Glass cutting method and glass materials

The ultrasonic cutting machine generates linear frictional heat and mechanical stress on the glass, which solves the problems of inaccurate and uneven glass cutting in the existing technology, achieves efficient and precise cutting surfaces, and is suitable for various glass materials.

CN112645580BActive Publication Date: 2024-10-18HOYA CORPORATION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202011077241.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-10
Publication Date
2024-10-18
Estimated Expiration
2040-10-10

AI Technical Summary

Technical Problem

Existing glass cutting methods are difficult to achieve efficient, accurate and beautiful cutting surfaces, especially on thick glass, and the devices are complex or difficult to control the crack direction, resulting in uneven and inaccurate cutting surfaces.

Method used

The ultrasonic vibration blade of the ultrasonic cutting machine is used to contact the glass, and the ultrasonic vibration generates linear friction heat and mechanical stress to form a linear incision, thereby achieving a high-precision and small waviness cutting surface.

Benefits of technology

It achieves efficient and precise cutting of glass, reduces the amount of grinding and the generation of glass chips, and obtains a smooth and small waviness cutting surface, which is suitable for glass materials of various shapes and sizes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112645580B_ABST
    Figure CN112645580B_ABST
Patent Text Reader

Abstract

The present invention provides a glass cutting method and a glass material produced by the cutting method. The glass cutting method does not require complicated equipment and can efficiently and accurately obtain a beautiful cut surface. A glass cutting method includes: a step of bringing an ultrasonic vibration blade of an ultrasonic cutter into contact with a portion of the glass to be cut; a step of causing the ultrasonic vibration blade to vibrate ultrasonically; and a step of cutting the glass into an incision while generating friction heat in a linear shape using the ultrasonic wave.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a glass cutting method and a glass material cut thereby. Background Art

[0002] In the past, the following methods are known as methods for cutting brittle materials such as glass into specified sizes: 1) using a cutting blade embedded with abrasive grains harder than glass, such as a round blade embedded with diamond abrasive grains, to physically cut the glass; 2) causing a crack in a part of the glass and expanding the crack by applying pressure, that is, using the stress generated on the glass to be greater than the bending strength of the glass to cut (sever) the glass.

[0003] As a method of cutting glass using the latter cutting method, manual cutting is generally used. Manual cutting is a method in which the glass is first pressed against a disc-shaped blade rotated by a motor or the like to physically make a cut less than about 3 mm deep on the glass, and then pressure is applied to the glass or the vicinity of the cut is heated or cooled, thereby generating mechanical stress or thermal stress on the glass, thereby cutting the glass.

[0004] When cutting manually, it is preferred to make the direction of the crack consistent with the specified direction. However, since the glass and the disc-shaped blade are in point contact, the thermal stress acting on the crack has a concentric distribution from the contact point between the glass and the blade. The concentric heat distribution acts on the crack generated at the contact point between the glass and the blade. Therefore, depending on the shape of the glass sample, the crack cannot be extended in the specified direction, and the glass cannot be cut with the correct size. In particular, for thick glass, it is difficult to apply uniform mechanical stress to the glass to make the crack extend in the same direction as required, so the cut surface becomes a curved surface, and there is also a problem that it is difficult to cut it cleanly.

[0005] As a method for solving such a problem, for example, Patent Document 1 discloses a method of "applying uniform lateral pressure to the side surfaces of the glass to be cut, thereby utilizing the internal stress generated in the glass to cut it." This method states that it is suitable for expensive materials because it does not generate chips and has little loss.

[0006] In addition, Patent Document 2 discloses a method of "a cutting method, wherein a brittle material is heated along a cutting line, cooled along the cutting line, cracks are generated on the surface of the brittle material by thermal stress, and the material is cut along the cracks, and the brittle material is cooled along the cutting line at or near a stress inflection point where the compressive stress of the brittle material changes to a tensile stress due to the expansion caused by the heating, so as to generate cracks on the surface of the brittle material." This method describes the advantages of being able to perform operations more efficiently and to obtain a beautiful cut surface.

[0007] However, the method using lateral pressure disclosed in Patent Document 1 may cause the internal cracks to be not located at one place when used for glass with a large number of microcracks on the surface of a filed workpiece or a heated cut workpiece, making it difficult to cut accurately at the target position. In addition, in the laser beam cutting method disclosed in Patent Document 2, the laser beam irradiation method and the cooling method are repeated along the cutting line, so the device becomes complicated. In addition, the microscopic heat distribution on the glass surface is concentric with the laser irradiation point as the starting point, so the cracks may not extend in the specified direction (depth direction), and thick glass is particularly difficult to cut.

[0008] In addition, there is a method such as placing glass on a heated straight heating line to generate cracks on the end face of the glass, and cutting the glass by extending the cracks in the direction of the thermal stress portion generated by the heating line. Although this method imparts a linear heat distribution to the glass, the physical stress imparted to the glass is only the thermal stress caused by thermal expansion, so the possibility of cutting and the accuracy of cutting strongly depend on the shape of the mother glass, and the position that can be cut is limited to the center of the glass. As a result, it is only suitable for a method of dividing a relatively large plate glass into two equal parts, and is not suitable for manufacturing small cutting workpieces of arbitrary shapes.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: (Japanese) Patent Publication No. 61-266323

[0012] Patent Document 2: (Japanese) Patent Publication No. 2004-155159 Summary of the invention

[0013] Problems to be solved by the invention

[0014] The present invention provides a glass cutting method and a glass material obtained by the cutting method. The glass cutting method does not require complicated equipment and can obtain a beautiful cutting surface efficiently and accurately.

[0015] Solutions to Solve Problems

[0016] The present inventors have found that when an ultrasonic cutter is used, the state of the cut surface is significantly better than that of conventional manual cutting, and have completed the present invention. The present invention includes the following contents.

[0017] [1] A method for cutting glass, comprising: a step of bringing an ultrasonic vibration blade of an ultrasonic cutter into contact with a portion of the glass to be cut; a step of causing the ultrasonic vibration blade to vibrate ultrasonically; and a step of cutting the glass into an incision while generating frictional heat in a linear shape using the ultrasonic wave.

[0018] [2] The glass cutting method according to claim 1, wherein the frequency of the ultrasonic vibration is greater than or equal to 5 kHz and less than or equal to 50 kHz.

[0019] [3] The glass cutting method according to claim 1 or 2, wherein the amplitude of the ultrasonic vibration is 5 μm or more and 40 μm or less.

[0020] [4] A glass material obtained by the cleavage method according to claim 1.

[0021] [5] The cleavage method according to claim 4, wherein the waviness of the cleaved surface of the glass material is 100 or less.

[0022] [6] A method for manufacturing a glass material, comprising: a step of bringing an ultrasonic vibration blade of an ultrasonic cutter into contact with a portion of the glass to be cut; a step of causing the ultrasonic vibration blade to vibrate ultrasonically; and a step of cutting into the glass while generating frictional heat in a linear shape using the ultrasonic wave.

[0023] [7] A glass material having at least a surface having a waviness of 100 or less and a surface roughness Ra of 500 μm or less.

[0024] [8] The glass material according to [7], wherein the surface is a fractured surface.

[0025] [9] The glass material as described in [7] or [8], wherein the content of boron and / or alkali components and / or fluorine in the surface is higher than the content of these elements in the glass surface of the glass material that is not contained in the surface.

[0026]

[10] A glass material as described in [7] or [8], wherein the content of boron and / or alkali components and / or fluorine in the surface is 5% or more higher than the content of these elements in the glass surface of the glass material that is not contained in the surface.

[0027] Effects of the Invention

[0028] In the present invention, the ultrasonic vibration blade of the ultrasonic cutter performs ultrasonic vibration at the part where the glass is to be cut, so that the contact state between the glass and the ultrasonic vibration blade is not the point contact of the circular blade of the previous diamond cutter, but a linear uniform contact. As a result, the heat distribution generated by the cutting blade in the glass is also linear. As a result, since the ultrasonic cutter heats the glass linearly while forming the incision, the corrugation is small and a beautiful cut surface can be obtained. If the corrugation of the cut surface is small, the grinding amount can be suppressed in the subsequent grinding process, and the amount of glass scraps can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1This is a perspective view showing a state where a cut is made in glass G using an ultrasonic cutter used in the present invention.

[0030] Figure 2 This is a schematic diagram showing heat distribution when the ultrasonic cutter of the present invention is brought into contact.

[0031] Figure 3 This is a perspective view showing the situation when the incision is made in the conventional cutting method.

[0032] Figure 4 This is a schematic diagram showing the heat distribution when cutting into the cut in the conventional cutting method.

[0033] Figure 5 This is a diagram showing a formula for calculating the degree of difficulty N of cutting of a glass material and the meanings of variables in the formula.

[0034] Figure 6 This is a side view when measuring the waviness X of a glass material having a fractured surface.

[0035] Figure 7 This is a graph showing the relationship between the cutting difficulty N and the waviness X.

[0036] Description of Reference Numerals

[0037] G Glass

[0038] G1, G2 The part you want to cut

[0039] 1 Ultrasonic cutting machine

[0040] 11 Ultrasonic vibration blade

[0041] 11a Arrow indicating the vibration direction of the ultrasonic vibration blade

[0042] 2 Manual cutting

[0043] 21 disc blade

[0044] 22 Motor

[0045] 3.4 Heating section

[0046] D The gap distance between the cut surface and the simple surface

[0047] T Thickness

[0048] W Width

[0049] L Length DETAILED DESCRIPTION

[0050] [Glass cutting method]

[0051] Hereinafter, a glass cutting method using an ultrasonic cutting machine will be described with reference to the drawings. Figure 1 This is a perspective view showing the cutting of glass by an ultrasonic cutting machine. Figure 2 This is a schematic diagram showing the heat distribution when cutting with an ultrasonic cutter 1. The ultrasonic vibration blade 11 of the ultrasonic cutter 1 is brought into contact with the portion G1 to be cut of the glass G to be cut, and ultrasonic vibration is applied to the ultrasonic vibration blade 11 in the direction of the arrow 11a indicating the vibration direction. The ultrasonic vibration blade 11 is brought into contact with the glass G by ultrasonic vibration, and friction heat is generated linearly at the portion G1 to be cut, and a linear cut is generated. Thus, due to the linear thermal stress and linear mechanical stress generated in the direction of the glass to be cut, the glass can be cut without substantially applying any other pressure to the glass base material.

[0052] The heat generated by ultrasonic vibration is distributed on the ultrasonic vibration blade of the ultrasonic cutting machine as follows Figure 1 In the case of an ultrasonic vibration blade 11 such as the cutter shown in FIG. 1 , heat is distributed linearly with the linear heating portion as the center ( Figure 2 ). While frictional heat is generated linearly, mechanical stress is generated through the linear cut, thereby generating and extending cracks at the position where the ultrasonic vibration blade contacts and cutting the glass, so that the cut surface becomes a clean surface, that is, a smooth surface with small waviness. The definition of waviness will be explained later.

[0053] The depth of the cracks produced by the ultrasonic cutting machine 1 also depends on the thickness of the glass, and the depth of the cut is about 0.2 to 2 mm, preferably 0.2 mm to 1 mm or less. This cut-in depth is shallower than the cut-in depth during the previous manual cutting. It should be noted that the time required for cutting is not particularly limited, but since the glass is cut by the above-mentioned mechanism, it is not preferred to apply only mechanical stress before sufficient friction heat is generated, and on the contrary, it is not preferred to apply only mechanical stress after the friction heat diffuses outside the cut portion. According to this viewpoint, the time required for the cut-in of the cracks can be appropriately changed according to the hardness and size of the glass. The lower limit of the cut-in time when the glass is actually cut is based on 0.1 seconds / mm or more, preferably 0.3 seconds / mm, more preferably 0.5 seconds / mm, and further preferably about 0.1 seconds / mm. The upper limit of the cut-in time is preferably about 15 seconds / mm, preferably about 10 seconds / mm, and more preferably about 5 seconds / mm. On the contrary, if the cut-in time exceeds 30 seconds / mm or 60 seconds / mm, the friction heat diffuses to the periphery and the mechanical stress decreases, so it is not preferred.

[0054] The size of the glass used for cutting is not particularly limited, but in the case of rectangular glass, it can be a glass with a height of 1 to 40 mm, a width of 1 to 40 mm, and a length of, for example, 10 mm or more. It should be noted that it is not limited to rectangular glass, and can also be used for cylindrical glass, triangular prism glass, etc. (The difficulty of cutting at this time can be distinguished according to the difficulty of cutting shown later.)

[0055] (Ultrasonic cutting machine)

[0056] As the ultrasonic cutter used in the present invention, a commercially available product can be used, and for example, a small ultrasonic cutter USW-334 manufactured by Honda Electronics Co., Ltd. can be used.

[0057] The lower limit of the ultrasonic frequency of the ultrasonic cutter is preferably 5 kHz or more, more preferably 10 kHz or more, and further preferably 15 kHz or more, and the upper limit is preferably 50 kHz or less, more preferably 45 kHz or less, and further preferably 40 kHz or less.

[0058] The lower limit of the amplitude of the ultrasonic vibration blade is preferably 5 μm or more, more preferably 10 μm or more, and the upper limit is preferably 40 μm or less, more preferably 30 μm or less.

[0059] In addition, the output of the ultrasonic vibration blade is not particularly limited, but for example, in the range of 5W to 500W, the lower limit of the output can be changed to 5W, 10W, 20W, 30W, 40W, 50W, 60W, 70W, 80W, 90W, 100W, 150W, ..., and the upper limit can also be changed to 30W, 60W, 80W, 100W, 150W, 200W, 300W, 400W, 500W, and the output is appropriately changed according to the hardness of the glass, the width when cutting, and the difficulty of cutting described later. The output range can be, for example, 10W to 30W, 20W to 60W, 40W to 100W, 100W to 300W, 200W to 400W, etc. When the hardness of the glass is high, by increasing the output, the friction heat in the shear direction of the glass can be increased, and the glass can be cut. Therefore, when the hardness of the glass is high, the cutting difficulty varies, but for example, the glass can be cut by setting the output to more than 80 W. However, if the output is too large, it is difficult to heat the glass unless the contact between the glass and the blade is uniform, so it is not necessary to increase the output to more than the output at which the glass can be cut.

[0060] The size of the ultrasonic vibration blade is not particularly limited, but the thickness of the blade is preferably 0.1 mm or more and 1.0 mm or less, and more preferably 0.3 mm or more and 0.8 mm or less.

[0061] The total length of the ultrasonic vibration blade can be appropriately selected according to the size of the glass to be cut, and for example, a length of 20 mm or more and 100 mm or less can be used.

[0062] The material is not particularly limited as long as it has a predetermined hardness such as ceramics or metal, and steel such as SKH51 can be used.

[0063] like Figure 1 As shown, the ultrasonic vibration blade of the ultrasonic cutter is a thin plate-shaped blade like the blade of a paper cutter, but it is not limited to such an ultrasonic vibration blade. For example, a pen-shaped ultrasonic vibration blade with point contact can also be used. In this case, by cutting into the glass in a contact state in the form of a line, a linear crack is generated, and an incision with a shape close to the same as that of the ultrasonic vibration blade can be made.

[0064] The ultrasonic vibration direction is the direction of vibration in the direction of the axis of the handle of the ultrasonic cutting machine (in Figure 1 is the direction of 11a).

[0065] On the other hand, Figure 3 As shown, the conventional manual cutting method makes the disc-shaped blade 21 contact the glass G, physically forms a cut with a depth of about 3 mm, and then cuts the glass. However, in such a device, the contact point is concentrated at one point, and there is also a distribution of thermal stress in the direction other than the direction to be cut. Therefore, if the cutting difficulty described below is high, it is difficult to cut neatly.

[0066] [Difficulty of Cutting]

[0067] The cutting method of the present invention has the characteristic of being able to cut neatly even when the cutting difficulty is high. Figure 5 The higher the glass cutting difficulty, the harder it is to cut. In the formula for the cutting difficulty, T is the thickness, W is the width, and L is the length. The smaller the values ​​of T / L and W / L in the formula, the easier it is to cut, and preferably they are less than 1 respectively. In addition, the smaller the thickness T, the easier it is to cut.

[0068] Regarding the difficulty of cutting, in the previous manual cutting, if the cutting difficulty exceeds 2, it becomes difficult to cut, and even if it is assumed that it can be cut, the waviness described later becomes larger. Therefore, in the previous manual cutting, it is generally suitable for glass with a height of 5 to 20 mm and a width of 5 to 20 mm. In contrast, in the cutting method using the ultrasonic cutting machine of the present invention, even when the cutting difficulty is 2 to 5, it is possible to cut with a small waviness. In addition, by increasing the amplitude of the reciprocating motion of the ultrasonic output of the cutting blade, that is, the direction of shearing the glass, it is also possible to easily cut the glass.

[0069] [Glass with a cut surface]

[0070] Next, the glass material cut by the cutting method of the present invention is described. The glass material has the characteristics of small waviness, small surface roughness Ra, and, depending on the situation, a cut surface with a high boron content on the surface. It should be noted that in this specification, the cut surface refers to a surface newly generated by cutting.

[0071] (Waviness of the cut surface)

[0072] The cut surface of the glass obtained by the glass cutting method of the present invention has a characteristic of small waviness. The waviness of the cut surface refers to the planarity of the cut surface and is defined by the value obtained by the following measurement method. Figure 6 The method for measuring the waviness of the cut surface is described below. Regarding the waviness, a vertical surface at an angle of 90° to the plane is pressed against the cut surface, and the size of the gap D between the vertical surface and the cut surface is measured N times (N=5 in the embodiment of the present invention), and the gap D per glass thickness T, that is, the average value of D / T is measured as the waviness. If the waviness is small, the angle between the bottom surface of the glass and the cut surface is close to 90°, such as Figure 6 As shown, in the case of prism-shaped glass, it is close to a rectangular parallelepiped. Therefore, the deviation between individual glass materials is also reduced, and the grinding amount can be suppressed in the subsequent grinding process, etc., and the amount of glass scraps can be reduced. When the cutting difficulty is 2 to 5 (for example, when the cutting difficulty is 3), the waviness of the cut surface is preferably 100 or less, more preferably 80 or less, and further preferably 60 or less.

[0073] In the case of the cutting method using the conventional manual cutting, since the cut portion that becomes the starting point of the cutting is a point, the heat diffuses in a circular shape with the point as the center. In this case, the waviness of the cut surface is large, and when the cutting difficulty is 2 to 5 (for example, when the cutting difficulty is 3), the waviness exceeds 100.

[0074] In contrast, in the present invention, since the incision is made linearly while applying ultrasonic waves, the incision portion that becomes the starting point of the cutting is linear. In this case, the waviness of the cut surface is small because the heat diffusion is wide.

[0075] (Surface roughness Ra of the cut surface)

[0076] Compared with the cut surface obtained by physical cutting, the cut surface obtained according to the present invention has a smaller surface roughness Ra. If the surface roughness Ra is small, it is easy to understand the situation inside the glass even without grinding, and impurities can be visually observed. In the cutting of a conventional glass cutter, the surface roughness Ra is large, and it becomes a friction glass, and the inside of the glass cannot be visually observed. The Ra of at least one cut surface of the glass material of the present invention is preferably 500nm or less, more preferably 400nm or less, further preferably 300nm or less, further preferably 200nm or less, further preferably 100nm or less, particularly preferably 20nm or less, for example 5nm or less.

[0077] (Glass composition)

[0078] The composition of the glass material of the present invention is not particularly limited, and it can be applied to various glasses. For example, phosphate glass and / or borate glass and / or silicate glass can be cited. In particular, the present invention is easily applicable to materials with low bending strength and large thermal expansion coefficient.

[0079] As a standard for bending strength, in common optical glasses, when 150 (unit: Pa) or less or even 120 or less is used as a standard, the strength of the glass that is easily applicable to the present invention is preferably 100 or less, more preferably 85 or less, further preferably 75 or less, further preferably 65 or less, and further further preferably 55 or less. Furthermore, as a standard for expansion coefficient, in the average linear expansion coefficient at 100 to 300° C., it is preferably 60×10 -7 (Unit: K -1 ) or more, more preferably 80×10 -7 More preferably, 100×10 -7 More preferably, 120×10 -7 More preferably, 130×10 -7 Above, particularly preferably 140×10 -7 above.

[0080] It should be noted that regarding the bending strength σ, a glass sample (number of samples, ten) with a width of 4×thickness of 3×total length of 40 (mm) was used, the upper and lower surfaces were ground, the edges were chamfered by C0.2 (mm) (the right-angled isosceles triangle with a side length of 0.2 mm was removed), and the breaking load P (N) was measured by the "three-point bending test method" specified in JIS R 1601:2008. It can be calculated by σ=3PL / (2w·t 2 ) for calculation.

[0081] Here, L is the distance between the supporting points (mm), w is the width of the sample (mm), and t is the thickness of the sample (mm). The bending strength σ obtained can be expressed in MPa units, for example, 1 MPa = 1.01972 × 10 -1 kgf / mm 2 In kgf / mm 2 Units etc. are converted appropriately.

[0082] In addition, the average linear expansion coefficient α at 100°C to 300°C is determined by referring to the measurement method of the Japan Optical Glass Industry Association standard JOGIS08. A glass round rod with a length of 20 mm and a diameter of 5 mm to a diameter of 4±0.5 mm is used. A differential thermal dilatometer is used to heat the sample at a constant rate of 4°C per minute, and the elongation of the sample relative to the temperature is measured.

[0083] It should be noted that the bending strength σ is mainly determined by the content of alkaline elements and the content of SiO2 in the glass, but is also affected by other elements. Specifically, when the sum of the mass percentages of elements that reduce the bending strength σ (Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Bi) is set to A (wherein the sum of the mass percentages of Li, Na, K, Rb, and Cs is 10 times), and the sum of the mass percentages of elements that increase the bending strength σ (Si, B, P, and Nb) is set to B, the greater the value of A / B, the easier it is to cut the glass. In terms of easy cutting, the value of A / B is 0 or more, preferably in the order of 0.1 or more, 0.2 or more, 0.4 or more, 0.8 or more, 1.2 or more, 1.6 or more, 2.0 or more, 2.4 or more, 2.8 or more, 3.2 or more, 3.5 or more, and 4.0 or more. Note that A and B are represented by the following formula (wherein W(X) represents the mass % of element X contained in the glass, for example, W(Li) represents the mass % of the Li component).

[0084] A=W[(Li)+W(Na)+W(K)+W(Rb)+W(Cs)]×10+W(Mg)+W(Ca)+W(Sr)+W(Ba)+W(Bi)]

[0085] B=[W(Si)×10]+W(B)+W(P)+W(Nb)+W(La)

[0086] In addition, the present invention is applicable even to glass that does not have a low bending strength σ. For hard glass, that is, glass with an A / B value of 1.0 or less, or glass with an A / B value of 0.5 or less, 1 or less, or 0.0, it can be cut by paying attention to the output of the cutting blade. For example, the A / B value of glass D is 0.0, but by increasing the ultrasonic output of the cutting blade, that is, the amplitude of the reciprocating motion in the direction of shearing the glass, the glass can be cut as shown in the embodiment.

[0087] (Element content and composition distribution of the cut surface)

[0088] For example, when the glass contains a silicate skeleton, elements such as alkali ions also dissolve from the strong Si-O glass structure, and there are cases where the content of alkali elements on the polished surface is reduced. In addition, when the glass contains boron, since the boron located on the glass surface is in a state where it can react with water and dissolve, the boron content of the unprocessed free surface after manufacturing the glass (the so-called free surface refers to the surface that is in contact with the atmosphere when the glass solidifies) or the polished surface processed by polishing with water is low. Furthermore, when the glass contains halogen ions such as fluorine (chlorine, bromine, iodine, etc.), due to the exchange reaction between oxygen ions on the glass surface and halogen ions, the amount of halogen ions decreases, and the glass surface is exposed to the atmosphere, so the component distribution on the glass surface is sometimes different from the component distribution inside the sample.

[0089] In contrast, the fractured surface obtained by the present invention is a fractured surface obtained by cutting the interior of the glass (bulk glass structure) to form the surface. Furthermore, since no water is used during the fracture, the components of the entire glass are evenly distributed.

[0090] Therefore, the content of boron and / or alkali components and / or fluorine in the fractured surface of the glass of the present invention is higher than the content of these elements in the glass surface such as the free surface and the polished surface not contained in the above-mentioned surface in the glass material (converted into atomic mass %).

[0091] More specifically, the content of boron and / or alkali components and / or fluorine in the cut surface is preferably 5% or more higher, more preferably 7% or more higher, and further preferably 10% or more higher than the content of these elements in the glass surface such as the free surface and the polished surface not contained in the above-mentioned surface in the glass material. It should be noted that these values ​​are calculated by (the content of boron and / or alkali components and / or fluorine in the cut surface) / (the content of these elements in the glass surface not contained in the cut surface).

[0092] When the glass sample of the present invention is deformed by reheating or pressurizing, the glass on the sample surface is somewhat folded into the interior of the optical element, but at this time, the difference in component distribution between the sample surface and the interior is small, so the minute difference in refractive index between the sample surface and the interior is also small, so an optically homogeneous optical element can be obtained. This effect is particularly produced when the lens is used in a higher performance optical system.

[0093] [Example]

[0094] Example

[0095] Hereinafter, the present invention will be further described by way of examples. It should be noted that the present invention is not limited to the examples.

[0096] [Ultrasonic cutting machine]

[0097] As an ultrasonic cutter, an ultrasonic small cutter USW-334 manufactured by Honda Electronics Co., Ltd. was used. The material of the ultrasonic vibration blade was SKH51, and ultrasonic vibration with a frequency of 22 kHz and an amplitude of 5 to 30 μm was applied to perform the following cutting.

[0098] [Production of glass materials based on cutting]

[0099] (Measurement of optical glass properties)

[0100] Using raw materials such as oxides, hydroxides, carbonates, nitrates, chlorides, fluorides, and sulfates of optical glass grade with high purity, the raw materials are weighed and mixed to obtain a glass (glass E) having the components recorded in the items of glasses A to D in Table 1 and the cut surface in Table 4 as a blending raw material. Next, each blending raw material is placed in a platinum crucible, heated to the specified temperature as described above, and melted in a nitrogen atmosphere for two or four hours from the beginning of melting, stirred for homogenization, left to stand for clarification, and then poured into a mold. After the glass solidifies, it is then transferred to an electric furnace heated to a temperature close to the slow cooling point of the glass and slowly cooled to room temperature. In this way, blocks composed of the glass of each embodiment are produced. Glass of the specified size required for measurement is cut out from each glass block obtained, and grinding is performed to evaluate the characteristics. For glasses A to D, Tables 1 and 2 show the components and characteristics, and Table 3 shows the results of cutting. For glass E, Table 4 shows the components of the cut surface, the polished surface, and the free-form surface.

[0101] It should be noted that there is no limit to the amount of glass raw materials, but when reproducing the embodiments, depending on the specific gravity of the glass, raw materials that can form glass of about 200g, 300g, 400g, or 500g can be used to make samples for cutting, or glass with a volume larger than the size recorded in the embodiments can be cut out for cutting.

[0102] (Example 1)

[0103] Glass A of 10mm (thickness) × 10mm (width) × 100mm (length) is cut into a rectangular parallelepiped of 10mm (thickness) × 10mm (width) × 20mm (length after cutting) and the ultrasonic cutting machine is brought into contact with the portion to be cut when the cutting difficulty is 0.50. After making an incision using ultrasonic vibration, the base glass is pressed by hand to generate tensile stress in the cut portion of the glass material, thereby applying pressure to cut the glass to obtain a slice A1.

[0104] (Example 2)

[0105] The length after cutting was changed to 15 mm, and the glass A of 10 mm (thickness)×10 mm (width)×100 mm (length) was cut in the same manner as in Example 1 at a cutting difficulty of 0.69 to obtain a slice A2.

[0106] (Example 3)

[0107] The length after cutting was changed to 10 mm, and the glass A of 10 mm (thickness)×10 mm (width)×100 mm (length) was cut in the same manner as in Example 1 at a cutting difficulty of 1.25 to obtain a slice A3.

[0108] (Example 4)

[0109] The thickness is changed to 20 mm, the width is changed to 20 mm (width), and the length after cutting is changed to 20 mm. Under the condition of cutting difficulty of 3.00, glass A of 20 mm (thickness) × 20 mm (width) × 100 mm (length) is cut in the same manner as in Example 1 to obtain slice A4.

[0110] (Example 5)

[0111] The thickness is changed to 20 mm, the width is changed to 38 mm (width), and the length after cutting is changed to 38 mm. Under the condition of cutting difficulty of 4.66, glass A of 20 mm (thickness) × 38 mm (width) × 100 mm (length) is cut in the same manner as in Example 1 to obtain slice A5.

[0112] (Example 6)

[0113] Except that glass A was changed to glass B, the glass was cut in the same manner as in Example 1 to obtain a slice B1.

[0114] (Example 7)

[0115] Except that glass A was replaced by glass B, the glass was cut in the same manner as in Example 3 to obtain a slice B2.

[0116] (Embodiment 8)

[0117] The length after cutting was changed to 7.5 mm, and the cutting was carried out in the same manner as in Example 7 at a cutting difficulty of 2.03 to obtain a slice B3.

[0118] (Example 9)

[0119] Except that glass A was changed to glass C, the glass was cut in the same manner as in Example 1 to obtain a slice C1.

[0120] (Example 10)

[0121] Except that glass A was changed to glass C, the glass was cut in the same manner as in Example 2 to obtain a slice C2.

[0122] (Example 11)

[0123] Except that glass A was replaced by glass C, the glass was cut in the same manner as in Example 3 to obtain a slice C3.

[0124] (Example 12)

[0125] Change the thickness to 15 mm, the width to 15 mm, and the length after cutting to 15 mm. Under the condition of cutting difficulty of 2.06, cut glass C of 15 mm (thickness) × 15 mm (width) × 100 mm (length) in the same manner as in Example 9 to obtain slice C4.

[0126] (Example 13)

[0127] The length after cutting was changed to 12.5 mm, and the cutting was carried out in the same manner as in Example 12 at a cutting difficulty of 2.72 to obtain a slice C5.

[0128] (Example 14)

[0129] The length after cutting was changed to 10 mm, and the cutting was carried out in the same manner as in Example 12 at a cutting difficulty of 3.94 to obtain a slice C6.

[0130] (Example 15)

[0131] Except that glass A was changed to glass D, the glass was cut in the same manner as in Example 3 to obtain a slice D1.

[0132] [Measurement of waviness of cut surface]

[0133] Regarding the waviness, a vertical plane at an angle of 90° to the plane is pressed against the cut surface cut in the embodiment, and the size of the gap D between the vertical plane and the above-mentioned cut surface is measured five times. The gap D per thickness T of the glass, that is, the average value of D / T is measured as the waviness.

[0134] As a waviness measuring device, an L-type stand (manufactured by Sigma Koki Co., Ltd.) was used (see Figure 6 The results are shown in Figure 7For samples with low cutting difficulty, the waviness of samples obtained by manual cutting and by the present invention is of the same degree. On the other hand, even if the cutting difficulty is 0.30 or more, 0.50 or more, 0.70 or more, 0.90 or more, 1.00 or more, 1.25 or more, 1.50 or more, 1.75 or more, or 2.00 or more, for example, 1.00 to 5.00, the waviness is smaller than that of manual cutting, and the sample can be cut into a desired size.

[0135] [Table 1]

[0136]

[0137] [Table 2]

[0138]

[0139] [Table 3]

[0140]

[0141] [Measurement of surface roughness Ra of cut surface]

[0142] In the measurement of the surface roughness Ra of the glass, a scanning white interferometer device, NewView7300 manufactured by ZYGO, was used. The measurement range was 0.36 mm×0.27 mm. The roughness Ra when glass A was cut into 10 mm×10 mm×10 mm was 14.98 nm (the glass material of Example 3 was used).

[0143] On the other hand, as a reference example of a glass surface not included in the cut surface described in the present invention, when glass A was cut into 10 mm × 10 mm × 10 mm using a glass cutter (with a round blade embedded with diamond abrasive grains), the internal conditions could not be observed because the glass surface was in a state of rubbing glass. In addition, Ra was 1000 μm, which was a value larger than Ra of the cut surface.

[0144] Furthermore, as a reference example, when glass A was cut into pieces of 10 mm×10 mm×10 mm and the cut surfaces were polished, Ra of the polished surfaces was 1.19.

[0145] [Measurement of surface element composition]

[0146] X-ray photoelectron spectroscopy (X-ray Photoelectron Spectroscopy, abbreviated as XPS) was used to measure the elemental composition of the surface of Glass E. As an X-ray photoelectron spectrometer, K-Alpha+ manufactured by Thermo Fisher Scientific was used.

[0147] For the cut surface cut by the ultrasonic cutting machine described in this specification and the non-cut surface (polished surface and free surface) described in this specification, the element composition (atomic %) of the surface was measured. The results are shown in Table 4. On the glass surface, compared with the inside of the glass, there is a tendency for the carbon and oxygen content to increase by reacting with carbon dioxide and water in the air to form carbonates, and there is a tendency for the content of ions such as boron and alkali elements that are easily dissolved into water to decrease. However, it can be seen that the cut surface obtained in the present invention has a high content of boron and alkali elements relative to the polished surface and the free surface, and has a composition ratio closer to the inside of the glass.

[0148] [Table 4]

[0149]

Claims

1. A method for cutting glass, characterized in that: include: The process of bringing the ultrasonic vibration blade of the ultrasonic cutting machine into contact with the portion of the glass to be cut; the process of making the ultrasonic vibration blade vibrate ultrasonically in parallel and linearly relative to the contacted glass; and the process of cutting into the glass while generating friction heat in a linear shape using the ultrasonic wave.

2. The glass cutting method according to claim 1, characterized in that: The frequency of the ultrasonic vibration is 5 kHz or more and 50 kHz or less.

3. The glass cutting method according to claim 1 or 2, characterized in that: The amplitude of the ultrasonic vibration is 5 μm or more and 40 μm or less.

4. A glass material, characterized in that: The cutting method according to claim 1 is obtained, wherein the waviness of the cut surface of the glass material is 100 or less, Regarding waviness, a vertical plane at an angle of 90° to the plane is pressed against the cut surface, and the size of the gap D between the vertical plane and the above-mentioned cut surface is measured N times. The gap D per thickness T of the glass, that is, the average value of D / T, is measured as the waviness.

5. A method for manufacturing a glass material, characterized in that: include: The process of bringing the ultrasonic vibration blade of the ultrasonic cutting machine into contact with the part of the glass to be cut; the process of making the ultrasonic vibration blade vibrate ultrasonically in parallel and linearly relative to the contacted glass; and the process of cutting into the glass while generating friction heat in a linear shape using the ultrasonic wave.

6. A glass material obtained by the method for producing a glass material according to claim 5, characterized in that: At least one surface having a waviness of 100 or less and a surface roughness Ra of 500 μm or less, The surface is a cutting surface, Regarding waviness, a vertical plane at an angle of 90° to the plane is pressed against the cut surface, and the size of the gap D between the vertical plane and the above-mentioned cut surface is measured N times. The gap D per thickness T of the glass, that is, the average value of D / T, is measured as the waviness.

7. The glass material according to claim 6, wherein The content of boron and / or alkali components and / or fluorine in the plane is higher than the content of these elements in the glass surface of the glass material that is not contained in the plane.

8. The glass material according to claim 6, wherein The content of boron and / or alkali components and / or fluorine in the surface is 5% or more higher than the content of these elements in the glass surface of the glass material that are not contained in the surface, This value is calculated by (the content of boron and / or alkali components and / or fluorine in the fractured surface) / (the content of these elements in the glass surface not included in the fractured surface).

Citation Information

Patent Citations

  • Cutting-off equipment and cutting-off method

    JP2004155159A

  • The glass cutting device which uses ultrasonic vibration

    KR200384199Y1