345 mpa-grade hot-rolled steel plate for building structures resistant to sea wave splash zone corrosion and manufacturing method thereof
Through the design of low-carbon microalloy composition and the control of the interface transition layer, the corrosion and mechanical properties of the steel structure in the environment of the wave splash zone are solved, and the development of corrosion-resistant steel plates in the 345MPa-level wave splash zone is achieved, with excellent resistance Corrosive and mechanical properties, suitable for facilities such as harbor terminals and marine oil production platforms.
Patent Information
- Application Number
- PCT/CN2024/094461
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-05
AI Technical Summary
The existing technology is difficult to provide corrosion resistance and good mechanical properties for building structures in the environment of wave splashing areas, especially in facilities such as harbor docks and marine oil production platforms. The corrosion rate of steel structures in the wave splashing areas is high and strong. The performance of the ratio and low temperature shock is insufficient, resulting in shorter service life and safety hazards.
Designed with low-carbon microalloy composition, the interface transition layer is formed between titanium and carbon steel, and the thickness of the interface transition layer is controlled, the excellent combination of titanium and carbon steel is achieved, ensuring the mechanical properties of the base layer and the corrosion resistance of the corrosion resistance of the corrosion resistance of the corrosion resistance of the corrosion resistance of the corrosion resistance of the corrosion resistance of the corrosion resistance of the corrosion resistance of the corrosion resistance of the , has excellent yield ratio and low temperature impact toughness.
A 345MPa-level corrosion-resistant steel plate has achieved a yield strength ≥350MPa, tensile strength ≥490MPa, yield strength ratio 0.71~0.80, impact work ≥190J in -40℃, interface transition layer thickness ≤10μm, interface shear strength ≥ 252MPa meets the corrosion resistance and mechanical properties requirements in the environment of the wave splash zone, and improves the applicability, safety and durability of the steel structure.
Smart Images

Figure CN2024094461_05122024_PF_FP_ABST
Abstract
Description
345MPa grade hot-rolled steel plate for building structure resistant to sea wave splash zone corrosion and manufacturing method thereof Technical Field
[0001] The present invention relates to the technical field of steel for building structures, and in particular to a hot-rolled steel plate for building structures that is resistant to corrosion in a wave splash zone and a manufacturing method thereof. Background Art
[0002] The ocean is a harsh and complex corrosive environment. Seawater is a strong electrolyte solution containing high concentrations of chloride ions. Steel structures, the backbone of offshore infrastructure, are susceptible to electrochemical reactions with the surrounding medium, leading to severe corrosion and significantly reducing their service life. This is particularly true in the splash zone, the harshest marine corrosion zone. Facilities are subject to a range of external factors, including alternating wet and dry conditions, seawater spray, sunlight, corrosive atmospheric components, and oxygen, leading to particularly severe corrosion.
[0003] Investigations show that steel piles at facilities such as harbor terminals and offshore oil platforms suffer severe corrosion in the wave splash zone, typically 3 to 10 times more than in areas fully immersed in seawater. Once severe localized corrosion damage occurs in this area, the load-bearing capacity of the entire facility is significantly reduced, shortening its service life, impacting production safety, and even leading to premature decommissioning.
[0004] Because the wave splash zone is located in a dry and wet alternating zone with sufficient oxygen supply, the corrosion products produced have no protective effect on the steel matrix. Due to the splash of seawater, its droplets can directly hit the metal surface, causing severe corrosion. Corrosion tests and survey results show that under normal circumstances, the average corrosion rate of ordinary carbon steel and low-alloy steel in the marine atmosphere is about 0.03 to 0.08 mm / year, while the average corrosion rate of these steels in the wave splash zone is about 0.3 to 0.5 mm / year. Steel is prone to severe corrosion damage in the wave splash zone, which greatly reduces the bearing capacity of the entire steel structure, affecting safe production, shortening its service life, and causing it to be scrapped prematurely.
[0005] Based on the aforementioned operating conditions, industrially pure titanium was selected as the corrosion-resistant layer. Titanium is highly chemically active and readily reacts with oxygen in air to form oxides. The oxides on the titanium metal surface are dense, stable, and possess a strong self-healing ability. This self-healing ability primarily refers to the ability of titanium oxide to rapidly form a new film after damage to a specific area on the titanium surface, preventing further contact with corrosive media.
[0006] Steel used in marine structures must not only meet corrosion resistance requirements but also possess excellent mechanical properties. Yield ratio and low-temperature impact toughness are becoming increasingly important indicators for structural steel. The yield ratio is the ratio of a steel material's yield strength to its tensile strength, reflecting its ability to withstand plastic deformation without strain concentration. The lower the yield ratio, the more evenly the plastic deformation is distributed over a wider area. Steel structures constructed with low-yield ratio steel can evenly distribute plastic deformation over a wide area under seismic forces. High-yield ratio materials, on the other hand, may experience strain concentration, reducing the overall plastic deformation capacity of the steel, leading to brittle failure and sudden collapse. Steel undergoes a brittle transition at low temperatures, shifting its fracture mode from ductile to brittle. This has engineering significance because steel components can operate at temperatures above this threshold without experiencing brittle fracture. Therefore, the low-temperature impact properties of structural steel are typically adjusted according to the material's service environment. Ocean temperatures vary significantly at different latitudes. For example, near China's Bohai Bay, winter seaside temperatures can drop below -20°C. This requires building materials to meet impact resistance requirements at -40°C to prevent brittle fracture. If the increase in tensile strength is small while improving plastic toughness, the yield strength ratio will increase significantly, making it difficult to achieve a low yield strength ratio.
[0007] Chinese patent application CN201210260231.7 discloses a method for preparing a titanium-steel-titanium double-sided composite plate. Four titanium plates and three steel plates are stacked in a specific order within a closed frame welded together with the two outermost steel plates. A separator consisting of 1 part by weight of activated α-Al₂O₃ and 1.5 parts by weight of a 4% polyvinyl alcohol aqueous solution is added between the titanium plates. A nickel-based alloy is used as a transition layer between the titanium and steel plates. The process is then heated to 500°C to 630°C and evacuated. The temperature is maintained for 1-2 hours, with a vacuum level of 20-200 Pa. This method is characterized by welding after assembly, followed by evacuation. Conventional arc welding and submerged arc welding are sufficient. Compared to welding under vacuum, this method requires less demanding welding conditions, is less expensive, and eliminates the need for a separate vacuum chamber. The combined blanks are then rolled and laminated in a conventional heating furnace at a temperature of 700°C to 900°C. The carbon in the coal gas is isolated by welding the outermost steel plate and evacuating the plate. A nickel-based alloy barrier layer is added to prevent the formation of TiC at the interface, resulting in a titanium-steel composite plate with a shear strength of 230-260 MPa and an interface bonding rate of 99.6%-100%.
[0008] Chinese patent application CN201710769999.X discloses a method for preparing a titanium-steel composite plate, which comprises selecting the surfaces of titanium-steel composite billets in contact with each other, applying a high-temperature resistant anti-carburizing and anti-nitriding isolation coating on the contacting titanium surfaces, and drying them at room temperature; after the drying process, the titanium billets are aligned and stacked in pairs, and a steel billet is placed in the middle to complete the assembly to obtain a composite billet, wherein the thickness of a single titanium billet is greater than 2 mm, and the thickness of the steel billet is greater than 5 mm, and then the composite billet is sealed and welded around and a certain size of unwelded area is left, and the billet is vacuumed to 10 -2 ~10 -3 Pa and then welded. The slab is heated to 500-700℃ and rolled, with the first pass reduction exceeding 25%, the final pass reduction not exceeding 15%, the total reduction rate being 60-70%, and the rolling speed being 0.1-1.0mm / s. The coating used in this patent has a high-temperature anti-seepage protection function, which can prevent the diffusion and oxidation of other impurity elements at high temperatures and block the diffusion of elements such as C and N. Its embodiment uses Q235 combined with TA1, and the shear strength of the produced steel plates reaches 176MPa, 181MPa, and 182MPa.
[0009] The above two patents mainly avoid the formation of brittle Ti compounds by adding an additional nickel-based alloy isolation layer between titanium and carbon steel.
[0010] Chinese patent application CN201811327623.4 discloses a titanium-steel-titanium composite sheet and its preparation method. This involves fixing a sheet of carbon steel between two titanium sheets of the same size. Warm composite rolling is performed using an irreversible, high-force warm rolling mill to combine the three strips into one. After rolling, the rolled composite sheet undergoes a heat treatment. This includes an initial annealing at 500-600°C for 20-60 minutes and a recrystallization annealing at 680-700°C for 30-120 minutes. Finally, the product is obtained through straightening, flattening, shearing, and shaping. This patent primarily describes a method for preparing a non-hot-rolled composite titanium steel sheet. Due to the use of an irreversible rolling mill, only a single rolling pass is possible, and heat treatment is also required. The examples primarily focus on the steel strip production method and do not mention the properties of the composite sheet.
[0011] Chinese patent application CN201510543767.3 discloses a method for preparing titanium-steel composite plates, which have high bonding strength. The patent involves fixing a titanium plate between two ordinary carbon steel plates or billets, welding the billets around the edges in a vacuum environment, heating the combined billets to 850-900°C for 120-360 minutes, controlling the start rolling temperature to above 800°C and the final rolling temperature to below 700°C, and controlling the deformation per pass to 20-30%, with the total rolling deformation ≥90%. High reduction rate rolling is performed to break up brittle phase compounds formed at the interface and reduce their impact on the bonding surface. The rolling process produces titanium-steel composite plates with a bonding strength greater than 240 MPa. The high reduction rate and total deformation required by the patent are both very high, which can easily cause edge weld cracking during the rolling process, destroying the vacuum level and hindering interfacial bonding.
[0012] Chinese patent application CN201610994234.1 discloses a method for producing titanium-steel composite plates, which relates to an annealing technology production method for titanium-steel plates. First, the titanium plate and the steel plate are assembled to form a symmetrical multi-layer composite billet with a structure of steel plate-titanium plate-isolator-titanium plate-steel plate, which is compounded by rolling compounding or explosion compounding. The compounded billet is annealed and pickled, first heated to 500-750°C to recrystallize the core titanium plate, and then heated to 950-1050°C to recrystallize the base steel plate. The purpose of this patent is to simultaneously improve the performance of the composite material and the substrate through a two-stage heat treatment. However, the two-stage heat treatment will cause excessive diffusion of titanium, iron and carbon elements, produce brittle substances such as iron-titanium intermetallic compounds and titanium carbide, and deteriorate the interface shear strength.
[0013] Chinese patent application CN201710996925.X discloses a thin-layer double-sided titanium-steel composite plate and its preparation method. Through large-thickness billet assembly and large-reduction rolling technology, a good composite between titanium and steel is achieved. The patent is a double-sided titanium composite plate composed of a titanium composite layer, a base layer and a titanium composite layer. The titanium composite layer is made of TA2 with a thickness of 0.2 to 1 mm. The billets are stacked in the order of cover plate, titanium composite material, carbon steel substrate, titanium composite material, and cover plate from top to bottom. After vacuum is drawn in a vacuum chamber, the gaps around them are vacuum electron beam sealed and welded. The vacuum degree is 1.0×10 -2 ~4.5×10 -2Pa, heat the sealed and welded composite billet to 900-920℃ and keep it warm. The holding time is calculated as 1min / mm×total thickness of the composite billet. The starting rolling temperature is 880-900℃, the final rolling temperature is above 800℃, and it is air-cooled to room temperature. The single-pass reduction rate is ≥15%, and the first three-pass reduction rate is ≥20%, and the total reduction rate is ≥80%. The composite plate obtained after rolling is trimmed, split, and surface-grinded to obtain a double-sided titanium-steel composite plate. This patent uses surface cleaning treatment of the composite slab, the air-isolating effect of the cover plate, the control of the rolling temperature, and the use of large reduction to break and refine the titanium iron and titanium carbon compounds generated at the composite interface, disperse them at the composite interface, improve the distribution state of the compounds, further ensure the composite quality and performance stability, and achieve a shear strength of 241MPa.
[0014] Chinese patent application CN201710983322.6 discloses a thin-layer titanium-steel composite plate and its preparation method. It adopts a double-layer structure of titanium and carbon steel composite, and its assembly method and heating process are similar to those of Chinese patent application CN201710996925.X. The starting rolling temperature is 880-900℃, the single-pass reduction rate is 25-30%, and the total reduction rate is ≥85%. While controlling the single-pass reduction rate and the total reduction rate, the thickness of the titanium-steel composite plate is limited to 3-16mm, the final rolling temperature is above 800℃, and it is air-cooled to room temperature. A titanium-steel composite plate is obtained by surface treatment, in which the thickness of the titanium composite layer is ≤1mm. This patent improves the composite quality by symmetrical assembly and welding titanium seals into carbon steel plates. After rolling, the shear strength of the steel plate reaches more than 238MPa, and the composite interface bonding rate is 100%. Its carbon steel layer meets the national standard for Q345 grade carbon steel.
[0015] However, the above patent does not mention the detailed elements and organizational design of the composite layer and the base layer, and only describes the tensile properties and shear strength. The required pass reduction rate and total reduction rate of the composite layer are both relatively high, and there is no control over the corrosion resistance of the material, the low-temperature impact performance of the base material, the yield strength ratio and other performance indicators, which do not meet the requirements for steel used in building structures.
[0016] In summary, the above patents primarily describe methods for preparing composite steel plates, and the specific embodiments in the specification provide only a brief description of performance, primarily focusing on interface shear strength and tensile properties. Steel used in wave splash zones, in addition to being corrosion-resistant in the wave splash zone, must also meet the necessary structural steel performance requirements, such as the aforementioned low yield ratio and corresponding low-temperature impact resistance to ensure structural safety. However, the above patents do not include any relevant composition or process design for the corrosion rate, yield ratio, and low-temperature impact of the corrosion-resistant layer, and cannot guarantee that the requirements for highly corrosion-resistant steel plates used in wave splash zone environments can be met.
[0017] Summary of the Invention
[0018] One of the objectives of the present invention is to provide a 345MPa-grade hot-rolled steel plate for building steel structures, preferably having a yield strength ≥350MPa, a tensile strength ≥490MPa, a yield strength ratio of 0.71-0.80, an impact energy ≥190J at -40°C, a wave splash corrosion rate ≤0.006mm / year, an interface transition layer thickness ≤10μm, and an interface shear strength ≥252MPa. This steel plate can meet the corrosion resistance requirements for use in wave splash zones, combines good mechanical properties for wave splash zone corrosion resistance with high economic efficiency, and is suitable for use in steel structures such as steel piles in facilities such as harbors, docks, and offshore oil platforms.
[0019] This invention utilizes a low-carbon microalloying composition design to achieve an excellent bond between titanium and carbon steel without adding a metal barrier layer. By controlling the thickness of the interfacial transition layer, the mechanical properties of the base layer (carbon steel) meet the corresponding strength level requirements without compromising the corrosion resistance of the corrosion-resistant layer itself, resulting in excellent yield strength ratio and low-temperature impact toughness.
[0020] Specifically, the hot-rolled steel plate for building structures of the present invention comprises a base layer, a corrosion-resistant layer, and an interface transition layer between the base layer and the corrosion-resistant layer;
[0021] In addition to Fe and other inevitable impurities, the base layer also contains the following chemical elements in mass percentage: C 0.03-0.10%, Si 0.10-0.30%, Mn 1.00-1.50%, P 0.0005-0.003%, S 0.0005-0.010%, Cr 0.02-0.20%, Ni 0.01-0.10%, Cu 0.002-0.020%, Al 0.015-0.03%, Ti 0.008-0.018%, Nb 0.02-0.065%, N 0.0005-0.005%;
[0022] The corrosion-resistant layer is made of industrial pure titanium, and its composition meets the standard of GB / T3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Composition".
[0023] Preferably, the yield strength of hot-rolled steel plates for building structures is ≥350MPa, the tensile strength is ≥490MPa, the yield strength ratio is 0.71-0.80, the impact energy at -40°C is ≥190J, the wave splash corrosion rate is ≤0.006mm / year, the interface transition layer thickness is ≤10μm, and the interface shear strength is ≥252MPa.
[0024] During the heating and rolling process, atoms at the interface between the titanium and the base carbon steel diffuse, forming an interfacial transition layer between the two. In the present invention, the location where the Fe content in the carbon steel decreases by 5% compared to the base is defined as the first boundary of the interfacial transition layer, and the location where the Ti content in the pure titanium layer decreases by 5% compared to the base is defined as the second boundary of the interfacial transition layer. The distance from the first boundary to the second boundary is defined as the thickness of the interfacial transition layer.
[0025] Preferably, the chemical composition of the base layer also satisfies the following relationship: 0.02%≤Cu+Ni≤0.20%; 2(C+N)≤Ti+Nb+Cr≤0.22%;
[0026] When calculating, each element in the relationship is input as the mass percentage of the corresponding element in the base layer.
[0027] Preferably, the mass percentage content of each chemical element in the base layer is: C 0.03-0.10%, Si 0.10-0.30%, Mn 1.00-1.50%, P 0.0005-0.003%, S 0.0005-0.01%, Cr 0.02-0.20%, Ni 0.01-0.10%, Cu 0.002-0.020%, Al 0.015-0.03%, Ti 0.008-0.018%, Nb 0.02-0.065%, N 0.0005-0.005%, and the balance is Fe and other inevitable impurities.
[0028] Preferably, the microstructure of the base layer is ferrite + pearlite and / or a small amount of bainite, with the pearlite content being ≥5% and the average ferrite grain size being ≥8.5. Preferably, the bainite content is ≤10%. Unless otherwise specified, the content of each structure in the steel is expressed as volume fraction.
[0029] Preferably, in the base layer of the hot-rolled steel plate of the present invention, the volume fraction of ferrite is 80%-90%, the volume fraction of pearlite is 5%-10%, and the volume fraction of bainite is below 8%.
[0030] Preferably, the yield strength of the base layer in the present invention is ≥350 MPa, the tensile strength is ≥497 MPa, the yield strength ratio is 0.71-0.80, and the impact energy at -40°C is ≥190 J.
[0031] In the hot-rolled steel strip of the present invention, the thickness of the base layer accounts for more than 80% of the total thickness of the hot-rolled steel strip, and the mechanical properties of the hot-rolled steel strip finally obtained are mainly controlled by the base layer carbon steel.
[0032] Preferably, the corrosion-resistant layer is made of TA1, TA2, TA3 or TA4.
[0033] Preferably, the microstructure of the corrosion-resistant layer is single, equiaxed α-Ti.
[0034] Preferably, the wave splash corrosion resistance rate of the corrosion-resistant layer is ≤0.006 mm / year.
[0035] Preferably, the interface transition layer achieves 100% metallurgical bonding and high atomic coherence; and / or the thickness of the interface transition layer is ≤10 μm, and the interface shear strength is ≥252 MPa.
[0036] Preferably, the interface transition layer has fine grains with an average grain size of 15 to 50 μm, and contains (Ti, Nb)C precipitated particles with a size of less than 120 nm.
[0037] Preferably, the thickness of the hot-rolled steel plate for building structures is 3 to 80 mm.
[0038] In the base layer of the hot-rolled steel plate for building steel structure of the present invention, the design ideas of each element are as follows:
[0039] C: It plays a role of solid solution strengthening in steel and can significantly improve the strength of steel. However, too high a C content is detrimental to welding performance and toughness. More importantly, when the C content is too high, it will diffuse to the composite interface, forming a large amount of large-granular TiC hard phase in the interface transition layer, reducing the composite interface strength. In order to ensure the shear strength of the interface, the present invention adopts a low C content. The change in C content has less effect on the yield strength of steel than on the tensile strength. Under the premise of ensuring the product forming and welding performance, appropriately increasing the C content is beneficial to reducing the yield strength ratio of steel. Based on this, in the base composition of the hot-rolled steel plate of the present invention, the C content is controlled at 0.03-0.10%.
[0040] Si: Adding Si to steel effectively deoxidizes and improves steel purity. Furthermore, Si acts as a solid solution strengthener in steel, increasing its strength and hardness. However, Si is detrimental to the material's weldability. Therefore, the Si content in the base composition of the hot-rolled steel sheet of this invention is controlled to 0.10-0.30%.
[0041] Mn: Mn is the cheapest matrix-strengthening element. It can lower the austenite transformation temperature, delay pearlite transformation, refine ferrite grains, and increase steel strength. Mn also counteracts the adverse effects of sulfur on steel. However, excessive Mn content can easily lead to segregation bands and martensitic structures, which negatively impact steel toughness. Therefore, the Mn content in the base composition of the hot-rolled steel sheet of the present invention is controlled to 1.00% to 1.50%.
[0042] Al: Al is mainly added to steel in excess as a deoxidizing element to ensure that the O content in the steel is as low as possible. After deoxidization, the excess Al combines with the N element in the steel to form AlN precipitates. During the heating process, AlN hinders the growth of austenite grains, refines the austenite grains, and improves the strength and toughness of the matrix. At the same time, the formation of AlN fixes part of the N in the matrix, reduces the diffusion of interstitial atomic N in the carbon steel base layer to the composite interface, forms hard TiN in the interface transition layer, and deteriorates the interface shear strength of the composite plate. In addition, the addition of Al can appropriately reduce the amount of Ti and Nb added, thereby reducing production costs. Based on this, the Al content in the base composition of the hot-rolled steel plate of the present invention is controlled at 0.015-0.03%.
[0043] Ti: Ti forms stable TiN or Ti(N, C) at high temperatures, which plays a role in fixing C and N, preventing interstitial C and N atoms in the carbon steel base from diffusing to the interface, and forming hard TiN or Ti(N, C) precipitation in the interface transition layer to obtain a composite plate with high interface shear strength. At the same time, TiN hinders the growth of austenite during the heating process, refines the austenite grains, and can improve the strength and toughness of the matrix. In the subsequent welding process, especially in the heat-affected zone (HAZ) close to the molten boundary of the weld, it inhibits the growth of austenite grains, thereby improving the toughness of the weld HAZ and meeting the needs of large welding heat input processes. Ti helps to improve the strength of the low-carbon matrix, reduce the diffusion of C and N to the interface, and obtain a composite plate with high interface shear strength. Based on this, the Ti content in the base composition of the hot-rolled steel plate of the present invention is controlled to be 0.008-0.018%.
[0044] Nb: Nb exists in the steel in the form of solid solution Nb and Nb(C, N), and plays the role of solid solution drag and precipitation pinning during the recrystallization process. The main purpose of adding a small amount of Nb to the base carbon steel is to increase the recrystallization temperature, so that the base carbon steel can be grain refined after rolling in the recrystallization and non-recrystallization zones, which is beneficial to improving the low-temperature impact toughness of the base carbon steel. Due to the formation of Nb(C, N) precipitation phase, the original austenite grains will be finer, thereby promoting the formation of finer recrystallized grains and obtaining an ideal combination of high strength and high toughness. In addition, Nb can fix the interstitial C and N atoms in the matrix, reduce the diffusion of C and N to the interface, and help to obtain a composite plate with high interface shear strength. Based on this, the Nb content in the base composition of the hot-rolled steel plate of the present invention is controlled to be 0.02-0.065%.
[0045] Cu: Cu plays a role in solid solution strengthening. Furthermore, as the Cu content increases, the room temperature impact toughness of the steel slightly improves. Therefore, the Cu content in the base composition of the hot-rolled steel sheet of the present invention is controlled to be between 0.002% and 0.020%.
[0046] N: Elemental N can react with Ti and Al to form second-phase particles, refining austenite grains and improving matrix strength and toughness. However, excessively high N content results in excessive TiN and coarse particles, which can affect the plasticity and toughness of the base carbon steel. Therefore, the N content in the base composition of the hot-rolled steel sheet of the present invention is controlled to 0.0005-0.005%.
[0047] Nickel: Nickel stabilizes austenite and contributes to strength. Adding nickel to steel significantly improves its low-temperature impact toughness. However, nickel is expensive, and adding too much increases the cost of the composite plate. Therefore, an appropriate amount of nickel is added to the base composition of the hot-rolled steel plate of the present invention, with the nickel content controlled to 0.01-0.10%.
[0048] Cr: Cr is a strong carbide-forming element with a slow diffusion rate in austenite, hindering the diffusion of carbon. During the low-temperature process, it forms fine carbides, which act as precipitation strengthening agents. Simultaneously, it fixes interstitial carbon and nitrogen atoms in the matrix, reducing their diffusion toward the interface and resulting in a composite plate with high interfacial shear strength. While Cr increases matrix strength in steel, it also reduces toughness. To achieve the optimal balance of strength and toughness, the Cr content in the base composition of the hot-rolled steel plate of this invention is controlled to 0.02-0.20%.
[0049] S and P are both unavoidable impurity elements, and their contents should be as low as possible. Taking into account the actual steelmaking process, in the base layer of the hot-rolled steel plate of the present invention, the S and P contents are controlled to be: 0.0005% ≤ S ≤ 0.010%; 0.0005% ≤ P ≤ 0.003%;
[0050] The corrosion-resistant layer of the hot-rolled steel plate of the present invention adopts industrial pure titanium, preferably TA1, TA2, TA3 and TA4, and its composition meets the standard of GB / T3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Composition".
[0051] In addition, in the base chemical composition design of the hot-rolled steel plate for building steel structure of the present invention:
[0052] Both Cu and Ni can improve the toughness of the base layer, with the combined addition effect being particularly significant. Furthermore, the addition of Ni can reduce the diffusion rate of carbon in the steel, thereby reducing its diffusion to the interface. Therefore, in a preferred embodiment of the present invention, controlling the Cu+Ni ratio to 0.02% ≤ Cu+Ni ≤ 0.20% helps to keep the interface transition layer within 10 μm. An interface transition layer thickness exceeding 10 μm can adversely affect the durability of the coating.
[0053] In addition, Ti, Nb, and Cr are all strong carbonitride-forming elements. They will form corresponding carbonitrides in the base carbon steel, which can fix the interstitial atoms in the base, hinder the diffusion of C and N interstitial atoms to the interface, and form large-particle, aggregated carbonitrides in the interface transition layer, which helps to control the interface transition layer within 10μm, thereby improving the interface shear strength. At the same time, Ti, Nb, and Cr can play a role in refining the base carbon steel grains and improving toughness at different stages of hot rolling. Therefore, in a preferred embodiment of the present invention, the control is: 2(C+N)≤Ti+Nb+Cr≤0.22%.
[0054] In the relationship, each chemical element is entered as the mass percentage of the corresponding element in the base layer during calculation.
[0055] In another aspect, the present invention provides a method for manufacturing the hot-rolled steel plate for building structures, comprising the following steps performed in sequence:
[0056] 1) Smelting and casting
[0057] According to the compositions of the base layer and the corrosion-resistant layer, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively;
[0058] 2) Assembly
[0059] The base blank and the corrosion-resistant layer blank are subjected to surface grinding and polishing, the base blank and the corrosion-resistant layer blank are laminated, and the laminating surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the laminating surfaces after welding and sealing are vacuumed;
[0060] 3) Heating
[0061] Heating the composite blank to 900-1000° C. to form an interface transition layer between the base layer and the corrosion-resistant layer;
[0062] 4) Rolling
[0063] The composite billet is rolled, wherein the pass reduction rate is 5-20%, the cumulative reduction rate is ≥70%, and the final rolling temperature is 750-850°C, so that the base layer and the cladding layer are fully combined;
[0064] 5) Cooling
[0065] After rolling, the steel is cooled by water, the cooling rate is controlled at 5-20°C / s, and the final cooling temperature is 300-650°C to obtain a hot-rolled steel plate.
[0066] Preferably, the thickness of the corrosion-resistant layer in step 2) is 0.5-20% of the total thickness of the composite blank.
[0067] Preferably, in step 3), the thickness of the interface transition layer formed between the base layer and the corrosion-resistant layer is ≤10 μm. More preferably, the thickness of the interface transition layer is greater than 0.5 μm.
[0068] Preferably, the rolling reduction rate used in step 4) is 10-20%.
[0069] In the manufacturing method of the present invention, the design ideas of each process are as follows:
[0070] 1) Smelting: P and S elements deteriorate the fracture toughness of steel, so their contents must be kept low during the smelting process to improve billet quality. Using clean steel production technology reduces the gas and inclusion content in the steel, improving the overall performance of the steel, especially its resistance to lamellar tearing.
[0071] 2) Assembly: The corrosion-resistant layer thickness is set at 0.5-20% of the total composite sheet thickness. The corrosion-resistant layer and base carbon steel sheet are pre-treated, and the steel sheet bonding surfaces are welded and sealed on all sides. The sealed surfaces are then vacuumed. Vacuuming protects the corrosion-resistant layer from oxidation and is crucial for ensuring the corrosion-resistant layer resists corrosion in the splash zone during use.
[0072] 3) Heating: For the base carbon steel, the slab heating temperature is generally controlled at 1000-1250°C, which is conducive to the dissolution and full diffusion of precipitates in the steel, promotes the homogenization of the slab elements, and exerts the strengthening effect of microalloying elements in the steel. For the cladding industrial pure titanium plate, the heating temperature is generally controlled at 850-1000°C. Excessively high heating temperatures will produce β phase transformation, and the β phase will grow rapidly, deteriorating the performance of industrial pure titanium. In addition, excessively high heating temperatures will also allow the elements to fully diffuse, promoting the subsequent realization of 100% metallurgical bonding at the interface. However, higher heating temperatures will increase the tendency of austenite grains to coarsen, increasing the difficulty of subsequent controlled rolling. Most importantly, it will accelerate the diffusion of C, N, Ti, and Fe to the interface, forming thicker brittle precipitates and intermetallic compounds at the interface, forming a thick interface transition layer, and deteriorating the interface shear strength. Preferably, the heating temperature is set between 900 and 1000°C.
[0073] 4) Rolling: A large amount of deformation is applied in the high temperature zone to fully recrystallize the structure, refine the grains, and improve the strength and toughness of the material. The pass reduction rate is between 5% and 20%, and the cumulative reduction rate is ≥70%. Controlled rolling is performed in the non-recrystallized zone. At this stage, austenite recrystallization no longer occurs. Through reasonable reduction rate and final rolling temperature, deformation energy and deformation dislocations are accumulated, forming a high-density deformation band inside the austenite grains, increasing the phase deformation nuclei, further refining the grain size after the matrix phase transformation, and improving the strength and toughness of the material. In addition, at this stage, deformation induces the precipitation of carbonitrides of Nb, Ti, and Cr, which increases the strength of the matrix, inhibits the diffusion of C to the interface, and avoids the formation of excessively thick TiC at the interface, which deteriorates the interface shear strength. Preferably, the final rolling temperature is controlled at 750-850°C, while ensuring the corrosion resistance of titanium, avoiding rolling of the base layer in the two-phase region, and obtaining ferrite + pearlite with an average grain size greater than 8.5 and / or bainite content less than or equal to 10%.
[0074] 5) Cooling: The present invention controls the type and size of the post-rolling microstructure by controlling the initial cooling, final cooling, and cooling rate. Excessively fast cooling rates can result in the formation of bainite and martensite. Since martensite has low toughness and a high yield ratio, it is detrimental to the performance of the steel plate. Excessively slow cooling rates can lead to the formation of large amounts of coarse ferrite, which favors crack propagation and reduces impact properties. Therefore, the cooling rate should be appropriately controlled.
[0075] Controlling the final rolling temperature can avoid the formation of abnormally coarse microstructures caused by rolling in the two-phase region. Furthermore, rapid cooling to the phase transition temperature after rolling further inhibits microstructure growth, improving material strength and low-temperature impact toughness through grain refinement. Preferably, water cooling is employed, with a cooling rate controlled between 5 and 20°C / s and a final cooling temperature between 300 and 650°C, to ensure a low yield strength ratio and high low-temperature impact toughness for the base layer.
[0076] Preferably, if the corrosion-resistant layer is too thick, it will affect the mechanical properties of the material and production costs. If the corrosion-resistant layer is too thin, it will reduce the corrosion resistance and service life of the material. Therefore, during the above-mentioned assembly process, the corrosion-resistant layer preferably accounts for 0.5-20% of the total thickness of the composite blank.
[0077] The present invention combines a corrosion-resistant layer with a base layer, combining component design and thickness ratio design, and forms a corrosion-resistant layer resistant to splash zone corrosion on the base carbon steel plate through a rolling process. The result is a steel plate that combines splash zone corrosion resistance with excellent mechanical properties and high economic efficiency. The steel plate can then be processed into structural components for use in splash zone environments.
[0078] Compared with the prior art, the present invention has the following beneficial effects:
[0079] This invention utilizes a low-carbon microalloying composition design to achieve excellent bonding between titanium and carbon steel without adding a metal barrier layer. By controlling the thickness of the interfacial transition layer, the mechanical properties of the base layer (carbon steel) meet the corresponding strength level requirements without compromising the corrosion resistance of the corrosion-resistant layer itself. Furthermore, the base layer exhibits excellent yield strength ratio and low-temperature impact toughness.
[0080] In addition, by reducing the carbon content in the base carbon steel, the present invention reduces the formation of TiC compounds in the interface transition layer and the formation of carbonitrides in the base, hindering grain growth and improving the low-temperature impact toughness of the base. On the other hand, the addition of microalloying elements to the steel and the combination of a reasonable rolling and cooling process solve the problem of low material strength under low-carbon conditions. The resulting composite steel plate (hot-rolled steel plate) has a yield strength of ≥350MPa and a tensile strength of ≥490MPa. At the same time, the material yield strength ratio is 0.71 to 0.80, and the -40°C impact energy is ≥190J, all of which exceed the performance requirements of the national standard GB / T 19879-2015 "Steel Plate for Building Structures".
[0081] Chinese patent application CN201210260231.7 does not specify the heating temperature. By adding a nickel plate as an isolation layer between the cladding layer and the base layer to prevent the formation of TiC at the interface, the resulting titanium-steel composite plate has an interface bonding rate of 99.6-100%. However, the present invention specifies that the heating temperature of the composite billet is 900-1000°C. Through low-carbon and micro-alloy design, the addition of Ni is reduced, lowering production costs. Furthermore, through process optimization such as heating and rolling, a transition layer with a certain thickness is formed, and the formation of brittle TiC in the interface transition layer is reduced, achieving 100% metallurgical bonding at the interface (complete metallurgical bonding).
[0082] The heating temperature of the slab in Chinese patent application CN201710769999.X is 500-700°C, the total reduction rate is 60-70%, and the interface shear strength of the produced steel plate is up to 182MPa. The present invention fully considers the impact of the high-temperature phase transformation of industrial pure titanium in the corrosion-resistant layer on the corrosion resistance, and controls the strength and toughness of the base carbon steel. Combined with the low-carbon microalloy design and the global design of the processing technology, the heating temperature of the composite billet is set to 900-1000°C. At this temperature, the corrosion-resistant layer does not undergo phase transformation, and the precipitates in the base carbon steel are fully dissolved. During the controlled rolling process, the base grains are refined to improve the strength and toughness of the base. Combined with a total reduction rate of ≥70%, the brittle phase at the interface is broken, thereby improving the interface shear strength.
[0083] The above two patents mainly avoid the formation of brittle Ti compounds by adding an additional nickel-based alloy isolation layer between titanium and carbon steel. However, the present invention does not add an isolation layer through composition and process design, and the assembly method is different from the above two patents, and the material of the base carbon steel is also significantly different.
[0084] The process conditions of the present invention ensure both the original corrosion resistance of the industrial pure titanium in the corrosion-resistant layer and the mechanical properties of the base layer, solving the problem of the large difference in the processing window between traditional titanium and carbon steel, which makes it difficult to take both into account. At the same time, the elements of the base layer and the corrosion-resistant layer are fully diffused to form an interface transition layer no larger than 10μm. This layer has fine grains with an average grain size of 15 to 50μm and contains (Ti, Nb)C precipitated particles with a size of less than 120nm, which strengthens the interface bonding performance and ensures an interface shear strength of ≥252MPa, which is higher than the interface shear strength of 182MPa in the prior art.
[0085] Chinese patent application CN201811327623.4 achieves composite by warm rolling, followed by a two-stage heat treatment operation, including a primary annealing at 500-600°C for 20-60 minutes and a recrystallization annealing at 680-700°C for 30-120 minutes. It is a preparation method for a non-hot-rolled composite titanium steel plate, which is completely different from the manufacturing method of the present invention.
[0086] Chinese patent application CN201510543767.3 has a heating temperature of 850-900°C, a final rolling temperature below 700°C, and controls the deformation of each pass to be between 20-30%, the total deformation of rolling is ≥90%, and the shear strength of the titanium-steel composite plate is greater than 240MPa. The pass reduction rate and total deformation required by this solution are both very high, which can easily cause cracking of the edge welds during the rolling process, destroy the vacuum, make it difficult to composite, and have poor rolling stability. The single-pass reduction rate of the present invention is controlled at 5-20%, which can effectively prevent the welds from cracking during the rolling process, ensure the vacuum inside the slab, and effectively improve the interface shear strength, rolling stability, and success rate.
[0087] Chinese patent application CN201610994234.1 is a production method of annealing technology for titanium steel plates. First, the titanium plate and the steel plate are assembled to form a symmetrical multi-layer composite billet of steel plate-titanium plate-isolator-titanium plate-steel plate, which is compounded by rolling compounding or explosion compounding. The compounded billet is annealed and pickled, first heated to 500-750°C to recrystallize the core titanium plate, and then heated to 950-1050°C to recrystallize the base steel plate. The rolling process and the corrosion and structural properties of the obtained steel plate are not specifically defined. The present invention is significantly different from the present invention in terms of manufacturing process. The present invention does not require a two-stage heat treatment, and the two-stage heat treatment will cause excessive diffusion of titanium, iron and carbon elements, resulting in brittle intermetallic compounds of iron and titanium and titanium carbide, which deteriorates the interface shear strength.
[0088] The corrosion-resistant layer material of Chinese patent application CN201710996925.X is TA2, in which the titanium composite layer is 0.2 to 1 mm thick, heated to 900 to 920 ° C for insulation, the starting rolling temperature is 880 to 900 ° C, the final rolling temperature is above 800 ° C, and air-cooled to room temperature, and the shear strength reaches 241 MPa. The heating temperature of the present invention is 900 to 1000 ° C, the final rolling temperature is 750 to 850 ° C, and water cooling is used, with a controlled cooling rate of 5 to 20 ° C / s. Under this process, it is possible to achieve hot-rolled plates with TA1, TA2, TA3 and TA4 as corrosion-resistant layers, with the corrosion-resistant layers accounting for 0.5 to 20% of the total thickness of 3-80 mm, and the interface shear strength is ≥ 252 MPa.
[0089] Chinese patent application CN201710983322.6 uses a similar assembly method and heating process to that of Chinese patent application CN201710996925.X. The single-pass reduction is 25-30%, and the total reduction is ≥85%. While controlling both the single-pass and total reduction rates, the thickness of the titanium-steel composite plate is limited to 3-16 mm. The final rolling temperature is above 800°C, followed by air cooling to room temperature. The titanium-steel composite plate is surface treated to achieve a titanium cladding thickness of ≤1 mm. The present invention uses a single-pass reduction of 5-20% to control rolling stability. Significant differences are also observed in the thickness of the corrosion-resistant layer and the total thickness of the composite steel plate.
[0090] In summary, the 345MPa-grade hot-rolled steel plate for building structures resistant to seawater splash zone corrosion described in the present invention can solve the essential pain points of stainless steel or carbon steel used in seawater splash zone environments. The 345MPa-grade hot-rolled steel plate for building structures resistant to seawater splash zone corrosion can be effectively applied to the manufacture of steel structural components used in seawater splash zone environments (for example, seaport terminals, offshore oil platforms, and other facilities), meeting the requirements of these components for seawater splash zone corrosion resistance and mechanical properties, significantly improving the applicability, safety, and durability of these components, and having great economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] FIG1 is a schematic diagram of the interlayer structure of the hot-rolled steel plate for building structures of the present invention.
[0092] FIG2 is another schematic diagram of the interlayer structure of the hot-rolled steel plate for building structures of the present invention.
[0093] FIG3 is a microstructure photograph of the corrosion-resistant layer of the hot-rolled steel plate for building structures according to Example 3 of the present invention.
[0094] FIG4 is a scanning image of the interface transition layer of the hot-rolled steel plate for building structure according to Example 3 of the present invention.
[0095] FIG5 is a photograph of the base microstructure of the hot-rolled steel plate for building structure according to Example 3 of the present invention.
[0096] Reference numerals: 1-base layer, 2-corrosion-resistant layer, 3-interface transition layer. DETAILED DESCRIPTION
[0097] The technical solution of the present invention will be further described in detail below with reference to the examples and drawings. It should be understood that the following examples are only used to describe the specific embodiments of the present invention and do not constitute any limitation on the scope of protection of the present invention.
[0098] 1 and 2 , which are schematic diagrams of two interlayer structures of the hot-rolled steel plate for building structure of the present invention, wherein 1 is the base layer, 2 is the corrosion-resistant layer, and 3 is the interface transition layer.
[0099] The composition of the base layer of the hot-rolled steel plate (composite steel plate) for building structures of the present invention is shown in Table 1, with the remainder being Fe and unavoidable impurities. Table 2 shows the manufacturing process parameters of the composite steel plate of the present invention and the comparative example. Table 3 shows the metallographic structure of the base layer and the mechanical properties, interface transition layer thickness and shear strength of the composite steel plates of the embodiments and comparative examples. The metallographic structure of carbon steel, excluding pearlite and a possible small amount of bainite, is composed of ferrite. Taking the hot-rolled steel plate of Example 1 as an example, the volume fraction of ferrite is 95.0%.
[0100] Among them, the yield strength and tensile strength of the composite steel plate are measured in accordance with GB / T 6396-2008 "Mechanical and process performance methods of composite steel plates" and GB / T 228-2010 "Room temperature tensile test methods for metallic materials"; the -40℃ impact energy KV2 / J (longitudinal) is measured in accordance with GB / T 6396-2008 "Mechanical and process performance methods of composite steel plates" and GB / T 229-2020 "Charpy pendulum impact test method for metallic materials"; the interface shear strength is measured according to GB / T 6396-2008 "Mechanical and process performance methods of composite steel plates".
[0101] The yield strength and tensile strength of the base carbon steel are measured in accordance with GB / T 6396-2008 "Mechanical and process properties of composite steel plates" and GB / T 228-2010 "Room temperature tensile test method for metallic materials". The impact energy KV2 / J (longitudinal) at -40°C is measured in accordance with GB / T 6396-2008 "Mechanical and process properties of composite steel plates" and GB / T 229-2020 "Charpy pendulum impact test method for metallic materials".
[0102] The grain size rating of ferrite in the base carbon steel is carried out as follows: the grain size of ferrite in carbon steel is rated using the intercept method according to GB / T 6394-2017 "Method for determination of average grain size of metals".
[0103] The comparative example was prepared by the same steps as those in the embodiment of the present invention, except that the composition of the base carbon steel and certain process parameters used in the rolling or cooling steps did not meet the requirements of the present invention.
[0104] FIG3 shows the metallographic structure of the corrosion-resistant layer of Example 3, which is single, equiaxed α-Ti with an average grain size of 102.8 μm.
[0105] FIG4 shows the structure of the interface transition layer of Example 3. The thickness of the interface transition layer 3 is 7.5 μm, and the discontinuous fine particles are TiC with a size of less than 120 nm.
[0106] FIG5 shows the metallographic structure of the base layer of Example 3, which shows that the metallographic structure of the base carbon steel is ferrite+pearlite, wherein the volume fraction of pearlite is 6.8%, and the grain size of ferrite is ≥8.5.
[0107] Table 4 shows the corrosion behavior of composite steel plate coupons from Examples 1-8 and Comparative Examples 1-4 after six months in the South China Sea's wave splash zone. The corrosion tests were conducted in accordance with GB / T 5776-2005, "Corrosion of Metals and Alloys - Guide for the Assessment of Metals and Alloys Exposure to Surface Seawater." The chloride ion concentration (%) in Table 4 represents the percentage of chloride ions in the total mass of the solution. For example, a chloride ion concentration of 5% means that 5 grams of chloride ions are present in 100 grams of solution. Observation results show that, with the exception of Comparative Example 4, the corrosion rates of all other Examples and Comparative Examples were ≤0.006 mm / year.
[0108] Comparative Examples 1-4 use unqualified composition design requirements or thermal processing process conditions, resulting in certain properties of the composite steel plates failing to meet the use requirements (performance parameters are not within the scope of the invention).
[0109] In Comparative Example 1, since the chemical composition does not contain Ti, Nb and Cr additions and the rolling reduction rate used is not within the range defined by the present invention, the yield strength, yield strength ratio, impact properties and interface shear strength cannot meet the requirements.
[0110] In Comparative Example 2, since the chemical composition does not contain Ni addition, the final rolling temperature, cooling rate, and final cooling temperature are not within the range defined by the present invention, its yield strength ratio and impact properties cannot meet the requirements.
[0111] In Comparative Example 3, since the addition amount of Cu+Ni in the chemical composition is less than 0.02% and the cooling rate and final cooling temperature are not within the range specified by the present invention, its metallographic structure is bainite, and the mechanical properties, yield strength ratio and impact properties cannot meet the requirements.
[0112] In Comparative Example 4, since the heating temperature and the final rolling temperature are not within the range specified by the present invention, the thickness of the interface transition layer is too thick, resulting in the shear strength not meeting the performance requirements. Since the heating temperature is too high, β-Ti cannot be completely eliminated during the subsequent processing and cooling process, resulting in a high corrosion rate.
[0113] The technical solution of the present invention enables the base layer in the steel plate to exhibit excellent yield strength ratio and low-temperature impact toughness, while the cladding layer has excellent corrosion resistance and high bonding strength. The hot-rolled steel plate has a yield strength of 352 to 445 MPa, a tensile strength of 497 to 602 MPa, a yield strength ratio of 0.71 to 0.80, an impact energy of more than 190 J at -40°C, and an interfacial shear strength greater than 252 MPa. The preparation method of the present invention, especially the control of the heating, rolling, and cooling processes, also helps achieve the corresponding steel properties.
[0114] It should be noted that all technical features described in the present invention can be freely combined or combined in any way unless there is a contradiction between them. Various modifications and variations can be made to the present invention without departing from the scope of the present invention, which will be apparent to those skilled in the art. For example, a feature shown or described as part of one embodiment can be used together with another embodiment to produce yet another embodiment. Therefore, the present invention is intended to cover these modifications that fall within the scope of the appended claims and their equivalents.
Claims
1. Hot rolled steel plate for building structure, characterized in that: The hot-rolled steel plate comprises a base layer, a corrosion-resistant layer and an interface transition layer between the base layer and the corrosion-resistant layer; In addition to Fe and other inevitable impurities, the base layer also contains the following chemical elements in mass percentage: C 0.03-0.10%, Si 0.10-0.30%, Mn 1.00-1.50%, P 0.0005-0.003%, S 0.0005-0.01%, Cr 0.02-0.20%, Ni 0.01-0.10%, Cu 0.002-0.020%, Al 0.015-0.03%, Ti 0.008-0.018%, Nb 0.02-0.065%, N 0.0005-0.005%; The corrosion-resistant layer is industrial pure titanium, preferably TA1, TA2, TA3 or TA4.
2. The hot-rolled steel plate for building structure according to claim 1, characterized in that: The chemical composition of the base layer also satisfies the following relationship: 0.02%≤Cu+Ni≤0.20%; 2(C+N)≤Ti+Nb+Cr≤0.22%; Each element in the relational formula is input as the mass percentage of the corresponding element in the base layer during calculation.
3. The hot-rolled steel sheet for building structure according to claim 1 or 2, characterized in that: The mass percentage content of each chemical element of the base layer is: C 0.03-0.10%, Si 0.10-0.30%, Mn 1.00-1.50%, P 0.0005-0.003%, S 0.0005-0.01%, Cr 0.02-0.20%, Ni 0.01-0.10%, Cu 0.002-0.020%, Al 0.015-0.03%, Ti 0.008-0.018%, Nb 0.02-0.065%, N 0.0005-0.005%, and the balance is Fe and other inevitable impurities.
4. The hot-rolled steel sheet for building structure according to any one of claims 1 to 3, characterized in that: The microstructure of the base layer is ferrite+pearlite and / or bainite structure, the pearlite content is ≥5%, and the average ferrite grain size is ≥8.5; preferably, the content of bainite structure is ≤10%.
5. The hot-rolled steel sheet for building structure according to any one of claims 1 to 4, characterized in that: The yield strength of the base layer is ≥350MPa, the tensile strength is ≥497MPa, the yield strength ratio is 0.71-0.80, and the impact energy at -40°C is ≥190J.
6. The hot-rolled steel plate for building structure according to claim 1, characterized in that: The microstructure of the corrosion-resistant layer is single, equiaxed α-Ti.
7. The hot-rolled steel sheet for building structure according to claim 1 or 6, characterized in that: The sea wave splash corrosion resistance rate of the corrosion resistant layer is ≤0.006mm / year.
8. The hot-rolled steel plate for building structure according to claim 1, characterized in that: The interface transition layer has a thickness of 0.5-10 μm, an average grain size of 15-50 μm, and contains (Ti, Nb)C precipitated particles with a size less than 120 nm.
9. The hot-rolled steel plate for building structure according to claim 1, characterized in that: The thickness of the hot-rolled steel plate for building structure is 3 to 80 mm.
10. The hot-rolled steel sheet for building structure according to any one of claims 1 to 9, characterized in that: The yield strength of the hot-rolled steel plate is ≥350MPa, the tensile strength is ≥490MPa, the yield strength ratio is 0.71-0.80, the impact energy at -40℃ is ≥190J, the wave splash corrosion rate is ≤0.006mm / year, the thickness of the interface transition layer is 0.5-10μm, and the interface shear strength is ≥252MPa.
11. The method for producing a hot-rolled steel sheet for building structures according to any one of claims 1 to 10, characterized in that: The method comprises the following steps performed in sequence: 1) Smelting and casting According to the composition of the base layer and the corrosion-resistant layer as described in claim 1, 2 or 3, the base layer and the corrosion-resistant layer are smelted and cast into blanks respectively; 2) Assembly The base blank and the corrosion-resistant layer blank are subjected to surface grinding and polishing, the base blank and the corrosion-resistant layer blank are bonded together, and the bonding surfaces of the blanks are welded and sealed all around to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are subjected to vacuum treatment; 3) Heating The composite blank is heated to 900-1000° C. to form an interface transition layer between the base layer and the corrosion-resistant layer; 4) Rolling The composite billet is rolled, wherein the pass reduction rate is 5-20%, preferably 10-20%, the cumulative reduction rate is ≥70%, and the final rolling temperature is 750-850°C; 5) Cooling After rolling, water cooling is adopted, the cooling rate is controlled at 5-20°C / s, and the final cooling temperature is 300-650°C to obtain a hot-rolled steel plate.
12. The method according to claim 11, characterized in that In step 2), the thickness of the corrosion-resistant layer is 0.5-20% of the thickness of the composite blank; and / or in step 3), the thickness of the interface transition layer formed between the base layer and the corrosion-resistant layer is 0.5-10 μm.
Citation Information
Patent Citations
Manufacturing method of titanium-steel-titanium two-sided composite plate
CN102773670A
Preparation method of titanium-steel clad plate
CN105107841A
Production method of titanium-steel composite plate
CN106269963A
A method for preparing titanium-steel composite plates
CN107626764B
A titanium-steel-titanium composite plate and its preparation method
CN109304367B
Cited By
Titanium steel composite plate manufacturing optimization method and system based on neural network model
CN120297159A
Production method of low-residual-stress steel plate for ship and ocean engineering
CN120945290A