High-temperature-resistant filtrate reducer, water-based drilling fluid and use of the high-temperature-resistant filtrate reducer in drilling engineering in high-temperature subsurface environments

By blending carboxymethyl cellulose with water-soluble polymer containing epoxy groups, self-crosslinking of cellulose filter reduction loss agent at high temperature is achieved, and the problem of insufficient temperature resistance of cellulose filter reduction loss agent in high temperature environment is solved, and an efficient and environmentally friendly filter reduction effect is achieved.

WO2025140017A1PCT designated stage expired Publication Date: 2025-07-03CHINA NAT PETROLEUM CORP +1

Patent Information

Application Number
PCT/CN2024/140797
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-25
Filing Date
2024-12-20
Publication Date
2025-07-03

AI Technical Summary

Technical Problem

The existing cellulose filter reduction agents have insufficient temperature resistance in high temperature environments, and the modification methods are complex, high cost and unenvironmental, making it difficult to meet the needs of underground high-temperature drilling projects.

Method used

Carboxymethyl cellulose is blended with a water-soluble polymer containing epoxy groups, and carboxymethyl cellulose is self-crosslinked at high temperature to improve the rigidity of the cellulose main chain. It is self-crosslinked in a downhole high-temperature environment through a ring-opening coupling reaction to form an anti-high temperature filter loss agent.

Benefits of technology

Maintain excellent filtration loss reduction performance at high temperatures, reduce the impact of hydrolysis and chain breaking of cellulose main chain, simplify operation, reduce costs, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024140797_03072025_PF_FP_ABST
    Figure CN2024140797_03072025_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present invention are a high-temperature-resistant filtrate reducer, a water-based drilling fluid and the use of the high-temperature-resistant filtrate reducer in drilling engineering in high-temperature subsurface environments. The filtrate reducer comprises carboxymethyl cellulose and a water-soluble polymer containing epoxy, and an open-loop coupling reaction of carboxyl and epoxy groups in high-temperature environments is utilized to induce in-situ self-crosslinking of carboxymethyl cellulose in high-temperature deep downhole environments, so that the filtrate loss reduction performance of the filtrate reducer at high temperatures is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Application of high temperature resistant fluid loss reducer, water-based drilling fluid and high temperature resistant fluid loss reducer in underground high temperature environment drilling projects

[0001] Cross-reference information

[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on December 25, 2023, with application number 202311793322.1 and invention name “Fluid loss reducer, water-based drilling fluid and application of fluid loss reducer in underground high temperature environment drilling engineering”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present invention relates to a high-temperature resistant fluid loss reducer, a water-based drilling fluid and application of the high-temperature resistant fluid loss reducer in underground high-temperature environment drilling engineering, belonging to the technical field of oilfield chemistry. Background Art

[0004] With the rapid increase in demand for oil and natural gas and the increasing depletion of shallow oil and gas resources, deep oil and gas exploration and development is a crucial path for the sustainable development and energy security of my country's oil industry. However, as exploration and development progresses deeper, formation temperatures continue to rise. During underground high-temperature drilling operations, high temperatures severely damage drilling fluid properties. This loss of drilling fluid performance can easily lead to complex conditions such as wellbore instability and pipe sticking, severely impacting the safety, cost-effectiveness, and efficiency of drilling operations. Furthermore, exposure of chemical treatment agents in drilling fluids to soil, surface water, and groundwater can cause significant environmental pollution. With growing environmental awareness and increasingly stringent environmental regulations worldwide, green and environmentally friendly drilling fluid treatment agents and systems have become a future trend. Therefore, developing drilling fluid systems that meet the demands of drilling operations under complex high-temperature, high-pressure conditions while also meeting environmental requirements is a common technical challenge both domestically and internationally. This challenge holds significant significance and application value for the exploration and development of deep oil and gas resources.

[0005] Fluid loss control agents are core treatment agents for drilling fluids. Researching and developing environmentally friendly, high-temperature-resistant fluid loss control agent systems is crucial for maintaining and controlling fluid loss in high-temperature, high-pressure drilling environments and is a key technology for the success of underground high-temperature drilling. Fluid loss control agents primarily include synthetic polymer-based fluid loss control agents and bio-based natural polymer-based fluid loss control agents. Due to their widespread availability, low cost, biodegradability, and environmental friendliness, the development and utilization of natural polymers has become a key research direction in fluid loss control technology. Among the numerous natural polymer materials, cellulose and its derivatives, which are inexpensive and most abundant, have been widely used to prepare drilling fluid treatment agents such as fluid loss control agents. In particular, carboxymethyl cellulose (CMC) has become one of the most widely used fluid loss control agents [Carbohydrate Polymers, 2021, 259, 117740; Polymer Reviews, 2022, 62, 585-625; ACS Applied Materials Interfaces 2015, 7, 8, 5006–5016]. However, the cellulose backbone is linked by ether bonds. Under high temperatures and shear, the cellulose backbone is susceptible to thermal oxidative degradation or hydrolysis, leading to chain breakage and loss of fluid loss control. Furthermore, the cellulose backbone lacks rigidity and easily warps at high temperatures, reducing its ability to disperse and aggregate clay particles at high temperatures, resulting in a loss of control over fluid loss and rheological properties of the drilling fluid [Carbohydrate Polymers, 2021, 259, 117740; Polymer Reviews, 2022, 62, 585-625].

[0006] In the existing technology, in order to improve the fluid loss reduction performance of cellulose fluid loss additives in high-temperature underground environments, researchers at home and abroad have carried out a lot of research on the physical and chemical modification of cellulose polymer chains, mainly using reactions such as esterification, etherification, sulfonation, cross-linking, and graft copolymerization of the hydroxyl groups on the glucose units in the cellulose molecular chains [Journal of Applied Polymer Science 2012,124,2340-2347; Carbohydrate Polymers,2021,259,117740; Carbohydrate Polymers 2020,229,115465; RSC Adv.,2020,10,43204-43212; Polymer Reviews,2022,62,585-625; International Journal of Molecular Sciences 2021,22,352; Carbohydrate Polymers 2009,78,95–99].

[0007] However, these modification methods still have limited potential for improving the temperature resistance of cellulose fluid loss additives, and the temperature resistance of modified cellulose fluid loss additives is generally below 150°C. Furthermore, modification methods such as graft copolymerization also present complex processes, the introduction of non-degradable and environmentally unfriendly polymer segments, and significant impacts on the rheological properties of drilling fluids, hindering drilling operations. Furthermore, currently, most conventional modification methods are only applicable to cellulose with a large number of hydroxyl groups in the main chain, while research on modification methods for the most commonly used fluid loss additives, such as carboxymethyl cellulose, which contains a large number of carboxyl groups on the polymer chain, is still limited. Therefore, the research and development of environmentally friendly fluid loss additives with excellent high-temperature fluid loss performance is a critical issue that needs to be urgently addressed in fields such as oilfield chemistry and drilling engineering. Summary of the Invention

[0008] The main purpose of the present invention is to provide a high-temperature resistant fluid loss reducer, a water-based drilling fluid, and the application of the high-temperature resistant fluid loss reducer in underground high-temperature environment drilling projects, so as to solve the problems of insufficient temperature resistance, environmental unfriendliness, high cost and complicated operation in the temperature-resistant modification of existing cellulose fluid loss additives.

[0009] In order to achieve the above object, according to one aspect of the present invention, a high temperature resistant fluid loss reducer is provided, which comprises carboxymethyl cellulose and a water-soluble polymer containing an epoxy group, wherein the water-soluble polymer containing an epoxy group is selected from (CH3CH2CCOOCH2CHCH2O) x -[CH2CHCOO(CH2CH2O) n CH3] y、(CH3CH2CCOOCH2CHCH2O) x -[CH3CH2CCOO(CH2CH2O) n CH3] y 、(CH3CH2CCOOCH2CHCH2O) x -[CH3CH2CCOOCH2CH2N + (CH3)2CH2CH2CH2SO3 - ] y wherein x:y are each independently 1:20 to 5, and n is each independently 3 to 20; and the number average molecular weight of the water-soluble polymer containing epoxy groups is 5,000 to 50,000, for example, 5,000, 10,000, 15,000, 20,000, 25,000, 30,000, 35,000, 40,000, 45,000, or 50,000.

[0010] (CH3CH2CCOOCH2CHCH2O) x -[CH2CHCOO(CH2CH2O) n CH3] y Having the structure shown in formula I1;

[0011] (CH3CH2CCOOCH2CHCH2O) x -[CH3CH2CCOO(CH2CH2O) n CH3] y Having the structure shown in formula I2;

[0012] (CH3CH2CCOOCH2CHCH2O) x -[CH3CH2CCOOCH2CH2N + (CH3)2CH2CH2CH2SO3 - ] y Having the structure shown in formula I3;

[0013] First of all, carboxymethyl cellulose is not only easy to obtain and environmentally friendly, but more importantly, it contains a large number of carboxyl groups on its polymer chain, so there is no need to perform any chemical modification on it. By simply blending it with the above-mentioned water-soluble polymer containing epoxy groups of the present invention, the carboxymethyl cellulose (containing carboxyl groups) and the water-soluble polymer (containing epoxy groups) can be used to undergo a ring-opening coupling reaction in a subsequent underground high-temperature, water-containing environment, inducing the carboxymethyl cellulose to undergo in-situ self-crosslinking in the underground high-temperature environment, reducing the impact of high-temperature hydrolysis and chain scission of the cellulose main chain while increasing the rigidity of the cellulose polymer main chain, thereby significantly improving the temperature resistance of the fluid loss reducer on the basis of lower cost, simpler operation, and more environmentally friendly, so that it can maintain excellent fluid loss reduction performance even in high-temperature working environments. The above-mentioned ring-opening coupling reaction is shown in the following formula:

[0014] Secondly, it should be further explained that, unlike the traditional pre-crosslinking method, the self-crosslinking reaction of the above-mentioned fluid loss reducer of the present invention is carried out in a subsequent high-temperature environment downhole. The viscosity of the carboxymethyl cellulose before crosslinking is maintained at the viscosity of the carboxymethyl cellulose itself. After crosslinking, the viscosity of the carboxymethyl cellulose can be maintained at the high temperature downhole, and the influence of the fluid loss reducer on the rheological properties of the drilling fluid is avoided.

[0015] In a preferred embodiment, the weight ratio of the water-soluble polymer containing epoxy groups to the carboxymethyl cellulose is 1:10 to 1:5, for example, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10.

[0016] In an optional embodiment, the water-soluble polymer containing epoxy groups represented by formula I1 can be prepared by free radical copolymerization of a functional monomer containing epoxy groups, glycidyl methacrylate, and a hydrophilic monomer, polyethylene glycol methyl ether acrylate. The synthesis route is as follows:

[0017] Specifically, the free radical copolymerization of glycidyl methacrylate and polyethylene glycol methyl ether acrylate is to dissolve glycidyl methacrylate and polyethylene glycol methyl ether acrylate in a solvent (such as N,N-dimethylformamide) according to a stoichiometric ratio, add an initiator (such as azobisisobutyronitrile) for polymerization, and then precipitate in icy ether and vacuum dry to obtain the above-mentioned water-soluble polymer containing epoxy groups.

[0018] During the preparation process, the number average molecular weight of polyethylene glycol in the hydrophilic monomer polyethylene glycol methyl ether acrylate is preferably 130 to 1100, that is, the number of -CH2CH2O- units is 3 to 20, and polyethylene glycol methyl ether acrylate with a number average molecular weight of polyethylene glycol of 440 is further preferred, that is, the number of -CH2CH2O- units is 10; the molar ratio of glycidyl methacrylate to polyethylene glycol methyl ether acrylate is preferably 1:20 to 5, and more preferably 1:11 to 9; the polymerization temperature is preferably 60 to 80° C. and the polymerization time is preferably 12 to 24 hours.

[0019] In another optional embodiment, the water-soluble polymer containing epoxy groups represented by formula I2 can be prepared by free radical copolymerization of a functional monomer containing epoxy groups, glycidyl methacrylate, and a hydrophilic monomer, polyethylene glycol methyl ether methacrylate. The synthesis route is as follows:

[0020] Specifically, glycidyl methacrylate and polyethylene glycol methyl ether methacrylate are dissolved in a solvent (such as N,N-dimethylformamide) in a stoichiometric ratio, an initiator (such as azobisisobutyronitrile) is added for polymerization, and then the mixture is precipitated in ice ether and vacuum-dried to obtain the above-mentioned water-soluble polymer containing epoxy groups.

[0021] During the preparation process, the number average molecular weight of polyethylene glycol in the hydrophilic monomer polyethylene glycol methyl ether methacrylate is preferably 130 to 1100, that is, the number of -CH2CH2O- units is 3 to 20, and polyethylene glycol methyl ether acrylate with a number average molecular weight of polyethylene glycol is further preferred to be 440, that is, the number of -CH2CH2O- units is 10; the molar ratio of glycidyl methacrylate to polyethylene glycol methyl ether methacrylate is preferably 1:20 to 5, more preferably 1:11 to 9; the polymerization temperature is preferably 50 to 80°C and the polymerization time is 8 to 24 hours.

[0022] In another optional embodiment, the water-soluble polymer containing epoxy groups shown in Formula I3 can be prepared by free radical copolymerization of a functional monomer containing epoxy groups, glycidyl methacrylate, and a hydrophilic monomer, methacryloylethyl sulfobetaine. The synthesis route is as follows:

[0023] Specifically, the free radical copolymerization of glycidyl methacrylate and methacryloylethyl sulfobetaine is to dissolve glycidyl methacrylate and methacryloylethyl sulfobetaine in a solvent (e.g., a mixed solution of water and N,N-dimethylformamide, with a volume ratio of 5 to 20:1) in a stoichiometric ratio, add an initiator (e.g., ammonium persulfate and / or potassium persulfate) for polymerization, and then dialyze in water and freeze-dry to obtain the above-mentioned water-soluble polymer containing epoxy groups.

[0024] During the preparation process, the molar ratio of glycidyl methacrylate to methacryloylethyl sulfobetaine is preferably 1:20-5, more preferably 1:11-9; the polymerization temperature is preferably 40-80° C., and the polymerization time is preferably 16-48 h.

[0025] It is further explained that the above-mentioned water-soluble polymer containing epoxy groups of the present invention can be obtained by copolymerizing commercially available glycidyl methacrylate and a hydrophilic monomer. The polymerization reaction is simple and easy, and the epoxy group content is easy to control. It is suitable for large-scale industrial production and has a better prospect for industrial application.

[0026] The present invention does not impose any particular limitation on carboxymethyl cellulose. The carboxymethyl cellulose used in the present invention is currently well-known, commercially available, and widely used carboxymethyl cellulose. Considering the optimization of the fluid loss additive's solubility, thickening properties, stability, acid resistance, and salt resistance, carboxymethyl cellulose with a carboxymethyl degree of substitution of 0.5 to 2.0 and a glucose unit degree of polymerization of 200 to 1000 is preferred.

[0027] To achieve the above objectives, according to another aspect of the present invention, a water-based drilling fluid is provided, comprising the aforementioned high-temperature resistant fluid loss additive, wherein the weight content of the high-temperature resistant fluid loss additive in the water-based drilling fluid is 1 to 6 wt %. Based on the aforementioned reasons, the water-based drilling fluid of the present invention has excellent temperature resistance.

[0028] To achieve the above objectives, according to another aspect of the present invention, a high-temperature resistant fluid loss additive is provided for use in underground high-temperature drilling operations, where the high-temperature environment is 150-220°C. Based on the aforementioned reasons, the fluid loss additive exhibits excellent fluid loss reduction performance in high-temperature underground environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] FIG1 shows the water-soluble polymer prepared in Example 1 of the present invention. 1 HNMR nuclear magnetic spectrum.

[0030] FIG2 shows the FTIR spectrum of the water-soluble polymer prepared in Example 1 of the present invention.

[0031] FIG3 shows the water-soluble polymer prepared in Example 9 of the present invention. 1 HNMR nuclear magnetic spectrum.

[0032] FIG4 shows the FTIR spectrum of the water-soluble polymer prepared in Example 9 of the present invention.

[0033] FIG5 shows a photo of the filter cake after aging at 160° C. for 16 h in Example 16 of the present invention.

[0034] FIG6 shows a photo of the filter cake after aging at 160° C. for 16 hours in Example 23 of the present invention. DETAILED DESCRIPTION

[0035] In order to have a clearer understanding of the technical features, objectives and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be understood as limiting the scope of implementation of the present invention.

[0036] Preparation Example of Water-Soluble Polymer Containing Epoxy Groups

[0037] Example 1

[0038] Glycidyl methacrylate (1.42 g, 10 mmol), polyethylene glycol methyl ether acrylate with three ethylene glycol units (10.9 g, 50 mmol), and AIBN (0.24 g, 1.5 mmol) were added to a 100 mL reaction flask. 80 mL of N,N-dimethylformamide was then added and dissolved. The system was then vacuumed and filled with nitrogen three times to remove oxygen. The reaction was then allowed to proceed at 80°C for 12 hours. The solution was then slowly added dropwise to a large amount of icy ether for precipitation. After centrifugation and discarding the supernatant, the white precipitate was dried in a vacuum oven for 24 hours to yield a water-soluble polymer containing epoxy groups.

[0039] The water-soluble polymer containing epoxy groups is prepared by using 1 HNMR characterization, with the NMR spectrum shown in Figure 1, shows characteristic H-spectral peaks at the methylene and methine groups in the polymer backbone, the adjacent methylene and methine groups of the epoxy group, and the methylene group in the polyethylene glycol unit. This confirms the successful preparation of a water-soluble polymer containing epoxy groups, with a number-average molecular weight of approximately 12,000.

[0040] The resulting water-soluble polymer containing epoxy groups was characterized by FTIR, and the spectrum is shown in Figure 2. Characteristic peaks for methine and methylene groups in the polymer backbone, epoxy bonds, and carbon-oxygen bonds in the polyethylene glycol unit are all observed in Figure 2, confirming the successful preparation of a water-soluble polymer containing epoxy groups.

[0041] Example 2

[0042] Glycidyl methacrylate (0.284 g, 2 mmol), polyethylene glycol methyl ether acrylate with three ethylene glycol units (8.72 g, 40 mmol), and AIBN (0.164 g, 1 mmol) were added to a 100 mL reaction flask. 80 mL of N,N-dimethylformamide was then added and dissolved. The system was then vacuumed and nitrogen-filled three times to remove oxygen. Polymerization was then carried out at 60°C for 24 hours. The solution was then slowly added dropwise to a large amount of glacial ether for precipitation. After centrifugation and the supernatant was discarded, the white precipitate was dried in a vacuum oven for 24 hours to yield a water-soluble polymer containing epoxy groups with a number-average molecular weight of approximately 25,000.

[0043] Example 3

[0044] Glycidyl methacrylate (0.284 g, 2 mmol), polyethylene glycol methyl ether acrylate with 10 ethylene glycol units (10.52 g, 20 mmol), and AIBN (0.328 g, 2 mmol) were added to a 150 mL reaction flask. 80 mL of N,N-dimethylformamide was then added and dissolved. The system was then vacuumed and filled with nitrogen three times to remove oxygen. Polymerization was then carried out at 60°C for 24 hours. The solution was then slowly added dropwise to a large amount of glacial ether for precipitation. After centrifugation and the supernatant was discarded, the white precipitate was dried in a vacuum oven for 24 hours to yield a water-soluble polymer containing epoxy groups with a number-average molecular weight of approximately 45,000.

[0045] Example 4

[0046] Glycidyl methacrylate (0.284 g, 2 mmol), polyethylene glycol methyl ether acrylate with 20 ethylene glycol units (11.86 g, 10 mmol), and AIBN (0.328 g, 2 mmol) were added to a 150 mL reaction flask. 80 mL of N,N-dimethylformamide was then added and dissolved. The system was then vacuumed and filled with nitrogen three times to remove oxygen. Polymerization was then carried out at 80°C for 12 hours. The solution was then slowly added dropwise to a large amount of glacial ether for precipitation. After centrifugation and the supernatant was discarded, the white precipitate was dried in a vacuum oven for 24 hours to yield a water-soluble polymer containing epoxy groups with a number-average molecular weight of approximately 35,000.

[0047] Example 5

[0048] Glycidyl methacrylate (1.42 g, 10 mmol), polyethylene glycol methyl ether methacrylate (11.6 g, 50 mmol) with three ethylene glycol units, and AIBN (0.24 g, 1.5 mmol) were added to a 100 mL reaction flask. 80 mL of N,N-dimethylformamide was then added and dissolved. The system was then vacuumed and filled with nitrogen three times to remove oxygen. Polymerization was then carried out at 80°C for 8 hours. The solution was then slowly added dropwise to a large amount of glacial ether for precipitation. After centrifugation and the supernatant was discarded, the white precipitate was dried in a vacuum oven for 24 hours to yield a water-soluble polymer containing epoxy groups with a number-average molecular weight of approximately 8000.

[0049] Example 6

[0050] Glycidyl methacrylate (0.284 g, 2 mmol), polyethylene glycol methyl ether methacrylate (9.28 g, 40 mmol) with three ethylene glycol units, and AIBN (0.164 g, 1 mmol) were added to a 100 mL reaction flask. 80 mL of N,N-dimethylformamide was then added and dissolved. The system was then vacuumed and filled with nitrogen three times to remove oxygen. Polymerization was then carried out at 70°C for 18 hours. The solution was then slowly added dropwise to a large amount of glacial ether for precipitation. After centrifugation and the supernatant was discarded, the white precipitate was dried in a vacuum oven for 24 hours to yield a water-soluble polymer containing epoxy groups with a number-average molecular weight of approximately 15,000.

[0051] Example 7

[0052] Glycidyl methacrylate (0.284 g, 2 mmol), polyethylene glycol methyl ether methacrylate (10.8 g, 20 mmol) with 10 ethylene glycol units, and AIBN (0.328 g, 2 mmol) were added to a 150 mL reaction flask. 80 mL of N,N-dimethylformamide was then added and dissolved. The system was then vacuumed and filled with nitrogen three times to remove oxygen. Polymerization was then carried out at 50°C for 24 hours. The solution was then slowly added dropwise to a large amount of glacial ether for precipitation. After centrifugation and the supernatant was discarded, the white precipitate was dried in a vacuum oven for 24 hours to yield a water-soluble polymer containing epoxy groups with a number-average molecular weight of approximately 32,000.

[0053] Example 8

[0054] Glycidyl methacrylate (0.284 g, 2 mmol), polyethylene glycol methyl ether methacrylate (12 g, 10 mmol) with 20 ethylene glycol units, and AIBN (0.328 g, 2 mmol) were added to a 150 mL reaction flask. 80 mL of N,N-dimethylformamide was then added and dissolved. The system was then vacuumed and filled with nitrogen three times to remove oxygen. Polymerization was then carried out at 80°C for 12 hours. The solution was then slowly added dropwise to a large amount of glacial ether for precipitation. After centrifugation and the supernatant was discarded, the white precipitate was dried in a vacuum oven for 24 hours to yield a water-soluble polymer containing epoxy groups with a number-average molecular weight of approximately 50,000.

[0055] Example 9

[0056] Glycidyl methacrylate (0.284 g, 2 mmol) and 5 mL of N,N-dimethylformamide were stirred and dissolved in a 50 mL reaction flask, followed by the addition of methacryloylethyl sulfobetaine (2.79 g, 10 mmol) dissolved in 25 mL of water. After mixing and stirring evenly, ammonium persulfate (0.23 g, 1 mmol) was added. After sufficient dissolution and nitrogen deoxygenation, the mixture was placed at 40°C for polymerization reaction for 48 hours. The solution was then transferred to a dialysis bag and dialyzed with deionized water for 48 hours to remove unreacted monomers and impurities such as N,N-dimethylformamide. After freeze-drying, a water-soluble polymer containing epoxy groups was obtained with a number average molecular weight of approximately 5000.

[0057] The water-soluble polymer containing epoxy groups is prepared by using 1 HNMR characterization, the NMR spectrum is shown in Figure 3. Characteristic peaks of the H-spectrum of the methylene and methine groups in the polymer backbone, the H-spectrum peaks of the methylene and methine groups adjacent to the epoxy group, the H-spectrum peaks of the methyl and methylene groups adjacent to the nitrogen atom, and the H-spectrum peak of the methylene group adjacent to the sulfonate group can all be observed in Figure 3, confirming that a water-soluble polymer containing epoxy groups was successfully prepared.

[0058] The resulting water-soluble polymer containing epoxy groups was characterized by FTIR, and the spectrum is shown in Figure 4. Characteristic peaks for methine and methylene groups in the polymer backbone, epoxy bonds, methyl and methylene groups adjacent to nitrogen atoms, carbon-nitrogen bonds, and carbon-sulfur bonds in sulfonate groups are all observed in Figure 4, confirming the successful preparation of a water-soluble polymer containing epoxy groups.

[0059] Example 10

[0060] Glycidyl methacrylate (0.284 g, 2 mmol) and 5 mL of N,N-dimethylformamide were stirred and dissolved in a 100 mL reaction flask, followed by the addition of methacryloylethyl sulfobetaine (5.6 g, 20 mmol) dissolved in 50 mL of water. After mixing and stirring evenly, ammonium persulfate (0.35 g, 1.5 mmol) was added. After sufficient dissolution and nitrogen deoxygenation, the mixture was placed at 60°C for polymerization reaction for 32 hours. The solution was then transferred to a dialysis bag and dialyzed with deionized water for 48 hours to remove unreacted monomers and impurities such as N,N-dimethylformamide. After freeze-drying, a water-soluble polymer containing epoxy groups was obtained with a number average molecular weight of approximately 14,000.

[0061] Example 11

[0062] Glycidyl methacrylate (0.142 g, 1 mmol) and 2 mL of N,N-dimethylformamide were stirred and dissolved in a 50 mL reaction flask, followed by the addition of methacryloylethyl sulfobetaine (5.6 g, 20 mmol) dissolved in 40 mL of water. After mixing and stirring evenly, ammonium persulfate (0.46 g, 2 mmol) was added. After sufficient dissolution and nitrogen deoxygenation, the mixture was placed at 80°C for polymerization reaction for 16 hours. The solution was then transferred to a dialysis bag and dialyzed with deionized water for 48 hours to remove unreacted monomers and impurities such as N,N-dimethylformamide. After freeze-drying, a water-soluble polymer containing epoxy groups was obtained with a number average molecular weight of approximately 21,000.

[0063] Example 12

[0064] Glycidyl methacrylate (0.284 g, 2 mmol) and 5 mL of N,N-dimethylformamide were stirred and dissolved in a 50 mL reaction flask, followed by the addition of methacryloylethyl sulfobetaine (4.2 g, 15 mmol) dissolved in 30 mL of water. After mixing and stirring evenly, ammonium persulfate (0.23 g, 1 mmol) was added. After sufficient dissolution and nitrogen deoxygenation, the mixture was placed at 50°C for polymerization reaction for 32 hours. The solution was then transferred to a dialysis bag and dialyzed with deionized water for 48 hours to remove unreacted monomers and impurities such as N,N-dimethylformamide. After freeze-drying, a water-soluble polymer containing epoxy groups was obtained with a number average molecular weight of approximately 18,000.

[0065] Example 13

[0066] The water-soluble polymer containing epoxy groups prepared in Example 1 was blended with carboxymethyl cellulose (with a carboxymethyl substitution degree of 0.5 and a glucose unit polymerization degree of 200) in a high-speed mill at a blending weight ratio of 1:10 to prepare a fluid loss additive.

[0067] The fluid loss additive was subjected to a biotoxicity test in accordance with Q / SY17111-2019 "Biotoxicity Classification and Detection Methods for Oilfield Chemicals and Drilling Fluids." The results showed that the water-soluble polymer containing epoxy groups prepared in this embodiment and the fluid loss additive formed by blending with carboxymethyl cellulose were non-biotoxic, free of heavy metals, and safe and environmentally friendly.

[0068] Example 14

[0069] The water-soluble polymer containing epoxy groups prepared in Example 5 was blended with carboxymethyl cellulose (carboxymethyl substitution degree of 0.8, glucose unit polymerization degree of 500) using a high-speed grinder at a blending weight ratio of 1:5 to prepare a fluid loss additive.

[0070] The fluid loss additive was subjected to a biotoxicity test in accordance with Q / SY17111-2019 "Biotoxicity Classification and Detection Methods for Oilfield Chemicals and Drilling Fluids." The results showed that the water-soluble polymer containing epoxy groups prepared in this embodiment and the fluid loss additive formed by blending with carboxymethyl cellulose were non-biotoxic, free of heavy metals, and safe and environmentally friendly.

[0071] Example 15

[0072] The water-soluble polymer containing epoxy groups prepared in Example 10 was blended with carboxymethyl cellulose (carboxymethyl substitution degree of 2.0, glucose unit polymerization degree of 1000) using a high-speed grinder at a blending weight ratio of 1:8 to prepare a fluid loss additive.

[0073] The fluid loss additive was subjected to a biotoxicity test in accordance with Q / SY17111-2019 "Biotoxicity Classification and Detection Methods for Oilfield Chemicals and Drilling Fluids." The results showed that the water-soluble polymer containing epoxy groups prepared in this embodiment and the fluid loss additive formed by blending with carboxymethyl cellulose were non-biotoxic, free of heavy metals, and safe and environmentally friendly.

[0074] Examples 16 to 32

[0075] The water-soluble polymers containing epoxy groups prepared in Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 and 12 were respectively blended with carboxymethyl cellulose (with a carboxymethyl substitution degree of 0.5 and a glucose unit polymerization degree of 500) using a high-speed grinder to prepare fluid loss additives of different compositions. The formulas are shown in Table 1.

[0076] Prepare a freshwater-based slurry with a mass concentration of 2% by adding 400 mL of water to a high-speed stirring cup, adding 16 g of bentonite and 1.2 g of sodium carbonate to the water under stirring conditions, stirring at high speed for 20 minutes until uniform, and sealing and curing for 24 hours. Then, take a certain amount of freshwater-based slurry, add 2 wt% of carboxymethyl cellulose or 2 wt% of fluid loss reducer, stir and dissolve evenly, and then divide it into two parts of equal volume. One part is cured at room temperature (25 ° C) for 24 hours, and the other part is aged at 160 ° C for 16 hours. Then, the apparent viscosity and fluid loss reduction performance (FL) of the fluid loss reducer are evaluated according to GB / T16783.1-2014 "Petroleum and Natural Gas Industry-Drilling Fluid Field Test-Part 1: Water-based Drilling Fluid". API ), the test results are shown in Table 1:

[0077] Table 1

[0078] As shown in Table 1, Example 16, in which carboxymethyl cellulose was added to a freshwater-based slurry as a fluid loss control agent, showed a significant decrease in base slurry viscosity after high-temperature aging, from 42.3 mPa·s to 8.2 mPa·s. This indicates that the carboxymethyl cellulose fluid loss control agent underwent significant pyrolysis during the high-temperature aging process. This also resulted in a significant increase in API fluid loss, from 11.2 mL to 34.8 mL, indicating that this fluid loss control agent exhibited poor high-temperature fluid loss performance. Figure 5 shows the filter cake formed after high-temperature aging in Example 16. As shown in Figure 5, the filter cake is thick, confirming that high temperature causes a decrease in the fluid loss control agent's performance.

[0079] As shown in Table 1, Examples 17-32 provide the performance of carboxymethyl cellulose fluid loss control agents mixed with varying amounts of water-soluble polymers containing epoxy groups before and after aging. When the carboxymethyl cellulose fluid loss control agents containing water-soluble polymers containing epoxy groups, as described in Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12, were mixed into freshwater slurries, the viscosity drop due to thermal degradation of the carboxymethyl cellulose was significantly reduced after aging at 160°C for 16 hours, demonstrating significantly improved high-temperature stability. Furthermore, the increase in API fluid loss was minimal compared to pre-aging, demonstrating that the fluid loss control agents used in Examples 17-26 exhibit excellent high-temperature fluid loss reduction performance. Furthermore, Figure 6 shows the filter cake formed after high-temperature aging in Example 23. As shown in Figure 6, the filter cake is very thin and dense, further demonstrating that the fluid loss control agent used in Example 23 can achieve excellent high-temperature fluid loss reduction performance.

[0080] Example 33

[0081] The water-soluble polymer containing epoxy groups prepared in Example 7 was blended with carboxymethyl cellulose (carboxymethyl substitution degree of 0.5, glucose unit polymerization degree of 1000) using a high-speed grinder at a blending weight ratio of 1:10 to prepare a fluid loss additive.

[0082] The preparation process of freshwater-based slurry with a mass concentration of 4% is as follows: add 400mL of water to a high-speed stirring cup, add 16g of bentonite and 1.2g of sodium carbonate to the water under stirring conditions, stir at high speed for 20 minutes until uniform, seal and place for curing for 24 hours. Then take a certain amount of freshwater-based slurry and add 4% of the above-mentioned fluid loss reducer. After stirring and dissolving evenly, divide it into two equal volumes, one for curing at room temperature (25℃) for 24 hours, and the other for aging at 150℃ for 16 hours. Then, the fluid loss reduction performance (FL) of the fluid loss reducer was evaluated according to GB / T16783.1-2014 "Petroleum and Natural Gas Industry-Field Testing of Drilling Fluids-Part 1: Water-based Drilling Fluids". API The results show that the API filtration loss before aging was 9.8 mL, and after aging at 150°C for 16 hours, the API filtration loss was 12.7 mL. The increase in API filtration loss was very small compared to that before aging, which shows that the filtration loss reducer used has good high temperature resistance and filtration loss reduction effect.

[0083] Example 34

[0084] The water-soluble polymer containing epoxy groups prepared in Example 9 was blended with carboxymethyl cellulose (carboxymethyl substitution degree of 1.0, glucose unit polymerization degree of 500) using a high-speed grinder at a blending weight ratio of 1:10 to prepare a fluid loss additive.

[0085] The preparation process of freshwater-based slurry with a mass concentration of 2% is as follows: add 400mL of water to a high-speed stirring cup, add 16g of bentonite and 1.2g of sodium carbonate to the water under stirring conditions, stir at high speed for 20 minutes until uniform, seal and place for curing for 24 hours. Then take a certain amount of freshwater-based slurry and add 2wt% of the above-mentioned fluid loss reducer. After stirring and dissolving evenly, divide it into two equal volumes, one for curing at room temperature (25℃) for 24 hours, and the other for aging at 180℃ for 16 hours. Then, the fluid loss reduction performance (FL) of the fluid loss reducer is evaluated according to GB / T16783.1-2014 "Petroleum and Natural Gas Industry-Field Testing of Drilling Fluids-Part 1: Water-based Drilling Fluids". API The results show that the API filtration loss before aging was 13.4 mL, and after aging at 180°C for 16 hours, the API filtration loss was 18.6 mL. The increase in API filtration loss compared to before aging was still very small, indicating that the filtration loss reducer used has good high temperature resistance and filtration loss reduction effect.

[0086] Example 35

[0087] The water-soluble polymer containing epoxy groups prepared in Example 5 was blended with carboxymethyl cellulose (carboxymethyl substitution degree of 1.6, glucose unit polymerization degree of 800) using a high-speed grinder at a blending weight ratio of 1:8 to prepare a fluid loss additive.

[0088] The preparation process of freshwater-based slurry with a mass concentration of 2% is as follows: add 400mL of water to a high-speed stirring cup, add 16g of bentonite and 1.2g of sodium carbonate to the water under stirring conditions, stir at high speed for 20 minutes until uniform, seal and place for curing for 24 hours. Then take a certain amount of freshwater-based slurry and add 6wt% of the above-mentioned fluid loss reducer. After stirring and dissolving evenly, divide it into two equal volumes, one for curing at room temperature (25℃) for 24 hours, and the other for aging at 200℃ for 16 hours. Then, the fluid loss reduction performance (FL) of the fluid loss reducer is evaluated according to GB / T16783.1-2014 "Petroleum and Natural Gas Industry-Field Testing of Drilling Fluids-Part 1: Water-based Drilling Fluids". API The results show that the API filtration loss before aging was 10.2 mL, and after aging at 200°C for 16 hours, the API filtration loss was 17.6 mL. The increase in API filtration loss compared to before aging was still very small, indicating that the filtration loss reducer used has good high-temperature resistance and filtration loss reduction effect.

[0089] Example 36

[0090] The water-soluble polymer containing epoxy groups prepared in Example 12 was blended with carboxymethyl cellulose (carboxymethyl substitution degree of 2.0, glucose unit polymerization degree of 600) using a high-speed grinder at a blending weight ratio of 1:6 to prepare a fluid loss additive.

[0091] The preparation process of freshwater-based slurry with a mass concentration of 2% is as follows: add 400mL of water to a high-speed stirring cup, add 16g of bentonite and 1.2g of sodium carbonate to the water under stirring conditions, stir at high speed for 20 minutes until uniform, seal and place for curing for 24 hours. Then take a certain amount of freshwater-based slurry and add 6wt% of the above-mentioned fluid loss reducer. After stirring and dissolving evenly, divide it into two equal volumes, one for curing at room temperature (25℃) for 24 hours, and the other for aging at 220℃ for 16 hours. Then, the fluid loss reduction performance (FL) of the fluid loss reducer is evaluated according to GB / T16783.1-2014 "Petroleum and Natural Gas Industry-Field Testing of Drilling Fluids-Part 1: Water-based Drilling Fluids". API The results show that the API filtration loss before aging was 12.1 mL, and after aging at 220°C for 16 hours, the API filtration loss was 16.9 mL. The increase in API filtration loss compared to before aging was still very small, indicating that the filtration loss reducer used has good high-temperature resistance and filtration loss reduction effect.

Claims

1. A high-temperature resistant fluid loss reducer, wherein, Comprising carboxymethyl cellulose and a water-soluble polymer containing an epoxy group, the water-soluble polymer containing an epoxy group being selected from (CH3CH2CCOOCH2CHCH2O) x -[CH2CHCOO(CH2CH2O) n CH3] y 、(CH3CH2CCOOCH2CHCH2O) x -[CH3CH2CCOO(CH2CH2O) n CH3] y and (CH3CH2CCOOCH2CHCH2O) x -[CH3CH2CCOOCH2CH2N + (CH3)2CH2CH2CH2SO3 - y and combinations of one or more of the foregoing;​ x and y are each independently 1:20 to 5, and n is each independently 3 to 20; the number-average molecular weight of the water-soluble polymer containing an epoxy group is 5,000 to 50,000.

2. The high-temperature resistant fluid loss reducer according to claim 1, wherein, The weight ratio of the water-soluble polymer containing an epoxy group to the carboxymethyl cellulose is 1:10 to 5.

3. The high-temperature resistant fluid loss reducer according to claim 1, wherein, The (CH3CH2CCOOCH2CHCH2O) x -[CH2CHCOO(CH2CH2O) n CH3] y It is obtained by free radical copolymerization of glycidyl methacrylate and polyethylene glycol methyl ether acrylate in a molar ratio of 1:20 to 5.

4. The high-temperature resistant fluid loss reducer according to claim 3, wherein, The polymerization temperature of glycidyl methacrylate and poly(ethylene glycol) methyl ether acrylate is 60 to 80 °C, and the polymerization time is 12 to 24 h.

5. The high-temperature resistant fluid loss reducer according to claim 1, wherein, The said (CH3CH2CCOOCH2CHCH2O) x -[CH3CH2CCOO(CH2CH2O) n CH3] y It is obtained by free radical copolymerization of glycidyl methacrylate and methoxypolyethylene glycol methacrylate in a molar ratio of 1:20 to 5.

6. The high-temperature resistant fluid loss reducer according to claim 5, wherein, The polymerization temperature of glycidyl methacrylate and poly(ethylene glycol) methyl ether methacrylate is 50 to 80 °C, and the polymerization time is 8 to 24 h.

7. The high-temperature resistant fluid loss reducer according to claim 1, wherein, The said (CH3CH2CCOOCH2CHCH2O) x -[CH3CH2CCOOCH2CH2N + (CH3)2CH2CH2CH2SO3 - y It is obtained by free radical copolymerization of glycidyl methacrylate and methacryloylethyl sulfobetaine in a molar ratio of 1:20 to 5.​ 8. The high-temperature resistant fluid loss reducer according to claim 7, wherein, The polymerization temperature of glycidyl methacrylate and methacryloylethyl sulfobetaine is 40 to 80 °C, and the polymerization time is 16 to 48 h.

9. A water-based drilling fluid, wherein, Comprising the high-temperature filtration reducer according to any one of claims 1 to 8, and in the drilling fluid, the weight content of the filtration reducer is 1 to 6 wt%.

10. Use of the high-temperature filtration reducer according to any one of claims 1 to 8 in a drilling engineering in a high-temperature underground environment, wherein the temperature of the high-temperature environment is 150 to 220 °C.

Citation Information

Patent Citations

  • Preparation method of grafted hydrophilic polymer bionic ultrafiltration membrane

    CN110743371A

  • Polyfunctional group copolymer as well as preparation method and application thereof in collagen modification

    CN115894784A

  • Degradable shape memory polythiourea hydrogel and preparation method thereof

    CN117024750A

Cited By

  • Low-molecular-weight filtrate reducer and preparation method thereof

    CN120699199A

  • Modified cellulose filtrate reducer and preparation method thereof

    CN122427331A