos. 49 to 98 satisfied the ranges of the present invention and the manufacturing conditions were within the preferred ranges, the total area ratio of white pixels was in the range of 30 to 70%, resulting in a good appearance. They also had excellent corrosion resistance. Furthermore, the chemical conversion coating layer had excellent adhesion, and the low interlayer resistance provided good conductivity with the welding electrode, resulting in excellent weldability.
[0095] No. 99 to 102 were not coated with a chemical conversion coating layer. No. 99 to 102 had a chemical composition outside the range of the present invention, and therefore exhibited reduced corrosion resistance.
[0096] No chemical conversion coating layer was formed in No. 103. Although the chemical composition of the hot-dip plating layer in No. 103 satisfied the range of the present invention, the cooling conditions after hot-dip plating were conventional cooling conditions, so the total area ratio of white pixels was less than 30%, and scratches were easily noticeable.
[0097] No chemical conversion coating layer was formed in No. 104. Although the chemical composition of the hot-dip plating layer in No. 104 satisfied the range of the present invention, the cooling conditions after hot-dip plating were outside the preferred cooling conditions, so the total area ratio of white pixels exceeded 70%, failing to achieve a metallic appearance and resulting in a deterioration in appearance.
[0098] A chemical conversion coating layer was formed on Nos. 105 to 108. In Nos. 105 to 108, the chemical composition of the hot-dip plated layer was outside the range of the present invention, and therefore the corrosion resistance was reduced.
[0099] No. 109 was a specimen in which a chemical conversion coating layer was formed. Although the chemical composition of the hot-dip coating layer of No. 109 satisfied the range of the present invention, the cooling conditions after hot-dip coating were conventional cooling conditions, so the total area ratio of white pixels was less than 30%, making scratches more noticeable. In addition, the adhesion of the chemical conversion coating layer was reduced.
[0100] No. 110 was formed with a chemical conversion coating layer. Although the chemical composition of the hot-dip plating layer of No. 110 satisfied the range of the present invention, the cooling conditions after hot-dip plating were outside the preferred cooling conditions, so the total area ratio of white pixels exceeded 70%, and a metallic appearance was not obtained, resulting in a deterioration in appearance. In addition, the electrical conductivity was reduced, and the weldability was poor.
[0101]
[0102]
[0103]
[0104]
[0105]
[0106]
[0107]
[0108]
[0109]
[0110] The Zn-Al-Mg hot-dip plated steel member of the present disclosure has excellent corrosion resistance and adhesion of a chemical conversion coating layer, and even when a chemical conversion coating layer is formed, has excellent electrical conductivity with a welding electrode, and further has an excellent appearance in which scratches are less noticeable, and therefore has high industrial applicability.
[0111] 1... Steel plate 2... Hot-dip galvanizing bath 3... Sink roll 4... Wiping nozzle 5... Cooling device
Claims
1. A steel member and a hot-dip coating layer disposed on a surface of the steel member, the hot-dip coating layer having an average composition, in mass%, of Al: 4-22%, Mg: 1.0-10.0%, Fe: 0.0001-2%, Si: 0-2%, Ni: 0-2%, Ti: 0-2%, Zr: 0-2%, Sr: 0-2%, Sb: 0-2%, Pb: 0-2%, Sn: 0-2%, Ca: 0-2%, Co: 0-2%, Mn: 0-2%, P: 0-2%, B: 0-2%, Bi: 0-2%, Cr: 0-2%, Sc: 0-2%, Y: 0-2%, REM: 0-2%, Hf: 0-2%, and C. : 0 to 2% with the remainder containing Zn and impurities, wherein a total area ratio of white pixels is 30% or more and 70% or less in binary image data of image data obtained by capturing an image of a surface of the said hot-dip plated layer, and the said binary image data is obtained by subjecting the image data to a binarization process by Otsu's binarization method.
2. The Zn-Al-Mg hot-dip plated steel member according to claim 1, further comprising a chemical conversion treatment layer on the surface of the hot-dip plated layer.
3. The Zn-Al-Mg hot-dip plated steel member according to claim 2, wherein the chemical conversion coating layer has a metallic appearance.
4. The Zn-Al-Mg hot-dip plated steel member according to claim 1, wherein the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered is 150 or less, and the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where black pixels are gathered is 1.5 times or more the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered.
5. The Zn-Al-Mg hot-dip plated steel member according to claim 2, wherein the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered is 150 or less, and the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where black pixels are gathered is 1.5 times or more the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered.
6. The Zn-Al-Mg hot-dip plated steel member according to claim 1, wherein the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered is 70 or less, and the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where black pixels are gathered is 1.5 times or more the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered.
7. The Zn-Al-Mg hot-dip plated steel member according to any one of claims 1 to 6, wherein the average composition of the hot-dip plated layer contains one or more elements selected from the following group A, group B, or group C. Group A: Si: 0.0001 to 2% Group B: One or more elements selected from Ni, Ti, Zr, and Sr, with a total content of 0.0001 to 2% Group C: One or more elements selected from Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C, with a total content of 0.0001 to 2% 8. The Zn-Al-Mg hot-dip plated steel member according to claim 5, wherein the average composition of the hot-dip plated layer contains the Group A element.
9. The Zn-Al-Mg hot-dip plated steel member according to claim 5, wherein the average composition of the hot-dip plated layer contains the B group.
10. The Zn-Al-Mg hot-dip plated steel member according to claim 5, wherein the average composition of the hot-dip plated layer contains the C group element.