Conductive carbon material dispersant for lithium ion battery, slurry for lithium ion battery electrode, electrode for lithium ion battery, and battery
By using specific water-soluble poly(meth)acrylamide as a dispersant, the problem of poor dispersion of conductive carbon materials in lithium-ion batteries is solved, the swellability of the electrolyte and the stability of the electrode are improved, and the overall performance of the battery is improved. .
Patent Information
- Application Number
- CN202011260101.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-15
- Filing Date
- 2020-11-12
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-11-12
AI Technical Summary
The conductive carbon material in lithium-ion batteries is not easy to disperse, resulting in low swelling in the electrolyte and poor electrolyte resistance, affecting the performance of the battery.
Water-soluble poly(meth)acrylamide is used as a dispersant for conductive carbon materials, containing 2-60 mole % methacrylamide compound and 10-70 mole % unsaturated sulfonic acid or its salt, weight average molecular weight It is 10,000 to 300,000, and is used to prepare a slurry for electrodes of lithium-ion batteries, including electrode active substances, conductive carbon materials and water.
Good dispersion of conductive carbon materials is achieved, the swelling rate and electrolyte resistance of the electrolyte are improved, and the storage stability of the electrode and the discharge capacity maintenance rate of the battery are enhanced.
Smart Images

Figure BDA0002774354270000041 
Figure BDA0002774354270000081 
Figure BDA0002774354270000082
Abstract
Description
Technical Field
[0001] The present disclosure relates to a conductive carbon material dispersant for lithium ion batteries, a slurry for lithium ion battery electrodes, an electrode for lithium ion batteries, and a lithium ion battery. Background Art
[0002] Lithium-ion batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and have been used in a wide range of applications. Therefore, in recent years, research has been conducted on improving battery components such as electrodes in order to further improve the performance of lithium-ion batteries.
[0003] The positive and negative electrodes of lithium-ion batteries are manufactured by the following method: a slurry formed by dispersing an electrode active material and a binder resin in a solvent is applied to both sides of a current collector (such as a metal foil), the solvent is dried and removed to form an electrode layer, and then the electrode layer is compression-molded using a roller press or the like.
[0004] The slurry for lithium ion batteries may contain a conductive carbon material as a conductive auxiliary agent. Examples of the conductive carbon material include carbon black and the like. Summary of the invention
[0005] Technical problem to be solved by the invention
[0006] When a conductive carbon material is included in the slurry for lithium ion batteries, such conductive carbon material is sometimes not dispersed in the slurry. In such a case, the conductive carbon material cannot fully play the role of a conductive aid. Therefore, a dispersant for dispersing the conductive carbon material is required. In addition, since the dispersant is used in lithium ion batteries, it is preferred that the swelling property (swelling property) is low relative to the electrolyte of the lithium ion battery and the electrolyte resistance is good.
[0007] Therefore, the technical problem to be solved by the present invention is to provide a conductive carbon material dispersant for lithium ion batteries that can well disperse the conductive carbon material for lithium ion batteries, has low swelling properties with respect to the electrolyte of lithium ion batteries, and has good electrolyte resistance.
[0008] Technical means to solve technical problems
[0009] As a result of intensive studies, the present inventors have found that the above-mentioned technical problems are solved by using specific components.
[0010] The following items are provided by the present disclosure.
[0011] (Item 1)
[0012] A conductive carbon material dispersant for lithium ion batteries, the conductive carbon material dispersant for lithium ion batteries containing a water-soluble poly(meth)acrylamide (A-1), the water-soluble poly(meth)acrylamide (A-1) containing 2 mol% to 60 mol% of a structural unit derived from a compound (a) containing a (meth)acrylamide group and 10 mol% to 70 mol% of a structural unit derived from an unsaturated sulfonic acid or a salt thereof (b), and having a weight average molecular weight of 10,000 to 300,000.
[0013] (Item 2)
[0014] In the conductive carbon material dispersant for lithium ion batteries as described in the above item, the water-soluble poly(meth)acrylamide (A-1) contains 20 mol % to 70 mol % of a structural unit derived from the (meth)acrylate (c).
[0015] (Item 3)
[0016] A slurry for lithium-ion battery electrodes, comprising:
[0017] The conductive carbon material dispersant for lithium ion batteries as described in any one of the above items;
[0018] Polymer (A-2);
[0019] Electrode active material (B-1);
[0020] A conductive carbon material (B-2); and
[0021] water.
[0022] (Item 4)
[0023] In the slurry for lithium ion battery electrodes as described in the above item, the polymer (A-2) is a water-soluble poly (meth)acrylamide (A-2A) containing a structural unit derived from the (meth)acrylamide group-containing compound (a).
[0024] (Item 5)
[0025] An electrode for a lithium ion battery obtained by applying the slurry for a lithium ion battery electrode as described in any one of the above items on a current collector and drying the slurry.
[0026] (Item 6)
[0027] A lithium ion battery comprising the lithium ion battery electrode as described in the above item.
[0028] In the present disclosure, in addition to the combinations explicitly described, one or more of the above features may be provided in further combinations.
[0029] Beneficial Effects
[0030] The conductive carbon material dispersant for lithium ion batteries of the present invention makes the conductive carbon material for lithium ion batteries dispersed well. Moreover, the conductive carbon material dispersant for lithium ion batteries has a low electrolyte swelling rate and high electrolyte resistance. In addition, the slurry for lithium ion battery electrodes of the present invention has excellent storage stability. Further, the electrode of the present invention has excellent electrode adhesion (close adhesion). Moreover, the battery of the present invention has an excellent discharge capacity retention rate. DETAILED DESCRIPTION
[0031] In the entire scope of the present disclosure, the range of the numerical values of each physical property value, content, etc. can be appropriately set (for example, selected from the upper and lower limit values described in each of the following items). Specifically, with respect to the numerical value α, when A4, A3, A2, A1 (A4>A3>A2>A1) and the like are exemplified as the upper and lower limits of the numerical value α, the range of the numerical value α is exemplified as less than A4, less than A3, less than A2, more than A1, more than A2, more than A3, A1-A2, A1-A3, A1-A4, A2-A3, A2-A4, A3-A4, etc.
[0032] [Conductive carbon material dispersant for lithium-ion batteries: also called dispersant]
[0033] The present disclosure provides a conductive carbon material dispersant for lithium ion batteries, wherein the conductive carbon material dispersant for lithium ion batteries contains a water-soluble poly(meth)acrylamide (A-1), wherein the water-soluble poly(meth)acrylamide (A-1) contains 2 mol% to 60 mol% of structural units derived from a compound (a) containing a (meth)acrylamide group and 10 mol% to 70 mol% of structural units derived from an unsaturated sulfonic acid or a salt thereof (b), and has a weight average molecular weight of 10,000 to 300,000.
[0034] <Water-soluble poly(meth)acrylamide (A-1): also referred to as component (A-1). >
[0035] The component (A-1) may be used alone or in combination of two or more.
[0036] In the present disclosure, "water-soluble" means that when 0.5 g of the compound is dissolved in 100 g of water at 25°C, the insoluble component is less than 0.5% by mass (less than 2.5 mg).
[0037] In the present disclosure, “(meth)acrylic acid” means “at least one selected from the group consisting of acrylic acid and methacrylic acid”. Similarly, “(meth)acrylate” means “at least one selected from the group consisting of acrylate and methacrylate”. Furthermore, “(meth)acryloyl” means “at least one selected from the group consisting of acryloyl and methacryloyl”.
[0038] <(Meth)acrylamide-containing compound (a): also referred to as component (a)>
[0039] In the present disclosure, "a (meth)acrylamide group-containing compound" refers to a compound having a (meth)acrylamide group. The (meth)acrylamide group-containing compound can be any known compound without particular limitation, and can be used alone or in combination of two or more.
[0040] In one embodiment, the (meth)acrylamide-containing compound is represented by the following structural formula:
[0041] [Chemistry 1]
[0042]
[0043] (Where R 1 is a hydrogen atom or a methyl group; R 2 and R 3 are each independently a hydrogen atom, a substituted or unsubstituted alkyl group, or an acetyl group, or R 2 and R 3 are groups that together form a ring structure; R 4 and R 5 are each independently a hydrogen atom, a substituted or unsubstituted alkyl group, a hydroxyl group, an amino group (-NR a R b (R a and R b Each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group) or an acetyl group. Examples of substituents of the substituted alkyl group include hydroxyl, amino, acetyl, and the like. 2 and R 3 Examples of the groups that form a ring structure together include morpholino and the like. )
[0044] Examples of the alkyl group include a linear alkyl group, a branched alkyl group, and a cycloalkyl group.
[0045] Straight chain alkyl is composed of the general formula -C n H 2n+1 (n is an integer greater than or equal to 1). Examples of the linear alkyl group include methyl, ethyl, propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl.
[0046] The branched alkyl group is a group in which at least one hydrogen atom of a linear alkyl group is substituted by an alkyl group. Examples of the branched alkyl group include isopropyl, isobutyl, sec-butyl, tert-butyl, diethylpentyl, trimethylbutyl, trimethylpentyl, and trimethylhexyl.
[0047] Examples of the cycloalkyl group include a monocyclic cycloalkyl group, a bridged ring cycloalkyl group, and a condensed ring cycloalkyl group.
[0048] In the present disclosure, a monocyclic ring refers to a ring structure formed by a covalent bond of carbon and having no internal bridge structure. In addition, a fused ring refers to a ring structure in which two or more monocyclic rings share two atoms (i.e., each ring only shares (condenses) one side with each other). A bridged ring refers to a ring structure in which two or more monocyclic rings share three or more atoms.
[0049] Examples of the monocyclic cycloalkyl group include cyclopentyl, cyclohexyl, cycloheptyl, cyclodecyl, and 3,5,5-trimethylcyclohexyl.
[0050] Examples of the bridged cycloalkyl group include tricyclodecanyl, adamantyl, and norbornyl.
[0051] Examples of the fused ring cycloalkyl group include bicyclodecanyl and the like.
[0052] Examples of the (meth)acrylamide group-containing compound (a) include (meth)acrylamide, N-isopropyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, diacetone (meth)acrylamide, maleic acid amide (maleic acid amide), (meth)acryloyl morpholine, hydroxyethyl (meth)acrylamide and salts thereof; examples of the salt include dimethylaminopropyl (meth)acrylamide methyl chloride quaternary salt (Methyl quaternary salt), dimethylaminoethyl (meth)acrylate benzyl chloride quaternary salt (benzyl chloride quaternary salt) and the like. Among them, when (meth)acrylamide, especially acrylamide, is used, it is possible to produce a binder that not only reduces water absorption while maintaining water solubility, but also reduces irreversible capacity, has high interaction with electrode active materials, high dispersibility in slurry, and high adhesion between electrode active materials inside the electrode.
[0053] The upper and lower limits of the content of the structural unit derived from the (meth)acrylamide group-containing compound relative to 100 mol% of all structural units of the component (A-1) are exemplified by 60 mol%, 59 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 9 mol%, 5 mol%, 3 mol%, 2 mol%, etc. In one embodiment, the above content is preferably 2 mol% to 60 mol%.
[0054] The upper and lower limits of the content of the structural unit derived from the compound containing a (meth)acrylamide group relative to 100 mass% of all structural units of the (A-1) component are exemplified by 70 mass%, 65 mass%, 60 mass%, 55 mass%, 50 mass%, 45 mass%, 40 mass%, 35 mass%, 30 mass%, 25 mass%, 20 mass%, 15 mass%, 10 mass%, 9 mass%, 5 mass%, 4 mass%, 2 mass%, 1 mass%, etc. In one embodiment, the above content is preferably 1 mass% to 70 mass%.
[0055] <Unsaturated sulfonic acid or its salt (b): also referred to as component (b)>
[0056] The component (b) may be any of various known components without particular limitation, and may be used alone or in combination of two or more. In addition, in the present disclosure, when compound A is both component (a) and component (b), the compound A is component (b).
[0057] Examples of the unsaturated sulfonic acid include α,β-ethylenically unsaturated sulfonic acids such as vinylsulfonic acid, styrylsulfonic acid, and (meth)allylsulfonic acid; (meth)acrylamide-tert-butylsulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, 2-(meth)acrylamide-2-hydroxypropanesulfonic acid, 3-sulfopropane (meth)acrylate, and bis-(3-sulfopropyl)itaconate.
[0058] Examples of the salt of unsaturated sulfonic acid include inorganic salts of unsaturated sulfonic acid. The inorganic salt of unsaturated sulfonic acid refers to a salt whose cation part is a metal cation. Examples of the inorganic salt include main group metal salts (typical metal salts), transition metal salts, and the like.
[0059] Examples of the main group metal salt include alkali metal salts, alkaline earth metal salts, and Group 13 metal salts.
[0060] Examples of the alkali metal salt include lithium salt, sodium salt, potassium salt and the like.
[0061] Examples of the alkaline earth metal salt include magnesium salt and calcium salt.
[0062] Examples of the Group 13 metal salt include aluminum salts and the like.
[0063] Examples of the transition metal salt include iron salts and the like.
[0064] The upper and lower limits of the content of the structural unit derived from the unsaturated sulfonic acid or its salt (b) relative to 100 mol% of all structural units of the component (A-1) are exemplified by 70 mol%, 69 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, etc. In one embodiment, the above content is preferably 10 mol% to 70 mol%.
[0065] The upper and lower limits of the content of the structural unit derived from the unsaturated sulfonic acid or its salt (b) relative to 100% by mass of all structural units of the component (A-1) are exemplified by 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, 15% by mass, 10% by mass, 5% by mass, etc. In one embodiment, the above content is preferably 5% to 70% by mass.
[0066] <(Meth)acrylate (c): also referred to as component (c)>
[0067] As the component (c), various known components can be used without particular limitation, and the component (c) may be used alone or in combination of two or more.
[0068] Examples of the (meth)acrylate include (meth)acrylates not containing a substituent and (meth)acrylates containing a substituent.
[0069] In the present disclosure, a (meth)acrylate having no substituent refers to a (meth)acrylate in which the atoms forming the compound are carbon atoms and hydrogen atoms except for the oxygen atom forming the ester bond. A (meth)acrylate having a substituent refers to a (meth)acrylate that is not a (meth)acrylate having no substituent.
[0070] Examples of the (meth)acrylates not containing a substituent include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate.
[0071] Examples of the substituted (meth)acrylate include a hydroxyl group-containing (meth)acrylate and an alkoxy group-containing (meth)acrylate.
[0072] Examples of the hydroxyl-containing (meth)acrylate include 1-hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxy-1-methylethyl (meth)acrylate, 1-hydroxy-2-methylethyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1-hydroxy-1-methyl-propyl (meth)acrylate, 2-hydroxy-1-methyl-propyl (meth)acrylate, 3-hydroxy-1-methyl-propyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1-hydroxy-1-methyl-propyl (meth)acrylate, 2-hydroxy-1-methyl-propyl (meth)acrylate, 3-hydroxy-1-methyl-propyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxy-1-methyl-propyl (meth)acrylate, 3 ... Ethyl-2-hydroxyethyl ester, 1-hydroxy-2-methyl-propyl (meth)acrylate, 2-hydroxy-2-methyl-propyl (meth)acrylate, 3-hydroxy-2-methyl-propyl (meth)acrylate, 1,1-dimethyl-2-hydroxyethyl (meth)acrylate, 3-hydroxy-1-adamantyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, glycerol mono(meth)acrylate, glycerol di(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, polyethylene glycol-mono(meth)acrylate, polypropylene glycol-mono(meth)acrylate, polyethylene glycol-propylene glycol-mono(meth)acrylate, and the like.
[0073] Examples of the alkoxy-containing (meth)acrylate include methoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 1-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, 1-methoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-methoxybutyl (meth)acrylate, 1-methoxybutyl (meth)acrylate, ethoxymethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 1-ethoxyethyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 2-ethoxypropyl (meth)acrylate, 1-ethoxypropyl (meth)acrylate, propoxymethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 1-propoxyethyl (meth)acrylate, butoxymethyl (meth)acrylate, and the like.
[0074] In one embodiment, the (meth)acrylate is represented by the following structural formula:
[0075] [Chemistry 2]
[0076]
[0077] In the formula, R α1 is a hydrogen atom or a methyl group;
[0078] R α2 It is an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group or a polyoxyalkylene group represented by [Chemical 3]:
[0079] [Chemistry 3]
[0080]
[0081] (wherein, q is an integer of 1 to 3, and n is an integer of 0 to 100, preferably 0 to 10);
[0082] R α3 and R α4 are each independently a hydrogen atom, a substituted or unsubstituted alkyl group, a carboxyl group, a hydroxyl group, an amino group [-NR a R b (R a and R b Each is independently a hydrogen atom or a substituted or unsubstituted alkyl group)], or an acetyl group. Examples of the substituent of the substituted alkyl group include a hydroxyl group, an alkoxy group, an amino group, and an acetyl group.
[0083] The hydroxyalkyl group is a group in which at least one hydrogen atom of an alkyl group is substituted with a hydroxyl group (hydrogen acid group).
[0084] The alkoxyalkyl group is a group in which at least one hydrogen atom of an alkyl group is substituted with an alkoxy group.
[0085] An alkoxy group is a monovalent group in which an alkyl group is bonded to an oxygen atom.
[0086] The upper and lower limits of the content of the structural unit derived from the (meth)acrylate (c) relative to 100 mol% of all structural units of the component (A-1) are exemplified by 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, etc. In one embodiment, the above content is preferably 20 mol% to 70 mol%.
[0087] The upper and lower limits of the content of the structural unit derived from the (meth)acrylate (c) relative to 100% by mass of all the structural units of the component (A-1) are exemplified by 80% by mass, 75% by mass, 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, etc. In one embodiment, the above content is preferably 20% to 80% by mass.
[0088] <Monomers other than component (a), component (b), and component (c): also referred to as component (d)>
[0089] As long as the desired effect of the present invention is not impaired, among all the structural units of the component (A-1), a structural unit derived from a monomer (component (d)) that does not belong to any of the components (a), (b), and (c) can be used. The component (d) can be used alone or in combination of two or more. Examples of the component (d) include unsaturated carboxylic acids, unsaturated phosphoric acids, α, β-unsaturated nitriles, conjugated dienes, vinyl ethers, aromatic vinyl compounds, and the like.
[0090] Examples of the unsaturated carboxylic acid include (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid.
[0091] The content of the structural units derived from the unsaturated carboxylic acid is preferably less than 40 mol% (for example, less than 30 mol%, less than 25 mol%, less than 20 mol%, less than 19 mol%, less than 15 mol%, less than 10 mol%, less than 5 mol%, less than 1 mol%, or 0 mol%) relative to 100 mol% of all the structural units of the component (A-1).
[0092] The content of the structural unit derived from the unsaturated carboxylic acid relative to 100 mass % of all the structural units of the component (A-1) is preferably less than 40 mass % (for example, less than 30 mass %, less than 25 mass %, less than 20 mass %, less than 19 mass %, less than 15 mass %, less than 10 mass %, less than 5 mass %, less than 1 mass %, or 0 mass %).
[0093] Examples of the unsaturated phosphoric acid include vinylphosphonic acid, vinyl phosphate, bis((meth)acryloyloxyethyl)phosphate, diphenyl-2-(meth)acryloyloxyethyl phosphate, dibutyl-2-(meth)acryloyloxyethyl phosphate, dioctyl-2-(meth)acryloyloxyethyl phosphate, monomethyl-2-(meth)acryloyloxyethyl phosphate, and 3-(meth)acryloyloxy-2-hydroxypropanephosphoric acid.
[0094] The content of the structural units derived from unsaturated phosphoric acid relative to 100 mol% of all the structural units of the component (A-1) is preferably less than 40 mol% (for example, less than 30 mol%, less than 25 mol%, less than 20 mol%, less than 19 mol%, less than 15 mol%, less than 10 mol%, less than 5 mol%, less than 1 mol%, 0 mol%).
[0095] The content of the structural unit derived from unsaturated phosphoric acid relative to 100 mass % of all the structural units of the component (A-1) is preferably less than 40 mass % (for example, less than 30 mass %, less than 25 mass %, less than 20 mass %, less than 19 mass %, less than 15 mass %, less than 10 mass %, less than 5 mass %, less than 1 mass %, or 0 mass %).
[0096] α,β-unsaturated nitriles can be suitably used for the purpose of imparting flexibility to electrodes. Examples of α,β-unsaturated nitriles include (meth)acrylonitrile, α-chloro(meth)acrylonitrile, α-ethyl(meth)acrylonitrile, vinylidene cyanide, etc. Among them, (meth)acrylonitrile is preferred, and acrylonitrile is particularly preferred.
[0097] The content of the structural unit derived from the α,β-unsaturated nitrile is not particularly limited, but is preferably less than 40 mol% (for example, less than 30 mol%, less than 25 mol%, less than 20 mol%, less than 19 mol%, less than 15 mol%, less than 10 mol%, less than 5 mol%, less than 1 mol%, or 0 mol%) relative to 100 mol% of all the structural units of the component (A-1).
[0098] In one embodiment, the content of the structural unit derived from the α,β-unsaturated nitrile is preferably less than 40 mass% (e.g., less than 30 mass%, less than 25 mass%, less than 20 mass%, less than 19 mass%, less than 15 mass%, less than 10 mass%, less than 5 mass%, less than 1 mass%, or 0 mass%) relative to 100 mass% of all the structural units of the component (A-1).
[0099] Examples of the conjugated diene include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted straight-chain conjugated pentadiene, and substituted side-chain conjugated hexadiene (substituted and side-chain conjugated hexadiene).
[0100] The content of the structural unit derived from the conjugated diene is not particularly limited, but is preferably less than 10 mol%, more preferably 0 mol%, based on 100 mol% of all the structural units of the component (A-1).
[0101] In one embodiment, the content of the structural unit derived from the conjugated diene is preferably less than 10% by mass, more preferably 0% by mass, based on 100% by mass of all the structural units of the component (A-1).
[0102] Examples of the vinyl ether include hydroxyalkyl vinyl ether and polyalkylene glycol monovinyl ether.
[0103] Examples of the hydroxyalkyl vinyl ether include hydroxy linear alkyl vinyl ether, hydroxy branched alkyl vinyl ether, and hydroxy cycloalkyl vinyl ether.
[0104] Examples of the hydroxy linear alkyl vinyl ether include 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, and 5-hydroxypentyl vinyl ether.
[0105] Examples of the hydroxy branched alkyl vinyl ether include 2-hydroxypropyl vinyl ether, 2-hydroxy-2-methylpropyl vinyl ether, and 4-hydroxy-2-methylbutyl vinyl ether.
[0106] Examples of the hydroxycycloalkyl vinyl ether include 4-hydroxycyclopentyl vinyl ether and the like.
[0107] Examples of the polyalkylene glycol monovinyl ether include polymethylene glycol monovinyl ether, polyethylene glycol monovinyl ether, and polypropylene glycol monovinyl ether.
[0108] The content of the structural unit derived from vinyl ether is not particularly limited, but is preferably less than 30 mol%, more preferably 0 mol%, based on 100 mol% of all the structural units of the component (A-1).
[0109] In one embodiment, the content of the structural unit derived from vinyl ether is preferably less than 30% by mass, more preferably 0% by mass, based on 100% by mass of all structural units of the component (A-1).
[0110] Examples of the aromatic vinyl compound include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, chlorostyrene, and divinylbenzene.
[0111] The content of the structural unit derived from the aromatic vinyl compound is not particularly limited, but is preferably less than 10 mol%, more preferably 0 mol%, based on 100 mol% of all the structural units of the component (A-1).
[0112] In one embodiment, the content of the structural unit derived from the aromatic vinyl compound is preferably less than 10% by mass, more preferably 0% by mass, based on 100% by mass of all structural units of the component (A-1).
[0113] The ratio of the structural units derived from the component (d) other than the unsaturated carboxylic acid, unsaturated phosphoric acid, α,β-unsaturated nitrile, conjugated diene, vinyl ether and aromatic vinyl compound in all the structural units of the component (A-1) is less than 10 mol%, less than 5 mol%, less than 1 mol%, less than 0.1 mol%, less than 0.01 mol% or 0 mol% relative to 100 mol% of all the structural units of the component (A-1); and less than 10 mass%, less than 5 mass%, less than 1 mass%, less than 0.5 mass%, less than 0.1 mass%, less than 0.01 mass% or 0 mass% relative to 100 mass% of all the structural units of the component (A-1).
[0114] Water-soluble poly (meth) acrylamide (A-1) can be synthesized using various known polymerization methods, preferably using a free radical polymerization method. The polymerization reaction is carried out by adding a free radical polymerization initiator and a chain transfer agent as required to a monomer mixture containing components (a) and (b) and components (c) and (d) as required, and stirring at a reaction temperature of about 50°C to 100°C. The reaction time is not particularly limited, and is preferably about 1 hour to 10 hours. In one embodiment, it is preferred that component (A-1) is manufactured by simultaneously dropping a solution containing a monomer and a solution containing an initiator to carry out a polymerization reaction.
[0115] The radical polymerization initiator is not particularly limited, and various known radical polymerization initiators can be used. Examples of the radical polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; redox polymerization initiators in which the above persulfates are combined with a reducing agent such as sodium bisulfite; azo initiators such as 2,2'-azobis-2-amidinopropane dihydrochloride (2,2'-azobis-2-amidinopropane dihydrochloride). The amount of the radical polymerization initiator used is not particularly limited, but is preferably 0.05% to 5.0% by mass, more preferably 0.1% to 3.0% by mass, relative to 100% by mass of all structural units of the component (A-1) providing the component (A-1).
[0116] Before the free radical polymerization reaction and / or when the obtained component (A-1) is dissolved in water, the pH of the reaction solution may be adjusted using a common neutralizing agent such as ammonia and organic amines, potassium hydroxide, sodium hydroxide, lithium hydroxide, etc. for the purpose of improving the manufacturing stability. In this case, the pH is preferably 2 to 11. In addition, EDTA or its salts may be used as metal ion sealants for the same purpose.
[0117] <Physical Properties of Water-Soluble Poly(Meth)acrylamide (A-1)>
[0118] The upper limit and lower limit of the glass transition temperature of the water-soluble poly(meth)acrylamide (A-1) are exemplified by 160°C, 155°C, 150°C, 145°C, 140°C, 135°C, 130°C, 125°C, 120°C, 115°C, 110°C, 105°C, 100°C, 95°C, 90°C, 85°C, 80°C, 75°C, 70°C, 65°C, 60°C, 55°C, 50°C, 45°C, 40°C, 35°C, 30°C, 25°C, 20°C, 15°C, 10°C, 5°C, 0°C, etc. In one embodiment, it is preferably 0°C or higher, and more preferably 30°C or higher from the viewpoint of mechanical strength and heat resistance.
[0119] The glass transition temperature of the water-soluble poly(meth)acrylamide can be adjusted by the combination of monomers. The glass transition temperature of the water-soluble poly(meth)acrylamide (A-1) can be determined from the glass transition temperature (Tg, absolute temperature: K) of the homopolymer of the monomers and their mass fractions according to the Fox equation shown below.
[0120] 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+(W3 / Tg3)+…+(W n / Tg n )
[0121] [Wherein, Tg represents the glass transition temperature (K) of the polymer to be determined, W1~W n Indicates the mass fraction of each monomer, Tg1~Tg n represents the glass transition temperature (K) of each monomer homopolymer].
[0122] For example, the glass transition temperature is 165°C for acrylamide homopolymers, 106°C for acrylic acid homopolymers, -15°C for hydroxyethyl acrylate homopolymers, and 105°C for acrylonitrile homopolymers. In order to obtain a water-soluble poly(meth)acrylamide (A-1) having a desired glass transition temperature, the composition of the monomers constituting it can be determined. In addition, the glass transition temperature of the homopolymer of the monomer can be measured by DSC (differential scanning calorimeter), DTA (differential thermal analyzer), TMA (thermomechanical analyzer), etc., for example, under conditions of heating from -100°C to 300°C (heating rate 10°C / min.). In addition, the values recorded in the literature can also be used. The literature exemplifies "Chemical Handbook (Chemical Handbook) Basics II Edited by the Chemical Society of Japan (Revised 5th Edition)", p325, etc.
[0123] The upper and lower limits of the weight average molecular weight (Mw) of the water-soluble poly (meth) acrylamide (A-1) are exemplified by 300,000, 290,000, 250,000, 200,000, 150,000, 100,000, 90,000, 50,000, 40,000, 30,000, 20,000, 10,000, etc. In one embodiment, the weight average molecular weight (Mw) of the water-soluble poly (meth) acrylamide (A-1) is preferably 10,000 to 300,000; from the viewpoint of improving the dispersibility of the conductive carbon material and preventing the formation of agglomerates, it is more preferably 10,000 or more and less than 300,000.
[0124] The upper and lower limits of the number average molecular weight (Mn) of the water-soluble poly(meth)acrylamide (A-1) are exemplified by 110,000, 100,000, 90,000, 70,000, 50,000, 30,000, 20,000, 10,000, 9,000, 7,000, 5,000, etc. In one embodiment, the number average molecular weight (Mn) of the water-soluble poly(meth)acrylamide (A-1) is preferably 5,000 to 110,000.
[0125] The weight average molecular weight and the number average molecular weight can be determined as polyacrylic acid-equivalent values measured by gel permeation chromatography (GPC) in an appropriate solvent, for example.
[0126] The upper and lower limits of the molecular weight distribution (Mw / Mn) of the water-soluble poly(meth)acrylamide (A-1) are exemplified by 15, 14, 13, 12, 11, 10, 9, 8, 7.5, 6, 5, 4, 3, 2.9, 2.5, 2, 1.5, 1.1, etc. In one embodiment, the molecular weight distribution (Mw / Mn) of the water-soluble poly(meth)acrylamide (A-1) is preferably 1.1 to 15.
[0127] The upper and lower limits of the B-type viscosity of the conductive carbon material dispersant for lithium ion batteries containing water-soluble poly (meth) acrylamide (A-1) are exemplified by 500mPa·s, 450mPa·s, 400mPa·s, 350mPa·s, 300mPa·s, 250mPa·s, 200mPa·s, 150mPa·s, 100mPa·s, 50mPa·s, 25mPa·s, 10mPa·s, etc. In one embodiment, the above-mentioned B-type viscosity is preferably 10mPa·s to 500mPa·s.
[0128] The B-type viscosity is measured using a B-type viscometer such as "B-type Viscometer TVB-10M Model" manufactured by Toki Sangyo Co., Ltd.
[0129] The upper and lower limits of the pH of the conductive carbon material dispersant for lithium ion batteries are exemplified by 7, 6.9, 6.5, 6, 5.9, 5.6, 5.5, 5.4, 5.2, 5.1, 5, etc. In one embodiment, from the viewpoint of solution stability, the pH is preferably pH 5 to 7, more preferably pH 5 or more and less than 7.
[0130] The pH can be measured at 25° C. using a glass electrode pH meter (for example, manufactured by Horiba, Ltd., product name “pH meter D-52”).
[0131] The upper and lower limits of the content of the water-soluble poly (meth) acrylamide (A-1) relative to 100% by mass of the conductive carbon material dispersant for lithium ion batteries are exemplified by 100% by mass, 95% by mass, 90% by mass, 85% by mass, 80% by mass, 75% by mass, 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, 19% by mass, 17% by mass, 15% by mass, 13% by mass, 10% by mass, 9% by mass, 7% by mass, 5% by mass, etc. In one embodiment, the above content is preferably 5% to 100% by mass.
[0132] In one embodiment, the conductive carbon material dispersant for lithium ion batteries may include water. Relative to 100% by mass of the conductive carbon material dispersant for lithium ion batteries, the upper and lower limits of the content of water are exemplified by 95% by mass, 90% by mass, 85% by mass, 80% by mass, 75% by mass, 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, 15% by mass, 10% by mass, 5% by mass, 0% by mass, etc. In one embodiment, the above content is preferably 0% to 95% by mass.
[0133] The upper and lower limits of the mass ratio of water to the component (A-1) [mass of water / mass of the component (A-1)] contained in the conductive carbon material dispersant for lithium ion batteries are exemplified by 19, 17, 15, 13, 10, 9, 7, 5, 3, 2, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0, etc. In one embodiment, the mass ratio is preferably 0 to 19.
[0134] In one embodiment, the conductive carbon material dispersant for lithium ion batteries may include an organic solvent.
[0135] Examples of organic solvents include ether solvents, ketone solvents, alcohol solvents, and amide solvents. Examples of ether solvents include dioxane and tetrahydrofuran (THF). Examples of ketone solvents include acetone and methyl ethyl ketone (MEK). Examples of alcohol solvents include methanol, ethanol, 2-propanol, and isopropanol. Examples of amide solvents include N-methyl-2-pyrrolidone (NMP).
[0136] The upper and lower limits of the content of the organic solvent relative to 100% by mass of the above-mentioned (A-1) component are exemplified by 200% by mass, 175% by mass, 150% by mass, 125% by mass, 100% by mass, 75% by mass, 50% by mass, 25% by mass, 0% by mass, etc. In one embodiment, the above-mentioned content is preferably 0% by mass to 200% by mass.
[0137] <Neutralizer>
[0138] In one embodiment, the conductive carbon material dispersant for lithium ion batteries may include a neutralizer.
[0139] Examples of the neutralizing agent include alkali metal salts and alkaline earth metal salts.
[0140] Examples of the alkali metal salt include lithium salt, sodium salt, potassium salt and the like.
[0141] Examples of the lithium salt include lithium hydroxide, lithium chloride, lithium fluoride, lithium bromide, lithium acetate, lithium sulfate, lithium carbonate, lithium phosphate, and lithium hydrogen carbonate.
[0142] Examples of the sodium salt include sodium hydroxide, sodium chloride, sodium fluoride, sodium bromide, sodium acetate, sodium sulfate, sodium carbonate, sodium phosphate, and sodium bicarbonate.
[0143] Examples of the potassium salt include potassium hydroxide, potassium chloride, potassium fluoride, potassium bromide, potassium acetate, potassium sulfate, potassium carbonate, potassium phosphate, and potassium hydrogen carbonate.
[0144] Examples of the alkaline earth metal salt include calcium salt and magnesium salt.
[0145] Examples of the magnesium salt include magnesium hydroxide, magnesium chloride, magnesium fluoride, magnesium bromide, magnesium acetate, magnesium sulfate, magnesium carbonate, magnesium phosphate, and magnesium hydrogen carbonate.
[0146] Examples of the calcium salt include calcium hydroxide, calcium chloride, calcium fluoride, calcium bromide, calcium acetate, calcium sulfate, calcium carbonate, calcium phosphate, and calcium hydrogen carbonate.
[0147] The upper and lower limits of the content of the neutralizer relative to 100 mol% of the acidic group (acidic group) contained in the above-mentioned (A-1) component are exemplified by 100 mol%, 95 mol%, 90 mol%, 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 0 mol%, etc. In one embodiment, the above-mentioned content is preferably 0 mol% to 100 mol%.
[0148] Examples of the acidic group contained in the component (A-1) include a sulfonic acid group, a carboxylic acid group, and a phosphoric acid group.
[0149] <Additives>
[0150] The conductive carbon material dispersant for lithium ion batteries may contain an agent that does not belong to any of the components (A-1), water, organic solvents, and neutralizers as an additive. Examples of additives include the additives described below. As for the content of the additive, relative to 100% by mass of the component (A-1), examples include 0% to 5% by mass, less than 1% by mass, less than 0.1% by mass, less than 0.01% by mass, and 0% by mass; in addition, relative to 100% by mass of the conductive carbon material dispersant for lithium ion batteries, examples include 0% to 5% by mass, less than 1% by mass, less than 0.1% by mass, less than 0.01% by mass, and 0% by mass.
[0151] The conductive carbon material dispersant for lithium ion batteries can be used as a conductive carbon material dispersant for lithium ion battery electrodes, a conductive carbon material dispersant for lithium ion battery negative electrodes, and a conductive carbon material dispersant for lithium ion battery positive electrodes.
[0152] Examples of the conductive carbon material include the materials described later.
[0153] [Lithium-ion battery electrode slurry: also called slurry]
[0154] The present disclosure provides a slurry for lithium ion battery electrodes, which comprises the above-mentioned conductive carbon material dispersant for lithium ion batteries, a polymer (A-2), an electrode active material (B-1), a conductive carbon material (B-2) and water.
[0155] Relative to 100 mass % of the slurry, the upper and lower limits of the content of the conductive carbon material dispersant for lithium ion batteries are exemplified by 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 9 mass %, 5 mass %, 4 mass %, 2 mass %, 1 mass %, 0.9 mass %, 0.5 mass %, 0.4 mass %, 0.2 mass %, 0.1 mass %, etc. In one embodiment, the content is preferably 0.1 mass % to 40 mass %.
[0156] The upper and lower limits of the content of the component (A-1) relative to 100 mass % of the slurry are exemplified by 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 9 mass %, 5 mass %, 4.5 mass %, 2 mass %, 1 mass %, 0.9 mass %, 0.5 mass %, 0.4 mass %, 0.2 mass %, 0.1 mass %, etc. In one embodiment, the content is preferably 0.1 mass % to 40 mass %.
[0157] <Polymer (A-2): Also referred to as (A-2) component>
[0158] The polymer can be used alone or in combination of two or more. The polymer can be used as an adhesive or a water-based adhesive. The polymer refers to a polymer solid component synthesized in water or an organic solvent.
[0159] Examples of the polymer include water-soluble polymers and water-insoluble polymers.
[0160] Examples of water-soluble polymers include cellulose compounds, denpin, starch, alginic acid, xanthan gum, chitosan, carrageenan, agar, dextrin, gelatin, polyvinyl alcohol, poly(meth)acrylamide, poly(meth)acrylic acid, polysulfonic acid, polyethyleneimine, polyethylene oxide, polyvinyl pyrrolidone, polyethylene glycol, polystyrene sulfonic acid, ethylene-acrylic acid copolymer, ethylene-acrylamide-acrylic acid copolymer, polyamidine, polyvinyl imidazoline, and derivatives or salts thereof.
[0161] In the present disclosure, "water-insoluble" means that when 0.5 g of the compound is dissolved in 100 g of water at 25°C, the insoluble component is 0.5% by mass or more.
[0162] Examples of the water-insoluble polymer include styrene-butadiene copolymer latex, polystyrene polymer latex, polybutadiene polymer latex, acrylonitrile-butadiene copolymer latex, polyurethane polymer latex, polymethyl methacrylate polymer latex, methyl methacrylate-butadiene copolymer latex, polyacrylate polymer latex, vinyl chloride polymer latex, vinyl acetate polymer emulsion, vinyl acetate-ethylene copolymer emulsion, polyethylene emulsion, carboxyl-modified styrene-butadiene copolymer resin emulsion, acrylic resin emulsion, polyethylene, polypropylene, polyethylene terephthalate, polyamide (PA), polyimide (PI), polyamideimide (PAI), aromatic polyamide, alginic acid and its salts, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), and the like.
[0163] In one embodiment, the polymer (A-2) is a water-soluble poly (meth)acrylamide (A-2A) containing a structural unit derived from the (meth)acrylamide group-containing compound (a).
[0164] <Water-soluble poly(meth)acrylamide (A-2A): also referred to as (A-2A) component>
[0165] The component (A-2A) contains a structural unit derived from a (meth)acrylamide-containing compound (a). The (meth)acrylamide-containing compound (a) may be used alone or in combination of two or more. From the viewpoint of electrode adhesion, the components (A-1) and (A-2A) are preferably compatible.
[0166] The upper and lower limits of the content of the structural unit derived from the (meth)acrylamide group-containing compound relative to 100 mol% of all structural units of the component (A-2A) are exemplified by 100 mol%, 99.99 mol%, 99.9 mol%, 99.7 mol%, 99.5 mol%, 99 mol%, 95 mol%, 90 mol%, 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 9 mol%, 5 mol%, 3 mol%, 2 mol%, 1 mol%, etc. In one embodiment, the above content is preferably 1 mol% to 100 mol%.
[0167] The upper and lower limits of the content of the structural unit derived from the (meth)acrylamide group-containing compound relative to 100% by mass of all the structural units of the component (A-2A) are exemplified by 100% by mass, 99.99% by mass, 99.9% by mass, 99.7% by mass, 99.5% by mass, 99% by mass, 95% by mass, 90% by mass, 85% by mass, 80% by mass, 75% by mass, 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, 15% by mass, 10% by mass, 9% by mass, 5% by mass, 3% by mass, 2% by mass, 1% by mass, etc. In one embodiment, the above content is preferably 1% to 100% by mass.
[0168] In one embodiment, the component (A-2A) may contain a structural unit derived from an unsaturated organic acid or a salt thereof. The unsaturated organic acid or a salt thereof may be used alone or in combination of two or more.
[0169] In the present disclosure, the unsaturated organic acid refers to a compound having an acidic group and a polymerizable unsaturated bond.
[0170] Examples of the unsaturated organic acid include unsaturated carboxylic acid, unsaturated sulfonic acid, unsaturated phosphoric acid, etc. Examples of the salt of the unsaturated organic acid include inorganic salts of unsaturated organic acid, etc. The inorganic salt of the unsaturated organic acid refers to a salt in which the cation part is a metal cation.
[0171] The upper and lower limits of the content of the structural unit derived from the unsaturated organic acid or its salt relative to 100 mol% of all structural units of the component (A-2A) are exemplified by 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 4 mol%, 2 mol%, 1 mol%, 0 mol%, etc. In one embodiment, the above content is preferably 0 mol% to 50 mol%.
[0172] The upper and lower limits of the content of the structural unit derived from the unsaturated organic acid or its salt relative to 100% by mass of all the structural units of the component (A-2A) are exemplified by 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, 15% by mass, 10% by mass, 5% by mass, 4% by mass, 2% by mass, 1% by mass, 0% by mass, etc. In one embodiment, the above content is preferably 0% to 70% by mass.
[0173] In one embodiment, the component (A-2A) may contain a structural unit derived from a (meth)acrylate (c). The (meth)acrylate may be used alone or in combination of two or more.
[0174] The upper and lower limits of the content of the structural unit derived from the (meth)acrylate (c) relative to 100 mol% of all structural units of the component (A-2A) are exemplified by 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 4 mol%, 2 mol%, 1 mol%, 0 mol%, etc. In one embodiment, the above content is preferably 0 mol% to 75 mol%.
[0175] The upper and lower limits of the content of the structural unit derived from the (meth)acrylate (c) relative to 100% by mass of all the structural units of the component (A-2A) are exemplified by 80% by mass, 75% by mass, 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, 15% by mass, 10% by mass, 5% by mass, 4% by mass, 2% by mass, 1% by mass, 0% by mass, etc. In one embodiment, the above content is preferably 0% to 80% by mass.
[0176] In one embodiment, the component (A-2A) may contain a structural unit derived from an α,β-unsaturated nitrile. The α,β-unsaturated nitrile may be used alone or in combination of two or more.
[0177] The upper and lower limits of the content of the structural unit derived from the α,β-unsaturated nitrile relative to 100 mol% of all structural units of the component (A-2A) are exemplified by 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 2 mol%, 1 mol%, 0 mol%, etc. In one embodiment, the above content is preferably 0 mol% to 45 mol%.
[0178] The upper and lower limits of the content of the structural unit derived from the α,β-unsaturated nitrile relative to 100% by mass of all structural units of the component (A-2A) are exemplified by 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, 15% by mass, 10% by mass, 5% by mass, 4% by mass, 2% by mass, 1% by mass, 0% by mass, etc. In one embodiment, the above content is preferably 0% to 40% by mass.
[0179] In one embodiment, the component (A-2A) may contain a structural unit derived from a trihydroxysilyl compound having a double bond and containing a vinyl group or a (meth)acryloyloxy group. The trihydroxysilyl compound having a double bond and containing a vinyl group or a (meth)acryloyloxy group may be used alone or in combination of two or more.
[0180] The upper and lower limits of the content of the structural unit derived from the trihydroxysilyl compound having a double bond containing a vinyl group or a (meth)acryloyloxy group relative to 100 mol% of all structural units of the component (A-2A) are exemplified by 0.8 mol%, 0.7 mol%, 0.5 mol%, 0.3 mol%, 0.2 mol%, 0.1 mol%, 0.09 mol%, 0.07 mol%, 0.05 mol%, 0 mol%, etc. In one embodiment, the above content is preferably 0 mol% to 0.8 mol%.
[0181] The upper and lower limits of the content of the structural unit derived from the trihydroxysilyl compound having a double bond containing a vinyl group or a (meth)acryloyloxy group relative to 100% by mass of all the structural units of the component (A-2A) are exemplified by 10% by mass, 9% by mass, 7% by mass, 5% by mass, 3% by mass, 1% by mass, 0.9% by mass, 0.5% by mass, 0.3% by mass, 0.1% by mass, 0.09% by mass, 0.05% by mass, 0.01% by mass, 0.009% by mass, 0.005% by mass, 0.001% by mass, 0% by mass, etc. In one embodiment, the above content is preferably 0% to 10% by mass.
[0182] In one embodiment, the component (A-2A) may contain a structural unit derived from a hydroxyl group-containing vinyl ether. The hydroxyl group-containing vinyl ether may be used alone or in combination of two or more.
[0183] The upper and lower limits of the content of the structural unit derived from the hydroxyl-containing vinyl ether relative to 100 mol% of all structural units of the component (A-2A) are exemplified by 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 4 mol%, 2 mol%, 1 mol%, 0 mol%, etc. In one embodiment, the above content is preferably 0 mol% to 80 mol%.
[0184] The upper and lower limits of the content of the structural unit derived from the hydroxyl-containing vinyl ether relative to 100% by mass of all the structural units of the component (A-2A) are exemplified by 85% by mass, 80% by mass, 75% by mass, 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, 15% by mass, 10% by mass, 5% by mass, 4% by mass, 2% by mass, 1% by mass, 0% by mass, etc. In one embodiment, the above content is preferably 0% to 85% by mass.
[0185] The ratio of the structural unit derived from any compound not belonging to the (meth)acrylamide group-containing compound (a), the unsaturated organic acid or its salt, the (meth)acrylate, the α,β-unsaturated nitrile, the trihydroxysilyl compound having a double bond containing a vinyl group or a (meth)acryloyloxy group, and the hydroxyl group-containing vinyl ether in all the structural units of the component (A-2A) is less than 10 mol%, less than 5 mol%, less than 1 mol%, less than 0.1 mol%, less than 0.01 mol%, or 0 mol% relative to 100 mol% of all the structural units of the component (A-2A); and less than 10 mass%, less than 5 mass%, less than 1 mass%, less than 0.5 mass%, less than 0.1 mass%, less than 0.01 mass%, or 0 mass% relative to 100 mass% of all the structural units of the component (A-2A).
[0186] The water-soluble poly(meth)acrylamide (A-2A) can be produced by the same conditions and method as for the component (A-1).
[0187] The upper and lower limits of the content of the neutralizer relative to 100 mol% of the acidic groups contained in the above-mentioned (A-2A) component are exemplified by 100 mol%, 95 mol%, 90 mol%, 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 0 mol%, etc. In one embodiment, the above-mentioned content is preferably 0 mol% to 100 mol%.
[0188] <Physical Properties of Water-Soluble Poly(Meth)acrylamide (A-2A)>
[0189] The upper limit and lower limit of the glass transition temperature of the water-soluble poly (meth) acrylamide (A-2A) are exemplified by 160°C, 155°C, 150°C, 145°C, 140°C, 135°C, 130°C, 125°C, 120°C, 115°C, 110°C, 105°C, 100°C, 95°C, 90°C, 85°C, 80°C, 75°C, 70°C, 65°C, 60°C, 55°C, 50°C, 45°C, 40°C, 35°C, 30°C, 25°C, 20°C, 15°C, 10°C, 5°C, 0°C, etc. In one embodiment, the glass transition temperature is preferably 0°C or higher, and more preferably 30°C or higher from the viewpoint of mechanical strength and heat resistance.
[0190] The upper and lower limits of the weight average molecular weight (Mw) of the water-soluble poly (meth) acrylamide (A-2A) are exemplified by 7 million, 6.5 million, 6 million, 5.5 million, 5 million, 4.5 million, 4 million, 3.5 million, 3 million, 2.5 million, 2 million, 1.5 million, 1 million, 950,000, 900,000, 850,000, 800,000, 750,000, 700,000, 650,000, 600,000, 550,000, 500,000, 450,000, 400,000, 350,000, 300,000, 250,000, 200,000, 150,000, 100,000, etc. In one embodiment, the weight average molecular weight (Mw) is preferably 100,000 to 7 million, more preferably 500,000 to 1 million.
[0191] The upper and lower limits of the weight average molecular weight ratio of the component (A-2A) to the component (A-1) [weight average molecular weight of (A-2A) / weight average molecular weight of (A-1)] are exemplified by 600, 550, 500, 450, 400, 350, 300, 250, 200, 150, 100, 90, 75, 50, 25, 10, 5, 2, 1, etc. In one embodiment, the above ratio is preferably 1 to 600.
[0192] The upper limit and lower limit of the number average molecular weight (Mn) of the water-soluble poly (meth) acrylamide (A-2A) are exemplified by 6 million, 5.5 million, 5 million, 4.5 million, 4 million, 3.5 million, 3 million, 2.5 million, 2 million, 1.5 million, 1 million, 950,000, 900,000, 850,000, 800,000, 750,000, 700,000, 650,000, 600,000, 550,000, 500,000, 450,000, 400,000, 300,000, 200,000, 150,000, 100,000, 50,000, 10,000, etc. In one embodiment, the number average molecular weight (Mn) of the water-soluble poly (meth) acrylamide (A-2A) is preferably 10,000 or more, more preferably 150,000 to 500,000.
[0193] The upper and lower limits of the ratio of the number average molecular weights of the components (A-2A) and (A-1) [number average molecular weight of (A-2A) / number average molecular weight of (A-1)] are exemplified by 100, 90, 75, 50, 25, 10, 5, 2, 1, 0.9, 0.5, 0.2, 0.1, 0.09, etc. In one embodiment, the ratio is preferably 0.09 to 100.
[0194] The upper and lower limits of the molecular weight distribution (Mw / Mn) of the water-soluble poly(meth)acrylamide (A-2A) are exemplified by 15, 14, 13, 11, 10, 9, 7.5, 5, 4, 3, 2.9, 2.5, 2, 1.5, 1.1, etc. In one embodiment, the molecular weight distribution (Mw / Mn) is preferably 1.1 to 15.
[0195] The upper and lower limits of the B-type viscosity of the slurry are exemplified by 100,000 mPa·s, 90,000 mPa·s, 80,000 mPa·s, 70,000 mPa·s, 60,000 mPa·s, 50,000 mPa·s, 40,000 mPa·s, 30,000 mPa·s, 20,000 mPa·s, 10,000 mPa·s, 9000 mPa·s, 8000 mPa·s, 7000 mPa·s, 6000 mPa·s, 5000 mPa·s, 4000 mPa·s, 3000 mPa·s, 2000 mPa·s, 1000 mPa·s, etc. In one embodiment, the B-type viscosity is preferably 1000 mPa·s to 1000,000 mPa·s.
[0196] The upper and lower limits of the pH of the slurry are exemplified by 9, 8, 7, 6.9, 6.5, 6, 5.9, 5.6, 5.5, 5.4, 5.2, 5.1, 5, etc. In one embodiment, from the viewpoint of solution stability, the pH is preferably pH 5 to 9, more preferably pH 5 to 7, and even more preferably pH 5 or more and less than 7.
[0197] The upper and lower limits of the content of the component (A-2) relative to 100 mass % of the slurry are exemplified by 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 9 mass %, 5 mass %, 4.5 mass %, 2 mass %, etc. In one embodiment, the content is preferably 2 mass % to 40 mass %.
[0198] The upper and lower limits of the content of the component (A-2A) relative to 100 mass % of the slurry are exemplified by 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 9 mass %, 5 mass %, 4.5 mass %, 2 mass %, 0 mass %, etc. In one embodiment, the content is preferably 0 mass % to 40 mass %.
[0199] The upper and lower limits of the mass ratio of the component (A-2A) to the component (A-1) in the slurry [mass of the component (A-2A) / mass of the component (A-1)] are exemplified by 19, 17, 15, 13, 11, 10, 9, 7, 5, 4, 3, 2.5, 2.3, etc. In one embodiment, the mass ratio is preferably 2.3 to 19.
[0200] <Compatibility of polymers obtained by mixing components (A-1) and (A-2A)>
[0201] From the viewpoint of electrode adhesion, the component (A-1) and the component (A-2A) are preferably miscible (without microphase separation).
[0202] As a method for determining the phase separation structure, a method of measuring the HAZE of a film is exemplified.
[0203] The film of the components (A-1) and (A-2A) is preferably obtained by premixing an aqueous solution containing the components (A-1) and (A-2A), applying the aqueous solution on a flat glass plate, and preparing a film in a circulating air dryer at 80° C. so as to have a thickness of 5 μm to 30 μm. The HAZE of the prepared film can be measured by a turbidimeter “NDH-2000 (manufactured by Nippon Denshoku Industries Co., Ltd.)”. The HAZE of the film is preferably 20% or less, particularly preferably 10% or less.
[0204] If the HAZE of the film is less than 20%, it means that the components (A-1) and (A-2A) are miscible. On the other hand, if the HAZE of the film is more than 20%, it means that the components (A-1) and (A-2A) are immiscible (microphase separation).
[0205] <Electrode active material (B-1): also referred to as (B-1) component>
[0206] Examples of the electrode active material include negative electrode active materials, positive electrode active materials, etc. The electrode active material may be used alone or in combination of two or more.
[0207] <Negative Electrode Active Material>
[0208] As long as it is a material that can reversibly absorb and release lithium, the negative electrode active material is not particularly limited and can be used alone or in combination of two or more. The negative electrode active material can be appropriately selected according to the type of the target power storage device. Examples of the negative electrode active material include carbon materials and silicon materials, oxides containing lithium atoms, lead compounds, tin compounds, arsenic compounds, antimony compounds, and aluminum compounds that are alloyed with lithium. Carbon materials and materials that are alloyed with lithium can significantly exert the effect of the present invention because of their large volume expansion rate when the battery is charged.
[0209] Examples of the above-mentioned carbon materials include graphite (also called black lead, examples include natural graphite, artificial graphite, etc.) as highly crystalline carbon, low-crystalline carbon (soft carbon, hard carbon), carbon black (ketjen black, acetylene black, channel black, lamp black, oil furnace black, thermal black, etc.), fullerenes, carbon nanotubes, carbon nanofibers, carbon nanohorns, carbon fibrils, mesophase carbon microbeads (MCMB), pitch-based carbon fibers, etc.
[0210] The silicon material includes SiC, SiO x C y (0<x≤3, 0<y≤5); Si3N4; Si2N2O; with SiO x Silicon oxide composites represented by (0<x≤2) (for example, materials described in Japanese Patent Publication No. 2004-185810 and Japanese Patent Publication No. 2005-259697); silicon materials described in Japanese Patent Publication No. 2004-185810, etc. In addition, silicon materials described in Japanese Patent Publication No. 5390336 and Japanese Patent Publication No. 5903761 can also be used.
[0211] The silicon oxide is preferably of the composition formula SiO x Silicon oxide represented by (0<x<2, preferably 0.1≤x≤1).
[0212] The silicon alloy is preferably an alloy of silicon and at least one transition metal, and the transition metal is selected from the group consisting of titanium, zirconium, nickel, copper, iron and molybdenum. These transition metal silicon alloys have high electronic conductivity and high strength, so they are preferred. The silicon alloy is more preferably a silicon-nickel alloy or a silicon-titanium alloy, and is particularly preferably a silicon-titanium alloy. Relative to 100 mol% of the metal element in the silicon alloy, the content of silicon in the silicon alloy is preferably 10 mol% or more, and more preferably 20 mol% to 70 mol%. In addition, the silicon material can be any of single crystal, polycrystalline and amorphous.
[0213] In addition, when a silicon material is used as the negative electrode active material, a negative electrode active material other than a silicon material may be used in combination. Examples of such negative electrode active materials include the above-mentioned carbon material; conductive polymers such as polyphenylene; X B Y O Z (A represents an alkali metal or a transition metal; B represents at least one transition metal selected from cobalt, nickel, aluminum, tin, manganese, etc.; O represents an oxygen atom; X, Y and Z are numbers in the range of 0.05<X<1.10, 0.85<Y<4.00, 1.5<Z<5.00, respectively) represented by a composite metal oxide; and other metal oxides, etc. When a silicon material is used as a negative electrode active material, the volume change accompanying the absorption and release of lithium is small, so it is preferably used in combination with a carbon material.
[0214] Examples of the above-mentioned oxides containing lithium atoms include ternary nickel cobalt manganese oxide, lithium-manganese composite oxides (LiMn2O4, etc.), lithium-nickel composite oxides (LiNiO2, etc.), lithium-cobalt composite oxides (LiCoO2, etc.), lithium-iron composite oxides (LiFeO2, etc.), lithium-nickel-manganese composite oxides (LiNi 0.5 Mn 0.5 O2, etc.), lithium-nickel-cobalt composite oxide (LiNi 0.8 Co 0.2 O2, etc.), lithium-transition metal phosphate compounds (LiFePO4, etc.) and lithium-transition metal sulfate compounds (Li x Fe2(SO4)3), lithium-titanium composite oxide (lithium titanate: Li4Ti5O 12 ) and other lithium-transition metal composite oxides and other previously known negative electrode active materials.
[0215] The shape of the negative electrode active material is not particularly limited, and can be any shape such as microparticles and thin films, preferably microparticles. The average particle size of the negative electrode active material is not particularly limited, and its upper and lower limits are exemplified by 50μm, 45μm, 40μm, 35μm, 30μm, 25μm, 20μm, 15μm, 10μm, 5μm, 4μm, 3μm, 2.9μm, 2μm, 1μm, 0.5μm, 0.1μm, etc. More specifically, in one embodiment, from the viewpoint of uniformly forming a thin coating film, if it is above 0.1μm, the operability is good, and if it is below 50μm, it is easy to coat the electrode, so the average particle size of the negative electrode active material is preferably 0.1μm to 50μm, more preferably 0.1μm to 45μm, further preferably 1μm to 10μm, and particularly preferably 5μm.
[0216] In the present disclosure, "particle size" refers to the maximum distance between any two points on the contour line of a particle (the same below). In addition, in the present disclosure, unless otherwise specified, "average particle size" refers to a value calculated as the average value of the particle sizes of particles observed in several to dozens of fields of view using an observation method such as a scanning electron microscope (SEM) and a transmission electron microscope (TEM) (the same below).
[0217] In order to significantly exert the effects of the present invention, the carbon material and / or the material alloying with lithium contained in the negative electrode active material is preferably 50 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and particularly preferably 100 mass %.
[0218] In one embodiment, from the viewpoint of increasing the battery capacity of the lithium ion battery, the content of silicon or silicon oxide covered by the carbon layer in the negative electrode active material is preferably 5% by mass or more (e.g., 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 100% by mass) relative to 100% by mass of the negative electrode active material.
[0219] <Positive Electrode Active Material>
[0220] Examples of positive electrode active materials include inorganic positive electrode active materials and organic positive electrode active materials. Examples of inorganic positive electrode active materials include transition metal oxides, composite oxides of lithium and transition metals, transition metal sulfides, etc. Examples of the above transition metals include Fe, Co, Ni, Mn, Al, etc. Examples of inorganic compounds used in positive electrode active materials include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiFePO4, LiNi 1 / 2 Mn 3 / 2 O4、LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li[Li 0.1 Al 0.1 Mn 1.8 ]O4, LiFeVO4 and other lithium-containing composite metal oxides; TiS2, TiS3, amorphous MoS2 and other transition metal sulfides; Cu2V2O3, amorphous V2O-P2O5, MoO3, V2O5, V6O 13Transition metal oxides, etc. These compounds may also be compounds with partial element substitution. Examples of organic positive electrode active materials include conductive polymers such as polyacetylene and polyparaphenylene. By allowing the presence of a carbon source during reduction calcination, iron-based oxides with poor conductivity may also be used as electrode active materials covered with carbon materials. In addition, these compounds may also be compounds with partial element substitution. Among them, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiFePO4, LiNi 1 / 2 Mn 3 / 2 O4、LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li[Li 0.1 Al 0.1 Mn 1.8 ]O4.
[0221] The upper and lower limits of the content of the electrode active material (B-1) relative to 100 mass % of the slurry are exemplified as 65 mass %, 60 mass %, 55 mass %, 50 mass %, 45 mass %, 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, etc. In one embodiment, the content is preferably 20 mass % to 65 mass %.
[0222] <Conductive carbon material (B-2): also referred to as (B-2) component>
[0223] Examples of the conductive carbon material include fibrous carbon and carbon black. The conductive carbon material may be used alone or in combination of two or more. The conductive carbon material may be used as a conductive auxiliary carbon material.
[0224] Examples of the fibrous carbon include vapor grown carbon fibers (VGCF), carbon nanotubes (CNTs), and carbon nanofibers (CNFs).
[0225] Examples of carbon black include graphite particles, acetylene black, Ketjen black, furnace black, and the like.
[0226] Relative to 100 mass % of the slurry, the upper and lower limits of the content of the conductive carbon material (B-2) are exemplified by 5 mass %, 4 mass %, 3 mass %, 2 mass %, 1 mass %, 0.9 mass %, 0.7 mass %, 0.5 mass %, 0.3 mass %, 0.1 mass %, 0.09 mass %, 0.07 mass %, 0.05 mass %, 0.03 mass %, 0.01 mass %, etc. In one embodiment, the above content is preferably 0.01 mass % to 5 mass %.
[0227] The upper and lower limits of the water content relative to 100% by mass of the slurry are exemplified by 79% by mass, 75% by mass, 70% by mass, 65% by mass, 60% by mass, 55% by mass, 50% by mass, 45% by mass, 40% by mass, 35% by mass, 30% by mass, 25% by mass, 20% by mass, etc. In one embodiment, the content is preferably 20% to 79% by mass.
[0228] <Slurry Viscosity Adjusting Solvent>
[0229] In one embodiment, the slurry may contain a slurry viscosity adjusting solvent. The slurry viscosity adjusting solvent may be any known substance without particular limitation, and may be used alone or in combination of two or more. Examples of the solvent include ether solvents, ketone solvents, alcohol solvents, amide solvents, water, and the like.
[0230] The upper and lower limits of the content of the slurry viscosity adjusting solvent relative to 100 mass % of the slurry are exemplified by 10 mass %, 9 mass %, 7 mass %, 5 mass %, 3 mass %, 2 mass %, 1 mass %, 0 mass %, etc. In one embodiment, the content is preferably 0 mass % to 10 mass %.
[0231] <Hydroxysilane compounds>
[0232] In one embodiment, the slurry may include a hydroxysilane compound. In the present disclosure, a hydroxysilane compound refers to a compound having a structure in which a hydroxyl group (-OH) is directly bonded to a silicon atom, a trihydroxysilane compound refers to a compound having a trihydroxysilane group (-Si(OH)3), and a tetrahydroxysilane compound refers to a compound represented by Si(OH)4.
[0233] In one embodiment, the trihydroxysilyl compound is a compound represented by the following general formula:
[0234] RSi(OH)3
[0235] (In the formula, R represents a substituted or unsubstituted alkyl group, vinyl group or (meth)acryloyloxy group; examples of the substituents include amino group, mercapto group, glycidyloxy group, (meth)acryloyloxy group, epoxy group and the like.)
[0236] The hydroxysilane compound is preferably prepared by hydrolyzing a silane coupling agent or a tetraalkoxysilane. The hydroxysilane compound may also be partially polycondensed within a range where it does not lose its water solubility. The silane coupling agent may be a silane coupling agent commonly used in the technical field to which the present invention belongs.
[0237] The silane coupling agent is not particularly limited. The hydroxysilane compound produced from the silane coupling agent may be used alone or in combination of two or more. In one embodiment, the hydroxysilane compound includes trihydroxysilylpropylamine.
[0238] Examples of trialkoxysilane include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2 (aminoethyl) 3-aminopropyltrimethoxysilane, N-2 (aminoethyl) 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, and tetrahydroxysilane.
[0239] Moreover, as a tetraalkoxysilane, tetramethoxysilane, a tetramethoxysilane oligomer, tetraethoxysilane, a tetraethoxysilane oligomer, etc. are illustrated.
[0240] The upper and lower limits of the content of the hydroxysilane compound relative to 100 mass % of the slurry are exemplified by 15 mass %, 13 mass %, 10 mass %, 9 mass %, 7 mass %, 5 mass %, 3 mass %, 2 mass %, 1 mass %, 0.9 mass %, 0.7 mass %, 0.5 mass %, 0.3 mass %, 0.1 mass %, 0.09 mass %, 0.07 mass %, 0.05 mass %, 0.04 mass %, 0.02 mass %, 0.01 mass %, 0 mass %, etc. In one embodiment, the content is preferably 0 mass % to 15 mass %.
[0241] <Crosslinking agent>
[0242] In one embodiment, the slurry may include a cross-linking agent. The cross-linking agent may be used alone or in combination of two or more.
[0243] Examples of the crosslinking agent include water-soluble polyols, formaldehyde, glyoxal, hexamethylenetetramine, urea-formaldehyde resins, methylolmelamine resins, carbodiimide, polyfunctional epoxides, oxazoline, polyfunctional hydrazides, isocyanates, melamine, urea, and mixtures thereof.
[0244] The water-soluble polyol is a water-soluble alcohol among alcohols having two or more hydroxyl groups.
[0245] Examples of the water-soluble polyol include methylene glycol, ethylene glycol, propylene glycol, isoprene glycol, 1,3-butylene glycol, 1,4-butylene glycol, diethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, glycerol, diglycerol, and polyglycerol.
[0246] Among them, water-soluble polyols represented by the general formula (B1), particularly polyethylene glycol (n=1 to 6), are preferred:
[0247] [Chemistry 4]
[0248]
[0249] (In the formula, R is a methylene group, an ethylene group or a propylene group, and n is an integer greater than 1.)
[0250] The upper and lower limits of the content of the crosslinking agent relative to 100 mass % of the slurry are exemplified by 20 mass %, 19 mass %, 17 mass %, 15 mass %, 13 mass %, 10 mass %, 9 mass %, 7 mass %, 5 mass %, 3 mass %, 2 mass %, 1 mass %, 0.9 mass %, 0.7 mass %, 0.5 mass %, 0.3 mass %, 0.1 mass %, 0.09 mass %, 0.05 mass %, 0.03 mass %, 0.01 mass %, 0.009 mass %, 0.005 mass %, 0.003 mass %, 0.001 mass %, 0 mass %, etc. In one embodiment, the content is preferably 0 mass % to 20 mass %.
[0251] <Thickener>
[0252] In one embodiment, the slurry may contain a thickener. The thickener may be used alone or in combination of two or more.
[0253] Examples of thickeners include cellulose polymers such as carboxymethyl cellulose, methyl cellulose, hydroxypropyl cellulose, and their ammonium salts and alkali metal salts; (modified) poly(meth)acrylic acid and their ammonium salts and alkali metal salts; (modified) polyvinyl alcohol, copolymers of acrylic acid or acrylic acid salts and vinyl alcohol, polyvinyl alcohols such as copolymers of maleic anhydride or maleic acid or fumaric acid and vinyl alcohol; polyethylene glycol, polyethylene oxide, polyvinyl pyrrolidone, modified polyacrylic acid, oxidized starch, starch phosphate, casein, various modified starches, acrylonitrile-butadiene copolymer hydrogenates, etc.
[0254] The upper and lower limits of the content of the thickener relative to 100 mass% of the slurry are exemplified by 20 mass%, 19 mass%, 17 mass%, 15 mass%, 13 mass%, 10 mass%, 9 mass%, 7 mass%, 5 mass%, 3 mass%, 2 mass%, 1 mass%, 0.9 mass%, 0.7 mass%, 0.5 mass%, 0.3 mass%, 0.1 mass%, 0.09 mass%, 0.05 mass%, 0.03 mass%, 0.01 mass%, 0.009 mass%, 0.005 mass%, 0.003 mass%, 0.001 mass%, 0 mass%, etc. In one embodiment, the content is preferably 0 mass% to 20 mass%.
[0255] <Additives>
[0256] The above-mentioned slurry may contain as an additive any reagent that is not a conductive carbon material dispersant for lithium-ion batteries, a water-soluble poly(methyl)acrylamide (A-1), a polymer (A-2), an electrode active substance (B-1), a conductive carbon material (B-2), water, a slurry viscosity adjusting solvent, a hydroxysilane compound, a crosslinking agent, and a thickening agent.
[0257] Examples of the content of the additives relative to 100 mass % of the slurry include 0 mass % to 5 mass %, less than 1 mass %, less than 0.1 mass %, less than 0.01 mass %, and 0 mass %.
[0258] Examples of the additive include a dispersant other than the above-mentioned conductive carbon material dispersant for lithium ion batteries, a leveling agent, an antioxidant, and the like.
[0259] Examples of the dispersant other than the above-mentioned conductive carbon material dispersant for lithium ion batteries include anionic dispersants, cationic dispersants, nonionic dispersants, and polymer dispersants.
[0260] Examples of the leveling agent include surfactants such as alkyl surfactants, silicon surfactants, fluorine surfactants, and metal surfactants. By using a surfactant, craters generated during coating can be prevented, and the smoothness of the slurry layer (coating) can be improved.
[0261] Examples of the antioxidant include phenol compounds, hydroquinone compounds, organic phosphine compounds, sulfur compounds, phenylenediamine compounds, polymer phenol compounds, etc. The polymer phenol compound is a polymer having a phenol structure in the molecule. The weight average molecular weight of the polymer phenol compound is preferably 200 to 1000, more preferably 600 to 700.
[0262] Examples of additives other than the above-mentioned additives include at least one compound selected from the group consisting of unsaturated carboxylic acids, unsaturated amides, and salts thereof.
[0263] The method for producing the slurry includes, for example, a method of mixing a conductive carbon material dispersant for lithium ion batteries, a polymer (A-2), an electrode active material (B-1), a conductive carbon material (B-2) and water; and a method of mixing a water-soluble poly(meth)acrylamide (A-1), a polymer (A-2), an electrode active material (B-1), a conductive carbon material (B-2) and water. In addition, in the above method, the mixing order is not particularly limited.
[0264] Examples of the mixing means for the slurry include a ball mill, a sand mill, a pigment disperser, a pounder, an ultrasonic disperser, a homogenizer, a planetary mixer, and a Hobart mixer.
[0265] The slurry for lithium ion battery electrodes can be used as a slurry for lithium ion battery negative electrodes or a slurry for lithium ion battery positive electrodes.
[0266] [Electrodes for lithium-ion batteries]
[0267] The present disclosure provides a lithium ion battery electrode obtained by applying the above-mentioned slurry for lithium ion battery electrodes on a current collector and drying and solidifying the slurry. The above-mentioned electrode has a solidified product of the above-mentioned slurry for lithium ion battery electrodes on the current collector.
[0268] The coating means is not particularly limited, and examples thereof include conventionally known coating devices such as a comma coater, a gravure coater, a micro gravure coater, a die coater, and a bar coater.
[0269] The drying means is not particularly limited, and the temperature is preferably about 80°C to 200°C, more preferably about 90°C to 180°C; the atmosphere may be dry air or an inert atmosphere. In addition, from the viewpoint of improving electrode adhesion, a drying means using far infrared rays may also be used.
[0270] The thickness of the electrode (cured coating film) is not particularly limited, but is preferably about 5 μm to 300 μm, more preferably about 10 μm to 250 μm. Within the above range, a sufficient Li absorption-release function for a high-density current value can be easily obtained.
[0271] The current collector may be any of various known current collectors without particular limitation. The material of the current collector is not particularly limited, and examples thereof include metal materials such as copper, iron, aluminum, nickel, stainless steel, and nickel-plated steel; and carbon materials such as carbon cloth and carbon paper. The shape of the current collector is also not particularly limited, and in the case of metal materials, examples thereof include metal foil, metal cylinder, metal coil, and metal plate; and in the case of carbon materials, examples thereof include carbon plate, carbon film, and carbon cylinder. Among them, in the case of using the electrode active material for the negative electrode, copper foil is preferably used as the current collector because it is currently used in industrial products.
[0272] The above-mentioned electrode for lithium ion batteries can be used as a negative electrode for lithium ion batteries or a positive electrode for lithium ion batteries.
[0273] [Lithium-ion battery]
[0274] The present disclosure provides a lithium ion battery including the above-mentioned lithium ion battery electrode. In one embodiment, the above-mentioned battery includes an electrolyte, a separator, a positive electrode, etc. These are not particularly limited.
[0275] Examples of the electrolyte include a non-aqueous electrolyte solution in which a supporting electrolyte is dissolved in a non-aqueous solvent. The non-aqueous electrolyte solution may contain a film-forming agent.
[0276] The non-aqueous solvent may be any known non-aqueous solvent without particular limitation, and may be used alone or in combination of two or more. Examples of the non-aqueous solvent include chain carbonate solvents such as diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate; cyclic carbonate solvents such as ethylene carbonate, propylene carbonate, and butylene carbonate; chain ether solvents such as 1,2-dimethoxyethane; cyclic ether solvents such as tetrahydrofuran, 2-methyltetrahydrofuran, sulfolane, and 1,3-dioxolane; chain ester solvents such as methyl formate, methyl acetate, and methyl propionate; cyclic ester solvents such as γ-butyrolactone and γ-valerolactone; acetonitrile, etc. Among them, a combination of mixed solvents containing cyclic carbonates and chain carbonates is preferred.
[0277] A lithium salt may be used as the supporting electrolyte. Various known lithium salts may be used as the lithium salt without particular limitation, and may be used alone or in combination of two or more. Examples of the supporting electrolyte include LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. Among them, LiPF6, LiClO4, and CF3SO3Li, which are easily soluble in a solvent and show a high degree of dissociation, are preferred. The higher the degree of dissociation of the supporting electrolyte used, the higher the lithium ion conductivity, and therefore, the lithium ion conductivity can be adjusted by the type of supporting electrolyte.
[0278] The film-forming agent can use various known film-forming agents without particular limitation, and can be used alone or in combination of two or more. Examples of the film-forming agent include carbonate compounds such as vinylene carbonate, vinyl ethylene carbonate, vinyl ethyl carbonate, methyl phenyl carbonate, fluoroethylene carbonate, and difluoroethylene carbonate; cyclosulfides such as ethylene sulfide and propane sulfide; sultone compounds such as 1,3-propane sultone and 1,4-butane sultone; anhydrides such as maleic anhydride and succinic anhydride. The content of the film-forming agent in the electrolyte is not particularly limited, and is preferably in the order of less than 10% by mass, less than 8% by mass, less than 5% by mass, and less than 2% by mass. By making the content less than 10% by mass, the advantage of the film-forming agent is that it is easy to achieve the suppression of the initial irreversible capacity, the improvement of low temperature characteristics and rate characteristics, etc.
[0279] The separator is an article between the positive electrode and the negative electrode, and is used to prevent short circuits between the electrodes. Specifically, porous separators such as porous films and nonwoven fabrics can be preferably used, and these separators are impregnated with the above-mentioned non-aqueous electrolyte and used. The material of the separator can use polyolefins such as polyethylene and polypropylene, polyether sulfone, etc., preferably polyolefins.
[0280] When a lithium ion battery is manufactured using a negative electrode manufactured using the above lithium ion battery electrode slurry as a negative electrode and a positive electrode manufactured without using the above lithium ion battery electrode slurry as a positive electrode, the positive electrode can be any known positive electrode without particular limitation.
[0281] The positive electrode may be any known positive electrode without particular limitation. Examples of the positive electrode include a positive electrode obtained by mixing a positive electrode active material, a conductive aid, a positive electrode binder, and an organic solvent to prepare a slurry, coating the prepared slurry on a positive electrode collector, drying, and pressing the slurry.
[0282] The positive electrode binder can be used without particular limitation, and various known positive electrode binders can be used alone or in combination of two or more. Examples of the positive electrode binder include fluorine resins (polyvinylidene fluoride, polytetrafluoroethylene, etc.), polyolefins (polyethylene, polypropylene, etc.), polymers with unsaturated bonds (styrene-butadiene rubber, isoprene rubber, butadiene rubber, etc.), acrylic polymers (acrylic copolymers, methacrylic copolymers, etc.), etc.
[0283] Examples of the positive electrode current collector include aluminum foil and stainless steel foil.
[0284] The form of the lithium-ion battery is not particularly limited. Examples of the form of the lithium-ion battery include a cylindrical type in which the electrode sheet and the separator are spirally shaped; a cylindrical type in which the plate electrode and the separator are combined with an inside-out structure; and a button type in which the plate electrode and the separator are stacked. In addition, by placing these batteries in any outer packaging box, they can be used in any shape such as a button type, a cylindrical type, a square type, etc.
[0285] The manufacturing method of the lithium ion battery is not particularly limited, and can be assembled by taking appropriate procedures according to the structure of the battery. The manufacturing method of the lithium ion battery is exemplified by the method described in Japanese Patent Publication No. 2013-089437. The battery can be manufactured by installing a negative electrode on an outer packaging box, setting an electrolyte and a diaphragm thereon, and then installing a positive electrode so that the positive electrode and the negative electrode are opposite to each other, and fixing them with a gasket and a sealing plate.
[0286] Example
[0287] The present invention is described in detail below by way of examples and comparative examples. However, the description in the above preferred embodiments and the following examples are provided only for the purpose of illustration and are not provided for the purpose of limiting the present invention. Therefore, the scope of the present invention is not limited to the embodiments or examples specifically described in this specification, but is limited only by the scope of the claims. In addition, in each example and comparative example, unless otherwise specified, the numerical values of parts, % and the like are based on mass.
[0288] Production of water-soluble poly(meth)acrylamide (A-1)
[0289] Example 1-1
[0290] 387 g of ion-exchanged water was added to a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet pipe, and the oxygen in the reaction system was removed by nitrogen gas, and then the temperature was raised to 80°C.
[0291] 300 g (2.11 mol) of 50% acrylamide aqueous solution, 581 g (1.27 mol) of 50% sodium acrylamide tert-butyl sulfonate aqueous solution, 0.55 g (0.0035 mol) of sodium methallyl sulfonate, 12.7 g (0.14 mol) of 80% acrylic acid, 8 g of ion exchange water, and 21 g of isopropyl alcohol were placed in a 2 L beaker and stirred for 30 minutes to obtain a uniform solution A.
[0292] 4.1 g of 2,2′-azobis-2-amidinopropane dihydrochloride (manufactured by Nihon Ho Chemical Co., Ltd., product name “NC-32”) and 199 g of ion-exchanged water were added to a 300 mL beaker, and stirred for 30 minutes to obtain a uniform solution B.
[0293] Solution A and solution B were simultaneously added dropwise to the reaction apparatus over 3 hours to perform a polymerization reaction. Then, 5.8 g (0.07 mol) of a 48% sodium hydroxide aqueous solution was added as a neutralizer and stirred to obtain a conductive carbon material dispersant for lithium ion batteries containing water-soluble poly(meth)acrylamide (A-1) with a solid content concentration of 30% by mass. The dispersant had a B-type viscosity of 350 mPa·s at 25°C and a pH of 5.2.
[0294] Examples 1 other than Example 1-1 were carried out in the same manner as Example 1-1 except that the composition in Example 1-1 was changed as shown in the following table.
[0295] Comparative Example 1-1
[0296] In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, 1310 g of ion exchange water, 80.0 g (0.56 mol) of a 50% acrylamide aqueous solution, 5.8 g (0.06 mol) of 80% acrylic acid, 266.0 g (0.58 mol) of a 50% sodium acrylamide tert-butylsulfonate aqueous solution, 46.8 g (0.40 mol) of 2-hydroxyethyl acrylate, and 0.25 g (0.0016 mol) of sodium methallylsulfonate were added, and the oxygen in the reaction system was removed by nitrogen gas, and the temperature was raised to 50°C. 2.0 g of 2,2′-azobis-2-amidinopropane dihydrochloride (manufactured by Nihon Kagaku Co., Ltd., product name "NC-32") and 20 g of ion exchange water were added thereto, and the temperature was raised to 80°C for 3 hours to react. A dispersant containing water-soluble poly(meth)acrylamide having a solid content concentration of 13% was obtained. The B-type viscosity of the dispersant at 25° C. was 730 mPa·s, and the pH was 5.1.
[0297] Comparative Example 1 other than the above-mentioned Comparative Example 1-1 was carried out in the same manner as in Example 1-1 except that the composition was changed as shown in the following table.
[0298] [Table 1]
[0299]
[0300] AM: Acrylamide (manufactured by Mitsubishi Chemical Co., Ltd., “50% Acrylamide”)
[0301] DMAA: N,N-dimethylacrylamide (manufactured by KJ Chemicolor Co., Ltd., “DMAA”)
[0302] · ATBSNa: Sodium tert-butyl acrylate sulfonate (manufactured by Toagosei Co., Ltd., "ATBS-Na")
[0303] · SMAS: Sodium methallyl sulfonate
[0304] · HEA: 2-Hydroxyethyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., "HEA")
[0305] · HEMA: 2-Hydroxyethyl methacrylate
[0306] · AN: Acrylonitrile (manufactured by Mitsubishi Chemical Corporation, "acrylonitrile")
[0307] · AA: Acrylic acid (manufactured by Osaka Organic Chemical Industry Co., Ltd., "80% acrylic acid")
[0308] · NaOH: Sodium hydroxide (manufactured by Kanto Chemical Co., Inc., "48% sodium hydroxide solution")
[0309] <B-type viscosity>
[0310] The viscosity of each dispersant was measured at 25 °C using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd., product name "B-type viscometer TVB-10M") under the following conditions.
[0311] When the viscosity is less than 500 mPa·s: Use No. 2 rotor, rotation speed 60 rpm.
[0312] When the viscosity is 500 mPa·s to less than 1,000 mPa·s: Use No. 3 rotor, rotation speed 30 rpm.
[0313] When the viscosity is 1,000 mPa·s to less than 10,000 mPa·s: Use No. 3 rotor, rotation speed 12 rpm.
[0314] When the viscosity is 10,000 mPa·s or more: Use No. 3 rotor, rotation speed 6 rpm.
[0315] <Weight average molecular weight>
[0316] The weight average molecular weight was determined as the polyacrylic acid conversion value measured by gel permeation chromatography (GPC) in a 0.2 M phosphate buffer / acetonitrile solution (90 / 10, pH 8.0). The GPC apparatus used was HLC-8220 (manufactured by Tosoh Corporation), and the column used was SB-806M-HQ (manufactured by SHODEX).
[0317] <ph>
[0318] The pH of each dispersant was measured at 25° C. using a glass electrode pH meter (product name: “Handy pH Meter D-52”, manufactured by Horiba, Ltd.).
[0319] (A-2) Production of ingredients
[0320] Production Example 1
[0321] In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, 1007 g of ion exchange water, 100 g (0.70 mol) of a 50% acrylamide aqueous solution, 63.8 g (0.70 mol) of 80% acrylic acid, 69.8 g (0.60 mol) of 2-hydroxyethyl acrylate, and 0.32 g (0.0020 mol) of sodium methallyl sulfonate were added, and the oxygen in the reaction system was removed by nitrogen gas, and the temperature was raised to 55°C. 1.6 g of 2,2′-azobis-2-amidinopropane dihydrochloride (manufactured by Nihon Kagaku Co., Ltd., product name "NC-32") and 16 g of ion exchange water were added thereto, and the temperature was raised to 80°C for 3 hours to react. Then, 52.7 g (0.63 mol) of a 48% sodium hydroxide aqueous solution was added as a neutralizing agent and stirred, and ion exchange water was added so that the solid content concentration was 13% by mass to obtain an aqueous solution containing water-soluble poly (meth) acrylamide. The B-type viscosity of the aqueous solution at 25° C. was 3000 mPa·s, and the pH was 6.0.
[0322] Production Examples other than Production Example 1 were carried out in the same manner as Production Example 1 except that the composition in Production Example 1 was changed as shown in the following table.
[0323] [Table 2]
[0324]
[0325] ※The amount of the neutralizing agent is a value based on 100 mol % of the acidic group (carboxyl group) contained in the component (A-2).
[0326] Conductive carbon material paste evaluation, resin swelling ratio and electrolyte resistance evaluation
[0327] Example 2-1
[0328] Using a commercially available rotation-revolution mixer (product name: "Awatori Ren Tarou", manufactured by Shinchi Co., Ltd.), in a container dedicated to this mixer, 40 parts by mass of the water-soluble poly(meth)acrylamide (A-1) obtained in Example 1-1 in terms of solid components and 60 parts by mass of a conductive carbon material (manufactured by Imerys C.C. Japan Co., Ltd., "Super C65") were put in. Ion-exchanged water was added thereto to make the solid component concentration 13.5%, and this container was set in the above rotation-revolution mixer. Then, after kneading at 2000 rpm for 10 minutes, a conductive carbon material paste was obtained.
[0329] For Example 2 and Comparative Examples other than Example 2-1, a conductive carbon material paste was prepared in the same manner as in Example 2-1 except that the composition in the above Example 2-1 was changed as shown in the following table.
[0330] <Initial dispersion test of conductive carbon material paste>
[0331] Using a commercially available laser diffraction / scattering particle size distribution measuring device (product name: "LA-960", manufactured by HORIBA), the median diameter (D50) of the conductive carbon material paste obtained in Example 2-1 was measured. The higher the measured value of the median diameter, the worse the initial dispersibility of the conductive aid and the more it aggregates. The lower the value of the median diameter, the better the initial dispersibility of the conductive aid.
[0332] The numerical value of the median diameter (D50) was evaluated according to the following evaluation criteria.
[0333] A: Less than 3.0 μm
[0334] B: 3.0 μm or more
[0335] <Dispersion stability test of conductive carbon material paste>
[0336] After allowing the conductive carbon material paste obtained in Example 2-1 to stand at room temperature for 24 hours, the median diameter (D50) was measured. The greater the change in the measured value of the median diameter, the worse the dispersion stability of the conductive aid and the more it aggregates. The smaller the change in the value of the median diameter, the better the dispersion stability of the conductive aid. The change rate of the median diameter (D50) was calculated by the following formula and evaluated according to the following evaluation criteria.
[0337] Change rate (%) = [((D50 of the conductive carbon material paste after 24 hours) - (D50 of the conductive carbon material paste after the initial dispersion test)) / (D50 of the conductive carbon material paste after the initial dispersion test)] × 100
[0338] A: Less than ±20%
[0339] B: ±20% or more
[0340] <Evaluation of Electrolyte Swelling Ratio and Electrolyte Resistance of Water-soluble Poly(meth)acrylamide (A-1)>
[0341] The water-soluble poly(meth)acrylamide (A-1) obtained in Example 1-1 is poured into a culture dish (シャーレ) and dried in a circulating air dryer at 105°C for 3 hours to produce a solid resin. Then, the mass α of the obtained solid resin is measured. Next, the obtained solid resin is immersed in 50 mL of dimethyl carbonate solvent and stored at 25°C for 48 hours. Then, the immersed solid resin is taken out from the dimethyl carbonate solvent, the dimethyl carbonate attached to the surface of the solid resin is fully wiped off, and the mass β is measured. Then, the mass γ of the wiped solid resin after it is dried in a circulating air dryer at 105°C for 1 hour is measured.
[0342] The measured mass β and mass γ are used to calculate the electrolyte swelling ratio of the polymer = (β / γ) x 100 (%). The lower the electrolyte swelling ratio (closer to 100%), the lower the electrolyte swelling property of the polymer.
[0343] A: The electrolyte swelling rate is less than 110%
[0344] B: The electrolyte swelling ratio is 110% or more and less than 120%
[0345] C: The electrolyte swelling rate is more than 120%
[0346] Similarly, using the measured mass α and mass γ, the electrolyte resistance of the polymer is calculated as (γ / α)×100(%). The lower the electrolyte resistance (closer to 100%), the lower the solubility of the polymer in the electrolyte.
[0347] A: Electrolyte resistance rate is more than 95%
[0348] B: Electrolyte resistance rate is less than 95%
[0349] [Table 3]
[0350]
[0351] CMC: Carboxymethyl cellulose
[0352] PVP: Polyvinylpyrrolidone
[0353] Manufacturing of slurry for lithium-ion battery electrodes and battery production and evaluation
[0354] <Manufacturing of slurry for lithium-ion battery electrodes>
[0355] Example 3-1
[0356] The slurry was prepared using a commercially available homodisperser ("Homodesper 2.5 Model" manufactured by PRIMIX Corporation). In a mayonnaise bottle as a container, 0.5 parts by mass of the water-soluble poly(meth)acrylamide (A-1) obtained in Example 1-1, 4.5 parts by mass of the binder (A-2) obtained in Production Example 1, 80 parts by mass of graphite having a D50 (median particle size) of 20 μm, 20 parts by mass of silicon monoxide particles having a D50 (median particle size) of 5 μm ("CC powder", manufactured by Osaka Chitanium Technology Co., Ltd.), and 1 part by mass of a conductive carbon material ("Super C65", manufactured by Imelis Diapan Co., Ltd.) were mixed. Ion exchange water was added thereto so that the solid content concentration was 47%, and the container was placed in the above-mentioned homogeneous disperser. Then, the mixture was kneaded at 2000 rpm for 30 minutes and then degassed for 1 minute using a rotary and revolving mixer ("Awato Ri Rentaro" manufactured by Shinki Co., Ltd.) to obtain a slurry for lithium ion battery electrodes.
[0357] For Example 3 and Comparative Examples other than Example 3-1, the same procedures as in Example 3-1 were carried out except that the composition in Example 3-1 was changed as shown in the following table.
[0358] Example 4-1
[0359] A slurry was prepared using a commercially available homodisperser ("Homodisperser 2.5 Model" manufactured by PRIMIX Co., Ltd.). In a mayonnaise bottle as a container, 0.5 parts by mass of the water-soluble poly(meth)acrylamide (A-1) obtained in Example 1-2, 4.5 parts by mass of the binder (A-2) obtained in Production Example 3, and 100 parts by mass of lithium nickel manganese oxide (Li[Ni 1 / 2 Mn 3 / 2 ]O4, median particle size D50: 3.7μm) and 1 mass part of conductive carbon material (manufactured by Imelis Digi-Jiapan Co., Ltd., "Super C65"). Ion exchange water is added thereto so that the solid content concentration is 50%, and the container is set in the above-mentioned homogeneous disperser. Then, kneading is carried out at 2000rpm for 30 minutes. Then, a rotary revolution mixer (manufactured by Shinki Co., Ltd., "Awato Ri Rentaro") is used for 1 minute to degas, and a slurry for lithium ion battery electrodes is obtained.
[0360] Regarding Comparative Example 4-1, except that the composition in the above-mentioned Example 4-1 was changed as shown in Table 4, a slurry was prepared in the same manner as in Example 4-1.
[0361] <Storage stability test of slurry for lithium-ion battery electrodes>
[0362] The storage stability of the slurry for lithium ion battery electrodes was evaluated as follows.
[0363] The viscosity of the lithium ion battery electrode slurry (unit: mPa·s) was measured with a B-type viscometer and then stored in an oven heated to 40° C. for 3 days. After storage, the viscosity was measured again with a B-type viscometer, and the viscosity change was calculated using the following formula and evaluated according to the following evaluation criteria.
[0364] Viscosity change (%) = {(viscosity of electrode slurry after storage) / (viscosity of electrode slurry before storage)}×100
[0365] A: Less than 110%
[0366] B: 110% or more and less than 120%
[0367] C: 120% or more
[0368] <Manufacturing of negative electrode>
[0369] The slurry was evenly applied to the surface of the collector composed of copper foil by a doctor blade method in a manner that the film thickness after drying was 170 μm, dried at 150°C for 30 minutes, and then heated at 150°C / vacuum for 120 minutes. Then, the film (electrode active material layer) was pressed by a roller press to a density of 1.5 g / cm 3 , thus obtaining an electrode.
[0370] <Manufacturing of positive electrode>
[0371] The slurry was evenly applied to the surface of the current collector composed of aluminum foil by a doctor blade method in such a way that the film thickness after drying was 110 μm, dried at 150°C for 30 minutes, and then heat-treated at 150°C / vacuum for 120 minutes. Then, the film (electrode active material layer) was pressed by a roller press to a density of 3.0 g / cm 3 , thus obtaining an electrode.
[0372] <Evaluation of Electrode Adhesion>
[0373] The electrode adhesion was evaluated as follows.
[0374] A test piece with a width of 2 cm and a length of 10 cm is cut out from the electrode and fixed with the coated surface facing up. Then, a 15-mm-wide adhesive tape ("Cellotape (registered trademark)", manufactured by Nichiban Co., Ltd.) (specified in JIS Z1522) is pressed and pasted onto the surface of the active material layer of the test piece. After that, at 25 °C, using a tensile testing machine (manufactured by A&D Company, Ltd., "TENSILON RTM-100"), the stress is measured when the adhesive tape is peeled off from one end of the test piece at a speed of 30 mm / minute in the 180° direction. The measurement is carried out twice, and the average value is calculated as the peel strength. The greater the peel strength, the higher the adhesion strength between the current collector and the active material layer or the adhesiveness between the active materials, indicating that the active material layer is difficult to peel off from the current collector or the active materials are difficult to peel off from each other.
[0375] <Assembly of lithium half-cell>
[0376] Inside a glove box purged with argon, the material obtained by punching the above electrode into a diameter of 16 mm is loaded inside a gasket of the Al lower cover of a test cell (manufactured by Nippon Tomcell Co., Ltd.). Then, a separator formed of a polypropylene porous membrane with a diameter of 24 mm (manufactured by CS TECH CO., LTD, product name "SelionP2010") is loaded. Further, 500 μL of electrolyte is injected to prevent air from entering, and then a material obtained by punching a commercially available metallic lithium foil into a diameter of 16 mm is loaded. The outer package of the aforementioned test cell is sealed with screws to assemble a lithium half-cell. The electrolyte used here is a solution in which LiPF6 is dissolved at a concentration of 1 mol / L in a solvent of ethylene carbonate / ethyl methyl carbonate = 1 / 1 (mass ratio).
[0377] <Charge and discharge measurement>
[0378] The lithium half-cell is placed in a constant temperature bath at 25 °C and charged at a constant current (0.1C). Charging is completed (cut off) when the voltage reaches 0.01V. Then, discharging is started at a constant current (0.1C), and discharging is completed (cut off) when the voltage reaches 1.0V. Such charge and discharge are repeated 30 times.
[0379] In addition, under the above measurement conditions, "1C" represents the current value at which a battery with a certain capacitance is discharged at a constant current and the discharge ends within 1 hour. For example, "0.1C" refers to the current value at which the discharge ends after 10 hours, and "10C" refers to the current value at which the discharge ends after 0.1 hour.
[0380] <Discharge capacity retention rate>
[0381] The discharge capacity retention rate was calculated by the following formula.
[0382] Discharge capacity retention rate = {(discharge capacity at the 30th cycle) / (discharge capacity at the 1st cycle)}×100 (%)
[0383] <haze>
[0384] The aqueous solutions of Example 3, Example 4, Comparative Example 3 and Comparative Example 4 were applied on a flat glass plate and formed into films with a thickness of 5 μm to 30 μm in a circulating air dryer at 80° C. The HAZE of the formed films was measured using a turbidity meter "NDH-2000 (manufactured by Nippon Denshoku Industries Co., Ltd.)".
[0385] As a result of the measurement, the HAZE of Example 3-3, Example 3-8, and Example 3-9 were 3, 6, and 26, respectively. On the other hand, the HAZE of Example 3 and Example 4 other than the above was 1 or less.
[0386] [Table 4]
[0387]
[0388] SBR: Styrene-butadiene copolymer latex
[0389] CMC: carboxymethyl cellulose.< / haze> < / ph>
Claims
1. A conductive carbon material dispersant for lithium ion batteries, comprising a water-soluble poly(meth)acrylamide (A-1), wherein the water-soluble poly(meth)acrylamide (A-1) contains 2 mol% to 60 mol% of structural units derived from a compound (a) containing a (meth)acrylamide group and 10 mol% to 70 mol% of structural units derived from an unsaturated sulfonic acid or a salt thereof (b) and has a weight average molecular weight of 10,000 to 250,000.
2. The conductive carbon material dispersant for lithium ion batteries according to claim 1, in, The water-soluble poly(meth)acrylamide (A-1) contains 20 mol % to 70 mol % of a structural unit derived from the (meth)acrylate (c).
3. A slurry for lithium-ion battery electrodes, comprising: The conductive carbon material dispersant for lithium ion batteries according to claim 1 or 2; Polymer (A-2); Electrode active material (B-1); A conductive carbon material (B-2); and water.
4. The lithium ion battery electrode slurry according to claim 3, in, The polymer (A-2) is a water-soluble poly (meth)acrylamide (A-2A) containing a structural unit derived from a (meth)acrylamide group-containing compound (a). 5 . A lithium ion battery electrode obtained by applying the slurry for lithium ion battery electrodes according to claim 3 or 4 onto a current collector and drying the slurry.
6. A lithium ion battery comprising the lithium ion battery electrode according to claim 5.