Lithium secondary battery
By using lithium difluoroxaloborate and a moisture-controlled electrolyte in a lithium secondary battery, combined with a conductive current collector and a positive active material plate with a layered rock salt structure, the problem of high internal resistance of the lithium secondary battery is solved and achieved It has low reaction resistance and high heat resistance, and is suitable for high current pulse discharge applications such as smart cards.
Patent Information
- Application Number
- CN201980065756.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-18
- Filing Date
- 2019-12-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2039-12-11
AI Technical Summary
Existing lithium secondary batteries are difficult to meet the demand for high-current pulse discharge in applications such as smart cards. The internal resistance is high, which affects the performance of the battery.
A lithium secondary battery design containing lithium difluorooxalate borate (LiDFOB) as an electrolyte additive. The moisture content in the electrolyte is controlled at 10-15 ppm. The structure of the positive and negative electrodes is optimized, including conductive collectors and layers. An active material plate with a rock salt structure, plus fluoroethylene carbonate as a heat-resistant additive.
It effectively reduces the reaction resistance of lithium secondary batteries, improves the cycle performance and heat resistance of the battery, and is suitable for high-current pulse discharge applications such as thin flexible devices and smart cards.
Smart Images

Figure CN113169378B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a lithium secondary battery.
[0002] [References to related applications]
[0003] This application claims the benefit of priority of Japanese patent application JP2018-236548 filed on December 18, 2018, the entire disclosure of which is incorporated into this application. Background Art
[0004] In recent years, the use of lithium secondary batteries has been studied as a power supply source for smart cards. As an electrolyte solution for lithium secondary batteries, for example, an electrolyte solution obtained by dissolving lithium hexafluorophosphate (LiPF6) in an organic solvent is known.
[0005] "Jiho Cha et al.,"Mechanisms for electrochemical performance enhancement by the salt-type electrolyte additive,lithium difluoro(oxalato)borate,in high-voltage lithium-ion batteries"Journal of Power Sources 357(2017)97-106" (Document 1) states that by adding lithium difluorooxalate borate (LiDFOB) to the electrolyte, the interfacial stability of the high-voltage Li-rich cathode and the graphite anode is improved. In addition, it is recorded that by adding LiDFOB to the electrolyte, the reduction in the cycle performance of the electrode is also suppressed.
[0006] However, in a smart card with fingerprint authentication and wireless communication functions, a large current pulse discharge from a power supply source is required, and therefore, the internal resistance (particularly reaction resistance) of a lithium secondary battery is required to be reduced. Summary of the invention
[0007] The present invention relates to a lithium secondary battery, and its object is to reduce the reaction resistance of the lithium secondary battery.
[0008] A lithium secondary battery according to a preferred embodiment of the present invention comprises: a positive electrode; a separator, which is arranged on the positive electrode in a specified overlapping direction; a negative electrode, which is arranged on the side of the separator opposite to the positive electrode in the overlapping direction; an electrolyte, which is impregnated in the positive electrode, the negative electrode and the separator; and a sheet-like outer body, which covers the positive electrode and the negative electrode from both sides of the overlapping direction, and accommodates the positive electrode, the separator, the negative electrode and the electrolyte inside. The electrolyte contains: an electrolyte material as a main agent, and lithium difluorooxalate borate as an additive. The water content in the electrolyte is greater than 10 mass ppm and less than 15 mass ppm. As a result, the reaction resistance of the lithium secondary battery can be reduced.
[0009] Preferably, the content of the lithium difluorooxalatoborate in the electrolytic solution is 0.1 mass % or more and 4.0 mass % or less.
[0010] Preferably, the reaction resistance per unit reaction area of the lithium secondary battery is 3.5Ω·cm 2 Above and 5.8Ω·cm 2 the following.
[0011] Preferably, the electrolyte further comprises fluoroethylene carbonate as an additive.
[0012] Preferably, the positive electrode includes: a sheet-shaped current collector having conductivity; and an active material plate, the active material plate being a plate-shaped ceramic sintered body containing a lithium composite oxide.
[0013] Preferably, the active material plate has a structure in which a plurality of primary particles having a layered rock salt structure are combined. The average tilt angle of the plurality of primary particles is greater than 0° and is less than 30°. The average tilt angle is the average value of the angles formed by the (003) crystal planes of the plurality of primary particles and the main surface of the active material plate.
[0014] Preferably, the lithium secondary battery is used as a power supply source in a sheet-like device or a flexible device.
[0015] Preferably, the lithium secondary battery is used as a power supply source in the flexible device, ie, a smart card.
[0016] The above-mentioned object and other objects, features, aspects and advantages will become more apparent from the following detailed description of the present invention with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a cross-sectional view of a lithium secondary battery according to one embodiment.
[0018] Figure 2 It is a top view of a lithium secondary battery.
[0019] Figure 3 is a cross-sectional view of another lithium secondary battery.
[0020] Figure 4A It is a diagram showing the production flow of a lithium secondary battery.
[0021] Figure 4B It is a diagram showing the production flow of a lithium secondary battery. DETAILED DESCRIPTION
[0022] Figure 1 It is a cross-sectional view showing the structure of a lithium secondary battery 1 according to one embodiment of the present invention. Figure 2 It is a top view of the lithium secondary battery 1 . Figure 1 In order to make the figure easier to understand, the lithium secondary battery 1 and its structure are depicted thicker than actual. Figure 1 In the figure, the widths of the positive electrode 2, separator 4, and negative electrode 3 described later in the left-right direction are depicted smaller than the actual widths, and the joints of the outer casing 6 (i.e., Figure 1 The width of the left and right ends in the left and right directions is drawn larger than the actual width. Figure 1 In the figure, a portion of the structure closer to the front side and the back side than the cross section is shown together. Figure 3 The same is true in .
[0023] The lithium secondary battery 1 is a small and thin battery. The shape of the lithium secondary battery 1 when viewed from above is, for example, a substantially rectangular shape. For example, the length of the lithium secondary battery 1 when viewed from above is 10 mm to 46 mm in the longitudinal direction, and 10 mm to 46 mm in the lateral direction. The thickness (i.e., Figure 1 The thickness in the vertical direction of the battery is, for example, 0.30 mm to 0.45 mm, preferably 0.40 mm to 0.45 mm. The lithium secondary battery 1 is a sheet-like or flexible thin plate-like component. The sheet-like component is a thin component that is easily deformed by a relatively small force, and is also called a film-like component. The same applies to the following description.
[0024] The lithium secondary battery 1 is mounted on, for example, a sheet device or a flexible device and is used as a power supply source. A sheet device is a thin device that is easily deformed by a relatively small force, and is also called a film device. In the present embodiment, the lithium secondary battery 1 is built into, for example, a smart card having a computing and processing function, and is used as a power supply source in the smart card. A smart card is a card-shaped flexible device. Smart cards are used as cards with fingerprint authentication and wireless communication functions, such as wireless communication ICs, ASICs for fingerprint analysis, and fingerprint sensors. In the following description, devices such as smart cards that are objects for which the lithium secondary battery 1 is used as a power supply source are also referred to as "object devices."
[0025] For example, the lithium secondary battery 1 is mounted on the smart card by cold lamination at room temperature or hot lamination by heating and pressing. The processing temperature in hot lamination is, for example, 110° C. to 260° C. In this embodiment, the lithium secondary battery 1 mounted on the smart card by cold lamination is described.
[0026] The lithium secondary battery 1 includes a positive electrode 2, a negative electrode 3, a separator 4, an electrolyte 5, an outer casing 6, and two terminals 7. The positive electrode 2, the separator 4, and the negative electrode 3 are stacked in a predetermined stacking direction. Figure 1 In the example shown, the positive electrode 2, the separator 4 and the negative electrode 3 are stacked in the vertical direction in the figure. Figure 1 The upper side and the lower side in the text are referred to as the "upper side" and the "lower side". Figure 1 The up-down direction in is referred to as the "up-down direction", also called the "overlapping direction". Figure 1 The up-down direction in FIG. 1 does not need to coincide with the actual up-down direction when the lithium secondary battery 1 is mounted on a target device such as a smart card.
[0027] Figure 1 In the example shown, the separator 4 is arranged on the upper surface of the positive electrode 2 in the vertical direction (i.e., the overlapping direction). The negative electrode 3 is arranged on the upper surface of the separator 4 in the vertical direction. In other words, the negative electrode 3 is arranged on the side of the separator 4 opposite to the positive electrode 2 in the vertical direction. The positive electrode 2, the separator 4, and the negative electrode 3 are each, for example, roughly rectangular in a plan view. The positive electrode 2, the separator 4, and the negative electrode 3 are roughly the same shape (i.e., roughly the same shape and roughly the same size) in a plan view.
[0028] The outer casing 6 is a sheet-shaped and bag-shaped component. The outer casing 6 is roughly rectangular when viewed from above. The outer casing 6 includes two layers of sheet portions 65 and 66 that overlap in the vertical direction. In the following description, the sheet portion 65 located on the lower side of the positive electrode 2 is referred to as the "first sheet portion 65", and the sheet portion 66 located on the upper side of the negative electrode 3 is referred to as the "second sheet portion 66". The outer peripheral edge of the first sheet portion 65 and the outer peripheral edge of the second sheet portion 66 are joined by, for example, a heat seal (so-called heat seal). The first sheet portion 65 and the second sheet portion 66 of the outer casing 6 are respectively formed by a laminated film obtained by laminating a metal foil 61 formed of a metal such as aluminum (Al) and an insulating resin layer 62. In the first sheet portion 65 and the second sheet portion 66, the resin layer 62 is located on the inner side of the metal foil 61.
[0029] The outer casing 6 covers the positive electrode 2 and the negative electrode 3 from both sides in the up-down direction. The outer casing 6 accommodates the positive electrode 2, the separator 4, the negative electrode 3 and the electrolyte 5 inside. The electrolyte 5 is continuously present around the positive electrode 2, the separator 4 and the negative electrode 3. In other words, the electrolyte 5 is between the positive electrode 2 and the negative electrode 3. The electrolyte 5 is impregnated in the positive electrode 2, the separator 4 and the negative electrode 3. Two terminals 7 extend from the inside of the outer casing 6 to the outside. Inside the outer casing 6, one terminal 7 is electrically connected to the positive electrode 2, and the other terminal 7 is electrically connected to the negative electrode 3.
[0030] The positive electrode 2 includes a positive electrode collector 21, a positive electrode active material plate 22, and a conductive bonding layer 23. The positive electrode collector 21 is a sheet-like member having conductivity. The lower surface of the positive electrode collector 21 is bonded to the resin layer 62 of the outer casing 6 by means of a positive electrode bonding layer 63. The positive electrode bonding layer 63 is formed, for example, of a mixed resin of an acid-modified polyolefin resin and an epoxy resin. The positive electrode bonding layer 63 can be formed of various other materials. The thickness of the positive electrode bonding layer 63 is, for example, 0.5 μm to 10 μm.
[0031] The positive electrode current collector 21 includes, for example, a metal foil formed of a metal such as aluminum, and a conductive carbon layer stacked on the upper surface of the metal foil. In other words, the main surface of the positive electrode current collector 21 that faces the positive electrode active material plate 22 is covered with a conductive carbon layer. The above-mentioned metal foil can be formed of various metals other than aluminum (for example, copper, nickel, silver, gold, chromium, iron, tin, lead, tungsten, molybdenum, titanium, zinc, or alloys containing these metals). In addition, the above-mentioned conductive carbon layer can be omitted from the positive electrode current collector 21.
[0032] The positive electrode active material plate 22 (i.e., the active material plate of the positive electrode 2) is a relatively thin plate-shaped ceramic sintered body containing a lithium composite oxide. The positive electrode active material plate 22 is bonded to the upper surface of the positive electrode collector 21 via a conductive bonding layer 23. The positive electrode active material plate 22 is opposed to the separator 4 in the vertical direction. The upper surface of the positive electrode active material plate 22 is in contact with the lower surface of the separator 4.
[0033] The positive electrode active material plate 22 has a structure in which a plurality of (i.e., a large number of) primary particles are bonded. The primary particles are composed of a lithium composite oxide having a layered rock salt structure. The lithium composite oxide is typically represented by the general formula: Li p An oxide represented by MO2 (wherein 0.05<p<1.10). M is at least one transition metal, for example, one or more selected from cobalt (Co), nickel (Ni) and manganese (Mn). The layered rock salt structure is a crystalline structure in which lithium layers and transition metal layers other than lithium are alternately stacked with oxygen layers sandwiched therebetween. That is, the layered rock salt structure is a crystalline structure in which transition metal ion layers and lithium single layers are alternately stacked with oxide ions sandwiched therebetween (typically an α-NaFeO2 type structure: a structure in which transition metals and lithium are regularly arranged on the
[111] axis of a cubic rock salt type structure).
[0034] Preferred examples of lithium composite oxides having a layered rock salt structure include: lithium cobalt oxide (Li p CoO2 (where 1≤p≤1.1), lithium nickel oxide (LiNiO2), lithium manganese oxide (Li2MnO3), lithium nickel manganese oxide (Li p (Ni 0.5 ,Mn 0.5 )O2), by the general formula: Li p (Co x ,Ni y ,Mn z )O2 (where 0.97≤p≤1.07, x+y+z=1) represented by a solid solution, Li p (Co x ,Ni y ,Al z )O2 (wherein, 0.97≤p≤1.07, x+y+z=1, 0<x≤0.25, 0.6≤y≤0.9 and 0<z≤0.1) or a solid solution of Li2MnO3 and LiMO2 (wherein, M is a transition metal such as Co and Ni). In particular, the lithium composite oxide is preferably lithium cobalt oxide Li p CoO2 (wherein 1≤p≤1.1), for example LiCoO2 (LCO).
[0035] It should be noted that the positive electrode active material plate 22 may further include one or more of elements such as magnesium (Mg), aluminum, silicon (Si), calcium (Ca), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zinc (Zn), gallium (Ga), germanium (Ge), strontium (Sr), yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), silver (Ag), tin (Sn), antimony (Sb), tellurium (Te), barium (Ba), and bismuth (Bi). In addition, gold (Au) or the like as a current collecting aid may be sputtered on the positive electrode active material plate 22.
[0036] In the positive electrode active material plate 22, the average particle size of the above-mentioned multiple primary particles, i.e., the primary particle size, is, for example, less than 20 μm, preferably less than 15 μm. In addition, the primary particle size is, for example, more than 0.2 μm, preferably more than 0.4 μm. The primary particle size can be measured by analyzing the SEM (scanning electron microscope) image of the cross section of the positive electrode active material plate 22. Specifically, for example, the positive electrode active material plate 22 is processed using a cross-section polisher (CP) to expose the ground cross section, and the ground cross section is observed using SEM at a specified magnification (e.g., 1000 times) and a specified field of view (e.g., 125 μm×125 μm). At this time, the field of view is set in such a way that there are more than 20 primary particles in the field of view. The diameter of the circumscribed circle when the circumscribed circle is drawn is solved for all the primary particles in the obtained SEM image, and their average value is used as the primary particle size.
[0037] In the positive electrode active material plate 22, the average tilt angle (i.e., average orientation angle) of the plurality of primary particles is preferably greater than 0° and less than 30°. In addition, the average tilt angle is more preferably greater than 5° and less than 28°, and further preferably greater than 10° and less than 25°. The average tilt angle is the average value of the angles formed by the (003) crystal planes of the plurality of primary particles and the main surface of the positive electrode active material plate 22 (e.g., the lower surface of the positive electrode active material plate 22).
[0038] For the inclination angle of a primary particle (i.e., the angle between the (003) crystal plane of the primary particle and the main surface of the positive electrode active material plate 22), the inclination angle of the primary particle can be measured by analyzing the cross section of the positive electrode active material plate 22 using electron backscatter diffraction (EBSD). Specifically, for example, the positive electrode active material plate 22 is processed using a cross-section polisher to expose the ground cross section, and the ground cross section is analyzed using EBSD at a specified magnification (e.g., 1000 times) and a specified field of view (e.g., 125μm×125μm). In the obtained EBSD image, the inclination angle of each primary particle is represented by the color intensity, and the darker the color, the smaller the inclination angle. Then, the average value of the inclination angles of multiple primary particles obtained from the EBSD image is taken as the above-mentioned average inclination angle.
[0039] Among the primary particles constituting the positive electrode active material plate 22, the proportion of primary particles having an inclination angle greater than 0° and less than 30° is preferably 60% or more, more preferably 80% or more, and further preferably 90% or more. The upper limit of this ratio is not particularly limited and can be 100%. The total area of primary particles having an inclination angle greater than 0° and less than 30° can be obtained in the above-mentioned EBSD image, and the total area of the primary particles is divided by the total particle area to obtain the ratio.
[0040] The porosity of the positive electrode active material plate 22 is, for example, 25% to 45%. The porosity of the positive electrode active material plate 22 is the volume ratio of the pores (including open pores and closed pores) in the positive electrode active material plate 22. The porosity can be measured by analyzing the SEM image of the cross section of the positive electrode active material plate 22. For example, the positive electrode active material plate 22 is processed using a cross-section polisher (CP) to expose the ground cross section, and the ground cross section is observed using an SEM at a specified magnification (for example, 1000 times) and a specified field of view (for example, 125μm×125μm). The obtained SEM image is analyzed, and the value obtained by dividing the area of all pores in the field of view by the area (cross-sectional area) of the positive electrode active material plate 22 in the field of view is multiplied by 100, thereby obtaining the porosity (%).
[0041] The average value of the diameter of the pores contained in the positive electrode active material plate 22, i.e., the average pore diameter, is, for example, less than 15 μm, preferably less than 12 μm, and more preferably less than 10 μm. In addition, the average pore diameter is, for example, greater than 0.1 μm, preferably greater than 0.3 μm. For the diameter of the above-mentioned pores, it is typically the diameter of the sphere when the pore is assumed to be a sphere with the same volume or the same cross-sectional area. The average pore diameter is a value calculated based on the number of average values of the diameters of multiple pores. The average pore diameter can be obtained by well-known methods such as analysis of cross-sectional SEM images or mercury intrusion. Preferably, a mercury porosimeter is used to measure the average pore diameter using mercury intrusion.
[0042] exist Figure 1 In the example shown, the positive electrode active material plate 22 is a single plate-like component, but it can also be divided into a plurality of plate-like components (hereinafter referred to as "active material plate elements"). In this case, the plurality of active material plate elements are respectively bonded to the positive electrode collector 21 by means of a conductive bonding layer 23. The plurality of active material plate elements are, for example, arranged in a matrix (i.e., a grid) on the positive electrode collector 21. The shape of each active material plate element when viewed from above is, for example, roughly rectangular. The plurality of active material plate elements can be roughly the same shape (i.e., roughly the same shape and roughly the same size) when viewed from above, or they can have different shapes. The plurality of active material plate elements are configured to be separated from each other when viewed from above.
[0043] The conductive bonding layer 23 includes a conductive powder and a binder. The conductive powder is, for example, a powder of acetylene black, flaky natural graphite, carbon nanotubes, carbon nanofibers, carbon nanotube derivatives or carbon nanofiber derivatives. The binder includes, for example, a polyimideamide resin. The polyimideamide resin contained in the binder may be one kind or more than two kinds. In addition, the binder may include a resin other than the polyimideamide resin. The conductive bonding layer 23 is formed as follows, that is, a liquid or paste adhesive containing the above-mentioned conductive powder and binder, and a solvent is applied to the positive electrode collector 21 or the positive electrode active material plate 22, and the solvent is evaporated between the positive electrode collector 21 and the positive electrode active material plate 22, and solidified to form the conductive bonding layer 23.
[0044] The thickness of the positive electrode collector 21 is, for example, 9 μm to 50 μm, preferably 9 μm to 20 μm, and more preferably 9 μm to 15 μm. The thickness of the positive electrode active material plate 22 is, for example, 15 μm to 200 μm, preferably 30 μm to 150 μm, and more preferably 50 μm to 100 μm. By thickening the positive electrode active material plate 22, the active material capacity per unit area can be increased, so that the energy density of the lithium secondary battery 1 is increased. By thinning the positive electrode active material plate 22, the degradation of battery characteristics (especially the increase in resistance value) associated with repeated charge and discharge can be suppressed. The thickness of the conductive bonding layer 23 is, for example, 3 μm to 28 μm, and preferably 5 μm to 25 μm.
[0045] The negative electrode 3 includes a negative electrode collector 31 and a negative electrode active material layer 32. The negative electrode collector 31 is a sheet-like member having conductivity. The upper surface of the negative electrode collector 31 is bonded to the outer casing 6 via a negative electrode bonding layer 64. The negative electrode bonding layer 64 is formed of, for example, a mixed resin of an acid-modified polyolefin resin and an epoxy resin. The negative electrode bonding layer 64 can be formed of various other materials. The thickness of the negative electrode bonding layer 64 is, for example, 0.5 μm to 10 μm.
[0046] The negative electrode current collector 31 is a metal foil made of a metal such as copper. The metal foil may be made of various metals other than copper (e.g., stainless steel, nickel, aluminum, silver, gold, chromium, iron, tin, lead, tungsten, molybdenum, titanium, zinc, or alloys containing these metals).
[0047] The negative electrode active material layer 32 includes: a binder with a resin as a main component, and a carbonaceous material as a negative electrode active material. The negative electrode active material layer 32 is coated on the lower surface of the negative electrode collector 31. That is, the negative electrode 3 is a so-called coated electrode. The negative electrode active material layer 32 is opposed to the separator 4 in the vertical direction. The lower surface of the negative electrode active material layer 32 is in contact with the upper surface of the separator 4.
[0048] In the negative electrode active material layer 32, the above-mentioned carbonaceous material is, for example, graphite (natural graphite or artificial graphite), pyrolytic carbon, coke, resin sintered body, mesophase microspheres or mesophase asphalt, etc. In the negative electrode 3, lithium storage material can be used instead of carbonaceous material as the negative electrode active material. The lithium storage material is, for example, silicon, aluminum, tin, iron, iridium or alloys, oxides or fluorides containing these metals. The binder is, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF) or a mixture of these substances. In this embodiment, PVDF is used as a binder.
[0049] The thickness of the negative electrode current collector 31 is, for example, 5 μm to 25 μm, preferably 8 μm to 20 μm, and more preferably 8 μm to 15 μm. The thickness of the negative electrode active material layer 32 is, for example, 20 μm to 300 μm, preferably 30 μm to 250 μm, and more preferably 30 μm to 150 μm. By thickening the negative electrode active material layer 32, the active material capacity per unit area can be increased, so that the energy density of the lithium secondary battery 1 is increased. By thinning the negative electrode active material layer 32, the degradation of battery characteristics (especially the increase in resistance value) associated with repeated charging and discharging can be suppressed.
[0050] In the lithium secondary battery 1, the Figure 3 As shown, a negative electrode 3a having a structure different from that of the negative electrode 3 is provided instead of the negative electrode 3 as the coating electrode. The negative electrode 3a has a structure substantially the same as that of the positive electrode 2 described above. Specifically, the negative electrode 3a includes: a negative electrode collector 31a, a negative electrode active material plate 32a, and a conductive bonding layer 33a. The negative electrode collector 31a is a sheet-like member having conductivity. The negative electrode collector 31a is, for example, a member having the same structure formed of the same material as the negative electrode collector 31 described above.
[0051] The negative electrode active material plate 32a (i.e., the active material plate of the negative electrode 3a) is a relatively thin plate-shaped ceramic sintered body containing a lithium composite oxide (e.g., lithium titanium oxide (LTO)). The negative electrode active material plate 32a is bonded to the lower surface of the negative electrode collector 31a by means of a conductive bonding layer 33a. The conductive bonding layer 33a is formed of, for example, the same material as the conductive bonding layer 23 of the positive electrode 2 described above. The negative electrode active material plate 32a is opposed to the separator 4 in the up and down direction. The lower surface of the negative electrode active material plate 32a is in contact with the upper surface of the separator 4.
[0052] The thickness of the negative electrode collector 31 is, for example, 5 μm to 25 μm, preferably 8 μm to 20 μm, and more preferably 8 μm to 15 μm. The thickness of the negative electrode active material plate 32a is, for example, 10 μm to 300 μm, preferably 30 μm to 200 μm, and more preferably 30 μm to 150 μm. By thickening the negative electrode active material plate 32a, the active material capacity per unit area can be increased, so that the energy density of the lithium secondary battery 1 is increased. By thinning the negative electrode active material plate 32a, the degradation of battery characteristics (especially the increase in resistance value) associated with repeated charging and discharging can be suppressed. The thickness of the conductive bonding layer 33a is, for example, 3 μm to 30 μm, and preferably 5 μm to 25 μm.
[0053] exist Figure 3 In the example shown, the negative electrode active material plate 32a is a single plate-like component, but it can also be divided into a plurality of plate-like components (hereinafter referred to as "active material plate elements"). In this case, the plurality of active material plate elements are respectively bonded to the negative electrode current collector 31a by means of a conductive bonding layer 33a. The plurality of active material plate elements are, for example, arranged in a matrix (i.e., a grid) on the negative electrode current collector 31a. The shape of each active material plate element when viewed from above is, for example, roughly rectangular. The plurality of active material plate elements can have roughly the same shape (i.e., roughly the same shape and roughly the same size) when viewed from above, or they can have different shapes. The plurality of active material plate elements are configured to be separated from each other when viewed from above.
[0054] Figure 1 and Figure 3 In the lithium secondary battery 1 shown, the electrolyte 5 includes: an electrolyte material as a main agent, and lithium difluorooxalatoborate (LiDFOB) as an additive. The electrolyte material is: for example, a solution obtained by dissolving lithium hexafluorophosphate (LiPF6) as a solute in an organic solvent. The organic solvent is: for example, a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC), a mixed solvent of EC and methyl ethyl carbonate (MEC), or a mixed solvent of EC and diethyl carbonate (DEC). The organic solvent can be a single solvent of any of the above solvents. The organic solvent can contain substances other than the above. In the present embodiment, the organic solvent is a mixed solvent of EC and EMC. The volume ratio of EC:EMC in the organic solvent is, for example, 8:2 to 2:8, preferably 3:7 to 5:5. In the present embodiment, the volume ratio of EC:EMC is 3:7.
[0055] The LiPF6 concentration in the electrolyte 5 is, for example, 0.8 mol / L to 2.0 mol / L, preferably 0.8 mol / L to 1.5 mol / L, more preferably 1.0 mol / L to 1.5 mol / L, and further preferably 1.0 mol / L to 1.2 mol / L. It should be noted that the electrolyte material of the electrolyte 5 can be changed in various ways. For example, the solute dissolved in the organic solvent can be lithium tetrafluoroborate (LiBF4).
[0056] The above-mentioned LiDFOB as an additive is also called LiODFB, and its molecular formula is LiF2BC2O4. The content of LiDFOB in the electrolyte 5 is, for example, 0.01 mass % or more, preferably 0.05 mass % or more, and more preferably 0.1 mass % or more. The content of LiDFOB in the electrolyte 5 is, for example, 10.0 mass % or less, preferably 5.0 mass % or less, and more preferably 4.0 mass % or less.
[0057] In addition to LiDFOB, the electrolyte 5 may further include other additives. Other additives are, for example, fluoroethylene carbonate (FEC). FEC has excellent heat resistance. Therefore, by including FEC in the electrolyte 5, an SEI film with excellent heat resistance can be formed on the surface of the negative electrode 3, further improving the heat resistance of the lithium secondary battery 1. The above-mentioned other additives may be, for example, vinylene carbonate (VC). VC also has excellent heat resistance, therefore, by including VC in the electrolyte 5, the heat resistance of the lithium secondary battery 1 can be further improved.
[0058] The electrolyte 5 contains a small amount of water. The water content of the electrolyte 5 is, for example, 30 mass ppm or less, preferably 20 mass ppm or less, and more preferably 15 mass ppm or less. In addition, the water content of the electrolyte 5 is, for example, 10 mass ppm or more, and preferably 11 mass ppm or more.
[0059] The partition 4 is a sheet-like or thin-plate-like insulating component. The partition 4 is, for example, a single-layer partition formed of a resin. The resin is, for example, polyimide, polyethylene, polyester (for example, polyethylene terephthalate (PET)) or polypropylene. In the present embodiment, the partition 4 is formed mainly of polypropylene. The thickness of the partition 4 is, for example, 8 μm or more, preferably 10 μm or more, and more preferably 15 μm or more. In addition, the thickness of the partition 4 is, for example, 30 μm or less, preferably 28 μm or less, and more preferably 25 μm or less.
[0060] In addition, the partition 4 may be, for example, a two-layer partition obtained by laminating a resin layer on a ceramic substrate. Alternatively, the partition 4 may be a two-layer partition obtained by coating a ceramic on a substrate as a resin layer. The partition 4 may have a multilayer structure of three or more layers. For example, the partition 4 may be a three-layer partition obtained by laminating resin layers on the upper surface and the lower surface of a ceramic substrate.
[0061] In the lithium secondary battery 1, by using the above-mentioned electrolyte 5, a lower internal resistance (especially reaction resistance) can be achieved. The reaction resistance represents the diameter of the arc component in the Cole-Cole diagram obtained by the AC impedance test in the real axis direction, which is consistent with the resistance value at about 10 Hz. The reaction resistance per unit reaction area of the lithium secondary battery 1 (i.e., the resistance at 10 Hz measured by the AC impedance method) is, for example, 5.8 Ω·cm 2 (ohm·square centimeter) or less, preferably 5.5Ω·cm 2 Below, more preferably 5.0Ω·cm 2 In addition, the reaction resistance per unit reaction area is, for example, 3.5 Ω·cm 2 Above, preferably 3.8Ω·cm 2 More preferably, 4.0Ω·cm 2 It should be noted that the above reaction area is the area of the portion where one of the positive electrode active material plate 22 and the negative electrode active material layer 32 faces the other. In other words, the reaction area is the area of the overlapping portion of the positive electrode active material plate 22 and the negative electrode active material layer 32 when viewed from above.
[0062] Next, refer to Figure 4A and Figure 4B , an example of the manufacturing process of the lithium secondary battery 1 is described. First, two aluminum laminate films (manufactured by Showa Denko Packaging, thickness 61 μm, 3-layer structure of polypropylene film / aluminum foil / nylon film) are prepared as the first sheet portion 65 and the second sheet portion 66 of the outer casing 6. In addition, a positive electrode active material plate 22 is prepared. The positive electrode active material plate 22 is formed by sintering a LiCoO2 green sheet. Figure 4A In the example shown, the positive electrode active material plate 22 has a plurality of active material plate elements 24. When the positive electrode active material plate 22 is an integrally connected member (ie, a single plate), the following manufacturing method is substantially the same.
[0063] LiCoO2 green sheets were prepared as follows. First, Co3O4 powder (manufactured by Shodo Chemical Industry Co., Ltd.) and Li2CO3 powder (manufactured by Honjo Chemical Co., Ltd.) weighed at a Li / Co molar ratio of 1.01 were mixed and kept at 780°C for 5 hours. Next, the obtained powder was crushed and broken into a volume reference D50 of 0.4 μm using a pot mill to obtain a powder consisting of LiCoO2 plate-like particles.
[0064] 100 parts by weight of the obtained LiCoO2 powder, 100 parts by weight of the dispersion medium (toluene: isopropanol = 1:1), 10 parts by weight of the binder (polyvinyl butyral: model BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of the plasticizer (DOP: di(2-ethylhexyl) phthalate, manufactured by Kurokin Chemicals Co., Ltd.), and 2 parts by weight of the dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) are mixed. The obtained mixture is stirred and degassed under reduced pressure, and the viscosity is adjusted to 4000 cP, thereby preparing LiCoO2 slurry. The viscosity is measured using an LVT viscometer manufactured by Brookfield. The slurry prepared in this way is formed into a sheet on a polyethylene terephthalate (PET) film by a scraper method, thereby forming a LiCoO2 green sheet. The thickness of the dried LiCoO2 green sheet is 98 μm.
[0065] Next, the LiCoO2 green sheet peeled off from the PET film is cut into 50 mm squares with a cutter and placed in the center of a magnesium oxide setter (size 90 mm square, height 1 mm) as a lower setter. In addition, a porous magnesium oxide setter as an upper setter is placed on the LiCoO2 green sheet. The LiCoO2 green sheet is placed in a 120 mm square alumina sagger (manufactured by Nikkato Co., Ltd.) in a state of being sandwiched by the setter. At this time, there is no need to seal the alumina sagger, and the lid is covered with a gap of 0.5 mm. The obtained stack is heated to 600°C at a heating rate of 200°C / h, degreased for 3 hours, and then heated to 870°C at 200°C / h, maintained for 20 hours, and fired. After firing, the fired body is taken out of the alumina sagger after cooling to room temperature. In this way, a LiCoO2 sintered body plate with a thickness of 90 μm is obtained. The obtained LiCoO 2 sintered body plate was cut into a rectangle of 10.5 mm×9.5 mm by a laser processing machine to obtain a plurality of active material plate elements 24 (ie, positive electrode active material plates 22 ).
[0066] After the positive electrode active material plate 22 is prepared, acetylene black is mixed with a solution obtained by dissolving polyamideimide (PAI) in N-methylpyrrolidone to prepare a slurry, and 2 μL (microliters) of the slurry is dripped onto the positive electrode collector 21 (aluminum foil with a thickness of 9 mm) to form a conductive bonding layer 23. Next, the positive electrode active material plate 22 is placed on the conductive bonding layer 23 and dried. Figure 4AIn the example shown, the positive electrode active material plate 22 having a plurality of active material plate elements 24 is bonded to the positive electrode current collector 21 via the conductive bonding layer 23. Then, the composite of the positive electrode current collector 21 and the positive electrode active material plate 22 (i.e., the plurality of active material plate elements 24) is stacked on the first sheet portion 65 and bonded to the first sheet portion 65 via the positive electrode bonding layer 63, thereby forming the positive electrode assembly 20. In addition, one end of a terminal 7 is fixed to the positive electrode current collector 21 in advance by welding.
[0067] On the other hand, a negative electrode active material layer 32 (a carbon layer with a thickness of 130 μm) is coated on the negative electrode collector 31 (a copper foil with a thickness of 10 μm). The negative electrode active material layer 32 is a carbon coating film containing a mixture of graphite as an active material and PVDF as a binder. Next, the composite of the negative electrode collector 31 and the negative electrode active material layer 32 is stacked on the second sheet portion 66 and joined to the second sheet portion 66 by means of the negative electrode bonding layer 64, thereby forming a negative electrode assembly 30. In addition, one end of a terminal 7 is fixed in advance to the negative electrode collector 31 by welding.
[0068] As the separator 4, a porous polyolefin film (Celgard#2500) is prepared. Then, the positive electrode assembly 20, the separator 4 and the negative electrode assembly 30 are stacked in sequence in such a manner that the positive electrode active material plate 22 and the negative electrode active material layer 32 are opposite to the separator 4 to form an intermediate laminate 10. In the intermediate laminate 10, the upper and lower surfaces are covered with an outer body 6 (i.e., a first sheet portion 65 and a second sheet portion 66), and the first sheet portion 65 and the second sheet portion 66 extend around the positive electrode assembly 20, the separator 4 and the negative electrode assembly 30. In addition, the thickness of the positive electrode assembly 20, the separator 4 and the negative electrode assembly 30 (hereinafter collectively referred to as the "battery element 15") in the vertical direction is 0.33 mm. The shape of the battery element 15 when viewed from above is a roughly rectangular shape of 2.3 cm×3.2 cm.
[0069] Next, three of the four sides of the substantially rectangular intermediate laminate 10 are sealed by heat sealing. Figure 4A In the example shown, three sides except one side on the upper side in the figure are sealed. Among the three sides, one side is included for two terminals 7 to protrude. In the sealing of the three sides, a pressing fixture adjusted to a sealing width of 2 mm is used to heat and pressurize the outer peripheral portion of the intermediate stack 10 at 200°C and 1.5MPa (megapascal) for 10 seconds. Thus, the first sheet portion 65 and the second sheet portion 66 of the outer body 6 are heat-sealed. After the three sides are sealed, the intermediate stack 10 is placed in a vacuum dryer 81 to remove moisture and dry the adhesive (i.e., the positive electrode bonding layer 63, the negative electrode bonding layer 64 and the conductive bonding layer 23).
[0070] Next, if Figure 4B As shown, the intermediate stack 10 is stored in a glove box 82. Then, an injection device 83 is inserted between the first sheet portion 65 and the second sheet portion 66 at an unsealed side of the intermediate stack 10, and the electrolyte 5 is injected into the intermediate stack 10 via the injection device 83. The electrolyte 5 is a liquid obtained by dissolving LiPF6 at a concentration of 1 mol / L in a mixed solvent containing EC and EMC at a volume ratio of 3:7, and then adding a predetermined amount of LiDFOB with a water content of 50 ppm as an additive. In Examples 1 to 3 and Comparative Examples 1 to 3 described later, the amount of LiDFOB added is changed between 1.0 mass% and 4.0 mass%. In addition, in Example 4 and Comparative Example 4, the amount of LiDFOB added is 1.0 mass%, and as an additive other than LiDFOB, 1.0 mass% of FEC is also added to the electrolyte 5.
[0071] After the injection of the electrolyte 5 is completed, the unsealed side is pre-sealed (i.e., decompression sealing) using a simple sealer in a reduced pressure atmosphere of 5 kPa absolute pressure in the glove box 82. Next, the intermediate stack 10 is initially charged and aged for 7 days. After the aging is completed, the portion near the outer edge of the pre-sealed side of the first sheet portion 65 and the second sheet portion 66 (i.e., the end portion not containing the battery element 15) is cut off to remove the gas containing moisture generated by aging (i.e., gas release).
[0072] After the gas release is completed, the edges formed by the above-mentioned cutting are sealed by heat sealing in a reduced pressure atmosphere of 5 kPa absolute pressure in the glove box 82. In this sealing, as with the sealing of the above-mentioned three edges, a pressing fixture adjusted to a sealing width of 2 mm is used to heat and pressurize the first sheet portion 65 and the second sheet portion 66 at 200°C and 1.5 MPa for 10 seconds. Thus, the first sheet portion 65 and the second sheet portion 66 of the outer body 6 are heat-sealed to form a lithium secondary battery 1. Then, the excess parts at the periphery of the outer body 6 are cut off to adjust the shape of the lithium secondary battery 1. The shape of the lithium secondary battery 1 when viewed from above is a rectangle of 38 mm × 27 mm, a thickness of less than 0.45 mm, and a capacity of 30 mAh.
[0073] In the lithium secondary battery 1 manufactured by the above-mentioned manufacturing method, the average orientation angle of the primary particles in the positive electrode active material plate 22 (i.e., LiCoO2 sintered body plate) is 16°. The average orientation angle is determined as follows. First, the above-mentioned LiCoO2 sintered body plate is polished using a cross-section polisher (CP) (manufactured by JEOL Ltd., IB-15000CP), and the obtained cross section (i.e., a cross section perpendicular to the main surface of the LiCoO2 sintered body plate) is subjected to EBSD measurement with a 1000-fold field of view (125 μm × 125 μm) to obtain an EBSD image. The EBSD measurement is performed using a Schottky field emission scanning electron microscope (manufactured by JEOL Ltd., model JSM-7800F). Then, for all particles identified in the obtained EBSD image, the angle formed by the (003) crystal plane of the primary particle and the main surface of the LiCoO2 sintered body plate (i.e., the inclination of the crystal orientation relative to the (003) crystal plane) is calculated as the inclination angle, and the average value of these angles is set as the average orientation angle of the primary particle.
[0074] As described above, the thickness of the LiCoO2 sintered body plate is 90 μm. The LiCoO2 sintered body plate is ground using a cross-section polisher (CP) (manufactured by JEOL Ltd., IB-15000CP), and the obtained cross section is observed by SEM (manufactured by JEOL Ltd., JSM6390LA) to measure the plate thickness. In addition, the thickness of the above-mentioned dried LiCoO2 green sheet is also measured in the same manner.
[0075] The porosity of the LiCoO2 sintered body plate is 30%. The porosity is measured as follows. The LiCoO2 sintered body plate is ground using a cross-section polisher (CP) (manufactured by JEOL Ltd., IB-15000CP), and the obtained cross section is observed by SEM (manufactured by JEOL Ltd., JSM6390LA) at a 1000-fold field of view (125 μm × 125 μm). The obtained SEM image is analyzed, and the area of all pores is divided by the area of the LiCoO2 sintered body plate, and the obtained value is multiplied by 100, thereby calculating the porosity (%).
[0076] The average pore diameter of the LiCoO2 sintered body plate is 0.8 μm, which is measured by mercury porosimetry (AutoPore IV9510 manufactured by Shimadzu Corporation).
[0077] Next, referring to Table 1, the relationship between the water content of the electrolytic solution 5 and the reaction resistance per unit reaction area of the lithium secondary battery 1 will be described.
[0078] [Table 1]
[0079]
[0080] The reaction resistance in the table is the reaction resistance per unit reaction area of the lithium secondary battery 1 (i.e., the resistance at 10 Hz measured by the AC impedance method). The reaction resistance per unit reaction area (hereinafter referred to as "reaction resistance") was measured by the AC impedance method using a VMP-300 manufactured by Bio-Logic at a battery voltage of 3.8 V, and the resistance value at 10 Hz (Ω·cm) was read from the obtained Cole-Cole plot. 2 ). The measurement was performed at an amplitude of 2 mV and a measurement frequency range of 250 kHz to 200 mHz.
[0081] The moisture content in the table is the moisture content of the electrolyte 5 of the lithium secondary battery 1. The lithium secondary battery 1 after the reaction resistance measurement was disassembled, and the moisture content was measured using a moisture measuring device CA-200 / KF200 manufactured by Mitsubishi Chemical Analysis Tech Co., Ltd. In order to also measure the moisture content of the electrolyte 5 impregnated in the battery element 15 (i.e., the positive electrode 2, the separator 4, and the negative electrode 3), the measurement object includes not only the electrolyte 5 but also the battery element 15.
[0082] In the lithium secondary battery 1 of Example 1, LiDFOB having a water content of 50 ppm was added to the electrolyte 5 so as to have a concentration of 1.0 mass %.
[0083] In the lithium secondary battery 1 of Example 2, LiDFOB having a water content of 50 ppm was added to the electrolyte 5 so as to have a concentration of 2.0 mass %.
[0084] In the lithium secondary battery 1 of Example 3, LiDFOB having a water content of 50 ppm was added to the electrolyte 5 so as to have a concentration of 4.0 mass %.
[0085] In the lithium secondary battery 1 of Example 4, LiDFOB having a water content of 50 ppm was added to the electrolyte 5 at a concentration of 1.0 mass %, and FEC was further added to the electrolyte 5 at a concentration of 1.0 mass %.
[0086] In the lithium secondary battery 1 of Comparative Example 1, LiDFOB having a water content of 1000 ppm was added to the electrolyte 5 so as to have a concentration of 1.0 mass %.
[0087] In the lithium secondary battery 1 of Comparative Example 2, LiDFOB having a water content of 1000 ppm was added to the electrolyte 5 so as to have a concentration of 2.0 mass %.
[0088] In the lithium secondary battery 1 of Comparative Example 3, LiDFOB having a water content of 1000 ppm was added to the electrolyte 5 so as to have a concentration of 4.0 mass %.
[0089] In the lithium secondary battery 1 of Comparative Example 4, LiDFOB having a water content of 1000 ppm was added to the electrolyte 5 at a concentration of 1.0 mass %, and FEC was further added to the electrolyte 5 at a concentration of 1.0 mass %.
[0090] In Examples 1 to 4, the water content of the electrolyte 5 was 11 mass ppm to 14 mass ppm. In addition, the reaction resistance per unit reaction area of the lithium secondary battery 1 was 4.68 Ω·cm 2 ~5.75Ω·cm 2 On the other hand, in Comparative Examples 1 to 4, the water content of the electrolyte 5 was 20 mass ppm to 50 mass ppm. In addition, the reaction resistance per unit reaction area of the lithium secondary battery 1 was 5.09 Ω·cm 2 ~5.93Ω·cm 2 According to Examples 1 to 4 and Comparative Examples 1 to 4, it is found that when the water content of the electrolytic solution 5 is 11 mass ppm or more and 14 mass ppm or less, the reaction resistance per unit reaction area of the lithium secondary battery 1 is reduced.
[0091] As described above, the lithium secondary battery 1 comprises: a positive electrode 2, a separator 4, a negative electrode 3, an electrolyte 5, and an outer casing 6. The separator 4 is arranged on the positive electrode 2 in a predetermined overlapping direction. The negative electrode 3 is arranged on the side of the separator 4 opposite to the positive electrode 2 in the overlapping direction. The electrolyte 5 is impregnated in the positive electrode 2, the negative electrode 3, and the separator 4. The outer casing 6 is in the form of a sheet, and covers the positive electrode 2 and the negative electrode 3 from both sides of the above-mentioned overlapping direction. The outer casing 6 accommodates the positive electrode 2, the separator 4, the negative electrode 3, and the electrolyte 5 inside. The electrolyte 5 contains: an electrolyte material as a main agent, and LiDFOB as an additive. The water content in the electrolyte 5 is greater than 10 mass ppm and less than 15 mass ppm.
[0092] In the lithium secondary battery 1, the reaction resistance can be reduced by including LiDFOB in the electrolyte 5. In addition, by making the water content in the electrolyte 5 less than 15 mass ppm, the reaction resistance of the lithium secondary battery 1 can be further reduced. On the other hand, by making the water content in the electrolyte 5 more than 10 mass ppm, the water removal time in the manufacturing process of the lithium secondary battery 1 can be suppressed from becoming longer. Therefore, it is possible to prevent the time required for aging from being too long and prevent the battery characteristics from being deteriorated due to excessive aging.
[0093] Thus, the lithium secondary battery 1 can achieve low resistance despite being thin, and is therefore particularly suitable as a power supply source for thin devices, such as sheet devices or flexible devices (e.g., smart cards), that require low resistance for high current pulse discharge.
[0094] In the lithium secondary battery 1, the content of LiDFOB in the electrolyte 5 is preferably 0.1 mass % or more and 4.0 mass % or less. By setting the content of LiDFOB to 0.1 mass % or more, the reaction resistance of the lithium secondary battery 1 can be well reduced. In addition, by setting the content of LiDFOB to 4.0 mass % or less, the increase in the amount of water in the electrolyte 5 can be suppressed.
[0095] In the lithium secondary battery 1, the reaction resistance per unit reaction area is preferably 3.5 Ω·cm 2 Above and 5.8Ω·cm 2 By reducing the reaction resistance in this way, it is possible to provide the lithium secondary battery 1 suitable for large current pulse discharge.
[0096] In the lithium secondary battery 1 , the electrolyte 5 preferably further contains FEC as an additive. Thereby, as shown in Example 4, the reaction resistance of the lithium secondary battery 1 can be further reduced compared with Examples 2 and 3.
[0097] As described above, the positive electrode 2 preferably includes a sheet-shaped current collector having conductivity (i.e., positive electrode current collector 21) and an active material plate (i.e., positive electrode active material plate 22) which is a plate-shaped ceramic sintered body containing lithium composite oxide. This can further reduce the reaction resistance of the lithium secondary battery 1.
[0098] More preferably, the positive electrode active material plate 22 of the positive electrode 2 has: a structure obtained by combining multiple primary particles having a layered rock salt structure. In addition, the average tilt angle of the multiple primary particles is preferably greater than 0° and less than 30°. The average tilt angle is the average value of the angles formed by the (003) crystal planes of the multiple primary particles and the main surface of the positive electrode active material plate 22. Thus, the internal stress of the positive electrode active material plate 22 generated during the lattice expansion and contraction accompanying the charge and discharge cycle can be suppressed from being applied to the main surface of the positive electrode active material plate 22 that is opposite to the conductive bonding layer 23 and the positive electrode collector 21.
[0099] In this way, by making the main surface of the positive electrode active material plate 22 in contact with the conductive bonding layer 23 a main surface to which the internal stress generated during lattice expansion is not easily applied, it is possible to suppress the reduction in the bonding strength between the positive electrode active material plate 22 and the positive electrode collector 21. As a result, the voltage stability of the lithium secondary battery 1 during charging and discharging can be improved.
[0100] The above-mentioned lithium secondary battery 1 can be modified in various ways.
[0101] For example, the content of LiDFOB in the electrolyte 5 may be less than 0.1% by mass or more than 4.0% by mass. In addition, the reaction resistance per unit reaction area of the lithium secondary battery 1 may be less than 3.5 Ω·cm 2, can also be greater than 5.8Ω·cm 2 .
[0102] The structure of the positive electrode active material plate 22 of the positive electrode 2 can be changed in various ways. For example, in the positive electrode active material plate 22, the average tilt angle of the plurality of primary particles having a layered rock salt structure can be greater than 30° or can be 0°. Alternatively, the structure of the plurality of primary particles can be a structure other than a layered rock salt structure.
[0103] The positive electrode 2 may be a coated electrode in which a positive electrode active material layer including a binder mainly composed of a resin and a positive electrode active material is coated on a positive electrode current collector 21 .
[0104] The lithium secondary battery 1 can be used as a power supply source for flexible devices (e.g., card-type devices) or sheet-like devices (e.g., wearable devices provided on clothes, etc., or body-adhesive devices) other than smart cards. In addition, the lithium secondary battery 1 can be used as a power supply source for various objects (e.g., IoT modules) other than the above-mentioned devices.
[0105] The configurations in the above-described embodiment and each modified example may be appropriately combined unless they are mutually contradictory.
[0106] Although the invention has been described in detail, the above description is illustrative and not restrictive. Therefore, it can be said that various modifications and variations can be adopted without departing from the scope of the present invention.
[0107] Industrial Applicability
[0108] The lithium secondary battery of the present invention can be used in various fields utilizing lithium secondary batteries, such as, for example, as a power supply source in a smart card having a calculation processing function.
[0109] Explanation of symbols
[0110] 1 Lithium secondary battery
[0111] 2 Positive electrode
[0112] 3. 3a Negative electrode
[0113] 4 Partition
[0114] 5 Electrolyte
[0115] 6 outer body
[0116] 21. Positive electrode collector
[0117] 22. Positive active material plate
Claims
1. A lithium secondary battery, wherein: have: positive electrode; a separator, the separator being arranged on the positive electrode in a prescribed overlapping direction; a negative electrode, the negative electrode being arranged on the side of the separator opposite to the positive electrode in the overlapping direction; An electrolyte, the electrolyte being impregnated into the positive electrode, the negative electrode and the separator; as well as a sheet-shaped outer casing, which covers the positive electrode and the negative electrode from both sides in the overlapping direction and accommodates the positive electrode, the separator, the negative electrode and the electrolyte solution inside; The electrolyte comprises: Electrolyte material as the main agent, and Lithium difluorooxalate borate as an additive, The water content in the electrolyte is 11 mass ppm or more and 15 mass ppm or less, The content of the lithium difluorooxalatoborate in the electrolyte is 0.1 mass % or more and 4 mass % or less, The reaction resistance per unit reaction area is 4.68Ω·cm 2 Above and 5.8Ω·cm 2 the following.
2. The lithium secondary battery according to claim 1, wherein The electrolyte further comprises fluoroethylene carbonate as an additive.
3. The lithium secondary battery according to claim 1 or 2, wherein: The positive electrode has: a sheet-shaped current collector having conductivity; and An active material plate is a plate-shaped ceramic sintered body containing a lithium composite oxide.
4. The lithium secondary battery according to claim 3, wherein: The active material plate has a structure in which a plurality of primary particles having a layered rock salt structure are bonded together. The average tilt angle of the plurality of primary particles is greater than 0° and less than 30°, The average tilt angle is an average value of angles formed between the (003) crystal planes of the plurality of primary particles and the main surface of the active material plate.
5. The lithium secondary battery according to claim 1 or 2, wherein: The lithium secondary battery is used as a power supply source in a sheet-like device or a flexible device.
6. The lithium secondary battery according to claim 5, wherein: The lithium secondary battery is used as a power supply source in the smart card which is a flexible device.