Method for producing 2,5-furandicarboxylic acid

The use of a combination of platinum and palladium, along with optional transition metals, as catalysts for the selective oxidation of HMF addresses the issue of high intermediate residues and low FDCA production ratios, achieving efficient and cost-effective FDCA production by ensuring consistent catalytic acceleration across all reaction steps.

WO2024253178A1PCT designated stage expired Publication Date: 2024-12-12CUYUSYOJI +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/020784
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-09
Filing Date
2024-06-06
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Existing methods for producing 2,5-furandicarboxylic acid (FDCA) from 5-hydroxymethylfurfural (HMF) using a single metal catalyst result in high residual rates of intermediates and low production ratios due to varying catalytic effects across different reaction steps.

Method used

A method involving the selective oxidation of HMF's hydroxy and formyl groups using a combination of two or more metal catalysts, specifically platinum (Pt) and palladium (Pd), with optional transition metals like ruthenium (Ru), chromium (Cr), and others, supported on a carbon carrier, to enhance catalytic acceleration across all reaction steps.

Benefits of technology

This approach significantly reduces intermediate residues and achieves a high production ratio of FDCA by ensuring sufficient acceleration of oxidation reactions in all steps, improving efficiency and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024020784_12122024_PF_FP_ABST
    Figure JP2024020784_12122024_PF_FP_ABST
Patent Text Reader

Abstract

The method for producing 2,5-furandicarboxylic acid includes an oxidation step for selectively oxidizing a hydroxy group and a formyl group of 5-hydroxymethylfurfural in the presence of two or more metal catalysts and includes platinum and palladium as the metal catalysts. By using a combination of two or more specific metal catalysts in this way, the residual percentages of the intermediate forms DFF, HMFCA, and FFCA can be reduced, and FDCA can be obtained at a high generation ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing 2,5-furandicarboxylic acid

[0001] The present disclosure relates to a method for producing 2,5-furandicarboxylic acid (hereinafter referred to as "FDCA") from 5-hydroxymethylfurfural (hereinafter referred to as "HMF").

[0002] In recent years, in pursuit of a carbon-neutral society, high-performance bioplastics such as polyethylene furanoate (PEF) have been attracting attention as an alternative polymer to the petroleum-based polyethylene terephthalate (PET). PEF is a polymer produced by polycondensation or ring-opening polymerization of FDCA and ethylene glycol. FDCA, used as a raw material for PEF, can be produced, for example, by oxidizing HMF, which can be derived from cellulose. However, only limited catalysts are available that can convert the hydroxyl and formyl groups of HMF with high selectivity. Therefore, active research has been conducted on catalysts that can selectively oxidize the hydroxyl and formyl groups of HMF.

[0003] For example, Patent Document 1 discloses a method for producing FDCA by oxidizing HMF in the presence of a noble metal-containing metal catalyst supported on activated carbon, water, and oxygen, and describes the use of platinum as the noble metal.

[0004] Furthermore, Patent Document 2 discloses a method for producing FDCA from HMF, which includes the steps of oxidizing HMF in an alkaline aqueous solution containing caustic alkali to produce FDCA and its intermediate, and adding a chlorine-based oxidizing agent to the aqueous solution after the oxidation and oxidizing the intermediate to produce FDCA. Patent Document 2 also describes an example in which the method for oxidizing HMF is air oxidation using a noble metal catalyst, and uses a palladium-supported carbon catalyst as the noble metal catalyst.

[0005] Furthermore, Patent Document 3 discloses a method for producing FDCA, which comprises carboxylating a furan-based compound or its derivative containing a hydroxyl group and a carbonyl group in the presence of a catalyst containing noble metal nanoparticles in a support having a spinel structure. Patent Document 3 discloses HMF as an example of the furan-based compound and MnCo as an example of the support having a spinel structure. 2 O 4 However, ruthenium is listed as an example of a noble metal.

[0006] Thus, when FDCA is produced by oxidizing the hydroxyl group and formyl group of HMF, one type of metal catalyst has generally been used alone.

[0007] JP 2015-83559 A JP 2009-29751 A JP 2019-513538 A

[0008] However, when only one type of metal catalyst is used for the oxidation of HMF as in Patent Documents 1 to 3, a large amount of intermediates produced during the production of FDCA from HMF remains, resulting in a problem of a low production ratio of FDCA.

[0009] Therefore, an object of the present disclosure is to reduce the residual rate of intermediates and obtain FDCA at a high production rate in a method for producing FDCA by oxidizing HMF.

[0010] To achieve this objective, the technology disclosed in this specification is a method for producing 2,5-furandicarboxylic acid, which includes an oxidation step of selectively oxidizing the hydroxy group and formyl group of 5-hydroxymethylfurfural in the presence of two or more metal catalysts, the metal catalysts including platinum and palladium.

[0011] Here, the metal catalyst used in combination with platinum and palladium in the oxidation step preferably contains one or more transition metals (excluding platinum and palladium). In this case, the transition metal may be one or more metal elements selected from the group consisting of ruthenium, chromium, gold, silver, copper, iron, nickel, and cobalt. Furthermore, in the oxidation step, the total amount of the metal catalysts may be 0.01 mol to 0.1 mol per 1 mol of 5-hydroxymethylfurfural. Furthermore, the metal catalyst may contain a platinum catalyst in which platinum is supported on a carbon support and a palladium catalyst in which palladium is supported on a carbon support. Furthermore, the metal catalyst may contain a transition metal catalyst in which the transition metal is supported on a carbon support.

[0012] According to the present disclosure, in a method for producing FDCA by oxidation of HMF, by using a combination of two or more specific metal catalysts, the residual rate of intermediates can be reduced and FDCA can be obtained at a high production rate.

[0013] FIG. 1 shows the structures of raw materials, intermediates, and target products in the production of FDCA using HMF as a raw material.

[0014] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings.

[0015] [Method for Producing FDCA] The method for producing FDCA according to the present disclosure includes an oxidation step of selectively oxidizing the hydroxyl and formyl groups of HMF in the presence of two or more metal catalysts. In addition, the metal catalysts according to the present disclosure include at least two types of metal catalysts: platinum (Pt) and palladium (Pd).

[0016] Here, the process for producing FDCA using HMF will be described with reference to Figure 1. Figure 1 shows the structures of raw materials, intermediates, and the target product in the production of FDCA using HMF as the raw material.

[0017] (HMF) The raw material HMF is a furan compound containing one hydroxyl group and one formyl group. HMF can be synthesized using sugars such as glucose as raw materials. The sugars used as raw materials for HMF may be natural or synthetic, or a mixture of these. Specifically, the raw sugars may be selected from monosaccharides, disaccharides, and polysaccharides. These sugars may be used alone or in combination of two or more. Furthermore, sugars (aldohexoses) produced from pulp, rice husks, etc. may also be used as raw sugars for HMF. Pulp and rice husks are readily available, providing a stable supply of raw materials, allowing for efficient and low-cost synthesis of HMF. As a result, FDCA production efficiency and cost reduction can be achieved.

[0018] (Reaction Steps in the Oxidation Process) Furthermore, as shown in Figure 1, three types of intermediates are produced in the process of oxidizing HMF to produce FDCA. These intermediates include 2,5-diformylfuran (hereinafter referred to as "DFF"), 5-(hydroxymethyl)furan-2-carboxylic acid (hereinafter referred to as "HMFCA"), and 5-formyl-2-furancarboxylic acid (FFCA). HMF has one hydroxy group and one formyl group, and FDCA is produced when both of the two functional groups of HMF are oxidized to carboxyl groups (carboxylic acids), such as hydroxy group → formyl group → carboxyl group (alcohol → aldehyde → carboxylic acid) or formyl group → carboxyl group (aldehyde → carboxylic acid). That is, the production of FDCA from HMF goes through multiple reaction steps, such as the oxidation reaction of HMF → DFF, the oxidation reaction of HMF → HMFCA, the oxidation reaction of DFF → FFCA, the oxidation reaction of HMFCA → FFCA, and the oxidation reaction of FFCA → FDCA.

[0019] (Metal Component of Metal Catalyst) While investigating the optimum catalyst for the oxidation reaction of HMF, the present inventors came to the following conclusion. Because the catalysts that are most effective in the above-mentioned multiple reaction steps are different for each, when a single type of metal catalyst (Pt, Pd, Ru, etc.) is used alone, it is possible that the catalytic effect, i.e., the effect of accelerating the reaction rate, is likely to be exhibited in a specific reaction step, but the reaction acceleration effect in other reaction steps may be low. As a result, it is believed that the production ratio of intermediates such as DFF, HMFCA, and FFCA will be high, and the production ratio of FDCA will be low. For example, the present inventors speculate that when only a Pt catalyst is used, the oxidation reaction will proceed quickly in the HMF → DFF reaction step, but the effect of accelerating the oxidation reaction in the subsequent DFF → FFCA reaction step and the FFCA → FDCA reaction step will not be very significant.

[0020] Therefore, in the method for producing FDCA according to the present disclosure, a combination of two or more specific metal catalysts is used in the oxidation step, which selectively oxidizes the hydroxyl and formyl groups of HMF, thereby achieving a sufficient acceleration effect of the oxidation reaction in all reaction steps from HMF to FDCA. Specifically, by using two or more metal catalysts containing at least Pt and Pd as metal components in the oxidation step, it is believed that the combined use of two or more metal catalysts can achieve an acceleration effect of the oxidation reaction in reaction steps other than the HMF → DFF reaction step (e.g., the DFF → FFCA reaction step and the FFCA → FDCA reaction step), unlike when a Pt catalyst is used alone. This reduces the residual rates of the intermediates DFF, HMFCA, and FFCA, allowing FDCA to be produced at a high production rate. Note that combining multiple catalysts is not usually considered due to the risk of canceling out the effects of other catalysts.

[0021] In order to produce FDCA at a higher production rate, it is preferable that the metal catalyst (hereinafter referred to as the "promoter") used in combination with Pt and Pd in ​​the oxidation step contains one or more transition metals (excluding Pt and Pd). Examples of the promoter include transition metals of Groups 8, 9, 10, and 11 (hereinafter referred to as "late transition metals"), as well as chromium (Cr) and manganese (Mn). Among these transition metals, the promoter is preferably one or more metal elements selected from the group consisting of Ru, Cr, Au, Ag, Cu, Fe, Ni, and Co, with Ru being particularly preferred. The use of these promoter catalysts, combined with the catalytic effect of Pd, can dramatically accelerate the oxidation reactions in the reaction stages of HMF → HMFCA, DFF → FFCA, HMFCA → FFCA, and FFCA → FDCA. For example, the present inventors speculate that the use of a Ru catalyst together with a Pt catalyst and a Pd catalyst is particularly effective in accelerating the oxidation reaction in reaction steps such as DFF→FFCA and FFCA→FDCA.

[0022] (Support for Metal Catalyst) The metal catalyst of the present disclosure uses a metal catalyst in which a metal component is supported on a support. The support is used to increase the dispersibility of the metal component and improve reaction activity, but is also thought to have the effect of promoting the oxidation reaction through interaction with the reaction substrate. Supports that can be used for the metal catalyst of the present disclosure are not particularly limited, and examples include activated carbon (carbon), zeolite, silica, alumina, titania, zirconia, diatomaceous earth, and other metal oxides and porous bodies. From the viewpoint of enhancing the effect of accelerating the oxidation reaction from HMF to FDCA, it is preferable to use activated carbon as the support. The form of the activated carbon is not particularly limited, and may be powder, granular, fibrous, cylindrical, honeycomb, etc., but powder or granular forms are preferred from the viewpoint of improving workability during catalyst preparation and dispersibility in the reaction solution.

[0023] (Shape and Size of Metal Catalyst) The metal components and carriers of the metal catalyst of the present disclosure are as described above. Suitable metal catalysts of the present disclosure include a combination of a Pt / C catalyst in which Pt is supported on a carbon carrier and a Pd / C catalyst in which Pd is supported on a carbon carrier. The shape of the metal catalyst of the present disclosure is not particularly limited. However, from the viewpoints of improving workability during catalyst preparation and dispersibility in the reaction solution, as well as accelerating the oxidation reaction in flow synthesis to increase the FDCA production ratio, the Pt / C catalyst and Pd / C catalyst are preferably in the form of beads (particulates). In this case, the particle diameter of the bead-shaped Pt / C catalyst and Pd / C catalyst is preferably 100 μm to 500 μm, more preferably 100 μm to 400 μm, and even more preferably 200 μm to 300 μm.

[0024] Furthermore, when a promoter is used as the third metal catalyst, it is preferable that the catalyst contains a transition metal catalyst in which the transition metal is supported on a carbon support. In this case, the transition metal catalyst is preferably in the form of a powder, from the viewpoints of improving workability during catalyst preparation and dispersibility in the reaction solution, as well as accelerating the oxidation reaction and increasing the production ratio of FDCA.

[0025] (Amount of Metal Catalyst Used) In the oxidation step of the method for producing FDCA according to the present disclosure, the amount of metal catalyst used is not particularly limited. However, from the viewpoint of increasing the production ratio of FDCA and also taking into consideration economic efficiency, the total amount of metal catalyst relative to 1 mol of HMF is preferably 0.01 mol to 0.1 mol, more preferably 0.01 mol to 0.08 mol, and even more preferably 0.01 mol to 0.05 mol.

[0026] (Ratio of each metal catalyst) The amount of platinum catalyst used is preferably 20 mol% to 40 mol%, and more preferably 30 mol% to 40 mol%, when the total amount of metal catalysts is 100 mol%. The amount of palladium catalyst used is preferably 20 mol% to 40 mol%, and more preferably 30 mol% to 40 mol%, when the total amount of metal catalysts is 100 mol%. The amount of co-catalyst used is preferably 40 mol% or less (more than 0 mol%), and more preferably 20 mol% to 40 mol%, when the total amount of metal catalysts is 100 mol%. By having each catalyst in the above ratio range, the production ratio of FDCA can be increased and economic efficiency is also excellent.

[0027] (Method for preparing metal catalyst) The metal catalyst of the present disclosure can be prepared by a known method. For example, the metal catalyst of the present disclosure can be obtained by adsorbing the precursors of the above-mentioned Pt, Pd, other metals, etc., and, if necessary, precursors of other metal components onto a carrier such as activated carbon or Si, followed by a reduction treatment. In addition, commercially available products may be used as the metal catalyst of the present disclosure. Examples of commercially available products include those described in the Examples below.

[0028] As a method for adsorbing a metal component onto a support, known methods such as impregnation, deposition precipitation, ion exchange, and equilibrium adsorption can be used. The impregnation method is a method in which a support is immersed in a precursor solution of the metal component, and then the solvent is removed. The deposition precipitation method is a method in which a precursor of the metal component and a metal salt serving as a raw material for the metal oxide support are made into aqueous solutions, and this is added to an alkaline aqueous solution to precipitate hydroxide or carbonate precipitates. The ion exchange method is a method in which metal cations or complex anions are adsorbed onto hydroxy groups on the surface or H groups on the surface of a support having ion exchange capacity. + , O.H. - The equilibrium adsorption method is a method in which a support is immersed in an aqueous solution of a precursor of a metal component, and then the metal component that has not been adsorbed on the support surface is removed by filtration.

[0029] After the metal components are adsorbed onto the support as described above, the support may be washed with water, dried, and calcined as necessary, followed by a reduction treatment to prepare a metal catalyst. The drying and calcination temperatures may be appropriately set based on known conditions. The reduction treatment may be either a liquid-phase reduction method or a gas-phase reduction method, and the temperature and time of the reduction treatment may be appropriately set based on known conditions. Each metal component may be individually supported on a support, or multiple metal components may be simultaneously supported on a single support.

[0030] (Reaction Solution) In the method for producing FDCA of the present disclosure, a reaction solution is prepared by dissolving the raw material HMF in an aqueous solvent. The aqueous solvent is not particularly limited as long as it contains at least water and is capable of dissolving HMF, but from the viewpoints of production efficiency and economy, a polar solvent is preferable. Examples of polar solvents include water, polar aprotic organic solvents, ionic liquids, etc., with water being particularly preferable. Examples of aprotic organic solvents include dimethyl sulfoxide, dimethylacetamide, N,N-dimethylformamide, cyclohexanone, ethyl acetate, dichloromethane, etc. Examples of ionic liquids include imidazolium salts, pyridinium salts, etc.

[0031] The concentration of HMF in the reaction solution is preferably 0.050 M or more and 10 M or less, more preferably 0.10 M or more and 5.0 M or less, and even more preferably 0.20 M or more and 2.5 M or less, relative to the total amount of the reaction solution, from the viewpoints of improving the solubility of the product and the yield of FDCA, as well as preventing leaching of the catalyst (elution of metals such as Pt and Pd). In addition to the raw material HMF, the reaction solution may contain, for example, potassium carbonate (K 2 CO 3 ), sodium carbonate (Na 2 CO 3 A base such as potassium hydroxide (KOH) or sodium hydroxide (NaOH) may be added.

[0032] (Oxygen) The oxygen used in the oxidation step of the present disclosure is not particularly limited, and can be supplied to the reaction system as, for example, oxygen gas, air, or a gas obtained by diluting air with an inert gas such as nitrogen or argon to a predetermined oxygen concentration. Any method for supplying oxygen to the reaction system can be used as long as it can be supplied to the reaction system at a predetermined pressure and flow rate. The oxygen pressure during the reaction can be controlled, for example, by adjusting a back pressure regulator (BPR) connected to the reactor (in the case of flow synthesis) or by adjusting the pressure inside the autoclave (in the case of batch synthesis). The oxygen flow rate can be controlled by a mass flow controller connected to an oxygen cylinder or a mixer for oxygen and other gases. The oxygen concentration can also be controlled by mixing air with a diluting inert gas using a known mixer.

[0033] (Synthesis Method) The synthesis method for FDCA of the present disclosure is not particularly limited and may be either flow synthesis or batch synthesis. Flow synthesis is a synthesis method in which an oxidation reaction is carried out while continuously supplying the raw materials HMF and oxygen to a reactor. As the reactor, for example, a column reactor in which a metal catalyst is packed in a column can be used. Furthermore, the reaction solution after the oxidation reaction may be recovered all at once after the reaction is completed, or may be recovered continuously while the oxidation reaction is being carried out.

[0034] Batch synthesis is a synthesis method in which a reaction solution containing dissolved HMF as a raw material and a catalyst are all charged into a reactor in advance, and oxygen is passed through the reaction solution in the reactor to carry out an oxidation reaction. An autoclave, for example, can be used as the reactor. The reaction solution after the oxidation reaction is recovered all at once after the reaction is completed. Batch synthesis is suitable for synthesizing products with complex structures, but it is difficult to control the reaction and productivity, and it tends to have low energy efficiency. On the other hand, flow synthesis can improve energy efficiency by controlling the reaction time and productivity by adjusting the feed rate of the raw materials. As described above, flow synthesis is more energy efficient than batch synthesis and also reduces waste emissions. Therefore, flow synthesis is considered preferable from an industrial perspective in terms of energy conservation and productivity.

[0035] (Reaction Temperature) From the viewpoints of suppressing decomposition of HMF, increasing the production ratio of FDCA, and accelerating the reaction rate, the temperature of the oxidation reaction in the oxidation step is preferably 80°C or higher and 160°C or lower, more preferably 90°C or higher and 140°C or lower, and even more preferably 100°C or higher and 120°C or lower.

[0036] (Reaction Time) From the viewpoint of increasing the production ratio of FDCA and preventing catalyst leaching, the time of the oxidation reaction in the oxidation step is, for example, in the case of batch synthesis, preferably 8 to 20 hours, more preferably 10 to 18 hours, and even more preferably 12 to 16 hours. In the case of flow synthesis, the production ratio of FDCA can be increased even with a shorter reaction time. For example, depending on the reaction conditions, it is possible to complete the reaction of oxidizing HMF to FDCA in about several minutes to several tens of minutes.

[0037] (Pressure during reaction) From the viewpoint of increasing the production ratio of FDCA and improving productivity, the pressure during the oxidation reaction in the oxidation step is preferably 0.2 MPa or more and 1.5 MPa or less, more preferably 0.3 MPa or more and 1.4 MPa or less, and even more preferably 0.4 MPa or more and 1.3 MPa or less. The pressure during the reaction may be, for example, the indicated pressure of a plunger pump that sends the reaction solution to the reactor when a BPR is connected to the reactor.

[0038] (Amount of oxygen supplied) From the viewpoint of increasing the production ratio of FDCA and improving the yield, the amount of oxygen supplied in the oxidation step is preferably 8 equivalents or more and 17 equivalents or less, more preferably 9 equivalents or more and 16 equivalents or less, and even more preferably 10 equivalents or more and 15 equivalents or less, relative to the amount of HMF charged. Note that, in the method for producing FDCA according to the present disclosure, 1 equivalent of oxygen means the amount (mol) of oxygen supplied per 1 mol of HMF as a raw material.

[0039] (Method for Identifying FDCA) FDCA can be identified by H-NMR (Nuclear Magnetic Resonance) and C-NMR. NMR measurements can be performed using, for example, deuterated dimethyl sulfoxide (DMSO) as a measurement solvent and a JEOL ECS-400 (400 MHz (H-NMR), 10 MHz (C-NMR)) as a measurement instrument.

[0040] (Production ratio of FDCA) The production ratio of FDCA can be determined by analyzing the reaction solution after the oxidation reaction by high performance liquid chromatography (HPLC) or a mass spectrometer, and calculating the peak area ratios of the raw material HMF, the intermediate (a mixture of DFF, HMFCA, and FFCA), and the target product FDCA from the HPLC chart. The production ratios of HMF, the intermediate, and FDCA can be determined, for example, as follows.

[0041] The column may be, for example, a COSMOSIL Packed Column 5C18-MS-II (4.6 ID x 150 mm, Code: 38019-81) manufactured by Nacalai Tesque. The column temperature may be, for example, room temperature. The mobile phase may be, for example, a mixed solution of 5 mM aqueous sulfuric acid (Solution A) and acetonitrile (Solution B). The flow rate of the measurement solution may be, for example, 1 mL / min, and the measurement wavelength may be 280 nm (the maximum absorption wavelength of FDCA detected by a photodetector (Photodiode Array)).

[0042] Furthermore, gradient analysis may be used. In this case, the ratio of solution A to solution B in the mobile phase may be changed, for example, as follows: 0 minutes to 2 minutes: The concentration ratio of solution A to solution B is set to 95% solution A:5% solution B. 2 minutes to 12 minutes: The concentration ratio of solution A to solution B is changed linearly with time from 95% solution A:5% solution B to 88% solution A:12% solution B (linear gradient). 12 minutes to 20 minutes: The concentration ratio of solution A to solution B is set to 70% solution A:30% solution B. 20 minutes to 25 minutes: The concentration ratio of solution A to solution B is set to 95% solution A:5% solution B.

[0043] In addition to confirming the purity of FDCA in the gradient analysis described above, it is desirable to confirm that no other peaks are present in the range of 0% to 100% of Solution B in order to confirm the absence of impurities.

[0044] In addition, when performing HPLC analysis, by connecting a mass spectrometer to the HPLC measurement equipment, it is possible to simultaneously identify FDCA and measure the production ratio.

[0045] In the present disclosure, when the FDCA production ratio (peak area ratio in the HPLC chart) measured in this manner is 70% or more, it is determined that the FDCA production ratio is high and the object of the present disclosure has been achieved, and when it is 80% or more, it is determined that the effect of the present disclosure is excellent.

[0046] (Isolation and Purification of FDCA) FDCA synthesized by oxidation of HMF is dissolved in the reaction solution in an alkaline environment. Therefore, in order to use FDCA as a raw material for PEF and the like, it is necessary to isolate FDCA from the reaction solution. In order to isolate FDCA, an acid is added to the reaction solution to create an acidic environment, causing the FDCA dissolved in the reaction solution to crystallize and precipitate. The precipitated FDCA is collected, for example, by filtration, to obtain solid FDCA. When creating an acidic environment in the reaction solution, the acid may be added to the reaction solution in a state where it has been concentrated under reduced pressure. The acid added to create an acidic environment in the reaction solution is not particularly limited, and examples thereof include hydrochloric acid (HCl) and sulfuric acid (H 2 SO 4The collected FDCA may be purified to improve its purity, for example, by washing, recrystallization, drying, and, if necessary, decolorization.

[0047] [Uses of FDCA] The uses of FDCA produced by the production method of the present disclosure are not particularly limited, but can be suitably used, for example, as a raw material for producing PEF.

[0048] Although various modifications have been described above, these modifications may be combined together. The present disclosure is not limited to the above-described embodiments, and may be implemented in various forms without departing from the spirit and scope of the present disclosure.

[0049] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these examples.

[0050] [Preparation of Catalyst] (Pt / C Catalyst) "Pt / C, Beads (Pt 5%)" (Pt / C catalyst with a Pt content of 5% by mass) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used.

[0051] (Pd / C Catalyst) "Pd / C, Beads (Pd 5%)" (Pd / C catalyst with a Pd content of 5% by mass) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used.

[0052] (Ru / C catalyst) "Ruthenium 5% on Carbon (wetted with ca. 50% Water)" (Ru / C catalyst with a Ru content of 5% by mass) manufactured by Tokyo Chemical Industry Co., Ltd. (Cas No. 7440-18-8) was used.

[0053] [Synthesis of FDCA] FDCA was synthesized by oxidizing HMF as follows: After the oxidation reaction, the reaction solution was analyzed by HPLC to calculate the peak area ratios of the raw material HMF, the intermediate (a mixture of DFF, HMFCA, and FFCA), and the target product FDCA, thereby determining the production ratios of HMF, the intermediate, and FDCA.

[0054] Example 1 In Example 1, flow synthesis of FDCA was performed by oxidizing HMF using a ternary catalyst consisting of a particulate Pt / C catalyst (particle size: 200 μm), a particulate Pd / C catalyst (particle size: 200 μm), and a powdered Ru / C catalyst. Specifically, the raw materials HMF and 1 equivalent of potassium carbonate relative to HMF were first added to distilled water, and the reaction solution was then diluted with water to a 0.1 M HMF concentration. A column (column reactor) with an inner diameter of 4 mm and a length of 5 cm was used as the reactor. Three types of metal catalysts were packed into this column reactor in a molar ratio of Pt / C catalyst:Pd / C catalyst:Ru / C catalyst of 1:1:1. The total amount of metal catalyst packed was 420 mg (0.16 mmol). The loading amount of each metal catalyst was 111.1 mg (0.052 mmol) for the Pd / C catalyst, 203.9 mg (0.052 mmol) for the Pt / C catalyst, and 104.3 mg (0.052 mmol) for the Ru / C catalyst.

[0055] Next, the reaction solution was continuously pumped into a column reactor packed with a metal catalyst using a plunger pump, while 12 equivalents of oxygen relative to the raw material HMF were continuously supplied to carry out the oxidation reaction of HMF. The flow rate of the reaction solution was adjusted to 0.10 mL / min. The flow rate of oxygen was adjusted to 1.2 mL / min using a mass flow controller. The reaction temperature was maintained at 100°C by heating the column reactor. The pressure during the reaction was 0.3 MPa, as confirmed by connecting a 20 psi (0.14 MPa) BPR to the column reactor and checking the indicated pressure of the plunger pump. The residence time in the oxidation reaction was 3.1 minutes, and the reaction time was 10 minutes. That is, the outflowing reaction solution was collected for 10 minutes.

[0056] HPLC analysis of the reaction solution after the oxidation reaction revealed that the production ratio of HMF was 0, the production ratio of the intermediate was 11%, and the production ratio of FDCA was 89%. That is, FDCA was obtained as the main product in Example 1. The type and amount of the metal catalyst and the production ratio of each compound in Example 1 are shown in Table 1 below.

[0057] (Example 2, Comparative Examples 1 to 5) In Example 2 and Comparative Examples 1 to 5, to confirm the difference in the FDCA production ratio depending on the number and combination of metal catalysts, batch synthesis of FDCA was performed by oxidizing HMF using one or more metal catalysts selected from Pt / C catalyst, Pd / C catalyst, and Ru / C catalyst. All metal catalysts were in powder form. Specifically, the air in a 15 mL screw-cap test tube was first purged with nitrogen and then with oxygen. Next, 0.5 mmol (63 mg) of HMF, 1 equivalent of potassium carbonate (0.5 mmol, 69 mg) relative to HMF, 1.0 mL of distilled water, and a predetermined amount of each metal catalyst were added to the screw-cap test tube whose interior had been purged with oxygen to prepare a reaction solution.

[0058] In Example 2, the amount of each metal catalyst added was 40 mg (2 mol%) of Pt / C catalyst, 20 mg (2 mol%) of Pd / C catalyst, and 20 mg (2 mol%) of Ru / C catalyst. In Comparative Example 1, the amount of Pt / C catalyst was 100 mg (5 mol%). In Comparative Example 2, the amount of Pd / C catalyst was 50 mg (5 mol%). In Comparative Example 3, the amount of Pt / C catalyst was 50 mg (5 mol%). In Comparative Example 4, the amount of Pt / C catalyst was 40 mg (2 mol%) and the amount of Ru / C catalyst was 20 mg (2 mol%). In Comparative Example 5, the amount of Pd / C catalyst was 20 mg (2 mol%) and the amount of Ru / C catalyst was 20 mg (2 mol%).

[0059] Next, the screw-cap test tube was capped with a septum, and a balloon filled with oxygen gas was attached to the screw-cap test tube. The oxygen gas pressure in the balloon was 1 atmosphere. The screw-cap test tube was then placed in an oil bath, and the oxidation reaction of HMF was carried out at 100°C for 15 hours.

[0060] The reaction solution after the oxidation reaction was filtered through Celite, and a portion was collected and analyzed by HPLC. The types and amounts of metal catalysts and the production ratios of each compound in Example 2 and Comparative Examples 1 to 5 are shown in Table 1 below. As shown in Table 1, in Example 2, which contained at least Pt and Pd as metal catalysts and Ru as a promoter, the production ratio of FDCA was very high at 94%, whereas in Comparative Examples 1 to 3, which contained only one type of metal catalyst, and in Comparative Examples 4 and 5, which contained two or more types of metal catalysts but did not contain either Pt or Pd, the production ratio of FDCA was low at less than 70%.

[0061] In Examples 3 to 8, in order to confirm the difference in the production ratio of FDCA depending on the ratio of each metal catalyst, batch synthesis of FDCA was carried out by oxidizing HMF using three types of metal catalysts: Pt / C catalyst, Pd / C catalyst, and Ru / C catalyst. All of the metal catalysts used were in powder form.

[0062] A reaction solution was prepared by adding 1 equivalent of potassium carbonate relative to the raw material HMF and a predetermined amount of each metal catalyst to distilled water, and diluting the mixture with distilled water to a HMF concentration of 0.1 M. The amount of each metal catalyst added was as shown in Table 1 below.

[0063] Next, the screw-cap test tube was capped with a septum, and a balloon filled with oxygen gas was attached to the screw-cap test tube. The oxygen gas pressure in the balloon was 1 atmosphere. The screw-cap test tube was then placed in an oil bath, and the oxidation reaction of HMF was carried out at 100°C for 16 hours.

[0064] The reaction solution after the oxidation reaction was filtered through Celite, and a portion was collected and analyzed by HPLC. The types and amounts of metal catalysts and the production ratios of each compound in Examples 3 to 8 are shown in Table 1 below. As shown in Table 1, the production ratio of FDCA was high, at 80% or more, in all Examples.

[0065] (Examples 9 and 10) In Examples 9 and 10, in order to confirm the difference in the production ratio of FDCA depending on the ratio of each metal catalyst, batch synthesis of FDCA was carried out by oxidizing HMF using three types of metal catalysts: Pt / C catalyst, Pd / C catalyst, and Ru / C catalyst. All of the metal catalysts used were in powder form. Specifically, the oxidation reaction of HMF was carried out in the same manner as in Example 2, except that the amounts of metal catalyst added were as shown in Table 1 below, and the reaction time was 5 hours.

[0066] The reaction solution after the oxidation reaction was filtered through Celite, and a portion was collected and analyzed by HPLC. The types and amounts of metal catalysts used in Examples 9 and 10, as well as the production ratios of each compound, are shown in Table 1 below. As shown in Table 1, the production ratio of FDCA was high, at 80% or more, in all Examples. In particular, when the ratio of Pt / C catalyst:Pd / C catalyst:Ru / C catalyst was 1:1:1, an extremely high production ratio of FDCA was obtained.

[0067] In Examples 11 to 13, in order to confirm the difference in the production ratio of FDCA depending on the type of transition metal used as a promoter in a ternary catalyst containing Pt and Pd, batch synthesis of FDCA was carried out by oxidizing HMF using three types of metal catalysts: a Pt / C catalyst, a Pd / C catalyst, and the metal catalysts shown in Table 1. All of the metal catalysts used were in powder form.

[0068] Specifically, the air in a 15 mL screw-cap test tube was first replaced with nitrogen and then replaced with oxygen. Subsequently, 0.5 mmol (63 mg) of HMF, 1 equivalent of potassium carbonate (0.5 mmol, 69 mg) relative to HMF, 1.0 mL of distilled water, 20 mg (1 mol%) of a Pt / C catalyst with a Pt content of 5% by mass, 11 mg (1 mol%) of a Pd / C catalyst with a Pd content of 5% by mass, and 5 mol% of various promoters were added to the screw-cap test tube whose interior had been replaced with oxygen to prepare a reaction solution. In Example 11, CrO 3 In Example 12, Ag 2 O, Cu in Example 13 2 O was used.

[0069] Next, the screw-cap test tube was capped with a septum, and a balloon filled with oxygen gas was attached to the screw-cap test tube. The oxygen gas pressure in the balloon was 1 atmosphere. The screw-cap test tube was then placed in an oil bath, and the oxidation reaction of HMF was carried out at 100°C for 16 hours.

[0070] The reaction solution after the oxidation reaction was filtered through Celite, and a portion was collected and analyzed by HPLC. The types and amounts of metal catalysts and the production ratios of each compound in Examples 11 to 13 are shown in Table 1 below. As shown in Table 1, the production ratio of FDCA was high, at 80% or more, in all Examples. In particular, the use of CrO as a promoter 3 or Ag 2 In Examples 12 and 13, in which O was used, an extremely high FDCA production ratio was obtained.

[0071]

[0072] Reference Examples 1 to 6 In Reference Examples 1 to 6, in order to confirm the tendency of differences in the production ratio of FDCA depending on the type of transition metal used as a promoter in a binary or ternary catalyst containing Pt and Pd, batch synthesis of FDCA was carried out by oxidizing HMF using three types of metal catalysts: a Pt / C catalyst, a Pd / C catalyst, and the metal catalysts shown in Table 2 below. All of the metal catalysts used were in powder form.

[0073] Specifically, the air in a 15 mL screw-cap test tube was first purged with nitrogen and then with oxygen. Subsequently, 0.5 mmol (63 mg) of HMF, 1.1 equivalents of potassium carbonate (0.5 mmol, 69 mg) relative to HMF, 1.0 mL of distilled water, 40 mg (1 mol%) of a Pt / C catalyst with a Pt content of 5% by mass, 11 mg (1 mol%) of a Pd / C catalyst with a Pd content of 10% by mass, and 5 mol% of each of the various cocatalysts (listed in Table 1) were added to the screw-cap test tube whose interior had been purged with oxygen to prepare a reaction solution. In Reference Example 6, a binary catalyst was used, and no cocatalyst was used.

[0074] Next, the screw-cap test tube was capped with a septum, and a balloon filled with oxygen gas was attached to the screw-cap test tube. The pressure of the oxygen gas in the balloon was 1 atmosphere. The screw-cap test tube was then placed in an oil bath, and the oxidation reaction of HMF was carried out at 100°C for 5 hours. In Reference Examples 1 to 6, the reaction time was shortened to 5 hours in order to confirm only the tendency of the oxidation reaction.

[0075] The reaction solution after the oxidation reaction was filtered through Celite, and a portion was collected and analyzed by HPLC. The types and amounts of metal catalysts and the production ratios of each compound in Reference Examples 1 to 6 are shown in Table 2 below. As shown in Table 2, when a Ru / C catalyst was used (Reference Example 1), HMF was completely consumed (reacted), and the production ratio of FDCA was the highest. In addition, CrO 3 Catalyst and Ag 2 When the TiO catalyst was used (Reference Examples 2 and 3), HMF was almost completely consumed (reacted) as in the case of using the Ru / C catalyst, but the proportion of intermediates was higher than in the case of using the Ru / C catalyst. 2 When a catalyst was used (Reference Example 5), the amount of HMF consumed was almost the same as when a binary catalyst was used (Reference Example 6), but more of the intermediate was oxidized to FDCA than when a binary catalyst was used. 5 H 6 NO 3 When a ClCr catalyst was used (Reference Example 5), the tendency was almost the same as when a binary catalyst was used (Reference Example 6).

[0076]

Claims

1. A method for producing 2,5-furandicarboxylic acid, comprising an oxidation step of selectively oxidizing the hydroxyl and formyl groups of 5-hydroxymethylfurfural in the presence of two or more metal catalysts, the metal catalysts including platinum and palladium.

2. The method for producing 2,5-furandicarboxylic acid according to claim 1, wherein the metal catalyst used in combination with platinum and palladium contains one or more transition metals (excluding platinum and palladium).

3. The method for producing 2,5-furandicarboxylic acid according to claim 2, wherein the transition metal is one or more metal elements selected from the group consisting of ruthenium, chromium, gold, silver, copper, iron, nickel and cobalt.

4. A method for producing 2,5-furandicarboxylic acid according to any one of claims 1 to 3, wherein the total amount of the metal catalyst is 0.01 mol to 0.1 mol per 1 mol of 5-hydroxymethylfurfural.

5. The method for producing 2,5-furandicarboxylic acid according to any one of claims 1 to 3, wherein the metal catalyst comprises a platinum catalyst in which platinum is supported on a carbon support and a palladium catalyst in which palladium is supported on a carbon support.

6. The method for producing 2,5-furandicarboxylic acid according to claim 2 or 3, wherein the metal catalyst comprises a transition metal catalyst in which the transition metal is supported on a carbon support.

Citation Information

Patent Citations

  • Preparation method of 5-hydroxymethyl furoic acid and 2,5-furandicarboxylic acid

    CN103626726A

  • Selective oxidization method for furan alcohol or aldehyde compounds

    CN108299358A

  • Method of producing 5-hydroxymethylfurfural oxide

    JP2013203666A

  • Method for producing 2,5-furan dicarboxylic acid

    JP2015083559A

  • Method for producing carbonyl compound

    JP2019142842A